Secondary particle graphite negative electrode material, negative electrode sheet, and electric device
By preparing secondary granular graphite anode materials with high tap density and smooth surface, the shortcomings of graphite anode materials in tap density and processing performance are solved, the cycle performance and safety of batteries are improved, and more efficient electrode processing and electrochemical performance are achieved.
Patent Information
- Application Number
- CN202610713266.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2025-05-22
- Filing Date
- 2026-05-22
- Publication Date
- 2026-11-24
AI Technical Summary
Existing graphite anode materials have shortcomings in tap density and processing performance, which limits the improvement of battery performance, especially poor cycle performance and high-temperature performance.
A secondary particulate graphite anode material is provided. By controlling the relationship between its tap density, oil absorption value and particle crush strength, the material is ensured to have a smooth surface while maintaining a high tap density. Mechanical shaping and graphitization treatment are used to improve the particle strength and processing performance.
It improves the stability and electrochemical performance of electrode processing, reduces the risk of copper foil breakage, enhances battery cycle performance and energy density, reduces side reactions and lithium consumption, and strengthens safety performance.
Smart Images

Figure CN123162192A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery technology, and in particular to secondary particulate graphite anode materials, anode sheets, and electrical equipment. Background Technology
[0002] Currently, the main structural designs for graphite anode materials include single-particle, secondary-particle, and composite structures of these two types. Single-particle graphite anode materials exhibit poor isotropy, resulting in inferior expansion and fast-charging performance, but they offer good cycle and high-temperature performance, and a relatively high tap density, typically less than 1.30 g / cc. Secondary-particle graphite anode materials possess isotropy, offering advantages in lithium-ion intercalation, fast charging, and expansion, but their lower tap density makes the slurry preparation process more difficult, and the lower solids content also increases production costs; the tap density of secondary-particle graphite anode materials is typically less than 1.10 g / cc. With increasing market demands for extreme battery performance and pushing the limits of battery design, the requirements for the tap density of graphite anode materials are further increasing.
[0003] Improvements in material properties have a direct impact on the cycle life, rate capability, and energy density of lithium-ion batteries. Further increasing the tap density of secondary granular graphite anode materials can not only improve the processing performance of the anode, reduce the difficulty of processing and storing the anode slurry, and reduce the rolling pressure of the electrode sheet, thereby reducing the risk of copper foil breakage, but also improve the yield and electrical performance of the battery, especially the cycle performance of the battery.
[0004] In view of this, this invention is hereby proposed. Summary of the Invention
[0005] The primary objective of this invention is to provide a secondary particulate graphite anode material with high tap density.
[0006] The second objective of this invention is to provide a negative electrode.
[0007] A third objective of this invention is to provide a lithium-ion battery.
[0008] The fourth objective of this invention is to provide an electrical device.
[0009] In order to achieve the above-mentioned objectives of the present invention, the following technical solution is adopted: In a first aspect, the present invention provides a secondary particle graphite anode material, wherein the tap density of the secondary particle graphite anode material is ≥1.10 g / cc; the secondary particle graphite anode material satisfies the following relationship: ρ t ×L o ≤55.0; where ρ tL is the tap density of the secondary particulate graphite anode material, expressed in g / cc. o The oil absorption value of the secondary particulate graphite anode material is expressed in mL / 100g.
[0010] Furthermore, the tap density of the secondary particulate graphite anode material is 1.3~1.5 g / cc.
[0011] Furthermore, the secondary particulate graphite anode material includes a plurality of secondary graphite particles, each of which includes a plurality of primary graphite particles and a graphitic material for bonding the plurality of primary graphite particles.
[0012] Furthermore, 40.0 ≤ ρ t ×L o ≤50.0.
[0013] Furthermore, the oil absorption value of the secondary particulate graphite anode material is ≤50mL / 100g.
[0014] Furthermore, the secondary particle graphite anode material satisfies the following relationship: ρ t ×L o ÷P cs ≤1.83; where ρ t L is the tap density of the secondary particulate graphite anode material, expressed in g / cc. o The oil absorption value of the secondary particulate graphite anode material is expressed in mL / 100g; P cs The compressive strength of the secondary granular graphite anode material is expressed in MPa.
[0015] Furthermore, 0 < ρ t ×L o ÷P cs ≤0.83.
[0016] Furthermore, the compressive strength of the secondary granular graphite anode material is ≥30MPa.
[0017] Furthermore, the compressive strength of the secondary granular graphite anode material is ≥60MPa.
[0018] Furthermore, the oil absorption value of the secondary particulate graphite anode material is ≤50mL / 100g.
[0019] Furthermore, the particle size Dv50 of the secondary particulate graphite anode material is 7~23μm.
[0020] Furthermore, the secondary particulate graphite anode material does not contain an amorphous carbon coating layer.
[0021] Secondly, the present invention also provides a negative electrode sheet, comprising the secondary particulate graphite negative electrode material as described above, or the secondary particulate graphite negative electrode material obtained according to the above preparation method.
[0022] Thirdly, the present invention also provides a lithium-ion battery, including the negative electrode sheet as described above.
[0023] Fourthly, the present invention also provides an electrical device, including the lithium-ion battery described above.
[0024] Compared with the prior art, the beneficial effects of the present invention are as follows: The secondary particulate graphite anode material of the present invention has a high tap density. When used for electrode processing, it can not only effectively reduce the amount of binder added during the pulping process, but also the high tap material stacking state helps to reduce the rolling pressure of the electrode, thereby reducing the risk of copper foil breakage and making electrode processing easier. At the same time, the expansion rate of the electrode can also be effectively reduced, which is beneficial to improving the electrochemical performance of the battery, especially the cycle performance.
[0025] The secondary particulate graphite anode material of the present invention has a high tap density, satisfying the relationship that the value of tap density × oil absorption value ≤ 55.0 and the value of tap density × oil absorption value ÷ particle crushing strength ≤ 1.83; thus, the secondary particulate graphite anode material has a high tap density while the particle surface is relatively smooth and the particle firmness is high; thereby possessing both excellent processing performance and electrochemical performance. Attached Figure Description
[0026] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation of the scope. For those skilled in the art, other related drawings can be obtained from these drawings without creative effort.
[0027] Figure 1 This is a diagram showing the changes in particle morphology before and after the particle crushing strength test of this invention.
[0028] Figure 2 This is the crushing force curve and reading points for the particle crushing strength of this invention.
[0029] Figure 3 This is a schematic flowchart of the preparation method of the secondary particulate graphite anode material of the present invention.
[0030] Figure 4 This is a SEM image of the secondary particulate anode material of Embodiment 1 of the present invention, magnified 2000 times.
[0031] Figure 5This is a SEM image of the secondary particulate anode material of Embodiment 1 of the present invention, magnified 1000 times.
[0032] Figure 6 This is a 500x SEM image of the secondary particulate anode material of Embodiment 1 of the present invention.
[0033] Figure 7 This is a SEM image of the secondary particulate anode material of Comparative Example 1 of the present invention, magnified at 2000x.
[0034] Figure 8 This is a SEM image of the secondary particulate anode material of Comparative Example 1 of the present invention, magnified 1000 times.
[0035] Figure 9 This is a 500x SEM image of the secondary particulate anode material of Comparative Example 1 of the present invention.
[0036] Figure 10 The particle size distribution diagrams are for the secondary particulate anode materials of Embodiment 1 and Comparative Example 1 of the present invention.
[0037] Figure 11 This is a particle size distribution diagram of the secondary particulate anode materials of Embodiment 1 and Comparative Example 1 of the present invention. Detailed Implementation
[0038] The technical solution of the present invention will be clearly and completely described below with reference to the accompanying drawings and specific embodiments. However, those skilled in the art will understand that the embodiments described below are some embodiments of the present invention, but not all embodiments, and are only used to illustrate the present invention, and should not be regarded as limiting the scope of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall be followed. Where the manufacturers of reagents or instruments are not specified, they are all conventional products that can be purchased commercially.
[0039] The following provides a detailed description of the secondary particulate graphite anode material, preparation method, anode sheet, and electrical equipment according to embodiments of the present invention.
[0040] In some embodiments of the present invention, a secondary particulate graphite anode material is provided, wherein the tap density of the secondary particulate graphite anode material is ≥1.10 g / cc; typically, but not limitingly, for example, the tap density of the secondary particulate graphite anode material may be 1.10 g / cc, 1.15 g / cc, 1.20 g / cc, 1.25 g / cc, 1.30 g / cc, 1.35 g / cc, 1.40 g / cc, 1.45 g / cc, 1.55 g / cc, 1.60 g / cc, 1.65 g / cc, 1.70 g / cc, etc. Wherein, g / cc refers to g / cm³. 3 .
[0041] The tap density test was conducted in accordance with GB-T 24533-2019, standard for graphite anode materials for lithium-ion batteries.
[0042] The secondary particulate graphite anode material of the present invention has a high tap density, which is ≥1.10 g / cc. When used for electrode processing, it can not only effectively reduce the amount of binder (such as CMC) added during the pulping process, but also the high tap material stacking state helps to reduce the rolling pressure of the electrode, thereby reducing the risk of copper foil breakage and making electrode processing easier. At the same time, the expansion rate of the electrode can also be effectively reduced, which is beneficial to improving the electrochemical performance of the battery, especially the cycle performance.
[0043] In some preferred embodiments of the present invention, the tap density of the secondary particulate graphite anode material is 1.3~1.5 g / cc.
[0044] The tap density of the secondary particulate graphite anode material of the present invention is in the range of 1.3~1.5 g / cc, which is beneficial to further improve the processing performance and electrochemical performance.
[0045] In some embodiments of the present invention, the secondary particulate graphite anode material includes a plurality of secondary graphite particles, which in turn include a plurality of primary graphite particles and a graphitic material for bonding the plurality of primary graphite particles. It is understood that the graphitic material refers to a carbon material having a graphite crystal structure, as opposed to amorphous carbon materials.
[0046] In some embodiments of the present invention, the secondary particle graphite anode material satisfies the following relationship: ρ t ×L o ≤55.0; where ρ t L is the tap density of the secondary particle graphite anode material, expressed in g / cc. o The value represents the oil absorption value of the secondary particulate graphite anode material, expressed in mL / 100g.
[0047] It is understandable that calculating ρ t ×L o ρt Take the tap density value of the secondary particle graphite anode material, L o The oil absorption value of the secondary particle graphite anode material is taken as the numerical value; that is, the tap density × oil absorption value of the secondary particle graphite anode material is ≤ 55.0. Typical, but not limiting, examples include ρ t ×L o The values can be 55.0, 50.0, 48.0, 46.0, 44.0, 42.0, 40.0, 35.0, etc.; preferably, 40.0 ≤ ρ t ×L o ≤50.0.
[0048] The oil absorption value test method is: Method A (instrumental method) for carbon black oil absorption value test in GB / T 3780.2, with the test oil changed to linseed oil, and the testing equipment is the ASAHI SOKEN S-500 oil absorption value tester. The test results and reading points are as follows. Figure 7 As shown.
[0049] The tap density of the secondary particulate graphite anode material of the present invention is ≥1.10 g / cm³. 3 Simultaneously satisfying the relationship that the value of tap density × oil absorption value ≤ 55.0, that is, having high tap density while having a relatively smooth particle surface; it is beneficial to improve the performance of secondary particle graphite anode material during processing and in the battery; in the preparation of electrode sheets, it reduces the processing difficulty, improves the stability of slurry, and reduces the pressure of rolling; the fewer reaction sites provided by the material surface, the fewer side reactions are reduced; the contact points of particle accumulation are reduced, making it less likely to generate new cracks and interfaces.
[0050] The surface smoothness of secondary particulate graphite anode materials can be characterized by oil absorption value; for materials with the same tap density, the smoother the surface, the lower the oil absorption value; in the process of making batteries using secondary particulate graphite anode materials, the processing difficulty is reduced, that is, the stability of the slurry is improved and the pressure of rolling is reduced; understandably, the smoother the surface of the secondary particulate graphite anode material, the more favorable it is for processing, and it also has a significant impact on the energy density, life and safety performance of the battery, which is beneficial to improving battery performance.
[0051] The smoother the material surface, the fewer reaction sites it provides, thereby reducing side reactions (preventing excessive SEI growth), reducing lithium consumption, improving initial efficiency, energy density, and achieving long cycle life, as well as reducing high-temperature gas generation and improving safety performance.
[0052] When the tap density of the secondary particle graphite anode material is <1.10 g / cm³ 3At the same time, its oil absorption value is usually higher, and there are more contact points for particle accumulation. During the electrode rolling process, there is more extrusion deformation between particles, and the particles are prone to generating new cracks and interfaces, leading to the deterioration of battery performance. However, the tap density of the secondary particle graphite anode material of this invention is ≥1.10 g / cm³. 3 Furthermore, its smooth surface reduces the contact points where particles accumulate, minimizing the squeezing deformation between particles during the electrode rolling process, and making it less likely for new cracks and interfaces to form.
[0053] In some embodiments of the present invention, the above relation ρ t ×L o In this process, the oil absorption value of the secondary particulate graphite anode material is ≤50mL / 100g.
[0054] In some embodiments of the present invention, the secondary particle graphite anode material satisfies the following relationship: ρ t ×L o ÷P cs ≤1.83; where ρ t L is the tap density of the secondary particle graphite anode material, expressed in g / cc. o The oil absorption value of the secondary particulate graphite anode material is expressed in mL / 100g; P cs The compressive strength of the secondary particulate graphite anode material is expressed in MPa.
[0055] It is understandable that calculating ρ t ×L o ÷P cs At that time, ρ t Take the tap density value of the secondary particle graphite anode material, L o Take the oil absorption value of the secondary particulate graphite anode material, P cs The value of the particle crushing strength of the secondary particle graphite anode material is taken; that is, the value of the tap density × the value of the oil absorption ÷ the value of the particle crushing strength is ≤ 1.83; typically, but not limitingly, for example, ρ t ×L o ÷P cs The values can be 1.83, 1.70, 1.50, 1.30, 1.10, 0.90, 0.70, 0.50, 0.30, 0.10, etc.; preferably, 0 < ρ t ×L o ÷P cs ≤0.83.
[0056] The crushing strength (compressive strength) of the particles was measured according to the national standard GB / T 43091-2023. The specific steps were as follows: 10 particles with a particle size Dv50 (1±10%) were randomly selected, and the maximum pressure that these 10 particles could withstand at the moment of crushing was tested, and the results were obtained according to the formula in the national standard method. ;P cs For particle crushing strength, in MPa; α is a calculation coefficient, which is 2.48; F yk The crushing force is expressed in millinewtons (mN); d is the particle diameter in μm; the average value of the particle crushing strength is calculated and then averaged. The particle morphology before and after the crushing strength test is as follows. Figure 1 As shown, the crushing force curve and reading points for testing crushing strength are as follows: Figure 2 As shown.
[0057] The tap density of the secondary particulate graphite anode material of the present invention is ≥1.10 g / cm³. 3 At the same time, it meets the relationship that the value of tapped density × the value of oil absorption ÷ the value of particle crushing strength ≤ 1.83, that is, it has high tapped density and high particle strength; the material particles are not easy to crack and pulverize during the expansion and contraction of charging and discharging, thus avoiding capacity decay.
[0058] One of the factors affecting battery life in secondary particle graphite anode materials during cycling is the compactness of the particles. More compact particles are less prone to cracking and pulverization during charge-discharge expansion and contraction, thus reducing capacity decay. The compactness of the particles can be characterized by their crush strength. The tap density of secondary particle graphite anode materials is ≥1.10 g / cm³. 3 The value of tap density × oil absorption value ≤ 55.0 indicates that the higher the particle crushing strength, the better the material's performance in the battery. The value of tap density × oil absorption value ÷ particle strength ≤ 1.83 can better measure the material's good processing performance and performance in the battery. Secondary particle graphite anode materials that meet the above relationship have both excellent processing performance and electrochemical performance.
[0059] In some embodiments of the present invention, the particle crushing strength of the secondary particle graphite anode material is ≥30MPa; typically, but not limitingly, for example, the particle crushing strength of the secondary particle graphite anode material can be 30MPa, 50MPa, 70MPa, 90MPa, 100MPa, 110MPa, 120MPa, 130MPa, etc.
[0060] In some preferred embodiments of the present invention, the particle crushing strength of the secondary particle graphite anode material is ≥60MPa.
[0061] It is understandable that when the compressive strength of secondary particle graphite anode materials reaches 60 MPa, it is comparable to the strength level of single particle graphite anode materials.
[0062] In some embodiments of the present invention, the oil absorption value of the secondary particulate graphite anode material is ≤50mL / 100g; typically, but not limitingly, for example, the oil absorption value of the secondary particulate graphite anode material can be 50mL / 100g, 45mL / 100g, 40mL / 100g, 35mL / 100g, 30mL / 100g, 25mL / 100g, 20mL / 100g, etc.
[0063] In some embodiments of the present invention, the particle size Dv50 of the secondary particulate graphite anode material is 7~23 μm; typically, but not limitingly, for example, the particle size Dv50 of the secondary particulate graphite anode material can be 7.0 μm, 11 μm, 15 μm, 19 μm, 23 μm and any value between the two.
[0064] In some embodiments of the present invention, the secondary particulate graphite anode material does not contain an amorphous carbon coating layer.
[0065] See Figure 3 In some embodiments of the present invention, a method for preparing secondary particulate graphite anode material is also provided, comprising the following steps: Coke powder and surface modifier are mixed, and surface modification and granulation are carried out under heating conditions to obtain granulated material; A binder is added to the granulated material, which is then shaped by mechanical force and classified to obtain a graphite precursor material; the binder is liquid or can be softened under mechanical force. Graphitization is performed on the graphite precursor material to obtain secondary particulate graphite anode material.
[0066] The preparation method of the secondary particulate graphite anode material of the present invention involves mixing a surface modifier with coke powder, performing surface modification and granulation; then adding a liquid binder and using mechanical force to shape and smooth the edges of the particles, thus smoothing the protruding edges of the granulated particles without theoretical constraints. Part of the material debris removed during the shaping process fills the pits in the granulated material under the action of the binder, which helps improve the smoothness of the material surface; another part forms small-diameter particles under the action of the binder, increasing the tap density. Finally, after graphitization treatment, a secondary particulate graphite anode material with high tap density, excellent processing performance, and electrochemical performance is successfully prepared.
[0067] In some embodiments of the present invention, the method of shaping by mechanical force includes mechanical impact, and / or rolling, and / or friction.
[0068] In some embodiments of the present invention, the shaping time by mechanical force is 2 to 40 minutes, for example, 5 minutes, 10 minutes, 15 minutes, 20 minutes, 25 minutes, 30 minutes or 35 minutes.
[0069] After the binder is added to the granulated material, the raised edges of the particles are smoothed by mechanical collision, rolling and friction, which improves the tap density of the secondary particles. The material debris from the grinding is not bound by theory. Some of it fills the uneven areas on the particle surface during the shaping process under the action of the binder, and at the same time, it is bonded and granulated to make the particle surface smooth. Some of it forms small-diameter particles under the action of the binder, which optimizes the particle size distribution and improves the tap density.
[0070] In some embodiments of the present invention, the coke powder includes raw coke and / or calcined coke; the coke powder includes at least one of pitch coke, petroleum coke and needle coke; preferably, the coke powder includes at least one of calcined needle coke, raw needle coke, calcined petroleum coke, raw petroleum coke and pitch coke.
[0071] In some embodiments of the present invention, the particle size D50 of the coke powder is 3 to 15 μm; typically, but not limitingly, for example, the particle size D50 of the coke powder can be 3 μm, 6 μm, 8 μm, 10 μm, 12 μm, 15 μm and any value between any two; preferably, the particle size D50 of the coke powder is 6 to 12 μm.
[0072] In some embodiments of the present invention, the surface modifier includes asphalt and / or resin; preferably, the asphalt has a coking value of ≥30%, and the resin includes a resin with a residual carbon content of ≥10% after pyrolysis at 1000°C.
[0073] In some embodiments of the present invention, the mass ratio of surface modifier to coke powder is (5~50):100. Typically, but not limitingly, for example, the mass ratio of surface modifier to coke powder can be 5:100, 15:100, 25:100, 35:100, 45:100, 50:100 and any value between any two; preferably (10~30):100.
[0074] In some embodiments of the present invention, surface modification and granulation include: heating to 400~1200°C and holding for heat treatment; Stirring and / or tumbling are carried out during the surface modification and granulation process.
[0075] In some embodiments of the present invention, the heating process for surface modification and granulation is either a direct single heating or a multi-stage heating, which can be 1 to 10 steps; taking into account both operability and simplicity for mass production. For example, surface modification and granulation include: heating to 400-1200°C at a rate of 1-10°C / min and holding at that temperature; Alternatively, surface modification and granulation may include: heating to T1℃ at a rate of a1℃ / min and holding at that temperature, ..., heating to Tn℃ at a rate of an℃ / min and holding at that temperature, followed by cooling; Wherein, a1, ..., an are each independently 1~10℃ / min, typically but not limitingly, for example, a1, ..., an can each be 1℃ / min, 3℃ / min, 5℃ / min, 7℃ / min, 9℃ / min, 10℃ / min and any value between any two; T1≤……≤Tn, T1≥100℃, Tn is 400℃~1200℃; preferably, n is any value from 2 to 10.
[0076] In some embodiments of the present invention, the mass ratio of binder to granulation material is (3~20):100; typically, but not limitingly, for example, the mass ratio of binder to granulation material can be 3:100, 5:100, 10:100, 15:100, 20:100 and any value between any two; preferably (5~10):100.
[0077] In some embodiments of the present invention, the grading process includes airflow grading or sieving grading; preferably, airflow grading.
[0078] In some embodiments of the present invention, the particle size Dv50 of the graphite precursor material is 7 to 23 μm; typically, but not limitingly, for example, the particle size Dv50 of the graphite precursor material can be 7 μm, 11 μm, 15 μm, 19 μm, 23 μm, and any value between any two.
[0079] In some embodiments of the present invention, the K90 of the graphite precursor material is 0.8 to 1.80, K90 = (Dv90 - Dv10) / Dv50, where Dv90 is the particle size D9v0 of the graphite precursor material, Dv50 is the particle size Dv50 of the graphite precursor material, and Dv10 is the particle size Dv10 of the graphite precursor material; typically, but not limitingly, for example, the value of K90 of the graphite precursor material can be 0.80, 1.00, 1.20, 1.40, 1.60, 1.80, and any value between any two.
[0080] In some embodiments of the present invention, the equipment used for graphitization treatment includes, but is not limited to, Atchison furnace, internal furnace, continuous graphitization furnace, high-temperature induction furnace, etc., wherein the highest constant temperature for graphitization is ≥1800℃ and the duration is not less than 2 hours.
[0081] In some embodiments of the present invention, after graphitization treatment, the process further includes mixing, sieving, and demagnetization.
[0082] In some embodiments of the present invention, a negative electrode sheet is also provided, comprising the above-mentioned secondary particulate graphite negative electrode material, or the secondary particulate graphite negative electrode material prepared according to the above-mentioned preparation method.
[0083] Using the secondary particulate graphite anode material of the present invention for the processing of anode sheets can not only effectively reduce the amount of binder (such as CMC) added during the pulping process, but also the high-compact material accumulation state is more conducive to reducing the rolling pressure of the anode sheet, thereby reducing the risk of copper foil breakage; in other words, reducing the rolling pressure allows for the use of thinner copper foil, which is also beneficial to improving the energy density of the battery; the anode sheet processing process is easier, and the expansion of the anode sheet can also be effectively reduced.
[0084] In some embodiments of the present invention, a lithium-ion battery is also provided, including the above-described negative electrode sheet.
[0085] In some embodiments of the present invention, an electrical device is also provided, including the above-described lithium-ion battery.
[0086] Example 1 The preparation method of the secondary particulate graphite anode material provided in this embodiment includes the following steps: The surface modifier and coke powder are mixed by mechanical force at a mass ratio of 35:100 to obtain a mixture; wherein the surface modifier is pitch with a coking value of 30% and the coke powder is raw needle coke with a particle size Dv50 of 10μm. The mixture was heated to 600℃ at a rate of 3℃ / min and held for 180min, then naturally cooled to room temperature. The material was stirred throughout the process to obtain granulated material. The granulated material with a mass ratio of 100:6 and liquid epoxy resin (binder) with 10% residual carbon in a thermogravimetric analysis at 1000℃ were mixed and shaped for 25 minutes. The edges and corners of the particles were smoothed and spheroidized by rolling and friction. Then, air classification was performed to obtain graphite precursor material. The particle size Dv50 of the graphite precursor material was 15.98 μm and K90 was 1.31. The graphite precursor material was graphitized using an Atchison furnace and kept at 3000℃ for 5 hours. Then, the material was mixed, sieved, and demagnetized in sequence to obtain secondary particulate graphite anode material.
[0087] Example 2 The preparation method of the secondary particulate graphite anode material provided in this embodiment includes the following steps: The surface modifier and coke powder were mixed by mechanical force at a mass ratio of 50:100 to obtain a mixture. The surface modifier was hydroxymethylphenol with a residual carbon content of 30% as determined by thermogravimetric analysis at 1000℃. The coke powder was pitch coke with a particle size Dv50 of 7μm. The mixture is heated to 400℃ at a rate of 1℃ / min and held for 120min, then naturally cooled to room temperature. The material is stirred and tumbled throughout the process to obtain granulated material. The granulated material and binder were mixed at a mass ratio of 100:14. The binder was a solution of asphalt with a coking value of 60% and DMF (N,N-dimethylformamide) at a mass ratio of 1:1. The mixture was then shaped for 15 minutes by rolling and friction to smooth the edges and spheroidize the particles. Then, air classification was performed to obtain graphite precursor material. The particle size D50 of the graphite precursor material was 11.89 μm, and the K90 was 1.20. The graphite precursor material was graphitized in a high-temperature induction furnace at 2400℃ for 2 hours. Then, the material was mixed, sieved, and demagnetized to obtain secondary granular graphite anode material.
[0088] Example 3 The preparation method of the secondary particulate graphite anode material provided in this embodiment includes the following steps: The surface modifier and coke powder were mixed by mechanical force at a mass ratio of 20:100 to obtain a mixture; wherein the surface modifier is pitch with a coking value of 65%; and the coke powder is calcined needle coke with a particle size Dv50 of 3μm. The mixture is first heated to 500℃ at a rate of 3.5℃ / min and held for 120min, then heated to 1200℃ at a rate of 2℃ / min and held for 60min, and then naturally cooled to room temperature. The material is kept tumbling throughout the process to obtain granulated material. The granulation material and binder were mixed at a mass ratio of 100:20. The binder was epoxy resin and curing agent with a mass ratio of 90:10, containing 10% residual carbon from thermogravimetric analysis at 1000℃. The mixture was then shaped for 3 minutes, and the edges of the particles were smoothed and spheroidized by collision and friction. Then, air classification was performed to obtain the graphite precursor material. The particle size Dv50 of the graphite precursor material was 8.17 μm, and the K90 was 1.52. A continuous graphitization furnace was used to graphitize the graphite precursor material at 1800℃ for 3 hours; then, the material was mixed, sieved, and demagnetized sequentially to obtain secondary particulate graphite anode material.
[0089] Example 4 The preparation method of the secondary particulate graphite anode material provided in this embodiment includes the following steps: The surface modifier and coke powder were mixed by mechanical force at a mass ratio of 5:100 to obtain a mixture. The surface modifier was epoxy resin with a residual carbon content of 10% in a thermogravimetric analysis at 1000℃. The coke powder was raw petroleum coke with a particle size Dv50 of 15μm. The mixture is first heated to 200℃ at a rate of 10℃ / min and held for 60min, then heated to 600℃ at a rate of 3.5℃ / min and held for 120min, then heated to 900℃ at a rate of 7℃ / min and held for 60min, and then cooled naturally to room temperature. The material is stirred throughout the process to obtain granulated material. Granulated material and binder were mixed at a mass ratio of 100:3. The binder was asphalt with a coking value of 50%. The mixture was then shaped for 40 minutes. The edges of the particles were smoothed and spheroidized by impact, rolling and friction. Then, air classification was performed to obtain graphite precursor material. The particle size Dv50 of the graphite precursor material was 22.79 μm and K90 was 0.81. The graphite precursor material was graphitized using an internal furnace at 2600℃ for 3 hours; then, it was mixed, sieved, and demagnetized sequentially to obtain secondary granular graphite anode material.
[0090] Example 5 The preparation method of the secondary particulate graphite anode material provided in this embodiment includes the following steps: The surface modifier and coke powder were mixed by mechanical force at a mass ratio of 35:100 to obtain a mixture; wherein the surface modifier was pitch with a coking value of 45%; and the coke powder was raw petroleum coke with a particle size Dv50 of 8μm. The mixture was heated to 600℃ at a rate of 3℃ / min and held for 150min, then naturally cooled to room temperature. The material was stirred throughout the process to obtain granulated material. The granulated material and binder were mixed at a mass ratio of 100:5. The binder was a solution of asphalt with a coking value of 50% and DMF (N,N-dimethylformamide) at a mass ratio of 1:1. The mixture was then shaped for 20 minutes, and the edges of the particles were smoothed and spheroidized by rolling. Then, air classification was performed to obtain graphite precursor material. The particle size Dv50 of the graphite precursor material was 15.44 μm, and the K90 was 1.28. The graphite precursor material was graphitized using an Atchison furnace at 3000℃ for 2 hours; then it was mixed, sieved and demagnetized sequentially to obtain secondary particulate graphite anode material.
[0091] Example 6 The preparation method of the secondary particulate graphite anode material provided in this embodiment includes the following steps: The surface modifier and coke powder were mixed by mechanical force at a mass ratio of 45:100 to obtain a mixture; wherein the surface modifier was pitch with a coking value of 45%; and the coke powder was raw petroleum coke with a particle size Dv50 of 8μm. The mixture was heated to 600℃ at a rate of 3℃ / min and held for 120min, then naturally cooled to room temperature. The material was stirred throughout the process to obtain granulated material. The granulated material and binder were mixed at a mass ratio of 100:3. The binder was a solution of asphalt with a coking value of 50% and DMF (N,N-dimethylformamide) at a mass ratio of 1:1. The mixture was then shaped for 20 minutes by friction to smooth the edges and spheroidize the particles. Then, air classification was performed to obtain the graphite precursor material. The particle size Dv50 of the graphite precursor material was 14.99 μm, and the K90 was 1.30. The graphite precursor material was graphitized using an Atchison furnace at 3000℃ for 2.5 hours; then it was mixed, sieved and demagnetized sequentially to obtain secondary granular graphite anode material.
[0092] Example 7 The preparation method of the secondary particulate graphite anode material provided in this embodiment includes the following steps: The surface modifier and coke powder were mixed by mechanical force at a mass ratio of 35:100 to obtain a mixture; wherein the surface modifier was pitch with a coking value of 45%; and the coke powder was raw petroleum coke with a particle size Dv50 of 8μm. The mixture was heated to 600℃ at a rate of 3℃ / min and held for 150min, then naturally cooled to room temperature. The material was stirred throughout the process to obtain granulated material. The granulated material and binder were mixed at a mass ratio of 100:3. The binder was a solution of asphalt with a coking value of 50% and DMF (N,N-dimethylformamide) at a mass ratio of 1:1. The mixture was then shaped for 40 minutes, and the edges of the particles were smoothed and spheroidized by impact and rolling. Then, air classification was performed to obtain graphite precursor material. The particle size Dv50 of the graphite precursor material was 15.38 μm, and the K90 was 1.28. The graphite precursor material was graphitized using an Atchison furnace at 3000℃ for 2 hours; then it was mixed, sieved and demagnetized sequentially to obtain secondary particulate graphite anode material.
[0093] Example 8 The preparation method of the secondary particulate graphite anode material provided in this embodiment includes the following steps: The surface modifier and coke powder were mixed by mechanical force at a mass ratio of 40:100 to obtain a mixture; wherein the surface modifier was pitch with a coking value of 45%; and the coke powder was raw petroleum coke with a particle size Dv50 of 8μm. The mixture was heated to 600℃ at a rate of 3℃ / min and held for 180min, then naturally cooled to room temperature. The material was stirred throughout the process to obtain granulated material. The granulated material and binder were mixed at a mass ratio of 100:3. The binder was a solution of asphalt with a coking value of 50% and DMF (N,N-dimethylformamide) at a mass ratio of 1:1. The mixture was then shaped for 10 minutes, and the edges of the particles were smoothed and spheroidized by rolling and friction. Then, air classification was performed to obtain graphite precursor material. The particle size Dv50 of the graphite precursor material was 14.51 μm, and the K90 was 1.31. The graphite precursor material was graphitized using an Atchison furnace at 3000℃ for 2.5 hours; then it was mixed, sieved and demagnetized sequentially to obtain secondary granular graphite anode material.
[0094] Example 9 The preparation method of the secondary particulate graphite anode material provided in this embodiment includes the following steps: The surface modifier and coke powder are mixed by mechanical force at a mass ratio of 25:100 to obtain a mixture; wherein the surface modifier is pitch with a coking value of 50%; and the coke powder is pitch coke with a particle size Dv50 of 10μm. The mixture was heated to 700℃ at a rate of 3.5℃ / min and held for 120 minutes, then naturally cooled to room temperature. The material was kept tumbling throughout the process to obtain granulated material. The granulated material and binder were mixed at a mass ratio of 100:5. The binder was asphalt with a coking value of 50%. The mixture was then shaped for 20 minutes. The edges and corners of the particles were smoothed and spheroidized by rolling and friction. Then, air classification was performed to obtain graphite precursor material. The particle size Dv50 of the graphite precursor material was 15.30 μm and K90 was 1.26. The graphite precursor material was graphitized using an Atchison furnace at 3000℃ for 3 hours; then it was mixed, sieved and demagnetized sequentially to obtain secondary particulate graphite anode material.
[0095] Example 10 The preparation method of the secondary particulate graphite anode material provided in this embodiment includes the following steps: The surface modifier and coke powder are mixed by mechanical force at a mass ratio of 25:100 to obtain a mixture; wherein the surface modifier is pitch with a coking value of 60% and the coke powder is pitch coke with a particle size Dv50 of 10μm. The mixture was heated to 700℃ at a rate of 3.5℃ / min and held for 180min, then naturally cooled to room temperature. Throughout the process, the material was stirred and tumbled to obtain granulated material. Granulated material and binder with a mass ratio of 100:5 were mixed. The binder was asphalt with a coking value of 50%. The mixture was then shaped for 20 minutes. The edges and corners of the particles were smoothed and spheroidized by rolling and friction. Then, air classification was performed to obtain graphite precursor material. The particle size Dv50 of the graphite precursor material was 15.34 μm and K90 was 1.35. The graphite precursor material was graphitized using an Atchison furnace at 3000℃ for 3 hours; then it was mixed, sieved and demagnetized sequentially to obtain secondary particulate graphite anode material.
[0096] Example 11 The preparation method of the secondary particulate graphite anode material provided in this embodiment includes the following steps: The surface modifier and coke powder are mixed by mechanical force at a mass ratio of 25:100 to obtain a mixture; wherein the surface modifier is pitch with a coking value of 65% and the coke powder is pitch coke with a particle size Dv50 of 10μm. The mixture was heated to 700℃ at a rate of 3.5℃ / min and held at that temperature for 150min, then naturally cooled to room temperature. The material was stirred throughout the process to obtain granulated material. Granulated material and binder with a mass ratio of 100:5 were mixed. The binder was asphalt with a coking value of 50%. The mixture was then shaped for 30 minutes. The edges and corners of the particles were smoothed and spheroidized by rolling and friction. Then, air classification was performed to obtain graphite precursor material. The particle size Dv50 of the graphite precursor material was 15.29 μm and K90 was 1.24. The graphite precursor material was graphitized using an Atchison furnace at 3000℃ for 3 hours; then it was mixed, sieved and demagnetized sequentially to obtain secondary particulate graphite anode material.
[0097] Example 12 The preparation method of the secondary particulate graphite anode material provided in this embodiment includes the following steps: The surface modifier and coke powder are mixed by mechanical force at a mass ratio of 25:100 to obtain a mixture; wherein the surface modifier is pitch with a coking value of 75% and the coke powder is pitch coke with a particle size Dv50 of 10μm. The mixture was heated to 700℃ at a rate of 3.5℃ / min and held at that temperature for 150min, then naturally cooled to room temperature. The material was stirred throughout the process to obtain granulated material. Granulated material and binder with a mass ratio of 100:7 were mixed. The binder was asphalt with a coking value of 50%. The mixture was then shaped for 40 minutes. The edges of the particles were smoothed and spheroidized by rolling and friction. Then, air classification was performed to obtain graphite precursor material. The particle size Dv50 of the graphite precursor material was 15.35 μm and K90 was 1.37. The graphite precursor material was graphitized using an Atchison furnace at 3000℃ for 3 hours; then it was mixed, sieved and demagnetized sequentially to obtain secondary particulate graphite anode material.
[0098] Example 13 The preparation method of the secondary particulate graphite anode material provided in this embodiment includes the following steps: The surface modifier and coke powder are mixed by mechanical force at a mass ratio of 35:100 to obtain a mixture; wherein the surface modifier is pitch with a coking value of 30% and the coke powder is raw needle coke with a particle size Dv50 of 10μm. The mixture was heated to 600℃ at a rate of 3℃ / min and held for 180min, then naturally cooled to room temperature. The material was stirred throughout the process to obtain granulated material. The granulated material and binder were mixed at a mass ratio of 100:6. The binder was epoxy resin with 10% residual carbon in a thermogravimetric analysis at 1000℃. The mixture was then shaped for 2 minutes, and the edges of the particles were smoothed and spheroidized by rolling and friction. Then, air classification was performed to obtain graphite precursor material. The particle size Dv50 of the graphite precursor material was 16.57 μm, and K90 was 1.65. The graphite precursor material was graphitized using an Atchison furnace at 3000℃ for 2.5 hours; then it was mixed, sieved and demagnetized sequentially to obtain secondary granular graphite anode material.
[0099] Example 14 The preparation method of the secondary particulate graphite anode material provided in this embodiment includes the following steps: The surface modifier and coke powder are mixed by mechanical force at a mass ratio of 35:100 to obtain a mixture; wherein the surface modifier is pitch with a coking value of 30% and the coke powder is raw needle coke with a particle size Dv50 of 10μm. The mixture was heated to 600℃ at a rate of 3℃ / min and held for 180min, then naturally cooled to room temperature. The material was stirred throughout the process to obtain granulated material. The granulated material and binder were mixed at a mass ratio of 100:6. The binder was epoxy resin with 10% residual carbon in a thermogravimetric analysis at 1000℃. The mixture was then shaped for 2 minutes, and the edges of the particles were smoothed and spheroidized by rolling and friction. Then, air classification was performed to obtain graphite precursor material. The particle size Dv50 of the graphite precursor material was 16.77 μm, and the K90 was 1.31. The graphite precursor material was graphitized using an Atchison furnace at 3000℃ for 3 hours; then it was mixed, sieved and demagnetized sequentially to obtain secondary particulate graphite anode material.
[0100] The secondary particulate graphite anode materials prepared in each embodiment of the present invention all comprise multiple secondary graphite particles. Each secondary graphite particle includes multiple primary graphite particles and a graphitic material used to bind the primary graphite particles together. Furthermore, the secondary particulate graphite anode material does not contain an amorphous carbon coating layer.
[0101] Comparative Example 1 The preparation method of the secondary particulate graphite anode material provided in this comparative example is basically the same as that in Example 14, except that: no shaping is performed. The particle size Dv50 of the graphite precursor material obtained in this comparative example is 15.87 μm and K90 is 1.29.
[0102] Comparative Example 2 The preparation method of the secondary particulate graphite anode material provided in this comparative example is basically the same as that in Example 9, except that the mass ratio of granulation material and binder is replaced with 100:2. The particle size Dv50 of the graphite precursor material prepared in this comparative example is 19.50 μm and K90 is 1.80.
[0103] Comparative Example 3 The preparation method of the secondary particulate graphite anode material provided in this comparative example is basically the same as that in Example 9, except that the mass ratio of surface modifier to coke powder is replaced with 4:100. The particle size Dv50 and K90 of the graphite precursor material prepared in this comparative example are 7.90 μm and 1.92, respectively.
[0104] Test case Figure 4 This is a SEM image of the secondary particulate anode material of Embodiment 1 of the present invention, magnified 2000 times. Figure 5 This is a SEM image of the secondary particulate anode material of Embodiment 1 of the present invention, magnified 1000 times. Figure 6 This is a 500x SEM image of the secondary particulate anode material of Embodiment 1 of the present invention.
[0105] Figure 7 This is a SEM image of the secondary particulate anode material of Comparative Example 1 of the present invention, magnified at 2000x. Figure 8 This is a SEM image of the secondary particulate anode material of Comparative Example 1 of the present invention, magnified 1000 times. Figure 9 This is a 500x SEM image of the secondary particulate anode material of Comparative Example 1 of the present invention.
[0106] Figure 10 The particle size distribution diagrams are for the secondary particulate anode materials of Embodiment 1 and Comparative Example 1 of the present invention. Figure 11 The diagram shows the particle size distribution of the secondary particulate anode materials in Example 1 and Comparative Example 1 of this invention. The volumetric and number distributions of the secondary particulate graphite anode materials were obtained using a Malvern 3000 laser particle size analyzer according to the method in GB / T 19077-2016.
[0107] The test results of particle size Dv50, tap density, oil absorption value, and particle crushing strength of the secondary particulate graphite anode materials prepared in each embodiment and comparative example, as well as ρ t ×L o ρ t ×L o ÷P cs The calculation results are shown in Table 1.
[0108] The particle size Dv50 was obtained by Malvern 3000 according to the method in GB / T 19077-2016.
[0109] The crush strength (compressive strength) of the particles was measured according to the test method of national standard GB / T 43091-2023.
[0110] Tap density: The test density of graphite anode materials for lithium-ion batteries is obtained according to the test method of GB / T 24533-2019.
[0111] Oil absorption value: The oil absorption value test method for carbon black is based on Method A (instrumental method) in GB / T 3780.2, with linseed oil used instead of test oil. The testing equipment is an ASAHI SOKEN S-500 oil absorption value tester. During the test, the loading mass of the secondary particulate graphite anode material is 30g ± 0.001g. The material is then poured into the testing equipment, and the oil absorption value corresponding to the maximum torque is recorded as X, which is the oil absorption value test result for the sample, expressed in mL / 30g. The oil absorption value L of the secondary particulate graphite anode material is then calculated. o It is 100×X / 30 (unit: mL / 100g).
[0112] Table 1 Performance test results of various secondary particle graphite anode materials
[0113] As can be seen from Table 1, the secondary particulate graphite anode material of the present invention has high tap value, low oil absorption value, and high particle crushing strength.
[0114] Furthermore, the secondary particulate graphite anode materials from each embodiment and each comparative example were respectively prepared into anode sheets according to the formula graphite:SP:CMC:SBR=96.5:1.0:1.1:1.4 (mass ratio). The compacted density of the anode sheets was 1.55 g / cc, and the single-sided density was 8.0 g / m². 2 The full-charge expansion of each negative electrode was tested, and the rolling pressure required to roll it to the same density of 1.55 g / cc was tested. The negative electrodes were then assembled into a pouch cell with the positive electrode being an LFP and the NP ratio being 1.08. The capacity retention rate after 500 cycles at 1C / 1C was tested. The results are shown in Table 2.
[0115] Table 2 Electrochemical performance test results of each battery
[0116] The secondary particulate graphite anode material of the present invention makes the anode sheet processing easier and the expansion of the electrode sheet can be effectively reduced; the cycle performance of the battery is also significantly improved.
[0117] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A secondary particulate graphite anode material, characterized in that, The tap density of the secondary particulate graphite anode material is ≥1.10 g / cc; The secondary particle graphite anode material satisfies the following relationship: ρ t ×L o ≤55.0; Where, ρ t L is the tap density of the secondary particulate graphite anode material, expressed in g / cc. o The oil absorption value of the secondary particulate graphite anode material is expressed in mL / 100g.
2. The secondary particulate graphite anode material according to claim 1, characterized in that, The tap density of the secondary particulate graphite anode material is 1.3~1.5 g / cc.
3. The secondary particulate graphite anode material according to claim 1, characterized in that, The secondary particulate graphite anode material includes multiple secondary graphite particles, each of which includes multiple primary graphite particles and a graphitic material for bonding the multiple primary graphite particles.
4. The secondary particulate graphite anode material according to claim 1, characterized in that, 40.0≤ρ t ×L o ≤50.0。 5. The secondary particulate graphite anode material according to claim 1, characterized in that, The oil absorption value of the secondary particulate graphite anode material is ≤50mL / 100g.
6. The secondary particulate graphite anode material according to any one of claims 1 to 5, characterized in that, The secondary particle graphite anode material satisfies the following relationship: ρ t ×L o ÷P cs ≤1.83; Where, ρ t L is the tap density of the secondary particulate graphite anode material, expressed in g / cc. o The oil absorption value of the secondary particulate graphite anode material is expressed in mL / 100g; P cs The compressive strength of the secondary granular graphite anode material is expressed in MPa.
7. The secondary particulate graphite anode material according to claim 6, characterized in that, 0<ρ t ×L o ÷P cs ≤0.83。 8. The secondary particulate graphite anode material according to claim 6, characterized in that, The compressive strength of the secondary granular graphite anode material is ≥30MPa.
9. The secondary particulate graphite anode material according to claim 8, characterized in that, The compressive strength of the secondary granular graphite anode material is ≥60MPa.
10. The secondary particulate graphite anode material according to claim 1, characterized in that, The particle size Dv50 of the secondary particulate graphite anode material is 7~23μm.
11. The secondary particulate graphite anode material according to claim 1, characterized in that, The secondary particulate graphite anode material does not contain an amorphous carbon coating layer.
12. A negative electrode sheet, characterized in that, The secondary particulate graphite anode material included in any one of claims 1 to 11.
13. A lithium-ion battery, characterized in that, Includes the negative electrode sheet as described in claim 12.
14. An electrical appliance, characterized in that, Including the lithium-ion battery as described in claim 13.