Solid-state battery and method of manufacturing the same

By introducing phosphine-containing groups at the chain ends of the hydrogenated nitrile butadiene binder, the problem of insufficient interfacial interaction in solid-state batteries was solved, the interfacial adhesion performance and cycle stability of the cathode were improved, and efficient interfacial interaction and adhesion retention were achieved.

CN123162197APending Publication Date: 2026-11-24SHENZHEN XINYUANBANG TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611666770.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-27
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

In existing solid-state batteries, the interfacial interaction between the positive electrode binder and the positive electrode active material, solid electrolyte and current collector is insufficient, and the adhesion retention ability decreases after cycling, making it difficult to improve the interfacial interaction while maintaining the adhesion performance and flexibility of the main structure.

Method used

A hydrogenated butadiene-nitrile binder with chain end functionalization is prepared by introducing phosphine-containing groups at the ends of the hydrogenated butadiene-nitrile main chain, utilizing their polarity and coordinating structure to enhance interfacial adhesion. The content of functional groups in the hydrogenated butadiene-nitrile binder is 0.1%~3%, and it is prepared through functionalized metathesis and selective hydrogenation reaction.

Benefits of technology

While maintaining the original adhesive properties and flexibility of hydrogenated nitrile rubber, the peel strength and post-cycle peel strength retention rate of the composite cathode are significantly improved, maintaining stable contact between cathode particles and between the cathode film and the current collector.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

To overcome the problems of insufficient interfacial interaction between the binder and the positive electrode active material, solid electrolyte, and current collector in existing solid-state battery composite cathodes, and the resulting decrease in adhesion retention capacity after cycling, this invention provides a solid-state battery and its preparation method. The solid-state battery includes a solid electrolyte layer, a positive electrode, and a negative electrode. The solid electrolyte layer is located between the positive electrode and the negative electrode. The positive electrode includes a hydrogenated nitrile butadiene binder, which includes a hydrogenated nitrile butadiene binder main chain and functional groups located at the ends of the hydrogenated nitrile butadiene binder main chain. The functional groups include phosphine-containing groups.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of new energy battery technology, specifically relating to a solid-state battery and its preparation method. Background Technology

[0002] Nitrile butadiene rubber (NBR) is a random copolymer obtained by free radical polymerization of acrylonitrile and butadiene. Its molecular chain contains polar nitrile groups, exhibiting excellent adhesion to polar substrates and positive electrode active materials. Hydrogenated nitrile butadiene rubber (HNBR) is produced by selective hydrogenation of the carbon-carbon double bonds in NBR. Its main chain tends to be saturated, and it possesses excellent chemical corrosion resistance, heat aging resistance, and mechanical flexibility. In recent years, it has been widely used as an electrode binder in new energy systems such as lithium-ion batteries and sodium-ion batteries.

[0003] Solid-state batteries, which use solid electrolytes instead of traditional liquid electrolytes, show great promise in improving safety and energy density. Since the positive electrode active material, solid electrolyte, and conductive agent in a solid-state battery composite cathode primarily rely on solid-solid contacts for ion and electron transport, lacking the wetting and filling of particle surfaces by liquid electrolytes, the structural integrity and interfacial contact stability of the cathode layer are particularly important for the battery's long-term performance. Polyvinylidene fluoride (PVDF) is currently the mainstream cathode binder, but its rigid molecular chains and high glass transition temperature make it difficult to effectively buffer the volume changes of active particles during charge and discharge, and its interaction with inorganic particle surfaces is limited. High-temperature nitrile bran (HNBR), due to its highly saturated main chain, good flexibility, and high polar nitrile group bonding efficiency, has become an ideal alternative material for solid-state battery cathode binders; however, there is still room for improvement in the interfacial interactions between ordinary HNBR and the positive electrode active material, solid electrolyte, and current collector, and its post-cycle adhesion retention capability also needs further improvement.

[0004] Current battery-grade hydrogen-needle bioreactor (HNBR) technologies primarily optimize HNBR performance by adjusting bulk parameters such as acrylonitrile content, degree of hydrogenation, molecular weight, or Mooney viscosity. This aims to improve the mechanical and interfacial properties of HNBR to some extent. However, adjusting these bulk parameters simultaneously alters the polarity, flexibility, and processing properties of the HNBR. Relying solely on adjusting bulk parameters makes it difficult to further enhance the interfacial interaction between the HNBR and inorganic particles and current collectors without sacrificing the flexibility of the main chain segments, resulting in limited improvement in post-cycle adhesion retention. Furthermore, existing technologies pay relatively little attention to the molecular chain end structure, a key factor influencing interfacial interactions.

[0005] In other technical fields, to improve the interfacial and mechanical properties of nitrile butadiene rubber (NBR) or hydrogenated NBR, existing technologies often employ copolymerization by introducing functional monomers during the polymerization process. This allows functional groups, such as those containing phosphine, silicon, or carboxylic esters, to enter the polymer backbone or side chains through copolymerization. However, when this method of introducing functional groups through monomer copolymerization is directly applied to solid-state battery cathode binders, the functional copolymer units entering the HNBR backbone dilute the relative density of polar nitrile groups on the backbone, disrupting the original polar structure of the NBR backbone and affecting its flexibility. This results in a significant decrease in the adhesion performance of HNBR to active materials, solid electrolytes, and current collectors. Since adhesion performance is a core function of electrode binders, sacrificing adhesion to improve interfacial interaction is unacceptable in battery binder applications.

[0006] Therefore, how to improve the interfacial interaction between HNBR and positive electrode active materials, solid electrolytes and current collectors while maintaining the bonding performance and chain segment flexibility of the main structure, and improve the peel strength and post-cycle peel strength retention rate of the composite positive electrode, has become a technical problem that urgently needs to be solved in this field. Summary of the Invention

[0007] To address the problems of insufficient interfacial interaction between the binder and the positive electrode active material, solid electrolyte and current collector in existing solid-state battery composite cathodes, and the decline in adhesion retention capacity after cycling, this invention provides a solid-state battery and its preparation method.

[0008] The technical solution adopted by the present invention to solve the above-mentioned technical problems is as follows: On one hand, the present invention provides a solid-state battery, comprising a solid electrolyte layer, a positive electrode, and a negative electrode, wherein the solid electrolyte layer is located between the positive electrode and the negative electrode, the positive electrode comprises a hydrogenated nitrile butadiene binder, the hydrogenated nitrile butadiene binder comprising a hydrogenated nitrile butadiene backbone and functional groups located at the ends of the hydrogenated nitrile butadiene backbone, the functional groups comprising phosphine-containing groups; the characteristic element of the phosphine-containing groups is phosphorus (P), and the content of the characteristic element in the functional groups is 0.1% to 3% based on the total mass of the hydrogenated nitrile butadiene binder; The phosphine-containing group is shown in structural formula 1: R1-R2-* Structural Formula 1 Wherein, R1 is selected from phosphate ester groups, R2 is selected from C2~C10 alkylene groups, and * indicates the connection site between the functional group and the hydrogenated butyronitrile backbone; The degree of hydrogenation of the hydrogenated butyronitrile backbone is ≥99%; The hydrogenated nitrile butadiene binder is prepared by the following method: Nitrile rubber is dissolved in an organic solvent to obtain a nitrile rubber solution. A functionalized metathesis reaction is carried out in the presence of an olefin metathesis catalyst and a functionalized olefin chain transfer agent to obtain modified nitrile rubber with functional groups at the ends of the molecular chains; the functional groups include phosphine-containing groups. Hydrogen gas is introduced into the adhesive solution of modified nitrile butadiene rubber to carry out a hydrogenation reaction, thereby obtaining the hydrogenated nitrile butadiene adhesive.

[0009] Optionally, the positive electrode includes a positive electrode material layer, which includes a positive electrode active material, a solid electrolyte, a conductive agent, and the hydrogenated nitrile butadiene binder. The mass content of the hydrogenated nitrile butadiene binder is 0.5% to 5% based on the total mass of the positive electrode material layer as 100%.

[0010] Optionally, the functional group is a chain-terminal residue introduced when a functionalized olefinic chain transfer agent participates in a metathesis reaction; the functionalized olefinic chain transfer agent includes one or more of allylphosphonate dimethyl ester and allyltrimethoxysilane.

[0011] Optionally, the acrylonitrile content of the hydrogenated butyronitrile backbone is 15wt%~50wt%.

[0012] Optionally, the solid electrolyte in the solid electrolyte layer includes one or more of oxide solid electrolyte, sulfide solid electrolyte, halide solid electrolyte and polymer solid electrolyte; the positive electrode active material in the positive electrode material layer includes one or more of lithium iron phosphate, lithium manganese iron phosphate, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide and lithium cobalt oxide.

[0013] Furthermore, the present invention provides a method for preparing a solid-state battery as described above, comprising the following steps: A positive electrode slurry is prepared by mixing the hydrogenated nitrile butadiene binder, positive electrode active material, solid electrolyte, and conductive agent; the positive electrode slurry is coated onto a positive electrode current collector, dried, and rolled to form a positive electrode; a solid electrolyte layer is placed between the positive and negative electrodes, and the battery is encapsulated to obtain a solid-state battery. The hydrogenated nitrile butadiene binder is prepared by the following method: Nitrile rubber is dissolved in an organic solvent to obtain a nitrile rubber solution. A functionalized metathesis reaction is carried out in the presence of an olefin metathesis catalyst and a functionalized olefin chain transfer agent to obtain modified nitrile rubber with functional groups at the ends of the molecular chains. The functional groups include phosphine-containing groups or silicon-containing groups. Hydrogen gas is introduced into the adhesive solution of modified nitrile butadiene rubber to carry out a hydrogenation reaction, thereby obtaining the hydrogenated nitrile butadiene adhesive.

[0014] Optionally, the acrylonitrile content of the nitrile rubber is 15wt%~50wt%, and the mass concentration of the nitrile rubber solution is 1%~15%; the amount of the olefin metathesis catalyst is 0.01%~1% of the mass of the nitrile rubber; the amount of the functionalized olefin chain transfer agent is 0.1%~5% of the mass of the nitrile rubber; the temperature of the functionalized metathesis reaction is 40~80℃, and the reaction time is 2~24 h; the temperature of the hydrogenation reaction is 80~150℃, and the reaction time is 6~48 h.

[0015] Optionally, the olefin metathesis catalyst comprises (1,3-diisopropylimidazolium-2-yl)(tricyclohexylphosphine)benzyl ruthenium dichloride, benzyl methyl dichloro bis(tricyclohexylphosphine)ruthenium, (1,3-dimestrimethyl-4,5-dihydroimidazolium-2-yl)(tricyclohexylphosphine)benzyl ruthenium dichloride, (1,3-dimestrimethyl-4,5-dihydroimidazolium-2-yl)[bis(3-bromopyridine)]benzyl ruthenium dichloride, (1,3- One or more of the following: dimethyltrimethyl-4,5-dihydroimidazolium-2-yl)(2-isopropoxybenzyl)ruthenium dichloride, (1,3-bis-(2,4,6-trimethylphenyl)-2-imidazolium-yl)dichloro(o-isopropoxybenzyl)ruthenium, dichloro(o-isopropoxybenzyl)(tricyclohexylphosphine)ruthenium, and bis(tricyclohexylphosphine)-3-methyl-2-butenyl ruthenium dichloride; wherein the functionalized olefinic chain transfer agent includes dimethyl allylphosphonate.

[0016] The solid-state battery provided by this invention employs a modification route of chain-end functionalization rather than main-chain copolymerization. From a molecular structure perspective, the hydrogenated nitrile butadiene rubber main chain, after hydrogenation, is predominantly composed of saturated carbon-carbon single chains with compliant internal rotation, imparting good flexibility and elasticity to the binder. This allows it to buffer the volume changes of the positive electrode active material during charging and discharging, and fill the gaps between solid particles through chain segment deformation during the hot pressing and rolling processes of the composite positive electrode. The polar nitrile groups on the main chain provide interfacial adhesion and bulk cohesive strength between active particles, between active particles and the solid electrolyte, and between active particles and the current collector through dipole interactions and hydrogen bonding. Because the functional groups are only introduced to the molecular chain ends and not into the main chain or side chains, the relative density of the nitrile groups in the main chain does not decrease due to modification, thus enhancing interfacial interactions while retaining the original adhesive bulk properties of the hydrogenated nitrile butadiene rubber. On the one hand, the functional groups at the chain ends utilize their polar or coordinateable structures to form additional coordination and bonding with the metal sites on the surface of the positive electrode active material and the solid electrolyte. On the other hand, they spontaneously accumulate at the interface during the hot pressing film formation process. With a relatively low functional group density, the interfacial interaction between the binder and inorganic particles and the current collector can be significantly changed. Thus, while maintaining the basic adhesion and flexibility properties of the hydrogenated nitrile rubber body, the peel strength and post-cycle peel strength retention rate of the composite positive electrode are improved, which is beneficial to maintaining stable contact between positive electrode particles and between the positive electrode film layer and the current collector during cycling. Detailed Implementation

[0017] To make the technical problems solved, the technical solutions, and the beneficial effects of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.

[0018] An embodiment of the present invention provides a solid-state battery, comprising a solid electrolyte layer, a positive electrode, and a negative electrode, wherein the solid electrolyte layer is located between the positive electrode and the negative electrode, the positive electrode comprises a hydrogenated nitrile butadiene binder, the hydrogenated nitrile butadiene binder comprising a hydrogenated nitrile butadiene backbone and functional groups located at the ends of the hydrogenated nitrile butadiene backbone, the functional groups comprising phosphine-containing groups; the characteristic element of the phosphine-containing groups is phosphorus (P), and the content of the characteristic element in the functional groups is 0.1% to 3% based on the total mass of the hydrogenated nitrile butadiene binder; The phosphine-containing group is shown in structural formula 1: R1-R2-* Structural Formula 1 Wherein, R1 is selected from phosphate ester groups, R2 is selected from C2~C10 alkylene groups, and * indicates the connection site between the functional group and the hydrogenated butyronitrile backbone; The degree of hydrogenation of the hydrogenated butyronitrile backbone is ≥99%; The hydrogenated nitrile butadiene binder is prepared by the following method: Nitrile rubber is dissolved in an organic solvent to obtain a nitrile rubber solution. A functionalized metathesis reaction is carried out in the presence of an olefin metathesis catalyst and a functionalized olefin chain transfer agent to obtain modified nitrile rubber with functional groups at the ends of the molecular chains; the functional groups include phosphine-containing groups. Hydrogen gas is introduced into the adhesive solution of modified nitrile butadiene rubber to carry out a hydrogenation reaction, thereby obtaining the hydrogenated nitrile butadiene adhesive.

[0019] In this embodiment, nitrile butadiene rubber (NBR) is a random copolymer obtained by free radical polymerization of acrylonitrile and butadiene, with polar nitrile (-C≡N) side groups introduced by acrylonitrile units on the molecular chain; hydrogenated nitrile butadiene rubber (HNBR) is obtained by selectively hydrogenating and saturating the carbon-carbon double bonds on the main chain of nitrile butadiene rubber, resulting in a main chain that tends to be saturated. The hydrogenated nitrile butadiene binder is an end-functionalized hydrogenated nitrile butadiene rubber, whose monomer composition, nitrile content, and degree of hydrogenation of the hydrogenated nitrile butadiene main chain are basically the same as those of ordinary hydrogenated nitrile butadiene rubber, the only difference being that the molecular chain ends have phosphine-containing groups.

[0020] In this invention, the hydrogenated nitrile butadiene rubber (NBR) main chain, after hydrogenation, is predominantly composed of saturated carbon-carbon single chains with internal rotational flexibility, imparting excellent flexibility and elasticity to the binder. This allows it to buffer the volume changes of the positive electrode active material during charging and discharging, and fill the gaps between solid particles through chain segment deformation during the hot pressing and rolling processes of the composite positive electrode. The polar nitrile groups on the main chain provide interfacial adhesion and bulk cohesive strength between active particles, between active particles and the solid electrolyte, and between active particles and the current collector through dipole interactions and hydrogen bonding. Since the functional groups are only introduced into the molecular chain ends and not into the main chain or side chains, the relative density of the nitrile groups in the main chain does not decrease due to modification, thus enhancing interfacial interactions while retaining the original adhesive bulk properties of the hydrogenated NBR rubber.

[0021] From the perspective of chain segment motion and interfacial thermodynamics, the chain ends have higher degrees of freedom and migration ability than the chain middle. During the pulping, coating, and hot pressing film formation processes, the chain ends with functional groups will spontaneously accumulate at the interfaces between the binder and the positive electrode active material, the binder and the solid electrolyte, and the binder and the current collector under the drive of minimizing interfacial energy, resulting in surface segregation. Therefore, only a small amount of functional groups need to be introduced into the chain ends to efficiently control the interfacial properties. Specifically, the phosphonoyl group (P=O) in the phosphine-containing end group is highly polar, and the oxygen atom on the phosphorus-oxygen structure has a lone pair of electrons, which can form dipole and coordination interactions with metal ions at the metal oxide sites on the surface of the positive electrode active material and the solid electrolyte. Its coordination strength is moderate and the stress transmission is uniform.

[0022] On the one hand, the terminal functional groups utilize their polar or coordinateable structures to form additional coordination and bonding with the metal sites on the surface of inorganic particles. On the other hand, by enriching the chain ends at the interface, they restrict the slippage and network relaxation of the chain segments during the stress process. Thus, while maintaining the basic adhesion and flexibility properties of the hydrogenated nitrile rubber body, the peel strength and post-cycle peel strength retention rate of the composite cathode are improved, which is beneficial to maintaining stable contact between cathode particles and between the cathode film and the current collector during cycling.

[0023] The end-group content characterizes the degree of introduction of functional groups at the ends of the molecular chain and can be determined by elemental analysis. When the end-group content is too low, there are too few functional groups at the chain ends, resulting in insufficient interfacial interaction enhancement and limited improvement in peel strength and post-cycle peel strength retention. When the end-group content is too high, the amount of functionalized olefin chain transfer agent is excessive, leading to a lower polymer molecular weight, decreased cohesive strength of the binder, and the excessive polar end groups tend to aggregate at the interface, restricting chain segment movement and consequently reducing flexibility and cycle retention. The content of characteristic elements in the functional groups can be 0.1%, 0.5%, 0.8%, 1.0%, 1.2%, 1.5%, 1.8%, 2.0%, 2.2%, 2.5%, 2.8%, and 3.0%.

[0024] In some embodiments, the functional groups may be located at one or both ends of the hydrogenated nitrile butadiene main chain; the hydrogenated nitrile butadiene binder may be used alone or in combination with conventional binders such as polyvinylidene fluoride and polytetrafluoroethylene.

[0025] In some embodiments, the positive electrode includes a positive electrode material layer, which includes a positive electrode active material, a solid electrolyte, a conductive agent, and the hydrogenated nitrile butadiene binder. The mass content of the hydrogenated nitrile butadiene binder is 0.5% to 5% based on the total mass of the positive electrode material layer as 100%.

[0026] In this embodiment, the positive electrode material layer refers to a solid layer composed of positive electrode active material, solid electrolyte, conductive agent, and hydrogenated nitrile butadiene binder after coating, drying, and rolling. The total mass of the positive electrode material layer is the sum of the masses of the aforementioned solid components. The hydrogenated nitrile butadiene binder plays a role in bonding and maintaining the electrode structure in the positive electrode material layer. It forms a continuous elastic bonding network between the positive electrode active material particles and the solid electrolyte particles, and bonds and fixes each solid component to the current collector.

[0027] When the mass content of hydrogenated nitrile butadiene binder is less than 0.5%, the binder is insufficient to form a continuous and complete bonding network between solid particles and between particles and current collectors. This results in insufficient cohesive strength and peel strength of the electrode, making it prone to powder shedding and delamination during rolling, slitting, and battery cycling. This leads to degradation of the solid-solid contact interface, increased interfacial impedance, and rapid capacity decay. When the mass content of hydrogenated nitrile butadiene binder is greater than 5%, the proportion of the insulating rubber phase is too high. This can coat the active particles and conductive agents, blocking some electron conduction pathways, increasing the internal resistance of the electrode and reducing rate performance. Simultaneously, the mass proportion of active materials and solid electrolyte decreases accordingly, which is detrimental to battery energy density.

[0028] Within the specified range, the specific values ​​of the mass content of hydrogenated nitrile butadiene binder can be 0.5%, 0.8%, 1.0%, 1.2%, 1.5%, 1.8%, 2.0%, 2.2%, 2.5%, 2.8%, 3.0%, 3.5%, 4.0%, 4.5%, and 5.0%.

[0029] In some embodiments, the functional group is a chain-terminal residue introduced when a functionalized olefinic chain transfer agent participates in a metathesis reaction.

[0030] In this embodiment, the functionalized olefin chain transfer agent refers to an olefin compound containing both terminal olefin bonds capable of undergoing olefin metathesis with the carbon-carbon double bonds of the nitrile rubber main chain and a phosphine-containing group. The terminus chain residue refers to the structural fragment remaining after the functionalized olefin chain transfer agent undergoes cross-metathesis with the chain ends formed by the breakage of the nitrile rubber molecular chain during metathesis chain transfer, and is connected to the polymer chain end via an alkylene group.

[0031] The functional groups at the chain ends are introduced through an olefin metathesis chain transfer reaction in a nitrile rubber solution. The reaction process is as follows: under the action of an olefin metathesis catalyst, the carbon-carbon double bond introduced by the butadiene unit on the main chain of the nitrile rubber undergoes cross metathesis with the terminal olefin bond of the functionalized olefin-type chain transfer agent, forming a new carbon-carbon double bond and releasing a small molecule olefin. The functionalized olefin fragment is thus connected to the end of the polymer molecule chain in the form of chain end residues. Subsequently, in the hydrogenation reaction, the carbon-carbon double bond of the main chain and the newly formed chain end double bond are selectively hydrogenated and saturated, finally yielding a main chain saturated and a chain end functionalized hydrogenated nitrile rubber with functional groups at the chain ends.

[0032] The key to this introduction method lies in the fact that functional groups only appear at the ends of the molecular chain: the functionalized olefinic chain transfer agent does not participate in the addition polymerization of the main chain, and therefore will not enter the polymer main chain or side chain. The content of acrylonitrile units and the density of nitrile groups on the main chain remain unchanged, which is fundamentally different from the method of functional monomer copolymerization diluting nitrile groups and damaging adhesion in the background technology. At the same time, the degree of metathesis chain transfer reaction is directly related to the amount of functionalized olefinic chain transfer agent used. The greater the amount used, the more chain transfers occur, the lower the polymer molecular weight, and the higher the proportion of functional groups at the chain ends. Therefore, the molecular weight and end group density of the polymer can be simultaneously controlled by the amount of functionalized olefinic chain transfer agent used.

[0033] It should be noted that, since the functional groups are introduced into the hydrogenated nitrile butadiene binder through a functionalized olefinic chain transfer agent, a small amount of nitrile butadiene rubber without functional groups may remain in the hydrogenated nitrile butadiene rubber.

[0034] In some embodiments, the functionalized olefinic chain transfer agent includes dimethyl allylphosphonate.

[0035] Allyl phosphonate dimethyl ester is a phosphine-containing chain transfer agent used to introduce dimethyl phosphonate end groups.

[0036] In some embodiments, the acrylonitrile content of the hydrogenated butyronitrile backbone is 15wt%~50wt%, and the degree of hydrogenation of the hydrogenated butyronitrile backbone is ≥99%.

[0037] In this invention, the degree of hydrogenation refers to the percentage of carbon-carbon double bonds saturated by hydrogenation in hydrogenated nitrile rubber relative to the total number of carbon-carbon double bonds in the nitrile rubber before hydrogenation. The acrylonitrile content determines the relative density of the main chain nitrile groups: when the content is below 15 wt%, the main chain polarity is insufficient, resulting in low adhesion strength of the binder to inorganic particles and current collectors; when the content is above 50 wt%, the molecular chain rigidity is too high, the glass transition temperature increases, the binder flexibility decreases, making it difficult to buffer the volume changes of active particles, and its solubility in organic solvents deteriorates. The acrylonitrile content can be, for example, 15 wt%, 20 wt%, 25 wt%, 28 wt%, 30 wt%, 33 wt%, 35 wt%, 38 wt%, 40 wt%, 45 wt%, or 50 wt%, preferably 25 wt% to 40 wt%.

[0038] In some embodiments, the solid electrolyte in the solid electrolyte layer includes one or more of oxide solid electrolytes, sulfide solid electrolytes, halide solid electrolytes, and polymer solid electrolytes.

[0039] Among them, oxide solid electrolytes exhibit good chemical stability and a wide electrochemical window, and can be selected from one or more of LATP, LLZO, LLTO, and LLZTO; sulfide solid electrolytes have high ionic conductivity and can be cold-pressed, and can be selected from one or more of Li6PS5Cl and Li3PS4; halide solid electrolytes have good compatibility with positive electrode active materials, and can be selected from one or more of Li3YCl6 and Li3InCl6; polymer solid electrolytes are flexible and easy to process, and can be selected from one or more of polyoxyethylene electrolytes and polyvinylidene fluoride electrolytes. The hydrogenated nitrile butadiene binder of the present invention relies on the interfacial interaction between the polar nitrile groups of the main chain and the metal sites and hydroxyl groups on the surface of the above-mentioned solid electrolytes, thus improving interfacial adhesion and cycle contact stability for all of the above-mentioned solid electrolyte systems.

[0040] In some embodiments, the positive electrode active material includes one or more of lithium iron phosphate, lithium manganese iron phosphate, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and lithium cobalt oxide; the conductive agent includes one or more of conductive carbon black, acetylene black, Ketjen black, carbon nanotubes, and graphene; the positive electrode current collector can be aluminum foil or carbon-coated aluminum foil; and the negative electrode can be a graphite electrode, a silicon-carbon negative electrode, or a lithium metal negative electrode.

[0041] Another embodiment of the present invention provides a method for preparing a solid-state battery as described above, comprising the following steps: A positive electrode slurry is prepared by mixing the hydrogenated nitrile butadiene binder, positive electrode active material, solid electrolyte, and conductive agent; the positive electrode slurry is coated onto a positive electrode current collector, dried, and rolled to form a positive electrode; a solid electrolyte layer is placed between the positive and negative electrodes, and the battery is encapsulated to obtain a solid-state battery. The hydrogenated nitrile butadiene binder is prepared by the following method: Nitrile rubber is dissolved in an organic solvent to obtain a nitrile rubber solution. A functionalized metathesis reaction is carried out in the presence of an olefin metathesis catalyst and a functionalized olefin chain transfer agent to obtain modified nitrile rubber with functional groups at the ends of the molecular chains. The functional groups include phosphine-containing groups or silicon-containing groups. Hydrogen gas is introduced into the adhesive solution of modified nitrile butadiene rubber to carry out a hydrogenation reaction, thereby obtaining the hydrogenated nitrile butadiene adhesive.

[0042] The preparation method of this embodiment includes three stages: functionalization metathesis, selective hydrogenation, and reaction termination and polymer separation.

[0043] The first stage is functionalized metathesis. Nitrile rubber is first dissolved in an organic solvent to prepare a homogeneous nitrile rubber solution. The organic solvent needs to be dehydrated to prevent moisture from deactivating the olefin metathesis catalyst. Then, the olefin metathesis catalyst and a functionalized olefin chain transfer agent are added, and the metathesis reaction is carried out under nitrogen protection and stirring. The carbon-carbon double bonds introduced by the butadiene unit on the nitrile rubber backbone undergo cross-metathesis and chain transfer with the terminal olefin bonds of the functionalized olefin chain transfer agent, introducing functional groups into the polymer molecular chain ends. By adjusting the amount of functionalized olefin chain transfer agent added, the end-group content and molecular weight of the resulting nitrile rubber can be adjusted.

[0044] The second stage is selective hydrogenation. After the metathesis reaction reaches the predetermined extent, the reaction system is transferred to a high-pressure reactor. After nitrogen purging, hydrogen gas is introduced to selectively hydrogenate the carbon-carbon double bonds in the nitrile rubber backbone. The backbone gradually transforms into a saturated structure, while the phosphine- and silicon-containing functional groups at the chain ends remain stable and undamaged during this process. The reaction is stopped when the degree of hydrogenation is greater than 99.0%. The hydrogen pressure is determined based on the catalytic system and the target degree of hydrogenation.

[0045] The third stage involves reaction termination and polymer separation, as well as positive electrode preparation and battery assembly. After the reaction is complete, heating is stopped, the mixture is cooled to a safe temperature, and pressure is released. The gel solution is then added to ethanol, isopropanol, or other alcohol-based non-solvents to precipitate end-functionalized hydrogenated nitrile butadiene rubber. Repeated washing removes unreacted monomers, residual solvents, and low-molecular-weight byproducts. Finally, it is dried under vacuum to constant weight to obtain the hydrogenated nitrile butadiene binder. The hydrogenated nitrile butadiene binder is then formulated into a binder solution, pre-dispersed with a conductive agent and solid electrolyte, and then added to the positive electrode active material for uniform dispersion to obtain the positive electrode slurry. After vacuum degassing, the slurry is coated onto the positive electrode current collector, dried, rolled, and slit to obtain a composite positive electrode sheet. A solid electrolyte layer is placed between the positive and negative electrodes, and the resulting solid-state battery is obtained through stacking or winding and encapsulation.

[0046] In some embodiments, the acrylonitrile content of the nitrile rubber is 15wt%~50wt%, and the mass concentration of the nitrile rubber solution is 1%~15%; the amount of the olefin metathesis catalyst is 0.01%~1% of the mass of the nitrile rubber; the amount of the functionalized olefin chain transfer agent is 0.1%~5% of the mass of the nitrile rubber; the temperature of the functionalized metathesis reaction is 40~80℃, and the reaction time is 2~24h; the temperature of the selective hydrogenation reaction is 80~150℃, the reaction time is 6~48h, and the degree of hydrogenation is ≥99%.

[0047] When the temperature of the functionalized metathesis reaction is too low, the catalyst initiation efficiency is low and the metathesis reaction rate is too slow; when the temperature is too high, the olefin metathesis catalyst is prone to thermal decomposition and deactivation, and the side reactions increase.

[0048] The hydrogenation reaction ends with a degree of hydrogenation of not less than 99%. At temperatures below 80°C, the hydrogenation rate is too slow and the reaction cycle is too long; at temperatures above 150°C, the catalyst is prone to deactivation, and the chain-terminal functional groups are at risk of reduction or decomposition. The catalyst used in this invention exhibits high selectivity for carbon-carbon double bonds and low activity for hydrogenating nitrile groups, thus preserving the nitrile group—a polar binding group—while saturating the main chain double bonds.

[0049] In some implementation methods, the preparation of nitrile rubber compound, functionalization metathesis reaction, and selective hydrogenation reaction can be carried out sequentially in the same reaction system without intermediate polymer separation. This simplifies the operation and ensures good process continuity. During the metathesis reaction stage, the end group content and molecular weight are controlled by adjusting the amount of chain transfer agent. During the hydrogenation reaction stage, the degree of hydrogenation is controlled by adjusting the temperature, hydrogen pressure, and time. The two work together to achieve synergistic control of end group structure, molecular weight, and degree of hydrogenation while maintaining the density of the main chain nitrile groups, ensuring stable product performance and batch consistency.

[0050] In some embodiments, the organic solvent includes one or more of chlorobenzene, toluene, and dichlorobenzene; The organic solvent is preferably chlorobenzene that has undergone dehydration treatment, which has a strong ability to dissolve nitrile rubber and a moderate boiling point, making it easy to recover.

[0051] In some embodiments, the olefin metathesis catalyst comprises one or more ruthenium-based carbene catalysts; specifically, the olefin metathesis catalyst comprises (1,3-diisopropylimidazolium-2-yl)(tricyclohexylphosphine)benzylmethylruthenium dichloride, benzylmethyl dichlorobis(tricyclohexylphosphine)ruthenium, (1,3-dimestrimethyl-4,5-dihydroimidazolium-2-yl)(tricyclohexylphosphine)benzylmethylruthenium dichloride ... One or more of the following: (2-methylene)[bis(3-bromopyridine)]benzyl ruthenium dichloride, (1,3-dimestrimethyl-4,5-dihydroimidazol-2-methylene)(2-isopropoxybenzyl)ruthenium dichloride, (1,3-bis-(2,4,6-trimethylphenyl)-2-imidazolidinemethylene)dichloro(o-isopropoxybenzyl)ruthenium, dichloro(o-isopropoxyphenylmethylene)(tricyclohexylphosphine)ruthenium, and bis(tricyclohexylphosphine)-3-methyl-2-butenemethylene dichloride.

[0052] In some embodiments, the functionalized olefinic chain transfer agent includes dimethyl allylphosphonate.

[0053] The composite cathode slurry preparation, coating, drying and rolling processes described above, as well as the solid-state battery assembly method, process parameters, raw material types and ratios, can all be combined, replaced and adjusted without departing from the concept of this invention. All such combinations, replacements and adjustments should fall within the protection scope of this invention.

[0054] The present invention will be further illustrated by the following examples.

[0055] Example 1 This embodiment illustrates the solid-state battery and its preparation method disclosed in this invention, including the following steps: Step ①: Functionalized metathesis reaction 100g of acrylonitrile rubber (33wt%) and 1900g of dehydrated chlorobenzene were added to a reactor equipped with mechanical stirring, temperature control, and nitrogen protection. The mixture was stirred thoroughly under nitrogen protection until the acrylonitrile rubber was completely dissolved, yielding a homogeneous acrylonitrile rubber solution with a mass concentration of approximately 5%. 1% (by mass) of allylphosphonate dimethyl ester was added to the above solution as a functionalized olefin chain transfer agent, and 0.1% (by mass) of (1,3-dimethyltrimethyl-4,5-dihydroimidazolium-2-yl)(tricyclohexylphosphine)benzylmethylene ruthenium dichloride was added as an olefin metathesis catalyst. The functionalization metathesis reaction was carried out at 60°C under nitrogen protection and stirring conditions, causing metathesis and chain transfer of the carbon-carbon double bonds in the acrylonitrile rubber main chain, introducing phosphine-containing groups at the polymer molecular chain ends.

[0056] Step 2: Selective hydrogenation After the metathesis reaction reaches the predetermined extent, the reaction system is transferred to a high-pressure reactor. After nitrogen purging, hydrogen is introduced for selective hydrogenation at a pressure of 8 MPa and a temperature of 120 °C. This process gradually hydrogenates the carbon-carbon double bonds in the nitrile rubber main chain, resulting in phosphine-terminated hydrogenated nitrile rubber with a hydrogenation degree ≥99%.

[0057] Step ③: Reaction termination and polymer separation After the hydrogenation reaction is completed, heating is stopped and the mixture is cooled to a safe temperature. After depressurization, the adhesive solution is removed and added to excess ethanol to precipitate the polymer. The polymer solution is then repeatedly washed with ethanol to remove residual solvent, unreacted monomers, and low-molecular-weight byproducts. The resulting polymer is dried to constant weight under vacuum to obtain phosphonate-terminated hydrogenated nitrile butadiene rubber, denoted as P-HNBR.

[0058] Step 4: Prepare the positive electrode sheet Lithium iron phosphate was used as the positive electrode active material, conductive carbon black as the conductive agent, LATP as the oxide solid electrolyte, and the obtained P-HNBR as the binder. Based on 100 parts by total mass of the positive electrode solid components, the mass ratio of each component was lithium iron phosphate:LATP:conductive carbon black:P-HNBR = 70:25:3.5:1.5. First, P-HNBR was prepared into a binder solution, mixed with conductive carbon black and solid electrolyte, and fully pre-dispersed at about 3000 rpm for 30 min. Then, lithium iron phosphate was added, and the mixture was planetarily stirred at about 4000 rpm for 2 h. After vacuum degassing, the mixture was coated onto aluminum foil, which served as the positive electrode current collector. The positive electrode sheet was obtained by drying, rolling, and slitting.

[0059] Step 5: Fabrication of solid-state batteries A solid-state battery is obtained by using commercially available graphite electrodes as the negative electrode and setting a solid electrolyte layer between the positive and negative electrodes, and then stacking and encapsulating them.

[0060] Example 2 This embodiment illustrates the solid-state battery and its preparation method disclosed in this invention, including most of the operational steps in Example 1, with the following differences: Except for adjusting the amount of allyl phosphonate dimethyl ester added in Example 1 to 0.5% of the mass of nitrile rubber, the other conditions were the same as in Example 1, and the resulting product was denoted as P-HNBR-L.

[0061] Example 3 This embodiment illustrates the solid-state battery and its preparation method disclosed in this invention, including most of the operational steps in Example 1, with the following differences: Except for adjusting the amount of allyl phosphonate dimethyl ester added in Example 1 to 1.5% of the mass of nitrile rubber, the other conditions were the same as in Example 1, and the resulting product was denoted as P-HNBR-H.

[0062] Example 4 This embodiment illustrates the solid-state battery and its preparation method disclosed in this invention, including most of the operational steps in Example 1, with the following differences: Except for adjusting the amount of olefin metathesis catalyst added in Example 1 to 0.2% of the mass of nitrile rubber, the other conditions were the same as in Example 1.

[0063] Comparative Example 1 This comparative example is used to illustrate the solid-state battery and its preparation method disclosed in this invention, including the following steps: Step ①: Dissolve 100g of ordinary nitrile rubber with an acrylonitrile content of 33wt% and 1900g of dehydrated chlorobenzene were added to a reactor equipped with mechanical stirring, temperature control and nitrogen protection. The mixture was stirred thoroughly under nitrogen protection to completely dissolve the nitrile rubber solution with a mass concentration of about 5%. No functionalized olefin chain transfer agent was added in this step.

[0064] Step 2: Selective hydrogenation The above-mentioned adhesive solution was transferred to a high-pressure reactor, and after nitrogen purging, hydrogen was introduced for selective hydrogenation. The hydrogen pressure was 8 MPa and the temperature was 120°C, resulting in ordinary hydrogenated nitrile rubber with a hydrogenation degree ≥99%.

[0065] Step ③: Reaction termination and polymer separation After the hydrogenation reaction is completed, the mixture is cooled and depressurized. The adhesive solution is then added to excess ethanol to precipitate the polymer, followed by repeated washing. The mixture is then vacuum dried to constant weight to obtain ordinary hydrogenated nitrile rubber without functional end groups.

[0066] Step 4: Prepare the positive electrode sheet The positive electrode sheet was prepared by replacing the P-HNBR in Example 1 with ordinary hydrogenated nitrile butadiene rubber, while keeping the other positive electrode formulation, slurry dispersion, coating, drying and rolling processes the same as in Example 1.

[0067] Step 5: Fabrication of solid-state batteries The solid-state battery was assembled using the same method as in Example 1.

[0068] Comparative Example 2 This comparative example is used to illustrate the solid-state battery and its preparation method disclosed in this invention. The hydrogenated nitrile butadiene binder used in this comparative example is a phosphorus-containing hydrogenated nitrile butadiene rubber with a main chain, prepared by copolymerizing functionalized monomers with butadiene and acrylonitrile and then hydrogenating. The preparation steps are as follows: Step ①: Copolymerization reaction 100 parts butadiene, 33 parts acrylonitrile, and 1 part diethyl vinylphosphonate were mixed, and 3% by weight of potassium disproportionated rosinate soap, 1% sodium dodecyl sulfate, 0.2% p-menthane hydrogen peroxide, 0.1% sodium formaldehyde sulfoxylate, 0.01% disodium ethylenediaminetetraacetate, 0.005% ferrous sulfate heptahydrate, and 0.36% tert-dodecyl mercaptan were added. Emulsion polymerization was carried out at 10°C. When the monomer conversion reached 75%, 0.1% diethylhydroxylamine was added to terminate the reaction.

[0069] Step 2: Coagulation and Drying A 10% calcium chloride aqueous solution was used as a coagulant, and co-current flocculation was carried out at 50℃ and 2000 rpm. The resulting granules were washed 10 times with deionized water and then dried to obtain nitrile rubber with phosphonate ester units introduced into the main chain.

[0070] Step 3: Hydrogenation reaction The above-mentioned nitrile rubber was prepared into a chlorobenzene solution with a solid content of 10%, and 300 ppm of tris(triphenylphosphine) rhodium chloride catalyst was added. Hydrogen gas was introduced, and the reaction was carried out at a pressure of 6 MPa and a temperature of 125 °C for 7 hours. After drying, a main chain phosphine-containing hydrogenated nitrile rubber with a hydrogenation degree of ≥99% was obtained.

[0071] Step 4: Prepare the positive electrode sheet The positive electrode sheet was prepared by replacing the P-HNBR in Example 1 with a phosphorus-containing hydrogenated nitrile butadiene rubber in the main chain, while the remaining positive electrode formulation, slurry dispersion, coating, drying and rolling processes were the same as in Example 1.

[0072] Step 5: Fabrication of solid-state batteries The solid-state battery was assembled using the same method as in Example 1.

[0073] Comparative Example 3 This comparative example is used to illustrate the solid-state battery and its preparation method disclosed in this invention, including most of the operation steps in Example 1, the difference being: Except for replacing allylphosphonate dimethyl ester in Example 1 with methyl 10-undecenoate, the other conditions were the same as in Example 1, and the resulting product was denoted as E-HNBR.

[0074] Comparative Example 4 This embodiment illustrates the solid-state battery and its preparation method disclosed in this invention, including most of the operational steps in Example 1, with the following differences: Except for replacing allylphosphonic acid dimethyl ester in Example 1 with allyltrimethoxysilane, the other conditions were the same as in Example 1, and the resulting product was denoted as Si-HNBR.

[0075] Performance testing The hydrogenated nitrile butadiene binder sample and the positive electrode obtained above were subjected to the following performance tests: Characteristic element content test: The mass fraction of characteristic elements (such as phosphorus or silicon) in each hydrogenated nitrile butadiene binder sample was determined by an elemental analyzer. The mass fraction of characteristic elements was used to characterize the end group content. Three parallel samples were tested in each group, and the average value was taken as the final result.

[0076] Mechanical property testing: Each hydrogenated nitrile butadiene binder sample was dissolved in chlorobenzene solvent, dried and prepared into a strip with a length, width and thickness of 2cm × 1cm × 0.2cm. The tensile strength and elongation at break of each strip were tested using a universal testing machine. Five parallel samples were tested in each group, and the average value was taken as the final result.

[0077] 180° Peel Strength Test: A universal testing machine was used to test the 180° peel strength of the positive electrode material layer on the positive electrode sheet. The peel rate was 50 mm / min. The average force value during the stable peel stage was recorded, and the initial 180° peel strength (unit: N / m) was calculated. The positive electrode sheet was assembled into a solid-state battery and then disassembled after 200 cycles of 0.5C charge-discharge. The positive electrode sheet was then removed and the 180° peel strength was tested again using the same method. The peel strength retention rate after cycling was calculated: Peel strength retention rate after cycling (%) = (peel strength after cycling / initial peel strength) × 100%. Five parallel samples were tested in each group, and the average value was taken as the final result.

[0078] The test results are entered into Table 1.

[0079] Table 1 As can be seen from the test results in Table 1, compared with Comparative Example 1 which does not contain functional end groups, all examples of end-functionalized modified hydrogenated nitrile butadiene rubber prepared by the method of the present invention showed significant improvements in the initial peel strength and peel strength retention rate of the corresponding positive electrode sheets. This indicates that introducing polar functional groups at the molecular chain end can effectively improve the interfacial bonding ability of the binder to the positive electrode active particles and the current collector, and improve the interfacial structural stability during solid-state battery cycling.

[0080] In contrast to Comparative Example 2, which introduces functional groups into the main chain via copolymerization, the end-functionalized hydrogenated nitrile butadiene rubber prepared by the method of this invention exhibits superior tensile strength, initial peel strength, and peel strength retention rate after cycling, all within similar characteristic element content. This is because the present invention introduces functional groups only at the ends of the molecular chain, without disrupting the regular structure of the hydrogenated nitrile butadiene main chain. This allows for improved interfacial adhesion while preserving the excellent mechanical properties of the polymer itself, making it more suitable for the performance requirements of binders in solid-state battery cathodes.

[0081] Test results of Examples 1, 3, and 4, which replaced different types of functional end groups, show that different types of polar functional end groups can effectively improve the interfacial bonding performance of the binder. Among them, the phosphine-containing end group has the most prominent improvement effect and is more suitable for solid-state battery cathode systems.

[0082] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A solid-state battery, characterized in that, The device includes a solid electrolyte layer, a positive electrode, and a negative electrode. The solid electrolyte layer is located between the positive electrode and the negative electrode. The positive electrode includes a hydrogenated nitrile butadiene binder, which comprises a hydrogenated nitrile butadiene binder main chain and functional groups located at the ends of the hydrogenated nitrile butadiene binder main chain. The functional groups include phosphine-containing groups. The characteristic element of the phosphine-containing groups is phosphorus (P), and the content of the characteristic element in the functional groups is 0.1% to 3% based on the total mass of the hydrogenated nitrile butadiene binder. The phosphine-containing group is shown in structural formula 1: R1-R2-* Structural Formula 1 Wherein, R1 is selected from phosphate ester groups, R2 is selected from C2~C10 alkylene groups, and * indicates the connection site between the functional group and the hydrogenated butyronitrile backbone; The degree of hydrogenation of the hydrogenated butyronitrile backbone is ≥99%; The hydrogenated nitrile butadiene binder is prepared by the following method: Nitrile rubber is dissolved in an organic solvent to obtain a nitrile rubber solution. A functionalized metathesis reaction is carried out in the presence of an olefin metathesis catalyst and a functionalized olefin chain transfer agent to obtain modified nitrile rubber with functional groups at the ends of the molecular chains; the functional groups include phosphine-containing groups. Hydrogen gas is introduced into the adhesive solution of modified nitrile butadiene rubber to carry out a hydrogenation reaction, thereby obtaining the hydrogenated nitrile butadiene adhesive.

2. The solid-state battery according to claim 1, characterized in that, The positive electrode includes a positive electrode material layer, which includes a positive electrode active material, a solid electrolyte, a conductive agent, and the hydrogenated nitrile butadiene binder. The mass content of the hydrogenated nitrile butadiene binder is 0.5% to 5% based on the total mass of the positive electrode material layer as 100%.

3. The solid-state battery according to claim 1, characterized in that, The functionalized olefin chain transfer agent includes one or more of allyl phosphonate dimethyl ester and allyl trimethoxysilane.

4. The solid-state battery according to claim 1, characterized in that, The acrylonitrile content of the hydrogenated butyronitrile backbone is 15wt%~50wt%.

5. The solid-state battery according to claim 1, characterized in that, The solid electrolyte in the solid electrolyte layer includes one or more of oxide solid electrolytes, sulfide solid electrolytes, halide solid electrolytes, and polymer solid electrolytes; the positive electrode active material in the positive electrode material layer includes one or more of lithium iron phosphate, lithium manganese iron phosphate, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and lithium cobalt oxide.

6. The method for preparing a solid-state battery according to any one of claims 1 to 5, characterized in that, Includes the following steps: A positive electrode slurry is prepared by mixing the hydrogenated nitrile butadiene binder, positive electrode active material, solid electrolyte, and conductive agent; the positive electrode slurry is coated onto a positive electrode current collector, dried, and rolled to form a positive electrode; a solid electrolyte layer is placed between the positive and negative electrodes, and the battery is encapsulated to obtain a solid-state battery. The hydrogenated nitrile butadiene binder is prepared by the following method: Nitrile rubber is dissolved in an organic solvent to obtain a nitrile rubber solution. A functionalized metathesis reaction is carried out in the presence of an olefin metathesis catalyst and a functionalized olefin chain transfer agent to obtain modified nitrile rubber with functional groups at the ends of the molecular chains; the functional groups include phosphine-containing groups. Hydrogen gas is introduced into the adhesive solution of modified nitrile butadiene rubber to carry out a hydrogenation reaction, thereby obtaining the hydrogenated nitrile butadiene adhesive.

7. The method for preparing a solid-state battery according to claim 6, characterized in that, The acrylonitrile content of the nitrile rubber is 15wt%~50wt%, and the mass concentration of the nitrile rubber solution is 1%~15%; the amount of the olefin metathesis catalyst is 0.01%~1% of the mass of the nitrile rubber; the amount of the functionalized olefin chain transfer agent is 0.1%~5% of the mass of the nitrile rubber; the temperature of the functionalized metathesis reaction is 40~80℃, and the reaction time is 2~24 h; the temperature of the hydrogenation reaction is 80~150℃, and the reaction time is 6~48 h.

8. The method for preparing a solid-state battery according to claim 6, characterized in that, The olefin metathesis catalyst comprises (1,3-diisopropylimidazolium-2-yl)(tricyclohexylphosphine)benzyl ruthenium dichloride, benzyl dichlorobis(tricyclohexylphosphine)ruthenium, (1,3-dimethoxymethyl-4,5-dihydroimidazolium-2-yl)(tricyclohexylphosphine)benzyl ruthenium dichloride, (1,3-dimethoxymethyl-4,5-dihydroimidazolium-2-yl)[bis(3-bromopyridine)]benzyl ruthenium dichloride, (1,3-dimethoxymethyl-4,5-dihydroimidazolium-2-yl)[bis(3-bromopyridine)]benzyl ruthenium dichloride, and (1,3-dimethoxymethyl-4,5-dihydroimidazolium-2-yl)[bis(3-bromopyridine)]benzyl ruthenium dichloride, etc. One or more of the following: trimethyl-4,5-dihydroimidazolium-2-yl)(2-isopropoxybenzyl)ruthenium dichloride, (1,3-bis-(2,4,6-trimethylphenyl)-2-imidazolium-yl)dichloro(o-isopropoxybenzyl)ruthenium, dichloro(o-isopropoxyphenyl)(tricyclohexylphosphine)ruthenium, and bis(tricyclohexylphosphine)-3-methyl-2-butenyl ruthenium dichloride; wherein the functionalized olefinic chain transfer agent includes dimethyl allylphosphonate.