Solid-state battery and method of manufacturing the same

By using cobalt-free cathode materials and halide solid electrolytes in solid-state batteries, combined with lithium anodes with three-dimensional network layers, the problems of lithium dendrites and interfaces were solved, resulting in a high-efficiency and stable improvement in battery performance, especially in terms of first-efficiency performance, rate performance and cycle performance.

CN123162264APending Publication Date: 2026-11-24SVOLT ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510675366.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-23
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

While existing solid-state batteries address the lithium dendrite problem, improving their initial efficiency, rate performance, and cycle performance is complex, and the stability and interface issues of the lithium anode have not been effectively resolved.

Method used

By employing cobalt-free cathode materials and halide solid electrolytes, combined with a lithium anode with a three-dimensional network layer, and optimizing the electrolyte composition through doping with specific ions and anions, a battery structure with high stability and high conductivity is formed, which suppresses lithium dendrite growth and improves interface compatibility.

Benefits of technology

It significantly improves the initial efficiency, rate performance, and cycle performance of solid-state batteries, with an initial efficiency of over 88.1%, a 5C/1C capacity retention of over 63.3%, and a capacity retention of over 94.9% after 100 cycles, thereby enhancing the energy density and safety performance of the batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005417580100000051
    Figure BDA0005417580100000051
  • Figure BDA0005417580100000052
    Figure BDA0005417580100000052
  • Figure BDA0005417580100000151
    Figure BDA0005417580100000151
Patent Text Reader

Abstract

The application discloses a kind of solid-state battery and preparation method thereof, the solid-state battery includes positive electrode, lithium negative electrode and the solid-state electrolyte layer being arranged between positive electrode and lithium negative electrode;Positive electrode includes cobalt-free positive electrode material and halide solid-state electrolyte, lithium negative electrode includes lithium-containing base layer and the three-dimensional network layer being arranged on the surface of the lithium-containing base layer, three-dimensional network layer includes polymer and lithium salt, F element is contained in lithium salt, and urea group, ether group and isocyanuric acid group are included in polymer;Halide solid-state electrolyte is in Li a Yb b I c On the basis of doping at least one cation M, also doped with anion A or another cation N.The solid-state battery of the application has good initial efficiency, rate performance and cycle performance, the initial efficiency is above 88.1%, the 5C / 1C capacity retention rate is above 63.3%, and the cycle 100 cycle capacity retention rate is above 94.9%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of solid-state battery technology, and specifically to a solid-state battery and its preparation method. Background Technology

[0002] As people's demands for the driving range and safety of new energy vehicles increase, solid-state batteries, which use lithium as the negative electrode and a solid electrolyte layer as the separator and lithium-ion transport medium, are gaining increasing favor among researchers. This is because using lithium as the negative electrode can better improve the energy density of the battery compared to conventional graphite negative electrodes, and the solid electrolyte layer, replacing the electrolyte in liquid batteries, can significantly improve battery safety. However, lithium negative electrodes are prone to lithium dendrite formation, which reduces battery performance. Moreover, interface problems in the solid electrolyte layer can greatly affect battery performance.

[0003] To address the aforementioned issues, relevant research has provided the following improvement scheme. CN 114709370 A discloses a solid-state battery with a gel-phase lithium metal anode, comprising a gel-phase lithium metal anode sheet, a positive electrode sheet, and a casing. First, lithium metal or a conductive salt is placed in a base solvent, then a polymerization solvent and a conductive polymer are added and stirred until homogeneous. The gel-phase lithium mixture is then coated onto a current collector, flattened, wrapped in a separator bag, and the top of the separator bag is welded to the current collector to obtain the gel-phase lithium metal anode sheet. The positive electrode sheet consists of a positive electrode active material, a conductive agent, a binder, a solid electrolyte, and a current collector. The manufactured positive electrode sheet and the gel-phase lithium metal anode are stacked in a predetermined quantity, secured with tape, and positive and negative electrode tabs are welded on. The casing is then attached, and the tabs are connected to the casing to produce the finished product. This battery uses lithium metal in a gel phase, which can improve the problems of high interfacial contact resistance between solid lithium metal and solid electrolyte, easy delamination and collapse during charging and discharging, and dendrite formation. It also solves the problem that liquid lithium metal anodes are difficult to manufacture into sheet-like electrodes.

[0004] CN 116914230A discloses a method for suppressing lithium dendrite growth in a solid-state lithium battery and its application. The positive electrode contains a uniform flow layer structure, which enhances the uniform transport of lithium ions in the solid electrolyte and negative electrode of the all-solid-state lithium battery upstream of the lithium ion flow, thereby achieving remote suppression of lithium dendrite growth in the negative electrode and / or solid electrolyte. This invention remotely suppresses lithium dendrite growth by using a positive electrode with a uniform flow layer structure, simultaneously solving the interface problem of the positive electrode and the mechanical failure problem of the solid electrolyte, achieving multiple benefits. It also improves the matching between the negative electrode and the high-load positive electrode and the ultra-thin electrolyte in the all-solid-state battery, improves the fast-charging safety of the battery, and significantly enhances the overall performance of the all-solid-state battery.

[0005] However, the above methods are complex to operate. Moreover, for solid-state batteries containing lithium anodes, improving the battery's initial efficiency, rate performance, and cycle performance while solving the lithium dendrite problem is a technical problem that urgently needs to be solved. Summary of the Invention

[0006] In view of the above-mentioned technical problems existing in the prior art, the purpose of the present invention is to provide a solid-state battery and a method for preparing the same.

[0007] To achieve the above objectives, the present invention adopts the following technical solution:

[0008] In a first aspect, the present invention provides a solid-state battery, the solid-state battery comprising a positive electrode, a lithium negative electrode, and a solid electrolyte layer disposed between the positive electrode and the lithium negative electrode;

[0009] The positive electrode includes a cobalt-free positive electrode material and a halide solid electrolyte. The lithium negative electrode includes a lithium-containing substrate and a three-dimensional network layer disposed on the surface of the lithium-containing substrate. The three-dimensional network layer includes a polymer and a lithium salt. The lithium salt contains an element F. The polymer includes urea groups, ether groups and isocyanuric acid groups.

[0010] The halide solid electrolyte in Li a Yb b I c Based on the above, it is doped with at least one cation M, and also doped with an anion A or another cation N, where a, b, and c satisfy Li a Yb b I c Valence equilibrium;

[0011] The cation M is doped at Li sites, doped at Yb sites, or neither doped at Li sites nor at Yb sites, and the ionic radius of cation M is R. M The ionic radius of I is R I The doping site of cation M and R M / R I If conditions ①, ②, or ③ are met:

[0012] ① Cation M is doped at the Li site, R M / R I Within the range of 0.255 to 0.414;

[0013] ②Cation M is doped at the Yb site, R M / R I Within the range of 0.255 to 0.732;

[0014] ③Cation M is not doped at either the Li or Yb sites, therefore R M / R I≥0.732;

[0015] The anion A is O 2- or N 3- ;

[0016] The ionic radius of the cation N is R. N The ionic radius of I is R I R N / R I It is ≥0.732.

[0017] In this invention, M and N are different types of elements.

[0018] Because Yb exists in two valence states, the material can easily change uncontrollably during actual production synthesis, affecting production yield. For example: Yb 3+ / I - When the ionic radius ratio is between 0.255 and 0.414, the coordination polyhedron of the I anion is tetrahedral, and the coordination number of the Yb ion is 4. 2+ / I - The ionic radius ratio is between 0.414 and 0.732. In this range, the I anion coordination polyhedron is octahedral, and the coordination number of the Li anion is 6. + / I - When the ionic radius ratio is between 0.255 and 0.414, the shape of the coordination polyhedron of the I negative ion is tetrahedral, and the coordination number of the positive ion is 4. Therefore, the structural stability of the material is uncontrolled due to production factors.

[0019] Furthermore, if there are more +2 valence Yb ​​in the material, it will increase the proportion of tetrahedral structure in the material. The coordination number of positive ions in this structure is only 4, the space utilization is low, the material structure cell is relatively simple, the number of lattice points is small, the material stability is poor, so the oxidation resistance, electrical conductivity and cycle stability are poor.

[0020] This invention optimizes the composition of iodine-containing halide solid electrolytes to ensure the presence of at least two unit cell lattices, thereby increasing the coordination number of positive ions, improving the structural stability of the material, and reducing the impact of Yb valence state changes on the structure during production. Specifically, O... 2- or N 3- Doping can improve the amorphism of materials to some extent, and introducing ion transport mechanisms based on disordered local structures can significantly improve the electrical conductivity of materials. For materials without O... 2- or N 3- In the case of doping, using cation N for doping and controlling the relationship between the ionic radius of cation N and the ionic radius of I can significantly increase the coordination number of the cathode ion to ≥8, promote the formation of a superconducting structure material, and also significantly improve the conductivity.

[0021] Furthermore, the combination of the aforementioned solid electrolyte with cobalt-free cathode material can fully leverage the low cost advantage of cobalt-free cathode material and effectively improve the structural stability, oxidation resistance, and conductivity of the cobalt-free cathode electrode, thereby enhancing the battery's initial efficiency, rate performance, and cycle performance.

[0022] Furthermore, the lithium anode in the solid-state battery of the present invention has a three-dimensional network layer, in which a polymer and a lithium salt are introduced. The polymer, comprising urea, ether, and isocyanuric acid groups, can react with Li... + A suitable coordination strength is formed between them, which on the one hand increases the coordination strength with Li + The adsorption energy facilitates the dissociation of lithium salts, thereby obtaining a high concentration of free Li. + This improves the polymer's electrical conductivity. Furthermore, the ether and urea polar groups create a weak coordination environment around Li+, promoting rapid lithium-ion transport within the polymer network. Additionally, the isocyanuric acid groups preferentially reduce and induce the formation of a stable, LiF- and Li3N-rich solid electrolyte interface (SEI) on the lithium anode, promoting dense and uniform lithium-ion stripping / deposition, improving interfacial compatibility, and suppressing lithium dendrite growth, thereby enhancing the battery's cycle stability and safety.

[0023] In this invention, the element types are screened by limiting the relationship between the ionic radius of the cation and the radius of the iodide ion. Compared with the prior art, which uses various elements to try one by one, this method greatly reduces the amount of DOE experimental data.

[0024] Preferably, the mass ratio of the cobalt-free cathode material to the halide solid electrolyte is (70-97.5):(2.5-30), wherein the cobalt-free cathode material is selected from the range of "70-97.5", for example, it can be 70, 75, 80, 85, 90, 95 or 97.5, etc.; the halide solid electrolyte is selected from the range of "2.5-30", for example, it can be 2.5, 5, 10, 15, 20, 25 or 30, etc.

[0025] Preferably, the cation M is selected from at least one of the following elements: IA, IIA, IIIB, IVB, VB, VIB, VIIB, VIII, IB, IIB, IIIA, IVA, VA, VIA, VIIA, lanthanides, and actinides.

[0026] Preferably, the cation N is selected from at least one of alkali metals, alkaline earth metals, actinides, transition metals, lanthanides, and main group metals.

[0027] Preferably, the configurational entropy of the molecular formula of the halide solid electrolyte is S1, and the Li a Yb b I cThe configurational entropy is S0, S1>S0;

[0028] When the halide solid electrolyte is in Li a Yb b I c When a solid halide electrolyte is doped with at least one cation M and also with an anion A, the configuration entropy of the molecular formula is calculated according to the following formula:

[0029]

[0030] Where Sconfig is the configuration entropy of the molecular formula; x a Y is the mole fraction of Li. b M represents the mole fraction of element Yb. d For the mole fraction of element M, I c For the mole fraction of element I, A e Let A be the mole fraction of A, and N be the number of types of element M.

[0031] When the halide solid electrolyte is in Li a Yb b I c When a solid halide electrolyte is doped with at least one cation M and another cation N, the configuration entropy of the molecular formula is calculated according to the following formula:

[0032]

[0033] Where Sconfig is the configuration entropy of the molecular formula; x a Y is the mole fraction of Li. b M represents the mole fraction of element Yb. d For the mole fraction of element M, I c The mole fraction of element I, N e Let N be the mole fraction of N, N1 be the number of types of element M, and N2 be the number of types of element N.

[0034] The higher the configuration entropy, the more stable the electrolyte structure, the higher the conductivity, and the better the ion mobility. This invention, through the above limitations, affects the compositional disorder and ion mobility of the solid electrolyte, significantly improving the ionic conductivity of the solid electrolyte and promoting the improvement of battery performance.

[0035] In existing technologies, the selection of element doping / substitution often relies on extensive DOE experiments for verification, resulting in low R&D efficiency. This invention, by defining the relationship between the ionic radii of the first and second elements and the ionic radius of F, as well as the relationship with the configuration entropy, can eliminate the need for numerous DOE experiments.

[0036] Preferably, the solid electrolyte layer comprises a sulfide solid electrolyte.

[0037] Preferably, the sulfide solid electrolyte contains oxygen, preferably Li. 6.4 P 0.8 Bi 0.2 S 4.7 O 0.3 Cl1.

[0038] Preferably, the lithium-containing base layer is a lithium layer and / or a lithium alloy layer.

[0039] Preferably, the lithium salt comprises at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium difluorophosphate, lithium difluorooxalate borate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluorosulfonyl)imide, lithium difluorooxalate borate, lithium tetrafluoro(oxalate) phosphate, lithium bis(fluorosulfonyl)imide, and lithium trifluoromethanesulfonate.

[0040] In a second aspect, the present invention provides a method for preparing a solid-state battery as described in the first aspect, the method comprising the following steps:

[0041] (1) Mix the cobalt-free cathode material and halide solid electrolyte evenly, press them to obtain the cathode layer;

[0042] (2) Press the sulfide solid electrolyte into a solid electrolyte layer;

[0043] (3) Preparation of lithium anode;

[0044] (4) The solid electrolyte layer is disposed between the positive electrode layer and the lithium negative electrode, and a current collector is disposed on the opposite side of the positive electrode layer and the solid electrolyte layer to assemble a solid battery.

[0045] The preparation of steps (1), (2) and (3) is not in any particular order.

[0046] Preferably, the preparation method of the halide solid electrolyte in step (1) includes the following steps:

[0047] The raw materials for the halide solid electrolyte are mixed in N-methylpyrrolidone, then subjected to high-energy ball milling to remove N-methylpyrrolidone, and finally heat-treated by electromagnetic heating to obtain the halide solid electrolyte.

[0048] Preferably, the method for removing N-methylpyrrolidone is vacuum evaporation.

[0049] Preferably, the rotational speed of the high-energy ball mill is 400 rpm to 600 rpm, for example, it can be 400 rpm, 425 rpm, 450 rpm, 470 rpm, 480 rpm, 500 rpm, 525 rpm, 550 rpm, 560 rpm, 580 rpm or 600 rpm, etc.

[0050] Preferably, the high-energy ball milling time is 10h to 18h, for example, it can be 10h, 11h, 12h, 13h, 14h, 15h, 16h, 17h or 18h.

[0051] Preferably, the power of the electromagnetic heating is 8kW to 15kW, for example, it can be 8kW, 8.5kW, 9kW, 9.5kW, 10kW, 10.5kW, 11kW, 11.5kW, 12kW, 12.5kW, 13kW, 13.5kW, 14kW, 14.5kW or 15kW, etc.

[0052] Preferably, the electromagnetic heating time is 6h to 12h, for example, it can be 6h, 6.5h, 7h, 7.5h, 8h, 8.5h, 9h, 9.5h, 10h, 10.5h, 11h, 11.5h or 12h.

[0053] Preferably, the pressing pressure in step (1) is 300MPa to 600MPa, for example, it can be 300MPa, 325MPa, 350MPa, 370MPa, 400MPa, 420MPa, 440MPa, 460MPa, 480MPa, 500MPa, 525MPa, 550MPa, 570MPa, 580MPa or 600MPa, etc.; the pressing time is 30s to 2min, for example, it can be 30s, 45s, 1min, 1.2min, 1.5min, 1.8min or 2min, etc.

[0054] Preferably, the pressing pressure in step (2) is 100MPa to 200MPa, for example, it can be 100MPa, 110MPa, 120MPa, 130MPa, 140MPa, 150MPa, 160MPa, 170MPa, 180MPa, 190MPa or 200MPa, etc.; the pressing time is 30s to 2min, for example, it can be 30s, 45s, 1min, 1.2min, 1.5min, 1.8min or 2min, etc.

[0055] Preferably, step (3) includes:

[0056] (a) A cyclic urea compound and a lithium salt are dispersed in a long-chain ether compound and a cyclic compound to obtain a mixed solution;

[0057] (b) An initiator is added to the mixed solution, and after being mixed evenly, it is coated on the surface of the lithium-containing substrate. After standing, a three-dimensional network layer is formed on the surface of the lithium-containing substrate to obtain a lithium anode.

[0058] Preferably, the cyclic urea compound in step (a) comprises at least one of triglycidyl isocyanurate (CAS: 2451-62-9), triglycidyl triisocyanate (CAS: 28825-96-9), (S,S,S)-triglycidyl isocyanurate (CAS: 240408-81-5), and (R,R,R)-triglycidyl isocyanurate (CAS: 240408-78-0).

[0059] Preferably, the lithium salt in step (a) includes at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium difluorophosphate, lithium difluorooxalate borate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluorosulfonyl)imide, lithium difluorooxalate borate, lithium tetrafluoro(oxalate) phosphate, lithium bis(fluorosulfonyl)imide, and lithium trifluoromethanesulfonate.

[0060] Preferably, the long-chain ether compound in step (a) includes at least one of diethylene glycol diethyl ether, ethylene glycol dimethyl ether, and methyl tert-butyl ether.

[0061] In this invention, the cyclic compound described in step (a) includes at least one of 1,3-dioxolane, tetrahydrofuran, ethylene oxide, dioxane, 1,3-dioxane, and 1,4-dioxane.

[0062] Preferably, based on a total mass of 100 wt% of the mixed solution described in step (a), the mass fraction of the cyclic urea compound is 1 wt% to 10 wt%, for example, it can be 1 wt%, 1.5 wt%, 2 wt%, 2.5 wt%, 3 wt%, 3.5 wt%, 4 wt%, 4.5 wt%, 5 wt%, 5.5 wt%, 6 wt%, 6.5 wt%, 7 wt%, 7.5 wt%, 8 wt%, 8.5 wt%, 9 wt%, 9.5 wt%, or 10 wt%.

[0063] Preferably, based on a total mass of 100 wt% of the mixed solution described in step (a), the mass fraction of the lithium salt is 5 wt% to 40 wt%, for example, it can be 5 wt%, 5.5 wt%, 6 wt%, 7 wt%, 7.5 wt%, 8 wt%, 9 wt%, 10 wt%, 11 wt%, 12 wt%, 13 wt%, 14 wt%, 15 wt%, 16 wt%, 18 wt%, 20 wt%, 22 wt%, 23 wt%, 24 wt%, 25 wt%, 26 wt%, 28 wt%, 29 wt%, 30 wt%, 32 wt%, 33 wt%, 35 wt%, 36 wt%, 38 wt%, or 40 wt%, etc.

[0064] Preferably, based on a total mass of 100 wt% of the mixed solution described in step (a), the mass fraction of the long-chain ether compound is 30 wt% to 70 wt%, for example, it can be 30 wt%, 32 wt%, 35 wt%, 36 wt%, 38 wt%, 40 wt%, 43 wt%, 46 wt%, 48 wt%, 50 wt%, 52 wt%, 55 wt%, 56 wt%, 58 wt%, or 60 wt%, etc.

[0065] Preferably, the initiator in step (b) comprises Mg(OTf)3.

[0066] Preferably, based on a total mass of 100 wt% of the mixed solution described in step (a), the amount of initiator added in step (b) is 0.05 wt% to 5 wt%, for example, it can be 0.05 wt%, 0.1 wt%, 0.15 wt%, 0.2 wt%, 0.3 wt%, 0.5 wt%, 0.7 wt%, 0.8 wt%, 1 wt%, 1.5 wt%, 2 wt%, 2.5 wt%, 3 wt%, 3.5 wt%, 4 wt%, 4.5 wt%, or 5 wt%, etc.

[0067] Preferably, the settling temperature in step (b) is 35°C to 55°C, for example, it can be 35°C, 37°C, 40°C, 42°C, 44°C, 45°C, 48°C, 50°C, 53°C or 55°C.

[0068] Preferably, the settling time in step (b) is 12h to 36h, for example, it can be 12h, 14h, 15h, 16h, 18h, 20h, 22h, 23h, 25h, 26h, 28h, 30h, 32h, 34h or 36h.

[0069] Compared with existing technologies, the present invention has the following beneficial effects:

[0070] (1) This invention can effectively improve the structural stability and oxidation resistance of the cobalt-free cathode by introducing a halide solid electrolyte into the cobalt-free cathode. Furthermore, by adjusting the lithium anode, the lithium dendrite problem can be suppressed and the ionic conductivity can be improved, thereby enhancing the energy density, cycle stability and safety performance of the lithium metal solid-state battery.

[0071] (2) The solid-state battery of the present invention has good first efficiency, rate performance and cycle performance, with a first efficiency of over 88.1%, a 5C / 1C capacity retention rate of over 63.3%, and a capacity retention rate of over 94.9% after 100 cycles. Detailed Implementation

[0072] The technical solution of the present invention will be further illustrated below through specific embodiments.

[0073] The halide solid electrolyte used in the embodiments of the present invention is in Li a Yb b I c Based on the above, it is doped with at least one cation M, and also doped with an anion A or another cation N, where a, b, and c satisfy Li a Yb b I c Valence equilibrium;

[0074] The cation M is doped at Li sites, doped at Yb sites, or neither doped at Li sites nor at Yb sites, and the ionic radius of cation M is R. M The ionic radius of I is R I The doping site of cation M and R M / R I If conditions ①, ②, or ③ are met:

[0075] ① Cation M is doped at the Li site, R M / R I Within the range of 0.255 to 0.414;

[0076] ②Cation M is doped at the Yb site, R M / R I Within the range of 0.255 to 0.732;

[0077] ③Cation M is not doped at either the Li or Yb sites, therefore R M / R I ≥0.732;

[0078] The anion A is O 2- or N 3- ;

[0079] The ionic radius of the cation N is R.N The ionic radius of I is R I R N / R I It is ≥0.732.

[0080] The parameters of the halide solid electrolytes in the various embodiments and comparative examples are shown in Table 1.

[0081] In this embodiment of the invention, the CAS numbers of some raw materials are as follows: HoN (CAS: 12029-81-1), I2Yb (CAS: 19357-86-9), and I3Li3 (CAS: 59216-97-6).

[0082] Example 1

[0083] This embodiment provides a solid-state battery, including a positive lithium anode and a solid electrolyte layer disposed between the positive electrode and the lithium anode;

[0084] The positive electrode comprises a cobalt-free positive electrode material and a halide solid electrolyte (wherein the mass ratio of the cobalt-free positive electrode material to the halide solid electrolyte is 95:5), and the lithium negative electrode comprises a lithium-containing substrate and a three-dimensional network layer disposed on the surface of the lithium-containing substrate. The three-dimensional network layer comprises a polymer and a lithium salt, wherein the lithium salt is lithium hexafluorophosphate, and the polymer comprises urea groups, ether groups, and isocyanuric acid groups.

[0085] The chemical formula of the halide solid electrolyte is Li 3.45 Yb 0.3 N 0.3 Ho 0.3 I 4.35 Among them, Hf replaces the Yb site, Ho 3+ radius R Ho and I - radius R I Satisfy the following relation: R Ho / R I =89.4 / 216=0.4138.

[0086] The configurational entropy of the aforementioned halide solid electrolyte is -9.58R; this halide solid electrolyte is doped with Ho 3+ and N 3- Previously, it was a basic electrolyte with the molecular formula Li. 3.45 Yb 0.6 I 4.35 The configurational entropy is -10.36R.

[0087] This embodiment also provides a method for preparing the above-mentioned solid-state battery, including the following steps:

[0088] I. Preparation of halide solid electrolytes:

[0089] (1) The raw materials HoN, I3Yb and I3Li3 were physically mixed in the formula ratio of 0.3:0.3:1.15, and 1wt% of N-methylpyrrolidone was added. The mixture was thoroughly stirred by high-energy ball milling, which can even break the bond energy of the raw materials. The high-energy ball milling speed was 450 rpm and the high-energy ball milling time was 15 h.

[0090] (2) The material after high-energy ball milling in step (1) is subjected to reduced pressure evaporation and drying to remove N-methylpyrrolidone. It is then subjected to heat treatment by electromagnetic heating. The power of electromagnetic heating is 10kW and the time of electromagnetic heating is 8h to obtain the halide solid electrolyte.

[0091] II. Preparation of the positive electrode layer:

[0092] The cobalt-free cathode material and the synthesized halide solid electrolyte were ground in a mortar at a mass ratio of 70:30 for 15 minutes to ensure uniform mixing, yielding 130 mg of the mixture. The mixture was then pressed under a pressure of 400 MPa for 1 minute to obtain the cathode layer.

[0093] III. Preparation of the solid electrolyte layer:

[0094] Weigh out 120mg Li 6.4 P 0.8 Bi 0.2 S 4.7 O 0.3 Cl1 forms an electrolyte membrane under pressure of 128 MPa for 2 minutes;

[0095] IV. Preparation of the negative electrode:

[0096] (a) Isocyanuric acid (R,R,R)-triglycidyl ester and lithium hexafluorophosphate were added to a mixture of 1,3-dioxolane and diethylene glycol diethyl ether, and dissolved and dispersed thoroughly to obtain a mixed solution; based on a total mass of 100 wt% of the mixed solution, the mass fractions of isocyanuric acid (R,R,R)-triglycidyl ester and lithium hexafluorophosphate were 6 wt% and 25 wt%, respectively; based on a total mass of 1,3-dioxolane and diethylene glycol diethyl ether of 100 wt%, the mass fraction of diethylene glycol diethyl ether was 50 wt%.

[0097] (b) Add initiator Mg(OTf)3 to the above mixed solution, the amount of initiator added is 0.85 wt% of the total mass of the above mixed solution, mix evenly and coat it on the lithium surface, let it stand at 40°C for 15 h to complete the polymerization and obtain lithium anode;

[0098] V. Battery Assembly: In a glove box filled with argon gas, carbon-coated aluminum foil, positive electrode layer, solid electrolyte layer, and negative electrode are assembled and sealed in sequence to obtain the battery.

[0099] Example 2

[0100] The difference from Example 1 is the type of halide solid electrolyte.

[0101] The chemical formula of the halide solid electrolyte in this embodiment is Li 3.1 Yb 0.2 Er 0.2 Cs 0.6 I 4.9 ; where Er replaces the Li site, Er 3+ radius R Er and I - radius R I Satisfy the following relation: R Er / R I =88.1 / 216=0.4079; Cs doping occurs at neither Li nor Yb sites. + radius R Cs and I - radius R I Satisfy the following relation: R Cs / R I =169 / 216=0.782;

[0102] The configurational entropy of the aforementioned halide solid electrolyte is -10.34R; this halide solid electrolyte, when doped with Er... 3+ and Cs + Previously, it was a basic electrolyte with the molecular formula Li. 3.3 Yb 0.2 I 4.9 The configurational entropy is -11.41R.

[0103] This embodiment also provides a method for preparing the above-mentioned solid-state battery, including the following steps:

[0104] (1) The raw materials ErI3, ICs, I3Yb and LiI were physically mixed in the formula amount of 0.2:0.6:0.2:3.1. 2wt% of N-methylpyrrolidone was added and the mixture was thoroughly stirred by high-energy ball milling, which can even play a role in breaking the bond energy of the raw materials. The high-energy ball milling speed was 550 rpm and the high-energy ball milling time was 12 h.

[0105] (2) The material after high-energy ball milling in step (1) is subjected to reduced pressure evaporation drying to remove N-methylpyrrolidone, and then subjected to heat treatment by electromagnetic heating. The power of electromagnetic heating is 11kW and the time of electromagnetic heating is 10h to obtain the halide solid electrolyte.

[0106] Example 3

[0107] The difference from Example 1 lies in the type of halide solid electrolyte. The chemical formula of the halide solid electrolyte in this example is Li. 2.0 Yb 0.2 O 0.3 Mg 0.8 I 3.6 ; where Mg substitutes for Li sites, Mg 2+ radius R Mg and I - radius R I Satisfy the following relation: R Mg / R I =65 / 216=0.3009.

[0108] The configurational entropy of the aforementioned halide solid electrolyte is -5.14R; this halide solid electrolyte is doped with Mg 2+ and O 2- Previously, it was a basic electrolyte with the molecular formula Li. 2.8 Yb 0.2 I 3.6 The configurational entropy is -7.17R.

[0109] This embodiment also provides a method for preparing the above-mentioned solid-state battery, including the following steps:

[0110] (1) The raw materials I2Mg, O3Yb2 and LiI were physically mixed in the formula ratio of 0.8:0.1:2.0, and 2wt% of N-methylpyrrolidone was added. The mixture was thoroughly stirred by high-energy ball milling, which can even break the bond energy of the raw materials. The high-energy ball milling speed was 550 rpm and the high-energy ball milling time was 12 h.

[0111] (2) The material after high-energy ball milling in step (1) is subjected to reduced pressure evaporation drying to remove N-methylpyrrolidone, and then subjected to heat treatment by electromagnetic heating. The power of electromagnetic heating is 11kW and the time of electromagnetic heating is 10h to obtain the halide solid electrolyte.

[0112] Example 4

[0113] This embodiment provides a solid-state battery, including a positive lithium anode and a solid electrolyte layer disposed between the positive electrode and the lithium anode;

[0114] The positive electrode comprises a cobalt-free positive electrode material and a halide solid electrolyte (wherein the mass ratio of the cobalt-free positive electrode material to the halide solid electrolyte is 80:20), and the lithium negative electrode comprises a lithium-containing substrate and a three-dimensional network layer disposed on the surface of the lithium-containing substrate. The three-dimensional network layer comprises a polymer and a lithium salt, wherein the lithium salt is lithium tetrafluoroborate, and the polymer comprises urea groups, ether groups, and isocyanuric acid groups.

[0115] The chemical formula of the halide solid electrolyte is Li 4.6 Yb 0.55 N 0.2 Sb 0.45 I7; where Sb replaces the Yb site, Sb 3+ radius R Sb and I - radius R I Satisfy the following relation: R Sb / R I =92 / 216=0.4259.

[0116] The configurational entropy of the aforementioned halide solid electrolyte is -19.63R; this halide solid electrolyte is doped with Sb 3+ and N 3- Previously, it was a basic electrolyte with the molecular formula Li. 4.6 Yb1I7 has a configurational entropy of -20.64R.

[0117] This embodiment also provides a method for preparing the above-mentioned solid-state battery, including the following steps:

[0118] I. Preparation of halide solid electrolytes:

[0119] (1) The raw materials Li3N, LiI, I3Yb and I3Sb were physically mixed according to the formula amount of 0.20:4.0:0.55:0.45. 3wt% of N-methylpyrrolidone was added and the mixture was thoroughly stirred by high-energy ball milling, which can even play a role in breaking the bond energy of the raw materials. The high-energy ball milling speed was 500 rpm and the high-energy ball milling time was 10 h.

[0120] (2) The material after high-energy ball milling in step (1) is subjected to reduced pressure evaporation drying to remove N-methylpyrrolidone, and then subjected to heat treatment by electromagnetic heating. The power of electromagnetic heating is 12kW and the time of electromagnetic heating is 10h to obtain the halide solid electrolyte.

[0121] II. Preparation of the positive electrode layer:

[0122] The cobalt-free cathode material and the synthesized halide solid electrolyte were ground in a mortar at a mass ratio of 80:20 for 10 minutes to ensure uniform mixing, yielding 130 mg of the mixture. The mixture was then pressed under a pressure of 500 MPa for 1 minute to obtain the cathode layer.

[0123] III. Preparation of the solid electrolyte layer:

[0124] Weigh out 120mg Li 6.4 P 0.8 Bi 0.2 S 4.7 O 0.3Cl1 forms an electrolyte membrane under pressure of 128 MPa for 2 minutes;

[0125] IV. Preparation of the negative electrode:

[0126] (a) Triglycidyl triisocyanate and lithium tetrafluoroborate were added to a mixture of 1,3-dioxolane and ethylene glycol dimethyl ether, and dissolved and dispersed thoroughly to obtain a mixed solution; based on the total mass of the mixed solution of 100 wt%, the mass fractions of triglycidyl triisocyanate and lithium tetrafluoroborate were 8 wt% and 10 wt%, respectively, and based on the total mass of 1,3-dioxolane and ethylene glycol dimethyl ether of 100 wt%, the mass fraction of ethylene glycol dimethyl ether was 32 wt%.

[0127] (b) Add initiator Mg(OTf)3 to the above mixed solution, the amount of initiator added is 2.5 wt% of the total mass of the above mixed solution, mix evenly and coat it on the lithium surface, let it stand at 50°C for 20 h to complete the polymerization and obtain lithium anode;

[0128] V. Battery Assembly: In a glove box filled with argon gas, carbon-coated aluminum foil, positive electrode, solid electrolyte layer, and negative electrode are assembled and sealed in sequence to obtain the battery.

[0129] Comparative Example 1

[0130] The difference from Example 1 is that step one was not performed, and in step two, during the preparation of the positive electrode layer, Li was used. 3.45 Yb 0.6 I 4.35 Replace the halide solid electrolyte in step two.

[0131] Comparative Example 2

[0132] The difference from Example 1 is that step one was not performed, and in step two, during the preparation of the positive electrode layer, Li was used. 3.45 Yb 0.3 Hf 0.3 I 4.35 Replace the halide solid electrolyte in step two.

[0133] Table 1

[0134]

[0135] (a) Ionic conductivity testing of halide solid electrolytes:

[0136] (1) Weigh 100mg of halide solid electrolyte powder and put it into the mold liner (diameter 10mm). Press it into an electrolyte sheet using a press (parameter: 400MPa). Match stainless steel blocking electrodes at both ends of the electrolyte sheet to assemble a blocking symmetric battery.

[0137] (2) The impedance value of the sample was measured by electrochemical AC impedance spectroscopy using an electrochemical workstation to obtain the resistance value R (unit: Ω) of the solid electrolyte. The test frequency was from 0.01 Hz to 1 MHz, the test disturbance voltage was 5 mV, and the test temperature was the temperature inside the glove box.

[0138] (3) Take out the electrolyte sheet and use a micrometer to measure the thickness L (in cm) of the solid electrolyte sheet;

[0139] (4) Then, the ionic conductivity of the solid electrolyte at the temperature inside the glove box is calculated using the formula.

[0140] The formula is: σLi + =L / (R*S);

[0141] In the formula σLi + —Ionic conductivity of solid electrolytes (S cm⁻¹) -1 );

[0142] L—Thickness of the solid electrolyte (cm);

[0143] R—Intrinsic resistance (Ω) of solid electrolyte;

[0144] S—Cross-sectional area of ​​solid electrolyte (cm²) 2 ).

[0145] (II) Air stability test of halide solid electrolytes:

[0146] (1) Turn on the dehumidifier and wait for the dew point environment to stabilize to below -45℃ for at least half an hour;

[0147] Electrolyte exposure: Lay the dried weighing paper flat on the test bench; take 0.5±0.03g of halide solid electrolyte and spread it flat on the weighing paper, spread it to a thickness of 1±0.3mm with a medicine spoon, let it stand for 4.5h and then collect the material.

[0148] (2) Weigh 120mg of halide solid electrolyte powder and put it into the mold liner (diameter 10mm). Press it into an electrolyte sheet using a press (parameter: 400MPa). Match stainless steel blocking electrodes at both ends of the electrolyte sheet.

[0149] (3) The resistance value R (unit Ω) of the solid electrolyte is obtained by using an electrochemical workstation to test the impedance value of the sample through electrochemical AC impedance. The test frequency is 0.01MHz to 1MHz, the test disturbance voltage is 5mV, and the test is carried out in a glove box.

[0150] (4) Take out the electrolyte sheet and use a micrometer to measure the thickness L (in cm) of the solid electrolyte; then calculate the ionic conductivity σ of the solid electrolyte at the temperature inside the glove box using the formula, σ=L / (R·S);

[0151] In the formula, σ is the ionic conductivity of the solid electrolyte (S cm⁻¹). -1 );

[0152] L – Thickness of the solid electrolyte (cm);

[0153] R—Intrinsic resistance (Ω) of solid electrolyte;

[0154] S — Cross-sectional area of ​​solid electrolyte (cm²) 2 ).

[0155] (5) Test the conductivity of the solid electrolyte before and after exposure according to the process of steps (3) to (6), and calculate the air stability of the solid electrolyte by formula: air stability = ionic conductivity after exposure / ionic conductivity before exposure × 100%.

[0156] (III) Antioxidant capacity test of halide solid electrolytes:

[0157] (1) Weigh out 100 mg of total material according to the mass ratio of SP: halide solid electrolyte = 20: 80, place it in a mortar and grind it by hand for 10 min, mix it evenly to obtain a mixture;

[0158] (2) Weigh 100mg of halide solid electrolyte powder and put it into the inner liner of the mold (diameter 10mm), and press it into electrolyte sheet using a press (parameter: 400MPa);

[0159] (3) Spread 25mg of the mixture from step (1) on one end of the electrolyte tablet, flatten it with a mold, and then press it firmly with a press (parameter: 400MPa); introduce a Li tablet into the other end;

[0160] (4) Using an electrochemical workstation, LSV testing was performed with an open-circuit voltage of ~6V and a scan rate of 0.1mV / S to obtain the oxidation window (unit: V).

[0161] Battery electrical performance testing:

[0162] (1) Test method for first-time efficiency: At 35±3℃, charge the battery with a constant current of 0.1C to 4.25V, and charge it with a constant voltage of 4.25V to the cutoff current of 0.05C. Record the charging capacity as C1; then discharge the battery with a constant current of 0.1C to 3.0V and record the discharge capacity as D1; ​​calculate the first-time efficiency based on the discharge capacity and charging capacity. First-time efficiency = (D1 / C1)×100%.

[0163] (2) Test method for capacity retention: At 35±3℃, charge the battery at a constant current of 1C to 4.25V, charge at a constant voltage of 4.25V to the cutoff current of 0.05C, and discharge the battery at a constant current of 1C to 3.0V. The discharge capacity of the first 1C cycle is recorded as D1. Repeat the charge and discharge cycle 100 times, and the discharge capacity of the 100th cycle is recorded as D. 100 The capacity retention rate for the 100th cycle is calculated based on the discharge capacity of the first cycle and the discharge capacity of the 100th cycle. The capacity retention rate for the 100th cycle = (D...) 100 / D1)×100%.

[0164] (3) Rate performance test method: At 35±3℃, charge the battery with a constant current of 1C to 4.25V, charge it with a constant voltage of 4.25V to the cutoff current of 0.05C, and discharge the battery with a constant current of 1C to 3.0V. The 1C discharge capacity is recorded as D1. After five cycles, the average value M is calculated from the 1C discharge capacity. Charge the battery with a constant current of 1C to 4.25V, charge it with a constant voltage of 4.25V to the cutoff current of 0.05C, and discharge the battery with a constant current of 5C to 3.0V. The 5C discharge capacity is recorded as D2. After five cycles, the average value N is calculated from the 5C discharge capacity. 5C / 1C capacity retention rate = N / M×100%.

[0165] Table 2

[0166]

[0167] In summary, this invention, by introducing a halide solid electrolyte into the cobalt-free cathode, can effectively improve the structural stability, oxidation resistance, and conductivity of the cobalt-free cathode electrode. Furthermore, by adjusting the lithium anode, lithium dendrite formation can be suppressed, and ionic conductivity can be improved, thereby enhancing the energy density, cycle stability, and safety performance of the lithium metal solid-state battery. The solid-state battery of this invention exhibits excellent initial efficiency, rate performance, and cycle performance, with an initial efficiency exceeding 88.1%, a 5C / 1C capacity retention exceeding 63.3%, and a capacity retention exceeding 94.9% after 100 cycles.

[0168] A comparison of Example 1 and Comparative Example 1 shows that without the use of any element doping / substitution, the electrolyte conductivity, air stability, and oxidation voltage window are all low, indicating that the halide solid electrolyte prepared by this patent can improve the final electrical performance of the battery.

[0169] The comparison between Example 1 and Comparative Example 2 shows that the doped elements do not meet the requirements and cannot significantly improve the structural stability and conductivity of the material, thus failing to achieve the goal of significantly improving the performance of the battery.

[0170] The applicant declares that the detailed method of the present invention is illustrated by the above embodiments, but the present invention is not limited to the above detailed method, that is, it does not mean that the present invention must rely on the above detailed method to be implemented. Those skilled in the art should understand that any improvements to the present invention, equivalent substitutions of the raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A solid-state battery, characterized in that, The solid-state battery includes a positive electrode, a lithium negative electrode, and a solid electrolyte layer disposed between the positive electrode and the lithium negative electrode; The positive electrode includes a cobalt-free positive electrode material and a halide solid electrolyte. The lithium negative electrode includes a lithium-containing substrate and a three-dimensional network layer disposed on the surface of the lithium-containing substrate. The three-dimensional network layer includes a polymer and a lithium salt. The lithium salt contains an element F. The polymer includes urea groups, ether groups and isocyanuric acid groups. The halide solid electrolyte in Li a Yb b I c Based on the above, it is doped with at least one cation M, and also doped with an anion A or another cation N, where a, b, and c satisfy Li a Yb b I c Valence equilibrium; The cation M is doped at Li sites, doped at Yb sites, or neither doped at Li sites nor at Yb sites, and the ionic radius of cation M is R. M The ionic radius of I is R I The doping site of cation M and R M / R I If conditions ①, ②, or ③ are met: ① Cation M is doped at the Li site, R M / R I Within the range of 0.255 to 0.414; ②Cation M is doped at the Yb site, R M / R I Within the range of 0.255 to 0.732; ③Cation M is not doped at either the Li or Yb sites, therefore R M / R I ≥0.732; The anion A is O 2- or N 3- ; The ionic radius of the cation N is R. N The ionic radius of I is R I R N / R I It is ≥0.

732.

2. The solid-state battery according to claim 1, characterized in that, The mass ratio of the cobalt-free cathode material to the halide solid electrolyte is (70–97.5):(2.5–30); The cation M is selected from at least one of the following elements: IA, IIA, IIIB, IVB, VB, VIB, VIIB, VIII, IB, IIB, IIIA, IVA, VA, VIA, VIIA, lanthanides, and actinides. The cation N is selected from at least one of alkali metals, alkaline earth metals, actinides, transition metals, lanthanides, and main group metals.

3. The solid-state battery according to claim 1, characterized in that, The configurational entropy of the molecular formula of the halide solid electrolyte is S1, and the Li a Yb b I c The configurational entropy is S0, S1>S0; When the halide solid electrolyte is in Li a Yb b I c When a solid halide electrolyte is doped with at least one cation M and also with an anion A, the configuration entropy of the molecular formula is calculated according to the following formula. Perform calculations: (I) c Inl c ) I-site +(A e InA e ) A-site ]; Where Sconfig is the configuration entropy of the molecular formula; x a Y is the mole fraction of Li. b M represents the mole fraction of element Yb. d For the mole fraction of element M, I c For the mole fraction of element I, A e Let A be the mole fraction of A, and N be the number of types of element M. When the halide solid electrolyte is in Li a Yb b I c When a solid halide electrolyte is doped with at least one cation M and another cation N, the configuration entropy of the molecular formula is calculated according to the following formula: Where Sconfig is the configuration entropy of the molecular formula; x a Y is the mole fraction of Li. b M represents the mole fraction of element Yb. d For the mole fraction of element M, I c The mole fraction of element I, N e Let N be the mole fraction of N, N1 be the number of types of element M, and N2 be the number of types of element N.

4. The solid-state battery according to claim 1, characterized in that, The solid electrolyte layer includes a sulfide solid electrolyte; The sulfide solid electrolyte contains oxygen, preferably Li. 6.4 P 0.8 Bi 0.2 S 4.7 O 0.3 Cl1.

5. The solid-state battery according to claim 1, characterized in that, The lithium-containing base layer is a lithium layer and / or a lithium alloy layer; The lithium salt includes at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium difluorophosphate, lithium difluorooxalate borate, lithium difluorosulfonyl imide, lithium bis(trifluorosulfonyl imide), lithium difluorooxalate borate, lithium tetrafluoro(oxalate) phosphate, lithium difluorosulfonyl imide, and lithium trifluoromethanesulfonate.

6. A method for preparing a solid-state battery as described in any one of claims 1-5, characterized in that, The preparation method includes the following steps: (1) Mix the cobalt-free cathode material and halide solid electrolyte evenly, press them to obtain the cathode layer; (2) Press the sulfide solid electrolyte into a solid electrolyte layer; (3) Preparation of lithium anode; (4) The solid electrolyte layer is disposed between the positive electrode layer and the lithium negative electrode, and a current collector is disposed on the opposite side of the positive electrode layer and the solid electrolyte layer to assemble a solid battery. The preparation of steps (1), (2) and (3) is not in any particular order.

7. The preparation method according to claim 6, characterized in that, The preparation method of the halide solid electrolyte in step (1) includes the following steps: The raw materials for the halide solid electrolyte are mixed in N-methylpyrrolidone, then subjected to high-energy ball milling to remove N-methylpyrrolidone, and finally heat-treated by electromagnetic heating to obtain the halide solid electrolyte.

8. The preparation method according to claim 7, characterized in that, The method for removing N-methylpyrrolidone is vacuum evaporation; The high-energy ball mill rotates at a speed of 400 rpm to 600 rpm. The high-energy ball milling time is 10h to 18h; The power of the electromagnetic heating is 8kW to 15kW; The electromagnetic heating time is 6h to 12h.

9. The preparation method according to claim 6, characterized in that, The pressing pressure in step (1) is 300MPa to 600MPa, and the pressing time is 30s to 2min; The pressing pressure in step (2) is 100MPa to 200MPa, and the pressing time is 30s to 2min.

10. The preparation method according to claim 6, characterized in that, Step (3) includes: (a) A cyclic urea compound and a lithium salt are dispersed in a long-chain ether compound and a cyclic compound to obtain a mixed solution; (b) An initiator is added to the mixed solution, and after being mixed evenly, it is coated on the surface of the lithium-containing substrate. After standing, a three-dimensional network layer is formed on the surface of the lithium-containing substrate to obtain a lithium anode. The cyclic urea compound in step (a) includes at least one of triglycidyl isocyanurate, triglycidyl trimisocyanate, (S,S,S)-triglycidyl isocyanurate and (R,R,R)-triglycidyl isocyanurate. The lithium salt in step (a) includes at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium difluorophosphate, lithium difluorooxalate borate, lithium difluorosulfonyl imide, lithium bis(trifluorosulfonyl imide), lithium difluorooxalate borate, lithium tetrafluoro(oxalate) phosphate, lithium difluorosulfonyl imide, and lithium trifluoromethanesulfonate. The long-chain ether compound in step (a) includes at least one of diethylene glycol diethyl ether, ethylene glycol dimethyl ether, pentyl ether, methyl ether, butyl ether, ethylene glycol ethyl ether, ethylene glycol methyl ether, ethylene glycol butyl ether, ethylene glycol hexyl ether, ethylene glycol dibutyl ether, ethylene glycol methyl ethyl ether, tetraethylene glycol dimethyl ether, and methyl tert-butyl ether; The cyclic compound in step (a) includes at least one of 1,3-dioxolane, tetrahydrofuran, ethylene oxide, dioxane, 1,3-dioxane, and 1,4-dioxane; Based on a total mass of 100 wt% for the mixed solution described in step (a), the mass fraction of the cyclic urea compounds is 1 wt% to 10 wt%. Based on a total mass of 100 wt% of the mixed solution described in step (a), the mass fraction of the lithium salt is 5 wt% to 40 wt%. Based on a total mass of 100 wt% of the long-chain ether compounds and cyclic compounds described in step (a), the mass fraction of the long-chain ether compounds is 30 wt% to 70 wt%. The initiator in step (b) includes Mg(OTf)3; Based on a total mass of 100 wt% for the mixed solution described in step (a), the amount of initiator added in step (b) is 0.05 wt% to 5 wt%. The settling temperature in step (b) is 35℃~55℃; The settling time in step (b) is 12h to 36h.