A hollow mesoporous carbon supported high stability ordered platinum-based fuel cell cathode catalyst, and a preparation method and application thereof
By using hollow mesoporous carbon supports and ordered intermetallic compounds in the preparation method of proton exchange membrane fuel cell cathode catalysts, the instability of platinum and transition metal components under electrochemical conditions was solved, and a highly active and stable platinum-based alloy catalyst was achieved, thereby improving the performance of fuel cells.
Patent Information
- Application Number
- CN202611323451.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-28
- Publication Date
- 2026-11-24
AI Technical Summary
Existing proton exchange membrane fuel cell cathode catalysts are prone to oxidation, migration, and dissolution of platinum and transition metal components under long-term electrochemical conditions, leading to instability of catalyst active sites. Furthermore, high-temperature annealing treatment can easily cause particle sintering and growth, reducing platinum atom utilization efficiency.
Hollow mesoporous carbon supports were constructed using an in-situ hard template method. Platinum precursors and transition metal precursors were loaded onto the supports, and ordered intermetallic compounds were formed by high-temperature annealing. Unstable components were then removed by acid treatment, thus preparing a highly stable ordered platinum-based alloy catalyst supported on hollow mesoporous carbon.
It effectively inhibited the sintering and agglomeration of platinum-based nanoparticles, improved the utilization rate of platinum atoms, enhanced the oxygen reduction activity and long-term stability of the catalyst, reduced the amount of platinum used, and improved the catalytic activity.
Smart Images

Figure CN123162222A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of proton exchange membrane fuel cell technology, specifically relating to a hollow mesoporous carbon-supported, highly stable, ordered platinum-based fuel cell cathode catalyst, its preparation method, and its application. Background Technology
[0002] Proton exchange membrane fuel cells (PEMFCs) possess advantages such as high energy conversion efficiency and clean, environmentally friendly operation, and are considered one of the important electrochemical energy conversion technologies for the future. However, the oxygen reduction reaction (ORR) at the PEMFC cathode involves a multi-electron transfer process with sluggish reaction kinetics, typically requiring platinum-based catalysts to lower the reaction energy barrier. Due to the limited resources and high cost of platinum, its large-scale use significantly restricts the commercialization of PEMFCs. Therefore, designing and preparing cathode catalysts with high activity, high stability, and low platinum consumption has become a key scientific and technological problem urgently needing to be solved in this field.
[0003] Previous studies have shown that introducing transition metals to construct platinum-based alloys, controlling the composition and structure of the catalyst, and optimizing its geometry can effectively improve the oxygen reduction activity and service stability of proton exchange membrane fuel cell cathode catalysts. For example, Shi Jianlin's team designed an oxygen vacancy-induced ordered L10-PtCo catalyst with a Pt shell structure, achieving a mass activity of 1.28 A mg at a relatively low platinum loading. Pt -1 This catalyst surpasses commercial PtCo catalysts. It exhibits high stability, retaining 81% of its mass activity after 30,000 cycles. (Kong, Fantao; Huang, Yifan; Yu, Xu; Li, Min; Song, Kunming; Guo, Qiuyun; Cui, Xiangzhi; Shi, Jianlin. J. Am. Chem. Soc. 2024, 146, 30078-30090); Liang Haiwei's team reported a medium-sized ordered PtCo catalyst prepared via high-temperature pyrolysis of a bimetallic complex, with an average particle size of 6 nm. At 0.1 mg... Pt cm -2 At low loading rates, it has up to 0.80 A mg. Pt -1 Mass activity and up to 1.50 A cm at 0.7 V. -2The current density is high, and after 90,000 cycles, the current retention rate reaches 80%, making its application in heavy-duty vehicles possible. (Li, S.; Shao, RY; Tong, L.; Song, TW; Xu, C.; Ma, CS; Zhang, L.; Li, JJ; Li, ZR; Xue, KZ; Xiao, B.; Wu, C.; Liang, HW, Medium-Sized Intermetallic PtCo Catalysts for Low-Pt Heavy-Duty Fuel Cells. Angew. Chem. Int. Ed. 2026, e9440254). Although the ordered structure of Pt-M alloy helps optimize the electronic structure of platinum-based catalysts, thereby improving their oxygen reduction reaction activity and structural stability, in the actual operation of proton exchange membrane fuel cells, the cathode catalyst is under harsh electrochemical conditions for a long time. The transition metal components in the alloy are still prone to oxidation, migration, and dissolution, which in turn destroys the ordered structure and active site stability of the catalyst, ultimately causing rapid degradation of battery performance.
[0004] In contrast, introducing additional early transition metals can further enhance the transition metal's resistance to dissolution. For example, Li Qing's team designed an ordered L10-PtFeCr catalyst with a Pt shell structure doped with the transition metal Cr, achieving a mass activity of 1.41 A mg at a relatively low platinum loading. Pt -1 This is three times more potent than commercial Pt / C catalysts. The catalyst exhibits high stability and resistance to dissolution; its activity decay is negligible after 30,000 cycles, demonstrating stability far exceeding that of PtFe catalysts. (Liu, Xuan; Wang, Yuhan; Liang, Jiashun; Li, Shenzhou; Zhang, Siyang; Su, Dong; Cai, Zhao; Huang, Yunhui; Elbaz, Lior; Li, Qing, Introducing Electron Buffers into Intermetallic Pt Alloys against Surface Polarization for High-Performing Fuel Cells. J. Am. Chem. Soc. 2024, 146, 2033-2042) However, the formation of the ordered structure in Pt-M alloys typically relies on high-temperature annealing, a process that easily induces catalyst particle sintering and growth, leading to reduced platinum atom utilization efficiency. Therefore, achieving catalyst miniaturization and uniform dispersion while maintaining high order remains a significant challenge. Effectively suppressing the oxidation, migration, and dissolution of platinum and transition metal components in proton exchange membrane fuel cell cathode catalysts, and preparing small-sized, ordered, multi-component platinum-based alloy catalysts with high activity, high stability, and high platinum utilization, are key issues urgently needing to be addressed in this field. Summary of the Invention
[0005] The purpose of this section is to outline some aspects of embodiments of the present invention and to briefly describe some preferred embodiments. Simplifications or omissions may be made in this section, as well as in the abstract and title of this application, to avoid obscuring the purpose of these documents; however, such simplifications or omissions should not be construed as limiting the scope of the invention.
[0006] In view of the problems existing in the above and / or prior art, the present invention is proposed.
[0007] Therefore, the purpose of this invention is to overcome the shortcomings of the prior art and provide a hollow mesoporous carbon-supported, highly stable, ordered platinum-based fuel cell cathode catalyst, its preparation method, and its application.
[0008] To solve the above-mentioned technical problems, the present invention provides the following technical solution: tetraethyl orthosilicate, ammonia, resorcinol and formaldehyde are dispersed in a mixed solvent of ethanol and ultrapure water, and the mixture is stirred at room temperature to obtain a flocculent orange suspension; After centrifugation, washing and drying, the flocculent orange suspension is subjected to a first high-temperature annealing and carbonization treatment in an inert atmosphere, followed by alkaline washing and etching to remove the silicon template, resulting in a hollow mesoporous carbon support. The hollow mesoporous carbon support is dispersed in a water-alcohol mixture, and a platinum precursor and one or more metal precursors selected from iron, cobalt, copper and gallium are added. After stirring until fully adsorbed, the solvent is removed by rotary evaporation to obtain the catalyst precursor. The catalyst precursor was subjected to a second high-temperature annealing treatment in a reducing atmosphere to allow platinum to form an ordered intermetallic compound with the transition metal. The annealed product was subjected to acid treatment to remove unstable metal components on the surface, and then dried to obtain the cathode catalyst.
[0009] In a preferred embodiment of the preparation method described in this invention, the centrifugation speed is 11800-12000 rpm and the time is 2-3 min.
[0010] In a preferred embodiment of the preparation method described in this invention, the atmosphere for the first high-temperature annealing and carbonization treatment is argon or nitrogen, and the heating rate is 0.5-10℃ / min. -1 The temperature is 700-1000℃, and the time is 3-5 hours.
[0011] In a preferred embodiment of the preparation method described in this invention, the second high-temperature annealing treatment atmosphere is an argon-hydrogen mixture, with a hydrogen volume content of 5-10 vol% and a heating rate of 0.5-10℃ min. -1 The heat treatment temperature is 500-1100℃, and the heat treatment time is 1-6 h.
[0012] In a preferred embodiment of the preparation method described in this invention, the solution in the acid treatment includes dilute perchloric acid, dilute hydrochloric acid, or dilute sulfuric acid solution with a concentration of 0.08-0.1 M.
[0013] In a preferred embodiment of the preparation method described in this invention, the molar ratio of platinum precursor to metal precursor is 1-2:1-5, and the molar ratio of each metal precursor is 1-2:1-2.
[0014] Another objective of this invention is to overcome the shortcomings of the prior art and provide a hollow mesoporous carbon-supported, highly stable, ordered platinum-based fuel cell cathode catalyst prepared by a specific method.
[0015] Another objective of this invention is to overcome the shortcomings of the prior art and provide an application of a highly stable ordered platinum-based fuel cell cathode catalyst supported on hollow mesoporous carbon in the oxygen reduction reaction at the cathode of a proton exchange membrane fuel cell.
[0016] Beneficial effects of this invention: (1) This invention constructs a hollow mesoporous carbon support using an in-situ hard template method, providing abundant confined space and anchoring points for the nucleation, growth, and high-temperature ordering of platinum-based alloy nanoparticles. Using the aforementioned hollow mesoporous carbon as a support, platinum precursors and one or more metal precursors from iron, cobalt, copper, and gallium are introduced. After adsorption loading, solvent removal, and high-temperature annealing under a reducing atmosphere, the alloying and ordering of platinum with transition metals and gallium elements are achieved, enabling the preparation of binary, ternary, quaternary, and quinary ordered platinum-based alloy catalysts. Thanks to the spatial confinement effect of the hollow mesoporous carbon support and the anchoring effect of surface oxygen-containing functional groups, the sintering and agglomeration of platinum-based nanoparticles during high-temperature annealing can be effectively suppressed, ensuring that the resulting ordered platinum-based alloy nanoparticles maintain a small particle size and good dispersibility, thereby improving the utilization rate of platinum atoms.
[0017] (2) In this invention, the multi-metal components synergistically regulate the crystal and electronic structures of the platinum-based alloy, which helps to reduce the oxidative dissolution of platinum and transition metals during fuel cell operation and improve the oxygen reduction activity and long-term stability of the catalyst. The preparation method is simple, low-cost, and reproducible. The resulting hollow mesoporous carbon-supported ordered platinum-based alloy fuel cell cathode catalyst has lower platinum content, higher catalytic activity, and better stability compared to commercial platinum-carbon catalysts. Attached Figure Description
[0018] To more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort. Wherein: Figure 1 Nitrogen adsorption isotherm and pore size analysis diagram of the hollow mesoporous carbon support prepared in this invention.
[0019] Figure 2 Transmission electron microscopy (TEM) characterization of the hollow mesoporous carbon-supported, highly stable, ordered platinum-based fuel cell cathode catalyst prepared in Example 1 of this invention.
[0020] Figure 3 The image shows the statistical distribution of nanoparticle size of the hollow mesoporous carbon-supported, highly stable, ordered platinum-based fuel cell cathode catalyst prepared in Example 1 of this invention.
[0021] Figure 4 X-ray diffraction patterns of the hollow mesoporous carbon-supported, highly stable, ordered platinum-based fuel cell cathode catalysts prepared in Examples 1-4 of this invention.
[0022] Figure 5 The image shows the three-electrode accelerated aging performance of the hollow mesoporous carbon-supported, highly stable, ordered platinum-based fuel cell cathode catalyst prepared in Example 1 of this invention.
[0023] Figure 6 The polarization curve of the high-stability ordered platinum-based fuel cell cathode catalyst supported on hollow mesoporous carbon prepared in Example 1 of this invention is shown in the accelerated aging test diagram when the cathode catalyst is assembled into a single cell.
[0024] Figure 7 The three-electrode performance diagrams are for the hollow mesoporous carbon-supported, highly stable, ordered platinum-based fuel cell cathode catalysts prepared in Examples 1-4 of this invention.
[0025] Figure 8The graph shows a comparison of the stability retention rate of the hollow mesoporous carbon-supported high-stability ordered platinum-based fuel cell cathode catalyst prepared in Example 1 of this invention when assembled into a single cell with literature. Detailed Implementation
[0026] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, the specific embodiments of the present invention will be described in detail below with reference to the examples in the specification.
[0027] Many specific details are set forth in the following description in order to provide a full understanding of the invention. However, the invention may also be practiced in other ways different from those described herein, and those skilled in the art can make similar extensions without departing from the spirit of the invention. Therefore, the invention is not limited to the specific embodiments disclosed below.
[0028] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The phrase "in one embodiment" appearing in different places in this specification does not necessarily refer to the same embodiment, nor is it a single or selective embodiment that is mutually exclusive with other embodiments.
[0029] Unless otherwise specified, all raw materials used in the embodiments of this invention are commercially available. See Table 1 for details.
[0030] Table 1
[0031] The details of the three electrodes and fuel cell testing process involved in this invention are as follows.
[0032] The details of the three-electrode test are as follows.
[0033] (1) Preparation before testing: Weigh 5 mg of the synthesized catalyst and disperse it in a mixed solution of water, isopropanol and Nafion solution (5 wt.%) (component ratio 400:550:50). Disperse the catalyst evenly by ultrasonication (ultrasonication time greater than 30 min) until there is no sticking to the wall, and obtain a viscous ink with uniform sample mixing. Use a pipette to take an appropriate amount of catalyst ink and drop it onto the surface of the glassy carbon electrode in small amounts multiple times within a rotation speed range of 200 rpm to 700 rpm. After drying, an electrode with uniform catalyst coverage is obtained, in which the Pt loading is 20 μg. Pt cm -2Meanwhile, a commercial Pt / C-JM catalyst was used to prepare the working electrode for comparative testing, with the loading consistent with the catalyst synthesized in this study. Oxygen reduction electrochemical performance was tested using a CHI 750E electrochemical workstation (CHI Instruments) and a rotating disk electrode apparatus (PINE). The working electrode was a rotating disk electrode (PINE, 5 mm diameter), the counter electrode was a carbon rod, and the reference electrode was a standard hydrogen electrode, all of which were calibrated before use. Oxygen reduction performance was tested under constant room temperature conditions (22–26 °C), employing a standard three-electrode system.
[0034] (2) Cyclic voltammetry (CV): Before the test, cyclic voltammetry (CV) was performed to activate the working electrode until the CV curves overlapped. Then, N2 was introduced into the solution until saturation, and the aeration time was more than 30 min. Then, cyclic voltammetry (CV) was performed. The voltage scan range of the cyclic voltammetry test was 0.05-1.1 V (vs. RHE), and the scan rate was 10 mV s. -1 The electrode rotation speed was 1600 rpm, and N2 was continuously introduced during the test.
[0035] (3) Linear Voltammetric Scan (LSV): Before performing the linear voltammetric scan (LSV), the solution must be continuously purged with O2 to ensure it reaches saturation. The purging time should exceed 30 min. During the LSV test, the voltage scan range is set to 0.05-1.1 V (vs. RHE), and the scan rate is 10 mV / s. -1 The rotating disk electrode was rotated at 1600 rpm, and O2 was continuously introduced during the test. The linear voltammetric scan test curve should be subtracted for nitrogen background.
[0036] (4) Stability Testing: During the stability testing period, the low-Pt catalyst was subjected to continuous potential cycling tests in an O2-saturated 0.1 M HClO4 solution at a scan rate of 200 mV / s within a potential range of 0.6–1.0 V. This process simulates the durability under actual operating conditions to evaluate long-term operational stability. Linear voltammetry and cyclic voltammetry tests were performed after every 10 k cycles.
[0037] The fuel cell testing details are as follows.
[0038] (1) Membrane electrode preparation: A catalyst was prepared as the cathode. An appropriate amount of catalyst was placed in a centrifuge tube. Based on the weighed catalyst mass, 5 wt.% Nafion solution was added at a mass ratio of ionomer to catalyst of 0.7 (I / C = 0.7). Then, an appropriate amount of a 1:1 volume ratio of isopropanol to deionized water was added. The mixture was ultrasonically treated for 1 h to form a uniformly dispersed catalyst slurry. The slurry was uniformly sprayed onto the proton exchange membrane using ultrasonic spraying, controlling the cathode Pt loading to be 0.02 mg. Pt cm -2 The actual sprayed area is 2×2 cm. 2 The anode used a commercial Pt / C catalyst, prepared using the same method as the spraying process, and was sprayed onto the other side of the proton exchange membrane, with the Pt loading controlled at 0.025 mg. Pt cm -2 Subsequently, the gasket, gas diffusion layer, proton exchange membrane coated with catalyst, gas diffusion layer, and gasket were strictly aligned in sequence and placed in a hot press for hot pressing treatment. The hot pressing temperature was set to 135℃, the pressure to 1 ton, and the hot pressing time to 1 minute. Finally, the membrane electrode compression ratio was controlled to be about 20%.
[0039] (2) Performance testing: The membrane electrode assembly was installed into the fuel cell test mold. The fuel cell temperature was set to 80℃, and the relative humidity of the cathode and anode was 100%. Nitrogen and hydrogen gas at 0.2 slpm were introduced into the anode and cathode respectively. After stabilization for 4 hours, hydrogen permeation test was performed. The hydrogen permeation current density was less than 10 mA cm⁻¹. -2 This indicates that the membrane electrode is well sealed. Subsequently, oxygen gas at 1.0 slpm and hydrogen gas at 0.5 slpm were introduced into the anode and cathode respectively to perform cyclic activation of the polarization curves. The test potential range was set from open-circuit voltage (OCP) to 0.3 V (vs. absolute). Stabilization was performed for 10 s at 20 mA intervals, and data acquisition was conducted. Activation was complete when the polarization curves overlapped. Polarization curves were then acquired under hydrogen and oxygen conditions at a test pressure of 150 kPa. abs After completion, switch to air for testing at a pressure of 250 kPa. abs .
[0040] (3) Stability test: Hydrogen gas was introduced into the anode at a flow rate of 0.2 slpm, and nitrogen gas was introduced into the cathode at a flow rate of 0.2 slpm. The potential range was set to 0.6 V-1.0 V (vs. Reference), and the scan rate was set to 200 mV s. -1 After 10,000 cycles of accelerated aging test, the same battery polarization curve test needs to be performed according to the aforementioned experimental steps to determine its stability.
[0041] Example 1 This embodiment provides a method for preparing a highly stable ordered platinum-based fuel cell cathode catalyst supported on hollow mesoporous carbon, specifically as follows: (1) Measure 40 mL of ultrapure water and 280 mL of anhydrous ethanol into a 500 mL beaker and stir to mix. Then add 8 mL of tetraethyl orthosilicate and 6 mL of ammonia solution. After stirring for 15 min, weigh and add 1.6 g of resorcinol and 2.4 mL of formaldehyde solution. Stir at room temperature for 24 h, centrifuge, wash three times with a mixed solvent of water and ethanol in a volume ratio of 1:1, and then dry in a drying oven at 60℃ for 24 h. After grinding, an orange-brown solid powder is obtained.
[0042] (2) The obtained orange-brown solid powder was placed in a tube furnace and subjected to high-temperature annealing under an argon atmosphere at a heating rate of 5°C / min. -1 The high-temperature annealing temperature is 800℃, the holding time is 5 h, and after natural cooling, a black powder is obtained.
[0043] (3) The above black powder was dispersed in 150 mL of 6 M sodium hydroxide solution, sonicated for 30 min, and then in an oil bath at 80℃ for 48 h. After natural cooling, it was washed three times with a mixed solvent of water and ethanol in a volume ratio of 1:1. Then it was dispersed in 0.1 M perchloric acid, stirred at room temperature for 12 h, centrifuged, washed three times with a mixed solvent of water and ethanol in a volume ratio of 1:1, and then dried in a drying oven at 60℃ for 24 h. After grinding, hollow mesoporous carbon support was obtained.
[0044] (4) Disperse 40 mg of hollow mesoporous carbon support in 20 mL of ultrapure water, and add 1.5 mL of chloroplatinic acid solution (concentration of 7.4 mg). Pt mL -1 Afterwards, the mixture was sonicated for 30 min and labeled as solution A. 16 mg of cobalt acetylacetone, 8 mg of iron acetylacetone, 12 mg of copper acetylacetone, and 16 mg of gallium acetylacetone were weighed and dispersed in 20 mL of anhydrous ethanol, with a platinum to metal molar ratio of 1:2.8 and a cobalt:iron:copper:gallium molar ratio of 2:1:2:2. The mixture was sonicated until completely dissolved and labeled as solution B. Solution B was added dropwise to solution A, and after sonication for 30 min, the mixture was stirred at room temperature for 12 h to obtain a suspension. The suspension was then rotary evaporated at 60 °C to obtain the catalyst precursor. The obtained precursor was placed in a tube furnace and heat-treated in a 5 vol% argon-hydrogen mixed gas at a heating rate of 5 °C / min. -1The heat treatment temperature was 800℃, the holding time was 3 h, and then the temperature was reduced to 400℃ within 1 h. After natural cooling to room temperature, it was acid washed with 0.1 M HClO4 solution for 12 h, filtered, and dried to obtain a high-stability ordered platinum alloy fuel cell cathode catalyst with a noble metal loading of 20% supported on a hollow carbon support. The actual metal content was determined by ICP: Pt 22.8 wt.%, Fe 2.90 wt.%, Cu 1.77 wt.%, Co 1.59 wt.%, Ga 0.97 wt%, with an atomic ratio of Pt:Fe:Cu:Co:Ga = 8.4:3.3:2.0:1.9:1.0.
[0045] The prepared hollow carbon support was subjected to BET testing, and the results are as follows: Figure 1 As shown, based on the nitrogen adsorption isotherm and pore size analysis diagram, the specific surface area of the hollow carbon support is 1195 m². 2 g -1 The main feature is mesopores with a diameter of 6 nm. Combined with transmission electron microscopy images, it is confirmed that the synthesized support is a hollow mesoporous structure.
[0046] The high-stability ordered platinum alloy fuel cell cathode catalyst supported on a hollow carbon support prepared in Example 1 was characterized by transmission electron microscopy, and the results are as follows: Figure 2 As shown, the overall morphology is a hollow sphere, and the obtained nanoparticles are uniformly loaded on the surface of the carrier.
[0047] Statistical analysis was performed on the particle size of the high-stability ordered platinum alloy fuel cell cathode catalyst nanoparticles supported on hollow carbon support obtained in Example 1. The results are as follows: Figure 3 As shown, the average particle size of the nanoparticles is 2.08 nm. The small particle size and uniform distribution are beneficial for exposing more catalytic active sites.
[0048] The high-stability ordered platinum alloy fuel cell cathode catalyst supported on a hollow carbon support prepared in Example 1 was characterized by X-ray diffraction, and the results are as follows: Figure 4 As shown, the diffraction peaks of the obtained catalyst match those of the platinum-cobalt alloy, indicating the successful synthesis of the alloy. Furthermore, the presence of obvious superlattice peaks at 23° and 32° proves the formation of its ordered structure.
[0049] The high-stability ordered platinum alloy fuel cell cathode catalyst supported on a hollow carbon support prepared in Example 1 was tested in a three-electrode system to assess its performance and stability. A standard hydrogen electrode was used as the reference electrode, a carbon rod as the counter electrode, and a rotating disk electrode covered with a catalyst film as the working electrode. A 0.1 M HClO4 solution was used as the electrolyte. The results are as follows: Figure 5As shown, the catalyst exhibited no significant performance degradation after undergoing 80,000 cycles of accelerated aging testing, demonstrating excellent stability.
[0050] Figure 6 The figure shows the stability test results of the hollow carbon-supported, highly stable ordered platinum alloy fuel cell cathode catalyst prepared in Example 1 of this invention when assembled into a single cell. It can be seen that the hollow carbon-supported, highly stable ordered platinum alloy fuel cell cathode catalyst prepared in this invention exhibits high stability under hydrogen-air conditions, maintaining 96% of its peak power density even after 50,000 accelerated aging cycles. This demonstrates the excellent stability of the hollow carbon-supported, highly stable ordered platinum alloy fuel cell cathode catalyst prepared in this invention within the fuel cell.
[0051] Example 2 The difference between Example 2 and Example 1 is that step (4) was adjusted in terms of the addition of the transition metal. The original 16 mg cobalt acetylacetonate, 8 mg iron acetylacetonate, 12 mg copper acetylacetonate, and 16 mg gallium acetylacetonate were changed to 16 mg cobalt acetylacetonate, 8 mg iron acetylacetonate, and 12 mg copper acetylacetonate. The molar ratio of platinum to metal was 1:2, and the molar ratio of cobalt:iron:copper was 2:1:2. The rest of the preparation process was the same as in Example 1, and a cathode catalyst was obtained.
[0052] Example 3 The difference between Example 3 and Example 1 is that the addition of the transition metal in step (4) was adjusted. The original 16 mg cobalt acetylacetonate, 8 mg iron acetylacetonate, 12 mg copper acetylacetonate, and 16 mg gallium acetylacetonate were changed to 16 mg cobalt acetylacetonate and 8 mg iron acetylacetonate. The molar ratio of platinum to metal was 1:1.2, and the molar ratio of cobalt to iron was 2:1. The rest of the preparation process was the same as in Example 1, and the cathode catalyst was obtained.
[0053] Example 4 The difference between Example 4 and Example 1 is that the addition of the transition metal was adjusted in step (4). 16 mg of cobalt acetylacetonate, 8 mg of iron acetylacetonate, 12 mg of copper acetylacetonate, and 16 mg of gallium acetylacetonate were changed to 16 mg of cobalt acetylacetonate, wherein the molar ratio of platinum to metal was 1:1. The rest of the preparation process was the same as in Example 1, and a cathode catalyst was obtained.
[0054] Figure 7The figures show the three-electrode performance of the pentagonal, quaternary, ternary, and binary ordered platinum alloy fuel cell cathode catalysts prepared in Examples 1, 2, 3, and 4 of this invention. It can be seen that the three-electrode performance of the different high-stability ordered platinum alloy fuel cell cathode catalysts is superior to that of commercial Pt / C, and the performance order is: pentagonal ordered alloy > quaternary ordered alloy > ternary ordered alloy > binary ordered alloy. This indicates that the type and quantity of transition element doping has a significant impact on the performance of the prepared catalysts. This is because adding different doping elements produces different compressive strains, leading to changes in activity.
[0055] Example 5 The difference between Example 5 and Example 1 is that the addition of the transition metal in step (4) was adjusted. The original 16 mg cobalt acetylacetonate, 8 mg iron acetylacetonate, 12 mg copper acetylacetonate, and 16 mg gallium acetylacetonate were changed to 16 mg cobalt acetylacetonate, 8 mg iron acetylacetonate, and 16 mg gallium acetylacetonate. The molar ratio of platinum to metal was 1:2, and the molar ratio of cobalt:iron:gallium was 2:1:2. The rest of the preparation process was the same as in Example 1, and a cathode catalyst was obtained.
[0056] Example 6 The difference between Example 6 and Example 1 is that the addition of the transition metal in step (4) was adjusted. The original 16 mg cobalt acetylacetonate, 8 mg iron acetylacetonate, 12 mg copper acetylacetonate, and 16 mg gallium acetylacetonate were changed to 16 mg cobalt acetylacetonate, 12 mg copper acetylacetonate, and 16 mg gallium acetylacetonate. The molar ratio of platinum to metal was 1:2.4, and the molar ratio of iron to copper to gallium was 1:1:1. The rest of the preparation process was the same as in Example 1, and the cathode catalyst was obtained.
[0057] Example 7 The difference between Example 7 and Example 1 is that the addition of the transition metal in step (4) was adjusted. The original 16 mg cobalt acetylacetonate, 8 mg iron acetylacetonate, 12 mg copper acetylacetonate, and 16 mg gallium acetylacetonate were changed to 16 mg cobalt acetylacetonate and 16 mg gallium acetylacetonate. The molar ratio of platinum to metal was 1:1.6, and the molar ratio of cobalt to gallium was 1:1. The rest of the preparation process was the same as in Example 1, and the cathode catalyst was obtained.
[0058] The materials prepared in Examples 1-7 were subjected to electrochemical performance tests, and the results are shown in Table 2.
[0059] Table 2
[0060] As shown in Table 2, Examples 1-7 demonstrate that Ga exhibits a positive regulatory effect in different alloy compositions such as PtCo, PtFeCo, and PtCoCu. Its effect is not simply to increase the number of metal components, but rather to create a synergistic effect with transition metals such as Fe, Co, and Cu, optimizing the electronic structure and lattice state of the platinum-based alloy. Among these, the PtFeCoCuGa pentagonal alloy, which simultaneously exerts the synergistic regulatory effect of Fe, Co, Cu, and Ga, achieved the highest half-wave potential and mass activity, indicating that this pentagonal composition possesses superior overall catalytic performance.
[0061] Example 8 The difference between Example 8 and Example 1 is that the heat treatment temperature in step (4) was adjusted to 500℃, 600℃, 700℃ and 900℃, while the rest of the preparation process was the same as in Example 1, and a cathode catalyst was obtained.
[0062] Table 3
[0063] As shown in Table 3, Example 8 demonstrates that the oxygen reduction performance of the PtFeCoCuGa catalyst exhibits a volcano-like relationship of first increasing and then decreasing with increasing annealing temperature, reaching its optimum at 800℃. At lower annealing temperatures, the diffusion of multi-metal atoms is insufficient, resulting in lower alloying and ordering levels; at excessively high annealing temperatures, particle growth, agglomeration, and local component migration are easily induced, leading to a reduction in effective active sites. Therefore, 800℃ is the preferred annealing temperature.
[0064] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that the hollow mesoporous carbon support in step (4) is changed to the commercial carbon support Ketjenblack EC-600JD, and the rest of the preparation process is the same as in Example 1, and a cathode catalyst is obtained.
[0065] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that solution B in step (4) is replaced with 20 mL of ethanol that does not contain any metals, while the rest of the preparation process is the same as in Example 1, and a cathode catalyst is obtained.
[0066] Comparative Example 3 Commercial Pt / C catalysts produced by Johnson Matthey in the UK.
[0067] The electrochemical performance of the materials prepared in the comparative example was tested, and the results are shown in Table 4.
[0068] Table 4
[0069] As shown in Table 4, the activity of Comparative Examples 1-3 decreased to varying degrees compared to the Examples. This indicates that the morphology of the support and the doping of the transition metal have a significant impact. When the support was replaced with a commercial support, the nanoparticles were unevenly dispersed, the nanoparticle size was larger, the mass activity was significantly reduced, the platinum atom utilization rate was relatively low, and the activity decreased. When only platinum was used without the addition of transition metals, intermetallic compounds could not be formed, and the activity was lower than that of the ordered intermetallic compounds in Examples 1-4 and Comparative Example 1.
[0070] Comparative Example 4 The difference between Comparative Example 4 and Example 1 is that the acid washing with HClO4 solution in step (4) is not performed. The rest of the preparation process is the same as that in Example 1. The cathode catalyst was obtained. The test results showed that the active sites on the catalyst surface were covered and the activity decreased significantly.
[0071] Figure 8 The graph shows a comparison of the stability retention rate of the hollow mesoporous carbon-supported, highly stable, ordered platinum-based fuel cell cathode catalyst prepared in Example 1 of this invention when assembled into a single cell with literature. The analytical explanation is shown in Table 5.
[0072] Table 5
[0073] As shown above, the prepared catalyst exhibited high activity and stability at ultra-low loading (0.02 mg / L). Pt cm -2 This is significantly lower than the catalyst loading reported in the past five years (0.1 mg). Pt cm -2 Under the premise of average level, after 30,000 accelerated aging cycles, it has 1.30 A mg. Pt -1 With high mass activity and a 90% retention rate, it surpasses most platinum-based catalysts reported in the past five years, demonstrating its high application potential.
[0074] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the present invention.
Claims
1. A method for preparing a highly stable ordered platinum-based fuel cell cathode catalyst supported on hollow mesoporous carbon, characterized in that: include, Tetraethyl orthosilicate, ammonia, resorcinol and formaldehyde were dispersed in a mixed solvent of ethanol and ultrapure water and stirred at room temperature to obtain a flocculent orange suspension. After centrifugation, washing and drying, the flocculent orange suspension is subjected to a first high-temperature annealing and carbonization treatment in an inert atmosphere, followed by alkaline washing and etching to remove the silicon template, resulting in a hollow mesoporous carbon support. The hollow mesoporous carbon support is dispersed in a water-alcohol mixture, and a platinum precursor and one or more metal precursors selected from iron, cobalt, copper and gallium are added. After stirring until fully adsorbed, the solvent is removed by rotary evaporation to obtain the catalyst precursor. The catalyst precursor was subjected to a second high-temperature annealing treatment in a reducing atmosphere to allow platinum to form an ordered intermetallic compound with the transition metal. The annealed product was subjected to acid treatment to remove unstable metal components on the surface, and then dried to obtain the cathode catalyst.
2. The preparation method according to claim 1, characterized in that: The centrifugation speed is 11800-12000 rpm, and the time is 2-3 min.
3. The preparation method according to claim 1, characterized in that: The first high-temperature annealing and carbonization treatment is carried out in an argon or nitrogen atmosphere, with a heating rate of 0.5-10℃ / min. -1 The temperature is 700-1000℃, and the time is 3-5 hours.
4. The preparation method according to claim 1, characterized in that: The second high-temperature annealing treatment is performed in an argon-hydrogen mixture, with a hydrogen volume content of 5-10 vol%, and a heating rate of 0.5-10℃ / min. -1 The heat treatment temperature is 500-1100℃, and the heat treatment time is 1-6 h.
5. The preparation method according to claim 1, characterized in that: The solutions used in acid treatment include dilute perchloric acid, dilute hydrochloric acid, or dilute sulfuric acid solutions with a concentration of 0.08-0.1 M.
6. The preparation method according to claim 1, characterized in that: The molar ratio of platinum precursor to metal precursor is 1-2:1-5, wherein the molar ratio of each metal precursor is 1-2:1-2.
7. The hollow mesoporous carbon-supported, highly stable, ordered platinum-based fuel cell cathode catalyst prepared by the preparation method described in claims 1 to 6.
8. The application of the hollow mesoporous carbon-supported, highly stable, ordered platinum-based fuel cell cathode catalyst as described in claim 7 in the oxygen reduction reaction at the cathode of a proton exchange membrane fuel cell.