A battery cell, a method of manufacturing the same, a secondary battery, and an electric device

By using graphite with an aspect ratio ≥2 in lithium-ion batteries and subjecting it to magnetic field-induced treatment, graphite grains are vertically arranged on the surface of the negative electrode current collector, forming ordered 'ion channels'. This solves the problem of insufficient fast-charging performance of lithium-ion batteries and achieves faster charging speed and higher energy density.

CN123162267APending Publication Date: 2026-11-24CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510663431.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-22
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

The fast-charging performance of existing lithium-ion batteries has reached a bottleneck, and how to further improve the fast-charging performance of individual battery cells has become an urgent problem to be solved.

Method used

Graphite with an aspect ratio ≥ 2 is used as the negative electrode active material. Magnetic field induction treatment is used to arrange graphite grains on the surface of the negative electrode current collector, so that most of its basal planes tend to be perpendicular or nearly perpendicular to the current collector, forming an ordered 'ion channel', reducing the detour path of lithium ions, and achieving straight vertical transport.

Benefits of technology

It significantly shortens the transmission distance of lithium ions from the electrolyte to the negative electrode current collector, improves the fast charging performance of the battery cell, and takes into account the energy density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123162267A_ABST
    Figure CN123162267A_ABST
Patent Text Reader

Abstract

This application provides a battery cell and its preparation method, a secondary battery, and an electrical device, belonging to the field of lithium battery technology. The battery cell includes a negative electrode sheet, which includes a negative current collector and a negative electrode film layer disposed on at least one surface of the negative current collector. The negative electrode film layer includes a negative electrode active material, which includes graphite. The graphite has an aspect ratio ≥ 2, and the C004 / C110 ratio of the negative electrode sheet under X-ray diffraction is ≤ 3. This application selects graphite with an aspect ratio ≥ 2 as the negative electrode active material and limits the C004 / C110 ratio of the negative electrode sheet to ≤ 3 under X-ray diffraction, i.e., controls the basal planes of the graphite grains in the negative electrode sheet to be mostly perpendicular to the negative current collector. This not only shortens the straight-line distance of lithium ions from the electrolyte to the negative current collector, achieving straight-line vertical transport, but also reduces the detour paths between particles, significantly shortening the effective transport distance, thereby improving the fast-charging performance of the battery cell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of lithium battery technology, and in particular to a battery cell and its preparation method, a secondary battery and an electrical device. Background Technology

[0002] In recent years, with the increasingly widespread application of lithium-ion batteries, they have been widely used in energy storage systems such as hydropower, thermal power, wind power, and solar power plants, as well as in power tools, electric bicycles, electric motorcycles, electric cars, military equipment, aerospace, and many other fields. Due to the significant advancements in lithium-ion battery technology, higher demands have been placed on fast-charging performance.

[0003] Secondary graphite particles are agglomerated from primary graphite particles of the nanometer or micrometer size. Their smaller particle size significantly shortens the diffusion path of lithium ions inside graphite (from the micrometer to the nanometer scale), reducing diffusion resistance. In addition, the granulation process of secondary graphite particles partially disrupts the orientation of graphite crystals, reducing the layered anisotropy of natural graphite (such as the problem of slow diffusion along the c-axis). The diffusion rate of lithium ions in multiple directions is more balanced, thus exhibiting better fast-charging performance.

[0004] However, the improvement of fast charging performance by secondary graphite particles has reached a bottleneck, and how to improve the fast charging performance of individual battery cells has become an urgent problem to be solved. Summary of the Invention

[0005] This application is made in view of the above-mentioned issues, and its purpose is to provide a battery cell and its preparation method, a secondary battery and an electrical device, which have good fast charging performance.

[0006] To achieve the above objectives, a first aspect of this application provides a battery cell comprising a negative electrode sheet, the negative electrode sheet comprising a negative current collector and a negative electrode film layer disposed on at least one surface of the negative current collector, the negative electrode film layer comprising a negative electrode active material, the negative electrode active material comprising graphite, the aspect ratio of graphite being ≥2, and the C004 / C110 ratio of the negative electrode sheet being ≤3 under X-ray diffraction.

[0007] Therefore, this application selects graphite with an aspect ratio ≥ 2 as the negative electrode active material and limits the C004 / C110 ratio of the negative electrode sheet to ≤ 3 under X-ray diffraction. That is, it controls the basal plane of most of the graphite grains in the negative electrode sheet to be perpendicular or nearly perpendicular to the negative electrode current collector. On the one hand, during ion insertion and extraction, there is no need to diffuse laterally along the C-axis of the graphite, but to move directly along the direction perpendicular or nearly perpendicular to the negative electrode current collector. This shortens the straight distance of lithium ions from the electrolyte to the negative electrode current collector and realizes straight vertical transport. On the other hand, the graphite grains arranged perpendicular to the negative electrode current collector form an ordered "ion channel", which reduces the detour path between particles and significantly shortens the effective transport distance, thereby improving the fast charging performance of the battery cell.

[0008] In any embodiment, when the graphite powder is in a disordered state, the C004 / C110 ratio under X-ray diffraction is ≥5. This application demonstrates that graphite exhibits strong anisotropy by ensuring that the C004 / C110 ratio of the disordered graphite powder is within the aforementioned range under X-ray diffraction. This results in more basal planes tending to be perpendicular or nearly perpendicular to the current collector arrangement during magnetic field-induced processing, thereby shortening the lithium-ion transport distance and thus significantly improving the fast-charging performance of the battery cell.

[0009] In any embodiment, the graphite is natural graphite. Natural graphite has significant anisotropy and meets the aspect ratio requirement. When the negative electrode sheet satisfies the C004 / C110 ratio ≤ 3 under X-ray diffraction, the battery cell made of natural graphite as the negative electrode active material exhibits better fast charging performance than secondary graphite particles.

[0010] In any embodiment, the graphitization degree of natural graphite is ≥95%. By keeping the graphitization degree of natural graphite within the above range, natural graphite with a high graphitization degree has a higher energy density, thereby enabling the battery cell to balance fast charging performance and energy density.

[0011] The second aspect of this application provides a method for preparing a battery cell, which includes placing a negative electrode precursor in a magnetic field environment for magnetic field induction treatment. The negative electrode precursor includes a negative electrode current collector and a negative electrode slurry coated on at least one surface of the negative electrode current collector. The negative electrode slurry includes a negative electrode active material, which includes graphite. The aspect ratio of the graphite is ≥2. In the magnetic field induction treatment, the angle between the direction of the magnetic field and the negative electrode current collector is 60° to 120°, the magnetic field strength is ≥3000 Gs, the treatment time is ≥2s, and the slurry viscosity is 3000 mPa·s to 15000 mPa·s. After the magnetic field induction treatment is completed, drying and cold pressing are performed.

[0012] Therefore, the battery cell preparation method of this application, by placing the negative electrode precursor in a magnetic field environment for magnetic field induction treatment, and setting the angle between the magnetic field direction and the negative electrode current collector in the magnetic field induction treatment to 60° to 120°, can induce unshaped graphite grains with an aspect ratio ≥2 to be arranged on the surface of the negative electrode current collector. This makes the basal plane of most of the graphite grains in the negative electrode precursor tend to be perpendicular or nearly perpendicular to the negative electrode current collector. On the one hand, during ion insertion and extraction, there is no need to diffuse laterally along the C-axis direction of graphite, but to move directly along the direction perpendicular or nearly perpendicular to the negative electrode current collector, thereby shortening the straight distance of lithium ions from the electrolyte to the negative electrode current collector and realizing straight vertical transport. On the other hand, the graphite grains arranged perpendicular to the negative electrode current collector form an ordered "ion channel", reducing the detour path between particles and significantly shortening the effective transport distance, thereby improving the fast charging performance of the battery cell.

[0013] In any embodiment, the slurry viscosity is 3000 mPa·s to 9000 mPa·s, and the magnetic field-induced treatment time is ≥2 s. When the slurry viscosity is within the above range, by making the magnetic field-induced treatment time ≥2 s, the orientation of most graphite grains tends to be perpendicular or nearly perpendicular to the negative electrode current collector.

[0014] In any embodiment, the slurry viscosity is greater than 9000 mPa·s and less than or equal to 15000 mPa·s, and the magnetic field-induced treatment time is ≥5 s. When the slurry viscosity is within the above range, by making the magnetic field-induced treatment time ≥5 s, the orientation of most graphite grains tends to be perpendicular or nearly perpendicular to the negative electrode current collector.

[0015] In any embodiment, the magnetic field is an alternating magnetic field. An alternating magnetic field can provide a magnetic field environment with higher magnetic field strength, thereby causing the orientation of graphite grains to be mostly perpendicular or nearly perpendicular to the negative electrode current collector through magnetic field induction treatment.

[0016] A third aspect of this application provides a secondary battery comprising the battery cell described in the above embodiments or a battery cell prepared according to the preparation method of the battery cell described in the above embodiments.

[0017] The fourth aspect of this application provides an electrical device that includes the secondary battery described in the above embodiments, the secondary battery being used to provide electrical energy. Attached Figure Description

[0018] Figure 1 This is a schematic diagram of a battery cell according to one embodiment of this application.

[0019] Figure 2 yes Figure 1 An exploded view of a battery cell according to one embodiment of this application is shown.

[0020] Figure 3 This is a schematic diagram of a battery module according to one embodiment of this application.

[0021] Figure 4 This is a schematic diagram of a battery pack according to one embodiment of this application.

[0022] Figure 5 yes Figure 4 An exploded view of a battery pack according to one embodiment of this application is shown.

[0023] Figure 6 This is a schematic diagram of an electrical device in which a single battery cell is used as a power source according to one embodiment of this application.

[0024] Explanation of reference numerals in the attached figures:

[0025] 1 Battery pack; 2 Upper housing; 3 Lower housing; 4 Battery module; 5 Battery cell; 51 Housing; 52 Electrode assembly; 53 Cover plate. Detailed Implementation

[0026] The following detailed description, with appropriate reference to the accompanying drawings, discloses a battery cell, its preparation method, a secondary battery, and an electrical device according to this application. However, unnecessary details may be omitted. For example, detailed descriptions of well-known facts and repetitive descriptions of practically identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided for the purpose of enabling those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.

[0027] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values ​​of 1 and 2 are listed, and if maximum range values ​​of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0028] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.

[0029] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.

[0030] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.

[0031] Single-particle natural graphite has a relatively large particle size and high specific surface area, and its sheet-like or fibrous structure makes it easy to prepare, offering advantages such as low cost and high theoretical capacity. However, sheet-like or fibrous graphite exhibits poor lithium-ion diffusion kinetics, which limits its fast-charging performance.

[0032] To improve the fast-charging performance of sheet-like or fibrous graphite, such as single-particle natural graphite, strategies such as surface modification, spheroidization, compositing with highly conductive materials, and constructing a three-dimensional conductive network followed by doping with other elements are often employed to optimize this type of sheet-like graphite. However, the improvement effect is not significant, and the process cost is relatively high.

[0033] Based on this, this application proposes a battery cell and its preparation method, a secondary battery and an electrical device. The following provides a more detailed description of this application and its optional embodiments.

[0034] This application provides a battery cell comprising a negative electrode sheet, the negative electrode sheet comprising a negative current collector and a negative electrode film layer disposed on at least one surface of the negative current collector, the negative electrode film layer comprising a negative electrode active material, the negative electrode active material comprising graphite, the aspect ratio of graphite being ≥2, and the C004 / C110 ratio of the negative electrode sheet being ≤3 under X-ray diffraction.

[0035] Graphite with an aspect ratio ≥ 2 is generally flake graphite or fibrous graphite. For flake graphite, the aspect ratio is the ratio of the diameter or length of the flake graphite in the plane direction to the dimension in the thickness direction; for fibrous graphite, the aspect ratio is the ratio of the fiber length to the fiber diameter.

[0036] The aspect ratio of graphite can be measured by observing its morphology using a scanning electron microscope (SEM) or a transmission electron microscope (TEM) and statistically calculating the aspect ratio distribution.

[0037] As an example, the aspect ratio of graphite can be 2, 2.5, 3, 3.5, 4, 4.5, 5, or 5.5.

[0038] Optionally, the aspect ratio of graphite is ≥3.

[0039] Optionally, the aspect ratio of graphite is ≥4.

[0040] Optionally, the aspect ratio of graphite is ≥5.

[0041] The ratio of C004 / C110 under X-ray diffraction is the OI value of the negative electrode. The OI value of the negative electrode can be obtained by an X-ray diffractometer. According to the general rules of X-ray diffraction analysis and the methods for determining the lattice parameters of graphite JIS K0131-1996 and JB / T4220-2011, the X-ray diffraction pattern of the negative electrode is obtained, and the OI value of the negative electrode is calculated according to the formula OI=C004 / C110, where C004 is the peak area of ​​the 004 characteristic diffraction peak of the negative electrode and C110 is the peak area of ​​the 110 characteristic diffraction peak of the negative electrode.

[0042] As an example, the C004 / C110 ratio of the negative electrode sheet under X-ray diffraction can be 3, 2.5, 2, 1.8, 1.5, 1.2 or 1.

[0043] Optionally, the ratio of C004 / C110 of the negative electrode sheet under X-ray diffraction is ≤2.5.

[0044] Optionally, the ratio of C004 / C110 of the negative electrode sheet under X-ray diffraction is ≤2.

[0045] Optionally, the ratio of C004 / C110 of the negative electrode sheet under X-ray diffraction is ≤1.8.

[0046] Graphite with an aspect ratio ≥ 2 is usually in the form of flakes or fibers. In the negative electrode, the flakes or fibers of graphite are usually randomly arranged, which causes lithium ions to be transported laterally between graphite particles. This results in a longer lithium ion diffusion path. During fast charging, a large number of lithium ions need to migrate in a short time, which hinders the diffusion kinetics and leads to increased polarization. Therefore, graphite with an aspect ratio ≥ 2 exhibits worse fast charging performance than secondary graphite particles. This application selects graphite with an aspect ratio ≥ 2 as the negative electrode active material and limits the C004 / C110 ratio of the negative electrode sheet to ≤ 3 under X-ray diffraction. That is, it controls the basal plane (parallel to the graphite layer direction) of the graphite grains in the negative electrode sheet to be mostly perpendicular or nearly perpendicular to the negative electrode current collector. On the one hand, during ion insertion and extraction, there is no need to diffuse laterally along the C-axis direction of graphite (perpendicular to the graphite layer direction), but to move directly along the direction perpendicular or nearly perpendicular to the negative electrode current collector. This shortens the straight distance of lithium ions from the electrolyte to the negative electrode current collector and realizes straight vertical transport. On the other hand, the graphite grains arranged perpendicular to the negative electrode current collector form an ordered "ion channel", reducing the detour path between particles and significantly shortening the effective transport distance, thereby improving the fast charging performance of the battery cell.

[0047] In some embodiments, when the graphite powder is in a disordered state, the C004 / C110 ratio is ≥5 under X-ray diffraction.

[0048] The ratio of C004 / C110 under X-ray diffraction is the OI value of graphite powder. At this time, the graphite powder is in a disordered state. The OI value of graphite powder can be obtained by X-ray diffractometer. According to the general rules of X-ray diffraction analysis and the methods for determining the lattice parameters of graphite JIS K 0131-1996 and JB / T4220-2011, the X-ray diffraction pattern of graphite powder is obtained, and the OI value of graphite powder is calculated according to the formula OI=C004 / C110, where C004 is the peak area of ​​the characteristic diffraction peak of 004 ​​of graphite powder, and C110 is the peak area of ​​the characteristic diffraction peak of 110 of graphite powder.

[0049] As an example, the C004 / C110 ratio of graphite powder under X-ray diffraction can be 5, 5.5, 6, 6.5, 7, 7.5 or 8.

[0050] This application demonstrates that graphite has strong anisotropy by ensuring that the C004 / C110 ratio of disordered graphite powder under X-ray diffraction falls within the aforementioned range. This results in more basal planes tending to be perpendicular or nearly perpendicular to the current collector arrangement during magnetic field-induced processing, thereby shortening the lithium-ion transport distance and making the improvement in the fast-charging performance of the battery cell more significant.

[0051] In some implementations, the graphite is natural graphite.

[0052] Natural graphite is a layered crystalline mineral composed of carbon elements, formed in high-temperature and high-pressure geological environments. It boasts advantages such as low cost and relatively high theoretical capacity. However, due to issues with fast charging, natural graphite has not been widely used as a negative electrode active material in secondary batteries.

[0053] This application discovers that natural graphite has significant anisotropy and meets the aspect ratio requirement. When the negative electrode sheet satisfies the C004 / C110 ratio ≤3 under X-ray diffraction, that is, by changing the arrangement of natural graphite particles in the negative electrode sheet, the battery cell made of natural graphite as the negative electrode active material exhibits better fast charging performance than secondary graphite particles.

[0054] In some implementations, the graphitization degree of natural graphite is ≥95%.

[0055] The degree of graphitization indicates the amount of sp in carbon materials. 2 The degree to which hybrid carbon atoms are arranged into an ordered graphite layer structure.

[0056] The degree of graphitization of natural graphite can be obtained using an X-ray powder diffractometer (X'pert PRO). According to the general rules of X-ray diffraction analysis and the methods for determining the lattice parameters of graphite JIS K0131-1996 and JB / T4220-2011, the interlayer spacing d002 of natural graphite is obtained, and then the degree of graphitization of the natural graphite is calculated according to the formula G=(0.344-d002) / (0.344-0.3354).

[0057] As an example, the degree of graphitization of natural graphite can be 95%, 95.5%, 96%, 96.5%, 97%, 97.5%, 98%, 98.5%, 99%, or 99.5%.

[0058] By ensuring that the graphitization degree of natural graphite is within the aforementioned range, natural graphite with a high graphitization degree has a higher energy density, thereby enabling battery cells to balance fast charging performance and energy density.

[0059] Optionally, the specific surface area of ​​natural graphite is ≥1.5m². 2 / g.

[0060] The specific surface area of ​​natural graphite can be measured by the following methods:

[0061] At constant low temperature, the amount of gas adsorbed on the solid surface at different relative pressures was measured. Based on the Brown-Etter-Taylor (BET) multilayer adsorption theory and its formula, the amount of monolayer adsorption of the sample was obtained, and the specific surface area of ​​the solid was calculated.

[0062] This application also provides a method for preparing a battery cell, which includes placing a negative electrode precursor in a magnetic field environment for magnetic field induction treatment. The negative electrode precursor includes a negative current collector and a negative electrode slurry coated on at least one surface of the negative current collector. The negative electrode slurry includes a negative electrode active material, which includes graphite. The aspect ratio of the graphite is ≥2. In the magnetic field induction treatment, the angle between the direction of the magnetic field and the negative current collector is 60° to 120°, the magnetic field strength is ≥3000 Gs, the treatment time is ≥2s, and the slurry viscosity is 3000 mPa·s to 15000 mPa·s. After the magnetic field induction treatment is completed, drying and cold pressing are performed.

[0063] Magnetic field-induced treatment is an advanced technology that modulates the microstructure and properties of materials by applying an external magnetic field. Its core lies in utilizing the interaction between the magnetic field and matter (such as magnetization force and Lorentz force) to directionally guide the arrangement of atoms, molecules, or particles, thereby optimizing the physical, chemical, or functional properties of the material. Since graphite is a diamagnetic material, placing the negative electrode precursor in a magnetic field environment for magnetic field-induced treatment causes a change in the atomic orbital angular momentum under the influence of the external magnetic field. This results in the graphite acquiring a magnetic moment opposite to the direction of the external magnetic field, i.e., a magnetic moment perpendicular to the negative electrode current collector. Consequently, the La plane of the graphite gradually shifts uniformly, causing the orientation of most graphite grains to tend to be perpendicular to the negative electrode current collector, specifically manifested as a decrease in the OI value.

[0064] In magnetic field induced processing, the angle between the direction of the magnetic field and the negative electrode current collector refers to the geometric angle between the direction of the magnetic field and the plane of the negative electrode current collector.

[0065] Optionally, in the magnetic field-induced treatment, the direction of the magnetic field is perpendicular to the plane of the negative electrode current collector.

[0066] As an example, the magnetic field strength can be 3000 Gs, 5000 Gs, 8000 Gs, 10000 Gs, 12000 Gs or 15000 Gs, the processing time can be 2s, 3s, 5s, 6s, 8s or 10s, and the slurry viscosity can be 3000 mPa·s, 5000 mPa·s, 8000 mPa·s, 12000 mPa·s or 15000 mPa·s.

[0067] Optionally, the magnetic field strength is ≥8000 Gs.

[0068] The method for preparing the battery cell in this application involves placing the negative electrode precursor in a magnetic field environment for magnetic field induction treatment. The angle between the magnetic field direction and the negative electrode current collector during the magnetic field induction treatment is set to 60° to 120°. This induces unshaped graphite grains with an aspect ratio ≥2 to be arranged on the surface of the negative electrode current collector. This results in the basal planes of most of the graphite grains in the negative electrode precursor tending to be perpendicular or nearly perpendicular to the negative electrode current collector. On the one hand, during ion insertion and extraction, there is no need for lateral diffusion along the C-axis of the graphite. Instead, the ions move directly along the direction perpendicular or nearly perpendicular to the negative electrode current collector, thereby shortening the straight-line distance of lithium ions from the electrolyte to the negative electrode current collector and achieving straight-line vertical transport. On the other hand, the graphite grains arranged perpendicular to the negative electrode current collector form an ordered "ion channel," reducing the detour paths between particles and significantly shortening the effective transport distance, thereby improving the fast-charging performance of the battery cell.

[0069] In some embodiments, the slurry viscosity is 3000 mPa·s to 9000 mPa·s, and the magnetic field-induced treatment time is ≥2 s.

[0070] Optionally, the processing time for magnetic field-induced treatment is 2s to 5s.

[0071] When the slurry viscosity is within the above range, by making the magnetic field induced treatment time ≥2s, the orientation of most graphite grains tends to be perpendicular or nearly perpendicular to the negative electrode current collector.

[0072] In some embodiments, the slurry viscosity is greater than 9000 mPa·s and less than or equal to 15000 mPa·s, and the processing time for magnetic field-induced treatment is ≥5s.

[0073] When the slurry viscosity is within the above range, by making the magnetic field induced treatment time ≥5s, the orientation of most graphite grains tends to be perpendicular or nearly perpendicular to the negative electrode current collector.

[0074] In some implementations, the magnetic field is an alternating magnetic field.

[0075] An alternating magnetic field is a magnetic field generated by alternating current (such as alternating current) or a time-varying electric field, whose direction and intensity change periodically at a certain frequency (such as 50Hz, 60Hz or higher).

[0076] Alternating magnetic fields can provide a magnetic field environment with higher magnetic field strength, thereby causing the orientation of graphite grains to be mostly perpendicular or nearly perpendicular to the negative electrode current collector through magnetic field induction treatment.

[0077] In addition, the following description, with appropriate reference to the accompanying drawings, describes a battery cell, its preparation method, a secondary battery, and an electrical device according to this application.

[0078] [Battery cell]

[0079] This application does not impose any particular restrictions on the type of battery cell; for example, the battery cell can be a lithium-ion battery, etc.

[0080] Typically, a battery cell includes a positive electrode, a negative electrode, an electrolyte, and a separator. During charging and discharging, active ions move back and forth between the positive and negative electrodes, inserting and releasing. The electrolyte acts as a conductor between the positive and negative electrodes. The separator, positioned between the positive and negative electrodes, primarily prevents short circuits while allowing ions to pass through.

[0081] This application does not impose any particular limitation on the type of electrolyte, which can be selected according to actual needs. For example, the electrolyte can be selected from at least one of solid electrolytes and liquid electrolytes (i.e., electrolyte solutions). This includes battery cells using electrolyte solutions and some battery cells using solid electrolytes.

[0082] [Positive electrode plate]

[0083] The positive electrode includes a positive current collector and a positive electrode film layer disposed on at least one surface of the positive current collector, the positive electrode film layer including a positive electrode active material.

[0084] As an example, the positive current collector has two surfaces opposite each other in its own thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive current collector.

[0085] In some embodiments, the positive current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0086] In some embodiments, when the battery cell is a lithium-ion battery, the positive electrode active material may be a positive electrode active material known in the art for lithium-ion batteries. As an example, the positive electrode active material may include at least one of the following materials: lithium phosphates with an olivine structure, lithium transition metal oxides, and their respective modified compounds. However, this application is not limited to these materials, and other conventional materials that can be used as battery positive electrode active materials may also be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of lithium transition metal oxides include, but are not limited to, lithium cobalt oxides (such as LiCoO2), lithium nickel oxides (such as LiNiO2), lithium manganese oxides (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxides, lithium manganese cobalt oxides, lithium nickel manganese oxides, and lithium nickel cobalt manganese oxides (such as LiNi). 1 / 3 Co 1 / 3Mn 1 / 3 O2 (also known as NCM) 333 LiNi 0.5 Co 0.2 Mn 0.3 O2 (also known as NCM) 523 LiNi 0.5 Co 0.25 Mn 0.25 O2 (also known as NCM) 211 LiNi 0.6 Co 0.2 Mn 0.2 O2 (also known as NCM) 622 LiNi 0.8 Co 0.1 Mn 0.1 O2 (also known as NCM) 811 ), lithium nickel cobalt aluminum oxide (such as LiNi) 0.8 Co 0.15 Al 0.05 At least one of O2 and its modified compounds. Examples of lithium phosphates with an olivine structure include, but are not limited to, lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), lithium iron phosphate and carbon composites, lithium manganese phosphate (such as LiMnPO4), lithium manganese phosphate and carbon composites, lithium manganese iron phosphate, and lithium manganese iron phosphate and carbon composites.

[0087] In some embodiments, to further improve the energy density of a single battery cell, the positive electrode active material for a lithium-ion battery may include materials of the general formula Li. a Ni b Co c M d O e A fone or more of the lithium transition metal oxides and modified compounds thereof. 0.8≤a≤1.2, 0.5≤b<1, 0<c<1, 0<d<1, 1≤e≤2, 0≤f≤1, M is selected from one or more of Mn, Al, Zr, Zn, Cu, Cr, Mg, Fe, V, Ti and B, and A is selected from one or more of N, F, S and Cl.

[0088] In some embodiments, by way of example, the positive electrode active material for a lithium-ion battery may include LiCoO2, LiNiO2, LiMnO2, LiMn2O4, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (NCM333), LiNi 0.5 Co 0.2 Mn 0.3 O2 (NCM523), LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622), LiNi 0.8 Co 0.1 Mn 0.1 O2 (NCM811), LiNi 0.85 Co 0.15 Al 0.05 O2, LiFePO4, and LiMnPO4.

[0089] In the present application, the modified compounds of the aforementioned positive electrode active materials may be doping modification and / or surface coating modification performed on the positive electrode active materials.

[0090] As an optional technical solution of the present application, the polyanionic compound may be Li 1+x Mn 1-y A y P 1-z R z O4; wherein x is any value within a range of -0.100 to 0.100, y is any value within a range of 0.001 to 0.500, z is any value within a range of 0.001 to 0.100, A includes one or more elements selected from Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge, and R includes one or more elements selected from B, S, Si and N;

[0091] As an optional technical solution of the present application, the polyanionic compound may be Li a A e Mn 1-f B f P 1-g Cg O 4-n D n , wherein A includes one or more elements of Zn, Al, Na, K, Mg, Nb, Mo and W; B includes one or more elements of Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge; C includes one or more elements of B, S, Si and N; D includes one or more elements of S, F, Cl and Br; a is selected from a range of 0.9 to 1.1, e is selected from a range of 0.001 to 0.1, f is selected from a range of 0.001 to 0.5, g is selected from a range of 0.001 to 0.1, n is selected from a range of 0.001 to 0.1, and the second positive electrode active material is electrically neutral.

[0092] During charging and discharging processes of a battery, Li is deintercalated and consumed, and the molar content of Li varies when the battery is discharged to different states. In the lists of positive electrode materials in the present application, the molar content of Li is in an initial state of the materials, i.e., a state before material feeding. After the positive electrode materials are applied to a battery system and undergo charging and discharging cycles, the molar content of Li will change.

[0093] In the lists of positive electrode materials in the present application, the molar content of O is only a theoretical state value. Lattice oxygen release will cause a change in the molar content of oxygen, and the actual molar content of O will fluctuate.

[0094] A positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer formed on at least part of a surface of the positive electrode current collector. The positive electrode active material layer includes a positive electrode active material, which may be a positive electrode active material for sodium-ion batteries well known in the art. As an example, the positive electrode active material may include at least one of the following materials: polyanionic compounds, sodium transition metal oxides, Prussian blue analogues, and modified compounds thereof. However, the present application is not limited to these materials, and other conventional materials usable as a battery positive electrode active material may also be used. These positive electrode active materials may be used alone or in combination of two or more.

[0095] As an optional technical solution of the present application, the polyanionic compound may be Na 4+x R 3-y P 4-m O 15 / C, wherein 0<x<0.5, 0<y≤0.5, and 0<m≤0.2, and R includes at least one of Mg, Al, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Zr, Cr, Nb, Mo, In, Ga, Sn, Hf, Ta, W and Pb.

[0096] As an optional technical solution of the present application, the polyanionic compound may be Nax-a A a V y-b M b (PO4) 2-2c (DO4) 2c F z-d Q d Wherein, element A represents an alkali metal element that substitutes for element Na, element M represents a metal element that substitutes for element V, element D represents a dopant element that substitutes for element P, and element Q represents a dopant element that substitutes for element F. Element D includes at least one of Si and S, and element Q includes at least one of Cl and O; 3.5 ≤ x ≤ 4.5, 0 ≤ a ≤ 0.15x, 0.8 ≤ y ≤ 1.1, 0 ≤ b ≤ 0.3y, 0 ≤ c ≤ 0.15, 0.8 ≤ z ≤ 1.1, 0 ≤ d ≤ 0.2z. Optionally, element A includes at least one of K and Li; element M includes at least one of Fe, Cr, Al, Sc, Ga, In, Ti, Zr, Mn, Zn, Ni, Cu, and Co.

[0097] As an optional technical solution in this application, the polyanionic compound can be a compound containing sodium ions, transition metal ions, or a tetrahedral (YO4) structure. n- A class of compounds with anionic units. The transition metal can be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr, and Ce; Y can be at least one of P, S, and Si; n represents (YO4). n- The price state.

[0098] Polyanionic compounds can also contain sodium ions, transition metal ions, or tetrahedral (YO4) ions. n- A class of compounds containing anionic units and halide anions. The transition metal can be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr, and Ce; Y can be at least one of P, S, and Si; n represents (YO4). n- The valence state; the halogen can be at least one of F, Cl and Br.

[0099] Polyanionic compounds can also be sodium-containing tetrahedral (YO4) compounds. n- Anionic unit, polyhedral unit (ZO) y ) m+ And a class of compounds with optional halide anions. Y can be at least one of P, S, and Si, n represents the valence state of V; Z represents a transition metal, which can be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr, and Ce, m represents (ZO) y ) m+ The valence state; the halogen can be at least one of F, Cl and Br.

[0100] Polyanionic compounds include, for example, NaFePO4, Na3V2(PO4)3, NaM'PO4F (where M' is one or more of V, Fe, Mn, and Ni) and Na3(VO y )2(PO4)2F 3-2y At least one of (0≤y≤1).

[0101] As an optional technical solution in this application, in the sodium transition metal oxide, the transition metal can be at least one selected from Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr, and Ce. For example, the sodium transition metal oxide is Na. x MO2, where M is one or more of Ti, V, Mn, Co, Ni, Fe, Cr, and Cu, 0 <x≤1。

[0102] As an optional technical solution in this application, Prussian blue compounds may be those containing sodium ions, transition metal ions, and cyanide ions (CN). - A class of compounds. The transition metal can be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr, and Ce. Prussian blue compounds are, for example, Na. a Me b Me' c (CN)6, wherein Me and Me' are each independently at least one of Ni, Cu, Fe, Mn, Co, and Zn, 0 <a≤2,0<b<1,0<c<1。

[0103] In some embodiments, the positive electrode film layer may optionally include a binder. As an example, the binder may include at least one selected from polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), PVDF-tetrafluoroethylene-propylene terpolymer, PVDF-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorinated acrylate resin.

[0104] In some embodiments, the positive electrode film may optionally include a conductive agent. As an example, the conductive agent may include at least one selected from superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0105] In some embodiments, the positive electrode sheet can be prepared by dispersing the above-mentioned components for preparing the positive electrode sheet, such as positive active material, conductive agent, binder and any other components, in a solvent (e.g., N-methylpyrrolidone) to form a positive electrode slurry; coating the positive electrode slurry onto the positive electrode current collector, and then obtaining the positive electrode sheet after drying, cold pressing and other processes.

[0106] [Negative electrode plate]

[0107] In some embodiments, the negative electrode sheet includes a negative current collector and a negative electrode film layer disposed on at least one surface of the negative current collector.

[0108] As an example, the negative electrode current collector has two surfaces opposite each other in its own thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.

[0109] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0110] In some embodiments, the negative electrode film layer may optionally include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0111] In some embodiments, the negative electrode film may optionally include a conductive agent. The conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0112] In some embodiments, the negative electrode film may optionally include other additives, such as thickeners (e.g., sodium carboxymethyl cellulose (CMC-Na)).

[0113] In some embodiments, the negative electrode sheet can be prepared by dispersing the components used to prepare the negative electrode sheet, such as the negative electrode active material, conductive agent, binder and any other components, in a solvent (e.g., deionized water) to form a negative electrode slurry; coating the negative electrode slurry onto the negative electrode current collector, and then obtaining the negative electrode sheet after drying, cold pressing and other processes.

[0114] In other embodiments, the current collector of the negative electrode sheet typically includes a current collector body and a base coating. The base coating can be disposed on at least one side of the current collector body. The base coating basically does not contain negative electrode active material, and may include a small amount of carbon material. However, the carbon material forms a thin coating and cannot function as a negative electrode active material. In this embodiment, the negative electrode sheet can be an electrode sheet without a negative electrode active material layer. For a negative electrode sheet without a negative electrode active material layer, when the current collector of the negative electrode sheet does not contain a base coating, the film layer can be disposed on the surface of at least one side of the current collector; when the current collector of the negative electrode sheet includes a base coating, the film layer can be disposed on the surface of the base coating away from the current collector.

[0115] In some embodiments, the film layer may further include a binder for fixing the additive to the negative electrode sheet. The type of binder is not particularly limited, and those skilled in the art can choose flexibly according to actual needs.

[0116] [Electrolytes]

[0117] The electrolyte acts as a conductor of ions between the positive and negative electrodes. This application does not impose specific restrictions on the type of electrolyte; it can be selected according to requirements. For example, the electrolyte can be liquid, gel, or entirely solid.

[0118] In some embodiments, the electrolyte is an electrolyte solution. The electrolyte solution includes an electrolyte salt and a solvent.

[0119] In some embodiments, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalate borate, lithium dioxalate borate, lithium difluorodioxalate phosphate, and lithium tetrafluorooxalate phosphate.

[0120] In some embodiments, the solvent may be selected from at least one of ethylene carbonate, propylene carbonate, methyl ethyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butyl carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, sulfolane, dimethyl sulfone, methyl ethyl sulfone, and diethyl sulfone.

[0121] In some embodiments, the electrolyte may optionally include additives. For example, additives may include negative electrode film-forming additives, positive electrode film-forming additives, and may also include additives that can improve certain battery performance, such as additives that improve battery overcharge performance, additives that improve battery high-temperature or low-temperature performance, etc.

[0122] [Isolation membrane]

[0123] In some embodiments, the battery cell also includes a separator. This application does not impose any particular limitation on the type of separator; any known porous separator with good chemical and mechanical stability can be selected.

[0124] In some embodiments, the material of the separator can be selected from at least one of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.

[0125] In some implementations, the positive electrode, negative electrode, and separator can be fabricated into an electrode assembly using a winding or stacking process.

[0126] In some embodiments, the battery cell may include an outer packaging. This outer packaging can be used to encapsulate the electrode assembly and electrolyte described above.

[0127] In some embodiments, the outer packaging of the battery cell can be a rigid shell, such as a hard plastic shell, an aluminum shell, or a steel shell. The outer packaging of the battery cell can also be a flexible package, such as a pouch. The material of the flexible package can be plastic; examples of plastics include polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0128] This application does not impose any particular limitation on the shape of the battery cell; it can be cylindrical, square, or any other arbitrary shape. For example, Figure 1 The example shown is a square-structured battery cell 5.

[0129] In some implementations, refer to Figure 2 The outer packaging may include a housing 51 and a cover plate 53. The housing 51 may include a base plate and side plates connected to the base plate, the base plate and side plates forming a receiving cavity. The housing 51 has an opening communicating with the receiving cavity, and the cover plate 53 can be placed over the opening to close the receiving cavity. The positive electrode sheet, negative electrode sheet, and separator can be formed into an electrode assembly 52 by a winding process or a stacking process. The electrode assembly 52 is encapsulated within the receiving cavity. Electrolyte is immersed in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in a single battery cell 5 can be one or more, which can be selected by those skilled in the art according to specific practical needs.

[0130] In some implementations, individual battery cells can be assembled into a battery module. The number of individual battery cells contained in a battery module can be one or more, and the specific number can be selected by those skilled in the art based on the application and capacity of the battery module.

[0131] Figure 3This is battery module 4, used as an example. (See reference...) Figure 3 In battery module 4, multiple battery cells 5 can be arranged sequentially along the length of battery module 4. Of course, they can also be arranged in any other manner. Furthermore, these multiple battery cells 5 can be fixed in place using fasteners.

[0132] Optionally, the battery module 4 may also include a housing with a receiving space in which multiple battery cells 5 are received.

[0133] In some embodiments, the battery modules described above can also be assembled into a battery pack, and the number of battery modules contained in the battery pack can be one or more, the specific number of which can be selected by those skilled in the art according to the application and capacity of the battery pack.

[0134] Figure 4 and Figure 5 This is battery pack 1 as an example. (See reference...) Figure 4 and Figure 5 The battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box includes an upper body 2 and a lower body 3, with the upper body 2 covering the lower body 3 to form a closed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.

[0135] In addition, this application also provides an electrical device, which includes at least one of the battery cell, battery module, or battery pack provided in this application. The battery cell, battery module, or battery pack can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device may include, but is not limited to, mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc.

[0136] As the electrical device, a single battery cell, a battery module, or a battery pack can be selected according to its usage requirements.

[0137] Figure 6 This is an example of an electrical device. The device could be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of individual battery cells, a battery pack or battery module can be used.

[0138] Another example device could be a mobile phone, tablet, or laptop. These devices typically require a slim and lightweight design and can use a single battery cell as their power source.

[0139] Example

[0140] The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.

[0141] The relevant parameters of the battery cells of Examples 1-4 and Comparative Examples 1-3 are shown in Table 1 below.

[0142] Table 1. Relevant parameters of the battery cells in Examples 1-4 and Comparative Examples 1-3.

[0143]

[0144]

[0145] The aspect ratio of graphite was measured using the following method:

[0146] The graphite powders of the negative electrode sheets from Examples 1-4 and Comparative Examples 1-3 were tested using a Zeiss Sigma 300 microscope. Parameter settings: Mode: In-lens, Voltage: 10KV, Aperture: 30µm, Working distance: 4.5mm. Testing procedure: The sample was moved approximately 100x to confirm no significant abnormalities. Two fields of view were randomly selected on the anode, and two sets of images were taken at 10K, 5K, 3K, 1K, and 500 nm focusing on the particle surface. Based on the collected SEM images of the powder, statistical calculations were performed: taking a single particle as an example, its longest diameter was selected as the "length," and the length perpendicular to the length direction was designated as the "diameter." The length-diameter ratio (LAR) was calculated as the length-diameter ratio. As much LAR data as possible was collected, and the average of these values ​​was taken as the LAR of the graphite powder.

[0147] The degree of graphitization of graphite was measured by the following method:

[0148] The negative electrode sheets of Examples 1-4 and Comparative Examples 1-3 were tested using an X-ray diffractometer (Bruker D8 Discover, JIS K 0131-1996). The interlayer spacing d002 of the graphite (002) crystal plane was measured by X-ray diffraction, and then the degree of graphitization was calculated using the Mering-Maire formula (also known as the Franklin formula). The formula is as follows:

[0149] [G=(3.440-d002) / (3.440-3.354)×100%];

[0150] Where G is the degree of graphitization, 3.440 is the interlayer spacing of completely non-graphitized carbon, 3.354 is the interlayer spacing of an ideal graphite crystal, and d002 is the interlayer spacing of the (002) crystal plane of the carbon material.

[0151] The C004 / C110 ratio (OI value) of the negative electrode sheet under X-ray diffraction was measured by the following method:

[0152] The negative electrode sheets of Examples 1-4 and Comparative Examples 1-3 were tested using an X-ray diffractometer (Bruker D8 Discover, JIS K 0131-1996). The OI value of the negative electrode sheet was calculated using the formula OI = C004 / C110, where C004 is the peak area of ​​the 004 characteristic diffraction peak of the negative electrode sheet and C110 is the peak area of ​​the 110 characteristic diffraction peak of the negative electrode sheet.

[0153] The C004 / C110 ratio (OI value) of graphite under X-ray diffraction was determined by the following method:

[0154] The graphite powder in the negative electrode sheets of Examples 1-4 and Comparative Examples 1-3 was tested using an X-ray diffractometer (Bruker D8 Discover, JIS K 0131-1996). The OI value of the graphite powder was calculated using the formula OI = C004 / C110, where C004 is the peak area of ​​the 004 characteristic diffraction peak of the graphite powder and C110 is the peak area of ​​the 110 characteristic diffraction peak of the graphite powder.

[0155] The preparation methods of the battery cells in Examples 1-4 and Comparative Example 3 of this application include the following steps:

[0156] S1. Preparation of the positive electrode sheet

[0157] A positive electrode slurry was prepared by mixing lithium iron phosphate (LiFePO4) as the positive electrode active material, acetylene black as the conductive agent, and polyvinylidene fluoride as the binder in a weight ratio of 97.9:0.5:1.6 and dissolving them in N-methylpyrrolidone (NMP). The water content of the lithium iron phosphate positive electrode active material was 200 ppm. The positive electrode slurry was then coated onto an aluminum current collector foil, dried, and subjected to cold pressing, edge trimming, cutting, and slitting to obtain the positive electrode sheet. The density of the positive electrode active material layer in the positive electrode sheet was 2.8 g / cm³.

[0158] S2. Preparation of negative electrode sheet

[0159] A negative electrode slurry was prepared by dissolving the negative electrode active material (sheet graphite in Examples 1-4, and secondary graphite particles in Comparative Example 3), conductive agent SuperP, thickener CMC, and binder styrene-butadiene rubber (SBR) in deionized water at a weight ratio of 96:2:1:1. Magnets were placed symmetrically above and below the negative electrode coating to subject the negative electrode precursor to a perpendicular magnetic field. The negative electrode slurry was then uniformly coated onto the negative electrode current collector copper foil. After drying, the coating was cold-pressed, trimmed, cut, and slit to produce the negative electrode sheet for a lithium-ion battery.

[0160] S3. Preparation of the isolation membrane

[0161] Porous polyethylene (PP) film is used as the separator.

[0162] S4. Preparation of electrolyte

[0163] In an argon-atmospheric glove box with a water content of <10 ppm, ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate were mixed in a volume ratio of 3:3:4. Lithium hexafluorophosphate (LiPF6) was then uniformly dissolved in the solvent, and FEC was added to obtain the electrolyte. The molar concentration of LiPF6 in the electrolyte was 1 mol / L.

[0164] S5, Assembly

[0165] The positive electrode, separator, and negative electrode are prepared in sequence, with the separator positioned between the positive and negative electrodes to provide isolation. The electrodes are then wound, hot-pressed, shaped, and welded to obtain the electrode assembly. The electrode assembly is placed in a square aluminum shell, vacuum-dried, and then injected with electrolyte. After standing, formation testing, aging, and capacity testing, a single battery cell with a volume of 0.411L is finally obtained.

[0166] The preparation method of the battery cells in Comparative Examples 1 and 2 of this application includes the following steps:

[0167] S1. Preparation of the positive electrode sheet

[0168] A positive electrode slurry was prepared by mixing lithium iron phosphate (LiFePO4) as the positive electrode active material, acetylene black as the conductive agent, and polyvinylidene fluoride as the binder in a weight ratio of 97.9:0.5:1.6 and dissolving them in N-methylpyrrolidone (NMP). The water content of the lithium iron phosphate positive electrode active material was 200 ppm. The positive electrode slurry was then coated onto an aluminum current collector foil, dried, and subjected to cold pressing, edge trimming, cutting, and slitting to obtain the positive electrode sheet. The density of the positive electrode active material layer in the positive electrode sheet was 2.8 g / cm³.

[0169] S2. Preparation of negative electrode sheet

[0170] The negative electrode active material (comparative example 1 is flake graphite, comparative example 2 is secondary graphite particles), conductive agent SuperP, thickener CMC, and binder styrene-butadiene rubber (SBR) are dissolved in deionized water at a weight ratio of 96:2:1:1 and mixed evenly to prepare a negative electrode slurry. The negative electrode slurry is evenly coated on the negative electrode current collector copper foil, dried, and then cold-pressed, trimmed, cut, and slit to produce the negative electrode sheet of the lithium-ion battery.

[0171] S3. Preparation of the isolation membrane

[0172] Porous polyethylene (PP) film is used as the separator.

[0173] S4. Preparation of electrolyte

[0174] In an argon-atmospheric glove box with a water content of <10 ppm, ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate were mixed in a volume ratio of 3:3:4. Lithium hexafluorophosphate (LiPF6) was then uniformly dissolved in the solvent, and FEC was added to obtain the electrolyte. The molar concentration of LiPF6 in the electrolyte was 1 mol / L.

[0175] S5, Assembly

[0176] The positive electrode, separator, and negative electrode are prepared in sequence, with the separator positioned between the positive and negative electrodes to provide isolation. The electrodes are then wound, hot-pressed, shaped, and welded to obtain the electrode assembly. The electrode assembly is placed in a square aluminum shell, vacuum-dried, and then injected with electrolyte. After standing, formation testing, aging, and capacity testing, a single battery cell with a volume of 0.411L is finally obtained.

[0177] In addition, the 25°C fast charging time and 35°C fast charging time of the battery cells prepared in Examples 1-4 and Comparative Examples 1-3 were measured, and the test results are shown in Tables 2-4 below.

[0178] The testing method is as follows:

[0179] 1. Three-electrode fast charging test

[0180] First, the capacity was measured, then the system was adjusted to 50% SOC for lithium plating. After lithium plating, the system was fully discharged at room temperature before a three-electrode lithium plating test was performed.

[0181] S1, 25℃ Capacity Test;

[0182] At 25°C, after standing still for 5 minutes, discharge at a constant current of 0.33C to 2V. After standing still for 5 minutes, charge at a constant current of 0.33C to 3.65V, then charge at a constant voltage of 0.05C. After standing still for 5 minutes, discharge at a constant current of 0.33C to 2V. At this point, the test capacity C0 is obtained. After standing still for 5 minutes, charge at a constant current of 0.33C0 for 90 minutes. At this point, adjust to 50% SOC.

[0183] S2, lithium plating at 25℃, the negative electrode voltage after lithium plating is between 40 and 400mV;

[0184] At 25°C, after standing still for 1 minute, it was charged with a constant current of 0.00002A for 2 hours (positive electrode - reference), after standing still for 1 minute, it was charged with a constant current of 0.00002A for 2 hours (negative electrode - reference), and then stood still for 1 minute.

[0185] S3 and CC.Rate tests, programmable temperature 25℃, full monitoring of the battery and negative electrode potential, can use a multi-channel temperature measuring instrument, voltage protection range: 1.9V~3.8V;

[0186] Adjust the temperature of the constant temperature chamber to 25℃. After standing for 1 hour, discharge with a constant current of 0.33C0 to 2V. After standing for 10 minutes, charge with a constant current of 0.5C0 to 3.65V. After standing for 10 minutes, discharge with a constant current of 0.33C0 to 2V. After standing for 10 minutes, charge with a constant current of 0.8C0 to 3.65V. After standing for 10 minutes, discharge with a constant current of 0.33C0 to 2V. After standing for 10 minutes, charge with a constant current of 1C0 to 3.65V (cutoff voltage or anode potential (0V) jumps). After standing for 10 minutes, discharge with a constant current of 0.33C0 to 2V. After standing for 10 minutes, charge with a constant current of 1.5C0. Charge to 3.65V (jump at cutoff voltage or anode potential (0V)), let stand for 10 minutes, then discharge with 0.33C0 at a constant current to 2V, let stand for 10 minutes, then charge with 2C0 at a constant current to 3.65V, let stand for 10 minutes, then discharge with 0.33C0 at a constant current to 2V, let stand for 10 minutes, then charge with 2.5C0 at a constant current to 3.65V (jump at cutoff voltage or anode potential (0V)), let stand for 10 minutes, then discharge with 0.33C0 at a constant current to 2V, let stand for 10 minutes, then charge with 3C0 at a constant current to 3.65V (jump at cutoff voltage or anode potential (0V)), and let stand for 10 minutes.

[0187] S4, CC.Rate test, programmable temperature 35℃, full monitoring of the battery and negative electrode potential, can use a multi-channel temperature measuring instrument, voltage protection range: 1.9V~3.8V;

[0188] Adjust the temperature of the constant temperature chamber to 35℃. After standing for 1 hour, discharge with a constant current of 0.33C0 to 2V. After standing for 10 minutes, charge with a constant current of 0.5C0 to 3.65V. After standing for 10 minutes, discharge with a constant current of 0.33C0 to 2V. After standing for 10 minutes, charge with a constant current of 0.8C0 to 3.65V. After standing for 10 minutes, discharge with a constant current of 0.33C0 to 2V. After standing for 10 minutes, charge with a constant current of 1C0 to 3.65V (cutoff voltage or anode potential (0V) jumps). After standing for 10 minutes, discharge with a constant current of 0.33C0 to 2V. After standing for 10 minutes, charge with a constant current of 1.5C0. Charge to 3.65V (jump at cutoff voltage or anode potential (0V)), let stand for 10 minutes, then discharge with 0.33C0 at a constant current to 2V, let stand for 10 minutes, then charge with 2C0 at a constant current to 3.65V, let stand for 10 minutes, then discharge with 0.33C0 at a constant current to 2V, let stand for 10 minutes, then charge with 2.5C0 at a constant current to 3.65V (jump at cutoff voltage or anode potential (0V)), let stand for 10 minutes, then discharge with 0.33C0 at a constant current to 2V, let stand for 10 minutes, then charge with 3C0 at a constant current to 3.65V (jump at cutoff voltage or anode potential (0V)), and let stand for 10 minutes.

[0189] Table 2 Performance test results of Examples 1-4 and Comparative Example 1

[0190] project Fast charging time at 25℃ (min) 35℃ Fast Charging Time (min) Example 1 21.6 15.7 Example 2 23 17.5 Example 3 25.3 19.6 Example 4 22 16 Comparative Example 1 29.6 23.2

[0191] As can be seen from Examples 1-4, Examples 1-4 of this application use graphite with an aspect ratio ≥2, and perform magnetic field-induced treatment on the negative electrode precursor, which enables the C004 / C110 ratio of the negative electrode to be ≤3 under X-ray diffraction. The resulting battery cell has a fast charging time of [time missing] at 25°C.

[0192] The charging time is 21.6 min to 25.3 min, and the fast charging time at 35℃ is 15.7 min to 19.6 min.

[0193] Comparing Comparative Example 1 and Example 1, it can be seen that Comparative Example 1 uses natural graphite with an aspect ratio of 5.5 and does not perform magnetic field induction treatment on the negative electrode precursor. The battery cell prepared by it has a fast charging time of 29.6 min at 25°C and a fast charging time of 23.2 min at 35°C, both of which are much longer than those of Example 1.

[0194] Table 3 Performance test results of Examples 1-3 and Comparative Example 2

[0195] project Fast charging time at 25℃ (min) 35℃ Fast Charging Time (min) Example 1 21.6 15.7 Example 2 23 17.5 Example 3 25.3 19.6 Comparative Example 2 25.8 20

[0196] Comparing Comparative Example 2 with Examples 1-3, it can be seen that Comparative Example 2 uses secondary graphite particles with an aspect ratio of 1.9 and does not perform magnetic field induction treatment on the negative electrode precursor. The resulting battery cell has a fast charging time of 25.8 min at 25°C and a fast charging time of 20 min at 35°C, which is longer than that of Examples 1-3. This indicates that using sheet graphite with an aspect ratio ≥2 as the positive electrode active material, after magnetic field induction treatment, results in better fast charging performance than secondary graphite particles.

[0197] Table 4 Performance test results of Comparative Examples 2-3

[0198] project Fast charging time at 25℃ (min) 35℃ Fast Charging Time (min) Comparative Example 2 25.8 20 Comparative Example 3 24 18.4

[0199] Comparing Comparative Examples 2 and 3, it can be seen that Comparative Examples 2 and 3 all use secondary graphite particles with an aspect ratio of 1.9. Among them, Comparative Example 2 did not perform magnetic field induction treatment on the negative electrode precursor, while Comparative Example 3 performed magnetic field induction treatment on the negative electrode precursor. However, the fast charging time of Comparative Examples 2 and 3 at 25℃ and at 35℃ is not significantly different. This indicates that the effect of magnetic field induction treatment is not significant for secondary graphite particles with an aspect ratio of 1.9.

[0200] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.

Claims

1. A battery cell, characterized by, The battery cell includes: a negative electrode sheet, the negative electrode sheet including a negative current collector and a negative electrode film layer disposed on at least one surface of the negative current collector, the negative electrode film layer including a negative electrode active material, the negative electrode active material including graphite, the aspect ratio of the graphite being ≥2, and the C004 / C110 ratio of the negative electrode sheet being ≤3 under X-ray diffraction.

2. The battery cell of claim 1, wherein, When the graphite powder is in a disordered state, the ratio of C004 / C110 under X-ray diffraction is ≥5.

3. The battery cell according to claim 1, characterized in that, The graphite mentioned is natural graphite.

4. The battery cell according to claim 3, characterized in that, The degree of graphitization of the natural graphite is ≥95%.

5. A method for preparing a single battery cell, characterized in that, The method for preparing the battery cell includes placing a negative electrode precursor in a magnetic field environment for magnetic field induction treatment. The negative electrode precursor includes a negative current collector and a negative electrode slurry coated on at least one surface of the negative current collector. The negative electrode slurry includes a negative electrode active material, which includes graphite with an aspect ratio ≥2. In the magnetic field induction treatment, the angle between the magnetic field direction and the negative current collector is 60° to 120°, the magnetic field strength is ≥3000 Gs, the treatment time is ≥2s, and the slurry viscosity is 3000 mPa·s to 15000 mPa·s. After the magnetic field induction treatment is completed, drying and cold pressing are performed.

6. The method for preparing a battery cell according to claim 5, characterized in that, The viscosity of the slurry is 3000 mPa·s to 9000 mPa·s, and the processing time of the magnetic field-induced treatment is ≥2s.

7. The method for preparing a battery cell according to claim 5, characterized in that, The slurry viscosity is greater than 9000 mPa·s and less than or equal to 15000 mPa·s, and the processing time of the magnetic field-induced treatment is ≥5s.

8. The method for preparing a battery cell according to claim 5, characterized in that, The magnetic field is an alternating magnetic field.

9. A secondary battery, characterized in that, The secondary battery includes the battery cell according to any one of claims 1 to 4 or the battery cell prepared by the method according to any one of claims 5 to 8.

10. An electrical device, characterized in that, The electrical device includes the secondary battery as described in claim 9, the secondary battery being used to provide electrical energy.