Vanadium flow battery capacity recovery method and device

By using alcohol-based organic compounds as reducing agents to react with the positive electrode electrolyte of vanadium redox flow batteries at room temperature, the problems of high cost and poor stability in capacity recovery of vanadium redox flow batteries in the prior art are solved, achieving low-cost, high-efficiency electrolyte capacity recovery and battery life extension.

CN123162245APending Publication Date: 2026-11-24NATIONAL UNIVERSITY OF SINGAPORE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510669625.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-22
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing methods for restoring the capacity of vanadium redox flow batteries suffer from problems such as increased costs due to excessive use of reducing agents, instability caused by high-temperature reactions, and operational complexity, making it difficult to effectively restore the valence state and capacity of the electrolyte.

Method used

An alcohol-based organic compound is used as a reducing agent to react with the positive electrode electrolyte at room temperature. The reaction takes place through a catalyst bed, avoiding precipitation under high temperature conditions and ensuring the stability and capacity recovery of the electrolyte.

Benefits of technology

It achieves low-cost and efficient electrolyte capacity recovery, avoids electrode contamination, ensures reaction controllability and system compatibility, and significantly extends battery cycle life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123162245A_ABST
    Figure CN123162245A_ABST
Patent Text Reader

Abstract

This invention provides a method and apparatus for restoring the capacity of a vanadium redox flow battery. The method includes: providing a vanadium redox flow battery that has experienced capacity decay; uniformly mixing a positive electrolyte and a negative electrolyte and dividing them into two equal volumes to form a positive electrolyte to be restored and a negative electrolyte to be restored, and respectively containing them in the positive and negative electrode chambers of the vanadium redox flow battery; charging the vanadium redox flow battery to its original battery cutoff voltage; reacting the positive electrolyte to be restored with a certain volume of reducing agent under the action of a catalyst; and recharging the vanadium redox flow battery to its original battery cutoff voltage, thereby restoring the capacity of the vanadium redox flow battery; wherein the reducing agent is an alcohol-based organic compound; and the volume of the reducing agent is calculated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of vanadium redox flow batteries, and more particularly to a method and apparatus for capacity recovery of vanadium redox flow batteries. Background Technology

[0002] The statements herein are provided only as background information in connection with this application and do not necessarily constitute prior art.

[0003] Vanadium redox flow batteries (VFBs) have emerged as one of the most promising large-scale energy storage systems due to their power and capacity decoupling, high safety, and wide range of applications. However, their commercialization is hampered by performance degradation, such as capacity loss and reduced efficiency during long-term cycling, thus shortening the lifespan of VFB systems. The primary cause of VFB capacity loss is electrolyte imbalance due to the cross-contamination of different ion species. Factors such as electric field, concentration gradient, pressure difference, and side reactions contribute to the electrolyte imbalance caused by the cross-contamination of four vanadium ions (V4, V5, V6, V7, V8, V9, V10, V20, V3, V ...6, V7, V8, V9, V10 2+ V 3+ VO 2+ and VO2 + Vanadium molecules migrate across the membrane at different rates, leading to an imbalance in vanadium concentration and oxidation state. Furthermore, water molecules migrate along with protons and vanadium ions, causing a volume imbalance between the positive and negative electrode electrolytes. A widely used post-cycle capacity recovery method involves remixing the positive and negative electrode electrolytes to balance the concentration and volume of both. However, this method does not address problems such as valence state changes caused by side reactions and air oxidation due to imperfect battery sealing.

[0004] In the prior art, some methods have been proposed to restore the valence state and capacity of the electrolyte by remixing and quantitatively adding a reducing agent (e.g., oxalic acid), while simultaneously restoring energy efficiency by swapping the positive and negative electrodes. Further attempts include online recovery methods that use organic acids (e.g., oxalic acid or tartaric acid) as reducing agents and accelerate the reaction through heating and stirring. However, these methods have the following drawbacks: (1) excessive use of reducing agents increases costs; (2) high-temperature reactions may lead to VO2+ depletion. + (3) The process is complex and requires heating and subsequent cooling. Summary of the Invention

[0005] The purpose of this invention is to overcome the above-mentioned shortcomings of the prior art and provide a method and apparatus for capacity recovery of vanadium redox flow batteries. It uses an alcohol-based organic compound as a reducing agent, which can efficiently reduce high-valence vanadium ions at room temperature, avoid the risk of precipitation under high temperature conditions, and at the same time significantly reduce the consumption of reducing agent, thereby improving cost-effectiveness and ease of operation.

[0006] To achieve the above-mentioned objectives of the present invention, an embodiment of the first aspect of the present invention provides a method and apparatus for capacity recovery of a vanadium redox flow battery. The method includes:

[0007] Provide a vanadium redox flow battery that has experienced capacity decay, and uniformly mix the positive and negative electrolytes of the vanadium redox flow battery;

[0008] The resulting mixed electrolyte is divided into two equal parts of the same volume to form a positive electrolyte to be recovered and a negative electrolyte to be recovered. The positive electrolyte to be recovered and the negative electrolyte to be recovered are respectively contained in the positive electrode chamber and the negative electrode chamber of the vanadium redox flow battery.

[0009] Charge the vanadium redox flow battery to the original battery cutoff voltage;

[0010] The positive electrode electrolyte to be restored reacts with a certain volume of reducing agent under the action of a catalyst; and

[0011] The vanadium redox flow battery is recharged to its original cutoff voltage to restore its capacity.

[0012] The reducing agent is an alcohol-based organic compound;

[0013] The volume of the reducing agent is calculated as follows:

[0014]

[0015] In the formula, n is the number of moles of vanadium ions on each side, x is the change in the average valence state of vanadium ions relative to 3.5, M is the molecular weight of the reducing agent, and N is the ratio of the reducing agent to VO2. + The number of electrons transferred during the reaction, where ρ is the density of the reducing agent.

[0016] A second aspect of the present invention provides an apparatus for recovering the capacity of a vanadium redox flow battery, applied to a method for recovering the capacity of a vanadium redox flow battery according to an embodiment of the first aspect of the present invention. The apparatus includes:

[0017] The reaction chamber was restored, in which a catalyst bed was permanently installed.

[0018] The recovery reaction chamber is configured for:

[0019] This is connected to the positive electrode chamber of the vanadium redox flow battery.

[0020] The reducing agent and the positive electrolyte to be restored from the positive electrode chamber are received in a certain volume, thereby allowing the reducing agent and the positive electrolyte to be restored to react under the action of the catalyst.

[0021] The fully reacted positive electrode electrolyte is returned from the recovery reaction chamber to the positive electrode chamber.

[0022] The advantages of the method for recovering the capacity of vanadium redox flow batteries according to the present invention are summarized as follows:

[0023] In a method for restoring the capacity of vanadium redox flow batteries, the process involves mixing positive and negative electrode electrolytes to balance their valence states, concentrations, and volumes. Based on the electrolyte's valence state, a calculated amount of reducing agent is added to the positive electrode electrolyte so that its valence state and volume match those of the negative electrode electrolyte, thereby fully restoring the electrolyte's capacity. This method employs an alcohol-based organic compound capable of donating multiple electrons as the reducing agent, effectively mitigating the capacity decay associated with the increase in the average valence state of the electrolyte after prolonged use. This strategy is characterized by its simplicity, ease of implementation, and low cost, achieving near-complete recovery of coulombic efficiency and capacity.

[0024] The advantages of the method used to restore the capacity of vanadium redox flow batteries are summarized as follows:

[0025] In devices used to recover the capacity of vanadium redox flow batteries, direct contact between the reducing agent and the electrode is prevented by providing a recovery reaction chamber separate from the positive electrode chamber, thus avoiding electrode contamination. This configuration enhances reaction controllability to ensure the retention of high-valence vanadium ions (VO2+). + Complete restoration of the electrolyte. Furthermore, since positive electrolyte circulation can be easily achieved through piping connections, it exhibits strong system compatibility. Attached Figure Description

[0026] To more clearly illustrate the specific embodiments of this application or the technical solutions in the prior art, the accompanying drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings in the following description are some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without any creative effort.

[0027] Figure 1 This is a schematic diagram of a vanadium redox flow battery system, illustrating the reaction mechanism of capacity decay and average valence state increase during charge-discharge processes after long-term cycling.

[0028] Figure 2 The positive electrode electrolyte for vanadium redox flow batteries (VO) 2+ / VO2 + The CV curves of methanol and ethylene glycol, and the LSV curves of methanol and ethylene glycol;

[0029] Figure 3A VO with / without ethylene glycol as a reducing agent 2+ / VO2 + UV-Vis spectrum of the electrolyte;

[0030] Figure 3B This is a graph showing the relationship between electrolyte absorbance and the amount of ethylene glycol added.

[0031] Figure 4A The battery capacity and coulombic efficiency before and after the recovery process are shown;

[0032] Figure 4B The voltage curves after the initial cycle and recovery are shown. The current density is 100 mA / cm². 2 ;

[0033] Figure 5A The structure of the recovery reaction chamber for carrying out the electrolyte recovery reaction is shown;

[0034] Figure 5B The structure of a recovery reaction chamber for electrolyte capacity recovery, constructed as part of a battery system, is shown. Detailed Implementation

[0035] To make the technical problems, technical solutions, and beneficial effects to be solved by this application clearer, the following detailed description is provided in conjunction with embodiments. It should be understood that the specific embodiments described herein are for illustrative purposes only and are not intended to limit the scope of this application.

[0036] In this application, the term "and / or" describes the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can mean: A exists alone, A and B exist simultaneously, or B exists alone. A and B can be singular or plural. The character " / " typically indicates that the preceding and following related objects are in an "or" relationship.

[0037] In this application, "at least one" means one or more, and "more than one" means two or more. "At least one of the following" or similar expressions refer to any combination of these items, including any combination of single or multiple items. For example, "at least one of a, b or c" or "at least one of a, b and c" can mean: a, b, c, ab (i.e., a and b), ac, bc or abc, where a, b and c can be single or multiple.

[0038] It should be understood that in the various embodiments of this application, the sequence number of the above process does not represent the order of execution. Some or all steps can be executed in parallel or sequentially. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of this application.

[0039] The terminology used in the embodiments of this application is for describing specific embodiments only and is not intended to limit this application. The singular forms "a," "the," and "the" used in the embodiments of this application and the appended claims are also intended to include the plural forms, unless the context clearly indicates otherwise.

[0040] The weights of the components mentioned in the embodiments of this application refer not only to the specific content of each component but also to the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is scaled up or down proportionally according to the embodiments of this application, it is within the scope disclosed in the embodiments of this application. Specifically, the mass described in the embodiments of this application can be a mass unit known in the chemical industry, such as μg, mg, g, kg, etc.

[0041] The terms "first" and "second" are used for descriptive purposes only to distinguish objects such as matter, and should not be construed as indicating or implying relative importance or the number of technical features indicated. For example, without departing from the scope of the embodiments of this application, a first XX may also be referred to as a second XX, and similarly, a second XX may also be referred to as a first XX. Therefore, features defined as "first" and "second" may explicitly or implicitly include one or more of the stated features.

[0042] Figure 1 This is a schematic diagram of a vanadium redox flow battery system, illustrating the reaction mechanism of capacity decay and average valence state increase during long-term cycling and charge-discharge processes.

[0043] This application aims to develop a low-cost, high-efficiency online capacity and efficiency recovery strategy for vanadium redox flow batteries (VFBs). This strategy specifically addresses the capacity imbalance of VFB electrolytes after long-term cycling. It employs a series of low-cost alcohol-based organic molecules as recovery agents, which can significantly compensate for VFB capacity decay. Taking a commercial all-vanadium redox flow battery as an example, after long-term cycling, these organic molecules can balance the average valence state of the electrolyte, restoring the battery capacity to its initial level. This strategy does not introduce other impurities; the generated products are only water and carbon dioxide gas. Favorable reaction kinetics also ensure a rapid recovery process.

[0044] The capacity recovery strategy disclosed in this paper can significantly extend the cycle life of battery systems without disassembly or long-term downtime for maintenance. The rapid reaction at room temperature and the high energy density of the reducing agent ensure low chemical consumption, thereby reducing costs and enabling timely and rapid online capacity recovery of the battery system.

[0045] According to a first aspect of this application, a method for capacity recovery of a vanadium redox flow battery is provided. The method includes:

[0046] Provide a vanadium redox flow battery that has experienced capacity decay, and uniformly mix the positive and negative electrolytes of the vanadium redox flow battery;

[0047] The resulting mixed electrolyte is divided into two equal parts of the same volume to form a positive electrolyte to be recovered and a negative electrolyte to be recovered. The positive electrolyte to be recovered and the negative electrolyte to be recovered are respectively contained in the positive electrode chamber and the negative electrode chamber of the vanadium redox flow battery.

[0048] Charge the vanadium redox flow battery to the original battery cutoff voltage;

[0049] The positive electrode electrolyte to be restored reacts with a certain volume of reducing agent under the action of a catalyst;

[0050] The vanadium redox flow battery is recharged to its original cutoff voltage to restore its capacity.

[0051] The reducing agent is an alcohol-based organic compound.

[0052] The required volume of the reducing agent is calculated as follows:

[0053]

[0054] In the formula, n is the number of moles of vanadium ions on each side, x is the change in the average valence state of vanadium ions relative to 3.5, M is the molecular weight of the reducing agent, and N is the ratio of the reducing agent to VO2. + The number of electrons transferred during the reaction, where ρ is the density of the reducing agent.

[0055] The average valence state of vanadium ions can be calculated using the following formula: First, let's consider the theoretical capacity of the electrolyte:

[0056] Where Q is the theoretical capacity of the electrolyte, V is the volume of electrolyte on one side (equal for both positive and negative electrodes), C is the concentration of vanadium ions in the electrolyte, F is the Faraday constant, and N... V The number of electron transfers in the electrolyte is taken as 1, and 3600 is the unit conversion factor (3600 seconds / hour).

[0057]

[0058] Q0 is the initial charge capacity for the first cycle, Q R This refers to the recharge capacity after electrolyte mixing and before the valence state is restored. In actual operation of the battery pack, Q0 and Q... R The value is recorded by the control system.

[0059] A method for capacity recovery in vanadium redox flow batteries includes mixing positive and negative electrode electrolytes to achieve equilibrium in valence state, concentration, and volume. Based on the valence state of the electrolytes, a certain amount of reducing agent is added to the positive electrode electrolyte to match its valence state and volume with those of the negative electrode electrolyte, thereby fully restoring the electrolyte capacity. This method uses an alcohol-based organic compound capable of donating multiple electrons as the reducing agent, effectively mitigating capacity decay caused by the increase in the average valence state of the electrolyte after prolonged use. This method is simple, easy to implement, and inexpensive, achieving near-complete recovery of coulombic efficiency and capacity.

[0060] In one embodiment of this application, the reaction between the reducing agent and the positive electrolyte to be restored is carried out at room temperature in the presence of a catalyst.

[0061] In this embodiment, the room temperature reaction avoids the VO2 under high temperature conditions required in previously reported methods. + The precipitation of .

[0062] In one embodiment of this application, the step of reacting the positive electrode electrolyte to be restored with a certain volume of reducing agent under the action of the catalyst includes: adding the catalyst and the certain volume of reducing agent to a recovery reaction chamber connected to the positive electrode chamber; transferring the positive electrode electrolyte to be restored from the positive electrode chamber to the recovery reaction chamber for reaction; and returning the reacted positive electrode electrolyte from the recovery reaction chamber to the positive electrode chamber.

[0063] By conducting the reaction in a dedicated recovery chamber separate from the positive electrode chamber, direct contact between the reducing agent and the electrode is avoided, thus preventing electrode contamination. This structure enhances the controllability of the reaction, ensuring the preservation of high-valence vanadium ions (VO2+). + Complete reduction of the positive electrode electrolyte. Furthermore, since the circulation of the positive electrode electrolyte can be achieved through simple piping connections, it offers strong system compatibility.

[0064] In one embodiment of this application, the recovery reaction chamber is a packed bed reaction chamber, in which a catalyst bed is fixedly disposed, and the catalyst bed is filled with a support for an alcohol oxidation catalyst. When the positive electrode electrolyte to be recovered is transferred from the positive electrode chamber to the recovery reaction chamber for reaction, the positive electrode electrolyte to be recovered is introduced from the positive electrode chamber into the recovery reaction chamber and flows through the fixed catalyst bed until the positive electrode electrolyte to be recovered and the reducing agent react completely under the action of the catalyst.

[0065] In this embodiment, the recovery reaction chamber is designed as a packed bed reactor, wherein the fixed catalyst layer is a platinum-supported graphite felt composite material. This design increases the catalytic surface area, enhances mass transfer, and improves VO2... + The reduction rate is increased by more than 3 times, while preventing catalyst leaching.

[0066] In one embodiment of this application, the loading of the alcohol oxidation catalyst is 1-30 mg / cm³. 2 Preferably 10 mg / cm 2 Excessive loading may limit mass transfer and reduce catalytic efficiency, while insufficient loading will lead to incomplete reaction.

[0067] In one embodiment of this application, the reaction is carried out under stirring.

[0068] In one embodiment of this application, the carrier is a commercially available graphite felt composite material. In one embodiment of this application, the catalyst is a platinum (Pt) catalyst.

[0069] In one embodiment of this application, the oxidation potential of the alcohol-based organic compound is lower than that of V0. 2+ / VO2 + .

[0070] In this embodiment, the oxidation potential is selected to be lower than the redox potential (VO) of the positive electrode electrolyte. 2+ / VO2 + The alcohol-based organic compounds (1.01V vs. SHE) ensure cost-effectiveness.

[0071] In one embodiment of this application, the reducing agent is selected from any one of methanol (CH3OH), ethanol (C2H5OH), ethylene glycol (C2H6O2), 2-propanol (C3H7OH), 1-propanol (C3H7OH), glycerol (C3H8O3), and 1-butanol (C4H9OH).

[0072] These alcohols are widely used commercial alcohol-based organic compounds that are inexpensive and environmentally friendly, thus reducing processing costs and environmental hazards.

[0073] Unlike previous methods using organic acids, alcohol-based organic compounds have lower oxidation potentials and each molecule can provide more electrons. This can increase energy density and reduce cost. Furthermore, the final oxidation products of these alcohol molecules, CO2 and H2O, do not introduce other impurities, thus allowing VFB capacity to be recovered without affecting stability or other properties.

[0074] In one embodiment of this application, the reducing agent is methanol or ethylene glycol.

[0075] In one embodiment of this application, the vanadium redox flow battery that has experienced capacity decay is a vanadium redox flow battery with a capacity retention rate of less than 90% or after at least 50 cycles. In another embodiment of this application, the vanadium redox flow battery that has experienced capacity decay is a vanadium redox flow battery with a capacity retention rate of less than 80% or after at least 200 cycles.

[0076] In one embodiment of this application, an electrolyte mixing tube is provided between the positive electrode chamber and the negative electrode chamber, and an electrolyte balance valve is provided on the electrolyte mixing tube. The electrolyte balance valve is opened, and after the positive electrolyte and the negative electrolyte in the positive electrode chamber and the negative electrode chamber are mixed evenly and reach electrolyte volume balance, the electrolyte balance valve is closed, thereby obtaining equal volumes of the positive electrolyte to be restored and the negative electrolyte to be restored.

[0077] This embodiment achieves on-site mixing and volume balance of the electrolyte through integrated piping, eliminating the need for external equipment and maintaining the structural integrity of the battery system.

[0078] In one specific embodiment, a static mixer, such as a spiral blade, is provided in the electrolyte mixing tube to achieve uniform mixing of the positive and negative electrolytes.

[0079] In another specific embodiment, the mixing of the positive electrode electrolyte and the negative electrode electrolyte is carried out in a positive electrode chamber or a negative electrode chamber, in which a magnetic stirrer is provided.

[0080] In another embodiment of this application, a dedicated mixing chamber is provided for mixing the positive and negative electrolytes. This mixing operation may include the following steps: delivering the positive and negative electrolytes to the mixing chamber via a delivery pump; and performing forced circulation mixing within the mixing chamber until the electrolyte reaches a homogeneous state (confirmed by UV-Vis spectroscopy, VO at different sampling points). 2+ (Absorbance deviation less than 2%); then the mixed electrolyte is divided into equal parts to obtain equal volumes of positive electrode electrolyte to be restored and negative electrode electrolyte to be restored.

[0081] In this embodiment, higher mixing efficiency can be achieved, and an integrated liquid level sensor is used to control precise volume distribution.

[0082] In another embodiment, electrolyte mixing can be performed manually: extract the positive and negative electrolytes into an external container; stir manually for 10-15 minutes until completely homogeneous; use a graduated cylinder or scale to divide the mixed electrolyte into two equal parts, and return the two equal volumes of the two parts to their respective chambers.

[0083] In one embodiment of this application, a method for restoring the capacity of a vanadium redox flow battery (VFB) includes the following steps: (1) After long-term cycling, when the capacity retention rate drops below a certain value (e.g., 80%) or after a certain number of cycles (e.g., 200 cycles), the positive and negative electrolytes are mixed. (2) The mixture is then uniformly divided into two parts, which are used as new negative and positive electrolytes, respectively. (3) The new electrolytes are fully charged to the original battery cutoff voltage. (4) The required volume of reducing agent is calculated and added to the positive electrolyte, allowing it to react at room temperature under the action of a catalyst. (5) Finally, the electrolytes are fully charged to the original battery cutoff voltage to complete the capacity recovery process, enabling the battery system to return to normal operation and restoring its capacity and efficiency.

[0084] According to a second aspect of this application, an apparatus for restoring the capacity of a vanadium redox flow battery is provided, which is applied to the vanadium redox flow battery capacity restoration method according to the first aspect of this application. The apparatus includes a restoration reaction chamber in which a catalyst bed is fixedly disposed, and the restoration reaction chamber is configured to: communicate with the positive electrode chamber of the vanadium redox flow battery; receive a certain volume of reducing agent and the positive electrode electrolyte to be restored from the positive electrode chamber, thereby allowing the reducing agent and the positive electrode electrolyte to be restored to react under the action of the catalyst; and return the fully reacted positive electrode electrolyte from the restoration reaction chamber back to the positive electrode chamber.

[0085] In this vanadium redox flow battery capacity recovery device, by separating the recovery reaction chamber from the positive electrode chamber, direct contact between the reducing agent and the electrode is avoided, thus preventing electrode contamination. This structure enhances the controllability of the reaction, ensuring the efficient production of high-valence vanadium ions (VO2+). + Complete restoration of the positive electrode electrolyte. Furthermore, since the circulation of the positive electrode electrolyte can be achieved simply through pipe connections, the system boasts strong compatibility.

[0086] In one embodiment of this application, the device further includes: a liquid guide tube, through which the recovery reaction chamber is connected to the positive electrode chamber to form a circulation loop that allows the positive electrode electrolyte to circulate in the recovery reaction chamber and the positive electrode chamber, wherein a pump is provided in the circulation loop.

[0087] In one embodiment of this application, the catalyst bed is filled with a support for an alcohol oxidation catalyst.

[0088] In one embodiment of this application, the catalyst bed is filled with a graphite felt composite material loaded with a Pt catalyst.

[0089] In one embodiment of this application, the catalyst loading is 1-30 mg / cm³. 2 Preferably 10 mg / cm 2 .

[0090] In one embodiment of this application, a magnetic stirrer is provided in the recovery reaction chamber.

[0091] In one embodiment of this application, the recovery reaction chamber includes: an electrolyte inlet disposed at the bottom of the recovery reaction chamber, an electrolyte outlet disposed at the top of the recovery reaction chamber, and a reducing agent addition port.

[0092] In one embodiment of this application, the device further includes an electrolyte mixing device for mixing the positive electrolyte and the negative electrolyte and dividing the resulting mixed electrolyte into two equal parts of the same volume to form the positive electrolyte to be restored and the negative electrolyte to be restored.

[0093] In one embodiment of this application, the electrolyte mixing device includes: a pipeline disposed between the positive electrode chamber and the negative electrode chamber; a pump disposed on the pipeline for mixing the positive electrode electrolyte and the negative electrode electrolyte; and an electrolyte balance valve disposed on the pipeline for dividing the mixed electrolyte into two equal parts of the same volume to form the positive electrode electrolyte to be restored and the negative electrode electrolyte to be restored.

[0094] In one specific embodiment, a static mixer, such as a spiral blade, is provided on the electrolyte mixing tube to achieve uniform mixing of the positive and negative electrolytes.

[0095] In another embodiment of this application, the electrolyte mixing device includes: an independent mixing chamber connected to both the positive electrode chamber and the negative electrode chamber, and equipped with pipelines and a pump. In this embodiment, the positive electrode electrolyte and the negative electrode electrolyte are transported to the mixing chamber through pipelines under the action of the pump. After being mixed evenly in the mixing chamber, the mixed electrolyte is divided into two parts, which are respectively contained in the positive electrode chamber and the negative electrode chamber.

[0096] The following are demonstrations of detailed experiments and results used to verify the embodiments of the present invention. Specifically: Example 1: LVS Test

[0097] To ensure cost-effectiveness, an oxidation potential lower than the redox potential (VO2) of the positive electrode electrolyte is selected. 2+ / VO2 + A reducing agent (1.01V vs. SHE). Taking two basic alcohols, methanol and ethylene glycol (IUPAC name: ethane-1,2-diol), as examples, their chemical structures are as follows:

[0098] The oxidation potentials of methanol and ethylene glycol were measured using linear sweep voltammetry (LSV) in a 3.00 M sulfuric acid solution, and the redox potential of the positive electrode electrolyte was measured using cyclic voltammetry (CV) in the same solution.

[0099] Figure 2 VFB positive electrode electrolyte (VO 2+ / VO2 + The CV curves of methanol and ethylene glycol were obtained. Scan rate: 5 mV / s. Electrolyte: 1 M methanol / ethylene glycol / VOSO4 dissolved in 3 M H2SO4.

[0100] like Figure 2 As shown, the oxidation potentials of both methanol and ethylene glycol are lower than that of VO. 2+ / VO2 + The redox potentials of these molecules confirm their suitability as reducing agents in the capacity recovery strategy of this invention. Example 2: Reducing agents and VO2 + Experimental verification of electrolyte reaction

[0101] These reducing agents and VO 2+ The reaction of the electrolyte was experimentally verified.

[0102] Using ethylene glycol as a reducing agent, 1.00 M VO2 was used in 3.00 M sulfuric acid (diluted 10 times for measurement). 2+ Positive electrode electrolyte.

[0103] Figure 3A VO with / without ethylene glycol as a reducing agent 2+ / VO2 + Ultraviolet-visible spectrum of the electrolyte.

[0104] Figure 3B This is a graph showing the relationship between the absorbance of the electrolyte and the amount of ethylene glycol added.

[0105] like Figure 3A As shown, with the increase of ethylene glycol addition, the absorbance of the electrolyte increases, corresponding to VO 2+ Concentration increases. Figure 3B The 10-electron reaction was confirmed to occur in the presence of a Pt / C catalyst, which was generated by VO 2+ The linear change in absorbance value with the volume change of ethylene glycol confirms the effectiveness of the reducing agent.

[0106] Methanol and VO2 were also measured. + The 6-electron transfer between them. The equations for the two reactions are as follows. In this process, Pt acts as a catalyst, accelerating the reaction rate, increasing the reaction depth, and ensuring that all reducing agents are completely oxidized to CO2 and H2O. Ethylene glycol (10-electron transfer): Methanol (6-electron transfer): Ethanol (12-electron transfer): 1 / 2-Propanol (18-electron transfer): 1-Butanol (24-electron transfer): Example 3: Reducing agents and VO2 + Experimental verification of electrolyte reaction

[0107] The effectiveness of the capacity recovery strategy proposed in this application has been further verified in actual VFB operation.

[0108] A 1.00M vanadium electrolyte (vanadium ion valence of 3.5) was dissolved in a 3.00M sulfuric acid solution, and 2 mL of 1.00M vanadium electrolyte was used. 2+ As the positive electrode electrolyte, 20 mL of 1.00 MV 3+ As the negative electrode electrolyte, an electrode with an area of ​​5 cm² was fabricated. 2 A single-flow battery, at 100 mA / cm 2 It operates under a constant current density. For example... Figure 4A As shown, significant capacity decay was observed after prolonged cycling. The capacity recovery procedure after the 255th cycle is as follows:

[0109] 1) Mix the electrolytes in the two tanks; 2) Divide the mixed electrolyte into two equal parts and refill them into the two tanks of the battery; 3) Charge the battery according to the original cycle procedure and then stop; 4) Record the charging capacity and calculate the average valence state change of the electrolyte; 5) Determine the volume of alcohol reducing agent to be added based on the calculation result and formula of the average valence state change; 6) React the positive electrode electrolyte to be restored with the determined volume of reducing agent in the presence of a catalyst; 7) Recharge the vanadium redox flow battery to the cutoff voltage of the original battery to restore the capacity of the vanadium redox flow battery.

[0110] The capacity quickly recovered to the level of the initial cycle. Figure 4B The voltage curve is shown, in which a slight increase in polarization is observed, which may be due to a problem with the carbon felt electrode.

[0111] Based on the capacity changes observed before and after the recovery process, this strategy exhibits excellent capacity recovery performance while maintaining a high coulombic efficiency. Furthermore, the absence of significant side reactions and byproducts indicates a clean recovery process. Concentration change analysis further confirms that the reducing agent ethylene glycol underwent a complete 10-electron transfer reaction, ensuring its full utilization in the vanadium electrolyte capacity recovery process. Example 4: Construction of the Reconstruction Reaction Chamber

[0112] Figure 5AThe structure of the recovery reaction chamber for carrying out the electrolyte recovery reaction is shown.

[0113] The Pt catalyst (10 mg / cm) was coated 2 ) graphite felt immersed in VO 2 The electrolyte is added and stirred with a magnetic stirrer to complete the reaction. The recovery reaction chamber, used to restore electrolyte capacity, is constructed as part of the battery system, and its structure is as follows: Figure 5B As shown, the cathode electrolyte tank is connected to a packed bed reactor containing the catalyst, and a pump circulates the electrolyte between the two. The packed bed reactor is connected to the positive electrode chamber, i.e., the cathode electrolyte tank. A reducing agent is added to the reactor to allow the electrolyte to recover as it flows through the catalyst bed.

[0114] The above description is merely a preferred embodiment of this application and is not intended to limit this application. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.

Claims

1. A method for restoring the capacity of a vanadium redox flow battery, the method comprising: A vanadium redox flow battery with capacity decay is provided, wherein the positive and negative electrolytes of the vanadium redox flow battery are uniformly mixed. The resulting mixed electrolyte is divided into two equal parts of the same volume to form a positive electrolyte to be recovered and a negative electrolyte to be recovered. The positive electrolyte to be recovered and the negative electrolyte to be recovered are respectively contained in the positive electrode chamber and the negative electrode chamber of the vanadium redox flow battery. Charge the vanadium redox flow battery to the original battery cutoff voltage; The positive electrode electrolyte to be restored reacts with a certain volume of reducing agent under the action of a catalyst; as well as The vanadium redox flow battery is recharged to its original battery cutoff voltage to restore its capacity. The reducing agent is an alcohol-based organic compound; The volume of the reducing agent is calculated as follows: In the formula, n is the number of moles of vanadium ions on each side. x represents the change in the average valence state of vanadium ions relative to 3.

5. M is the molecular weight of the reducing agent. N represents the reducing agent and VO2. + The number of electrons transferred during the reaction ρ is the density of the reducing agent.

2. The method according to claim 1, wherein, The reaction between the reducing agent and the positive electrode electrolyte to be restored is carried out at room temperature in the presence of a catalyst.

3. The method according to claim 2, wherein, The step of reacting the positive electrode electrolyte to be restored with a certain volume of reducing agent under the action of the catalyst includes: The catalyst and a certain volume of reducing agent are added to the recovery reaction chamber connected to the positive electrode chamber, and the positive electrode electrolyte to be recovered is transferred from the positive electrode chamber to the recovery reaction chamber for reaction. The reacted positive electrolyte is returned from the recovery reaction chamber to the positive electrode chamber.

4. The method according to claim 3, wherein, The recovery reaction chamber is a packed bed reaction chamber, in which a catalyst bed is fixedly arranged, and the catalyst bed is filled with a support for alcohol oxidation catalyst.

5. The method according to claim 4, wherein, The loading of the alcohol oxidation catalyst is 1-30 mg / cm³. 2 ; and / or The reaction is carried out under stirring; and / or The carrier is a graphite felt composite material; and / or The catalyst is a Pt catalyst.

6. The method according to claim 1, wherein, The oxidation potential of the alcohol-based organic compound is lower than that of V0. 2+ / VO2 + .

7. The method according to claim 6, wherein, The reducing agent is selected from any one of methanol (CH3OH), ethanol (C2H5OH), ethylene glycol (C2H6O2), 2-propanol (C3H7OH), 1-propanol (C3H7OH), glycerol (C3H8O3), and 1-butanol (C4H9OH).

8. The method according to claim 7, wherein, The reducing agent is methanol or ethylene glycol.

9. The method according to claim 1, wherein, The vanadium redox flow battery that has experienced capacity decay is a vanadium redox flow battery with a capacity retention rate of less than 90% or after at least 50 cycles.

10. The method according to claim 1, wherein, An electrolyte mixing tube is provided between the positive electrode chamber and the negative electrode chamber, and an electrolyte balance valve is provided on the electrolyte mixing tube. The electrolyte balance valve is opened, and after the positive electrolyte and the negative electrolyte in the positive electrode chamber and the negative electrode chamber are mixed evenly and reach electrolyte volume balance, the electrolyte balance valve is closed, thereby obtaining equal volumes of the positive electrolyte to be restored and the negative electrolyte to be restored.

11. An apparatus for restoring the capacity of a vanadium redox flow battery, applied to the method of claim 1, comprising: A recovery reaction chamber, in which a catalyst bed is fixedly disposed, and the recovery reaction chamber is configured to communicate with the positive electrode chamber of the vanadium redox flow battery. The reducing agent and the positive electrolyte to be restored from the positive electrode chamber are received in a certain volume, thereby allowing the reducing agent and the positive electrolyte to be restored to react under the action of the catalyst. The fully reacted positive electrode electrolyte is returned from the recovery reaction chamber to the positive electrode chamber.

12. The apparatus of claim 11, further comprising: A liquid guide tube connects the recovery reaction chamber to the positive electrode chamber, forming a circulation loop that allows the positive electrode electrolyte to circulate in the recovery reaction chamber and the positive electrode chamber, wherein a pump is provided in the circulation loop.

13. The apparatus according to claim 11, wherein: The catalyst bed is filled with a support carrying an alcohol oxidation catalyst; and / or The loading of the alcohol oxidation catalyst is 1-30 mg / cm³. 2 ; and / or The recovery reaction chamber is equipped with a magnetic stirrer; and / or The recovery reaction chamber includes: an electrolyte inlet located at the bottom of the recovery reaction chamber, an electrolyte outlet located at the top of the recovery reaction chamber, and a reducing agent addition port.

14. The apparatus according to claim 13, wherein: The carrier is a graphite felt composite material; and / or The catalyst is a Pt catalyst.

15. The apparatus of claim 11, further comprising: An electrolyte mixing device is used to mix the positive electrolyte and the negative electrolyte and divide the resulting mixed electrolyte into two equal parts of the same volume to form the positive electrolyte to be restored and the negative electrolyte to be restored.

16. The apparatus according to claim 11, wherein, The electrolyte mixing device includes: A pipeline is disposed between the positive electrode chamber and the negative electrode chamber; A pump, disposed on the pipeline and used for mixing the positive and negative electrolytes; and An electrolyte balance valve is installed on the pipeline and is used to divide the mixed electrolyte into two equal parts of the same volume to form the positive electrolyte to be restored and the negative electrolyte to be restored.