Cyclization of polyacrylonitrile-zinc composite modified lithium metal negative electrode copper current collector, and preparation method and application thereof
By modifying the copper current collector of lithium metal anode with cyclized polyacrylonitrile-zinc composite, the problems of lithium dendrites and dead lithium are solved by utilizing the synergistic effect of the CPAN buffer layer and the zinc lithiophilic layer. This achieves a simple and efficient modification of lithium metal batteries, which is suitable for industrial production.
Patent Information
- Application Number
- CN202611220281.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-12
- Publication Date
- 2026-11-24
AI Technical Summary
Existing copper current collector modification technologies cannot simultaneously achieve uniform lithium-ion conduction, deposition volume buffering, and uniform lithium nucleation induction, resulting in severe lithium dendrite and dead lithium problems. Furthermore, traditional composite modification processes are complex, consume high-temperature energy, and have expensive raw material costs, making them difficult to adapt to large-scale deep processing production lines for electrolytic copper foil.
A cyclized polyacrylonitrile-zinc composite modified lithium metal anode copper current collector is adopted. Through the synergistic effect of the CPAN buffer layer and the zinc lithiophilic layer, uniform lithium ion conduction, deposition volume buffering and uniform lithium nucleation are achieved, reducing the electrode interface impedance. A simple three-step process of coating, annealing and electrodeposition is adopted.
It significantly improves the cycle stability of lithium metal batteries, reduces electrode interface impedance, suppresses dendrite and dead lithium formation, is suitable for continuous industrial production of copper foil, and has low cost and simple process.
Smart Images

Figure CN123162199A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the fields of metallurgical functional new materials and electrochemical energy storage battery technology, specifically to a cyclized polyacrylonitrile-zinc composite modified lithium metal anode copper current collector and its preparation method and application. Background Technology
[0002] Lithium metal has a capacity of 3860 mAh·g -1 Lithium metal anodes are among the most promising anode materials for energy storage batteries due to their ultra-high theoretical specific capacity and extremely low electrochemical reduction potential. However, when lithium metal is deposited on the surface of traditional commercial copper current collectors, it is prone to uneven deposition, forming lithium dendrites that can pierce the battery separator, causing safety issues such as short circuits and thermal runaway. Furthermore, lithium metal can form "dead lithium" that cannot participate in electrochemical reactions, leading to capacity decay, accelerated battery aging, and shortened cycle life. In addition, compared to graphite intercalation reactions, lithium metal deposition / dissolution involves significant volume changes, easily causing electrode pulverization, further exacerbating dendrite growth and battery performance degradation, thus limiting the application of lithium metal anodes.
[0003] Currently, copper current collector modification mainly falls into two technical routes: single polymer coating modification and single metal lithiophilic coating modification. Single cyclized polyacrylonitrile (CPAN) coated copper current collectors (Cu@CPAN) utilize the N2 and N3 generated after PAN cyclization to induce uniform Zn metal nucleation and growth, constructing lithium-ion transport channels. The polymer's own mechanical toughness buffers lithium deposition volume expansion, suppressing dendrites and dead lithium to some extent. However, pure CPAN has lower electronic conductivity than metallic copper, resulting in relatively high battery interface impedance before cycling. During long cycles, the polymer coating is prone to cracking and damage, limiting the improvement in lithium deposition uniformity. Single zinc coating modified copper current collectors (Cu@Zn) utilize the alloying effect of zinc and lithium to reduce lithium nucleation overpotential, inducing uniform lithium deposition and exhibiting excellent conductivity. However, metallic zinc lacks a volume buffer structure, and electrode damage during cycling can easily shorten the lifespan of the CZ current collector. A composite lithium metal anode, its preparation method, and battery, disclosed in CN109742323A, employs a single metal transition layer as the functional layer, effectively improving the bonding strength at the copper-lithium interface and the overall conductivity of the electrode. However, it lacks a flexible organic buffer framework, resulting in limited effectiveness in controlling the large volume deformation during lithium deposition / stripping. Further improvements are needed in suppressing lithium dendrites and enhancing cycle life under long-term cycling conditions. Existing modification schemes all utilize a single functional layer, failing to simultaneously address the triple requirements of structural buffering, ion conduction, and lithiophilic induction. Furthermore, traditional composite modification processes are complex, energy-intensive at high temperatures, and costly in raw materials, making them unsuitable for large-scale deep processing lines of electrolytic copper foil. Therefore, developing a short-process, low-cost composite copper current collector with dual synergistic modification effects is of significant engineering and scientific research value in solving common industry problems such as lithium dendrite formation, dead lithium, and cycle degradation. Summary of the Invention
[0004] To overcome the above technical problems, the present invention aims to provide a cyclized polyacrylonitrile-zinc composite modified lithium metal anode copper current collector, its preparation method and application. Through the synergistic effect of the CPAN buffer layer and the zinc lithiophilic layer, uniform lithium ion conduction, deposition volume buffering and uniform lithium nucleation induction are achieved simultaneously, reducing electrode interface impedance and significantly improving the cycle stability of lithium metal batteries. The whole process is green and simple, and is suitable for continuous industrial production of copper foil.
[0005] To achieve the above objectives, the technical solution adopted by the present invention is as follows: A method for preparing a cyclized polyacrylonitrile-zinc composite modified lithium metal anode copper current collector includes the following steps; Step 1: Substrate pretreatment: Commercial electrolytic copper foil with a thickness of 7~11μm was selected, and the surface oxide film and rolling oil were removed by dilute acid washing. After cleaning with deionized water and ethanol, it was dried to obtain a clean conductive copper substrate. Step 2: Preparation of polyacrylonitrile precursor coating: Polyacrylonitrile (PAN) was dissolved in N-methyl-2-pyrrolidone and stirred until completely dissolved to prepare a transparent precursor solution. The transparent precursor solution was uniformly coated on one side of the clean conductive copper substrate. The thickness of the PAN dry film after drying was controlled to be 10~20 μm. After drying, Cu@PAN composite electrode was obtained. Step 3: Inert atmosphere thermal circulation: The Cu@PAN composite electrode was placed in a tube furnace and argon gas was continuously introduced to isolate it from air. The annealing process was used to keep it at a certain temperature. The PAN molecular chain underwent cyclization and dehydrogenation reactions to generate cyclized polyacrylonitrile (CPAN) rich in pyridine N and graphite N conductive active sites. After natural cooling, the Cu@CPAN electrode intermediate substrate was obtained. Step 4: Constant current electrodeposition of zinc layer: The Cu@CPAN electrode substrate was attached to a glass slide, exposing only the side coated with CPAN. Metal Zn was deposited in H2SO4 solution. The deposited product was washed with water and ethanol and then dried at low temperature to obtain a cyclized polyacrylonitrile-zinc composite modified lithium metal anode copper current collector (Cu@CPAN@Zn).
[0006] In step 1, acid washing is performed using 0.5 mol / L dilute sulfuric acid.
[0007] In step 2, 0.05~0.15 g of polyacrylonitrile (PAN) is dissolved in 0.8~1.2 mL of N-methyl-2-pyrrolidone and stirred at 40~60℃ until completely dissolved, resulting in a uniform, intact coating without cracks.
[0008] The annealing process in step 3 is as follows: The process involves holding the sample at 380~420℃ for 0.8~1.2 h. Under these conditions, PAN cyclization is complete, and the content of pyridine N and graphite N active sites is the highest, while avoiding high-temperature oxidation of the copper substrate.
[0009] Furthermore, the electrodeposition parameters for step 4 are as follows: In a 1 mol / L H₂SO₄ solution, at a concentration of 0.8–1.2 mA·cm⁻¹ -2 Current density deposition: 0.08~0.12 mAh·cm -2 Metallic Zn. Under these parameters, zinc grows uniformly in the form of hexagonal nanosheets with dense, non-agglomerated sheets and a stable size controlled at around 1 μm.
[0010] Using commercial copper foil as a substrate, polyacrylonitrile as a cyclization precursor, and metallic zinc as a lithium-affinity modification layer, the pyridine N and graphitic N in the cyclized polyacrylonitrile serve as heterogeneous nucleation sites, which can reduce the zinc deposition nucleation barrier and regulate the zinc electrodeposition kinetics, resulting in fine, dense zinc nanosheets without significant agglomeration. Simultaneously, continuous lithium-ion transport channels are constructed to buffer lithium deposition volumetric strain. Furthermore, by controlling the annealing temperature and electrodeposition capacity, the microstructure of the composite layer and the electrode interface kinetics can be directionally regulated, simultaneously altering the battery cycle stability and interfacial impedance.
[0011] As the annealing temperature gradually increases, the degree of cyclization reaction of polyacrylonitrile continues to deepen, the density of conductive nitrogen active sites on the surface increases synchronously, the density of zinc deposition nucleation increases, and the size of zinc nanosheets is refined and the distribution uniformity is improved. However, when the annealing temperature exceeds 420℃, it will cause slight oxidation of the copper substrate, increase the interfacial contact impedance, and weaken the electrochemical performance of the current collector. When the annealing temperature is below 380℃, it will lead to insufficient PAN cyclization, insufficient conductive nitrogen sites, coarse zinc deposition, and reduced CPAN ion conductivity.
[0012] As the zinc electrodeposition capacity increases, the integrity of the surface zinc coverage continuously improves, the lithium nucleation overpotential gradually decreases, and the uniformity of lithium deposition is improved. However, excessively high deposition capacity can lead to an overly thick zinc layer, increasing the overall electrode resistance and making the zinc layer prone to detachment during cycling. When the deposition capacity is insufficient, the copper substrate is locally exposed. The exposed areas lack lithium-inducible sites, resulting in a high lithium-ion nucleation barrier and the formation of coarse lithium dendrites under long cycling. To simultaneously achieve structural buffering and uniform lithium deposition, a cyclized polyacrylonitrile interlayer is introduced. Its flexible framework accommodates the volume expansion of lithium, and a large number of heterogeneous nucleation sites assist in the uniform growth of zinc, thereby synergistically modifying the surface zinc layer.
[0013] Cyclomeric polyacrylonitrile-zinc composite modified lithium metal anode copper current collector has a surface covered by a dense zinc nanosheet layer. The zinc nanosheets have a hexagonal sheet structure with an average size of 0.5~1.5 μm and are uniformly distributed without agglomeration. Compared with zinc directly deposited on the copper foil surface (CZ), the zinc nanosheets on the CCZ surface are finer and denser, and the deposit morphology is smoother.
[0014] At the bottom of the zinc nanosheets is a non-nanosheet array structure substrate located on the surface of the cyclized polyacrylonitrile (CPAN) coating. This substrate is in the form of sheet-like crystals with uniform zinc distribution. The CPAN coating surface itself is relatively flat, but after annealing, a small number of microcracks appear on the surface. This is due to the volume change caused by the thermal cyclization of polyacrylonitrile molecules during the heat treatment process.
[0015] The entire composite current collector cross-section shows a distinct layered structure, consisting of a bottom layer of copper foil, an intermediate cyclized polyacrylonitrile buffer layer, and a surface layer of dense zinc nanosheets.
[0016] The application of cyclized polyacrylonitrile-zinc composite modified lithium metal anode copper current collector in lithium metal battery anodes: a coin cell (CR2025) was assembled using Cu@CPAN@Zn as the current collector and lithium metal as the counter electrode; the electrolyte was prepared by dissolving 0.8~1.2 mol / L lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) as the lithium salt in a 1:1 volume ratio mixed solvent of 1,3-dioxolane / 1,2-dimethoxyethane, with 1%~3% LiNO3 added as an additive; the separator was a Celgard 2500 polyethylene membrane.
[0017] The beneficial effects of this invention are: The core materials used in this invention, CPAN and Zn, are widely available and readily available. The equipment is universal, resulting in low-cost large-scale production and easy industrialization and market promotion. The preparation process consists of only three short steps: coating, annealing, and electrodeposition. The process is simple, compatible with existing copper foil deep processing and battery electrode production lines, and can directly replace traditional copper foil. It is suitable for lithium metal batteries and outperforms existing products.
[0018] The cyclized polyacrylonitrile layer is rich in pyridine nitrogen and graphitic nitrogen active sites, which can serve as heterogeneous nucleation sites for zinc deposition, regulating the generation of fine, dense, and non-agglomerated zinc nanosheets. At the same time, the flexible polymer framework can buffer the huge volume stress of lithium deposition, preventing peeling and detachment of the coating during the coating cycle, and enabling the current collector structure to cycle stably for a long time. Relying on the synergistic effect of CPAN ion channels and zinc lithiophilic layer, the uniformity of lithium deposition is greatly improved, and the continuous generation of dendrites and dead lithium is inhibited.
[0019] The Cu@CPAN@Zn composite current collector prepared in this invention exhibits a controllable microstructure, low electrode interface impedance, and excellent long-term cycling stability, making it suitable for lithium metal battery anode systems and applicable to new energy fields such as power batteries and large-scale energy storage batteries. Its controllable microstructure stems from the uniform Zn nucleation driving force provided by the N2 and N3 sites in the CPAN coating, guiding Zn to deposit uniformly in a fine and dense nanosheet morphology. During cycling, the enhanced electrochemical activity of CPAN and the synergistic effect of Zn's conductivity and lithiophilicity reduce the electrode interface impedance. The excellent long-term cycling stability benefits from the mechanical support of the CPAN framework, effectively suppressing volume expansion and dead lithium accumulation. Simultaneously, Zn's lithiophilic properties induce uniform lithium ion deposition within the CPAN, alleviating localized stress concentration.
[0020] The electrochemical performance of lithium metal anodes is greatly influenced by the surface morphology of the current collector, the interfacial lithiophilicity, and the buffer structure. The composite current collector prepared according to the method of this invention, after standard electrochemical characterization, exhibits a lithium deposition capacity of 1 mA·cm⁻¹. -2 1 mAh·cm -2 Under certain conditions, the coulombic efficiency of the half-cell reaches 95.2% after 100 cycles, and the symmetrical cell maintains a low overpotential of 20 mV after 420 hours of stable cycling. The interface impedance is as low as 6.2 Ω·cm after 30 cycles. 2 This study demonstrates that the composite modification of CPAN and zinc can significantly optimize lithium-ion deposition kinetics, effectively solving the problems of lithium dendrite induction and short cycle life in traditional copper foil, thus enabling its application in high-energy-density energy storage devices. Attached Figure Description
[0021] Figure 1 SEM images and schematic diagrams of lithium deposited on different current collectors. Detailed Implementation
[0022] The present invention will now be described in further detail with reference to the accompanying drawings.
[0023] Comparative Example 1 The copper current collector preparation and battery testing method of this comparative example includes the following steps: (1) Substrate pretreatment: Take a 9 μm thick commercial electrolytic copper foil, soak it in dilute sulfuric acid for 3 min to remove the surface oxide layer and rolling oil stains, and then ultrasonically clean it for 10 min each with deionized water and anhydrous ethanol. Finally, dry it in a forced-air drying oven at 100℃ to obtain a pure copper substrate. (2) Button cell assembly: CR2025 button cells were assembled using blank copper foil as the current collector and lithium metal as the counter electrode; 1.0 mol / L lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) was used as the lithium salt, dissolved in a 1:1 volume ratio of 1,3-dioxolane / 1,2-dimethoxyethane mixed solvent, and 2% LiNO3 was added as an additive to prepare the electrolyte; Celgard 2500 polyethylene membrane was used as the separator, and the entire encapsulation process was completed in an argon glove box; (3) Electrochemical testing conditions: Electrochemical impedance spectroscopy (EIS) test frequency range: 100 kHz - 0.01 Hz, amplitude: 5 mV. Linear voltammetry (LSV) test range: 0 - 1 V, scan rate: 0.01 V·s. -1 Simultaneously conduct half-cell cycle tests and symmetrical cell constant current long-cycle tests.
[0024] Test results: The efficiency of the half-cell dropped sharply after 40 cycles, and the stability of the symmetrical cell dropped sharply after 120 hours of operation.
[0025] Figure 1 (ac) is the SEM image of lithium deposition in this comparative example; the top view shows that the Li deposited on the copper foil surface is uneven, and the side view shows that the lithium deposit is filled with a large number of pores, which will generate a large amount of dead lithium during battery cycling and consume electrolyte. Schematic diagram of lithium deposition on Cu surface ( Figure 1 m), it can be seen that a large number of moss-like lithium dendrites are formed on the surface of the copper foil.
[0026] Comparative Example 2 The difference between Comparative Example 2 and Comparative Example 1 is that after completing the substrate pretreatment in step (1), PAN coating and thermal cyclization reaction at 400℃ are performed.
[0027] Test results: The symmetrical battery structure was damaged after 105 hours of cycling; the interfacial impedance dropped to 6.9 Ω·cm after 30 cycles. 2 .
[0028] Figure 1 (df) is the SEM image of lithium deposition in this comparative example; it can be seen that the CC surface is relatively smooth after lithium deposition, preserving the CC structure. A small amount of cracking and porosity are observed during the lithium deposition and stripping process, revealing the internal lithium (…). Figure 1 n); according to the side view ( Figure 1 f) It was found that the CPAN volume expansion was very serious and it also suffered some damage. However, due to the good mechanical strength of CPAN, the electrode did not pulverize. This proves that CPAN can regulate the volume change of lithium during battery cycling, but structural damage still exists.
[0029] Comparative Example 3 The difference between Comparative Example 3 and Comparative Example 1 is that 0.1 mAh·cm⁻¹ was electrodeposited directly on the surface of the acid-washed copper foil. -2 Metallic zinc.
[0030] Test results: In the initial stage of cycling, the voltage of the symmetrical battery fluctuated drastically due to changes in the volume of the electrode materials; after 30 cycles, the interfacial impedance decreased to 10.2 Ω·cm. 2 .
[0031] Figure 1 (gi) is the SEM image of the lithium deposition in this comparative example; the lithium deposition is more uniform and smooth, as shown in the side view. Figure 1 i) also reflects the dense deposition morphology of lithium. Schematic diagram of lithium deposition on CZ surface ( Figure 1 (o) It can be seen that lithium dendrites, as seen on the surface of the copper foil, did not form.
[0032] Example 1 The preparation method of the cyclized polyacrylonitrile-zinc composite modified lithium metal anode copper current collector in this embodiment includes the following steps: (1) Copper substrate pretreatment: Take a 9 μm thick commercial electrolytic copper foil, soak it in dilute sulfuric acid for 3 min to remove the surface oxide layer and rolling oil stains, and then ultrasonically clean it for 10 min each with deionized water and anhydrous ethanol. Finally, dry it in a forced-air drying oven at 100℃ to obtain a clean conductive copper substrate. (2) Preparation of polyacrylonitrile precursor coating: 0.1 g of polyacrylonitrile was dissolved in 1 mL of N-methyl-2-pyrrolidone and stirred at 50 °C until completely dissolved to obtain a transparent and uniform PAN coating solution; the PAN solution was uniformly coated on one side of the pretreated copper foil and dried to obtain Cu@PAN electrode sheet. (3) Argon atmosphere thermal cyclization treatment: The Cu@PAN electrode is placed in a tube furnace and argon is continuously introduced to isolate the air. The temperature is raised to 400℃ and kept at a constant temperature for 1 h before being naturally cooled to room temperature. PAN undergoes a dehydrogenation cyclization reaction to generate a CPAN layer rich in pyridine N and graphite N, thus obtaining the Cu@CPAN composite substrate. (4) Constant current electrodeposition of zinc functional layer: Prepare 1 mol / L H2SO4 electrolyte, use Cu@CPAN as working electrode and pure copper sheet as counter electrode, and electrode deposit at 1 mA·cm -2 Electrodeposition at constant current density resulted in a zinc deposition capacity controlled at 0.1 mAh·cm⁻¹. -2 After deposition, the material was rinsed with deionized water and then with anhydrous ethanol. After drying, Cu@CPAN@Zn(CCZ) composite current collector was obtained. (5) Assembly and electrochemical testing of button cells: CR2025 button cells were assembled using CCZ as the negative current collector and lithium metal as the counter electrode in this embodiment. 1.0 mol / L LiTFSI was used as the lithium salt, dissolved in a 1:1 volume ratio of 1,3-dioxolane / 1,2-dimethoxyethane mixed solvent, and 2% LiNO3 was added as an additive to prepare the electrolyte. Celgard 2500 polyethylene membrane was used as the separator. The entire battery assembly and packaging were completed in a glove box filled with high-purity argon.
[0033] Electrochemical performance of the composite current collector in this embodiment was tested at room temperature with a current density of 1 mA·cm⁻¹. -2 Single lithium deposition capacity 1 mAh·cm -2 The half-cell coulombic efficiency remained stable at 95.2% after 100 cycles; the symmetric cell maintained a low overpotential of 20 mV after 420 hours of long-term cycling testing; and the electrochemical interfacial impedance decreased to as low as 6.2 Ω·cm after 30 cycles. 2 .
[0034] Figure 1 (jl) is a SEM image of lithium deposition in this embodiment; the deposit is smoother and has fewer cracks and pores. Figure 1 (l) It can be seen that the electrode structure has not been significantly damaged, and a morphology of lithium metal growing along the Zn crystal direction has been observed. Simultaneously, due to the uniform deposition of lithium within the CPAN ( Figure 1 (p) CCZ can suppress the formation of dead lithium and maintain the CPAN structure from being destroyed during cycling.
[0035] Example 2 The difference between this embodiment and embodiment 1 is that the thermal circulatory annealing temperature in step (3) is adjusted to 380°C.
[0036] Electrochemical performance of the composite current collector in this embodiment was tested: Under the same test conditions, the coulombic efficiency of the half-cell after 100 cycles was 93.7%, the stable cycling time of the symmetric cell was 360 h, and the interfacial impedance after 30 cycles was 7.5 Ω·cm. 2 .
[0037] Example 3 The difference between this embodiment and embodiment 1 is that the thermal circulatory annealing temperature in step (3) is adjusted to 420°C.
[0038] Electrochemical performance of the composite current collector in this embodiment was tested: Under the same test conditions, the coulombic efficiency of the half-cell after 100 cycles was 94.1%, the stable cycling time of the symmetric cell was 385 h, and the interfacial impedance after 30 cycles was 8.1 Ω·cm. 2 .
[0039] Example 4 The preparation method of the cyclized polyacrylonitrile-zinc composite modified lithium metal anode copper current collector in this embodiment includes the following steps: (1) The copper substrate pretreatment, PAN coating preparation and 400℃ thermal cyclone process steps are completely consistent with those in Example 1; (2) Adjustment of electrodeposition steps: The electrolyte system remains unchanged, and the constant current deposition density is changed to 0.8 mA·cm. -2 The zinc deposition capacity remained at 0.1 mAh·cm⁻¹. -2 The subsequent water washing, ethanol rinsing, and drying processes remain unchanged; (3) The button cell assembly and electrochemical testing system are the same as those in Example 1.
[0040] Electrochemical performance of the composite current collector in this embodiment was tested: Under the same test conditions, the coulombic efficiency of the half-cell after 100 cycles was 94.5%, the stable cycle time of the symmetric cell was 392 h, and the interfacial impedance after 30 cycles was 6.8 Ω·cm. 2 .
[0041] Example 5 The difference between this embodiment and embodiment 4 is that the zinc electrodeposition capacity in step (4) is adjusted to 0.08 mAh·cm⁻¹. -2 .
[0042] Electrochemical performance of the composite current collector in this embodiment was tested: Under the same test conditions, the coulombic efficiency of the half-cell after 100 cycles was 93.9%, the stable cycle time of the symmetric cell was 370 h, and when the deposition capacity was insufficient, the copper substrate was locally exposed. The exposed area had no lithium-inducible sites, and lithium dendrites were easily formed under long-term cycling.
[0043] In summary, this invention employs a short process of coating-inert atmosphere annealing-constant current electrodeposition to prepare Cu@CPAN@Zn composite copper current collectors. The raw materials are widely available, the preparation conditions are mild, and the process is compatible with existing copper foil deep processing and battery electrode production lines. By adjusting the annealing temperature, deposition current density, and zinc deposition capacity, precise control over the surface morphology and interfacial electrochemical properties of the current collector can be achieved. Through the synergistic modification of the CPAN buffer layer and the surface zinc, continuous lithium-ion transport channels can be constructed, buffering the charge-discharge volume effect and inducing uniform lithium deposition. The composite current collector prepared using this method exhibits high coulombic efficiency, low interfacial impedance, and excellent long-cycle stability, making it suitable for applications in new energy fields such as power batteries and large-scale energy storage batteries.
Claims
1. A method for preparing a cyclized polyacrylonitrile-zinc composite modified lithium metal anode copper current collector, characterized in that, Includes the following steps; Step 1: Select commercial electrolytic copper foil with a thickness of 7~11μm, wash it with dilute acid to remove the surface oxide film and rolling oil stains, clean it with deionized water and ethanol and then dry it to obtain a clean conductive copper substrate. Step 2: Dissolve polyacrylonitrile (PAN) in N-methyl-2-pyrrolidone and stir until completely dissolved to prepare a transparent precursor solution; A transparent precursor solution was uniformly coated on one side of the clean conductive copper substrate. The thickness of the PAN dry film after drying was controlled to be 10~20 μm. After drying, Cu@PAN composite electrode was obtained. Step 3: Place the Cu@PAN composite electrode in a tube furnace, continuously introduce argon gas to isolate it from air, and maintain the temperature through an annealing process; after natural cooling, the Cu@CPAN electrode intermediate substrate is obtained; Step 4: The Cu@CPAN electrode intermediate substrate is attached to a glass slide, exposing only the side coated with CPAN. Metal Zn is deposited in H2SO4 solution. The deposited product is washed with water and ethanol and then dried at low temperature to obtain cyclized polyacrylonitrile-zinc composite modified lithium metal anode copper current collector.
2. The preparation method of the cyclized polyacrylonitrile-zinc composite modified lithium metal anode copper current collector according to claim 1, characterized in that, In step 1, acid washing is performed using 0.5 mol / L dilute sulfuric acid.
3. The preparation method of the cyclized polyacrylonitrile-zinc composite modified lithium metal anode copper current collector according to claim 1, characterized in that, In step 2, 0.05~0.15 g of polyacrylonitrile is dissolved in 0.8~1.2 mL of N-methyl-2-pyrrolidone and stirred at 40~60℃ until completely dissolved, resulting in a uniform, intact coating without cracks.
4. The preparation method of the cyclized polyacrylonitrile-zinc composite modified lithium metal anode copper current collector according to claim 1, characterized in that, The annealing process in step 3 is as follows: Keep warm at 380~420℃ for 0.8~1.2 h.
5. The preparation method of the cyclized polyacrylonitrile-zinc composite modified lithium metal anode copper current collector according to claim 1, characterized in that, The specific electrodeposition parameters for step 4 are as follows: In a 1 mol / L H₂SO₄ solution, at a concentration of 0.8–1.2 mA·cm⁻¹ -2 Current density deposition: 0.08~0.12 mAh·cm -2 Metal Zn.
6. A cyclized polyacrylonitrile-zinc composite modified lithium metal anode copper current collector prepared by the method according to any one of claims 1-5, characterized in that, The surface is covered by a dense layer of zinc nanosheets, which are hexagonal sheet-like structures with an average size of 0.5~1.5 μm, and are uniformly distributed without agglomeration. At the bottom of the zinc nanosheets, there is a non-nanosheet array structure substrate located on the surface of the cyclized polyacrylonitrile coating. This substrate has a sheet-like crystalline morphology and the zinc element is uniformly distributed. The entire composite current collector cross-section shows a distinct layered structure, consisting of a bottom layer of copper foil, an intermediate cyclized polyacrylonitrile buffer layer, and a surface layer of dense zinc nanosheets.
7. The application of the cyclized polyacrylonitrile-zinc composite modified lithium metal anode copper current collector prepared by the method according to any one of claims 1-5, characterized in that, Cyclomeric polyacrylonitrile-zinc composite modified lithium metal anode copper current collector is used in lithium metal battery anodes. A coin cell is assembled using Cu@CPAN@Zn as the current collector and lithium metal as the counter electrode. The electrolyte is prepared by dissolving 0.8~1.2 mol / L lithium bis(trifluoromethanesulfonyl)imide as the lithium salt in a 1:1 volume ratio mixed solvent of 1,3-dioxolane / 1,2-dimethoxyethane, with 1%~3% LiNO3 added as an additive. The separator is a Celgard 2500 polyethylene membrane.
Citation Information
Patent Citations
Composite lithium metal negative electrode and preparation method thereof and battery
CN109742323A