A thermal safety type composite foil and a battery prepared thereby
By designing an anisotropic base film structure and a specific stretching process, and combining multifunctional chain extenders with PA6 blending, the problem of power failure of composite foils during battery thermal runaway was solved, thereby improving the thermal safety and strength of the battery.
Patent Information
- Application Number
- CN202611419583.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-14
- Publication Date
- 2026-11-24
AI Technical Summary
Existing composite foil materials slow down heat diffusion when the battery overheats locally, the base film layer cannot be disconnected, and the metal layer melts, making it difficult to completely cut off the power, resulting in uncontrollable thermal runaway propagation.
The base film is designed with an anisotropic structure, with low thermal shrinkage in the MD direction and high thermal shrinkage in the TD direction. The tabs extend in the TD direction. The base film is treated with a specific stretching process and combined with a multifunctional epoxy chain extender and PA6 blend to improve the thermal shrinkage control and strength of the base film.
When the battery temperature rises abnormally, the base film in the tab area quickly contracts and cuts off the power, effectively preventing the propagation of thermal runaway, improving the cell's resistance to expansion and processing feasibility, and ensuring battery safety.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery technology, specifically to a thermally safe composite foil and the battery made therefrom. Background Technology
[0002] Composite foil is a "sandwich" structure formed by depositing micron-thick metal layers on both the upper and lower surfaces of a polymer base film using a vacuum evaporation process. Compared to traditional pure metal foil, composite foil offers numerous advantages, including saving metal resources, reducing battery weight, increasing energy density, and enhancing battery puncture resistance. It is currently a popular research and development product in the battery field.
[0003] However, existing composite foil materials have the following technical defects in practical applications: the polymer substrates of composite current collectors, such as PET (polyethylene terephthalate), PI (polyimide), and PP (polypropylene), have low thermal conductivity and high toughness. When the battery is locally overheated, heat diffusion is slowed down, the base film layer cannot be disconnected, and the metal layer melts, making it difficult to completely cut off the power.
[0004] In summary, to address the aforementioned problems, this invention proposes a thermally safe composite foil and a battery made from it. Summary of the Invention
[0005] The purpose of this invention is to provide a thermally safe composite foil and a battery made therefrom, so as to solve the problems mentioned in the background art.
[0006] To solve the above-mentioned technical problems, the present invention provides the following technical solution: A thermally safe composite foil includes a base film and aluminum layers disposed on the upper and lower surfaces of the base film; The base film has an anisotropic structure with different thermal shrinkage rates in the longitudinal (MD) and transverse (TD) directions; The thermal shrinkage rate of the base film in the MD direction is lower than that in the TD direction; The base film is wound along the MD direction as the cell winding direction; The TD direction of the base membrane serves as the direction in which the tabs extend.
[0007] Furthermore, the composite foil is prepared by the following steps: (1) Mix polyethylene terephthalate (PET) masterbatch granules and plasticizer dioctyl phthalate (DOP), and dry to obtain a mixture; (2) The mixture is melt-extruded to obtain a semi-finished film; (3) The semi-finished film is preheated with infrared and stretched in one direction in sequence, with MD first and then TD. After stretching, MD is stretched again. Then heat set to obtain the base film. (4) Aluminum layers are deposited on the upper and lower surfaces of the base film by vacuum evaporation to obtain composite foil.
[0008] Furthermore, in step (1), the drying process conditions are: temperature 78-82℃, time 4-6h; The mass ratio of PET masterbatch granules to plasticizer DOP is (20-22):1.
[0009] Furthermore, the mixture also includes nylon 6 (PA6). The amount of PA6 added is 3-7 wt%.
[0010] Furthermore, the mixture also includes multifunctional epoxy chain extenders and antioxidants; The multifunctional epoxy chain extender uses a Schiff base-type tetrafunctional epoxy compound chain extender, with an addition amount of 0.4-0.6 wt%. The antioxidant used is Irganox 1010, with an addition amount of 0.1-0.3 wt%.
[0011] Furthermore, the infrared preheating temperature is 78-82℃.
[0012] Further, in step (1), the process conditions for melt extrusion are as follows: a T-type die in a flat extrusion die is used, the extrusion temperature is 200-210℃, the die gap is 1-1.05mm, and the cooling roller temperature is 40-42℃.
[0013] Furthermore, in step (1), the process conditions for longitudinal stretching are: longitudinal stretching temperature of 88-93℃, longitudinal stretching ratio of 2.5-3.2 times, and strain rate of 30-32% / s; The process conditions for transverse stretching are: transverse stretching temperature of 90-96℃, transverse stretching ratio of 2.7-3.5 times, and strain rate of 30-32% / s. The stretching ratio for secondary stretching is 1-2 times; The heat setting process conditions are: temperature 175-185℃, time 2-4s.
[0014] In the above technical solution, the base film of the composite foil is prepared by uniaxial stretching. The molecular chains are oriented in a single direction by directional stretching, thereby giving the film anisotropy, such as controllable thermal shrinkage rate. By designing the matching relationship between the tab extension direction, the cell winding direction and the base film stretching direction, a battery product that can precisely control the propagation of thermal runaway can be obtained.
[0015] In the above technical solution, by reducing the stretch ratio, the degree of molecular chain extension along the TD / MD direction decreases, the storage elastic stress of TD / MD decreases, and thus the thermal shrinkage rate of TD / MD decreases. Simultaneously, increasing the stretching temperature enhances the mobility of PET chain segments at higher temperatures, making chain relaxation more likely during stretching and resulting in lower orientation at the same stretching ratio. By adopting a method of stretching MD first and then TD, and then performing a second stretching on MD after the initial stretching, a multifunctional epoxy chain extender can be added to prevent changes in properties, thereby improving the melt strength and viscosity of PET and reducing the likelihood of breakage under multiple stretching conditions.
[0016] In the above technical solution, PET and PA6 are further mixed to significantly reduce the elongation of PET. PET and PA6 are typical thermodynamically incompatible systems. When simply melt-blended, PA6 will be dispersed in the PET matrix in particulate form, forming a clear phase interface. This interface is very thin and is prone to becoming a stress concentration point and initiating cracks when subjected to stress, causing the material to fracture under stress far below the theoretical value.
[0017] A battery is prepared by the following steps: Step 1: Coat the surface of the composite foil with a positive electrode active material slurry, dry and roll to obtain a positive electrode semi-finished product; Step 2: Stamp the edge of the positive electrode sheet in the TD direction to obtain a positive electrode sheet with a positive electrode tab; Step 3: Wind the positive electrode sheet along the MD direction of the base film to obtain the battery cell; Step 4: Place the battery cell into the casing, weld the tabs to the cover plate on the casing, seal, inject electrolyte, and form to obtain the battery.
[0018] Further, in step 1, the positive electrode active material slurry includes the following components by mass: 97 parts NCM811, 1 part carbon nanotubes, 0.5 parts Super P, 1.5 parts PVDF, and the solvent is NMP (N-methylpyrrolidone); the solid content of the positive electrode active material slurry is 25%.
[0019] Compared with the prior art, the beneficial effects achieved by the present invention are: This invention designs a novel aluminum alloy composite current collector, which has the following advantages: 1. This invention designs the composite foil base film as an anisotropic structure, utilizing the characteristics of low MD thermal shrinkage rate and high TD thermal shrinkage rate, and uses the TD direction with high thermal shrinkage rate as the tab extension direction; when the battery experiences abnormal temperature rise and reaches the thermal runaway temperature, the base film in the tab area is heated and shrinks violently in the transverse direction, and the resulting shrinkage stress can quickly break the tab, physically severing the connection between the cell and the external circuit, effectively preventing further propagation of thermal runaway.
[0020] 2. The present invention uses the longitudinal direction with low thermal shrinkage as the winding direction of the battery cell. After being treated by a specific stretching process, this direction has high tensile strength, which can effectively resist the expansion force generated by the volume expansion of the battery cell during the charge and discharge cycle and reduce the risk of foil tearing.
[0021] 3. This invention further preferably uses a blend of PET and PA6 as the base film material. PA6 is dispersed in particulate form within the PET matrix, forming a weak phase interface. This interface is prone to becoming a stress concentration point and initiating cracks under stress, making the base film more susceptible to brittle fracture during thermal runaway shrinkage, thereby further improving the sensitivity and reliability of tab breakage. Simultaneously, by adding a multifunctional epoxy chain extender, the melt strength and viscosity of PET can be improved while maintaining appropriate brittle fracture properties, avoiding fracture due to repeated stretching during processing, thus balancing processing feasibility and safety performance. Detailed Implementation
[0022] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0023] It should be noted that the following quantities are by weight. There are no special restrictions on the manufacturers of the raw materials involved in this invention. Exemplary examples include: in the following embodiments, the PET masterbatch granules are of type JSYG030, with an intrinsic viscosity of 0.60 dL / g, a moisture content of ≤0.10%, and a melting point of 245℃; and other raw materials are commercially available.
[0024] Schiff base type tetrafunctional epoxy compound chain extender is prepared by the following process: p-phenylenediamine and 3,4-dihydroxybenzaldehyde were added to anhydrous ethanol in a molar ratio of 1:2 and reacted at 60°C for 5 h under nitrogen protection. The mixture was then filtered, washed, and dried to obtain a Schiff base compound. The ratio of p-phenylenediamine to anhydrous ethanol was 1 g: 18 mL. Schiff base compound, epichlorohydrin, and tetrabutylammonium bromide were mixed at a mass ratio of 10:75:0.4 and reacted at 90°C for 5 hours under nitrogen protection. The temperature was then lowered to 60°C, and a 30% sodium hydroxide aqueous solution was added dropwise over 30 minutes. The reaction continued for 6 hours. The organic phase was washed, precipitated, filtered, and dried to obtain a Schiff base type tetrafunctional epoxy chain extender. The mass ratio of Schiff base compound to sodium hydroxide aqueous solution was 1:3.2.
[0025] The positive electrode active material slurry comprises the following components by mass: 97 parts NCM811, 1 part carbon nanotubes, 0.5 parts Super P, and 1.5 parts PVDF, with NMP as the solvent; the solid content of the positive electrode active material slurry is 25%.
[0026] Example 1: Includes the following steps: S1: Preparation of composite foil S1-1: Mix PET masterbatch granules and plasticizer DOP at a mass ratio of 20:1, and dry for 5 hours to obtain the mixture; S1-2: Add the mixture to a single screw extruder, select the T-type die in the flat extrusion die head, perform melt extrusion, extrusion temperature 200℃, die head gap 1mm, cooling roller temperature 40℃, to obtain a semi-finished film; S1-3: The semi-finished film is preheated with infrared radiation at 80℃; a multi-roll stretching machine is used for unidirectional stretching, with the stretching sequence being MD first and then TD. The stretching temperature in the MD direction is 88℃ with a stretching ratio of 2.5, and the stretching temperature in the TD direction is 90℃ with a stretching ratio of 2.7. The strain rate is 30% / s for both directions; after stretching, the MD direction is stretched a second time with a stretching ratio of 1.5; then heat-set at 180℃ for 3s, and rapidly cooled to room temperature to lock the molecular chain orientation, thus obtaining the base film; S1-4: Aluminum layers are deposited on the upper and lower surfaces of the base film by vacuum evaporation to obtain composite foil; S2: Battery fabrication S2-1: Coating the surface of the composite foil with a positive electrode active material slurry, drying and rolling to obtain a positive electrode semi-finished product; S2-2: Punch away the excess part at the edge of the positive electrode sheet in the TD direction to obtain a positive electrode sheet with a positive electrode tab; S2-3: The positive electrode sheet is wound along the MD direction of the base film to obtain the battery cell; S2-4: The battery cell is placed into the casing, the tabs are welded to the cover plate on the casing, and after sealing, liquid injection, and formation, the battery is obtained.
[0027] Example 2: Includes the following steps: S1: Preparation of composite foil S1-1: Mix PET masterbatch granules and plasticizer DOP at a mass ratio of 20:1, and dry for 5 hours to obtain the mixture; S1-2: Add the mixture to a single screw extruder, select the T-type die in the flat extrusion die head, perform melt extrusion, extrusion temperature 200℃, die head gap 1mm, cooling roller temperature 40℃, to obtain a semi-finished film; S1-3: The semi-finished film is preheated with infrared radiation at 80℃; a multi-roll stretching machine is used for unidirectional stretching, with the stretching sequence being MD first and then TD. The stretching temperature in the MD direction is 88℃ with a stretching ratio of 2.7, and the stretching temperature in the TD direction is 90℃ with a stretching ratio of 2.9. The strain rate is 30% / s for both directions; after stretching, the MD direction is stretched a second time with a stretching ratio of 1.5; then heat-set at 180℃ for 3s, and rapidly cooled to room temperature to lock the molecular chain orientation, thus obtaining the base film; S1-4: Aluminum layers are deposited on the upper and lower surfaces of the base film by vacuum evaporation to obtain composite foil; S2: Battery fabrication S2-1: Coating the surface of the composite foil with a positive electrode active material slurry, drying and rolling to obtain a positive electrode semi-finished product; S2-2: Punch away the excess part at the edge of the positive electrode sheet in the TD direction to obtain a positive electrode sheet with a positive electrode tab; S2-3: The positive electrode sheet is wound along the MD direction of the base film to obtain the battery cell; S2-4: The battery cell is placed into the casing, the tabs are welded to the cover plate on the casing, and after sealing, liquid injection, and formation, the battery is obtained.
[0028] Example 3: Includes the following steps: S1: Preparation of composite foil S1-1: Mix PET masterbatch granules and plasticizer DOP at a mass ratio of 20:1, and dry for 5 hours to obtain the mixture; S1-2: Add the mixture to a single screw extruder, select the T-type die in the flat extrusion die head, perform melt extrusion, extrusion temperature 200℃, die head gap 1mm, cooling roller temperature 40℃, to obtain a semi-finished film; S1-3: The semi-finished film is preheated with infrared radiation at 80℃; a multi-roll stretching machine is used for unidirectional stretching, with the stretching sequence being MD first and then TD. The stretching temperature in the MD direction is 88℃ with a stretching ratio of 2.9 times, and the stretching temperature in the TD direction is 90℃ with a stretching ratio of 3.1. The strain rate is 30% / s for both directions; after stretching, the MD direction is stretched a second time with a stretching ratio of 1.5 times; then heat-set at 180℃ for 3 seconds, and rapidly cooled to room temperature to lock the molecular chain orientation, thus obtaining the base film; S1-4: Aluminum layers are deposited on the upper and lower surfaces of the base film by vacuum evaporation to obtain composite foil; S2: Battery fabrication S2-1: Coating the surface of the composite foil with a positive electrode active material slurry, drying and rolling to obtain a positive electrode semi-finished product; S2-2: Punch away the excess part at the edge of the positive electrode sheet in the TD direction to obtain a positive electrode sheet with a positive electrode tab; S2-3: The positive electrode sheet is wound along the MD direction of the base film to obtain the battery cell; S2-4: The battery cell is placed into the casing, the tabs are welded to the cover plate on the casing, and after sealing, liquid injection, and formation, the battery is obtained.
[0029] Example 4: Includes the following steps: S1: Preparation of composite foil S1-1: Mix PET masterbatch granules and plasticizer DOP at a mass ratio of 20:1, and dry for 5 hours to obtain the mixture; S1-2: Add the mixture to a single screw extruder, select the T-type die in the flat extrusion die head, perform melt extrusion, extrusion temperature 200℃, die head gap 1mm, cooling roller temperature 40℃, to obtain a semi-finished film; S1-3: The semi-finished film is preheated with infrared radiation at 80℃; a multi-roll stretching machine is used for unidirectional stretching, with the stretching sequence being MD first and then TD. The stretching temperature in the MD direction is 88℃ with a stretching ratio of 3.1, and the stretching temperature in the TD direction is 90℃ with a stretching ratio of 3.3. The strain rate is 30% / s for both directions; after stretching, the MD direction is stretched a second time with a stretching ratio of 1.5; then heat-set at 180℃ for 3s, and rapidly cooled to room temperature to lock the molecular chain orientation, thus obtaining the base film; S1-4: Aluminum layers are deposited on the upper and lower surfaces of the base film by vacuum evaporation to obtain composite foil; S2: Battery fabrication S2-1: Coating the surface of the composite foil with a positive electrode active material slurry, drying and rolling to obtain a positive electrode semi-finished product; S2-2: Punch away the excess part at the edge of the positive electrode sheet in the TD direction to obtain a positive electrode sheet with a positive electrode tab; S2-3: The positive electrode sheet is wound along the MD direction of the base film to obtain the battery cell; S2-4: The battery cell is placed into the casing, the tabs are welded to the cover plate on the casing, and after sealing, liquid injection, and formation, the battery is obtained.
[0030] Example 5: Includes the following steps: S1: Preparation of composite foil S1-1: Mix PET masterbatch granules and plasticizer DOP at a mass ratio of 20:1, add 3wt% of PA6, and dry for 5 hours to obtain the mixture; S1-2: Add the mixture to a single screw extruder, select the T-type die in the flat extrusion die head, perform melt extrusion, extrusion temperature 200℃, die head gap 1mm, cooling roller temperature 40℃, to obtain a semi-finished film; S1-3: The semi-finished film is preheated with infrared radiation at 80℃; a multi-roll stretching machine is used for unidirectional stretching, with the stretching sequence being MD first and then TD. The stretching temperature in the MD direction is 88℃ with a stretching ratio of 2.7, and the stretching temperature in the TD direction is 90℃ with a stretching ratio of 2.9. The strain rate is 30% / s for both directions; after stretching, the MD direction is stretched a second time with a stretching ratio of 1.5; then heat-set at 180℃ for 3s, and rapidly cooled to room temperature to lock the molecular chain orientation, thus obtaining the base film; S1-4: Aluminum layers are deposited on the upper and lower surfaces of the base film by vacuum evaporation to obtain composite foil; S2: Battery fabrication S2-1: Coating the surface of the composite foil with a positive electrode active material slurry, drying and rolling to obtain a positive electrode semi-finished product; S2-2: Punch away the excess part at the edge of the positive electrode sheet in the TD direction to obtain a positive electrode sheet with a positive electrode tab; S2-3: The positive electrode sheet is wound along the MD direction of the base film to obtain the battery cell; S2-4: The battery cell is placed into the casing, the tabs are welded to the cover plate on the casing, and after sealing, liquid injection, and formation, the battery is obtained.
[0031] Example 6: Based on Example 5, the amount of PA6 added was adjusted; the specific differences are as follows: S1-1: Mix PET masterbatch granules and plasticizer DOP at a mass ratio of 20:1, add 5wt% of PA6, and dry for 5 hours to obtain the mixture.
[0032] Example 7: Based on Example 5, the amount of PA6 added was adjusted; the specific differences are as follows: S1-1: Mix PET masterbatch granules and plasticizer DOP at a mass ratio of 20:1, add 7wt% of PA6, and dry for 5 hours to obtain the mixture.
[0033] Example 8: Based on Example 6, the composition of the mixture was adjusted; the specific differences are as follows: S1-1: Mix PET masterbatch granules and plasticizer DOP at a mass ratio of 20:1, add 5wt% PA6, 0.5wt% Schiff base type tetrafunctional epoxy chain extender, and 0.2wt% antioxidant Irganox 1010, and dry for 5 hours to obtain the mixture.
[0034] Comparative Example 1: Based on Example 1, the stretching ratio was adjusted; the specific differences are as follows: S1-3: The semi-finished film is preheated with infrared radiation at 80℃; a multi-roll stretching machine is used for unidirectional stretching, with the stretching sequence being MD first and then TD. The stretching temperature in the MD direction is 88℃ with a stretching ratio of 3.5 times, and the stretching temperature in the TD direction is 90℃ with a stretching ratio of 3.5. The strain rate is 30% / s for both directions; after stretching, the MD is stretched a second time with a stretching ratio of 1.5 times; then it is heat-set at 180℃ for 3s, and then rapidly cooled to room temperature to lock the molecular chain orientation and obtain the base film.
[0035] Comparative Example 2: Based on Comparative Example 1, without the addition of plasticizer DOP; the specific differences are as follows: S1: Preparation of composite foil S1-1: PET masterbatch granules, dried for 5 hours to obtain dried PET masterbatch granules; S1-2: Add the dried PET masterbatch granules to a single-screw extruder, select the T-type die in the flat extrusion die head, and perform melt extrusion at an extrusion temperature of 200℃, a die head gap of 1mm, and a cooling roller temperature of 40℃ to obtain a semi-finished film.
[0036] test: Tensile strength test: A4 paper and the composite foil prepared in the examples and comparative examples were laid flat on a shear. Two strips with the same length direction as the MD direction and TD direction of the base film were cut from the same composite foil. The size of the strips was 15×1.5cm. The two strips were tested using a Tesma universal testing machine: the strips to be tested were placed vertically in the clamp, the data was zeroed and the test was started. After the tensile tester pulled the strip and the strip broke, the tensile strength in the computer was recorded.
[0037] Heat shrinkage test: Cut 5 100mm×100mm samples and mark MD longitudinally and TD transversely; mark longitudinal and transverse reference lines at the center of the sample with an initial spacing of 80mm; avoid the 20cm area at the edge of the film roll, simulate the thermal runaway temperature of the battery, raise the temperature of the forced-air oven to 220℃, stabilize the temperature for 30min, remeasure the length of the markings, and calculate the heat shrinkage.
[0038] Intrinsic viscosity test: The intrinsic viscosity of PET was tested according to GB / T 14190-2017 standard. The PET sample, after being thoroughly vacuum dried, was dissolved in a phenol-1,1,2,2-tetrachloroethane mixed solvent with a mass ratio of 1:1 to prepare a dilute solution with a concentration of 0.5 g / dL. The outflow time of the pure solvent and the PET solution was measured separately in a constant temperature water bath at 25℃ using an Ubbelohde capillary viscometer. The relative viscosity was calculated, and the intrinsic viscosity [η] of the sample was calculated using the one-point method formula, with the unit being dL / g. Before the test, the solution was filtered through a G2 sand core funnel to remove gel particles. Each group of samples was tested in parallel three times, and the arithmetic mean was taken.
[0039] Battery thermal trigger test: 1. Discharge the sample battery and set heating points on both sides of the sample battery to heat the battery at a rate of 3℃ / min; 2. Set temperature detection points on the positive and negative terminals of the battery, read the battery temperature change, and use a battery internal resistance tester to measure the battery internal resistance at a specific battery temperature.
[0040]
[0041]
[0042] in conclusion: Comparing Examples 1-4, it can be seen that when the MD stretch ratio increases from 2.5 to 3.1, the tensile strength in the MD direction increases from 229 MPa to 261 MPa, and the thermal shrinkage rate in the MD direction decreases from 7.6% to 6.6%; when the TD stretch ratio gradually increases from 2.7 to 3.3, the tensile strength in the TD direction increases from 173 MPa to 198 MPa, and the thermal shrinkage rate in the TD direction decreases from 4.1% to 2.8%. These results indicate that appropriately increasing the stretch ratio helps to improve the molecular chain orientation, thereby enhancing mechanical strength while reducing thermal shrinkage.
[0043] Comparing Examples 5-7, it can be seen that under the same stretching process conditions, when the amount of PA6 added increases from 3wt% to 7wt%, the thermal shrinkage rate in the MD direction decreases from 4.9% to 4.6% and then increases to 4.7%, the thermal shrinkage rate in the TD direction increases from 1.5% to 1.6% and then increases to 1.7%, the tensile strength in the MD direction decreases from 239MPa to 225MPa, and the tensile strength in the TD direction decreases from 201MPa to 192MPa; the internal resistance at 220℃ is 5.1MΩ, 7.1MΩ, and 4.7MΩ, respectively, all reaching the megaohm level of melting. These results indicate that the addition of PA6 can significantly improve the melting sensitivity while maintaining the difference in longitudinal / transverse thermal shrinkage rates, but an excessively high addition amount (7wt%) will lead to a decrease in mechanical strength.
[0044] Comparing Examples 6 and 8, it can be seen that Example 8, based on Example 6, further added a chain extender and an antioxidant to the mixture. The addition of the chain extender increased the intrinsic viscosity from 0.55 dL / g to 0.76 dL / g, the molecular weight (MD) tensile strength from 237 MPa to 243 MPa, the tensile strength (TD) from 203 MPa to 214 MPa, the MD heat shrinkage rate from 4.6% to 4.4%, the TD heat shrinkage rate from 1.6% to 1.2%, and the internal resistance at 220℃ from 7.1 MΩ to 7.6 MΩ. These results indicate that the addition of the chain extender can effectively increase the molecular weight and melt strength of PET, further improving melt fracture reliability while enhancing mechanical strength and optimizing heat shrinkage rate.
[0045] Comparing Example 1 and Comparative Example 1, it can be seen that Comparative Example 1, based on Example 1, increased the MD direction stretch ratio from 2.5 to 3.5 and the TD direction stretch ratio from 2.7 to 3.5, resulting in an increase in MD tensile strength from 229 MPa to 265 MPa. However, the MD thermal shrinkage rate increased from 7.6% to 9.2%, and the difference between longitudinal and transverse thermal shrinkage rates widened from 3.5 percentage points to 4.0 percentage points. Consequently, Comparative Example 1 had an internal resistance of only 198.6 kΩ at 240°C, failing to achieve megaohm-level melting, while Example 1 had an internal resistance of 10.1 MΩ at 240°C, achieving complete melting. This result indicates that an excessively high stretch ratio leads to an excessively large MD direction thermal shrinkage rate. At high temperatures, the severe shrinkage in the winding direction weakens the friction between the cell and the casing, preventing the formation of directional tensile stress and thus hindering effective melting.
[0046] Comparing Comparative Example 1 and Comparative Example 2, it can be seen that Comparative Example 2, based on Comparative Example 1, without the addition of plasticizer DOP, shows that the tensile strength in the MD direction decreased from 265 MPa to 201 MPa, and the tensile strength in the TD direction decreased from 204 MPa to 153 MPa. Moreover, the internal resistance soared to 325.4 kΩ at 85℃, indicating premature melting and severely affecting normal use. This result shows that the addition of plasticizer DOP can effectively improve the extensibility and processing fluidity of PET base film, avoiding premature brittleness caused by insufficient extensibility.
[0047] Finally, it should be noted that the above descriptions are merely preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A thermally safe composite foil, characterized in that: It includes a base film and an aluminum layer disposed on the upper and lower surfaces of the base film; The base film is an anisotropic structure with different thermal shrinkage rates in the longitudinal and transverse directions; The thermal shrinkage rate of the base film in the longitudinal direction is lower than that in the transverse direction; The longitudinal direction of the base film is used as the winding direction of the battery cell; The transverse direction of the base film serves as the direction in which the tabs extend.
2. The thermally safe composite foil according to claim 1, characterized in that: The composite foil is prepared by the following steps: (1) Mix polyethylene terephthalate masterbatch granules and plasticizer dioctyl phthalate, and dry to obtain a mixture; (2) The mixture is melt-extruded to obtain a semi-finished film; (3) The semi-finished film is preheated with infrared and stretched in one direction in sequence, first in the longitudinal direction and then in the transverse direction; after stretching, the longitudinal direction is stretched again; then heat-set to obtain the base film. (4) Aluminum layers are deposited on the upper and lower surfaces of the base film by vacuum evaporation to obtain composite foil.
3. The thermally safe composite foil according to claim 2, characterized in that: The mixture also includes nylon 6.
4. The thermally safe composite foil according to claim 3, characterized in that: The amount of nylon 6 added is 3-7 wt%.
5. The thermally safe composite foil according to claim 3, characterized in that: The mixture also includes a multifunctional epoxy chain extender and an antioxidant.
6. The thermally safe composite foil according to claim 2, characterized in that: The process conditions for longitudinal stretching are: longitudinal stretching temperature of 88-93℃ and longitudinal stretching ratio of 2.5-3.2 times.
7. The thermally safe composite foil according to claim 2, characterized in that: The process conditions for the transverse stretching are: transverse stretching temperature of 90-96℃ and transverse stretching ratio of 2.7-3.5 times.
8. The thermally safe composite foil according to claim 2, characterized in that: The stretching ratio of the secondary stretching is 1-2 times.
9. A battery, characterized in that: The battery comprises the thermally safe composite foil as described in any one of claims 1-8.
10. A battery according to claim 9, characterized in that: It is prepared by the following steps: Step 1: Coat the surface of the composite foil with a positive electrode active material slurry, dry and roll to obtain a positive electrode semi-finished product; Step 2: Punch the edge of the positive electrode semi-finished product in the lateral direction to obtain a positive electrode with a positive electrode tab; Step 3: Wind the positive electrode sheet along the longitudinal direction of the base film to obtain the battery cell; Step 4: Place the battery cell into the casing, weld the tabs to the cover plate on the casing, seal, inject electrolyte, and form to obtain the battery.