A high-toughness composite copper foil applied to a secondary battery and a method for manufacturing the same

By electrodepositing a high-toughness copper layer on the surface of high-strength copper foil and controlling the grain configuration, the problem of insufficient tensile strength and toughness of lithium-ion battery negative electrode current collectors after thickness reduction is solved, achieving high safety and long life battery performance.

CN123162202APending Publication Date: 2026-11-24九江德富新能源有限公司 +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611519523.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-29
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

The copper foil used for current collectors in existing lithium-ion batteries has insufficient tensile strength and toughness after the thickness is reduced, which makes the batteries prone to cracking and internal short circuits during charging, discharging and mechanical abuse, and thus cannot meet the safety requirements of the new national standard.

Method used

By electrodepositing a high-toughness copper layer on the surface of a high-strength copper foil and controlling the grain configuration to reduce large-angle grain boundaries, a high-strength and high-toughness composite copper foil is formed. This process includes pre-acid washing, electrodepositing a high-toughness and flattening copper layer, and annealing.

Benefits of technology

It significantly improves the toughness and tear resistance of composite copper foil, reduces the risk of cracking in batteries during mechanical abuse, and improves battery safety and cycle life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123162202A_ABST
    Figure CN123162202A_ABST
Patent Text Reader

Abstract

This invention relates to a high-toughness composite copper foil for use in secondary batteries and its preparation method. The composite copper foil uses high-strength copper foil as the base copper foil, and a thickened high-toughness copper layer is formed by sequentially electrodepositing a high-toughness copper layer and a flat copper layer on its surface. This invention significantly improves the toughness, bending performance, and tear resistance of the composite copper foil by electroplating a high-toughness copper layer on the surface of the high-strength copper foil. The high-toughness copper layer has a large-size grain configuration, reducing the proportion of large-angle grain boundaries, inhibiting crack propagation along grain boundaries, and thus significantly improving the toughness, bending performance, and tear resistance of the composite copper foil.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of lithium battery current collector copper foil technology, and specifically relates to a high-toughness composite copper foil for secondary batteries and its preparation method. Background Technology

[0002] Lithium-ion batteries, as core components of new energy storage, are widely used in consumer electronics, power batteries, and large-scale energy storage power stations. Copper foil, as the negative electrode current collector in lithium-ion batteries, serves the dual function of collecting and conducting electrons and carrying the active material of the negative electrode. The mechanical toughness, elongation, and tear resistance of the copper foil directly determine the battery's cycle life, safety performance, and rate performance. Traditional electrolytic copper foil has a thickness limit; when the thickness is reduced to below 6-8 μm, the tensile strength and elongation at break of the copper foil decrease sharply. During high-speed coating, rolling, and winding processes, it is extremely prone to breakage, wrinkling, and pinhole rupture. During battery charging and discharging, the silicon-based negative electrode undergoes huge volume expansion. Ordinary thin copper foil cannot buffer the expansion stress, easily leading to current collector cracking and active material shedding, causing a sharp drop in battery capacity and the risk of internal short circuits and fires.

[0003] The mandatory national standard GB 38031-2025, implemented in July 2026, raises the safety requirements for electric vehicle power batteries. It adds safety tests after fast charging cycles and battery pack bottom impact tests, upgrades the criteria for thermal runaway and compression tests, and requires battery cells to suppress internal short circuits under aging and mechanical abuse conditions, reducing the risk of thermal runaway from the source. This standard indirectly places higher demands on lithium-ion battery negative electrode current collectors. Ultra-thin lithium-ion battery copper foil needs to possess both high tensile strength and good toughness to reduce the generation of microcracks and metal debris under charge-discharge cycles and external pressure. However, traditional electrolytic copper foil generally suffers from a technical contradiction where tensile strength and toughness are at odds.

[0004] Patent CN117219784B employs a PI polyimide polymer substrate with double-sided composite copper layers, resulting in lighter weight and lower metal usage compared to traditional electrolytic copper foil, significantly improving battery energy density. However, existing composite copper foil technology still has significant shortcomings: insufficient bonding between the polymer substrate and the copper layer, leading to peeling and detachment of the copper layer during bending and stretching; an unreasonable internal grain structure with small grains and numerous grain boundary defects, resulting in crack propagation at grain boundaries and poor overall product toughness, causing copper film breakage after dynamic bending; and the tendency for composite copper foil to develop through-cracks under battery rolling pressure and charge / discharge expansion stress, limiting its large-scale application.

[0005] Existing patents mostly focus on substrate modification and plating process optimization, lacking solutions for the directional control of the internal grain configuration of the copper layer. Conventional magnetron sputtering followed by electroplating produces composite copper foil layers with disordered grain orientation, significant variations in grain size, and numerous large-angle grain boundaries. Under external force, cracks propagate rapidly along these grain boundaries, resulting in insufficient material toughness. Therefore, developing a high-toughness composite copper foil with controllable grain configuration, high interfacial bonding strength, and excellent bending and tear resistance is a pressing technical challenge in this field. Summary of the Invention

[0006] The technical problem to be solved by the present invention is to provide a high-toughness composite copper foil for use in secondary batteries and a method for preparing the same. By electroplating a high-toughness copper layer on the surface of a high-strength copper foil, the high-toughness copper layer has a large-size grain configuration, which reduces the proportion of large-angle grain boundaries, inhibits crack propagation along grains, and significantly improves the toughness, bending performance and tear resistance of the composite copper foil.

[0007] This invention provides a high-toughness composite copper foil for use in secondary batteries. The composite copper foil uses a high-strength copper foil as the base copper foil, and a high-toughness copper layer and a flat copper layer are sequentially electrodeposited on its surface to form a thickened high-toughness copper layer. The thickness ratio of the high-strength copper foil to the high-toughness copper layer is 2-3.5:1.

[0008] Preferably, the thickness of the high-strength copper foil is 4~8μm; the thickness of the thickened high-toughness copper layer is 1~3μm.

[0009] Preferably, the high-toughness composite copper foil has a tensile strength > 600 MPa and a tensile strength attenuation rate < 20% after rolling.

[0010] This invention also provides a method for preparing a high-toughness composite copper foil for use in secondary batteries, comprising the following steps: (1) Electrolytic production of high-strength copper foil, using high-strength copper foil as the base copper foil, first pre-acid washing is performed to clean the oxide layer and impurities on the surface of the high-strength copper foil; (2) Electrodeposit a high-toughness copper layer in electrolyte A on the high-strength copper foil obtained in step (1) to obtain composite copper foil A; (3) Electrodeposit a smooth copper layer in electrolyte B on the composite copper foil A obtained in step (2) to obtain composite copper foil B; (4) The composite copper foil B obtained in step (3) is subjected to anti-oxidation treatment and finally annealed to obtain a high-toughness composite copper foil for use in secondary batteries.

[0011] Preferably, the pre-acid washing in step (1) uses dilute sulfuric acid with a concentration of 5-30% and a temperature of 5-50°C.

[0012] Preferably, the electrolyte A in step (2) has the following composition: Cu 2+10~40g / L, sulfuric acid 100~140g / L, Cl - 10~60ppm, additives 20~60mg / L.

[0013] Preferably, the electrolyte B in step (3) has the following composition: Cu 2+ 25~75g / L, sulfuric acid 100~140g / L, Cl - 20~40ppm, additives 30~50mg / L.

[0014] Preferably, the additives include a brightener, a positioning agent, and a leveling agent.

[0015] Preferably, the brightening agent is one or more of sodium dithiodipropane sulfonate (SPS), 3-thio-isothiourea propane sulfonate (UPS), sodium 3-mercapto-1-propane sulfonate (MPS), sodium N,N-dimethyl dithiocarbonyl propane sulfonate (DPS), and sodium phenyl dithiodipropane sulfonate (BSP); the positioning agent is one or more of collagen, polyethylene glycol (PEG), and polypropylene glycol (PPE); and the leveling agent is one or more of 2-mercaptopyridine (2-MP), benzotriazole (BTA), polyethyleneimine (PEI), Janus Green (JGB), and polyacrylamide (PAM).

[0016] Preferably, the annealing in step (4) is specifically: annealing at 150°C for 10 min to 3 h or annealing at 85°C for 10 to 60 h.

[0017] Beneficial effects (1) The present invention cleans the oxide layer and impurities on the surface of the high-strength copper layer by pre-acid washing, reduces the interface impurities between the high-strength copper layer and the high-toughness copper layer, and further improves the bonding strength of the interface.

[0018] (2) In this invention, a copper layer of a certain thickness is electrodeposited on the surface of a high-strength copper layer, and crystal nuclei are induced to form on the grains on the surface of the high-strength copper layer. By controlling the grain size of the high-toughness copper layer, the toughness of the composite copper foil can be significantly improved.

[0019] (3) In this invention, a copper layer with a small grain size is electrodeposited on the surface of a high-toughness copper layer with a large grain size. The small grains enter the pores of the large grains, which significantly improves the flatness of the surface of the high-toughness composite foil.

[0020] (4) The present invention promotes the fusion of interfacial grains between high-strength copper layer and high-toughness copper layer through heat treatment, which significantly improves the interfacial bonding strength between high-strength copper layer and high-toughness copper layer. Attached Figure Description

[0021] Figure 1 The cross-sectional EBSD grain orientation diagram of the high-toughness composite copper foil prepared in Example 2.

[0022] Figure 2 The diagram shows the equivalent circle diameter distribution of EBSD grains in the cross section of the high-toughness composite copper foil prepared in Example 2.

[0023] Figure 3 This is a schematic diagram of the layered structure of the high-toughness composite copper foil of the present invention. Detailed Implementation

[0024] The present invention will be further illustrated below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Furthermore, it should be understood that after reading the teachings of this invention, those skilled in the art can make various alterations or modifications to the invention, and these equivalent forms also fall within the scope defined by the appended claims.

[0025] The first objective of this invention is to provide a high-toughness composite copper foil for use in secondary batteries, wherein the high-toughness composite copper foil is composed of a high-strength copper layer and a high-toughness copper layer.

[0026] In the embodiments of the present invention, the high-strength copper foil used is produced by the preparation method disclosed in patent CN121938920A.

[0027] In some embodiments of the present invention, high-toughness copper layer electrodeposition is performed on the side of the high-strength copper foil that is not attached to the cathode roller.

[0028] In some embodiments of the present invention, the thickness of the high-strength copper foil is 4-8 μm, and the thickness of the thickened high-toughness copper layer is 1-3 μm, wherein the thickness ratio of the high-strength copper layer to the thickened high-toughness copper layer is 2-3.5:1. Specifically, the thickness of the high-strength copper foil can be 4, 4.5 μm, 5 μm, and 6 μm; the thickness of the thickened high-toughness copper layer can be 1 μm, 1.5 μm, and 2 μm. These embodiments are typical but not limiting. Limiting the copper foil thickness within the above range is beneficial to improving the yield of battery processing and improving battery performance. Limiting the thickness of the high-strength copper layer and the high-toughness copper layer is important because, as the main strength layer of the copper foil, a thickness of less than 4 μm may lead to a decrease in the overall strength of the copper foil, failing to meet the overall tensile strength requirements, while a thickness greater than 8 μm will result in an excessively high total copper foil thickness, which is not conducive to improving the energy density of the battery cell. The main function of thickening the high-toughness copper layer is to improve the toughness of the copper foil. A thickness of less than 1μm has no significant improvement effect, but its strength is low. If the thickness is greater than 3μm, it will lead to a decrease in the overall tensile strength of the copper foil.

[0029] In an embodiment of the present invention, the tensile strength of the high-strength copper foil is ≥70 kgf / mm². 2The elongation is >3%. High-strength copper foil can effectively suppress the large volume change rate of high-energy-density anode materials during charge-discharge cycles; therefore, the tensile strength of the composite copper foil should not be less than 50 kgf / mm². 2 Further reductions in elongation may cause copper foil to break during cell cycling. Insufficient copper foil elongation increases the rate of broken strips and wrinkles during cell manufacturing, reducing production yield.

[0030] A second objective of this invention is to provide a method for preparing a high-toughness composite foil, comprising the following steps: (1) Electrolytic production of high-strength copper foil, with high-strength copper foil serving as the base copper foil. (2) The base copper foil first undergoes a pre-acid washing process to clean the oxide layer and impurities on the foil surface. The specific acid washing solution is a dilute sulfuric acid solution with a concentration of 5~30%. The oxide layer and impurities on the surface are cleaned at a temperature of 5~50℃.

[0031] (3) The substrate copper foil obtained in step (2) is electrodeposited in electrolyte A to form a high-toughness copper layer with large grain size, thereby obtaining composite copper foil A; the electrolyte A comprises raw materials with the following mass concentrations: Cu 2+ 10~40g / L, sulfuric acid 100~140g / L, Cl - 10~60ppm, additives 3~160mg / L. Specific additives include brighteners, leveling agents, and sizing agents. Specific brighteners include sodium polydithiopropane sulfonate (SPS), 3-thio-isothiourea propane sulfonic acid (UPS), sodium 3-mercapto-1-propane sulfonate (MPS), sodium N,N-dimethyldithiocarbonylpropane sulfonate (DPS), and sodium phenyldithiopropane sulfonate (BSP). Specific leveling agents include collagen, polyethylene glycol (PEG), and poly… Propylene glycol (PPE); specific leveling agents include 2-mercaptopyridine (2-MP), benzotriazole (BTA), polyethyleneimine (PEI), Janus Green (JGB), and polyacrylamide (PAM); in specific embodiments, the brightener contains at least one additive, with a concentration of 1~60 mg / L, the leveling agent contains at least one additive, with a concentration of 1~50 mg / L, and the leveling agent contains at least one additive, with a concentration of 1~50 mg / L.

[0032] In an embodiment of the present invention, the electrodeposition temperature of electrolyte A in step (2) is 10~60℃; the current density is 20~90A / dm³. 2 Specifically, the temperature of the electrolyte A can be 10~15℃ or 20~25℃; typically, but not limitingly, it is 15℃, 20℃, and 25℃, for example. The current density can be 20~30 A / dm³. 2 40~50A / dm 260~70A / dm 2 and 80~90A / dm 2 Typical but not limiting, for example, 25 A / dm. 2 45A / dm 2 65A / dm 2 and 85A / dm 2 .

[0033] (4) The composite copper foil A obtained in step (2) is placed in electrolyte B for electrodeposition to deposit a smooth ordinary copper layer on the surface of the high-toughness copper layer, thus obtaining composite copper foil B; the electrolyte B includes raw materials with the following mass concentration: Cu 2+ 25~75g / L, sulfuric acid 100~140g / L, Cl - 20~40ppm, additives 3~160mg / L. Specific additives include brighteners, leveling agents, and polishing agents. Specific brighteners include sodium polydithiopropane sulfonate (SPS), 3-thio-isothiourea propane sulfonic acid (UPS), sodium 3-mercapto-1-propane sulfonate (MPS), sodium N,N-dimethyldithiocarbonyl propane sulfonate (DPS), and sodium phenyl dithiopropane sulfonate (BSP). Specific leveling agents include collagen, polyethylene glycol (PEG), and polypropylene. Diol (PPE); specific leveling agents include 2-mercaptopyridine (2-MP), benzotriazole (BTA), polyethyleneimine (PEI), Janus Green (JGB), and polyacrylamide (PAM); in specific embodiments, the brightener contains at least one additive, the concentration of the brightener is 1~60 mg / L, the leveling agent contains at least one additive, the concentration of the leveling agent is 1~50 mg / L, and the leveling agent contains at least one additive, the concentration of the leveling agent is 1~50 mg / L.

[0034] In an embodiment of the present invention, the electrodeposition temperature of electrolyte B in step (4) is 20~60℃; the current density is 30~100A / dm³. 2 Specifically, the temperature of the electrolyte B can be 20~30℃ or 50~60℃; typically, but not limitingly, it is 25℃ or 55℃. The current density can be 30~40A / dm³. 2 50~60A / dm 2 70~80A / dm 2 and 90~100A / dm 2 Typical but not limiting, for example, 35 A / dm. 2 55A / dm 2 75A / dm 2 and 95A / dm 2 .

[0035] In the embodiments of the present invention, the reason why the current density and electrolyte temperature ranges mentioned in steps (3) and (4) are inconsistent is that: generally, the higher the temperature, the more the copper foil grains tend to become finer, because the concentration polarization phenomenon in the electrolyte will be slowed down at high temperatures, and the additives will also maintain optimal activity. The combined effect of the two promotes the formation of crystal nuclei and inhibits the growth of grains. Similarly, the higher the current density, the smaller the grains. Therefore, the generation of a high-strength layer requires high temperature and high current density, while the generation of a high-toughness layer requires low temperature and low current density.

[0036] In embodiments of the present invention, the source of copper ions in the preparation of the electrolyte can be copper salts, such as copper sulfate.

[0037] In embodiments of the present invention, during the preparation of the electrolyte, the source of chloride ions can be hydrochloric acid or chloride salts, such as copper chloride, sodium chloride, or potassium chloride.

[0038] In embodiments of the present invention, the anode for electrodeposition in steps (3) and (4) is a titanium substrate. Preferably, the surface of the titanium substrate may be coated with a noble metal, such as iridium or tantalum.

[0039] In an embodiment of the present invention, the method for promoting the interfacial fusion of the high-strength copper layer and the high-toughness copper layer and improving the interfacial bonding strength is specifically annealing. The specific conditions are annealing at 150°C for 10 min to 3 h in an oven, or annealing at 85°C for 10 to 60 h.

[0040] Example 1 This embodiment provides a method for preparing a high-toughness composite copper foil for use in secondary batteries, including the following steps: (1) Substrate preparation: High-strength copper foil with a thickness of 4μm was produced using the preparation method of CN121938920A; (2) The surface of high-strength copper foil is pre-acid-washed and activated by using 10~20% dilute sulfuric acid to clean the oxide layer and impurities on the surface at a temperature of 25±2℃. (3) The high-strength copper foil obtained in step (2) is electrodeposited in electrolyte A, and a high-toughness copper layer is electrodeposited on the side of the high-strength copper layer that is not attached to the cathode roller to obtain composite copper foil A; the electrolyte A includes raw materials with the following mass concentrations: Cu 2+ 25g / L, sulfuric acid 120g / L, Cl -25 mg / L; Additive names and concentrations: Sodium dithiopropane sulfonate (SPS) concentration 20 mg / L, 3-thio-isothiourea propanesulfonic acid (UPS) concentration 10 mg / L, collagen concentration 9 mg / L, polyethylene glycol (PEG) with a molecular weight of 8000 concentration 3 mg / L, polyethylene glycol (PEG) with a molecular weight of 1000 concentration 15 mg / L, polyethyleneimine (PEI) concentration 4 mg / L; The thickness of the high-toughness copper layer is 1.3 μm; The current density is 70 A / dm³. 2 The electrodeposition temperature is 20±2℃. (4) The composite copper foil A obtained in step (3) is electrodeposited in electrolyte B, and a smooth copper layer is then electrodeposited on the surface of the side treated in the previous step; the electrolyte B includes raw materials with the following mass concentrations: Cu 2+ 60g / L, sulfuric acid 110g / L, Cl - 25 mg / L; Additive names and concentrations: Sodium dithiopropane sulfonate (SPS) concentration is 30 mg / L, 3-thio-isothiourea propanesulfonic acid (UPS) concentration is 15 mg / L, 2-mercaptopyridine (2-MP) concentration is 6 mg / L, polyethylene glycol (PEG) with a molecular weight of 8000 concentration is 4 mg / L, polyethylene glycol (PEG) with a molecular weight of 1000 concentration is 20 mg / L, and polyethyleneimine (PEI) concentration is 7 mg / L; The thickness of the flat copper layer is 0.1 μm, and the thickness ratio of the high-strength copper layer to the thickened high-toughness copper layer is 3:1; The current density is 85 A / dm³. 2 The electrodeposition temperature is 55±2℃. (5) The high-toughness composite copper foil obtained in step (4) is subjected to anti-oxidation treatment.

[0041] (6) The high-toughness composite copper foil obtained in step (5) is placed in an oven for annealing. The specific annealing temperature is 150℃ and the annealing time is 1h.

[0042] Example 2 This embodiment provides a method for preparing a high-toughness composite copper foil for secondary batteries. The difference from Embodiment 1 is that the thickness of the high-strength copper foil in step (1) is 4.5 μm, and the thickness of the thickened copper layer in steps (3) and (4) is 1.5 μm.

[0043] Example 3 This embodiment provides a method for preparing a high-toughness composite copper foil for secondary batteries. The difference from Embodiment 1 is that the thickness of the high-strength copper foil in step (1) is 5 μm, and the thickness of the thickened copper layer in steps (3) and (4) is 1.7 μm.

[0044] Example 4 This embodiment provides a method for preparing a high-toughness composite copper foil for secondary batteries. The difference from Embodiment 1 is that the thickness of the high-strength copper foil in step (1) is 6 μm, and the thickness of the thickened copper layer in steps (3) and (4) is 2.0 μm.

[0045] Comparative Example 1 This embodiment provides a method for preparing a high-toughness composite copper foil for secondary batteries. The difference from Embodiment 1 is that the sum of the thickness of the high-toughness copper layers in steps (3) and (4) is 1.2 μm.

[0046] Comparative Example 2 This embodiment provides a method for preparing a high-toughness composite copper foil for secondary batteries. The difference from Embodiment 1 is that the sum of the thickness of the high-toughness copper layers in steps (3) and (4) is 1.6 μm.

[0047] Comparative Example 3 This embodiment provides a method for preparing a high-toughness composite copper foil for secondary batteries. The difference from Embodiment 2 is that the sum of the thickness of the high-toughness copper layers in steps (3) and (4) is 1.1 μm.

[0048] Comparative Example 4 This embodiment provides a method for preparing a high-toughness composite copper foil for secondary batteries. The difference from Embodiment 2 is that the sum of the thickness of the high-toughness copper layers in steps (3) and (4) is 1.3 μm.

[0049] Comparative Example 5 This embodiment provides a method for preparing a high-toughness composite copper foil for secondary batteries. The difference from Embodiment 2 is that the sum of the thickness of the high-toughness copper layers in steps (3) and (4) is 1.7 μm.

[0050] Comparative Example 6 This embodiment provides a method for preparing a high-toughness composite copper foil for secondary batteries. The difference from Embodiment 2 is that the sum of the thickness of the high-toughness copper layers in steps (3) and (4) is 1.9 μm.

[0051] Comparative Example 7 This embodiment provides a method for preparing a high-toughness composite copper foil for use in secondary batteries. The difference from Embodiment 3 is that the sum of the thicknesses of the high-toughness copper layers in steps (3) and (4) is 1.3 μm. Comparative Example 8 This embodiment provides a method for preparing a high-toughness composite copper foil for secondary batteries. The difference from Embodiment 3 is that the sum of the thickness of the high-toughness copper layers in steps (3) and (4) is 1.5 μm.

[0052] Comparative Example 9 This embodiment provides a method for preparing a high-toughness composite copper foil for secondary batteries. The difference from Embodiment 3 is that the sum of the thickness of the high-toughness copper layers in steps (3) and (4) is 1.9 μm.

[0053] Comparative Example 10 This embodiment provides a method for preparing a high-toughness composite copper foil for secondary batteries. The difference from Embodiment 3 is that the sum of the thickness of the high-toughness copper layers in steps (3) and (4) is 2.1 μm.

[0054] Comparative Example 11 This embodiment provides a method for preparing a high-toughness composite copper foil for secondary batteries. The difference from Embodiment 4 is that the sum of the thickness of the high-toughness copper layers in steps (3) and (4) is 1.6 μm.

[0055] Comparative Example 12 This embodiment provides a method for preparing a high-toughness composite copper foil for secondary batteries. The difference from Embodiment 4 is that the sum of the thickness of the high-toughness copper layers in steps (3) and (4) is 1.8 μm.

[0056] Comparative Example 13 This embodiment provides a method for preparing a high-toughness composite copper foil for secondary batteries. The difference from Embodiment 4 is that the sum of the thickness of the high-toughness copper layers in steps (3) and (4) is 2.2 μm.

[0057] Comparative Example 14 This embodiment provides a method for preparing a high-toughness composite copper foil for secondary batteries. The difference from Embodiment 4 is that the sum of the thickness of the high-toughness copper layers in steps (3) and (4) is 2.4 μm.

[0058] Performance testing Test methods for tensile strength and elongation: The copper foil was cut into 15×100mm pieces using a sample cutting machine. 2 The sample strips of the specified size were used to test the tensile strength of the copper foil using a tensile tester. The clamping pressure was set to 15 psi, the clamp spacing was 50 mm, and the clamping speed was set to 50 mm / min. The cut sample strips were placed vertically and clamped to ensure that the direction of the tensile force was the same as the direction of the sample strip during the test. Then, the tensile tester was started to test the tensile strength and elongation of the sample strips. The tensile strength / elongation was taken as the average value of 10 tests.

[0059] Toughness performance testing methods: The copper foil was cut into 15×100mm pieces using a sample cutting machine. 2Sample strips of various sizes were rolled using a special fixture. If any breaks were found, further testing was discontinued. If no breaks were found, the rolled sample strips were tested for the tensile strength of the copper foil using a tensile testing machine. The clamping pressure was set to 15 psi, the clamp spacing to 50 mm, and the clamping speed to 50 mm / min. The cut sample strips were placed vertically and clamped to ensure the direction of the tensile force was the same as the sample strip's direction during testing. The tensile strength and elongation of the sample strips were then tested using the tensile testing machine. The tensile strength / elongation ratio was taken as the average of 10 tests. The results are shown in Table 1.

[0060] Table 1 Based on Examples 1, Comparative Examples 1 and 2, and the data in Table 1, it can be seen that the high-toughness composite copper foil prepared in Example 1 has a tensile strength of 687.35 MPa and a tensile strength attenuation rate of 7.74% after rolling, which meets the first objective. After rolling, the sample strip of Comparative Example 1 was damaged, indicating that its rolling resistance was insufficient. The tensile strength of Comparative Example 2 was <600 MPa, which does not meet the first objective.

[0061] Based on Examples 2, Comparative Examples 3, 4, 5, and 6, and the data in Table 1, it can be seen that the high-toughness composite copper foil prepared in Example 2 of this application has a tensile strength of 676.85 MPa and a tensile strength attenuation rate of 4.14 after rolling, which meets the first objective. After rolling, the sample strip of Comparative Example 3 was damaged, indicating that its rolling resistance was insufficient. The tensile strength attenuation rate of Comparative Example 4 was >20%, and the tensile strength of Comparative Examples 5 and 6 was <600 MPa, all of which do not meet the first objective. Figure 1 , 2 The EBSD data for Example 2 is from... Figure 1 , 2 As can be seen, the high-strength layer is fine-grained, with a specific grain size of 0.2~0.4μm, while the high-toughness layer is coarse-grained, with a maximum grain size of up to 1.423μm.

[0062] Based on Examples 3, 7, 8, 9, and 10, and the data in Table 1, it can be seen that the high-toughness composite copper foil prepared in Example 3 has a tensile strength of 645.38 MPa and a tensile strength attenuation rate of 4.14 after rolling, which meets the first objective. In Comparative Example 7, the sample strip broke after rolling, indicating that its rolling resistance was insufficient. The tensile strength attenuation rate of Comparative Example 8 was >20%, and the tensile strength of Comparative Example 9 was close to 600 MPa. For safety reasons, this comparative example does not meet the first objective. The tensile strength of Comparative Example 10 was <600 MPa, which also does not meet the first objective.

[0063] Based on Examples 4, Comparative Examples 11, 12, 13, and 14, and the data in Table 1, it can be seen that the high-toughness composite copper foil prepared in Example 4 has a tensile strength of 657.84 MPa and a tensile strength attenuation rate of 6.56 after rolling, which meets the first objective. After rolling, the sample strip of Comparative Example 11 was damaged, indicating that its rolling resistance was insufficient. The tensile strength attenuation rate of Comparative Example 12 was >20%, and the tensile strength of Comparative Examples 13 and 14 was <600 MPa, which do not meet the first objective.

[0064] In summary, when the ratio of high-strength copper layer thickness to thickened copper layer thickness is ≥4:1, the high-toughness composite copper foil will break after rolling, indicating poor toughness. This is because the thickness of the high-toughness copper layer is insufficient, and the toughness provided is not enough to improve the overall toughness of the composite copper foil to achieve the first objective of this invention. When the ratio of high-strength copper layer thickness to thickened copper layer thickness is approximately 3:1, the high-toughness composite copper foil meets all the objectives of this invention.

[0065] The high-toughness composite copper foil provided by this invention is formed by electroplating a high-toughness copper layer on the surface of a copper foil with high tensile strength. The thickness ratio of the high-strength copper layer to the high-toughness copper layer is approximately 3:1, creating a composite copper foil structure that combines a high-toughness layer and a high-strength layer. This structure combines high tensile strength and high toughness, solving the problem of simultaneously optimizing the tensile strength and toughness of copper foil. It can effectively prevent electrode breakage during the winding process of the battery cell. As a result, the negative electrode of a lithium-ion battery containing the high-toughness copper foil provided by this invention has better cycle life and safety.

[0066] The above embodiments are merely illustrative of the principles and effects of the present invention and are not intended to limit the invention. Any person skilled in the art can modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by those skilled in the art without departing from the spirit and technical concept disclosed in the present invention should still be covered by the claims of the present invention.

Claims

1. A high-toughness composite copper foil for use in secondary batteries, characterized in that, The composite copper foil uses high-strength copper foil as the base copper foil, and a thickened high-toughness copper layer is formed by sequentially electrodepositing a high-toughness copper layer and a flat copper layer on its surface; the thickness ratio of the high-strength copper foil to the high-toughness copper layer is 2-3.5:

1.

2. The high-toughness composite copper foil according to claim 1, characterized in that, The thickness of the high-strength copper foil is 4~8μm; the thickness of the thickened high-toughness copper layer is 1~3μm.

3. The high-toughness composite copper foil according to claim 1, characterized in that, The high-toughness composite copper foil has a tensile strength >600MPa and a tensile strength attenuation rate <20% after rolling.

4. A method for preparing a high-toughness composite copper foil for use in secondary batteries, characterized in that, Includes the following steps: (1) Electrolytic production of high-strength copper foil, using high-strength copper foil as the base copper foil, first pre-acid washing is performed to clean the oxide layer and impurities on the surface of the high-strength copper foil; (2) Electrodeposit a high-toughness copper layer in electrolyte A on the high-strength copper foil obtained in step (1) to obtain composite copper foil A; (3) Electrodeposit a smooth copper layer in electrolyte B on the composite copper foil A obtained in step (2) to obtain composite copper foil B; (4) The composite copper foil B obtained in step (3) is subjected to anti-oxidation treatment and finally annealed to obtain a high-toughness composite copper foil for use in secondary batteries.

5. The preparation method according to claim 4, characterized in that, The pre-acid washing in step (1) uses dilute sulfuric acid with a concentration of 5-30% and a temperature of 5-50℃.

6. The preparation method according to claim 4, characterized in that, The electrolyte A in step (2) has the following composition: Cu 2+ 10~40g / L, sulfuric acid 100~140g / L, Cl - 10~60ppm, additives 20~60mg / L.

7. The preparation method according to claim 4, characterized in that, The electrolyte B in step (3) has the following composition: Cu 2+ 25~75g / L, sulfuric acid 100~140g / L, Cl - 20~40ppm, additives 30~50mg / L.

8. The preparation method according to claim 6 or 7, characterized in that, The additives include brighteners, positioning agents, and leveling agents.

9. The preparation method according to claim 8, characterized in that, The brightening agent is one or more of sodium dithiodipropane sulfonate (SPS), 3-thio-isothiourea propane sulfonate (UPS), sodium 3-mercapto-1-propane sulfonate (MPS), sodium N,N-dimethyl dithiocarbonyl propane sulfonate (DPS), and sodium phenyl dithiodipropane sulfonate (BSP); the positioning agent is one or more of collagen, polyethylene glycol (PEG), and polypropylene glycol (PPE); and the leveling agent is one or more of 2-mercaptopyridine (2-MP), benzotriazole (BTA), polyethyleneimine (PEI), Janus Green (JGB), and polyacrylamide (PAM).

10. The preparation method according to claim 4, characterized in that, The annealing in step (4) specifically involves annealing at 150°C for 10 min to 3 h or annealing at 85°C for 10 to 60 h.

Citation Information

Patent Citations

  • A surface-modified composite current collector, preparation method and battery

    CN117219784B

  • Copper foil and preparation method thereof, current collector, negative pole piece and secondary battery

    CN121938920A