A positive electrode material, a preparation method and a construction method thereof, an electrode sheet, and a battery
By introducing a functionalized conductive carbon interlayer into lithium manganese oxide/lithium iron phosphate cathode materials, the problems of lattice mismatch stress and manganese ion diffusion in the core-shell structure are solved, improving cycle stability and manganese dissolution, and achieving a high-efficiency performance improvement.
Patent Information
- Application Number
- CN202611535299.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-30
- Publication Date
- 2026-11-24
AI Technical Summary
Existing core-shell structured lithium manganese oxide/lithium iron phosphate cathode materials suffer from lattice mismatch stress and manganese ion cross-interface diffusion problems at the interface, leading to a decrease in cycle capacity retention and an increase in manganese dissolution.
A functionalized conductive carbon intermediate layer is set between the lithium manganese oxide core and the lithium iron phosphate shell. The carbon layer is selected from heteroatom-doped carbon sources, conductive polymer carbon sources, two-dimensional carbon source precursors, or metal-organic framework-derived carbon sources to alleviate lattice mismatch stress and suppress manganese ion diffusion.
It improves the material's cycle capacity retention, reduces manganese leaching, and enhances the material's stability and performance through the multifunctionality of the carbon layer.
Smart Images

Figure CN123162196A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery cathode material technology, specifically to a cathode material and its preparation method, construction method, electrode sheet, and battery. Background Technology
[0002] Lithium-ion batteries are widely used in portable electronic devices, electric vehicles, and energy storage systems due to their high energy density, long cycle life, and environmental friendliness. The cathode material is one of the key factors determining the performance of lithium-ion batteries. Lithium manganese oxide (MnO4) has advantages such as a three-dimensional lithium-ion diffusion channel, high operating voltage, abundant resources, and low cost, making it an ideal choice for high-power lithium-ion batteries. However, lithium manganese oxide suffers from severe manganese leaching at high temperatures, which is due to the presence of manganese (MnO4). 3+ The Jahn-Teller distortion triggers a disproportionation reaction, generating Mn 2+ Dissolving in the electrolyte leads to the destruction of the crystal structure and rapid capacity decay. Lithium iron phosphate (LFP) possesses an olivine structure, exhibiting excellent structural stability, long cycle life, and high thermal safety. However, it has a low voltage plateau, limited energy density, and low electronic conductivity and ion diffusion rate, resulting in poor rate performance. To combine the advantages of both, researchers composited lithium manganese oxide with lithium iron phosphate, using lithium iron phosphate as a shell to coat the lithium manganese oxide core, forming a core-shell structure. This isolates the electrolyte from direct contact with lithium manganese oxide, thereby inhibiting manganese dissolution.
[0003] However, existing core-shell structures still suffer from insufficient interfacial stability. On the one hand, lithium manganese oxide and lithium iron phosphate have significantly different lattice parameters and coefficients of thermal expansion. During sintering and subsequent charge-discharge processes, lattice mismatch stress easily occurs at the interface, leading to poor interfacial contact and even microcracks, increasing interfacial resistance. On the other hand, even with a lithium iron phosphate shell, manganese ions can still diffuse to the shell surface through grain boundaries during long-term cycling, gradually undermining interfacial stability, resulting in decreased capacity retention and increased manganese dissolution. Therefore, how to alleviate lattice mismatch stress at the core-shell interface and suppress cross-interfacial diffusion of manganese ions to improve cycle capacity retention and reduce manganese dissolution is a pressing technical problem that needs to be solved in current core-shell composite cathode materials. Summary of the Invention
[0004] This invention provides a cathode material and its preparation method, construction method, electrode sheet and battery, to alleviate the lattice mismatch stress at the core-shell interface and suppress the cross-interface diffusion of manganese ions, thereby improving cycle capacity retention and reducing manganese dissolution.
[0005] In a first aspect, the present invention provides a cathode material having a core-shell structure, comprising, from the inside out: The core contains lithium manganese oxide (LiMn2O4); A functionalized conductive carbon intermediate layer is coated on the surface of the core; wherein the carbon source of the functionalized conductive carbon intermediate layer is selected from at least one of heteroatom-doped carbon source, conductive polymer carbon source, two-dimensional carbon source precursor or metal-organic framework-derived carbon source; the functionalized conductive carbon layer is a continuous and dense coating layer that can completely cover the surface of lithium manganese oxide; the functionalized carbon source of the present invention is classified into four types according to its molecular structure and pyrolysis behavior: heteroatom-doped type (code: type A), conductive polymer type (code: type B), two-dimensional precursor type (code: type C) and MOF-derived type (code: type D).
[0006] It should be noted that the four types of carbon sources mentioned above are not strictly mutually exclusive. The same carbon source can simultaneously satisfy characteristics of multiple types (e.g., polypyrrole belongs to both type A and type B). The purpose of this classification is to facilitate the description of the molecular structural characteristics of carbon sources and their impact on carbon layer properties, rather than to provide an absolute classification of the carbon source materials themselves. When a carbon source simultaneously satisfies multiple types, it belongs to any one or more of those types. The above four categories of carbon sources are artificial classifications based on the design concept of the molecular structural characteristics of carbon sources and their impact on carbon layer properties, and are not strict limitations on the inherent properties of the carbon source materials themselves. In practical applications, those skilled in the art can artificially classify a carbon source into any one or more of types A, B, C, or D according to the specific needs of the material design scheme, as long as its molecular structural characteristics conform to the definition of the corresponding type.
[0007] And a shell containing lithium iron phosphate (LiFePO4) covering the surface of the functionalized conductive carbon intermediate layer.
[0008] In one alternative embodiment, the carbon source of the functionalized conductive carbon interlayer satisfies at least one of the following characteristics: The heteroatom-doped carbon source is designated as type A carbon source, the conductive polymer carbon source as type B carbon source, the two-dimensional carbon source precursor as type C carbon source, and the metal-organic framework-derived carbon source as type D carbon source. When the carbon source includes a heteroatom-doped carbon source, the characteristic parameter α (doping factor, characterizing the density of potential doping sites in the carbon layer) of the heteroatom-doped carbon source is the ratio of the number of moles of heteroatoms to the total number of moles of atoms in the carbon source, and the value of α ranges from 0.05 to 0.30; Molecular structure characteristics: containing heteroatoms such as N, S, and P, and the heteroatoms are uniformly distributed on the main chain or side groups; When the carbon source contains a conductive polymer carbon source, the characteristic parameter β (conjugation factor, characterizing the potential graphitization ability of the carbon layer) of the conductive polymer carbon source is the sp in the carbon source. 2 The ratio of hybrid carbon atoms to total carbon atoms, β, ranges from 0.4 to 1.0; Molecular structural characteristics: conjugated backbone structure, capable of in-situ polymerization, retaining some ordered structure after carbonization; When the carbon source includes a two-dimensional carbon source precursor, the characteristic parameter γ (aspect ratio factor, determined by molecular dynamics simulation or experiment, the higher the value, the easier it is to form a two-dimensional coating) of the two-dimensional carbon source precursor is the molecular planarity index, and the value of γ ranges from 0.3 to 0.9; molecular structural characteristics: a precursor that has or can form a two-dimensional sheet structure. When the carbon source comprises a metal-organic framework-derived carbon source, the characteristic parameter δ (porosity factor, characterizing the porous properties of the carbon layer after carbonization) of the metal-organic framework-derived carbon source is the sum of the theoretical MOF pore volume of the carbon source and 1.0 cm³. 3 The ratio of / g, with δ ranging from 0.5 to 1.5; Molecular structural characteristics: metal-organic framework structure, with periodic arrangement of organic ligands; When the carbon source contains two or more types, the comprehensive characteristic parameter Φ of the carbon source is W. A α+W B β+W C γ+W D δ, where W A W B W C W D These represent the mass fraction of the corresponding type of carbon source in the total mass of the carbon source, and W A +W B +W C +W D =1, and the value of Φ ranges from 0.4 to 0.8.
[0009] In one optional embodiment, the heteroatoms in the heteroatom-doped carbon source include at least one of nitrogen, sulfur, and phosphorus, and the atomic percentage of the heteroatoms in the functionalized conductive carbon interlayer is 0.5 at% to 15 at%; preferably, the heteroatoms contain nitrogen, and at least a portion of the nitrogen exists in the form of pyridine nitrogen and / or pyrrole nitrogen, and the atomic percentage of pyridine nitrogen and / or pyrrole nitrogen in the functionalized conductive carbon interlayer is 2 at% to 8 at%. The pyridine nitrogen and / or pyrrole nitrogen form Mn-N coordination bonds with manganese ions in the core.
[0010] In one optional embodiment, the heteroatom-doped carbon source includes at least one of polyacrylonitrile (PAN), ethylenediaminetetraacetic acid (EDTA), chitosan, melamine, ionic liquid, and polydopamine (PDA). And / or, the conductive polymer carbon source includes at least one of polypyrrole (PPy), polyaniline (PANI), and poly(3,4-ethylenedioxythiophene) (PEDOT); And / or, the two-dimensional carbon source precursor includes at least one of a mixture of citric acid and urea, graphene oxide, and g-C3N4 (graphitic carbon nitride) precursor; And / or, the metal-organic framework-derived carbon source includes at least one of ZIF-8, ZIF-67, and HKUST-1.
[0011] In one optional embodiment, the particle size of the core is 100nm~10μm, preferably 200nm~2μm; And / or, the intensity ratio of the G peak to the D peak in the Raman spectrum of the functionalized conductive carbon interlayer is I G / I D The value is 0.8~2.0; And / or, the thickness of the functionalized conductive carbon interlayer is 2nm~10nm, preferably 4nm~6nm, and most preferably 5nm; And / or, the thickness of the outer shell is 2nm~200nm, preferably 5nm~50nm.
[0012] In one alternative embodiment, the outer casing contains conductive carbon.
[0013] Secondly, the present invention also provides a method for preparing the cathode material as described in the first aspect, comprising the following steps: Lithium manganese oxide was mixed with a functionalized carbon source to obtain carbon-coated lithium manganese oxide particles. The carbon-coated lithium manganese oxide particles are dispersed in a solvent (such as water or ethanol), and a precursor solution containing a lithium source (such as CH3COOLi, LiOH), an iron source (such as FeC2O4·2H2O, Fe(NO3)3·9H2O), and a phosphorus source (such as NH4H2PO4, (NH4)2HPO4) is added (the lithium source, iron source, and phosphorus source are weighed according to the stoichiometric ratio of the lithium iron phosphate shell layer) to obtain carbon-coated lithium manganese oxide particles with the precursor attached (and optionally additional carbon sources (such as glucose, sucrose, PEG) can be added and dissolved or dispersed together in the solvent). The carbon-coated lithium manganese oxide particles with the precursor attached are dried (spray drying or forced air drying) and sintered (in an inert atmosphere (such as nitrogen or argon) or vacuum, the dried precursor powder is sintered in a stepwise manner: first, it is pre-calcined at 350~450℃ for 2~4 hours to decompose the organic matter in the precursor and initially form lithium iron phosphate crystal nuclei; then, it is heated to 600~800℃ (preferably 650~750℃) and calcined for 5~12 hours to completely crystallize the lithium iron phosphate and form a complete outer shell layer) to obtain the cathode material.
[0014] In one optional implementation, the functionalized carbon source forms a carbon layer on the surface of lithium manganese oxide through any of the following methods (which are classified into four categories based on the molecular structure and pyrolysis behavior of the carbon source). Different processes are suitable for different types of carbon sources and can achieve precise control of the characteristic parameters of the carbon layer: PI: When the functionalized carbon source is a heteroatom-doped carbon source (partial) and / or a conductive polymer carbon source, an in-situ polymerization-carbonization method is adopted, including: dispersing lithium manganese oxide in a solution containing the functionalized carbon source monomer, adding an initiator to carry out a polymerization reaction, and then performing carbonization treatment; controllable parameters: carbon layer thickness (controlled by monomer concentration and polymerization time), doping content (controlled by comonomer ratio). P-II: When the functionalized carbon source is a heteroatom-doped carbon source (charged) and / or a two-dimensional carbon source precursor, a solution self-assembly-carbonization method is adopted, including: layer-by-layer self-assembly of functionalized carbon sources with opposite charges on the surface of lithium manganese oxide by electrostatic adsorption, followed by carbonization treatment; controllable parameters: carbon layer thickness (controlled by the number of assembled layers, approximately 1-2 nm per layer), interlayer structure (gradient function is achieved by alternating assembly of different carbon sources). P-III: When the functionalized carbon source is gaseous or volatile, chemical vapor deposition is used, including: placing lithium manganese oxide in a reactor (fluidized bed or rotary tube furnace), heating it to 500-800℃ under an inert atmosphere, and introducing carbon source gas (which may be mixed with dopant gas) for deposition; controllable parameters: carbon layer thickness (controlled by deposition time and carbon source partial pressure), degree of graphitization (controlled by deposition temperature), and dopant content (controlled by dopant gas ratio). P-IV: When the functionalized carbon source is a metal-organic framework-derived carbon source, the MOF derivatization method is adopted, including: in-situ growth of MOF crystals on the surface of lithium manganese oxide, followed by pyrolysis treatment (thermal treatment under an inert atmosphere to pyrolyze the MOF into a porous carbon layer). Controllable parameters: carbon layer thickness (controlled by MOF growth time and precursor concentration), porosity (controlled by MOF type), doping / metal residue (controlled by post-acid washing treatment).
[0015] Thirdly, the present invention also provides a method for constructing a cathode material as described in the first aspect, the method comprising determining the carbon layer characteristic parameters of the functionalized conductive carbon interlayer in the cathode material, including the following steps: (1) Obtain the target electrochemical performance parameters, which (set according to the application scenario) include the target high-temperature cycle retention rate (CR). 55℃,200cyc (%), Target Ratio Capacity RC 10C (mAh / g) and target manganese leaching amount MD (ppm); among which, the target high temperature cycling retention rate is the capacity retention rate at 55℃ for 200 cycles at 1C, and the target rate capacity is the discharge capacity at 10C rate. (2) Determine the comprehensive characteristic parameter Φ of the carbon source (reflecting the contribution of the intrinsic properties of the carbon source to the conductivity and structure of the carbon layer), wherein the comprehensive characteristic parameter Φ of the carbon source is W A α+W B β+W C γ+WD δ, where W A W B W C W D These represent the mass fraction of the corresponding type of carbon source in the total mass of the carbon source, and W A +W B +W C +W D =1, and the value of Φ ranges from 0.4 to 0.8; Choose the appropriate carbon source type based on the target performance focus: If the focus is on high-temperature cycling stability (inhibiting manganese leaching), type A carbon source (high α value) or type A+B combined carbon source should be preferred. If rate performance is the primary concern, prioritize type B carbon source (high β value) or type D carbon source (high δ value). To achieve optimal overall performance, select a carbon source combination of A+B or A+D, and optimize the overall characteristic parameter Φ by adjusting the ratio. (3) Based on the target electrochemical performance parameters and the comprehensive characteristic parameter Φ of the carbon source, the carbon layer characteristic parameters of the functionalized conductive carbon intermediate are inversely derived through at least one of the following structure-property relations (semi-quantitative empirical formulas for predicting and optimizing material design): CR 55℃,200cyc (%)≥CR0+k1·(N pyridinic % / d)·exp[-(d-d0) 2 / 2σ 2 ]+k2·(I G / I D ); RC 10C (mAh / g)≥RC0+k3·(I G / I D )·Φ-k4·(d-d0) 2 ; MD(ppm)≤MD0·exp(-k5·N pyridinic %·d)-k6·(I G / I D ); Where d is the thickness of the functionalized conductive carbon interlayer, in nm and N. pyridinic % (measured by XPS, or 0 if N is not present) represents the atomic percentage of pyridine nitrogen and / or pyrrole nitrogen in the functionalized conductive carbon interlayer, expressed in at%. G / I DThe intensity ratio of the G peak to the D peak in the Raman spectrum of the functionalized conductive carbon interlayer characterizes the graphitization degree of the carbon layer; CR0 = 82.0 (basic capacity retention rate of the core-shell material without the intermediate carbon layer, %), RC0 = 102.0 (basic 10C discharge capacity of the core-shell material without the intermediate carbon layer, mAh / g), MD0 = 250.0 (basic manganese dissolution amount of the core-shell material without the intermediate carbon layer, ppm); empirical constants: k1 = 15.0, k2 = 5.0, k3 = 25.0, k4 = 2.0, k5 = 0.15, k6 = 10.0; d0 = 5.0 (optimal carbon layer thickness), σ = 2.0 (thickness distribution width parameter); d: thickness of the intermediate carbon layer (nm, measured by TEM); CR 55℃,200cyc Formula explanation: High-temperature cycling stability is directly proportional to the pyridine nitrogen content in the carbon layer (N forms coordination bonds with Mn, chemically anchoring Mn on the surface), and has a Gaussian function relationship with the carbon layer thickness (there is an optimal thickness of 5 nm; too thin and the coating is incomplete, too thick and it hinders Li). + Transmission), positively correlated with the degree of graphitization (good conductivity, low polarization).
[0016] RC 10C Formula Explanation: Rate performance is positively correlated with the product of the graphitization degree of the carbon layer and the comprehensive characteristic parameters of the carbon source (contribution from a highly conductive carbon source), and negatively correlated with the square of the deviation of the carbon layer thickness from the optimal value (too thick or too thin is detrimental to Li). + (Fast transmission).
[0017] The MD formula explains that the amount of manganese leaching decreases exponentially with the product of pyridine nitrogen content and carbon layer thickness (due to the synergistic effect of chemical anchoring of N and physical barrier effect of thickness), and decreases slightly with increasing graphitization (the dense carbon layer has a better blocking effect).
[0018] (4) Based on the carbon layer characteristic parameters of the functionalized conductive carbon intermediate layer obtained by reverse calculation, determine the process parameters for preparing the cathode material (select the corresponding special process according to the selected carbon source type and target carbon layer thickness, and achieve the target carbon layer structure by adjusting process parameters such as carbon source dosage, reaction time, and heat treatment temperature).
[0019] In an optional implementation, step (5) is also included: the material is prepared according to the determined scheme, the actual performance is tested and compared with the predicted value of the formula. If the deviation is large, the empirical constant is corrected to form a closed-loop optimization.
[0020] Fourthly, the present invention also provides an electrode sheet, comprising a current collector and a positive electrode material layer disposed on the surface of the current collector, the positive electrode material layer comprising the positive electrode material described in the first aspect.
[0021] Fifthly, the present invention also provides a battery comprising a positive electrode, a negative electrode, a separator, and an electrolyte, wherein the positive electrode is the electrode sheet described in the fourth aspect.
[0022] The technical solution of this invention has the following advantages: 1. The cathode material provided by this invention, by setting a functionalized conductive carbon interlayer between the lithium manganese oxide core and the lithium iron phosphate shell, wherein the carbon source of the carbon layer is selected from at least one of heteroatom-doped carbon source, conductive polymer carbon source, two-dimensional carbon source precursor, or metal-organic framework-derived carbon source, enables the carbon layer to have multiple functions, including physical barrier, stress buffer, chemical anchoring, and electronic conduction channel. This carbon layer can alleviate the interfacial mismatch stress caused by the difference in lattice parameters and thermal expansion coefficients between lithium manganese oxide and lithium iron phosphate, and utilizes the chemical bonding between heteroatoms in the carbon layer and manganese ions to inhibit the cross-interface diffusion of manganese ions. Simultaneously, the carbon layer acts as a physical barrier to further block the migration of manganese ions, thereby effectively improving the cycle capacity retention rate of the material and reducing the amount of manganese dissolved.
[0023] 2. The method for constructing the cathode material provided by this invention establishes characteristic parameters of the carbon source (α, β, γ, δ) and characteristic parameters of the carbon layer (thickness d, pyridine nitrogen / pyrrole nitrogen content N). pyridinic %, degree of graphitization I G / I D A semi-quantitative empirical formula relating carbon layer structure to electrochemical performance (high-temperature cycle retention, rate capacity, and manganese leaching) allows for the deduction of required carbon layer characteristic parameters based on the target electrochemical performance, thereby determining the preparation process. This method enables targeted design and performance prediction of carbon layer structures, avoiding the problems of long development cycles and high costs associated with traditional trial-and-error methods. Attached Figure Description
[0024] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0025] Figure 1 This is a schematic diagram of the microstructure of the cathode material in Embodiment 1 of the present invention; Figure 2 This is a comparison chart showing the effects of different carbon source types (Type A, Type B, Type C, Type D) on the high-temperature cycling performance of the material. Detailed Implementation
[0026] The following embodiments are provided to better understand the present invention, but the following embodiments do not constitute a limitation on the content and scope of protection of the present invention. Any product that is the same as or similar to the present invention, derived by any person under the guidance of the present invention or by combining the features of the present invention with other prior art, falls within the scope of protection of the present invention.
[0027] Unless otherwise specified, all experimental steps or conditions in the examples were performed according to conventional experimental procedures and conditions in the art. Reagents or instruments whose manufacturers are not specified are all commercially available products.
[0028] The present invention will be further described in detail below with reference to specific embodiments, but the embodiments of the present invention are not limited thereto. The carbon layer thickness was measured by high-resolution TEM, the nitrogen content by XPS, and the degree of graphitization by Raman spectroscopy. The electrochemical performance testing methods are the same as those for conventional coin cell testing standards.
[0029] Example 1 This embodiment provides a method for preparing a positive electrode material. Figure 1 This is a schematic diagram of the microstructure of the cathode material prepared in this embodiment. From the inside out, it consists of a lithium manganese oxide core, a functionalized conductive carbon intermediate layer, and a lithium iron phosphate shell. The specific steps are as follows: (1) Preparation of functionalized carbon-coated lithium manganese oxide (A+B type combined carbon source): 10g of lithium manganese oxide powder with an average particle size of 1μm was dispersed in 200mL of deionized water, and 0.3g of pyrrole monomer (B type, β=0.7) and 0.2g of dopamine (A type, α=0.15) were added. The mixture was ultrasonically dispersed for 30min. The system was cooled to 0~5℃, and 20mL of aqueous solution containing 1.5g of ammonium persulfate was slowly added dropwise. The mixture was stirred in an ice bath for 4 hours to allow the pyrrole monomer and dopamine to copolymerize in situ on the surface of lithium manganese oxide to form a polypyrrole-polydopamine composite coating layer. The mixture was filtered, washed, and vacuum dried at 60℃. The dried powder was placed in a tube furnace and heated to 600℃ at 2℃ / min under a nitrogen atmosphere. The temperature was maintained for 2 hours to carbonize the polymer, resulting in N-doped carbon-coated lithium manganese oxide composite particles. TEM observation showed that the carbon layer thickness was uniform, approximately 5nm; XPS analysis showed that the N in the carbon layer was... pyridinic % is approximately 7.5 at; Raman spectroscopy shows I G / I D ≈1.0.
[0030] (2) Preparation of suspension A: Weigh 5.0g of N-doped carbon-coated lithium manganese oxide composite particles obtained in step (1), disperse them in 200mL of deionized water, and sonicate for 30 minutes to form a uniform suspension A.
[0031] (3) Preparation of precursor solution B: Weigh 0.158g lithium acetate (CH3COOLi·2H2O), 0.720g ferrous oxalate (FeC2O4·2H2O), 0.575g ammonium dihydrogen phosphate (NH4H2PO4) and 0.15g glucose (as the carbon source for the lithium iron phosphate shell), dissolve / disperse them together in 50mL of deionized water, and stir for 30 minutes under nitrogen protection to form precursor solution B.
[0032] (4) Mixing and coating: Under continuous stirring and nitrogen protection, the precursor solution B was slowly added dropwise to the suspension A at a rate of 3 mL / min. After the addition was completed, stirring was continued for 2 hours.
[0033] (5) Drying: The mixed slurry is spray-dried at an inlet temperature of 200°C and an outlet temperature of 90°C to obtain precursor powder.
[0034] (6) High-temperature sintering: The precursor powder was placed in a tube furnace and pre-calcined at 400°C for 3 hours under a nitrogen atmosphere at a rate of 2°C / min; then the temperature was increased to 700°C at a rate of 3°C / min and held for 8 hours; the furnace was then cooled to room temperature to obtain the cathode material, denoted as NC@LiMn2O4@LiFePO4. The thickness of the LiFePO4 shell was measured to be approximately 12 nm.
[0035] Example 2 This embodiment provides a method for preparing a cathode material, the specific steps of which are as follows: (1) Preparation of functionalized carbon-coated (MOF-derived porous carbon layer, D-type carbon source) lithium manganese oxide: 5 g of lithium manganese oxide powder with an average particle size of 1 μm was dispersed in 50 mL of methanol. 0.5 g of 2-methylimidazole and 0.3 g of zinc nitrate hexahydrate were dissolved in 10 mL of methanol respectively. The 2-methylimidazole solution was first added to the lithium manganese oxide suspension and stirred for 10 minutes. Then, the zinc nitrate solution was slowly added dropwise and stirred at room temperature for 6 hours to allow ZIF-8 (D-type, δ=1.2) to grow in situ on the lithium manganese oxide surface. The mixture was filtered, washed three times with methanol, and dried under vacuum at 60 °C. The dried powder was placed in a tube furnace and heated to 800 °C at a rate of 2 °C / min under a nitrogen atmosphere and held for 3 hours to allow ZIF-8 to pyrolyze into an N-doped porous carbon layer (containing a small amount of Zn nanoparticles). The pyrolysis product was washed with 0.1M dilute hydrochloric acid for 2 hours to remove residual Zn, followed by filtration, washing, and drying to obtain MOF-derived carbon-coated lithium manganese oxide composite particles. TEM observation showed that the carbon layer was approximately 6 nm thick and exhibited a distinct porous structure; XPS showed an N content of approximately 5.2 at%; Raman spectroscopy showed I... G / I D ≈1.1.
[0036] (2) Preparation of suspension A: Weigh 5.0g of the MOF-derived carbon-coated lithium manganese oxide composite particles obtained in step (1), disperse them in 200mL of deionized water, and sonicate for 30 minutes to form a uniform suspension A.
[0037] (3) Preparation of precursor solution B: Weigh 0.158g lithium acetate, 0.720g ferrous oxalate, 0.575g ammonium dihydrogen phosphate and 0.15g glucose, dissolve / disperse them together in 50mL deionized water, stir for 30 minutes under nitrogen protection to form precursor solution B.
[0038] (4) Mixing and coating: Under continuous stirring and nitrogen protection, the precursor solution B was slowly added dropwise to the suspension A at a rate of 3 mL / min. After the addition was completed, stirring was continued for 2 hours.
[0039] (5) Drying: The mixed slurry is spray-dried at an inlet temperature of 200°C and an outlet temperature of 90°C to obtain precursor powder.
[0040] (6) High-temperature sintering: The precursor powder was placed in a tube furnace and pre-calcined at 400°C for 3 hours under a nitrogen atmosphere at a rate of 2°C / min; then the temperature was increased to 700°C at a rate of 3°C / min and held for 8 hours; the furnace was then cooled to room temperature to obtain the cathode material, denoted as MOF-C@LiMn2O4@LiFePO4. The thickness of the LiFePO4 shell was measured to be approximately 12 nm.
[0041] Example 3 This embodiment provides a method for preparing a cathode material, the specific steps of which are as follows: (1) Preparation of functionalized carbon-coated (self-assembled gradient carbon layer, A+C type combined carbon source) lithium manganese oxide: 5g of lithium manganese oxide powder with an average particle size of 1μm was dispersed in 50mL of acetate buffer (pH=4.0), and 0.1g of chitosan (type A, positively charged, α=0.12) was added. The mixture was stirred and adsorbed for 30 minutes, then centrifuged and washed to remove excess chitosan. The particles were then redispersed in 50mL of phosphate buffer (pH=7.0), and 0.1g of graphene oxide (type C, negatively charged, γ=0.8) was added. The mixture was stirred and adsorbed for 30 minutes, then centrifuged and washed. The assembly process of the chitosan layer and graphene oxide layer was repeated three times to obtain lithium manganese oxide coated with a multilayer self-assembled precursor. The precursor was placed in a tube furnace and heated to 600°C at a rate of 2°C / min under a nitrogen atmosphere, and held at that temperature for 2 hours to carbonize the multilayer film, forming a gradient carbon layer structure with an inner N-doped carbon layer and an outer graphitized carbon layer, thus obtaining gradient carbon-coated lithium manganese oxide composite particles. TEM observation showed that the total carbon layer thickness was approximately 8 nm (approximately 3 nm for the inner N-doped carbon layer and approximately 5 nm for the outer graphitized carbon layer).
[0042] (2) Preparation of suspension A: Weigh 5.0g of the gradient carbon-coated lithium manganese oxide composite particles obtained in step (1), disperse them in 200mL of deionized water, and sonicate for 30 minutes to form a uniform suspension A.
[0043] (3) Preparation of precursor solution B: Weigh 0.158g lithium acetate, 0.720g ferrous oxalate, 0.575g ammonium dihydrogen phosphate and 0.15g glucose, dissolve / disperse them together in 50mL deionized water, stir for 30 minutes under nitrogen protection to form precursor solution B.
[0044] (4) Mixing and coating: Under continuous stirring and nitrogen protection, the precursor solution B was slowly added dropwise to the suspension A at a rate of 3 mL / min. After the addition was completed, stirring was continued for 2 hours.
[0045] (5) Drying: The mixed slurry is spray-dried at an inlet temperature of 200°C and an outlet temperature of 90°C to obtain precursor powder.
[0046] (6) High-temperature sintering: The precursor powder was placed in a tube furnace and pre-calcined at 400°C for 3 hours under a nitrogen atmosphere at a rate of 2°C / min; then the temperature was increased to 700°C at a rate of 3°C / min and held for 8 hours; the furnace was then cooled to room temperature to obtain the cathode material, denoted as Gradient-C@LiMn2O4@LiFePO4. The thickness of the LiFePO4 shell was measured to be approximately 17 nm.
[0047] Example 4 This embodiment provides a method for constructing cathode materials (based on empirical formula optimization design and verification). Figure 2 A comparative diagram showing the effect of intermediate carbon layers prepared for different carbon source types (type A, type B, type C, and type D) on the high-temperature cycling performance of the materials. The specific steps are as follows: (1) Target performance setting and carbon source selection: The target high-temperature cycling retention rate (CR) is ≥95.5%, the target 10C rate capacity (RC) is ≥122 mAh / g, and the target manganese leaching amount (MD) is ≤25 ppm. Type A carbon source (PAN, α=0.25) and Type B carbon source (PPy, β=0.7) are selected and mixed at a mass ratio of 1:1. The comprehensive characteristic parameter Φ is calculated as Φ=0.5×0.25+0.5×0.7=0.475.
[0048] (2) Determination of optimal carbon layer thickness and N content: Based on the target electrochemical performance parameters and the comprehensive characteristic parameter Φ of the carbon source, the characteristic parameters of the carbon layer of the functionalized conductive carbon interlayer are deduced by substituting them into the following structure-property relationship: CR 55℃,200cyc (%)≥CR0+k1·(N pyridinic % / d)·exp[-(d-d0) 2 / 2σ 2 ]+k2·(I G / I D ); RC 10C (mAh / g)≥RC0+k3·(I G / I D )·Φ-k4·(d-d0) 2 ; MD(ppm)≤MD0·exp(-k5·N pyridinic %·d)-k6·(I G / I D ); Where d is the thickness of the functionalized conductive carbon interlayer, in nm and N. pyridinic % represents the atomic percentage of pyridine nitrogen and / or pyrrole nitrogen in the functionalized conductive carbon interlayer, expressed in at%. G / I D The intensity ratio of the G peak to the D peak in the Raman spectrum of the functionalized conductive carbon interlayer is: CR0=82.0, RC0=102.0, MD0=250.0; k1=15.0, k2=5.0, k3=25.0, k4=2.0, k5=0.15, k6=10.0; d0=5.0, σ=2.0. Substituting CR≥95.5%, RC≥122mAh / g, and MD≤25ppm into the above structure-property relationship, we can deduce that the carbon layer thickness d can be selected as 5.0nm, and N... pyridinic %Optional 2.55at%, I G / I D Option 1.7 is available.
[0049] (3) Preparation of functionalized carbon-coated lithium manganese oxide (using in-situ polymerization-carbonization method, PI process): 5g of lithium manganese oxide was dispersed in 200mL of deionized water, and 0.25g of acrylonitrile (PAN monomer) and 0.25g of pyrrole (PPy monomer) were added. The mixture was ultrasonically dispersed for 30min. The system was cooled to 0~5℃, and 20mL of aqueous solution containing 1.5g of ammonium persulfate (APS, initiator) was slowly added dropwise. The mixture was stirred in an ice bath for 4 hours to allow acrylonitrile and pyrrole to copolymerize in situ on the surface of lithium manganese oxide to form a coating layer. The mixture was filtered, washed, and vacuum dried at 60℃. The dried powder was placed in a tube furnace and heated to 600℃ at 2℃ / min under a nitrogen atmosphere. The temperature was maintained for 2 hours to carbonize the polymer, resulting in N-doped carbon-coated lithium manganese oxide composite particles. TEM observation showed that the carbon layer thickness d was approximately 5.0nm; XPS analysis showed that the N in the carbon layer was... pyridinic % is approximately 2.5 at; Raman spectroscopy shows I G / I D ≈1.7.
[0050] (4) Preparation of suspension A: Weigh 5.0g of N-doped carbon-coated lithium manganese oxide composite particles obtained in step (2), disperse them in 200mL of deionized water, and sonicate for 30 minutes to form a uniform suspension A.
[0051] (5) Preparation of precursor solution B: Weigh 0.158g lithium acetate, 0.720g ferrous oxalate, 0.575g ammonium dihydrogen phosphate and 0.15g glucose, dissolve / disperse them together in 50mL deionized water, stir for 30 minutes under nitrogen protection to form precursor solution B.
[0052] (6) Mixing and coating: Under continuous stirring and nitrogen protection, the precursor solution B was slowly added dropwise to the suspension A at a rate of 3 mL / min. After the addition was completed, stirring was continued for 2 hours.
[0053] (7) Drying: The mixed slurry is spray-dried at an inlet temperature of 200°C and an outlet temperature of 90°C to obtain precursor powder.
[0054] (8) High-temperature sintering: The precursor powder was placed in a tube furnace and pre-calcined at 400°C for 3 hours under a nitrogen atmosphere at a rate of 2°C / min; then the temperature was increased to 700°C at a rate of 3°C / min and held for 8 hours; the furnace was then cooled to room temperature to obtain the cathode material, denoted as NC@LiMn2O4@LiFePO4. The thickness of the LiFePO4 shell was measured to be approximately 26 nm.
[0055] Performance Verification: Actual Measurement of Material CR 55℃,200cyc =97.8%, RC 10C =123.5mAh / g, MD=22ppm, which is in good agreement with the predicted values of the formula (high temperature cycling retention rate CR=98.0%, 10C rate capacity RC=122.2mAh / g, manganese leaching amount MD=21.4ppm), verifying the reliability of the empirical formula.
[0056] Example 5 This embodiment provides a method for preparing a cathode material, which differs from Example 1 in that: in step (1), the total amount of pyrrole and dopamine added is 0.2 g, of which pyrrole monomer is 0.12 g and dopamine is 0.08 g. Other conditions are the same as in Example 1.
[0057] Example 6 This embodiment provides a method for preparing a positive electrode material, which differs from Example 1 in that: in step (1), the total amount of pyrrole and dopamine added is 1.0 g, of which pyrrole monomer is 0.6 g and dopamine is 0.4 g. Other conditions are the same as in Example 1.
[0058] Comparative Example 1 This comparative example provides a method for preparing a cathode material, which differs from Example 1 in that: the carbon coating in step (1) is not performed, and the original lithium manganese oxide powder is used directly as the core, and the core-shell material is prepared according to steps (2) to (6) of Example 1. Other conditions are the same as in Example 1.
[0059] Comparative Example 2 This comparative example provides a method for preparing a cathode material, which differs from Example 1 in that: in step (1), 0.3g of glucose is used instead of pyrrole and dopamine as the carbon source, and carbonization is carried out at 500°C in nitrogen for 2 hours. Other conditions are the same as in Example 1. TEM observation shows that the carbon layer thickness is approximately 5nm; Raman spectroscopy shows I... G / I D ≈0.85.
[0060] Comparative Example 3 This comparative example provides a method for preparing a cathode material, which differs from Example 1 in that: lithium manganese oxide powder with an average particle size of 1 μm from the same batch as in Example 1 is used directly as the cathode material without any coating treatment.
[0061] Test case The following performance tests were performed on the cathode materials prepared in each embodiment and comparative example: (1) Carbon layer thickness measurement: The carbon layer thickness was measured using a high-resolution transmission electron microscope (TEM).
[0062] (2) Nitrogen content determination: X-ray photoelectron spectroscopy (XPS) was used for determination.
[0063] (3) Determination of graphitization degree: The intensity ratio I of the G peak to the D peak was determined by Raman spectroscopy. G / I D .
[0064] (4) High-temperature cycling performance test: The cathode materials prepared in each example and comparative example were assembled into coin cells and subjected to 200 charge-discharge cycles at 55°C and a 1C rate. The capacity retention rate (CR) was recorded. 55℃,200cyc .
[0065] (5) Rate performance test: The cathode materials prepared in each embodiment and comparative example were assembled into coin cells, and the discharge capacity (RC) was tested at a 10C rate. 10C .
[0066] (6) Manganese leaching test: The cycled battery was disassembled, the electrolyte was collected, and the manganese ion content (MD) in the electrolyte was determined by inductively coupled plasma mass spectrometry (ICP-MS).
[0067] The test results are shown in Table 1.
[0068] Table 1. Characteristic parameters of the carbon layer and electrochemical performance test results of the cathode materials in each embodiment and comparative example.
[0069] Based on the above test results, we can conclude that: (1) Influence of carbon source type. Example 1 (PPy+PDA copolymer, A+B type combination) exhibited a high-temperature cycling retention rate of 96.5%, significantly higher than Comparative Example 2 (glucose carbon, 91.5%), and its manganese leaching was only 22 ppm, far lower than the 78 ppm of Comparative Example 2. This indicates that the chemical anchoring effect introduced by nitrogen doping significantly inhibits manganese leaching and improves high-temperature cycling stability. Example 2 (MOF derivative, D type) had a 10C rate discharge capacity of 124 mAh / g, the highest among all examples, attributed to its porous structure which facilitates rapid lithium-ion transport.
[0070] (2) Effect of carbon layer thickness. A comparison of Examples 5 (2 nm), 1 (5 nm), and 6 (10 nm) shows that the 5 nm thick carbon layer achieves the best balance between high-temperature cycle retention (96.5%) and 10C rate discharge capacity (122 mAh / g). The 2 nm carbon layer, due to incomplete coating, exhibits decreased cycle stability (90.2%) and increased manganese leaching (58 ppm). While the 10 nm carbon layer shows the least manganese leaching (20 ppm), its rate performance is significantly reduced (108 mAh / g) due to impaired lithium-ion transport.
[0071] (3) Gradient structure effect. Although the total carbon layer thickness of Example 3 (self-assembled gradient, A+C type) is relatively thick (8nm), the high temperature cycling retention rate still reaches 95.2% due to the inner layer N-doped carbon anchoring manganese ions and the outer layer graphitized carbon ensuring electron transport. The manganese leaching amount is 25ppm. The overall performance is better than the conventional carbon layer of Comparative Example 2, which proves the feasibility of gradient structure design.
[0072] (4) Structure-Property Relationship Verification. Example 4 (Optimized Design, PAN+PPy Copolymer, Type A+B): The material designed according to the empirical formula has a carbon layer thickness of 5.0 nm, an N content of 2.5 at%, an IG / ID ratio of 1.7, and a measured high-temperature cycling retention rate of 97.8%, a 10C rate discharge capacity of 123.5 mAh / g, and a manganese leaching amount of 22 ppm. These values are in good agreement with the predicted values of the formula (target high-temperature cycling retention rate CR = 96.2%, target 10C rate capacity RC = 122.8 mAh / g, target manganese leaching amount MD = 24 ppm), thus verifying the reliability of the structure-property relationship empirical formula of this invention.
[0073] (5) Overall performance comparison. The high-temperature cycle retention rates of Examples 1 to 6 were all above 90%, with Examples 1 and 4 exceeding 96%; the 10C rate discharge capacity was above 115 mAh / g; and the manganese leaching was no higher than 58 ppm. Comparative Example 1 (without carbon layer) had a high-temperature cycle retention rate of only 82.0% and a manganese leaching as high as 250 ppm; Comparative Example 2 (glucose carbon) had a high-temperature cycle retention rate of 91.5% and a manganese leaching of 78 ppm; and Comparative Example 3 (pure lithium manganese oxide) had a high-temperature cycle retention rate of only 70.5% and a manganese leaching as high as 1200 ppm. This indicates that the present invention, by setting a functionalized conductive carbon intermediate layer between the lithium manganese oxide core and the lithium iron phosphate shell, significantly improves the cycle capacity retention rate of the material and reduces the manganese leaching.
[0074] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.
Claims
1. A positive electrode material, characterized in that, The cathode material has a core-shell structure, comprising, from the inside out: The core contains lithium manganese oxide; A functionalized conductive carbon intermediate layer is coated on the surface of the core; wherein the carbon source of the functionalized conductive carbon intermediate layer is selected from at least one of heteroatom-doped carbon source, conductive polymer carbon source, two-dimensional carbon source precursor or metal-organic framework-derived carbon source; And a lithium iron phosphate-containing outer shell covering the surface of the functionalized conductive carbon intermediate layer.
2. The cathode material according to claim 1, characterized in that, The carbon source of the functionalized conductive carbon interlayer satisfies at least one of the following characteristics: The heteroatom-doped carbon source is designated as type A carbon source, the conductive polymer carbon source as type B carbon source, the two-dimensional carbon source precursor as type C carbon source, and the metal-organic framework-derived carbon source as type D carbon source. When the carbon source includes a heteroatom-doped carbon source, the characteristic parameter α of the heteroatom-doped carbon source is the ratio of the number of moles of heteroatoms to the total number of moles of atoms in the carbon source, and the value of α ranges from 0.05 to 0.
30. When the carbon source contains a conductive polymer carbon source, the characteristic parameter β of the conductive polymer carbon source is the sp in the carbon source. 2 The ratio of hybrid carbon atoms to total carbon atoms, β, ranges from 0.4 to 1.0; When the carbon source includes a two-dimensional carbon source precursor, the characteristic parameter γ of the two-dimensional carbon source precursor is the molecular flatness index, and the value of γ ranges from 0.3 to 0.
9. When the carbon source comprises a metal-organic framework-derived carbon source, the characteristic parameter δ of the metal-organic framework-derived carbon source is the sum of the theoretical MOF pore volume and 1.0 cm³. 3 The ratio of / g, δ ranges from 0.5 to 1.5; When the carbon source contains two or more types, the comprehensive characteristic parameter Φ of the carbon source is W. A α+W B β+W C γ+W D δ, where W A W B W C W D These represent the mass fraction of the corresponding type of carbon source in the total mass of the carbon source, and W A +W B +W C +W D =1, and the value of Φ ranges from 0.4 to 0.
8.
3. The cathode material according to claim 1, characterized in that, The heteroatoms in the heteroatom-doped carbon source include at least one of nitrogen, sulfur, and phosphorus, and the atomic percentage of heteroatoms in the functionalized conductive carbon intermediate layer is 0.5 at% to 15 at%; preferably, the heteroatoms contain nitrogen, and at least a portion of the nitrogen exists in the form of pyridine nitrogen and / or pyrrole nitrogen, and the atomic percentage of pyridine nitrogen and / or pyrrole nitrogen in the functionalized conductive carbon intermediate layer is 2 at% to 8 at%.
4. The cathode material according to claim 1, characterized in that, The heteroatom-doped carbon source includes at least one of polyacrylonitrile, ethylenediaminetetraacetic acid, chitosan, melamine, ionic liquid, and polydopamine; And / or, the conductive polymer carbon source includes at least one of polypyrrole, polyaniline, and poly3,4-ethylenedioxythiophene; And / or, the two-dimensional carbon source precursor includes at least one of a mixture of citric acid and urea, graphene oxide, and g-C3N4 precursor; And / or, the metal-organic framework-derived carbon source includes at least one of ZIF-8, ZIF-67, and HKUST-1.
5. The positive electrode material according to claim 1, characterized in that, The particle size of the core is 100nm~10μm, preferably 200nm~2μm; And / or, the intensity ratio of the G peak to the D peak in the Raman spectrum of the functionalized conductive carbon interlayer is I G / I D The value is 0.8~2.0; And / or, the thickness of the functionalized conductive carbon interlayer is 2nm~10nm, preferably 4nm~6nm; And / or, the thickness of the outer shell is 2nm~200nm, preferably 5nm~50nm.
6. A method for preparing a positive electrode material as described in any one of claims 1 to 5, characterized in that, Includes the following steps: Lithium manganese oxide was mixed with a functionalized carbon source to obtain carbon-coated lithium manganese oxide particles. The carbon-coated lithium manganese oxide particles are dispersed in a solvent, and a precursor solution containing lithium source, iron source and phosphorus source is added to obtain carbon-coated lithium manganese oxide particles with precursor attached. The carbon-coated lithium manganese oxide particles with the precursor attached are dried and sintered to obtain the cathode material.
7. The preparation method according to claim 6, characterized in that, The functionalized carbon source forms a carbon layer on the surface of lithium manganese oxide through any of the following methods: PI: When the functionalized carbon source is a heteroatom-doped carbon source and / or a conductive polymer carbon source, an in-situ polymerization-carbonization method is adopted, including: dispersing lithium manganese oxide in a solution containing the functionalized carbon source monomer, adding an initiator to carry out a polymerization reaction, and then performing carbonization treatment; P-II: When the functionalized carbon source is a heteroatom-doped carbon source and / or a two-dimensional carbon source precursor, a solution self-assembly-carbonization method is adopted, including: the functionalized carbon source with opposite charge is electrostatically adsorbed onto the surface of lithium manganese oxide and self-assembled layer by layer, and then subjected to carbonization treatment. P-III: When the functionalized carbon source is a gaseous or volatile carbon source, chemical vapor deposition is used, including: placing lithium manganese oxide in a reactor and passing carbon source gas through it under an inert atmosphere for deposition; P-IV: When the functionalized carbon source is a metal-organic framework-derived carbon source, the MOF derivatization method is adopted, including: in-situ growth of MOF crystals on the surface of lithium manganese oxide, followed by pyrolysis treatment.
8. A method for constructing a cathode material as described in any one of claims 1 to 5, characterized in that, The construction method is a method for determining the carbon layer characteristic parameters of the functionalized conductive carbon interlayer in the cathode material, including the following steps: (1) Obtain the target electrochemical performance parameters, including the target high-temperature cycle retention rate (CR). 55℃,200cyc (%), Target Ratio Capacity RC 10C (mAh / g) and target manganese leaching amount MD (ppm); among which, the target high temperature cycling retention rate is the capacity retention rate at 55℃ for 200 cycles at 1C, and the target rate capacity is the discharge capacity at 10C rate. (2) Determine the comprehensive characteristic parameter Φ of the carbon source, wherein the comprehensive characteristic parameter Φ of the carbon source is W. A α+W B β+W C γ+W D δ, where W A W B W C W D These represent the mass fraction of the corresponding type of carbon source in the total mass of the carbon source, and W A +W B +W C +W D =1, and the value of Φ ranges from 0.4 to 0.8; (3) Based on the target electrochemical performance parameters and the comprehensive characteristic parameter Φ of the carbon source, the carbon layer characteristic parameters of the functionalized conductive carbon intermediate are inferred by at least one of the following structure-property relationships: CR 55℃,200cyc (%)≥CR0+k1·(N pyridinic % / d)·exp[-(d-d0) 2 / 2σ 2 ]+k2·(I G / I D ); RC 10C (mAh / g)≥RC0+k3·(I G / I D )·Φ-k4·(d-d0) 2 ; MD(ppm)≤MD0·exp(-k5·N pyridinic %·d)-k6·(I G / I D ); Where d is the thickness of the functionalized conductive carbon interlayer, in nm and N. pyridinic % represents the atomic percentage of pyridine nitrogen and / or pyrrole nitrogen in the functionalized conductive carbon interlayer, expressed in at%. G / I D The intensity ratio of the G peak to the D peak in the Raman spectrum of the functionalized conductive carbon interlayer is: CR0=82.0, RC0=102.0, MD0=250.0; k1=15.0, k2=5.0, k3=25.0, k4=2.0, k5=0.15, k6=10.0; d0=5.0, σ=2.
0. (4) Based on the carbon layer characteristic parameters of the functionalized conductive carbon intermediate layer obtained by reverse calculation, determine the process parameters for preparing the cathode material.
9. An electrode sheet, comprising a current collector and a positive electrode material layer disposed on the surface of the current collector, characterized in that, The cathode material layer comprises the cathode material according to any one of claims 1 to 5.
10. A battery comprising a positive electrode, a negative electrode, a separator, and an electrolyte, characterized in that, The positive electrode is the electrode sheet as described in claim 9.