Secondary battery and electric device

By employing an upper and lower layer combination of positive electrode active materials in lithium-ion batteries, and using a combination of single-crystal and polycrystalline particles, the oxygen release problem in medium- and high-nickel lithium-ion batteries has been solved, thereby improving safety and power performance.

CN123162268APending Publication Date: 2026-11-24CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510667921.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-22
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing lithium-ion battery cathode materials with high nickel content suffer from oxygen release during use, leading to a decline in safety performance and becoming an obstacle to large-scale industrialization.

Method used

The cathode active material layer is designed with an upper and lower combination. The upper layer uses a first cathode material with a single crystal particle morphology, and the lower layer uses a second cathode material with a polycrystalline particle morphology. This combination design reduces oxygen release at grain boundaries and improves safety performance.

Benefits of technology

It effectively reduces oxygen release at grain boundaries, improves battery safety and power performance, and balances overall battery safety, reliability, and cycle life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123162268A_ABST
    Figure CN123162268A_ABST
Patent Text Reader

Abstract

This application provides a secondary battery and an electrical device. The secondary battery includes a positive electrode sheet, which includes a positive current collector and a positive active material layer disposed on at least one surface of the positive current collector. The positive active material layer includes a first positive active material layer and a second positive active material layer, with the second positive active material layer disposed between the positive current collector and the first positive active material layer. The first positive active material layer includes a first positive electrode material with a single-crystal particle morphology, the first positive electrode material having a nickel content greater than or equal to 50%, and an average particle size D501 greater than or equal to 2.8 μm. The second positive active material layer includes a second positive electrode material with a polycrystalline particle morphology, the second positive electrode material having a nickel content greater than or equal to 50%. The secondary battery provided by this application has improved safety performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of battery technology, and in particular to a secondary battery and an electrical device. Background Technology

[0002] In recent years, with the increasingly widespread application of lithium-ion batteries, they have been widely used in energy storage systems such as hydropower, thermal power, wind power, and solar power plants, as well as in power tools, electric bicycles, electric motorcycles, electric cars, military equipment, aerospace, and many other fields. Due to the significant development of rechargeable batteries, higher requirements have been placed on their safety and other performance characteristics. Summary of the Invention

[0003] This application provides a secondary battery and an electrical device that improves the safety performance of the battery.

[0004] To achieve the above objectives, a first aspect of this application provides a secondary battery, comprising: a positive electrode sheet, the positive electrode sheet including a positive current collector and a positive active material layer disposed on at least one surface of the positive current collector, the positive active material layer including a first positive active material layer and a second positive active material layer, the second positive active material layer being disposed between the positive current collector and the first positive active material layer;

[0005] The first positive electrode active material layer includes a first positive electrode material with a single crystal particle morphology, the nickel content of the first positive electrode material is greater than or equal to 50%, and the average particle size D501 of the first positive electrode material is greater than or equal to 2.8 μm;

[0006] The second positive electrode active material layer includes a second positive electrode material with a polycrystalline particle morphology, and the nickel content of the second positive electrode material is greater than or equal to 50%.

[0007] The aforementioned secondary battery provided in this application uses a ternary cathode material with a medium- or high-nickel system. The cathode active material layer is designed as an upper and lower layer combination. In the upper layer (i.e., the first cathode active material layer) which is in direct contact with the electrolyte, the first cathode material has a single-crystal particle morphology, that is, the upper layer includes single-crystal particles with a relatively large average particle size. In the lower layer (i.e., the second cathode active material layer) which is relatively close to the cathode current collector, the second cathode material has a polycrystalline particle morphology, that is, the lower layer includes polycrystalline particles. Through this upper and lower layer combination design with large-sized single-crystal particles in the upper layer and polycrystalline particles in the lower layer, not only can the release of oxygen at grain boundaries be reduced and the safety performance improved, but the power performance can also be taken into account to a certain extent.

[0008] In some embodiments of this application, the nickel content of the first cathode material and the second cathode material is independently greater than or equal to 50% and less than or equal to 98%;

[0009] Optionally, each of the first positive electrode material and the second positive electrode material independently satisfies the chemical formula: Li x’ Ni x Co y M 1-x-y O y’ , where M includes at least one of Mn, Al, B, Zr, Sr, Y, Sb, W, Ti, Mg, Zn and Nb, 0.5≤x≤0.98, 0<y≤0.4, 0.6≤x'≤1.2, 1.6≤y'≤2.2; further optionally, M includes at least one of Mn, Al, B, Zr, Sr, W, Mg, Y and Nb.

[0010] In some embodiments of the present application, one or more of the following conditions are satisfied:

[0011] (1) a nickel content of the first positive electrode material is greater than or equal to 80% and less than or equal to 98%;

[0012] Optionally, the first positive electrode material satisfies the chemical formula: Li x1’ Ni x1 Co y1 M 1 1-x1-y1 O y1’ , where M 1 includes at least one of Mn, Al, B, Zr, Sr, W, Mg, Y and Nb, 0.8≤x1≤0.98, 0<y1≤0.3, 0.6≤x1'≤1.2, 1.6≤y1'≤2.2;

[0013] (2) a nickel content of the second positive electrode material is greater than or equal to 80% and less than or equal to 98%;

[0014] Optionally, the second positive electrode material satisfies the chemical formula: Li x2’ Ni x2 Co y2 M 2 1-x2-y2 O y2’ , where M 2 includes at least one of Mn, Al, B, Zr, Sr, W, Mg, Y and Nb, 0.8≤x2≤0.98, 0<y2≤0.3, 0.6≤x2'≤1.2, 1.6≤y2'≤2.2.

[0015] In some embodiments of the present application, an average particle size D501 of the first positive electrode material is 2.8 μm to 7.5 μm, optionally 4.5 μm to 6.5 μm.

[0016] In some embodiments of this application, the average particle size D502 of the second positive electrode material is 7μm~15μm, and can be selected as 9μm~12μm.

[0017] In some embodiments of this application, one or more of the following conditions are met:

[0018] (1) The particle size distribution span 1 of the first positive electrode material is 1.5~2.5;

[0019] (2) The particle size distribution span2' of the second positive electrode material is 1.1~1.8.

[0020] In some embodiments of this application, the mass ratio of the first positive electrode material to the second positive electrode material is (5:95) to (40:60), and can be (10:90) to (40:60).

[0021] In some embodiments of this application, the second positive electrode active material layer further includes a third positive electrode material having a single-crystal particle morphology, wherein the nickel content of the third positive electrode material is greater than or equal to 50%;

[0022] Optionally, the nickel content of the third cathode material is 1% to 3% higher than that of the second cathode material;

[0023] Optionally, in the second positive electrode active material layer, the mass ratio of the third positive electrode material to the second positive electrode material is (1:9) to (5:5);

[0024] Optionally, the average particle size of the second cathode material is D502, and the average particle size of the third cathode material is D503, where D503 / D502 = 0.2~0.5.

[0025] In some embodiments of this application, the nickel content of the third cathode material is greater than or equal to 50% and less than or equal to 98%.

[0026] Optionally, the third cathode material satisfies the chemical formula: Li x3’ Ni x3 Co y3 M 3 1-x3-y3 O y3’ The M 3 Includes at least one of Mn, Al, B, Zr, Sr, W, Mg, Y, and Nb, 0.5 ≤ x³ ≤ 0.98, 0 <y3≤0.4,0.6≤x3’≤1.2,1.6≤y3’≤2.2;

[0027] Further optionally, the nickel content of the third cathode material is greater than or equal to 80% and less than or equal to 98%;

[0028] Further alternatively, 0.8 ≤ x3 ≤ 0.98, 0 <y3≤0.3,0.6≤x3’≤1.2,1.6≤y3’≤2.2。

[0029] In some embodiments of this application, the particle size distribution span2 of the positive electrode material in the second positive electrode active material layer is 1.1~3.0.

[0030] In some embodiments of this application, the first positive electrode material accounts for 5% to 95% of the mass of the positive electrode active material layer.

[0031] In some embodiments of this application, the film resistance of the positive electrode is 0.35Ω~0.6Ω.

[0032] In some embodiments of this application, the electrolyte of the secondary battery includes a weak solvating solvent, wherein the solvation energy of the weak solvating solvent at 25°C and 101 kPa is less than or equal to 150 kJ / mol, and the ionic conductivity of the electrolyte at 25°C is greater than or equal to 10 mS / cm.

[0033] In some embodiments of this application, one or more of the following conditions are met:

[0034] (1) The weak solvating solvent includes one or more of carbonate solvents, sulfite solvents, and carboxylic acid ester solvents;

[0035] (2) The volume percentage of the weak solvating solvent in the electrolyte is 10% to 30%.

[0036] In some embodiments of this application, the electrolyte has an ionic conductivity of 10 mS / cm to 14 mS / cm at 25°C.

[0037] In some embodiments of this application, the electrolyte further includes additives, which include one or more of the following: ethylene carbonate, lithium difluorooxalate borate, succinate, lithium difluorophosphate, ethylene carbonate, fluoroethylene carbonate, propylene sulfite, ethylene sulfate, propylene-1,3-sulfonyl lactone, and methanedisulfonate.

[0038] Optionally, the additive accounts for 0.1% to 0.5% of the mass of the electrolyte.

[0039] A second aspect of this application provides an electrical device including a secondary battery as described in the first aspect of this application.

[0040] The electrical device of this application includes the secondary battery provided in this application, and therefore has at least the same advantages as the secondary battery.

[0041] Details of one or more embodiments of this application are set forth in the following drawings and description. Other features, objects, and advantages of this application will become apparent from the specification, drawings, and claims. Attached Figure Description

[0042] To better describe and illustrate the embodiments or examples provided in this application, reference may be made to one or more accompanying drawings. Additional details or examples used to describe the drawings should not be considered as limiting the scope of any of the disclosed applications, the currently described embodiments or examples, or the best mode of conduct of these applications as currently understood. Furthermore, the same reference numerals denote the same parts throughout the drawings. In the drawings:

[0043] Figure 1 This is a schematic diagram of the structure of the positive electrode in a secondary battery according to one embodiment of this application.

[0044] Figure 2 This is a schematic diagram of a battery cell according to one embodiment of this application.

[0045] Figure 3 for Figure 2 An exploded view of a battery cell according to one embodiment of this application is shown.

[0046] Figure 4 This is a schematic diagram of a battery device according to one embodiment of this application.

[0047] Figure 5 This is a schematic diagram of a battery pack according to one embodiment of this application.

[0048] Figure 6 for Figure 5 An exploded view of a battery pack according to one embodiment of this application is shown.

[0049] Figure 7 This is a schematic diagram of an electrical device that uses a secondary battery as a power source according to an embodiment of this application.

[0050] Explanation of reference numerals in the attached figures:

[0051] 1 Battery pack; 2 Upper casing; 3 Lower casing; 4 Battery assembly; 5 Individual battery cell; 51 Housing; 52 Electrode assembly; 53 Cover plate; 6 Electrical device. Detailed Implementation

[0052] Hereinafter, some embodiments of this application are described in detail with appropriate reference to the accompanying drawings. However, some unnecessary details may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of actually identical structures may be omitted. This is to avoid making the following description unnecessarily lengthy and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided to enable those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.

[0053] The "range" disclosed in this application can be defined in the form of a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints. Any endpoint can be independently included or excluded, and they can be combined arbitrarily; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60~120 and 80~110 are listed for a specific parameter, it is expected that ranges of 60~110 and 80~120 are also included. Furthermore, if minimum range values ​​of 1 and 2 are listed, and if maximum range values ​​of 3, 4, and 5 are also listed, then the following ranges are all expected: 1~3, 1~4, 1~5, 2~3, 2~4, and 2~5. In this application, unless otherwise stated, the numerical range "a~b" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0~5" indicates that all real numbers between "0" and "5" have been listed in this article; "0~5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is described as an integer ≥2, it is equivalent to listing integers such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc. For instance, when a parameter is described as an integer selected from "2~10", it is equivalent to listing the integers 2, 3, 4, 5, 6, 7, 8, 9, and 10.

[0054] In this application, the terms "multiple" or "various" are used unless otherwise specified, referring to a quantity greater than or equal to 2. For example, "one or more" means one or more types.

[0055] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.

[0056] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment or implementation of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments. The term "implementation" as used herein has a similar understanding.

[0057] Those skilled in the art will understand that the order in which the steps are written in the methods of various embodiments or examples does not imply a strict execution order and does not constitute any limitation on the implementation process. The detailed execution order of each step should be determined by its function and possible internal logic. Unless otherwise specified, all steps of this application may be performed sequentially or randomly, preferably sequentially. For example, if the method includes steps (a) and (b), it means that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, if the method may also include step (c), it means that step (c) can be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.

[0058] In this application, "optionally," "optionally," and "optional" mean that something is optional, that is, it means that it is selected from either "with" or "without." If there are multiple "optional" entries in a technical solution, unless otherwise specified and there are no contradictions or mutual constraints, each "optional" entry shall be independent.

[0059] Currently, increasing the nickel content is a crucial way to achieve high specific energy for NCM ternary cathode materials. However, with the increase of nickel content, oxygen release at the positive and negative electrode interfaces gradually emerges. Moreover, for medium and high nickel systems, the safety issues caused by this oxygen release at the positive and negative electrode interfaces pose a significant challenge to large-scale industrialization; this problem is particularly prominent in high nickel cases. Therefore, it is urgent to solve the safety issues caused by oxygen release in medium and high nickel ternary cathode materials, especially in high nickel systems.

[0060] To address the aforementioned technical problems, this application provides a secondary battery in which the positive electrode active material layer is designed as an upper and lower layer combination, and the upper and lower layers are respectively made of specific ternary positive electrode materials. This can reduce the oxygen release problem caused by medium and high nickel systems, especially high nickel systems, and is beneficial to improving battery safety performance.

[0061] It should be noted that the "medium and high nickel system" mentioned in this application refers to ternary cathode materials with a nickel content greater than or equal to 50%; while the "high nickel system" refers to ternary cathode materials with a nickel content greater than or equal to 80%.

[0062] Firstly, this application provides a secondary battery; please refer to [link to relevant documentation]. Figure 1 It includes: a positive electrode sheet, the positive electrode sheet including a positive current collector 10 and a positive active material layer 11 disposed on at least one surface of the positive current collector, the positive active material layer 11 including a first positive active material layer 110 and a second positive active material layer 120, the second positive active material layer 120 being disposed between the positive current collector 10 and the first positive active material layer 110;

[0063] The first positive electrode active material layer 110 includes a first positive electrode material with a single crystal particle morphology, wherein the nickel content of the first positive electrode material is greater than or equal to 50%, and the average particle size D501 of the first positive electrode material is greater than or equal to 2.8 μm.

[0064] The second positive electrode active material layer 120 includes a second positive electrode material with a polycrystalline particle morphology, and the nickel content of the second positive electrode material is greater than or equal to 50%.

[0065] It should be noted that the "ternary cathode material" mentioned in this application refers to a nickel-cobalt-manganese-based cathode material that includes lithium, nickel, cobalt, manganese and oxygen; the "nickel content of the cathode material" refers to the percentage of nickel atoms in the ternary cathode material based on the total number of atomic moles of all transition metal elements.

[0066] In ternary cathode materials, due to the low binding energy between Ni and O, Ni is the most unstable element in the ternary system and is most likely to gain electrons from the oxygen ions it binds to, causing the oxygen ions to lose electrons and release oxygen, thus deteriorating safety performance. Furthermore, oxygen release usually occurs first at grain boundaries because the current density and electrochemical reaction activity are higher at grain boundaries, and lattice oxygen is more likely to lose electrons and release oxygen.

[0067] In view of this, the aforementioned secondary battery provided in this application, in the ternary cathode material of medium and high nickel system, sets the cathode active material layer as an upper and lower layer combination design, and in the upper layer (i.e. the first cathode active material layer) which is in direct contact with the electrolyte, the first cathode material has a single crystal particle morphology, that is, the upper layer includes single crystal particles with a large average particle size, while in the lower layer (i.e. the second cathode active material layer) which is relatively close to the cathode current collector, the second cathode material has a polycrystalline particle morphology, that is, the lower layer includes polycrystalline particles. Through this upper and lower layer combination design with the upper layer including large single crystal particles and the lower layer including polycrystalline particles, the release of oxygen at grain boundaries can be reduced and the safety performance can be improved.

[0068] Specifically, the upper layer includes single-crystal particles, which can effectively reduce the number of grain boundaries and help reduce oxygen release from grain boundaries. At the same time, the single-crystal particles with an average particle size D501 greater than or equal to 2.8 μm are relatively large, and the grain boundary area formed by the contact between these single-crystal particles per unit volume is relatively small. As a result, the grain boundary reaction area for oxygen release reaction is small, and the resistivity of these relatively large single-crystal particles is high. Under extreme conditions, such as high temperature, overcharging, needle penetration, lithium plating, and short circuit between positive and negative electrodes, the electrochemical reaction intensity and short circuit current at the positive and negative electrode interface can be reduced from the intrinsic material properties, thereby reducing the amount of oxygen released and the short circuit current, and improving safety and reliability.

[0069] Furthermore, the relatively large single-crystal particles have a relatively low specific surface area, resulting in fewer side reactions with the electrolyte. They are also more pressure-resistant, less prone to breakage, and have higher structural stability. The lower layer includes polycrystalline particles, which have more ion pathways, facilitating lithium-ion conduction. This helps compensate for the slight decrease in lithium-ion diffusion kinetics caused by the upper single-crystal particles, thus maintaining overall cathode kinetic performance. Additionally, lithium ions are more easily inserted and extracted and exhibit weaker polarization within the polycrystalline particles, further contributing to energy density. Therefore, through the synergistic combination of the upper and lower layers, a balance between safety and power performance can be achieved in the ternary cathode material.

[0070] Furthermore, the single-crystal particles in the upper layer are more pressure-resistant and structurally more stable. Their higher structural stability can suppress electrode pulverization and reduce the reaction interface between the electrolyte and the lower polycrystalline particles, thus shielding the electrolyte from adverse side reactions and reducing electrolyte and cathode material losses. Meanwhile, the lower polycrystalline particles are located in a relatively "static" region (i.e., with low electrochemical reaction concentration and ion exchange density), so the volume expansion of the polycrystalline particles has less impact on the overall structure (polycrystalline particles are composed of small-diameter single-crystal particles, resulting in more grain boundaries and lattice expansion, which causes more intense stress concentration and release, and high-density ion deintercalation and intercalation, which cause more severe damage to the material structure). This contributes to a higher overall cycle life of the battery.

[0071] Furthermore, the synergistic combination between the upper and lower layers can achieve layered constraints. That is, the rigid structure of the upper single-crystal particles can physically constrain the volume expansion of the lower polycrystalline particles, reduce the overall deformation of the electrode, and avoid current collector peeling or electrode cracking caused by large expansion.

[0072] As a non-limiting example, the method for obtaining material samples of the first and second positive electrode active material layers in the positive electrode sheet of a battery is as follows: The porosity of the positive electrode sheet is observed using an ion polishing cross-sectional morphology method. When significant fluctuations in porosity are observed, this indicates the boundary between the first and second positive electrode active material layers, thus determining the first and second positive electrode active material layers. In the first positive electrode active material layer, a sample with a thickness of 2 / 3 is taken from the side relatively far from the second positive electrode active material layer as the upper layer sample; in the second positive electrode active material layer, a sample with a thickness of 2 / 3 is taken from the side relatively far from the first positive electrode active material layer as the lower layer sample. The upper and lower layer samples are respectively immersed in a dimethyl carbonate (DMC) solution for washing and then filtered for separation to obtain material samples of the first and second positive electrode active material layers. These material samples can be used for subsequent testing.

[0073] As a non-limiting example, the nickel content of the first or second cathode material can be tested using equipment and methods known in the art. For example, a cross-sectional sample of the cathode sheet can be used to identify the first and second cathode active material particles, and the nickel content of each particle can be tested using an energy dispersive spectroscopy (EDS) instrument. Alternatively, the following method can be used: powder is scraped from the cathode sheet along its thickness to obtain material samples of either the first or second cathode active material layer. These samples are then subjected to inductively coupled plasma (ICP) testing. Based on the test results, the types of elements contained in the material sample and their respective mass content can be determined, and the nickel content can be calculated from the mass content.

[0074] As a non-limiting example, the particle morphology of the first and second positive electrode active material layers can be tested using the following method: a cross-sectional sample is cut along the thickness direction of the positive electrode sheet, and the cross-section of the sample is tested using a scanning electron microscope (SEM). At the same magnification, if the material particles of the first positive electrode active material layer are observed to be individually discretely distributed particles under the electron microscope, and there is basically no adhesion between the particles and very few grain boundaries, then the first positive electrode active material layer is a single crystal particle; if the material particles of the second positive electrode active material layer contain more regular, larger spherical secondary particles, which are composed of smaller primary particles bonded together, and there are obvious grain boundaries between the primary particles, then the surface of the second positive electrode active material layer contains polycrystalline particles.

[0075] In this application, the median particle size D50 of the material (such as single crystal particles or polycrystalline particles) refers to the count median particle size of the material. That is, when the particle size distribution of the material is sorted by particle size during particle size testing, the particle size corresponding to the cumulative particle size distribution percentage reaches 50%, that is, 50% of the particles have a particle size smaller than this value, and the other 50% of the particles have a particle size larger than this value.

[0076] As a non-limiting example, the average particle size of the positive electrode active material can be tested using equipment and methods known in the art. As an example, the average particle size of the positive electrode active material can be tested by obtaining cross-sectional scanning electron microscope (SEM) images of the positive electrode sheet using a scanning electron microscope (e.g., ZEISS Sigma 300), referring to JY / T010-1996. Specifically, the test can be conducted as follows: Randomly select a test sample with dimensions of 50mm x 100mm from the positive electrode sheet. Cut a cross-sectional sample of the electrode sheet. Randomly select multiple test areas (e.g., 5 areas) within the test sample. Under a certain magnification (e.g., 1000x when measuring the positive electrode active material), read the particle size of each positive electrode active material particle in each test area (i.e., take the distance between the two farthest points on the positive electrode active material particle as the particle size). Count the number and particle size values ​​of the positive electrode active material particles in each test area. Take the arithmetic mean of the positive electrode active material particles in each test area; this is the number-average particle size of the positive electrode active material particles in the test sample. To ensure the accuracy of the test results, the above test can be repeated with multiple test samples (e.g., 10 samples), and the average value of each test sample can be taken as the final test result.

[0077] In some embodiments, the nickel content of the first cathode material is greater than or equal to 50% and less than or equal to 98%, and the nickel content of the second cathode material is greater than or equal to 50% and less than or equal to 98%. For example, the nickel content of the first cathode material and the second cathode material can each be independently 50%, 53%, 55%, 57%, 59%, 61%, 63%, 65%, 67%, 69%, 73%, 75%, 77%, 79%, 81%, 83%, 85%, 87%, 89%, 91%, 93%, 95%, 97%, 98%, or within any range of the above values.

[0078] Ternary cathode materials with nickel content in the above range have a serious problem of oxygen release at the positive and negative electrode interfaces. Based on this, this application adopts an upper and lower layer combination design with a larger single crystal particle upper layer and a polycrystalline particle lower layer, which can achieve a better effect of reducing oxygen release at grain boundaries and improving safety performance, while also taking into account power performance to a certain extent.

[0079] In some embodiments, the first positive electrode material and the second positive electrode material each independently satisfy the chemical formula: Li x’ Ni x Co y M 1-x-y O y’ , wherein M comprises at least one of Mn, Al, B, Zr, Sr, Y, Sb, W, Ti, Mg, Zn and Nb, 0.5≤x≤0.98, 0<y≤0.4, 0.6≤x’≤1.2, and 1.6≤y’≤2.2. On the basis that the first positive electrode material and / or the second positive electrode material satisfy the chemical formula, the upper layer comprising large-sized single crystal particles and the lower layer comprising polycrystalline particles are used in a matching design, which can achieve a better improvement effect of reducing oxygen release from grain boundaries and improving safety performance, and can also give consideration to power performance to a certain extent.

[0080] In some embodiments, M comprises at least one of Mn, Al, B, Zr, Sr, W, Mg, Y and Nb. In this way, a better improvement effect of reducing oxygen release from grain boundaries and improving safety performance can be achieved, and the power performance can be better taken into account.

[0081] In some embodiments, the nickel content of the first positive electrode material is greater than or equal to 80% and less than or equal to 98%. For example, the nickel content of the first positive electrode material may be 80%, 82%, 84%, 86%, 88%, 90%, 92%, 94%, 96%, 98%, or within a range consisting of any of the above values.

[0082] In some embodiments, the nickel content of the second positive electrode material is greater than or equal to 80% and less than or equal to 98%. For example, the nickel content of the second positive electrode material may be 80%, 82%, 84%, 86%, 88%, 90%, 92%, 94%, 96%, 98%, or within a range consisting of any of the above values.

[0083] For the first positive electrode material or the second positive electrode material having a nickel content within the above range, the oxygen release problem at the positive and negative electrode interface is more serious; on this basis, the positive electrode sheet adopts a matching design of the upper layer comprising larger-sized single crystal particles and the lower layer comprising polycrystalline particles, which can not only achieve a more obvious improvement effect of reducing oxygen release from grain boundaries and improving safety performance, but also achieve the effect of giving consideration to power performance.

[0084] In some embodiments, the first positive electrode material satisfies the chemical formula: Li x1’ Ni x1 Co y1 M 1 1-x1-y1 O y1’ , wherein M 1comprises at least one of Mn, Al, B, Zr, Sr, Y, Sb, W, Ti, Mg, Zn, Y and Nb, 0.8≤x1≤0.98, 0<y1≤0.3, 0.6≤x1’≤1.2, 1.6≤y1’≤2.2. In some other embodiments, the second cathode material satisfies the chemical formula: Li x2’ Ni x2 Co y2 M 2 1-x2-y2 O y2’ , where M 2 comprises at least one of Mn, Al, B, Zr, Sr, W, Mg, Y and Nb, 0.8≤x2≤0.98, 0<y2≤0.3, 0.6≤x2’≤1.2, 1.6≤y2’≤2.2.

[0085] On the basis that the first cathode material and / or the second cathode material satisfy the above chemical formula, the design of matching the upper and lower layers, where the upper layer includes large-sized single crystal particles and the lower layer includes polycrystalline particles, can achieve a more significant improvement effect of reducing oxygen release at grain boundaries and improving safety performance, and can also give consideration to power performance to a certain extent.

[0086] In some embodiments, the first cathode material and the second cathode material each independently comprise LiNi 0.5 Co 0.2 Mn 0.3 O2 (also may be abbreviated as NCM 523 ), LiNi 0.5 Co 0.25 Mn 0.25 O2 (also may be abbreviated as NCM 211 ), LiNi 0.6 Co 0.2 Mn 0.2 O2 (also may be abbreviated as NCM 622 ), LiNi 0.8 Co 0.1 Mn 0.1 O2 (also may be abbreviated as NCM 811 ), and LiNi 0.9 Co 0.05 Mn 0.05 O2 (also may be abbreviated as NCM 955 ) or a combination thereof.

[0087] In some embodiments, the average particle size D501 of the first cathode material is greater than or equal to 2.8 μm and less than or equal to 7.5 μm. For example, D501 can be 2.8 μm, 3 μm, 3.1 μm, 3.3 μm, 3.5 μm, 3.7 μm, 3.9 μm, 4.1 μm, 4.3 μm, 4.5 μm, 4.7 μm, 4.9 μm, 5.1 μm, 5.3 μm, 5.5 μm, 5.7 μm, 5.9 μm, 6.1 μm, 6.3 μm, 6.5 μm, 6.7 μm, 6.9 μm, 7.1 μm, 7.3 μm, 7.5 μm, or within any range of the above values. Optionally, the average particle size D501 of the first cathode material is 4.5 μm to 6.5 μm.

[0088] D501 falling within the above range indicates that the size of the single crystal particles is relatively large, and the grain boundary area formed by the contact between these single crystal particles per unit volume is relatively small. As a result, the grain boundary reaction area for oxygen release reaction is small, and the resistivity of these relatively large single crystal particles is high. Under extreme conditions, such as high temperature, overcharging, needle penetration, lithium plating, and short circuits between positive and negative electrodes, the material can intrinsically reduce the intensity of electrochemical reactions and short circuit current at the positive and negative electrode interfaces, thereby reducing oxygen release and short circuit current and improving safety and reliability.

[0089] Furthermore, the relatively large single-crystal particles have a relatively low specific surface area, resulting in fewer side reactions with the electrolyte. They are also more pressure-resistant, less prone to breakage, and have higher structural stability. Additionally, the average particle size D501 of the single-crystal particles falls within the above range, resulting in fewer defects such as dislocations and slips within the crystal lattice during charging and discharging, and better internal lattice stability. This improves the reversibility of the material's charge-discharge cycle performance, facilitating a better balance between cycle life and performance.

[0090] In some embodiments, the average particle size D502 of the second cathode material is 7 μm to 15 μm, and can be selected as 9 μm to 12 μm. For example, D502 can be 7 μm, 7.3 μm, 7.6 μm, 7.9 μm, 8.2 μm, 8.4 μm, 8.8 μm, 9.1 μm, 9.4 μm, 9.8 μm, 10.2 μm, 10.6 μm, 10.9 μm, 11.2 μm, 11.6 μm, 11.9 μm, 12.2 μm, 12.6 μm, 12.9 μm, 13.2 μm, 13.6 μm, 13.9 μm, 14.2 μm, 14.6 μm, 14.9 μm, 15 μm, or within any range of the above values. This configuration allows for a better overall balance between cathode kinetic performance and energy density; it also enables better integration with the upper single-crystal particles, further improving safety, reliability, and cycle life.

[0091] In some embodiments, the particle size distribution span1 of the first positive electrode material is 1.5 to 2.5. For example, span1 can be 1.5, 1.6, 1.7, 1.8, 1.9, 2, 2.1, 2.2, 2.3, 2.4, 2.5 or within any of the above values.

[0092] When span1 is within the above range, it indicates that the crystal grain size of the upper single-crystal particles is relatively uniform. This not only helps to achieve a higher compaction density of the electrode, but also allows the upper single-crystal particles to form a better particle size distribution with the lower polycrystalline particles at the upper and lower layer interface, enhancing the cohesion of the electrode. At the same time, the upper single-crystal particles, as a "buffer layer," can homogenize the lithium-ion flow due to their relatively uniform crystal grain size, reducing local polarization and lithium plating. On this basis, combined with the higher diffusion rate of lithium ions by the lower polycrystalline particles, lithium ions can be quickly transported to the near current collector end, thereby helping to reduce the overall internal resistance of the electrode.

[0093] In some embodiments, the particle size distribution span2 of the positive electrode material in the second positive electrode active material layer is 1.1~3.0. For example, span2 can be 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, or any value within the range above. This setting not only facilitates achieving a higher compaction density of the electrode, but also allows the lower layer particles to form a better particle size distribution with the upper layer single crystal particles at the upper and lower layer interface, enhancing the cohesion of the electrode. Simultaneously, it also achieves a better matching effect with the upper layer single crystal particles, which helps reduce the overall internal resistance of the electrode and further improves safety, reliability, and cycle life. Furthermore, span2 within the above range can reduce or even avoid damage to the lower layer current collector (such as aluminum foil) and the generation of burrs from cutting.

[0094] It is understood that in this application, the cathode material in the second cathode active material layer can be the second cathode material or a mixture of the second cathode material and the third cathode material.

[0095] As a non-limiting example, the particle size distribution span1 of the first positive electrode material or the particle size distribution span2 of the positive electrode material in the second positive electrode active material layer can be tested using the following method: Powder is scraped from the positive electrode sheet along its thickness direction to obtain material samples of either the first or second positive electrode active material layer. The material samples obtained by the above method are then measured using a laser particle size analyzer, referring to GB / T19077-2016. The testing instrument can be a Mastersizer 3000 laser particle size analyzer from Malvern Instruments Ltd., UK.

[0096] In some embodiments, the particle size distribution span 2' of the second positive electrode material is 1.1 to 1.8. For example, span 2' can be 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, or any value within the range above. This setting facilitates better particle size distribution between the lower polycrystalline particles and the upper monocrystalline particles at the interface between the upper and lower layers, enhancing the cohesion of the electrode. Simultaneously, it also achieves better matching with the upper monocrystalline particles, which helps reduce the overall internal resistance of the electrode and further improves safety, reliability, and cycle life.

[0097] In some embodiments, the mass ratio of the first cathode material to the second cathode material is (5:95) to (40:60), optionally (10:90) to (40:60), and further optionally (10:90) to (30:100). For example, this mass ratio can be 5:95, 10:90, 13:90, 17:90, 21:90, 24:90, 28:90, 21:65, 33:90, 35:90, 24:65, 29:65, 33:65, 35:65, 40:60, or within any range of the above values. This setting facilitates a better matching effect between the upper monocrystalline particles and the lower polycrystalline particles, and can better balance safety performance and energy density.

[0098] As a non-limiting example, when the second positive electrode active material layer only includes the second positive electrode material, the mass ratio of polycrystalline particles in the first positive electrode material to that in the second positive electrode material can be tested by the following method: Take a positive electrode active material layer with a fixed area (e.g., 1mm × 1mm), separate the first positive electrode active material layer and the second positive electrode active material layer, and weigh them separately. Record the masses as m1 and m2, respectively. By comparing m1:m2, the mass ratio of polycrystalline particles in the first positive electrode material to that in the second positive electrode material can be obtained.

[0099] In some embodiments, the second positive electrode active material layer further includes a third positive electrode material having a single-crystal particle morphology, wherein the nickel content of the third positive electrode material is greater than or equal to 50%. In this case, the lower layer includes a mixture of medium-high nickel polycrystalline particles and medium-high nickel single-crystal particles. The combination of medium-high nickel polycrystalline particles and medium-high nickel single-crystal particles can improve lithium-ion transport, thereby facilitating further optimization of power performance.

[0100] In some embodiments, the nickel content of the third cathode material is 1% to 3% higher than that of the second cathode material. For example, the nickel content of the third cathode material may be 1%, 1.3%, 1.6%, 1.9%, 2.2%, 2.6%, 2.8%, 3% higher than that of the second cathode material, or fall within any range of these values. This facilitates further improvement in lithium-ion transport, thereby promoting further optimization of power performance.

[0101] In some embodiments, the nickel content of the third cathode material is greater than or equal to 50% and less than or equal to 98%; for example, the nickel content of the third cathode material can be 50%, 53%, 55%, 57%, 59%, 61%, 63%, 65%, 67%, 69%, 73%, 75%, 77%, 79%, 81%, 83%, 85%, 87%, 89%, 91%, 93%, 95%, 97%, 98%, or within any range of the above values.

[0102] Ternary cathode materials with nickel content in the above range have a serious problem of oxygen release at the positive and negative electrode interfaces. Based on this, this application adopts an upper layer consisting of larger single crystal particles and a lower layer consisting of a mixture of polycrystalline and single crystal particles. This design can achieve a better effect of reducing oxygen release at grain boundaries and improving safety performance, while also taking into account power performance.

[0103] In some embodiments, the nickel content of the third cathode material is greater than or equal to 80% and less than or equal to 98%. For example, the nickel content of the third cathode material can be 80%, 82%, 84%, 86%, 88%, 90%, 92%, 94%, 96%, 98%, or within any range of these values. Thus, based on a high nickel content, by employing an upper layer comprising larger single-crystal particles and a lower layer comprising a mixture of polycrystalline and single-crystal particles, further improvements in reducing oxygen release at grain boundaries and enhancing safety performance can be achieved, while also better balancing power performance.

[0104] In some embodiments, the third cathode material satisfies the chemical formula: Li x3’ Ni x3 Co y3 M 31-x3-y3 O y3’ The M 3 Includes at least one of Mn, Al, B, Zr, Sr, W, Mg, Y, and Nb, 0.5 ≤ x³ ≤ 0.98, 0 <y3≤0.4,0.6≤x3’≤1.2,1.6≤y3’≤2.2。

[0105] In some implementations, 0.8 ≤ x3 ≤ 0.98, 0 <y3≤0.3,0.6≤x3’≤1.2,1.6≤y3’≤2.2。

[0106] In some embodiments, the third cathode material includes LiNi 0.5 Co 0.2 Mn 0.3 O2 (also known as NCM) 523 LiNi 0.5 Co 0.25 Mn 0.25 O2 (also known as NCM) 211 LiNi 0.6 Co 0.2 Mn 0.2 O2 (also known as NCM) 622 LiNi 0.8 Co 0.1 Mn 0.1 O2 (also known as NCM) 811 ) and LiNi 0.9 Co 0.05 Mn 0.05 O2 (also known as NCM) 955 One or more of the following.

[0107] In some embodiments, the mass ratio of the second positive electrode material to the third positive electrode material in the second positive electrode active material layer is (1:9) to (5:5). For example, this mass ratio can be 1:9, 1:5, 2:9, 3:9, 2:5, 4:9, 5:9, 3:5, 6:9, 7:9, 4:5, 8:9, 5:5, or any range of the above values. This setting facilitates a better matching effect between the polycrystalline and single-crystal particles in the lower layer, which is beneficial for further improvement in power performance and energy density.

[0108] In some embodiments, the average particle size of the third cathode material is D503, and D503 / D502 = 0.2~0.5. For example, D503 / D502 can be 0.2, 0.3, 0.4, 0.5, or within any range of these values. This setting facilitates a better matching effect between the polycrystalline and monocrystalline particles in the lower layer, thereby better balancing energy density and power performance.

[0109] As a non-limiting example, D503 / D502 can be tested using the average particle size testing method described above. Specifically, a cross-sectional sample of the positive electrode sheet is obtained, and the particles of the second and third positive electrode materials in the second positive electrode active material layer are calibrated. The average particle size of each type of particle is measured to obtain the D503 of the third positive electrode material and the D502 of the second positive electrode material.

[0110] In some embodiments, the first positive electrode material accounts for 5% to 95% of the mass of the positive electrode active material layer. For example, this mass percentage can be 5%, 7%, 9%, 11%, 17%, 23%, 28%, 31%, 37%, 43%, 49%, 52%, 58%, 63%, 67%, 74%, 77%, 86%, 89%, 91%, 95%, or any of the above values.

[0111] By adjusting the mass ratio of the upper single-crystal particles in the positive electrode active material layer, the film resistance of the positive electrode sheet can be controlled. Furthermore, by adjusting this mass ratio within the above range, the film resistance of the positive electrode sheet can be adjusted to a suitable range (such as 0.35Ω~0.6Ω). This not only helps to reduce the occurrence of short circuits within the electrode sheet and improve its safety performance, but also helps to take into account the lithium-ion diffusion kinetics, thereby achieving a balance between safety performance and power performance.

[0112] In some embodiments, the film resistance of the positive electrode is 0.35Ω to 0.6Ω. For example, the film resistance of the positive electrode can be 0.35Ω, 0.37Ω, 0.39Ω, 0.41Ω, 0.43Ω, 0.46Ω, 0.48Ω, 0.51Ω, 0.53Ω, 0.55Ω, 0.57Ω, 0.59Ω, 0.6Ω, or within any range of the above values. This configuration, under conditions such as extreme high temperatures, lithium plating, and internal short circuits, helps to reduce the intensity of electrochemical reactions and short-circuit current at the positive and negative electrode interfaces from the inherent properties of the materials, thereby reducing oxygen release and Joule heating, and improving safety and reliability.

[0113] It is understandable that the film resistance of the positive electrode can be achieved not only by adjusting the mass ratio of the upper single crystal particles in the positive electrode active material layer, but also by adjusting at least one of the following methods: the type and content of the conductive agent in the upper and / or lower layers of the positive electrode active material layer, and the type and content of the binder.

[0114] As a non-limiting example, the film resistance of the positive electrode can be tested using the following method: The positive electrode removed from the battery is measured using a film resistance tester, and the specific process is as follows:

[0115] 1) Cut the electrode to a size greater than four times the probe spacing and input the test area A of the terminal;

[0116] 2) The probe is in vertical contact with the sample surface, and a stable pressure (0.6T) is applied for a time interval of 10 seconds;

[0117] 3) Record the voltage U and current I, and calculate the resistance of the diaphragm (area A): ρ = U / I.

[0118] In some embodiments, the electrolyte of the secondary battery includes a weak solvating solvent, wherein the solvation energy of the weak solvating solvent at 25°C and 101 kPa is less than or equal to 150 kJ / mol, and the ionic conductivity of the electrolyte at 25°C is greater than or equal to 10 mS / cm.

[0119] For example, the solvation capacity can be 150 kJ / mol, 139 kJ / mol, 128 kJ / mol, 117 kJ / mol, 96 kJ / mol, 85 kJ / mol, 74 kJ / mol, 63 kJ / mol, 52 kJ / mol, 41 kJ / mol, 30 kJ / mol, 29 kJ / mol, 27 kJ / mol, 24 kJ / mol, 21 kJ / mol, 19 kJ / mol, 17 kJ / mol, 14 kJ / mol, 11 kJ / mol, 9 kJ / mol, 7 kJ / mol, 5 kJ / mol, 3 kJ / mol, 1 kJ / mol, etc.

[0120] The electrolyte includes the aforementioned weak solvation solvent, which can affect the solvation structure of lithium ions, thereby affecting the desolvation kinetics of lithium ions, reducing the desolvation energy barrier of lithium ions at the electrode interface, and improving the low-temperature high-voltage performance of the battery. Based on this, the weak solvation solvent is combined with the upper and lower electrode design of this application, which includes large-size single crystal particles on the upper layer and polycrystalline particles on the lower layer, and an electrolyte with relatively high ionic conductivity (corresponding to an ionic conductivity of the electrolyte greater than or equal to 10 mS / cm) is used, which is beneficial to balancing the kinetics of the cell system and improving safety performance.

[0121] As a non-limiting example, the solvation ability of the weak solvation solvent can be tested using the following method: Gas chromatography-mass spectrometry (GC-MS) and Fourier transform infrared (FTIR) are performed on the obtained electrolyte to determine the type of weak solvation solvent; LiPF6 is dissolved in a solvent of the same type as the weak solvation solvent to prepare a 0.5 mol / L electrolyte; the electrolyte is sealed in a quartz cuvette; Raman spectroscopy is used (laser wavelength of 532 nm or 785 nm, integration time of 10–60 seconds, spectral range of 200 nm). -1 ~2000cm-1 The spectra of the pure weak solvating solvent and the 0.5 mol / L electrolyte were measured and recorded. By comparing the shifts of the characteristic peaks of the solvent in the pure weak solvating solvent and the aforementioned electrolyte, the solvent coordination state was determined. The more obvious the shift of the characteristic peaks of the solvent molecules to higher frequencies in the electrolyte, the stronger the coordination between the solvent and the ions, and the higher the solvation energy.

[0122] In some embodiments, the electrolyte has an ionic conductivity of 10 mS / cm to 14 mS / cm at 25°C. For example, the ionic conductivity of the electrolyte at 25°C can be 10 mS / cm, 11 mS / cm, 12 mS / cm, 13 mS / cm, 14 mS / cm, or any value within the range above. This results in a better match between the electrolyte and the upper and lower electrode design of this application, which includes large-size single-crystal particles on the upper layer and polycrystalline particles on the lower layer, facilitating better balance of the cell system dynamics and improving safety performance.

[0123] The ionic conductivity of an electrolyte is a well-known concept in the art and can be tested using instruments and methods known in the art. For example, the following method can be used for testing: First, pretreat the electrolyte by heating the electrolyte to be tested to the test temperature and the standard solution to 25°C (with a deviation of ±0.1°C); then, calibrate the instrument using the two standard solutions at 25°C. After calibration and cleaning the electrodes, vertically place the test sample electrode into the electrolyte to be tested and start the test using a conductivity meter. Record the test results after the data has stabilized for more than 10 seconds to obtain the ionic conductivity of the electrolyte.

[0124] In some embodiments, the weak solvating solvent includes one or more of carbonate solvents, sulfite solvents, and carboxylic acid ester solvents. The inclusion of these types of weak solvating solvents is beneficial for further improving the low-temperature, high-voltage performance of the battery.

[0125] In some embodiments, carbonate solvents include one or more of ethylene carbonate, propylene carbonate, ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butene carbonate, and fluoroethylene carbonate (FEC).

[0126] In some embodiments, the carboxylic acid ester solvent includes one or more of methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, methyl butyrate, and ethyl butyrate.

[0127] In some embodiments, sulfite solvents include one or two of vinyl sulfite (ES), propylene sulfite, dimethyl sulfite, and diethyl sulfite.

[0128] In some embodiments, the weakly solvating solvent constitutes 10% to 30% of the volume of the electrolyte. For example, this volume percentage can be 10%, 12%, 14%, 16%, 18%, 20%, 21%, 23%, 25%, 27%, 29%, 30%, or any value within the range above. This configuration further improves the battery's low-temperature, high-voltage performance and better balances the cell system dynamics, thereby enhancing safety performance.

[0129] In some embodiments, the electrolyte further includes additives, including one or more of the following: ethylene carbonate, lithium difluorooxalate borate, succinic anhydride, lithium difluorophosphate, ethylene carbonate, fluoroethylene carbonate, propylene sulfite, vinyl sulfate, propylene-1,3-sulfonyl lactone, and methanedisulfonate. These additives can improve battery performance, such as improving high-temperature or low-temperature performance.

[0130] In some embodiments, the additive accounts for 0.1% to 0.5% of the mass of the electrolyte. For example, the mass percentage of the additive in the electrolyte can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, or any range thereof. Based on the upper and lower electrode design of this application, which includes large-size single-crystal particles on the upper layer and polycrystalline particles on the lower layer, by controlling the additive content within this range, the film thickness of the electrolyte interface film (CEI film and / or SEI film) can be reduced, which helps to reduce the positive electrode impedance and improve power performance while improving the stability of the positive electrode.

[0131] In addition, the secondary battery and power-consuming device of this application will be described below with appropriate reference to the accompanying drawings.

[0132] Typically, a secondary battery consists of a positive electrode, a negative electrode, an electrolyte, and a separator. During charging and discharging, active ions move back and forth between the positive and negative electrodes, inserting and releasing. The electrolyte acts as a conductor between the positive and negative electrodes. The separator, positioned between the positive and negative electrodes, primarily prevents short circuits while allowing ions to pass through.

[0133] Positive electrode sheet

[0134] As a non-limiting example, the positive current collector has two surfaces opposite each other in its own thickness direction, and the positive active material layer is disposed on either or both of the two opposite surfaces of the positive current collector.

[0135] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymeric material substrate and a metal layer formed on at least one surface of the polymeric material substrate. The composite current collector can be obtained by forming a metal material on a polymeric material substrate. Non-limiting examples of the metal material in the positive electrode current collector may include one or more of aluminum, aluminum alloys, nickel, nickel alloys, titanium, titanium alloys, silver, and silver alloys. Non-limiting examples of the polymeric material substrate in the positive electrode current collector may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).

[0136] Understandably, lithium (Li) is intercalated and deintercalated during the charging and discharging process of a battery, and the Li content in the positive electrode varies depending on the state of discharge. Unless otherwise specified, the Li content in the examples of positive electrode materials listed in this application refers to the initial state of the material. When a positive electrode material is applied to a positive electrode in a battery system, the Li content in the positive electrode material typically changes after charge-discharge cycles. The Li content can be measured using molar content, but is not limited to this. Regarding "Li content refers to the initial state of the material," the initial state of the material refers to its state before being added to the positive electrode slurry. It is understood that new materials obtained by appropriately modifying the listed positive electrode materials are also within the scope of positive electrode materials. The aforementioned appropriate modification refers to acceptable modification methods for the positive electrode material; non-limiting examples include coating modification.

[0137] In the examples of cathode materials in this application, the oxygen (O) content is only a theoretical value. Lattice oxygen release will cause changes in the molar content of oxygen, and the actual O content will fluctuate. The O content can be measured in molar content, but is not limited to this.

[0138] In some embodiments, the positive electrode active material layer may optionally include a binder. As a non-limiting example, the binder may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), PVDF-tetrafluoroethylene-propylene terpolymer, PVDF-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorinated acrylate resins.

[0139] In some embodiments, the positive electrode active material layer may optionally include a conductive agent. As a non-limiting example, the conductive agent may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0140] In some embodiments, the positive electrode sheet can be prepared by dispersing the components used to prepare the positive electrode sheet, such as the positive active material, conductive agent, binder, and any other components, in a solvent to form a positive electrode slurry; coating the positive electrode slurry onto at least one surface of the positive electrode current collector, and obtaining the positive electrode sheet after drying, cold pressing, and other processes. The solvent can be selected from, but is not limited to, any of the solvents described in the foregoing embodiments, such as N-methylpyrrolidone (NMP). The surface of the positive electrode current collector coated with the positive electrode slurry can be a single surface of the positive electrode current collector or both surfaces of the positive electrode current collector. The solid content of the positive electrode slurry can be 40wt%~80wt%. The viscosity of the positive electrode slurry at room temperature can be adjusted to 5000~25000 mPa·s. When coating the positive electrode slurry, the coating areal density (dry weight, minus solvent) can be 15~35 mg / cm². 2 The compaction density of the positive electrode sheet can be 3.0~3.6 g / cm³. 3 The concentration can be selected as 3.3~3.5 g / cm³. 3 .

[0141] Negative electrode sheet

[0142] The negative electrode sheet includes a negative current collector and a negative active material layer disposed on at least one surface of the negative current collector, wherein the negative active material layer includes a negative active material.

[0143] As a non-limiting example, the negative electrode current collector has two surfaces opposite each other in its own thickness direction, and the negative electrode active material layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.

[0144] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymeric material substrate and a metal layer formed on at least one surface of the polymeric material substrate. The composite current collector can be obtained by forming a metal material on the polymeric material substrate. Non-limiting examples of the metal material in the negative electrode current collector may include one or more of copper, copper alloys, nickel, nickel alloys, titanium, titanium alloys, silver, and silver alloys. Non-limiting examples of the polymeric material substrate in the negative electrode current collector may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).

[0145] In some embodiments, the negative electrode active material may be a negative electrode active material known in the art for use in batteries. As a non-limiting example, the negative electrode active material may include one or more of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate, etc. Silicon-based materials may include one or more of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. Tin-based materials may include one or more of elemental tin, tin oxide compounds, and tin alloys. However, this application is not limited to these materials, and other conventional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0146] In some embodiments, the negative electrode active material layer may optionally include a binder. The binder may include one or more of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0147] In some embodiments, the negative electrode active material layer may optionally include a conductive agent. The conductive agent may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0148] In some embodiments, the negative electrode active material layer may also optionally include other additives, such as thickeners (e.g., sodium carboxymethyl cellulose (CMC-Na)).

[0149] In some embodiments, the negative electrode sheet can be prepared by dispersing the components used to prepare the negative electrode sheet, such as the negative electrode active material, conductive agent, binder, and any other components, in a solvent (a non-limiting example of a solvent is deionized water) to form a negative electrode slurry; coating the negative electrode slurry onto at least one surface of a negative electrode current collector, and then obtaining the negative electrode sheet after drying, cold pressing, and other processes. The surface of the negative electrode current collector coated with the negative electrode slurry can be a single surface of the negative electrode current collector or both surfaces of the negative electrode current collector. The solid content of the negative electrode slurry can be 40wt%~60wt%. The viscosity of the negative electrode slurry at room temperature can be adjusted to 2000~10000 mPa·s. When coating the negative electrode slurry, the coating unit areal density (dry weight, minus solvent) can be 75~220 g / m². 2 The compaction density of the negative electrode sheet can be 1.0 g / cm³. 3 ~1.8g / cm 3 .

[0150] electrolytes

[0151] Electrolytes function to conduct ions between the positive and negative electrode plates. This application does not impose any particular restrictions on the type of electrolyte; it can be selected according to requirements. For example, the electrolyte can be liquid, semi-solid, or fully solid.

[0152] In some embodiments, the electrolyte is an electrolyte solution. The electrolyte solution includes an electrolyte salt and a solvent.

[0153] In some embodiments, the electrolyte salt may include one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorophosphate (LiPO2F2), lithium difluorooxalate borate (LiDFOB), lithium dioxalate borate (LiBOB), lithium difluorodioxalate phosphate (LiDFOP), and lithium tetrafluorooxalate phosphate (LiTFOP).

[0154] Separating membrane

[0155] In some embodiments, the secondary battery also includes a separator. This application does not impose any particular limitation on the type of separator; any known porous separator with good chemical and mechanical stability can be selected.

[0156] In some embodiments, the material of the separator may include one or more of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator may be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer may be the same or different, without particular limitation.

[0157] In some embodiments, the thickness of the isolation membrane is 6~40μm, optionally 12~20μm.

[0158] In some embodiments, the positive electrode, negative electrode, and separator can be fabricated into an electrode assembly using a winding process or a stacking process.

[0159] In some embodiments, the secondary battery may include an outer packaging. This outer packaging may be used to encapsulate the electrode assembly and electrolyte described above.

[0160] In some embodiments, the outer packaging of the secondary battery can be a rigid shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery can also be a soft pack, such as a pouch-type soft pack. The material of the soft pack can be plastic; further, non-limiting examples of plastic may include one or more of polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0161] A secondary battery includes at least one battery cell. A secondary battery may include one or more battery cells.

[0162] In this application, unless otherwise specified, "cell battery" refers to the basic unit capable of converting chemical energy into electrical energy, and generally includes at least a positive electrode, a negative electrode, and an electrolyte. During the charging and discharging process of the battery, active ions move back and forth between the positive and negative electrode plates, inserting and extracting. The electrolyte acts as a conductor for the active ions between the positive and negative electrode plates.

[0163] This application does not impose any particular limitation on the shape of the battery cell; it can be cylindrical, square, or any other arbitrary shape. For example, Figure 2 The example shown is a square-structured battery cell 5.

[0164] In some of these embodiments, reference is made to Figure 3 The outer packaging may include a housing 51 and a cover 53. The housing 51 may include a base plate and side plates connected to the base plate, the base plate and side plates forming a receiving cavity. The housing 51 has an opening communicating with the receiving cavity, and the cover 53 can be placed over the opening to close the receiving cavity. The positive electrode, negative electrode, and separator may be formed into an electrode assembly 52 by a winding process or a stacking process. The electrode assembly 52 is encapsulated within the receiving cavity. Electrolyte is immersed in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the battery cell 5 may be one or more, which can be selected by those skilled in the art according to actual needs.

[0165] The secondary battery can be either battery device 4 or battery pack 1.

[0166] The battery device includes at least one battery cell. The number of battery cells in the battery device can be one or more, and those skilled in the art can select an appropriate number according to the application and capacity of the battery device.

[0167] Figure 4 This is battery device 4, used as an example. (See reference...) Figure 4 In the battery assembly 4, multiple battery cells 5 can be arranged sequentially along the length of the battery assembly 4. Of course, they can also be arranged in any other manner. Furthermore, the multiple battery cells 5 can be fixed in place using fasteners.

[0168] Optionally, the battery device 4 may also include a housing with a receiving space in which multiple battery cells 5 are received.

[0169] In some embodiments, the battery devices described above can also be assembled into a battery pack, and the number of battery devices contained in the battery pack can be one or more. Those skilled in the art can select an appropriate number according to the application and capacity of the battery pack.

[0170] Figure 5 and Figure 6 This is battery pack 1 as an example. (See reference...) Figure 5 and Figure 6 The battery pack 1 may include a battery box and multiple battery devices 4 disposed within the battery box. The battery box includes an upper body 2 and a lower body 3, with the upper body 2 covering the lower body 3 to form a closed space for accommodating the battery devices 4. The multiple battery devices 4 can be arranged in any manner within the battery box.

[0171] In addition, this application also provides an electrical device, which includes the secondary battery provided in this application. The secondary battery can be used as the power source of the electrical device or as the energy storage unit of the electrical device. The electrical device may include, but is not limited to, mobile devices, electric vehicles, electric trains, ships and satellites, energy storage systems, etc. Among them, mobile devices may be, for example, mobile phones, laptops, etc.; electric vehicles may be, for example, pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc., but are not limited to.

[0172] As an electrical device, a rechargeable battery can be selected based on its usage requirements.

[0173] Figure 7 Here is an example of an electrical device 6. This electrical device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. To meet the high power and high energy density requirements of the secondary battery for this electrical device, a battery pack or battery device can be used.

[0174] Another example device could be a mobile phone, tablet, or laptop. These devices typically require a slim and lightweight design and can use a rechargeable battery as their power source.

[0175] Example

[0176] The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where the technology or conditions are not specified in the embodiments, they are performed according to the technology or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.

[0177] Example 1

[0178] (1) Preparation of positive electrode sheet

[0179] (1.1) The first cathode material LiNi 0.80 Co 0.13 Mn 0.07O2 single-crystal particles, conductive carbon black (Super P), and binder polyvinylidene fluoride (PVDF) were mixed uniformly in N-methylpyrrolidone (NMP) solvent at a mass ratio of 98.1:0.8:1.1 to obtain a first positive electrode slurry with a viscosity of 10000 mPa·s (corresponding to the first positive electrode active material layer, i.e., the upper layer). The single-crystal particles had a D501 of 5 μm and a span1 of 1.8.

[0180] (1.2) The second cathode material LiNi 0.80 Co 0.13 Mn 0.07 Polycrystalline O2 particles, conductive carbon black (Super P), and binder polyvinylidene fluoride (PVDF) were mixed uniformly in N-methylpyrrolidone (NMP) solvent at a mass ratio of 98.1:0.8:1.1 to obtain a second positive electrode slurry with a viscosity of 10000 mPa·s (corresponding to the second positive electrode active material layer, i.e., the lower layer). The polycrystalline particles had a D502 of 11 μm and a span2 of 1.6.

[0181] (1.3) Two positive electrode slurries are coated onto opposite surfaces of the positive electrode current collector aluminum foil using a double-layer coating machine. After drying, cold pressing, slitting, and cutting, a positive electrode sheet comprising a first positive electrode active material layer (i.e., the upper layer) and a second positive electrode active material layer (i.e., the lower layer) is obtained. The coating amount per unit area of ​​both the first and second positive electrode active material layers on each side is 0.27 g / 1540.25 mm. 2 Furthermore, the weight ratio of the second positive electrode active material layer to the first positive electrode active material layer is 70:30, meaning the mass ratio of the lower layer to the upper layer is 70:30, and the mass ratio of polycrystalline particles in the lower layer to single-crystal particles in the upper layer is 70:30. The film resistance of the positive electrode sheet is 385mΩ.

[0182] (2) Preparation of negative electrode sheet

[0183] Artificial graphite (negative electrode active material), sodium carboxymethyl cellulose (thickener), styrene-butadiene rubber (binder), and acetylene black (conductive agent) were mixed in a mass ratio of 96.9:1.15:1.4:0.55. Deionized water was added, and a negative electrode slurry with a solid content of 55% was obtained under vacuum stirring. The negative electrode slurry was uniformly coated on both sides of a copper foil. After the copper foil was dried at room temperature, it was transferred to a 120°C oven for 1 hour. Then, it was cold-pressed and slit to obtain the negative electrode sheet, with a coating amount of 0.17 g / 1540.25 mm² on both sides. 2 .

[0184] (3) Separating membrane

[0185] The base film is a 7μm thick polyethylene film, coated with a 1.5μm Al2O3 ceramic coating on both sides.

[0186] (4) Preparation of electrolyte

[0187] The solvent was a mixture of ethylene carbonate (EC), diethyl carbonate (DEC), and dimethyl carbonate (DMC), with a volume ratio of EC, DEC, and DMC of 2:1:1. The thoroughly dried lithium salt LiPF6 was dissolved in the organic solvent and mixed thoroughly in an argon-atmospheric glove box with a water content of <10 ppm to obtain the electrolyte. The concentration of the lithium salt was 1 mol / L; the solvation energy of the solvent at 25 °C and 101 kPa was 135 kJ / mol; and the ionic conductivity of the electrolyte at 25 °C was 10 mS / cm.

[0188] (5) Battery manufacturing

[0189] The positive electrode, separator, and negative electrode are stacked and wound in sequence to obtain an electrode assembly. The electrode assembly is placed in an outer packaging, dried, and then injected with electrolyte. After vacuum sealing, settling, formation, and shaping, a lithium-ion battery is obtained.

[0190] Example 2

[0191] Similar to the preparation method in Example 1, the main difference is that in step (1.1), single crystal particles with D501=3.2μm are used to replace the original single crystal particles, and the span1 of the replaced single crystal particles is 1.5, as detailed in Table 3 below.

[0192] Example 3

[0193] Similar to the preparation method in Example 1, the main difference is that in step (1.2), the polycrystalline particles are replaced with polycrystalline particles (D502=11μm) and single-crystal particles (D503=5μm, and satisfying the chemical formula LiNi). 0.80 Co 0.13 Mn 0.07 The mixture of O2) is such that the mass ratio of polycrystalline particles to single-crystal particles is 7:1, where D503 / D502≈0.46. At the same time, in step (1.3), the mass ratio of the lower layer to the upper layer is 80:20, and the mass ratio of polycrystalline particles in the lower layer to single-crystal particles in the upper layer is 70:20, as detailed in Table 1 below.

[0194] Examples 4-7

[0195] Similar to the preparation method in Example 1, the main difference is that in step (1.3), the mass ratio of the lower layer to the upper layer is 90:10, 95:5, 65:35, and 60:40, respectively, and correspondingly the mass ratio of polycrystalline particles in the lower layer to single crystal particles in the upper layer is 90:10, 95:5, 65:35, and 60:40, respectively, as detailed in Table 1 below; in Table 1, span2' refers to the particle size distribution of polycrystalline particles in the lower layer; " / " indicates that the value does not exist.

[0196] Table 1

[0197]

[0198] Example 8

[0199] Similar to the preparation method in Example 1, the main difference is that in step (1.1), the first cathode material in the upper layer is replaced with LiNi. 0.5 Co 0.2 Mn 0.3 O2, see Table 2 below for details.

[0200] Table 2

[0201]

[0202] Examples 9-10

[0203] Similar to the preparation method in Example 1, the main difference is that in step (1.1), single crystal particles with D501 of 2.8 μm and 7.5 μm are used to replace the original single crystal particles in the upper layer, and the span1 of the replaced single crystal particles are 1.4 and 1.9, respectively, as detailed in Table 3 below.

[0204] Table 3

[0205]

[0206] Examples 11-12

[0207] Similar to the preparation method in Example 3, the main difference is that in step (1.2), the mass ratio of polycrystalline particles to single crystal particles in the lower layer is 9:1 and 5:5, respectively, as detailed in Tables 4-1 and 4-2 below; in Tables 4-1 and 4-2, span2' refers to the particle size distribution of polycrystalline particles in the lower layer.

[0208] Table 4-1

[0209]

[0210] Table 4-2

[0211]

[0212] Examples 13-14

[0213] Similar to the preparation method in Example 1, the main difference is that in step (1.2), the lower layer uses polycrystalline particles with D502 of 7μm and 15μm to replace the original polycrystalline particles, and the span2 of the replaced polycrystalline particles is 1.5, as detailed in Table 5 below; in Table 5, span2' refers to the particle size distribution of the polycrystalline particles in the lower layer.

[0214] Table 5

[0215]

[0216] Examples 15-16

[0217] Similar to the preparation method in Example 3, the main difference is that in step (1.2), the average particle size D503 of the lower single crystal particles is 2.2 μm and 5.5 μm, the D503 / D502 ratio is 0.2 and 0.5, and the span2 ratio is 1.58 and 1.64, as detailed in Tables 6-1 and 6-2 below; in Tables 6-1 and 6-2, span2' refers to the particle size distribution of the polycrystalline particles in the lower layer.

[0218] Table 6-1

[0219]

[0220] Table 6-2

[0221]

[0222] Comparative Example 1

[0223] The preparation method is similar to that in Example 1, with the main difference being that the positive electrode active material layer is a single layer composed of a mixture of single-crystal particles and polycrystalline particles, and its preparation process is as follows:

[0224] (1.1) The ternary cathode material LiNi 0.80 Co 0.13 Mn 0.07 O2, conductive carbon black (Super P), and binder polyvinylidene fluoride (PVDF) were mixed uniformly in N-methylpyrrolidone (NMP) solvent at a mass ratio of 98.1:0.8:1.1 to obtain a positive electrode slurry with a viscosity of 10000 Pa·s. The ternary positive electrode material is a mixture of single-crystal and polycrystalline particles. The single-crystal particles have a D501 = 5 μm and span1 = 1.8; the polycrystalline particles have a D502 = 11 μm and span2 = 1.6; and the mass ratio of polycrystalline to single-crystal particles is 70:30.

[0225] (1.2) The positive electrode slurry is coated onto the opposing surfaces of the positive electrode current collector aluminum foil. After drying, cold pressing, slitting, and cutting, a positive electrode sheet containing a positive electrode active material layer is obtained. The coating amount per unit area of ​​the positive electrode active material layer on each side is 0.27 g / 1540.25 mm. 2 The film resistance of the positive electrode is 293mΩ, as detailed in Table 1 above.

[0226] Comparative Example 2

[0227] Similar to the preparation method in Example 1, the main difference is that in step (1.1), single crystal particles with D501=1.8μm are used to replace the original single crystal particles, and the span1 of the replaced single crystal particles is 1.2, as detailed in Table 3 above.

[0228] It should be noted that in the tables above, span1 represents the particle size distribution of the upper first cathode material (i.e., single crystal particles), span2' represents the particle size distribution of the lower second cathode material (i.e., polycrystalline particles), and span2 represents the overall particle size distribution of the lower cathode material (i.e., when the lower layer is the second cathode material, it represents the particle size distribution of the second cathode material; when the lower layer is a mixture of the second and third cathode materials, it represents the overall particle size distribution of the second and third cathode materials).

[0229] Test section

[0230] (1) Capacity test

[0231] At 25°C, the battery is charged to 4.20V with a constant current of 0.33C, then charged to 0.05C with a constant voltage of 5.0V, and left to stand for 10 minutes; then discharged to 2.50V with a current of 0.33C, and left to stand for 10 minutes. The resulting capacity is recorded as capacity C0.

[0232] (2) Direct Current Resistance (DCR) Test

[0233] At 25℃, the battery was charged to 4.20V with a current of 0.33C, and then charged to 0.05C with a constant voltage of 5.0V. The battery was then left to stand for 10 minutes. The battery was then discharged with a constant current of 0.33C for 60 minutes to adjust the battery to 50% SOC. The battery voltage at this time was recorded as U1. The battery was then discharged with a constant current of 4C for 10 seconds. The instantaneous voltage U2 at 10 seconds of discharge was recorded. The initial DCR of the battery was represented by the discharge DCR at 50% SOC. The initial DCR of the battery was calculated as (U1-U2) / 4C, where C is the nominal capacity of the battery.

[0234] (3) Energy density test

[0235] At 25℃, discharge to the lower limit voltage in the form of constant current discharge (0.33C rate), let stand for 30 minutes, then charge to the upper limit cutoff voltage in the form of constant current and constant voltage charging (constant current 0.33C, constant voltage charging to 0.05C), let stand for 30 minutes, and measure the discharge energy E (in Wh). Repeat 3 times and take the average value of the discharge energy E of the 3 times as E0. Divide it by the volume V of the hard-shell battery cell, and the volumetric energy density (in Wh / L) = E0 / V.

[0236] (4) Overcharge test

[0237] Charge the battery to 4.20V at a current of 0.33C, then charge it at a constant voltage of 5.0V to a current of 0.05C, and let it stand for 10 minutes. Continue charging at a current of 0.33C until the battery voltage reaches 1.5 times the upper limit voltage (4.20V) or fails (thermal runaway), and record the SOC (state of charge) of the battery at this time.

[0238] (5) Needle prick test

[0239] Charge the battery to 4.20V at a current of 0.33C, then charge it at a constant voltage of 4.20V to a current of 0.05C, and let it stand for 10 minutes.

[0240] Needle penetration procedure: Penetrate the positive terminal until the needle voltage reaches above 0.5V (determining that the needle tip has contacted the cell surface), continue penetrating to a depth of 6mm, and maintain for 1 hour. Record the time of failure and the battery temperature rise.

[0241] (6) Hot box test

[0242] Charge the battery to 4.20V at a current of 0.33C and let it stand for 10 minutes. Store it in a high-temperature chamber and heat it at a rate of 5℃ / min. When the temperature reaches 130℃, hold it for 60 minutes. Then heat it by 5℃ and hold it for 60 minutes until the temperature reaches 150℃ or thermal runaway occurs. Hold it for 60 minutes. Record the temperature and time when the failure occurs.

[0243] The table above, comparing Examples 1-16 with Comparative Example 1, shows that compared to a single-layer cathode active material layer mixed with monocrystalline and polycrystalline particles, the upper and lower layer design of this application, comprising a first cathode material with monocrystalline particle morphology on the upper layer and a second cathode material with polycrystalline particle morphology on the lower layer, enables the battery to have improved safety performance. The comparison between Examples 1-16 and Comparative Example 2 shows that controlling the average particle size of the first cathode material within a suitable range not only improves battery safety performance but also helps to balance capacity and cycle performance.

[0244] The description of the various embodiments above tends to emphasize the differences between the various embodiments. The similarities or similarities between them can be referred to, and for the sake of brevity, they will not be repeated here.

[0245] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.

Claims

1. A secondary battery, characterized in that, include: A positive electrode sheet, the positive electrode sheet comprising a positive current collector and a positive active material layer disposed on at least one surface of the positive current collector, the positive active material layer comprising a first positive active material layer and a second positive active material layer, the second positive active material layer being disposed between the positive current collector and the first positive active material layer; The first positive electrode active material layer includes a first positive electrode material with a single crystal particle morphology, the nickel content of the first positive electrode material is greater than or equal to 50%, and the average particle size D501 of the first positive electrode material is greater than or equal to 2.8 μm; The second positive electrode active material layer includes a second positive electrode material with a polycrystalline particle morphology, and the nickel content of the second positive electrode material is greater than or equal to 50%.

2. The secondary battery according to claim 1, characterized in that, The nickel content of the first cathode material and the second cathode material is independently greater than or equal to 50% and less than or equal to 98%; Optionally, the first positive electrode material and the second positive electrode material each independently satisfy the chemical formula: Li x’ Ni x Co y M 1-x-y O y’ , wherein M comprises at least one of Mn, Al, B, Zr, Sr, Y, Sb, W, Ti, Mg, Zn and Nb, 0.5≤x≤0.98, 0<y≤0.4, 0.6≤x’≤1.2, 1.6≤y’≤2.2; further optionally, the M comprises at least one of Mn, Al, B, Zr, Sr, W, Mg, Y and Nb.

3. The secondary battery according to claim 1 or 2, characterized in that, One or more of the following conditions must be met: (1) The nickel content of the first positive electrode material is greater than or equal to 80% and less than or equal to 98%; Optionally, the first cathode material satisfies the chemical formula: Li x1’ Ni x1 Co y1 M 1 1-x1-y1 O y1’ The M 1 Includes at least one of Mn, Al, B, Zr, Sr, W, Mg, Y, and Nb, 0.8 ≤ x1 ≤ 0.98, 0 <y1≤0.3,0.6≤x1’≤1.2,1.6≤y1’≤2.2; (2) The nickel content of the second cathode material is greater than or equal to 80% and less than or equal to 98%; Optionally, the second cathode material satisfies the chemical formula: Li x2’ Ni x2 Co y2 M 2 1-x2-y2 O y2’ The M 2 Includes at least one of Mn, Al, B, Zr, Sr, W, Mg, Y, and Nb, 0.8 ≤ x² ≤ 0.98, 0 <y2≤0.3,0.6≤x2’≤1.2,1.6≤y2’≤2.2。 4. The secondary battery according to any one of claims 1 to 3, characterized in that, One or more of the following conditions must be met: (1) The average particle size D501 of the first positive electrode material is 2.8 μm to 7.5 μm, and can be selected as 4.5 μm to 6.5 μm; (2) The average particle size D502 of the second positive electrode material is 7μm~15μm, and can be selected as 9μm~12μm.

5. The secondary battery according to any one of claims 1 to 4, characterized in that, One or more of the following conditions must be met: (1) The particle size distribution span 1 of the first positive electrode material is 1.5~2.5; (2) The particle size distribution span2' of the second positive electrode material is 1.1~1.

8.

6. The secondary battery according to any one of claims 1 to 5, characterized in that, The mass ratio of the first positive electrode material to the second positive electrode material is (5:95) to (40:60), and can be selected as (10:90) to (40:60).

7. The secondary battery according to any one of claims 1 to 6, characterized in that, The second positive electrode active material layer also includes a third positive electrode material with a single crystal particle morphology, wherein the nickel content of the third positive electrode material is greater than or equal to 50%; Optionally, the nickel content of the third cathode material is 1% to 3% higher than that of the second cathode material; Optionally, in the second positive electrode active material layer, the mass ratio of the third positive electrode material to the second positive electrode material is (1:9) to (5:5); Optionally, the average particle size of the second cathode material is D502, and the average particle size of the third cathode material is D503, where D503 / D502 = 0.2~0.

5.

8. The secondary battery according to claim 7, characterized in that, The nickel content of the third cathode material is greater than or equal to 50% and less than or equal to 98%. Optionally, the third cathode material satisfies the chemical formula: Li x3’ Ni x3 Co y3 M 3 1-x3-y3 O y3’ The M 3 Includes at least one of Mn, Al, B, Zr, Sr, W, Mg, Y, and Nb, 0.5 ≤ x³ ≤ 0.98, 0 <y3≤0.4,0.6≤x3’≤1.2,1.6≤y3’≤2.2; Further optionally, the nickel content of the third cathode material is greater than or equal to 80% and less than or equal to 98%; Further alternatively, 0.8 ≤ x3 ≤ 0.98, 0 <y3≤0.3,0.6≤x3’≤1.2,1.6≤y3’≤2.2。 9. The secondary battery according to any one of claims 1 to 8, characterized in that, One or more of the following conditions must be met: (1) The first positive electrode material accounts for 5% to 95% of the mass of the positive electrode active material layer; (2) The particle size distribution span2 of the positive electrode material in the second positive electrode active material layer is 1.1~3.

0.

10. The secondary battery according to any one of claims 1 to 9, characterized in that, The film resistance of the positive electrode is 0.35Ω~0.6Ω.

11. The secondary battery according to any one of claims 1 to 10, characterized in that, The electrolyte of the secondary battery includes a weak solvation solvent, wherein the solvation energy of the weak solvation solvent at 25°C and 101 kPa is less than or equal to 150 kJ / mol, and the ionic conductivity of the electrolyte at 25°C is greater than or equal to 10 mS / cm. Optionally, the weak solvating solvent includes one or more of carbonate solvents, sulfite solvents, and carboxylic acid ester solvents; Optionally, the volume percentage of the weakly solvating solvent in the electrolyte is 10% to 30%; Optionally, the electrolyte has an ionic conductivity of 10 mS / cm to 14 mS / cm at 25°C.

12. The secondary battery according to claim 11, characterized in that, The electrolyte also includes additives, which include one or more of the following: ethylene carbonate, lithium difluorooxalate borate, succinate, lithium difluorophosphate, ethylene carbonate, fluoroethylene carbonate, propylene sulfite, ethylene sulfate, propylene-1,3-sulfonyl lactone, and methane disulfonate. Optionally, the additive accounts for 0.1% to 0.5% of the mass of the electrolyte.

13. An electrical appliance, characterized in that, Includes the secondary battery as described in any one of claims 1 to 12.