Negative electrode material and battery

By optimizing the apparent density, true density, and pore volume of silicon-based anode materials, anode materials with porous structures and coatings were designed, solving the problem of volume expansion effect of silicon-based anode materials during cycling and achieving high-capacity, stable, and high-efficiency battery performance.

CN123162189APending Publication Date: 2026-11-24BTR NEW MATERIAL GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510662082.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-21
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing silicon-based anode materials suffer from severe volume expansion during cycling, resulting in poor cycle stability and rate performance.

Method used

Design an anode material that, by controlling its apparent density, true density, and total pore volume, satisfies the formula 10≤M≤20, where M=(ρ₂-ρ₁)/V. The anode material includes a carbon matrix and an active material, the active material being silicon, germanium, or tin, and possesses a porous structure and a coating layer. Optimize its structural stability and porosity.

Benefits of technology

It improves the structural stability of the anode material, reduces the volume expansion rate, enhances the capacity and initial coulombic efficiency, and improves cycle performance and lithium-ion transport efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005414084090000171
    Figure BDA0005414084090000171
  • Figure BDA0005414084090000181
    Figure BDA0005414084090000181
  • Figure BDA0005414084090000182
    Figure BDA0005414084090000182
Patent Text Reader

Abstract

This invention provides a negative electrode material and a battery. The negative electrode material comprises a carbon matrix and an active material, wherein the negative electrode material has pores, and the apparent density of the negative electrode material is ρ1 g / cm³. 3 The true density is ρ²g / cm³. 3 The total pore volume is V cm³. 3 / g, the anode material satisfies the following formula: M=(ρ2-ρ1) / V, 10≤M≤20. This application summarizes the parameters affecting the capacity, initial coulombic efficiency, and cycle performance of the anode material into a calculation formula for the comprehensive performance parameter M of the anode material. By adjusting and optimizing the relevant parameters in this calculation formula, the comprehensive performance parameter M of the anode material is kept within the above range, thereby enabling the anode material to simultaneously possess high initial reversible capacity, high initial coulombic efficiency, and excellent cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of negative electrode material technology, and more specifically, to a negative electrode material and a battery. Background Technology

[0002] In recent years, with market development, lithium-ion batteries have been widely used not only in mobile devices such as smartphones and laptops, but also in electric vehicles, power tools, and other fields. Developing lithium-ion batteries with higher energy density is a major current trend. The positive and negative electrode materials are the core of the battery, determining its working efficiency. Currently, the commercially available negative electrode material is graphite, whose capacity is already close to its theoretical limit, with limited room for further improvement. Therefore, there is an urgent need to develop a new generation of high-energy-density negative electrode materials.

[0003] Silicon-based anode materials are widely considered the next generation of battery anode materials, possessing advantages such as high capacity, abundant sources, and relative safety. However, silicon-based anode materials exhibit a severe volume expansion effect during cycling, causing pulverization and breakage, resulting in rapid cycle degradation. In existing technologies, carbon coating is typically used to reduce the volume expansion effect during cycling, which alleviates the volume expansion effect to some extent, but still suffers from insufficient cycle stability and poor rate performance, requiring further improvement and optimization. Summary of the Invention

[0004] The main objective of this invention is to provide a negative electrode material and a battery to solve the problems of high expansion rate and poor cycle stability of silicon-based negative electrode materials in the prior art.

[0005] To achieve the above objectives, according to one aspect of the present invention, a negative electrode material is provided, comprising a carbon matrix and an active material, wherein the negative electrode material has pores and the apparent density of the negative electrode material is ρ1g / cm³. 3 The true density is ρ²g / cm³. 3 The total pore volume is V cm³. 3 / g,

[0006] The negative electrode material satisfies the following formula: M=(ρ2-ρ1) / V, 10≤M≤20.

[0007] Furthermore, it satisfies at least one of the following technical features:

[0008] (1) The apparent density ρ1 of the negative electrode material satisfies: 1.2≤ρ1≤2.0;

[0009] (2) The true density ρ2 of the negative electrode material satisfies: 1.8≤ρ2≤2.2;

[0010] (3) The total pore volume V of the negative electrode material satisfies: 0.001≤V≤1.

[0011] Furthermore, the active material includes any one or a combination of two or more of silicon, germanium, and tin materials.

[0012] Furthermore, it satisfies at least one of the following technical features:

[0013] (1) The active material includes silicon material, and the mass percentage of silicon element in the negative electrode material is 30% to 65%;

[0014] (2) The mass content of carbon in the negative electrode material is 35% to 60%;

[0015] (3) The particle strength of the negative electrode material is 100MPa~1000MPa;

[0016] (4) The powder conductivity of the negative electrode material is ≥0.1S / cm.

[0017] Furthermore, it satisfies at least one of the following technical features:

[0018] (1) The particle size of the negative electrode material satisfies: 2μm≤Dn50≤10μm;

[0019] (2) The particle size of the negative electrode material satisfies: 0.8≤(Dn90-Dn10) / D50≤3;

[0020] (3) The specific surface area of ​​the negative electrode material is ≤100m² 2 / g;

[0021] (4) The average pore size of the pores in the negative electrode material is 0.5 nm to 20 nm.

[0022] Furthermore, the negative electrode material after removing the active material satisfies at least one of the following technical characteristics:

[0023] (1) The negative electrode material after removing the active material has pores, including at least one of micropores, mesopores and macropores;

[0024] (2) The negative electrode material after removing the active material has pores, including micropores, and the volume of micropores accounts for 55% to 95% of the total pore volume.

[0025] (3) The negative electrode material after removing the active material has pores, including mesopores, and the volume of mesopores accounts for 5% to 45% of the total pore volume.

[0026] (4) The negative electrode material after removing the active material has pores, including macropores, and the volume of macropores accounts for 0% to 5% of the total pore volume.

[0027] Furthermore, the negative electrode material after removing the active material satisfies at least one of the following technical characteristics:

[0028] (1) The powder conductivity of the negative electrode material after removing the active material is ≥0.3S / cm;

[0029] (2) The median particle size Dn50 of the negative electrode material after removing the active material is 2μm to 10μm;

[0030] (3) The particle strength of the negative electrode material after removing the active material is 50MPa~500MPa.

[0031] Furthermore, the carbon matrix has pores, with at least a portion of the active material located within the pores of the carbon matrix.

[0032] Furthermore, at least a portion of the surface of the negative electrode material has a coating layer with a thickness of 0 nm to 100 nm, and not 0 nm; and / or, the coating layer includes at least one of carbon, nitride, metal oxide, metal fluoride, metal oxyfluoride, and polymer.

[0033] To achieve the above objectives, according to one aspect of the present invention, a battery is provided comprising any of the aforementioned negative electrode materials.

[0034] Applying the technical solution of this invention, for negative electrode materials, when the above formula is satisfied, the negative electrode material exhibits strong structural stability, low volume expansion rate, and high capacity, high initial efficiency, and other properties. In the negative electrode material, the total pore volume V cm⁻¹ 3 / g refers to the unfilled space within the material. A larger V value indicates a larger reserved space within the negative electrode material, resulting in a more significant buffering effect against the expansion of active materials such as silicon. This helps reduce the volume expansion rate of the negative electrode material. However, an excessively large V value can lead to a decrease in the capacity of the negative electrode material, as well as a deterioration in its voltage resistance and a reduction in lithium-ion transport efficiency. Apparent density ρ1g / cm³ 3 The density is obtained by dividing the particle mass of the negative electrode material by the volume including internal pores, external defects, and the solid skeleton. For the negative electrode material of this application, the apparent density ρ1g / cm³ is... 3A higher apparent density allows for more negative electrode material to be packed into the limited space of the battery, improving energy density, enabling the battery to store more energy, and extending battery life. A suitable apparent density means the negative electrode material has good particle packing and pore structure, which is beneficial for the transport and diffusion of lithium ions during charging and discharging, thereby improving battery charging and discharging efficiency and reducing charging and discharging time. The apparent density of the negative electrode material is closely related to its structural stability. If the apparent density is too low, it may mean that the material has too many pores or a loose structure. During multiple charge-discharge cycles, the material is more prone to structural damage and pulverization, leading to a decrease in battery cycle life. True density ρ²g / cm³... 3 The density is obtained by dividing the mass of the negative electrode material particles by the volume excluding the internal and external pores of the particles. It is a density that is related to the total pore volume V cm³. 3 The standard value / g is irrelevant. For the negative electrode material of this application, since the density of the active material (such as silicon material) and the density of the carbon matrix are different, the value of ρ2 reflects the degree to which the carbon matrix is ​​filled by active material particles. The more the pores in the carbon matrix are filled by active material, the larger the true density ρ2 value of the negative electrode material will be, which is more conducive to improving the capacity and voltage resistance of the negative electrode material. However, it can also easily lead to excessive fit, or even interference fit, between the active material (such as silicon material) and the pore walls of the carbon matrix to which it is distributed. This is not conducive to providing buffer space for the expansion of the active material, which will lead to an increase in the volume expansion rate of the negative electrode material, thereby reducing the cycle performance of the negative electrode material.

[0035] This application considers the influence of apparent density, true density, and total pore volume of the negative electrode material, incorporating these three factors into the calculation formula for the comprehensive performance parameter M of the negative electrode material. The inventors discovered through research that when the negative electrode material satisfies the relationship 10≤M≤20, it exhibits characteristics such as high capacity, high initial coulombic efficiency, and excellent cycle performance, thus meeting application requirements. This application summarizes the parameters affecting the capacity, initial coulombic efficiency, and cycle performance of the negative electrode material into a calculation formula for the comprehensive performance parameter M. By adjusting and optimizing the relevant parameters in this formula, the comprehensive performance parameter M of the negative electrode material is kept within the aforementioned range, thereby enabling the negative electrode material to simultaneously possess high capacity, high initial coulombic efficiency, and excellent cycle performance. Detailed Implementation

[0036] It should be noted that, unless otherwise specified, the embodiments and features described in this application can be combined with each other. The present invention will now be described in detail with reference to the embodiments.

[0037] As analyzed in the background section of this application, existing technologies suffer from high expansion rates and poor cycle stability in silicon-based anode materials. To address this issue, this application provides an anode material and a battery.

[0038] According to a typical embodiment of this application, a negative electrode material is provided, comprising a carbon matrix and an active material, wherein the negative electrode material has pores; the apparent density of the negative electrode material is ρ1g / cm³. 3 The true density is ρ²g / cm³. 3 The total pore volume is V cm³. 3 / g, and the negative electrode material satisfies the following formula: M=(ρ2-ρ1) / V, 10≤M≤20.

[0039] For anode materials, when the above formula is satisfied, the anode material exhibits strong structural stability, low volume expansion rate, and high capacity and high initial efficiency. In the anode material, the total pore volume V cm⁻¹ 3 / g refers to the unfilled space within the material. A larger V value indicates a larger reserved space within the anode material, resulting in a more significant buffering effect against silicon expansion and reducing the volume expansion rate of the anode material. However, an excessively large V value can lead to a decrease in the anode material's capacity, as well as a deterioration in its voltage withstand performance and a reduction in lithium-ion transport efficiency. Apparent density ρ1g / cm³ 3 The density is obtained by dividing the particle mass of the negative electrode material by the volume including internal pores, external defects, and the solid skeleton. For the negative electrode material of this application, the apparent density ρ1g / cm³ is... 3 A higher apparent density allows for more negative electrode material to be packed into the limited space of the battery, improving energy density, enabling the battery to store more energy, and extending battery life. A suitable apparent density means the negative electrode material has good particle packing and pore structure, which is beneficial for the transport and diffusion of lithium ions during charging and discharging, thereby improving battery charging and discharging efficiency and reducing charging and discharging time. The apparent density of the negative electrode material is closely related to its structural stability. If the apparent density is too low, it may mean that the material has too many pores or a loose structure. During multiple charge-discharge cycles, the material is more prone to structural damage and pulverization, leading to a decrease in battery cycle life. True density ρ²g / cm³... 3 The density is obtained by dividing the mass of the negative electrode material particles by the volume excluding the internal and external pores of the particles. It is a density that is related to the total pore volume V cm³. 3The standard value / g is irrelevant. For the negative electrode material of this application, since the density of the active material (such as silicon) is different from that of carbon, the value of ρ2 reflects the degree to which the carbon matrix is ​​filled by the active material particles. The more the pores in the carbon matrix are filled by the active material, the larger the true density ρ2 value of the negative electrode material will be, which is more conducive to improving the capacity and voltage resistance of the negative electrode material. However, it can also easily lead to excessive fit, or even interference fit, between the active material (such as silicon) and the pore walls of the carbon matrix to which it is distributed. This is not conducive to providing buffer space for the expansion of the active material, which will lead to an increase in the volume expansion rate of the negative electrode material, thereby reducing the cycle performance of the negative electrode material.

[0040] This application considers the influence of apparent density, true density, and total pore volume of the negative electrode material, incorporating these three factors into the calculation formula for the comprehensive performance parameter M of the negative electrode material. The inventors discovered through research that when the negative electrode material satisfies the relationship 10≤M≤20, it exhibits characteristics such as high capacity, high initial coulombic efficiency, and excellent cycle performance, thus meeting application requirements. This application summarizes the parameters affecting the capacity, initial coulombic efficiency, and cycle performance of the negative electrode material into a calculation formula for the comprehensive performance parameter M. By adjusting and optimizing the relevant parameters in this formula, the comprehensive performance parameter M of the negative electrode material is kept within the aforementioned range, thereby enabling the negative electrode material to simultaneously possess high capacity, high initial coulombic efficiency, and excellent cycle performance.

[0041] Specifically, the M value of the negative electrode material can be 10, 10.5, 11, 11.5, 12, 12.5, 13, 14, 15, 16, 17, 18, 19, 20, or any value within the range of any two of the above values, and is not limited here. When the M value of the negative electrode material is less than 10, the porosity of the negative electrode material is too high, resulting in a low capacity. When the M value of the negative electrode material is greater than 20, the porosity of the negative electrode material is too low, making it unable to buffer the volume changes during the charging and discharging process, thus affecting the stability of the negative electrode material. Preferably, the M value of the negative electrode material is 14 to 16.

[0042] The apparent density of a negative electrode material refers to its density in its natural state, i.e., its density after long-term storage in air in a dry state. It is calculated by dividing the mass of each particle in the negative electrode material by the total volume of the particles; that is, the ratio of the mass to the apparent volume of the negative electrode material. The apparent volume includes the volume of internal pores, external defects, and the solid framework. The specific value of the apparent density ρ1 of the negative electrode material can be tested using existing techniques.

[0043] In some embodiments of this application, the apparent density ρ1 of the negative electrode material satisfies the following condition: 1.2 ≤ ρ1 ≤ 2.0. The apparent density ρ1 of the negative electrode material reflects the porosity and packing density of the material. The smaller the value of ρ1, the greater the porosity of the negative electrode material. This is beneficial for providing sufficient buffer space for the expansion of the active material (such as silicon), improving the material stability, but it also reduces the structural stability of the material. When the apparent density ρ1 of the negative electrode material is within the above range, the negative electrode material has a more suitable porosity, which is beneficial for better balancing the capacity and structural stability of the negative electrode material. Specifically, the value of the apparent density ρ1 can be any value within the range of 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, or any two of the above values, and is not limited here.

[0044] True density of negative electrode material ρ2g / cm³ 3 The density is calculated by dividing the mass of the negative electrode material particles by the volume excluding the voids inside and outside the particles, ρ²g / cm³. 3 The value reflects the degree to which the carbon matrix of the anode material is filled with active material. The more active material there is, the greater the true density of the anode material, which is beneficial to improving the specific capacity of the anode material. However, it is not conducive to providing sufficient buffer space for the expansion of the active material, thereby reducing the cycle stability of the anode material.

[0045] In some embodiments of this application, the true density ρ2 of the negative electrode material satisfies the following condition: 1.8 ≤ ρ2 ≤ 2.2. When the true density of the negative electrode material meets this range, the negative electrode material contains an appropriate amount of silicon material, which can better balance the specific capacity and cycle stability of the negative electrode material. Specifically, the true density ρ2 of the negative electrode material can be any value within the range of 1.8, 1.85, 1.9, 1.95, 2, 2.05, 2.1, 2.15, 2.2, or any two of the above values, without limitation. Preferably, the true density ρ2 of the negative electrode material is 2.0 to 2.1.

[0046] The total pore volume V cm of the negative electrode material 3 / g is a value related to apparent density, which refers to the unfilled space within the negative electrode material. A larger V value is beneficial for buffering the volume expansion of silicon, but an excessively large V value will reduce the material capacity and the particle strength of the material.

[0047] In some embodiments of this application, the total pore volume V of the negative electrode material satisfies: 0.001 ≤ V ≤ 1. Specifically, V can be any value within the range of 0.001, 0.005, 0.01, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 0.95, 1, or any two of the above values, and is not limited here. After the carbon matrix is ​​filled with silicon material, the remaining pores can reserve space for the volume expansion of the silicon material, mitigating the expansion effect of the negative electrode material, improving the cycle stability of the negative electrode material, and also adsorbing or containing a small amount of gas generated by the side reaction between the silicon material and the electrolyte, improving the gas generation phenomenon of the negative electrode material. This allows the negative electrode material to better balance structural stability and capacity, further improving the overall performance of the negative electrode material. The total pore volume measured in this application only includes open pores or partially permeable pores; closed pores are not included because they cannot be penetrated by the medium. As an example, a specific gravity meter and pore size analyzer (e.g., the Micron ASAP2460-2) can be used to calculate the total pore volume by analyzing the adsorption amount in the high-pressure region (P / P0 close to 1) using the adsorption isotherm. The testing process includes: 1) measuring the full-range adsorption isotherm (P / P0 from 0 to 0.99); 2) assuming the pores are filled with liquid adsorbate when P / P0≈0.99, converting the adsorption amount into pore volume (e.g., the liquid density of N2 is 0.808 g / cm³). 3 ).

[0048] In this application, the active material includes any one or a combination of two or more of silicon (Si), germanium (Ge), and tin (Sn). This application uses silicon as an example of an active material for illustration.

[0049] In some embodiments of this application, the particle size of the negative electrode material satisfies: 2μm ≤ Dn50 ≤ 10μm. Controlling the particle size of the negative electrode material within the above range ensures the time for lithium-ion insertion and extraction, allowing the negative electrode material to achieve a rapid and sufficient lithium insertion state, thereby ensuring the charge and discharge performance of the lithium-ion battery. Specifically, the particle size Dn50 of the negative electrode material is 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, or any value within the range of any two of the above values, and is not limited herein.

[0050] In some embodiments of this application, the particle size of the negative electrode material satisfies: 0.8 ≤ (Dn90 - Dn10) / Dn50 ≤ 3. Controlling the particle size of the negative electrode material within this range is beneficial to improving the cycle performance of the battery made from this negative electrode material. The value of (Dn90 - Dn10) / Dn50 (i.e., the particle size aggregation index PDI) of the negative electrode material can be any value within the range of 0.8, 1, 1.2, 1.4, 1.6, 1.8, 2, 2.2, 2.4, 2.6, 2.8, 3, or any two of the above values, and is not limited here. This means that the particle size distribution of the negative electrode material is more uniform, which helps to reduce the stress difference inside the negative electrode material, thereby reducing the interaction force between particles, reducing particle breakage and pulverization during cycling, and improving the cycle stability of the negative electrode material. In addition, the uniform particle size distribution helps to make the contact between the negative electrode material and the electrolyte more uniform, which helps to form a thinner and more stable SEI film, reduces electrolyte decomposition, and improves the electrochemical stability of the secondary battery.

[0051] In some embodiments of this application, the specific surface area of ​​the negative electrode material is ≤100m². 2 / g, specifically 1m 2 / g、3m 2 / g、5m 2 / g、8m 2 / g, 10m 2 / g、20m 2 / g、30m 2 / g、40m 2 / g, 50m 2 / g、60m 2 / g、70m 2 / g、80m 2 / g、90m 2 / g, 100m 2 / g or any value within the range of any two of the above values, without limitation. A specific surface area of ​​the negative electrode material within the above range can provide more insertion sites for lithium ions to increase the capacity of lithium-ion batteries, while reducing the contact area between the negative electrode material and the electrolyte, reducing the occurrence of side reactions between the negative electrode material and the electrolyte, and improving the cycle performance of batteries made from the negative electrode material.

[0052] In some embodiments of this application, the average pore size of the pores in the negative electrode material is 0.5 nm to 20 nm, specifically 0.5 nm, 1 nm, 3 nm, 5 nm, 7 nm, 9 nm, 11 nm, 13 nm, 15 nm, 17 nm, 19 nm, 20 nm, or any value within the range of any two of the above values, without limitation. It is understood that the average pore size of the negative electrode material is related to its surface density. Generally, a decrease in surface density, indicating an excessive number of micropores on the surface of the negative electrode material, will lead to a decrease in the average pore size. An average pore size within the above range indicates that the negative electrode material has a high surface density, which is beneficial for reducing the reaction between dissolved active materials, such as silicon, and the electrolyte, and reducing the gas production value.

[0053] In some embodiments of this application, the particle strength of the negative electrode material is 100 MPa to 1000 MPa. This enables the negative electrode material to have better structural stability, which is beneficial to further improving the cycle performance of the negative electrode material. Specifically, the particle strength of the negative electrode material can be any value within the range of 100 MPa, 200 MPa, 300 MPa, 400 MPa, 500 MPa, 600 MPa, 700 MPa, 800 MPa, 900 MPa, 1000 MPa, or any two of the above values, and is not limited herein.

[0054] In some embodiments of this application, the powder conductivity of the negative electrode material is ≥0.1 S / cm. Controlling the conductivity of the negative electrode material within the above range allows the negative electrode material to have better conductivity, which is beneficial to improving the overall performance of the battery including the negative electrode material. Specifically, the powder conductivity of the negative electrode material is any value within the range of 0.1 S / m, 0.5 S / m, 1 S / m, 2 S / m, 3 S / m, 4 S / m, 5 S / m, 6 S / m, 7 S / m, 8 S / m, 9 S / m, 10 S / m, or any combination of two of the above values, and is not limited herein.

[0055] In some embodiments of this application, the active material includes silicon, and the mass percentage of silicon in the anode material is 30% to 65%, specifically 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, or any value within the range of any two of the above values, without limitation herein. Controlling the silicon content in the anode material within the above range can better balance the specific capacity and stability of the anode material.

[0056] In some embodiments of this application, the silicon material includes at least one of elemental silicon, silicon oxide, and silicon alloy.

[0057] In some embodiments of this application, the silicon material includes elemental silicon, which includes at least one of crystalline silicon, amorphous silicon, and a composite of crystalline and amorphous silicon. Preferably, the elemental silicon includes amorphous silicon, which expands isotropically during lithium intercalation, reducing the collapse of the pore structure, suppressing rapid capacity decay, and improving the lithium intercalation cycle performance of the anode material.

[0058] In some embodiments of this application, the silicon material includes silicon oxide, the general formula of which is SiO. x Where 0.5 ≤ x < 2. Specifically, SiO x Specifically, it could be SiO 0.5 SiO 0.7 SiO 0.9 SiO, SiO 1.2 SiO 1.5 SiO 1.8 SiO 1.9 etc. are not specified here.

[0059] In some embodiments of this application, the silicon material includes silicon alloys, which may be at least one of silicon-lithium alloys, silicon-magnesium alloys, etc., and are not limited thereto.

[0060] In some embodiments of this application, the silicon material includes silicon particles and a silicon oxide layer located on the surface of the silicon particles. The silicon oxide layer includes silicon oxide, the general formula of which is SiO. x Where 0.5 ≤ x < 2. Specifically, SiO x Specifically, it could be SiO 0.5 SiO 0.7 SiO 0.9 SiO, SiO 1.2 SiO 1.5 SiO 1.8 SiO 1.9 etc. are not specified here.

[0061] In some embodiments of this application, the silicon material includes silicon particles and a silicon oxide layer on the surface of the silicon particles. The mass percentage of oxygen atoms in the silicon material, calculated as 100% of the silicon material, is 1% to 18%. Specifically, the mass percentage of oxygen atoms in the silicon material can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, or any value within the range of any two of the above values, and is not limited herein. Controlling the mass percentage of oxygen atoms in the silicon material within the above range is beneficial for forming a stable silicon oxide layer on the surface of the silicon particles, reducing direct contact between the silicon particles and the electrolyte, thereby reducing side reactions between the silicon particles and the electrolyte, and improving the cycle stability of the negative electrode material; it also ensures stable activity of the silicon material, increasing the specific capacity of the negative electrode material.

[0062] In some embodiments of this application, the carbon content in the negative electrode material is 35% to 60% by mass, specifically 35%, 40%, 42%, 45%, 48%, 50%, 52%, 55%, 58%, 60%, or any value within the range of any two of the above values, and is not limited herein. Controlling the carbon content in the negative electrode material within the above range is beneficial to improving the electron conductivity of the negative electrode material.

[0063] In some embodiments of this application, the carbon matrix has pores, with at least a portion of the silicon material located within these pores. Composite silicon material with a porous carbon matrix allows the carbon matrix to buffer volume changes in the silicon material. The carbon matrix also acts as a conductive network, maintaining good electronic conductivity within the negative electrode material. Furthermore, the reduced porosity of the carbon matrix after filling with silicon material can improve the specific capacity and energy density of the negative electrode material. It also effectively reduces the contact between the silicon material and the electrolyte, minimizing side reactions between the negative electrode material and the electrolyte, thus improving the cycle performance and cycle expansion resistance of the battery fabricated with the negative electrode material.

[0064] In some embodiments, the carbon matrix includes one or more of artificial graphite, natural graphite, amorphous carbon, activated carbon, mesophase carbon microspheres, carbon nanotubes, carbon nanofibers, and graphene.

[0065] The carbon matrix is ​​the portion remaining after removing the active material from the particles of the negative electrode material; that is, the negative electrode material after removing the active material. Taking silicon as the active material as an example, the method for removing the active material from the particles of the negative electrode material can be as follows: Under stirring, 150 mL of 20% HF acid solution is added dropwise to 10 g of negative electrode material. This will generate SiF4 and H2 gases and release heat. After no more gas is generated, the supernatant acid solution is removed by centrifugation. Another 150 mL of 20% HF solution is added to the negative electrode material, and the mixture is stirred for 12 h. The supernatant acid solution is removed again by centrifugation. Then, the negative electrode material is washed with pure water until neutral and dried to obtain the negative electrode material after removing the silicon material, i.e., the carbon matrix.

[0066] In some embodiments of this application, the negative electrode material after removing the active material has pores, including at least one of micropores, mesopores, and macropores. Specifically, micropores are pores with a diameter less than 2 nm, mesopores are pores with a diameter between 2 nm and 50 nm, and macropores are pores with a diameter greater than 50 nm.

[0067] In some embodiments of this application, the negative electrode material after removing the active material has pores, including micropores; the volume of the micropores accounts for 55% to 95% of the total pore volume. The pores of the negative electrode material after removing the active material are mainly micropores. This pore size distribution within this range helps in the deposition of active materials such as silicon during the deposition process, thereby improving the compactness of the negative electrode material.

[0068] In some embodiments of this application, the negative electrode material after removing the active material has pores, including mesopores; the volume of the mesopores accounts for 5% to 45% of the total pore volume.

[0069] In some embodiments of this application, the negative electrode material after removing the active material has pores, including macropores; the volume of the macropores accounts for 0% to 5% of the total pore volume.

[0070] Understandably, the volume ratio of micropores, mesopores, and macropores in the carbon matrix is ​​controlled within the above range. Since most of the pores in the carbon matrix are micropores, the size of the deposited silicon material can be adjusted, the dispersion uniformity of the carbon matrix and silicon material can be improved, the volume expansion of the silicon material can be reduced, and the cycle stability of the anode material can be enhanced.

[0071] For example, the above-mentioned methods for testing pore size and pore volume ratio can be as follows: The pore volume of a carbon matrix refers to the total pore volume per unit mass of carbon matrix material, which can be measured by gas adsorption. Nitrogen adsorption is a technique that characterizes the porosity and pore size distribution of a material by condensing gas within the pores of a solid. As the pressure increases, the gas first condenses in the pores with the smallest diameter, and the pressure increases until a saturation point is reached, at which point all pores are filled with liquid. Then the nitrogen pressure is gradually decreased to allow the liquid to evaporate from the system. Analysis of the adsorption and desorption isotherms allows for the determination of pore volume and pore size distribution, as well as the respective proportions of micropores, mesopores, and macropores in the total pore volume.

[0072] In some embodiments of this application, the powder conductivity of the negative electrode material after removing the active material is 0.3 S / cm to 10 S / cm. Specifically, it can be any value within the range of 0.3 S / cm, 0.5 S / cm, 1 S / cm, 1.5 S / cm, 2 S / cm, 3 S / cm, 4 S / cm, 5 S / cm, 6 S / cm, 7 S / cm, 8 S / cm, 9 S / cm, 10 S / cm, or any combination of the above values. No limitation is made herein. Controlling the powder conductivity of the negative electrode material after removing the active material within the above range is beneficial for improving the conductivity of the negative electrode material and further improving the overall performance of the battery including this negative electrode material.

[0073] In some embodiments of this application, the median particle size Dn50 of the negative electrode material after removing the active material is 2 μm to 10 μm. The median particle size of the negative electrode material after removing the active material is within the above range, which can ensure that the median particle size of the prepared negative electrode material is within a suitable range, so that the negative electrode material can achieve a state of rapid and sufficient lithium intercalation, thereby ensuring the charge and discharge performance of the battery.

[0074] In some embodiments of this application, the particle strength of the negative electrode material after removing the active material is 50 MPa to 500 MPa, which enables the negative electrode material to have better structural stability and is beneficial to further improving the cycle performance of the negative electrode material. Specifically, the particle strength of the negative electrode material after removing the active material is 50 MPa, 60 MPa, 65 MPa, 70 MPa, 80 MPa, 90 MPa, 100 MPa, 110 MPa, 120 MPa, 130 MPa, 140 MPa, 150 MPa, 200 MPa, 300 MPa, 400 MPa, 500 MPa, or any value within the range of any two of the above values, and is not limited herein.

[0075] In some embodiments of this application, at least a portion of the surface of the negative electrode material has a coating layer. The presence of the coating layer can effectively suppress the volume expansion of the negative electrode material, reduce structural damage to the negative electrode material during cycling, and also enhance the mechanical strength and compressive strength of the negative electrode material.

[0076] In some embodiments of this application, the thickness of the coating layer is 0 nm to 100 nm, and not 0 nm. Specifically, it can be 0.1 nm, 1 nm, 5 nm, 6 nm, 8 nm, 10 nm, 12 nm, 15 nm, 18 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, or 100 nm, etc., and is not limited here. In this application, controlling the coating layer thickness within the above range is beneficial to reducing the specific surface area of ​​the negative electrode material, reducing the occurrence of side reactions between the active material and the electrolyte, improving the safety of the negative electrode material, and improving the first coulombic efficiency of the negative electrode material. When the coating layer is too thin, the risk of contact between the active material and the outside environment increases, the active material is easily oxidized, or even spontaneously combustible, and the safety performance of the negative electrode material decreases. When the coating layer is too thick, the active ion transport efficiency in the electrolyte decreases, the interfacial impedance between the negative electrode material and the electrolyte increases, and the fast-charging performance of the negative electrode material decreases.

[0077] In some embodiments of this application, the coating layer includes at least one of carbon, nitride, metal oxide, metal fluoride, metal oxyfluoride, and polymer.

[0078] In some embodiments of this application, the coating layer may include lithium-ion-permeable carbon, which may include at least one of graphene, soft carbon, and hard carbon.

[0079] In some embodiments of this application, the coating layer may include a lithium-ion permeable nitride, which may include at least one of titanium nitride, vanadium nitride, cobalt nitride, nickel nitride, and carbon nitride.

[0080] In some embodiments of this application, the coating layer may include a lithium-ion-permeable metal oxide, which may include at least one of titanium oxide, aluminum oxide, lithium oxide, cobalt oxide, and vanadium oxide.

[0081] In some embodiments of this application, the coating layer may include aluminum oxide. In certain cases, oxides of other metals that naturally form a protective oxide layer on the surface may be used instead of aluminum oxide. These include, but are not limited to, titanium oxide (Ti), chromium oxide (Cr), tantalum oxide (Ta), niobium oxide (Nb), etc. Such oxide coatings can be deposited using a variety of oxide coating deposition techniques, including physical vapor deposition, chemical vapor deposition, magnetron sputtering, atomic layer deposition, microwave-assisted deposition, wet chemical deposition, etc.

[0082] For example, a metal oxide precursor in the form of a water-soluble salt can be added to a suspension of core particles (in water). The addition of an alkali (e.g., sodium hydroxide or amine) leads to the formation of a metal (M) hydroxide. The core particles suspended in the mixture then serve as nucleation sites for M-hydroxide precipitation. Once the core particles are coated with an M-hydroxide shell, they can be annealed to transform the hydroxide shell into a corresponding oxide layer, which then adheres well to the surface of the anode material.

[0083] In some embodiments of this application, the coating layer comprises a lithium-ion permeable metal fluoride or metal oxyfluoride. Examples of such metal fluoride materials include, but are not limited to: vanadium fluoride, vanadium oxyfluoride, iron fluoride, iron oxyfluoride, aluminum fluoride, aluminum oxyfluoride, titanium fluoride, titanium oxyfluoride, aluminum fluoride, aluminum oxyfluoride, zinc fluoride, zinc oxyfluoride, niobium fluoride, niobium oxyfluoride, tantalum fluoride, tantalum oxyfluoride, nickel fluoride, nickel oxyfluoride, magnesium fluoride, magnesium oxyfluoride, copper fluoride, copper oxyfluoride, manganese fluoride, and manganese oxyfluoride.

[0084] In some embodiments of this application, the coating layer comprises a polymer permeable to lithium ions.

[0085] In some embodiments of this application, the polymer layer is a conductive polymer. In other embodiments, the polymer is an electrically insulating polymer. Examples of lithium-ion permeable polymers include, but are not limited to, sulfonated polystyrene-grafted fluorinated ethylene propylene, sulfonated inorganic-organic hybrid polymers, partially fluorinated polystyrene, organically modified layered phosphonates, polyphenylene sulfide, polyether ether, polysaccharides, polyethylene glycol, and polyethylene oxide.

[0086] In some embodiments of this application, the coating layer may have several (two or more) layers of different or the same lithium-ion permeable material, including but not limited to lithium-ion permeable metal oxides, lithium-ion permeable metal fluorides, lithium-ion permeable carbon, and lithium-ion permeable polymers.

[0087] According to another typical embodiment of this application, a method for preparing the above-mentioned negative electrode material is provided. The method includes: mixing carbon material with an organic activator and an inorganic activator, heating to activate the mixture to obtain a carbon matrix, wherein the mass ratio of the organic activator to the inorganic activator is (0.1-10):1, and the mass ratio of the sum of the organic and inorganic activators to the carbon material is (1-5):1; depositing silicon into the carbon matrix framework to obtain a silicon-carbon composite precursor, wherein the flow rate of the silicon source for silicon deposition is 10 sccm to 500 sccm; and coating the silicon-carbon composite precursor with carbon to obtain the negative electrode material.

[0088] The anode material preparation method of this application employs both organic and inorganic activators in a specific ratio for activation and carbonization, precisely controlling the pore structure of the porous carbon material. The organic activator buffers the etching effect of the inorganic activator, resulting in a carbon matrix framework with a highly efficient micro-mesoporous structure. Further, through silicon deposition and carbon coating, the specific capacity and conductivity of the anode material are improved while simultaneously achieving suitable porosity and structural stability. The anode material prepared using this method has an M value in the range of 10–20, achieving superior structural stability and low volume expansion. This results in batteries containing the anode material of this application exhibiting high capacity, initial coulombic efficiency, and excellent cycle stability, among other electrochemical performance characteristics.

[0089] The preparation method will be described in detail below with reference to specific embodiments.

[0090] In some embodiments of this application, the carbon material includes at least one of hard carbon, soft carbon, graphite, mesophase carbon microspheres, activated carbon, porous carbon, carbon fiber, carbon gel, and mesoporous carbon. Through the activation and carbonization process of this application, the pore structure of these carbon materials can be precisely controlled under the combined action of organic and inorganic activators, resulting in a carbon matrix framework with a highly efficient micro-mesoporous structure.

[0091] In some embodiments of this application, the inorganic activator includes one or more of the following: sodium hydroxide, potassium hydroxide, carbon dioxide, potassium carbonate, sodium carbonate, phosphoric acid, zinc chloride, potassium chloride, potassium nitrate, potassium permanganate, potassium chromate, potassium ferrocyanide, potassium ferrocyanide, and potassium sulfate. These activators have a good etching effect on carbon materials and can significantly increase the porous structure of carbon materials.

[0092] In some embodiments of this application, the organic activator includes one or more of potassium acetate, sodium acetate, potassium oxalate, sodium oxalate, potassium citrate, sodium citrate, potassium sorbate, sodium sorbate, potassium diformate, sodium diformate, potassium lactate, and potassium aspartate, which can cooperate with the inorganic activator to effectively buffer the etching effect of the inorganic activator and better regulate the microporous structure of the carbon matrix framework.

[0093] Specifically, the mass ratio of organic activator to inorganic activator can be 0.1:1, 0.2:1, 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, or any value within the range of any two of the above values, and is not limited herein. Preferably, the mass ratio of organic activator to inorganic activator is (1 to 4):1.

[0094] The ratio of the combined mass of the organic and inorganic activators to the carbon material is 1 to 5:1, which has a significant effect on adjusting the porosity of the carbon material. Specifically, the ratio of the combined mass of the organic and inorganic activators to the carbon material is 1:1, 2:1, 3:1, 4:1, 5:1, or any value within the range of any two of the above values, and is not limited here.

[0095] In some embodiments of this application, in order to make the carbon material and the organic and inorganic activators more uniformly dispersed, and thus to form a more uniform microporous structure in the carbon matrix framework, the carbon material and the organic and inorganic activators are mixed by grinding for 1 to 2 hours.

[0096] In some embodiments of this application, in order to reduce the introduction of excessive oxides into the negative electrode material, the above-mentioned carbonization activation is carried out in an inert atmosphere. For example, the inert atmosphere can be one or more of nitrogen, helium, and neon. Preferably, the flow rate of the inert atmosphere is 0.1 to 1 L / min.

[0097] In some embodiments of this application, the carbonization activation temperature is 800–1000°C, specifically 800°C, 850°C, 900°C, 950°C, 1000°C, or any value within the range of any two of the above values, and is not limited herein. In some embodiments of this application, the carbonization activation time at the above temperature is 1–10 hours, specifically 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, or any value within the range of any two of the above values, and is not limited herein.

[0098] This application describes a method for combining silicon materials with a carbon matrix framework using chemical vapor deposition. The equipment used for silicon deposition can be selected from existing technologies; for example, it can be a CVD (Chemical Vapor Deposition) furnace or a fluidized bed. In some embodiments of this application, a plasma reactor is installed in the deposition equipment. A radio frequency (RF) plasma source is selected, and the RF electric field accelerates electrons to collide with gas molecules, generating highly reactive molecules that promote the decomposition of silanes. The silicon deposition is activated by controlling the RF power (50-1000W).

[0099] The silicon source flow rate is between 10 sccm and 500 sccm, specifically 10 sccm, 50 sccm, 100 sccm, 200 sccm, 300 sccm, 400 sccm, 500 sccm, or any value within the range of any two of the above values; no limitation is made here. Controlling the silicon source flow rate within the above range allows for the deposition of an appropriate amount of silicon in the anode material, and also ensures that the anode material has a suitable porosity, thereby improving cycle performance.

[0100] In some embodiments of this application, the silicon source used for silicon deposition may be silane or ethylsilane.

[0101] In some embodiments of this application, the silicon deposition temperature is 450 to 750°C, specifically 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, or any value within the range of any two of the above values, and is not limited herein.

[0102] In some embodiments of this application, the carrier gas for silicon deposition is an inert gas or nitrogen, wherein the inert gas can be helium, argon, etc. Preferably, the flow rate of the carrier gas is 50–1000 sccm. Preferably, the volume ratio of silicon source to carrier gas is 0.05–0.8.

[0103] In some embodiments of this application, the preparation method of the negative electrode material includes: placing a carbon matrix framework in a furnace, introducing a carrier gas at a flow rate of 50 to 1000 sccm, introducing a silicon source at a flow rate of 10 sccm to 500 sccm, and depositing at 450 to 750°C for 1 to 10 hours to obtain a silicon-carbon composite precursor.

[0104] The aforementioned silicon-carbon composite precursor was subjected to carbon coating treatment using a plasma reactor. A radio frequency (RF) plasma source was selected, and the electrons were accelerated to collide with gas molecules through the RF electric field, generating highly active molecules and promoting the coating of carbon source gas. By controlling the RF power (50-1000W), the deposition of carbon source gas was activated, which further optimized the apparent density, true density, and total pore volume of the silicon-carbon composite material, resulting in a negative electrode material with excellent cycle stability and low expansion rate.

[0105] In some embodiments of this application, a plasma reactor is used to assist in the carbon coating process. The plasma reactor is installed in a high-temperature coating device, where an RF electric field accelerates electrons to collide with gas molecules, generating highly reactive molecules. By controlling the RF power of the plasma reactor, the activation of gas molecules is accelerated, thereby improving the efficiency and quality of the coating. Preferably, the RF power of the plasma reactor is 50–1000 W.

[0106] In some embodiments of this application, the gaseous carbon source used in the carbon coating treatment includes at least one selected from acetylene, methane, propylene, benzene, ethanol, methanol, ethylene, propane, and butane. Preferably, the volume concentration of the gaseous carbon source is 40% to 60%. In some embodiments of this application, the flow rate of the gaseous carbon source is 0.1 L / min to 20 L / min, specifically 0.1 L / min, 1 L / min, 3 L / min, 5 L / min, 8 L / min, 10 L / min, 13 L / min, 15 L / min, 18 L / min, or 20 L / min, etc., and of course, other values ​​within the above range are also possible and are not limited here.

[0107] In some embodiments of this application, the carbon coating process includes: placing the precursor in a CVD coating furnace, introducing a carbon source gas that has been heated to 200-800°C in an inert gas atmosphere, and then introducing a carbon source gas activated by plasma. Coating is then performed continuously at a constant temperature, with the total coating time controlled by controlling the flow rate. Preferably, the carbon coating temperature is 200°C to 800°C, specifically 200°C, 300°C, 400°C, 500°C, 600°C, 700°C, 800°C, or any value within the range of any two of the above values, without limitation. In some embodiments of this application, the carbon coating time is 1 min to 800 min, specifically 1 min, 10 min, 50 min, 100 min, 200 min, 300 min, 400 min, 500 min, 600 min, 70 min, 800 min, or any value within the range of any two of the above values, without limitation.

[0108] According to another typical embodiment of this application, a negative electrode sheet is provided, which includes the negative electrode material described above.

[0109] Since the apparent density, true density and total pore volume of the negative electrode material provided in this application are within the above range, it can achieve better structural stability and lower volume expansion rate. Using it as a negative electrode material in a negative electrode sheet can enable the battery using the negative electrode sheet of this application to have high capacity, first coulombic efficiency and excellent cycle stability and other electrochemical performance.

[0110] According to another typical embodiment of this application, a battery is provided, which includes the aforementioned negative electrode. Due to the use of the aforementioned negative electrode, the battery of this application simultaneously possesses electrochemical performance such as high capacity, initial coulombic efficiency, and excellent cycle stability.

[0111] The beneficial effects that this application can achieve will be further illustrated below with reference to embodiments and comparative examples.

[0112] Example 1

[0113] (1) Hard carbon precursor, organic activator potassium acetate, and inorganic activator potassium hydroxide were ground and mixed at a mass ratio of 1:1:1 for 2 hours. The mixture was then activated by passing nitrogen gas through it at a flow rate of 10 L / min for 2 hours at an activation temperature of 900 °C. The carbon matrix skeleton was then obtained by acid washing and water washing.

[0114] (2) Place the carbon matrix framework in a CVD furnace, then introduce inert carrier gas nitrogen at a flow rate of 500 sccm, introduce silicon source silane gas at a flow rate of 250 sccm, turn on the radio frequency (RF) plasma source and control the RF power to 1000W, and deposit at 600℃ for 6h to obtain silicon-carbon composite precursor.

[0115] (3) Place the silicon-carbon composite precursor in a kiln, introduce acetylene gas, control the volume concentration of acetylene to 12%, the flow rate to 200 sccm, turn on the plasma equipment, set the power to 150W, heat treat at 700℃, keep warm for 4h, and obtain the negative electrode material.

[0116] Example 2

[0117] (1) Hard carbon, a carbon precursor, is ground and mixed with potassium citrate (an organic activator) and potassium hydroxide (an inorganic activator) at a mass ratio of 1:2:1 for 1 h. The mixture is then activated by passing nitrogen gas through it at a flow rate of 10 L / min for 1.5 h at an activation temperature of 900 °C. The carbon matrix framework is then obtained by acid washing and water washing.

[0118] (2) The carbon matrix framework is placed in a CVD furnace, and then inert carrier argon is introduced at a flow rate of 400 sccm, and silicon source silane is introduced at a flow rate of 300 sccm. The silicon-carbon composite precursor is obtained by deposition at 600℃ for 4 hours.

[0119] (3) Place the silicon-carbon composite precursor in a kiln, introduce propane gas, control the volume concentration of propane to 10%, the flow rate to 300 sccm, turn on the plasma equipment, set the power to 150W, heat treat at 600℃, keep warm for 5h, and obtain the negative electrode material.

[0120] Example 3

[0121] (1) Amorphous carbon precursor, organic activator potassium acetate, and inorganic activator phosphoric acid are ground and mixed at a mass ratio of 1:3:1 for 1 h. The mixture is then activated by passing nitrogen gas through it at a flow rate of 10 L / min for 1 h at an activation temperature of 800 °C. The carbon matrix framework is then obtained by acid washing and water washing.

[0122] (2) The carbon matrix framework is placed in a CVD furnace, and then inert carrier gas nitrogen is introduced at a flow rate of 600 sccm, and silicon source silane gas is introduced at a flow rate of 300 sccm. The mixture is deposited at 700℃ for 3 hours to obtain the composite precursor.

[0123] (3) Place the silicon-carbon composite precursor in a kiln, introduce methane gas, control the volume concentration of methane to be 15%, the flow rate to be 250 sccm, turn on the plasma equipment, set the power to 150W, heat treat at 700℃, keep warm for 2h, and obtain the negative electrode material.

[0124] Example 4

[0125] (1) The carbon precursor soft carbon, organic activator potassium sorbate, and inorganic activator sodium hydroxide were ground and mixed at a mass ratio of 1:1:2 for 1.5 h. The mixture was then activated by passing nitrogen gas through it at a flow rate of 10 L / min for 1 h at an activation temperature of 850 °C. The carbon matrix framework was then obtained by acid washing and water washing.

[0126] (2) The carbon matrix framework is placed in a CVD furnace, and then inert carrier gas nitrogen is introduced at a flow rate of 600 sccm, and silicon source silane gas is introduced at a flow rate of 350 sccm. The carbon matrix is ​​deposited at 500℃ for 3 hours to obtain the silicon-carbon composite precursor.

[0127] (3) Place the silicon-carbon composite precursor in a kiln, introduce ethylene gas, control the volume concentration of ethylene to 8%, the flow rate to 350 sccm, turn on the plasma equipment, set the power to 150W, heat treat at 500℃, keep warm for 8h, and obtain the negative electrode material.

[0128] Example 5

[0129] (1) Hard carbon, a carbon precursor, is ground and mixed with potassium oxalate (organic activator) and zinc chloride (inorganic activator) at a mass ratio of 1:1:3 for 2 hours. The mixture is then activated by passing nitrogen gas through it at a flow rate of 10 L / min for 1 hour at an activation temperature of 800 °C. The carbon matrix framework is then obtained by acid washing and water washing.

[0130] (2) The carbon matrix framework is placed in a CVD furnace, and then inert carrier argon gas is introduced at a flow rate of 700 sccm, and silicon source silane gas is introduced at a flow rate of 150 sccm. The silicon-carbon composite precursor is obtained by deposition at 700℃ for 5 hours.

[0131] (3) Place the silicon-carbon composite precursor in a kiln, introduce acetylene gas, control the volume concentration of acetylene to 15%, the flow rate to 250 sccm, turn on the plasma equipment, set the power to 150W, heat treat at 800℃ for 3 hours, and obtain the negative electrode material.

[0132] Example 6

[0133] (1) The carbon precursor soft carbon was ground and mixed with organic activator potassium lactate and inorganic activator potassium ferricyanide at a mass ratio of 1:1:1 for 2 hours. Then the mixture was activated by passing nitrogen gas at a flow rate of 10 L / min for 3 hours at an activation temperature of 800℃. The carbon matrix framework was then obtained by acid washing and water washing.

[0134] (2) The carbon matrix framework is placed in a CVD furnace, and then inert carrier gas nitrogen is introduced at a flow rate of 600 sccm, and silicon source silane gas is introduced at a flow rate of 500 sccm. The silicon-carbon composite precursor is obtained by deposition at 700℃ for 2 hours.

[0135] (3) Place the silicon-carbon composite precursor in a kiln, introduce propane gas, control the volume concentration of acetylene to 8%, the flow rate to 400 sccm, turn on the plasma equipment, set the power to 150W, heat treat at 800℃, keep warm for 5h, and obtain the negative electrode material.

[0136] Example 7

[0137] (1) The carbon precursor graphitized carbon was ground and mixed with organic activator potassium acetate and inorganic activator potassium permanganate at a mass ratio of 1:1:4 for 2 hours. Then the mixture was activated by passing nitrogen inert gas through it for 1 hour at an activation temperature of 900℃. The carbon matrix skeleton was then obtained by acid washing and water washing.

[0138] (2) The carbon matrix framework is placed in a CVD furnace, and then inert carrier gas nitrogen is introduced at a flow rate of 500 sccm, and silicon source silane gas is introduced at a flow rate of 500 sccm. The silicon-carbon composite precursor is obtained by deposition at 800℃ for 3 hours.

[0139] (3) Place the silicon-carbon composite precursor in a kiln, introduce ethylene gas, control the volume concentration of ethylene to 20%, turn on the plasma equipment, set the power to 150W, heat treat at 800℃, keep warm for 1h, and obtain silicon-carbon anode material.

[0140] Example 8

[0141] (1) Hard carbon precursor, organic activator potassium acetate, and inorganic activator potassium hydroxide are ground and mixed at a mass ratio of 1:1:1 for 2 hours. The mixture is then activated by purging nitrogen gas for 2 hours at an activation temperature of 900°C. The carbon matrix framework is then obtained by acid washing and water washing.

[0142] (2) The carbon matrix framework is placed in a CVD furnace, and then inert carrier gas nitrogen is introduced at a flow rate of 500 sccm, and silicon source silane gas is introduced at a flow rate of 500 sccm. The silicon-carbon composite precursor is obtained by deposition at 600℃ for 6 hours.

[0143] (3) Place the silicon-carbon composite precursor in a kiln, introduce acetylene gas, control the volume concentration of acetylene to 12%, the flow rate to 320 sccm, turn on the plasma equipment, set the power to 150W, heat treat at 700℃, keep warm for 4h, and obtain silicon-carbon anode material.

[0144] Example 9

[0145] (1) The carbon precursor graphitized carbon was ground and mixed with organic activator potassium acetate and inorganic activator potassium permanganate at a mass ratio of 1.2:0.8:4 for 2 hours. Then the mixture was activated by passing nitrogen inert gas through it for 0.5 hours at an activation temperature of 850°C. The carbon matrix framework was then obtained by acid washing and water washing.

[0146] (2) The carbon matrix framework is placed in a CVD furnace, and then inert carrier gas nitrogen is introduced at a flow rate of 600 sccm, and silicon source silane gas is introduced at a flow rate of 500 sccm. The silicon-carbon composite precursor is obtained by deposition at 800℃ for 2 hours.

[0147] (3) Place the silicon-carbon composite precursor in a kiln, introduce ethylene gas, control the volume concentration of ethylene to 20%, the flow rate to 150 sccm, turn on the plasma equipment, set the power to 150W, heat treat at 700℃, keep warm for 2 hours, and obtain silicon-carbon anode material.

[0148] Comparative Example 1

[0149] The difference from Example 1 is that in step (1), the mass ratio of the carbon precursor hard carbon to the organic activator potassium acetate and the inorganic activator potassium hydroxide is 1:5:2.

[0150] Comparative Example 2

[0151] The difference from Example 1 is that in step (1), the mass ratio of the carbon precursor hard carbon to the organic activator potassium acetate and the inorganic activator potassium hydroxide is 1:0.5:0.2.

[0152] Comparative Example 3

[0153] The difference from Example 1 is that in step (2), silicon source silane gas is introduced at a flow rate of 5 sccm.

[0154] Comparative Example 4

[0155] The difference from Example 1 is that no plasma device was used for deposition in step (1).

[0156] Comparative Example 5

[0157] The only difference from Example 1 is that the organic activator potassium acetate was not added in step (1).

[0158] Comparative Example 6

[0159] The only difference from Example 1 is that in step (3): the silicon-carbon composite precursor is placed in a kiln, acetylene gas is introduced, the volume concentration of acetylene is controlled to be 12%, and the temperature is raised to 700°C for gas phase carbon coating for 4 hours to obtain the negative electrode material.

[0160] The anode materials prepared in the above embodiments and comparative examples were tested for basic indicators and electrochemical performance according to the following methods, and the test results are listed in Tables 1-3. The anode material after removing silicon was prepared as follows: Under stirring, 150 mL of 20% HF acid solution was added dropwise to 10 g of anode material, which generated SiF4 and H2 gases and released heat. After no more gas was generated, the supernatant acid solution was removed by centrifugation. Another 150 mL of 20% HF solution was added to the anode material, and after stirring for 12 h, the supernatant acid solution was removed by centrifugation again. The anode material was then washed with pure water until neutral and dried to obtain the anode material after removing silicon.

[0161] (1) True density (ρg / cm³) 3 Test: The true density of the material shall be tested in accordance with the test method in Appendix D of GB / T 24533-2019.

[0162] (2) Specific surface area, average pore size, proportion of micropores, mesopores, and macropores, and total pore volume (V cm³) of the anode material or the anode material after removing silicon. 3 / g) Test: Measurements were performed according to GB / T 7702.20-2008 using a Mack ASAP2460 multi-station extended fully automated specific surface area and porosity analyzer (USA). At liquid nitrogen temperature, the equilibrium adsorption amount of nitrogen on an object's surface is related to its pore size and other characteristics. Combining the law of adsorption amount changing with relative pressure during the adsorption process, various models can be fitted to calculate the pore size. The software-generated report uses density functional theory (DFT) to calculate the specific surface area, pore size distribution, specific pore volume, and pore volume within a certain range.

[0163] (3) Apparent density: The apparent density of the material was determined using a QL-2106AB apparent density meter and the gas displacement volume method.

[0164] (4) Test method for silicon content of negative electrode material: After drying the sample overnight, place it in a corundum crucible and place the crucible in a muffle furnace (Nanyang Xinyu SA2-9-17TP) at 1200℃ for 480 minutes to complete the combustion of carbon and the oxidation reaction of silicon or silicon suboxide to silicon dioxide; during the process, record the weight of the crucible m0, the weight of the sample m1, and the total weight of the crucible and product after ignition m2, and calculate the silicon content according to the following formula: Si%=(m2-m0) / m1×28.09 / 60.09×100%.

[0165] (5) Test method for carbon content of negative electrode material: Using the German Bruker / German Airt infrared carbon-sulfur analyzer G4 ICARUS HF / CS-i, the sample is burned in a high temperature and oxygen-rich state. The carbon element contained therein is oxidized into carbon dioxide and enters the infrared detector with the carrier gas. The mass content of carbon element is quantitatively calculated by statistically analyzing the change in the intensity of the infrared absorption wavelength of the carbon dioxide signal.

[0166] (6) Test methods for particle size and particle size aggregation index of anode material or anode material after silicon removal: The particle size test method refers to GB / T 19077-2016. The cumulative particle size distribution of the anode material is determined by measuring the particle size distribution using a Malvern laser particle size analyzer (Mastersizer3000) and laser diffraction method.

[0167] The median particle size Dn50 represents the particle size at which the cumulative number distribution percentage of the negative electrode material reaches 50% when the particle sizes are arranged in ascending order. The particle size Dn90 represents the particle size at which the cumulative number distribution percentage of the negative electrode material reaches 90% when the particle sizes are arranged in ascending order. The particle size aggregation index PDI = (Dn90 - Dn10) / Dn50.

[0168] (7) Test method for average particle size of material: observe the particles of material by field emission scanning electron microscope or transmission electron microscope, randomly measure the particle size of 5 to 10 material particles by scale bar, and take the average particle size as the final average particle size of material.

[0169] (8) Coating thickness: The average coating thickness is obtained by cross-sectioning the material using FIB-SEM equipment and measuring it in SEM.

[0170] (9) Test method for powder conductivity of negative electrode material or negative electrode material after removing silicon material: The resistance of the powder at a pressure of 20KN was measured by using the MCP-PD51 powder conductivity tester of Mitsubishi Chemical, Japan, and the four-probe method to determine the volume resistivity of the sample. Finally, the powder conductivity of the powder was calculated by the instrument program.

[0171] (10) Test method for particle strength of negative electrode material or negative electrode material after removal of active material: Use a single particle strength tester to apply vertical pressure to a single particle until the particle breaks, and record the maximum force at the time of breakage. (11) Electrochemical performance test: Mix the negative electrode material and superP, LA133 in a ratio of 70:15:15 to form a slurry and coat it evenly on copper foil. After drying, prepare the electrode sheet, assemble it into a coin cell, and test its electrochemical performance on the Blue Battery Test Cabinet M340A.

[0172] The negative electrode materials prepared in the above examples and comparative examples were mixed with super P and LA133 in a ratio of 70:15:15 in the same way to form a slurry, which was then uniformly coated onto copper foil. After drying, the slurry was prepared into an electrode sheet, assembled into a button cell, and tested on the Blue Battery Test Cabinet M340A. The test results are listed in Table 3.

[0173] The test method for the first reversible capacity is as follows: The negative electrode material is assembled into a button cell and tested on the Blue Battery Test Cabinet M340A. The voltage window and charge / discharge current are set, and the first discharge capacity is obtained as the first reversible capacity.

[0174] The test method for 50-cycle expansion rate is as follows: Assemble the negative electrode material into a soft-pack battery, let the assembled battery stand for a period of time (e.g., 12 hours) to allow the electrolyte to fully wet the electrodes, and then perform a cycle test on the Blue Battery Test Cabinet M340A. Record the thickness of the electrode sheet before and after the cycle to obtain the 50-cycle expansion rate.

[0175] The test method for 50-cycle retention rate is as follows: Assemble the negative electrode material into a pouch battery, let the assembled battery stand for a period of time (e.g., 12 hours) to allow the electrolyte to fully wet the electrodes, and then perform cycle tests on the Blue Battery Test Cabinet M340A. Record the charge and discharge capacity before and after the cycle to obtain the 50-cycle retention rate.

[0176] Table 1

[0177]

[0178]

[0179] Table 2

[0180]

[0181] Table 3

[0182]

[0183]

[0184] Table 1-3 lists the performance parameters of the anode materials prepared in each embodiment and comparative example. As can be seen from the table, by controlling the ratio of organic activator to inorganic activator to carbon precursor during the preparation process, parameters such as the pore volume / pore size of the carbon matrix and the volume concentration of the silicon source gas can be controlled, resulting in an M value of the prepared anode material within the range of 10–20. When the M value of the prepared anode material is within the range of 10–20, the anode material exhibits a low expansion rate, along with excellent cycle performance and a high first-efficiency coulombic efficiency. When the M value is too low, the anode material has a low capacity and poor cycle stability, significantly limiting its application. When the M value is too high, the first-efficiency coulombic efficiency of the anode material decreases.

[0185] By comparing Example 1 and Comparative Example 1, it can be concluded that an excessively high ratio of organic to inorganic activators will intensify the etching of carbon materials, resulting in a larger pore volume of the carbon matrix framework. Although this provides a larger buffer space for the expansion of silicon materials, thereby reducing the volume expansion rate of the anode material, it also reduces the initial efficiency of the anode material.

[0186] By comparing Example 1 and Comparative Example 2, it can be concluded that an excessively low ratio of organic activator to inorganic activator will result in a light etching degree of carbon material, a small pore volume of carbon matrix framework, and thus a small amount of silicon deposition, which reduces the capacity of the anode material. At the same time, due to the small expansion space of silicon material, the volume expansion of the anode material increases and the stability decreases.

[0187] By comparing Example 1 and Comparative Example 3, it can be concluded that the decrease in silane concentration, while the time remains unchanged, leads to a decrease in the silicon content deposited in the carbon matrix, an increase in the total pore volume, and a decrease in the apparent density and true density. Although this provides more expansion space for the anode material, resulting in a decrease in the expansion rate of the anode material and an enhancement in cycle performance, it also leads to a significant decrease in the capacity of the prepared silicon-based anode material.

[0188] By comparing Example 1 and Comparative Example 4, it was found that the deposition was not carried out using a plasma device, resulting in lower deposition efficiency, lower silicon content deposited in the carbon matrix framework, increased total pore volume, and decreased apparent density and true density, which led to a decrease in the capacity of the silicon-based anode material.

[0189] The test data from Example 1 and Comparative Example 5 show that without the addition of an inorganic activator, the pores in the negative electrode material are too few, the true density is too high, resulting in a low M value, insufficient capacity of the negative electrode material, low cycle retention rate, and increased expansion rate, making it difficult to meet the requirements of the battery.

[0190] The test data from Example 1 and Comparative Example 6 show that the traditional coating method has low coating efficiency, large pore volume and apparent density in the negative electrode material, resulting in a low M value, insufficient capacity of the negative electrode material, low cycle retention rate, and increased expansion rate, which makes it difficult to meet the requirements of the battery.

[0191] The apparent densities of Examples 2 and 4 meet the requirements of both exclusive and subordinate claims. Compared with other examples, the material can maximize its performance, maintaining both higher capacity and sufficient pore volume to buffer volume expansion during cycling and maintain the material's cycling performance.

[0192] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A negative electrode material, characterized in that, It includes a carbon matrix and an active material, wherein the negative electrode material has pores; The apparent density of the negative electrode material is ρ1g / cm³. 3 The true density is ρ²g / cm³. 3 The total pore volume is V cm³. 3 / g, The negative electrode material satisfies the following formula: M=(ρ2-ρ1) / V, 10≤M≤20.

2. The negative electrode material according to claim 1, characterized in that, It meets at least one of the following technical features: (1) The apparent density ρ1 of the negative electrode material satisfies: 1.2≤ρ1≤2.0; (2) The true density ρ2 of the negative electrode material satisfies: 1.8 ≤ ρ2 ≤ 2.2; (3) The true density ρ2 of the negative electrode material satisfies: 2.0 ≤ ρ2 ≤ 2.1; (4) The total pore volume V of the negative electrode material satisfies: 0.001≤V≤1; (5) The value of M in the negative electrode material is 14 to 16; (6) The value of M in the negative electrode material is 10 to 14; (7) The value of M in the negative electrode material is 16 to 20.

3. The negative electrode material according to claim 1, characterized in that, The active material includes any one or a combination of two or more of silicon, germanium and tin.

4. The negative electrode material according to claim 1, characterized in that, It meets at least one of the following technical features: (1) The active material includes silicon material, and the mass percentage of silicon element in the negative electrode material is 30% to 65%; (2) The carbon content in the negative electrode material is 35% to 60% by mass; (3) The particle strength of the negative electrode material is 100MPa to 1000MPa; (4) The powder conductivity of the negative electrode material is ≥0.1S / cm.

5. The negative electrode material according to claim 1, characterized in that, It meets at least one of the following technical features: (1) The particle size of the negative electrode material satisfies: 2μm≤Dn50≤10μm; (2) The particle size of the negative electrode material satisfies: 0.8≤(Dn90-Dn10) / Dn50≤3; (3) The specific surface area of ​​the negative electrode material is ≤100m² 2 / g; (4) The average pore size of the pores in the negative electrode material is 0.5 nm to 20 nm.

6. The negative electrode material according to claim 1, characterized in that, The negative electrode material after removing the active material satisfies at least one of the following technical characteristics: (1) The negative electrode material after removing the active material has pores, the pores including at least one of micropores, mesopores and macropores; (2) The negative electrode material after removing the active material has pores, including micropores, and the volume of the micropores accounts for 55% to 95% of the total pore volume; (3) The negative electrode material after removing the active material has pores, the pores including mesopores, and the volume of the mesopores accounts for 5% to 45% of the total pore volume; (4) The negative electrode material after removing the active material has pores, including macropores, and the volume of the macropores accounts for 0% to 5% of the total pore volume.

7. The negative electrode material according to claim 1, characterized in that, The negative electrode material after removing the active material satisfies at least one of the following technical characteristics: (1) The powder conductivity of the negative electrode material after removing the active material is ≥0.3 S / cm; (2) The median particle size Dn50 of the negative electrode material after removing the active material is 2μm to 10μm; (3) The particle strength of the negative electrode material after removing the active material is 50MPa to 500MPa.

8. The negative electrode material according to claim 1, characterized in that, The carbon matrix has pores, and at least a portion of the active material is located within the pores of the carbon matrix.

9. The negative electrode material according to claim 1, characterized in that, At least a portion of the surface of the negative electrode material has a coating layer, the thickness of which is 0 nm to 100 nm and is not 0 nm; and / or, the coating layer comprises at least one of carbon, nitride, metal oxide, metal fluoride, metal oxyfluoride and polymer.

10. A battery, characterized in that, Includes the negative electrode material as described in any one of claims 1 to 9.