Secondary battery, method for manufacturing secondary battery, negative electrode sheet, and electric device

By setting a second negative electrode active material layer in the negative electrode sheet of a lithium-ion battery and coating the surface of the additive with a one-dimensional conductive agent, the problem of poor charging ability of lithium-ion batteries in low-temperature environments is solved. This enables rapid desolvation and intercalation of lithium ions at low temperatures, suppresses additive expansion, and improves the low-temperature charge and discharge performance of the battery.

CN123162271APending Publication Date: 2026-11-24CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510677612.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-23
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Lithium-ion batteries have poor charging capabilities at low temperatures, especially below 0°C, which is mainly due to increased electrolyte viscosity, slow lithium-ion migration speed, high interfacial impedance, and increased desolvation energy barrier, resulting in battery life degradation and slow charging speed under low temperature conditions.

Method used

A second negative electrode active material layer is set in the negative electrode sheet, and a one-dimensional conductive agent, including elemental tin, tin compounds and tin-containing alloys, is set on the surface of the additive. The additive is linearly wrapped by the one-dimensional conductive agent, which improves the lithium intercalation potential, reduces the lithium-ion desolvation energy barrier, inhibits the expansion of the additive, and improves the low-temperature charging performance.

Benefits of technology

To improve the charging capability of lithium-ion batteries in low-temperature environments, reduce the impact of additive expansion on cell capacity decay, and enhance the low-temperature charge and discharge performance of batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123162271A_ABST
    Figure CN123162271A_ABST
Patent Text Reader

Abstract

The application relates to a secondary battery, a preparation method of the secondary battery, a negative electrode sheet and an electric device. The secondary battery comprises a negative electrode sheet, the negative electrode sheet comprises a negative electrode current collector, a first negative electrode active material layer located on at least one side surface of the negative electrode current collector, and a second negative electrode active material layer located on a side surface of the first negative electrode active material layer away from the negative electrode current collector; the negative electrode active material layer comprises a first negative electrode active material, the second negative electrode active material layer comprises a second negative electrode active material and an additive, and a one-dimensional conductive agent is arranged on the surface of the delivery agent; the lithium intercalation potential of the first negative electrode active material and the second negative electrode active material at 25 DEG C is independently <1.2 V (Vs. Li + / Li), and the additive comprises one or more of tin element, a tin compound and a tin-containing alloy. By arranging the second negative electrode active material layer in the negative electrode sheet, the low-temperature charging capacity of the secondary battery can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of secondary battery technology, and in particular to a secondary battery, a method for preparing the secondary battery, a negative electrode sheet, and an electrical device. Background Technology

[0002] In recent years, with the increasingly widespread application of lithium-ion batteries, they have been widely used in energy storage systems such as hydropower, thermal power, wind power, and solar power plants, as well as in power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace, and many other fields. However, the application of lithium-ion batteries in low-temperature environments at high latitudes faces challenges. At lower temperatures, especially below 0°C, the low-temperature charging capability of lithium-ion batteries is poor, making it difficult to meet the growing demand. Summary of the Invention

[0003] This application provides a secondary battery, a method for preparing the secondary battery, a negative electrode sheet, and an electrical device.

[0004] To achieve the above objectives, a first aspect of this application provides a secondary battery, including a negative electrode, said negative electrode comprising:

[0005] Negative electrode current collector;

[0006] A first negative electrode active material layer is located on at least one side surface of the negative electrode current collector, and the first negative electrode active material layer comprises a first negative electrode active material; and

[0007] The second negative electrode active material layer is located on the surface of the first negative electrode active material layer away from the negative electrode current collector. The second negative electrode active material layer includes a second negative electrode active material and an additive. A one-dimensional conductive agent is disposed on the surface of the additive.

[0008] The lithium intercalation potentials of the first and second negative electrode active materials at 25°C are each independently < 1.2V (Vs. Li). + / Li), the additive includes one or more of elemental tin, tin compounds and tin-containing alloys.

[0009] Therefore, this application provides a second negative electrode active material layer in the negative electrode sheet, and the second negative electrode active material layer contains an additive with a one-dimensional conductive agent disposed on its surface. On the one hand, the additive has a conductivity greater than 1.2V (Vs. Li). + The lithium intercalation potential of Li ( / Li) during secondary battery charging or negative electrode lithium intercalation is less than 1.2V (Vs. Li) +Compared to Li-based negative electrode active materials, additives preferentially achieve lithium intercalation, increasing the lithium intercalation potential of the negative electrode and suppressing potential polarization to reach the lithium plating potential (0V). This is especially beneficial in low-temperature environments where the negative electrode voltage can decrease rapidly during charging. Furthermore, additives themselves can lower the lithium-ion desolvation energy barrier, enabling rapid desolvation and intercalation of lithium ions into the additive at low temperatures. Therefore, adding additives can improve the low-temperature charging capability of secondary batteries. Simultaneously, by setting a one-dimensional conductive agent on the surface of the additive, the expansion of the additive itself during charging and discharging can be reduced, minimizing repeated expansion and contraction during cycling. This inhibits the detachment of the additive from the conductive network due to its own expansion and contraction, reducing the impact of additive introduction on cell capacity decay.

[0010] In some embodiments of this application, the one-dimensional conductive agent includes one or more of carbon nanotubes, carbon fibers, metal fibers, and conductive polymer fibers. This facilitates the linear confinement of the additive.

[0011] In some embodiments of this application, the carbon nanotubes include one or more of single-walled carbon nanotubes and multi-walled carbon nanotubes.

[0012] In some alternative embodiments, the carbon nanotubes are single-walled carbon nanotubes. Single-walled carbon nanotubes have good electrical conductivity and, compared to multi-walled carbon nanotubes, a smaller mass percentage and better dispersibility.

[0013] In some embodiments of this application, the carbon nanotubes have a diameter of 0.5 nm to 100 nm and a length of 10 μm to 1000 μm. When the diameter and length of the carbon nanotubes are within the above ranges, the carbon nanotubes have suitable mechanical strength and stability, and at the same time have suitable encapsulation strength for additives, thereby reducing the occurrence of carbon nanotubes detaching from the surface of the additives and losing their binding effect.

[0014] In some embodiments of this application, the tin compound includes one or more of SnO2, SnO, SnS, and SnF.

[0015] In some embodiments of this application, the tin-containing alloy includes one or more of tin-bismuth alloy, lithium-tin alloy, tin-copper alloy, tin-silver alloy, tin-selenium alloy, tin-tellurium alloy, and sodium-tin alloy.

[0016] In some embodiments of this application, the mass percentage of the one-dimensional conductive agent relative to the mass of the additive is 1%-105%.

[0017] In some embodiments of this application, the mass percentage of the one-dimensional conductive agent relative to the mass of the additive is 2%-100%. This is advantageous in balancing the binding effect of the one-dimensional conductive agent on the additive, the conductivity of the one-dimensional conductive agent, and the low-temperature charge / discharge capability of the additive.

[0018] In some embodiments of this application, the sum of the mass percentages of the additive and the one-dimensional conductive agent in the second negative electrode active material layer is 0.1%-11%.

[0019] In some embodiments of this application, the combined mass percentage of the additive and the one-dimensional conductive agent in the second negative electrode active material layer is 0.2%-10%. This not only facilitates the effectiveness of the additive but also reduces the impact of additive expansion on the electrode or battery.

[0020] In some embodiments of this application, the sum of the mass percentages of the additive and the one-dimensional conductive agent in the second negative electrode active material layer is 1%-10%.

[0021] In some embodiments of this application, the second negative electrode active material includes one or more of graphite negative electrode materials and silicon-based negative electrode materials.

[0022] In some embodiments of this application, the second negative electrode active material includes a graphite negative electrode material and a silicon-based negative electrode material, wherein the graphite negative electrode material has a mass percentage content of ≥80% based on the total mass of the graphite negative electrode material and the silicon-based negative electrode material. Therefore, the additive has a greater advantage in graphite negative electrode systems with high graphite content and high initial efficiency, further enhancing the effectiveness of the additive.

[0023] In some embodiments of this application, the graphite anode material comprises first graphite particles, the first graphite particles having a Dv50 of 10μm-16μm and a specific surface area of ​​2m². 2 / g-6m 2 / g, OI value ≤3.5. The first graphite particles have small particle size and OI value, which is beneficial for ion transport in the negative electrode active material, thereby further improving the fast charging performance of the battery.

[0024] In some embodiments of this application, the first graphite particles account for 25%-75% of the mass of the graphite anode material. This is beneficial for the anode sheet to have a larger specific surface area and porosity, thereby improving the low-temperature charge-discharge performance of the battery.

[0025] In some embodiments of this application, the first graphite particles account for 50%-75% of the mass of the graphite anode material.

[0026] In some embodiments of this application, the silicon-based anode material has a Dv50 of 15μm-20μm and a specific surface area of ​​1m². 2 / g-5m 2 / g. Therefore, silicon-based anode materials have a large lithium insertion / delithiation area, numerous reaction sites, and superior kinetic performance.

[0027] In some embodiments of this application, the first negative electrode active material and the second negative electrode active material may be the same or different.

[0028] In some embodiments of this application, the secondary battery includes a positive electrode sheet, the positive electrode sheet includes a positive active material layer, the positive active material layer contains a positive active material, and the initial coulombic efficiency of the positive active material in a lithium metal half-cell is ≤90% at 25°C. Therefore, positive active materials with lower initial efficiency have poor low-temperature charging performance, allowing additives to better enhance their low-temperature charging performance in this system; simultaneously, positive active materials with lower initial efficiency have more lithium to compensate for lithium loss caused by additives.

[0029] In some embodiments of this application, the positive electrode active material includes one or more of lithium nickel cobalt manganese oxide, lithium nickel oxide, and lithium manganese oxide.

[0030] In some embodiments of this application, the general chemical formula of the positive electrode active material is Li. 1+d [Ni x Co y Mn z M1 e O2, where 0.5≤x≤1, 0<y<0.3, 0<z≤1, 0<d<0.2, 0<e<0.2, x+y+z+e=1, and M1 is one or more of Mg, Ca, Sb, Ce, Ti, Zr, Sr, Al, Zn, Mo, and B.

[0031] In some embodiments of this application, the secondary battery is a lithium-ion battery.

[0032] A second aspect of this application provides a method for preparing a secondary battery, the method comprising the step of preparing a negative electrode sheet, wherein the preparation of the negative electrode sheet includes:

[0033] A first negative electrode active material layer is formed on at least one side surface of the negative electrode current collector, the first negative electrode active material layer comprising a first negative electrode active material;

[0034] A one-dimensional conductive agent is linearly coated on the surface of an additive, wherein the additive includes one or more of elemental tin, tin compounds, and tin-containing alloys;

[0035] A second negative electrode slurry is prepared, the second slurry comprising a second negative electrode active material and the additive having the one-dimensional conductive agent linearly coated on its surface;

[0036] The second negative electrode slurry is applied to the surface of the first negative electrode active material layer on the side away from the negative electrode current collector to form the second negative electrode active material layer;

[0037] The lithium intercalation potentials of the first and second negative electrode active materials at 25°C are each independently < 1.2V (Vs. Li). + / Li).

[0038] In some embodiments of this application, the mass ratio of the one-dimensional conductive agent to the additive is (2-100):100. Therefore, the one-dimensional conductive agent can linearly encapsulate the additive, providing better binding of the additive.

[0039] In some embodiments of this application, the additive has a Dv50 of 1 μm-15 μm and a Dv99 of <40 μm. Therefore, the particle size of the additive is close to or smaller than that of the negative electrode active material, resulting in better lithium insertion / deintercalation kinetics and thus contributing to further improvement in low-temperature charge / discharge performance.

[0040] In some embodiments of this application, the step of linearly coating a one-dimensional conductive agent onto the surface of the additive includes:

[0041] The dispersion containing the one-dimensional conductive agent is mixed with the additive and then spray-dried to linearly coat the one-dimensional conductive agent on the surface of the additive.

[0042] In some embodiments of this application, the solvent of the dispersion includes one or more of water, polyvinyl alcohol, polyacrylic acid, such as polyethylene glycol, polyvinylpyrrolidone, N-methylpyrrolidone, and dimethyl sulfoxide.

[0043] In some embodiments of this application, the one-dimensional conductive agent accounts for 0.2%-5% of the mass of the dispersion. This results in a more stable dispersion of the one-dimensional conductive agent, which is more beneficial for subsequent coating processing.

[0044] A third aspect of this application provides a negative electrode sheet, comprising:

[0045] Negative electrode current collector;

[0046] A first negative electrode active material layer is located on at least one side surface of the negative electrode current collector, and the negative electrode active material layer comprises a first negative electrode active material; and

[0047] The second negative electrode active material layer is located on the surface of the first negative electrode active material layer away from the negative electrode current collector. The second negative electrode active material layer includes a second negative electrode active material and an additive. A one-dimensional conductive agent is disposed on the surface of the additive.

[0048] The lithium intercalation potentials of the first and second negative electrode active materials at 25°C are each independently < 1.2V (Vs. Li). + / Li), the additive includes one or more of elemental tin, tin compounds and tin-containing alloys.

[0049] In some embodiments of this application, the negative electrode is the negative electrode in the secondary battery of the first aspect of this application.

[0050] The fourth aspect of this application provides an electrical device, including one or more of the secondary battery of the first aspect of this application and the secondary battery prepared by the preparation method of the second aspect of this application.

[0051] The electrical device of this application includes the secondary battery provided in this application, and therefore has at least the same advantages as the secondary battery.

[0052] Details of one or more embodiments of this application are set forth in the following drawings and description. Other features, objects, and advantages of this application will become apparent from the specification, drawings, and claims. Attached Figure Description

[0053] To better describe and illustrate the embodiments or examples provided in this application, reference may be made to one or more accompanying drawings. Additional details or examples used to describe the drawings should not be considered as limiting the scope of any of the disclosed applications, the currently described embodiments or examples, or the best mode of conduct of these applications as currently understood. Furthermore, the same reference numerals denote the same parts throughout the drawings. In the drawings:

[0054] Figure 1 This is a scanning electron microscope image of SnS (SnS@CNT) with linearly coated carbon nanotubes on its surface, as shown in Example 1.

[0055] Figure 2 This is a schematic diagram of a battery cell according to one embodiment of this application.

[0056] Figure 3 for Figure 2 An exploded view of a battery cell according to one embodiment of this application is shown.

[0057] Figure 4 This is a schematic diagram of a battery module according to one embodiment of this application.

[0058] Figure 5This is a schematic diagram of a battery pack according to one embodiment of this application.

[0059] Figure 6 for Figure 5 An exploded view of a battery pack according to one embodiment of this application is shown.

[0060] Figure 7 This is a schematic diagram of an electrical device that uses a secondary battery as a power source according to an embodiment of this application.

[0061] Explanation of reference numerals in the attached figures:

[0062] 1 Battery pack; 2 Upper housing; 3 Lower housing; 4 Battery module; 5 Battery cell; 51 Housing; 52 Electrode assembly; 53 Cover plate; 6 Electrical device. Detailed Implementation

[0063] The following describes in detail, with appropriate reference to the accompanying drawings, some embodiments of the secondary battery, the method for preparing the secondary battery, the negative electrode plate, and the electrical device of this application. However, some unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of actually identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided to enable those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.

[0064] The "range" disclosed in this application can be defined in the form of a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints; any endpoint can be independently included or excluded, and they can be combined arbitrarily, meaning any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values ​​1 and 2 are listed, and maximum range values ​​3, 4, and 5 are also listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0" and "5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when describing a parameter as an integer ≥ 2, it is equivalent to listing integers such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, and 12 for that parameter. For instance, when describing a parameter as an integer selected from "2-10", it is equivalent to listing the integers 2, 3, 4, 5, 6, 7, 8, 9, and 10.

[0065] In this application, the terms "multiple" or "various" are used unless otherwise specified, referring to a quantity greater than or equal to 2. For example, "one or more" means one or more types.

[0066] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.

[0067] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment or implementation of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments. The term "implementation" as used herein has a similar understanding.

[0068] Those skilled in the art will understand that the order in which the steps are written in the methods of various embodiments or examples does not imply a strict execution order and does not constitute any limitation on the implementation process. The detailed execution order of each step should be determined by its function and possible internal logic. Unless otherwise specified, all steps of this application may be performed sequentially or randomly, preferably sequentially. For example, if the method includes steps (a) and (b), it means that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, if the method may also include step (c), it means that step (c) can be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.

[0069] In this application, unless otherwise specified, A (e.g., B) means that B is a non-limiting example of A, and it is understood that A is not limited to B.

[0070] In this application, "optionally," "optionally," and "optional" mean that something is optional, that is, it means that it is selected from either "with" or "without." If there are multiple "optional" entries in a technical solution, unless otherwise specified and there are no contradictions or mutual constraints, each "optional" entry shall be independent.

[0071] The application of lithium-ion batteries in low-temperature environments at high latitudes faces challenges. At lower temperatures, especially below 0°C, lithium-ion batteries exhibit poor low-temperature charging capabilities, failing to meet the increasing demand. This is because, under low-temperature conditions, especially below 0°C, electrolyte viscosity increases, lithium-ion migration speed slows down, interfacial impedance increases, and the desolvation barrier rises, leading to a significant reduction in battery life and slow charging speed at low temperatures. Research has found that introducing tin-containing delivery agents into the electrodes can improve the low-temperature charging capability of batteries. However, due to the expansion of the delivery agent itself during charge and discharge, repeated expansion and contraction during cycling can cause the delivery agent to detach from the conductive network, affecting battery capacity decay.

[0072] To address the aforementioned issues, this application introduces a one-dimensional conductive agent that can linearly wrap around the surface of the delivery agent, thereby enhancing the binding effect on the delivery agent. This not only improves the low-temperature charging performance of the battery but also effectively suppresses defects caused by the expansion and detachment of the delivery agent from the conductive network, such as the failure of the improvement effect on the low-temperature charging performance of the battery and the impact on battery capacity decay.

[0073] One or more embodiments of this application provide a secondary battery, including a negative electrode sheet. The negative electrode sheet includes a negative current collector, a first negative active material layer located on at least one side surface of the negative current collector, and a second negative active material layer located on the side surface of the first negative active material layer away from the negative current collector. The first negative active material layer contains a first negative active material, and the second negative active material layer contains a second negative active material and an additive. A one-dimensional conductive agent is disposed on the surface of the delivery agent. The lithium intercalation potential of the first and second negative active materials at 25°C is independently <1.2V (Vs. Li). + / Li), the additives include one or more of elemental tin, tin compounds and tin-containing alloys.

[0074] It should be noted that the terms "first negative electrode active material," "second negative electrode active material," "first negative electrode active material layer," and "second negative electrode active material layer" mentioned in the context are for descriptive purposes only and should not be construed as indicating or implying relative importance or quantity, nor should they be construed as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first," "second," etc., serve only as a non-exhaustive enumeration and should be understood as not constituting a closed limitation on quantity.

[0075] The “lithium insertion potential” mentioned in the context refers to the voltage value of the negative electrode active material in a lithium-ion battery relative to the reference electrode (such as Li⁺ / Li) during the lithium insertion (or delithiation) process.

[0076] Additives can deliver lithium ions and promote lithium ion migration.

[0077] As a non-limiting example, a one-dimensional conductive agent is linearly wrapped around the additive surface. In this context, "linearly wrapped" means that the one-dimensional conductive agent is wrapped in a line around the additive surface, and that the one-dimensional conductive agent does not completely cover the additive surface, but only covers a portion of it.

[0078] By linearly coating the surface of the additive with a one-dimensional conductive agent, the binding of the additive can be enhanced while the additive can be exposed, ensuring direct contact and intercalation between the additive and the electrolyte and lithium ions, thereby accelerating the desolvation of lithium ions.

[0079] Understandably, this application provides a second negative electrode active material layer in the negative electrode sheet, and the second negative electrode active material layer contains an additive with a one-dimensional conductive agent disposed on its surface. On the one hand, the additive has a conductivity greater than 1.2V (Vs. Li). + The lithium intercalation potential of Li ( / Li) during secondary battery charging or negative electrode lithium intercalation is less than 1.2V (Vs. Li) +Compared to Li-based negative electrode active materials, additives preferentially achieve lithium intercalation, increasing the lithium intercalation potential of the negative electrode and suppressing potential polarization to reach the lithium plating potential (0V). This is especially beneficial in low-temperature environments where the negative electrode voltage can decrease rapidly during charging. Furthermore, additives themselves can lower the lithium-ion desolvation energy barrier, enabling rapid desolvation and intercalation of lithium ions into the additive at low temperatures. Therefore, adding additives can improve the low-temperature charging capability of secondary batteries. Simultaneously, by setting a one-dimensional conductive agent on the surface of the additive, the expansion of the additive itself during charging and discharging can be reduced, minimizing repeated expansion and contraction during cycling. This inhibits the detachment of the additive from the conductive network due to its own expansion and contraction, reducing the impact of additive introduction on cell capacity decay.

[0080] Without limitation, the composition of the second negative electrode active material layer mentioned in the context, as well as the structural relationship between the additives and the one-dimensional conductive agent, can be determined by the following method: the secondary battery is split to obtain the negative electrode sheet, the negative electrode sheet is cut by focused ion beam (FIB) or argon ion polishing machine (Ar+) to obtain the second negative electrode active material layer on the side of the negative electrode sheet away from the negative electrode current collector, the electrode sheet cross section is adhered to conductive double-sided tape or silver tape, the sample is fixed on the sample stage, the composition of the second negative electrode active material layer is determined by X-ray energy dispersive spectroscopy (EDS), and the distribution relationship between the additives and the one-dimensional conductive agent is observed by scanning electron microscopy (SEM).

[0081] In some embodiments, the one-dimensional conductive agent includes one or more of carbon nanotubes, carbon fibers, metal fibers, and conductive polymer fibers. This facilitates the linear confinement of the additive.

[0082] As one possible implementation, carbon nanotubes include one or more of single-walled carbon nanotubes and multi-walled carbon nanotubes. Optionally, the carbon nanotubes are single-walled carbon nanotubes. Single-walled carbon nanotubes have good electrical conductivity and, compared with multi-walled carbon nanotubes, have a smaller mass percentage and better dispersibility.

[0083] In some embodiments, the diameter of the carbon nanotubes is 0.5nm-100nm; for example, it can be, but is not limited to, 0.5nm, 1nm, 5nm, 10nm, 15nm, 20nm, 25nm, 30nm, 35nm, 40nm, 45nm, 50nm, 55nm, 60nm, 65nm, 70nm, 75nm, 80nm, 85nm, 90nm, 95nm, 100nm, or any range between two of the above diameters.

[0084] As one possible implementation, the length of the carbon nanotubes is 10μm-1000μm; for example, it can be, but is not limited to, 10μm, 50μm, 100μm, 150μm, 200μm, 250μm, 300μm, 350μm, 400μm, 450μm, 500μm, 550μm, 600μm, 650μm, 700μm, 750μm, 800μm, 850μm, 900μm, 950μm, 1000μm or any range between two of the above lengths.

[0085] When the diameter and length of carbon nanotubes are within the above-mentioned ranges, the carbon nanotubes have suitable mechanical strength and stability, and at the same time have suitable encapsulation strength for additives, thereby reducing the occurrence of carbon nanotubes falling off the surface of the additives and losing their binding effect.

[0086] In some embodiments, the tin compound includes one or more of SnO2, SnO, SnS, and SnF.

[0087] As one possible implementation, the tin-containing alloy includes one or more of the following: tin-bismuth alloy, lithium-tin alloy, tin-copper alloy, tin-silver alloy, tin-selenium alloy, tin-tellurium alloy, and sodium-tin alloy.

[0088] As one possible implementation, the mass percentage of the one-dimensional conductive agent relative to the mass of the additive is 1%-105%.

[0089] In some embodiments, the mass percentage of the one-dimensional conductive agent relative to the mass of the additive is 2%-100%; for example, it can be, but is not limited to, 2%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 100%, or any range between two of the above percentages. When the mass percentage of the one-dimensional conductive agent relative to the mass of the additive is within the above range, it is advantageous to balance the binding effect of the one-dimensional conductive agent on the additive, the conductivity of the one-dimensional conductive agent, and the low-temperature charge-discharge capability of the additive.

[0090] In some embodiments, the combined mass percentage of the additive and the one-dimensional conductive agent in the second negative electrode active material layer is 0.1%-11%.

[0091] As one possible implementation, the sum of the mass percentages of the additive and the one-dimensional conductive agent in the second negative electrode active material layer is 0.2%-10%; for example, it can be, but is not limited to, 0.2%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10%, or any range between two of the above values. When the sum of the mass percentages of the additive and the one-dimensional conductive agent in the second negative electrode active material layer is within the above range, it is beneficial for the additive to play its role, while also reducing the impact of additive expansion on the electrode or battery.

[0092] In some alternative implementations, the combined mass percentage of the additive and the one-dimensional conductive agent in the second negative electrode active material layer is 1%-10%.

[0093] Without limitation, the mass percentage of the one-dimensional conductive agent and additives mentioned in the context in the second negative electrode active material layer can be determined by the following method: The secondary battery is disassembled to obtain the negative electrode sheet. The negative electrode sheet is cut using a focused ion beam (FIB) or argon ion polisher (Ar+) to obtain the powder of the second negative electrode active material layer on the side of the negative electrode sheet away from the negative electrode current collector. The powder is adhered to conductive double-sided tape or silver tape, and the sample is fixed on the sample stage. The characteristic element Sn of the additive and the mass percentage a of C on the surface of the additive are found by scanning electron microscopy (SEM) and energy dispersive X-ray spectroscopy (EDS). Then, a mass n of powder is taken from the second negative electrode active material layer and digested using a mixture of concentrated hydrochloric acid and concentrated nitric acid at a volume ratio of 1:3. The mass m of the additive in the material is determined by inductively coupled plasma atomic emission spectrometry (ICP), and the mass of the one-dimensional conductive agent on the surface of the additive is m×a. Therefore, the mass percentage of the one-dimensional conductive agent in the second active material layer is (m×a) / n, and the mass percentage of the additive in the second active material layer is (mm×a) / n.

[0094] In some embodiments, the second negative electrode active material includes one or more of graphite negative electrode materials and silicon-based negative electrode materials.

[0095] It should be noted that the term "graphite anode material" mentioned in the context may include at least one of natural graphite, artificial graphite, and modified graphite; modified graphite includes modified graphite with surface coatings (such as amorphous carbon, metal oxides, etc.).

[0096] The “silicon-based anode material” mentioned in the context may include at least one of nano-silicon, silicon oxide, silicon-carbon composite material and porous silicon.

[0097] As one possible implementation, the second negative electrode active material includes graphite negative electrode material and silicon-based negative electrode material, with the graphite negative electrode material accounting for ≥80% of the total mass of the graphite negative electrode material and silicon-based negative electrode material. Therefore, additives have a greater advantage in graphite negative electrode systems with high graphite content and high initial efficiency, further enhancing the effectiveness of the additives.

[0098] It should be noted that the type and amount of the second negative electrode active material mentioned in the context can be determined by the following method: the secondary battery is split to obtain the negative electrode sheet, the negative electrode sheet is cut by focused ion beam (FIB) or argon ion polishing machine (Ar+) to obtain the second negative electrode active material layer powder on the side of the negative electrode sheet away from the negative electrode current collector, the powder is adhered to conductive double-sided tape or silver tape, the sample is fixed on the sample stage, and the type and amount of the second negative electrode active material are determined by X-ray energy dispersive spectroscopy (EDS).

[0099] In some embodiments, the graphite anode material includes first graphite particles with a Dv50 of 10μm-16μm; for example, it can be, but is not limited to, 10μm, 10.5μm, 11μm, 11.5μm, 12μm, 12.5μm, 13μm, 13.5μm, 14μm, 14.5μm, 15μm, 15.5μm, 16μm or any range between two of the above values.

[0100] As one possible implementation, the graphite anode material includes first graphite particles with a specific surface area of ​​2 m². 2 / g-6m 2 / g; for example, it can be, but is not limited to, 2m. 2 / g, 2.2m 2 / g, 2.4m 2 / g, 2.6m 2 / g, 2.8m 2 / g、3m 2 / g, 3.2m 2 / g, 3.4m 2 / g, 3.6m 2 / g, 3.8m 2 / g、4m 2 / g, 4.2m 2 / g, 4.4m 2 / g, 4.6m 2 / g, 4.8m 2 / g、5m 2 / g, 5.2m 2 / g, 5.4m 2 / g, 5.6m 2 / g, 5.8m 2 / g、6m2 / g or the range between any two of the above values, etc.

[0101] In some embodiments, the graphite anode material includes first graphite particles, and the OI value of the first graphite particles is ≤3.5. It should be noted that the OI value refers to the ratio of the peak intensity of the end-face diffraction peak 2θ=27.2° to the basal-face diffraction peak 2θ=26.0° in the X-ray diffraction pattern of the first graphite particles.

[0102] The first graphite particles have a small particle size and OI value, which is beneficial for the transport of ions in the negative electrode active material, thereby further improving the fast charging performance of the battery.

[0103] Without limitation, the Dv50, specific surface area, and OI value of the first graphite particles mentioned in the context can be determined by the following method: the secondary battery is split to obtain the negative electrode sheet, the negative electrode sheet is cut by focused ion beam (FIB) or argon ion polishing machine (Ar+) to obtain the second negative electrode active material layer powder away from the negative electrode current collector side of the negative electrode sheet, the powder is treated with HF to remove silicon and silicon-containing active materials to obtain the first graphite particle powder;

[0104] The powder is adhered to conductive double-sided tape or silver tape, and the sample is fixed on the sample stage; the average particle size (Dv50) of the material in the powder sample is determined by scanning electron microscopy (SEM); the specific surface area of ​​the material is tested by a surface area and pore size analyzer (BET); the peak intensity ratio of (002) crystal plane 2θ=27.2° and (110) crystal plane 2θ=26° is calculated by measuring the X-ray diffraction (XRD) of the powder, which is the OI value.

[0105] It should be noted that, in the context of this article, Dv50 refers to the particle size corresponding to 50% of the volumetric distribution. Dv99 refers to the particle size corresponding to 99% of the volumetric distribution.

[0106] In some embodiments, the first graphite particles account for 25%-75% of the mass of the graphite anode material; for example, it can be, but is not limited to, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, or any range between two of the above mass percentages. This is beneficial for the anode sheet to have a larger specific surface area and porosity, thereby improving the low-temperature charge-discharge performance of the battery.

[0107] In some alternative implementations, the first graphite particles account for 50%-75% of the mass of the graphite anode material.

[0108] As one possible implementation, the Dv50 of the silicon-based anode material is 15μm-20μm; for example, it can be, but is not limited to, 15μm, 15.5μm, 16μm, 16.5μm, 17μm, 17.5μm, 18μm, 18.5μm, 19μm, 19.5μm, 20μm or any range between two of the above values.

[0109] In some alternative implementations, the specific surface area of ​​the silicon-based anode material is 1 m². 2 / g-5m 2 / g; for example, it can be, but is not limited to, 1m. 2 / g, 1.5m 2 / g、2m 2 / g, 2.5m 2 / g、3m 2 / g, 3.5m 2 / g、4m 2 / g, 4.5m 2 / g、5m 2 / g or the range between any two of the above values, etc.

[0110] When the Dv50 and specific surface area of ​​silicon-based anode materials are within the above ranges, the lithium insertion / delithiation area of ​​silicon-based anode materials is large, there are more reaction sites, and the kinetic performance is better.

[0111] It should be noted that the Dv50 and specific surface area of ​​silicon-based anode materials can be determined using the same testing methods as those for the Dv50 and specific surface area of ​​the first graphite particles, respectively, which will not be elaborated here.

[0112] In some embodiments, the first negative electrode active material and the second negative electrode active material may be the same or different. The first negative electrode active material contained in the negative electrode active material layer may be the same as or different from the second negative electrode active material contained in the second negative electrode active material layer, depending on actual needs.

[0113] As one possible implementation, the secondary battery includes a positive electrode sheet, which includes a positive active material layer containing positive active material. At 25°C, the initial coulombic efficiency of the positive active material in a lithium metal half-cell is ≤90%. Therefore, positive active materials with lower initial efficiency exhibit poor low-temperature charging performance, allowing additives to better enhance this performance. Simultaneously, positive active materials with lower initial efficiency provide greater lithium compensation for lithium loss caused by additives.

[0114] It should be noted that the "initial coulombic efficiency of the positive electrode active material in a lithium metal half-cell at 25°C" mentioned above was measured using the following method:

[0115] Take the electrode containing the positive electrode active material of the battery, assemble a lithium metal half cell, charge it with a current of 0.04C, record the delithiation capacity C0, then discharge it with a current of 0.04C, record the lithium insertion capacity C1, then the first effect CE = C1 / C0*100%.

[0116] In some embodiments, the positive electrode active material includes one or more of lithium nickel cobalt manganese oxide, lithium nickel oxide, and lithium manganese oxide.

[0117] As one possible implementation method, the general chemical formula of the positive electrode active material is Li 1+d [Ni x Co y Mn z M1 e O2, where 0.5≤x≤1, 0<y<0.3, 0<z≤1, 0<d<0.2, 0<e<0.2, x+y+z+e=1, and M1 is one or more of Mg, Ca, Sb, Ce, Ti, Zr, Sr, Al, Zn, Mo and B.

[0118] Understandably, lithium (Li) is intercalated and deintercalated during the charging and discharging process of a battery, and the Li content in the positive electrode varies depending on the state of discharge. In the examples of positive electrode active materials listed in this application, unless otherwise specified, the Li content refers to the initial state of the positive electrode active material. When a positive electrode active material is applied to the positive electrode in a battery system, the Li content in the positive electrode active material typically changes after charge-discharge cycles. The Li content can be measured in molar content, but is not limited to this. Regarding "Li content refers to the initial state of the positive electrode active material," the initial state of the positive electrode active material refers to its state before being added to the positive electrode slurry. It is understood that new materials obtained by appropriately modifying the listed positive electrode active materials are also within the scope of positive electrode active materials. The aforementioned appropriate modification refers to acceptable modification methods for the positive electrode active material; non-limiting examples include coating modification.

[0119] In the examples of positive electrode active materials in this application, the oxygen (O) content is only a theoretical value. Lattice oxygen release will cause changes in the molar content of oxygen, and the actual O content will fluctuate. The O content can be measured in molar content, but is not limited to this.

[0120] In some implementations, the secondary battery is a lithium-ion battery.

[0121] One or more embodiments of this application provide a method for preparing a secondary battery, which can be used to prepare the aforementioned secondary battery. The method includes the step of preparing a negative electrode sheet, the preparation of which includes: forming a first negative electrode active material layer on at least one side surface of a negative electrode current collector, the first negative electrode active material layer comprising a first negative electrode active material; linearly coating a one-dimensional conductive agent onto the surface of an additive, the additive comprising one or more of elemental tin, tin compounds, and tin-containing alloys; preparing a second negative electrode slurry, the second negative electrode slurry comprising a second negative electrode active material and an additive with a one-dimensional conductive agent linearly coated on its surface; applying the second negative electrode slurry to the surface of the first negative electrode active material layer away from the negative electrode current collector to form a second negative electrode active material layer; the lithium intercalation potential of the first and second negative electrode active materials at 25°C is independently <1.2V (Vs. Li). + / Li).

[0122] Understandably, by introducing additives and one-dimensional conductive agents during the preparation of the negative electrode sheet, with the one-dimensional conductive agent linearly encapsulating the additives, on the one hand, during the charging or lithium intercalation process of the secondary battery, the additives can preferentially achieve lithium intercalation compared to the negative electrode active material, thereby increasing the lithium intercalation potential of the negative electrode and suppressing potential polarization to reach the lithium plating potential (0V). This is especially beneficial in low-temperature charging environments where the negative electrode voltage can drop rapidly. On the other hand, the additives themselves can lower the lithium-ion desolvation energy barrier, enabling rapid desolvation and intercalation of lithium ions into the additives. Therefore, adding additives can improve the low-temperature charging capability of secondary batteries. Simultaneously, by using a one-dimensional conductive agent to linearly encapsulate the additives, the expansion of the additives themselves during charging and discharging can be reduced, minimizing repeated expansion and contraction during cycling. This inhibits the detachment of the additives from the conductive network due to their expansion and contraction, reducing the impact of additive introduction on cell capacity decay.

[0123] In one possible implementation, the total mass of the one-dimensional conductive agent and additives is 0.2%-10% of the total mass of the coating slurry. In some alternative implementations, the total mass of the one-dimensional conductive agent and additives is 1%-10% of the total mass of the coating slurry.

[0124] In some embodiments, the mass ratio of the one-dimensional conductive agent to the additive is (2-100):100; for example, it can be, but is not limited to, 2:100, 5:100, 10:100, 15:100, 20:100, 25:100, 30:100, 35:100, 40:100, 45:100, 50:100, 55:100, 60:100, 65:100, 70:100, 75:100, 80:100, 85:100, 90:100, 95:100, 100:100, or any range between two of the above ratios. Thus, the one-dimensional conductive agent can linearly encapsulate the additive, providing better binding of the additive.

[0125] As one possible implementation, the Dv50 of the additive is 1μm-15μm; for example, it can be, but is not limited to, 1μm, 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm or any range between two of the above values.

[0126] In some implementations, the additive's Dv99 is < 40 μm.

[0127] When the Dv50 and Dv99 of the additive are within the above ranges, the particle size of the additive is close to or smaller than the particle size of the negative electrode active material, and the lithium insertion / delithiation kinetics of the additive are better, which is conducive to further improving the effect of low-temperature charge and discharge.

[0128] In some embodiments, the step of linearly coating a one-dimensional conductive agent on the surface of the additive includes: mixing a dispersion containing a one-dimensional conductive agent with the additive and then spray-drying it to linearly coat the one-dimensional conductive agent on the surface of the additive.

[0129] As one possible implementation, the solvent for the dispersion includes one or more of water, polyvinyl alcohol, polyacrylic acid, such as polyethylene glycol, polyvinylpyrrolidone, N-methylpyrrolidone, and dimethyl sulfoxide.

[0130] In some embodiments, the mass percentage of the one-dimensional conductive agent in the dispersion is 0.2%-5%; for example, it can be, but is not limited to, 0.2%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, or any range between two of the above values. When the mass percentage of the one-dimensional conductive agent in the dispersion is within the above range, the dispersion of the one-dimensional conductive agent is more stable, which is more beneficial for subsequent coating processing.

[0131] In some alternative embodiments, the coating slurry may also contain a conductive agent. The conductive agent may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0132] As one possible implementation, the coating slurry may also optionally include a binder. The binder may include one or more of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0133] One or more embodiments of this application provide a negative electrode sheet, including a negative current collector, a first negative active material layer located on at least one side surface of the negative current collector, and a second negative active material layer located on the side surface of the first negative active material layer away from the negative current collector; the first negative active material layer contains a first negative active material, and the second negative active material layer contains a second negative active material and an additive, with a one-dimensional conductive agent disposed on the surface of the additive; the lithium intercalation potential of the first and second negative active materials at 25°C is independently <1.2V (Vs. Li). + / Li), the additives include one or more of elemental tin, tin compounds and tin-containing alloys.

[0134] In some embodiments, the one-dimensional conductive agent includes one or more of carbon nanotubes, carbon fibers, metal fibers, and conductive polymer fibers. This facilitates the linear confinement of the additive.

[0135] As one possible implementation, carbon nanotubes include one or more of single-walled carbon nanotubes and multi-walled carbon nanotubes. Optionally, the carbon nanotubes are single-walled carbon nanotubes. Therefore, single-walled carbon nanotubes have better electrical conductivity and, compared to multi-walled carbon nanotubes, a smaller mass percentage and better dispersibility.

[0136] In some embodiments, the diameter of the carbon nanotubes is 0.5nm-100nm; for example, it can be, but is not limited to, 0.5nm, 1nm, 5nm, 10nm, 15nm, 20nm, 25nm, 30nm, 35nm, 40nm, 45nm, 50nm, 55nm, 60nm, 65nm, 70nm, 75nm, 80nm, 85nm, 90nm, 95nm, 100nm, or any range between two of the above diameters.

[0137] As one possible implementation, the length of the carbon nanotubes is 10μm-1000μm; for example, it can be, but is not limited to, 10μm, 50μm, 100μm, 150μm, 200μm, 250μm, 300μm, 350μm, 400μm, 450μm, 500μm, 550μm, 600μm, 650μm, 700μm, 750μm, 800μm, 850μm, 900μm, 950μm, 1000μm or any range between two of the above lengths.

[0138] When the diameter and length of carbon nanotubes are within the above-mentioned ranges, the carbon nanotubes have suitable mechanical strength and stability, and at the same time have suitable encapsulation strength for additives, thereby reducing the occurrence of carbon nanotubes falling off the surface of the additives and losing their binding effect.

[0139] In some embodiments, the tin compound includes one or more of SnO2, SnO, SnS, and SnF.

[0140] As one possible implementation, the tin-containing alloy includes one or more of the following: tin-bismuth alloy, lithium-tin alloy, tin-copper alloy, tin-silver alloy, tin-selenium alloy, tin-tellurium alloy, and sodium-tin alloy.

[0141] As one possible implementation, the mass percentage of the one-dimensional conductive agent relative to the mass of the additive is 1%-105%.

[0142] In some embodiments, the mass percentage of the one-dimensional conductive agent relative to the mass of the additive is 2%-100%; for example, it can be, but is not limited to, 2%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 100%, or any range between two of the above percentages. When the mass percentage of the one-dimensional conductive agent relative to the mass of the additive is within the above range, it is advantageous to balance the binding effect of the one-dimensional conductive agent on the additive, the conductivity of the one-dimensional conductive agent, and the low-temperature charge-discharge capability of the additive.

[0143] In some embodiments, the combined mass percentage of the additive and the one-dimensional conductive agent in the second negative electrode active material layer is 0.1%-11%.

[0144] As one possible implementation, the sum of the mass percentages of the additive and the one-dimensional conductive agent in the second negative electrode active material layer is 0.2%-10%; for example, it can be, but is not limited to, 0.2%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10%, or any range between two of the above values. When the sum of the mass percentages of the additive and the one-dimensional conductive agent in the second negative electrode active material layer is within the above range, it is beneficial for the additive to play its role, while also reducing the impact of additive expansion on the electrode or battery.

[0145] In some alternative implementations, the combined mass percentage of the additive and the one-dimensional conductive agent in the second negative electrode active material layer is 1%-10%.

[0146] In some embodiments, the second negative electrode active material includes one or more of graphite negative electrode materials and silicon-based negative electrode materials.

[0147] As one possible implementation, the second negative electrode active material includes graphite negative electrode material and silicon-based negative electrode material, with the graphite negative electrode material accounting for ≥80% of the total mass of the graphite negative electrode material and silicon-based negative electrode material. Therefore, additives have a greater advantage in graphite negative electrode systems with high graphite content and high initial efficiency, further enhancing the effectiveness of the additives.

[0148] In some embodiments, the graphite anode material includes first graphite particles with a Dv50 of 10μm-16μm; for example, it can be, but is not limited to, 10μm, 10.5μm, 11μm, 11.5μm, 12μm, 12.5μm, 13μm, 13.5μm, 14μm, 14.5μm, 15μm, 15.5μm, 16μm or any range between two of the above values.

[0149] As one possible implementation, the graphite anode material includes first graphite particles with a specific surface area of ​​2 m². 2 / g-6m 2 / g; for example, it can be, but is not limited to, 2m. 2 / g, 2.2m 2 / g, 2.4m 2 / g, 2.6m 2 / g, 2.8m 2 / g、3m 2 / g, 3.2m 2 / g, 3.4m 2 / g, 3.6m 2 / g, 3.8m 2 / g、4m2 / g, 4.2m 2 / g, 4.4m 2 / g, 4.6m 2 / g, 4.8m 2 / g、5m 2 / g, 5.2m 2 / g, 5.4m 2 / g, 5.6m 2 / g, 5.8m 2 / g、6m 2 / g or the range between any two of the above values, etc.

[0150] In some embodiments, the graphite anode material includes first graphite particles, and the OI value of the first graphite particles is ≤3.5. It should be noted that the OI value refers to the ratio of the peak intensity of the end-face diffraction peak 2θ=27.2° to the basal-face diffraction peak 2θ=26.0° in the X-ray diffraction pattern of the first graphite particles.

[0151] The first graphite particles have a small particle size and OI value, which is beneficial for the transport of ions in the negative electrode active material, thereby further improving the fast charging performance of the battery.

[0152] In some embodiments, the first graphite particles account for 25%-75% of the mass of the graphite anode material; for example, it can be, but is not limited to, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, or any range between two of the above mass percentages. This is beneficial for the anode sheet to have a larger specific surface area and porosity, thereby improving the low-temperature charge-discharge performance of the battery.

[0153] In some alternative implementations, the first graphite particles account for 50%-75% of the mass of the graphite anode material.

[0154] As one possible implementation, the Dv50 of the silicon-based anode material is 15μm-20μm; for example, it can be, but is not limited to, 15μm, 15.5μm, 16μm, 16.5μm, 17μm, 17.5μm, 18μm, 18.5μm, 19μm, 19.5μm, 20μm or any range between two of the above values.

[0155] In some alternative implementations, the specific surface area of ​​the silicon-based anode material is 1 m². 2 / g-5m 2 / g; for example, it can be, but is not limited to, 1m. 2 / g, 1.5m 2 / g、2m 2 / g, 2.5m 2 / g、3m2 / g, 3.5m 2 / g、4m 2 / g, 4.5m 2 / g、5m 2 / g or the range between any two of the above values, etc.

[0156] When the Dv50 and specific surface area of ​​silicon-based anode materials are within the above ranges, the lithium insertion / delithiation area of ​​silicon-based anode materials is large, there are more reaction sites, and the kinetic performance is better.

[0157] In some embodiments, the first negative electrode active material and the second negative electrode active material may be the same or different. The first negative electrode active material contained in the negative electrode active material layer may be the same as or different from the second negative electrode active material contained in the second negative electrode active material layer, depending on actual needs.

[0158] One or more embodiments of this application provide an electrical device, including one or more of the secondary battery described above and the secondary battery prepared by the preparation method described above.

[0159] In addition, the secondary battery and power-consuming device of this application will be described below with appropriate reference to the accompanying drawings.

[0160] Typically, a secondary battery consists of a positive electrode, a negative electrode, an electrolyte, and a separator. During charging and discharging, active ions move back and forth between the positive and negative electrodes, inserting and releasing. The electrolyte acts as a conductor between the positive and negative electrodes. The separator, positioned between the positive and negative electrodes, primarily prevents short circuits while allowing ions to pass through.

[0161] The positive electrode sheet includes a positive current collector and a positive active material layer disposed on at least one surface of the positive current collector, the positive active material layer including a positive active material.

[0162] As a non-limiting example, the positive current collector has two surfaces opposite each other in its own thickness direction, and the positive active material layer is disposed on either or both of the two opposite surfaces of the positive current collector.

[0163] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymeric material substrate and a metal layer formed on at least one surface of the polymeric material substrate. The composite current collector can be obtained by forming a metal material on a polymeric material substrate. Non-limiting examples of the metal material in the positive electrode current collector may include one or more of aluminum, aluminum alloys, nickel, nickel alloys, titanium, titanium alloys, silver, and silver alloys. Non-limiting examples of the polymeric material substrate in the positive electrode current collector may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).

[0164] In some embodiments, the positive electrode active material layer may optionally include a binder. As a non-limiting example, the binder may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), PVDF-tetrafluoroethylene-propylene terpolymer, PVDF-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorinated acrylate resins.

[0165] In some embodiments, the positive electrode active material layer may optionally include a conductive agent. As a non-limiting example, the conductive agent may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0166] In some embodiments, the positive electrode sheet can be prepared by dispersing the components used to prepare the positive electrode sheet, such as the positive electrode active material, conductive agent, binder, and any other components, in a solvent to form a positive electrode slurry; coating the positive electrode slurry onto at least one surface of the positive electrode current collector, and then obtaining the positive electrode sheet after drying, cold pressing, and other processes. The solvent can be selected from, but is not limited to, any of the solvents described in the foregoing embodiments, such as N-methylpyrrolidone (NMP). The surface of the positive electrode current collector coated with the positive electrode slurry can be a single surface or both surfaces of the positive electrode current collector. The solid content of the positive electrode slurry can be 40wt%-80wt%. The viscosity of the positive electrode slurry at room temperature can be adjusted to 5000 mPa·s-25000 mPa·s. When coating the positive electrode slurry, the areal density per unit area of ​​the coating, based on dry weight (excluding solvent), can be 15 mg / cm³. 2 -35 mg / cm 2 The compaction density of the positive electrode sheet can be 3.0 g / cm³. 3 -3.8 g / cm 3The option is 3.3 g / cm³. 3 -3.75 g / cm 3 .

[0167] Negative electrode sheet

[0168] The negative electrode includes a negative current collector, a first negative active material layer disposed on at least one surface of the negative current collector, and a second negative active material layer disposed on the surface of the first negative active material layer away from the negative current collector. The first negative active material layer includes a first negative active material, and the second negative active material layer includes a second negative active material and an additive. A one-dimensional conductive agent is disposed on the surface of the additive. The lithium intercalation potential of the first and second negative active materials at 25°C is independently <1.2V (Vs. Li). + / Li), the additives include one or more of elemental tin, tin compounds and tin-containing alloys.

[0169] As a non-limiting example, the negative electrode current collector has two surfaces opposite each other in its own thickness direction, and the negative electrode active material layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.

[0170] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymeric material substrate and a metal layer formed on at least one surface of the polymeric material substrate. The composite current collector can be obtained by forming a metal material on the polymeric material substrate. Non-limiting examples of the metal material in the negative electrode current collector may include one or more of copper, copper alloys, nickel, nickel alloys, titanium, titanium alloys, silver, and silver alloys. Non-limiting examples of the polymeric material substrate in the negative electrode current collector may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).

[0171] In some embodiments, the negative electrode active material layer may optionally include a binder. The binder may include one or more of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0172] In some embodiments, the negative electrode active material layer may optionally include a conductive agent. The conductive agent may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0173] In some embodiments, the negative electrode active material layer may also optionally include other additives, such as thickeners (e.g., sodium carboxymethyl cellulose (CMC-Na)).

[0174] In some embodiments, the negative electrode sheet can be prepared by dispersing the components used to prepare the negative electrode sheet, such as the first negative electrode active material, the first conductive agent, the first binder, and any other components, in a solvent (a non-limiting example of the solvent is deionized water) to form a first negative electrode slurry; dispersing the second negative electrode active material, an additive with a one-dimensional conductive agent linearly coated on its surface, the second conductive agent, and the second binder in a solvent (a non-limiting example of the solvent is deionized water) to form a second negative electrode slurry; coating the first negative electrode slurry onto at least one side surface of the negative electrode current collector to form a first negative electrode active material layer; coating the side surface of the first negative electrode active material layer away from the negative electrode current collector with the second negative electrode slurry to form a second negative electrode active material layer; and obtaining the negative electrode sheet after drying, cold pressing, and other processes. The surface of the negative electrode current collector coated with the first negative electrode slurry can be a single surface of the negative electrode current collector or both surfaces of the negative electrode current collector. The solid content of the first negative electrode slurry and the second negative electrode slurry can be 40wt%-60wt%, respectively. The viscosities of the first and second negative electrode slurries at room temperature can be adjusted to 2000 mPa·s - 10000 mPa·s, respectively. When coating the first and second negative electrode slurries, the areal density per unit area (dry weight, minus solvent) can be 75 g / m², respectively. 2 -220 g / m 2 The compaction density of the negative electrode sheet can be 1.0 g / cm³. 3 -1.8 g / cm 3 .

[0175] electrolytes

[0176] Electrolytes have the function of conducting ions between the positive and negative electrode plates.

[0177] In some embodiments, the electrolyte is an electrolyte solution. The electrolyte solution includes an electrolyte salt and a solvent.

[0178] In some embodiments, the electrolyte salt may include one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorophosphate (LiPO2F2), lithium difluorooxalate borate (LiDFOB), lithium dioxalate borate (LiBOB), lithium difluorodioxalate phosphate (LiDFOP), and lithium tetrafluorooxalate phosphate (LiTFOP).

[0179] In some embodiments, the solvent may include ethylene carbonate (EC, ), propylene carbonate (PC, ), methyl ethyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), ethylene carbonate ( One or more of the following: fluoroethylene carbonate (FEC), methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, sulfolane, dimethyl sulfone, methyl ethyl sulfone, and diethyl sulfone.

[0180] In some embodiments, the electrolyte may optionally include additives. For example, additives may include negative electrode film-forming additives, positive electrode film-forming additives, and may also include additives that can improve certain battery performance, such as additives that improve battery overcharge performance, additives that improve battery high-temperature or low-temperature performance, etc.

[0181] In some embodiments, the additives in the electrolyte may include, but are not limited to, one or more of fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), trifluoromethyl ethylene carbonate (TFPC), etc.

[0182] Separating membrane

[0183] In some embodiments, the secondary battery also includes a separator. This application does not impose any particular limitation on the type of separator; any known porous separator with good chemical and mechanical stability can be selected.

[0184] In some embodiments, the material of the separator may include one or more of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator may be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer may be the same or different, without particular limitation.

[0185] In some embodiments, the thickness of the isolation membrane is 4-40 μm, optionally 5-7 μm.

[0186] In some embodiments, the positive electrode, negative electrode, and separator can be fabricated into an electrode assembly using a winding or stacking process.

[0187] In some embodiments, the secondary battery may include an outer packaging. This outer packaging may be used to encapsulate the electrode assembly and electrolyte described above.

[0188] In some embodiments, the outer packaging of the secondary battery can be a rigid shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery can also be a soft pack, such as a pouch-type soft pack. The material of the soft pack can be plastic; further, non-limiting examples of plastic may include one or more of polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0189] A secondary battery includes at least one battery cell. A secondary battery may include one or more battery cells.

[0190] In this application, unless otherwise specified, "cell battery" refers to the basic unit capable of converting chemical energy into electrical energy, and generally includes at least a positive electrode, a negative electrode, and an electrolyte. During the charging and discharging process of the battery, active ions move back and forth between the positive and negative electrode plates, inserting and extracting. The electrolyte acts as a conductor for the active ions between the positive and negative electrode plates.

[0191] This application does not impose any particular limitation on the shape of the battery cell; it can be cylindrical, square, or any other arbitrary shape. For example, Figure 2 The example shown is a square-structured battery cell 5.

[0192] In some of these embodiments, reference is made to Figure 3 The outer packaging may include a housing 51 and a cover 53. The housing 51 may include a base plate and side plates connected to the base plate, the base plate and side plates forming a receiving cavity. The housing 51 has an opening communicating with the receiving cavity, and the cover 53 can be placed over the opening to close the receiving cavity. The positive electrode, negative electrode, and separator may be formed into an electrode assembly 52 by a winding process or a stacking process. The electrode assembly 52 is encapsulated within the receiving cavity. Electrolyte is immersed in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the battery cell 5 may be one or more, which can be selected by those skilled in the art according to actual needs.

[0193] The secondary battery can be either battery module 4 or battery pack 1.

[0194] A battery module includes at least one battery cell. The number of battery cells in a battery module can be one or more, and those skilled in the art can select an appropriate number based on the application and capacity of the battery module.

[0195] Figure 4 This is battery module 4, used as an example. (See reference...) Figure 4 In battery module 4, multiple battery cells 5 can be arranged sequentially along the length of battery module 4. Of course, they can also be arranged in any other manner. Furthermore, these multiple battery cells 5 can be fixed in place using fasteners.

[0196] Optionally, the battery module 4 may also include a housing with a receiving space in which multiple battery cells 5 are received.

[0197] In some embodiments, the battery modules described above can also be assembled into a battery pack, and the number of battery modules contained in the battery pack can be one or more. Those skilled in the art can select an appropriate number according to the application and capacity of the battery pack.

[0198] Figure 5 and Figure 6 This is battery pack 1 as an example. (See reference...) Figure 5 and Figure 6 The battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box includes an upper body 2 and a lower body 3, with the upper body 2 covering the lower body 3 to form a closed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.

[0199] In addition, this application also provides an electrical device, which includes the secondary battery provided in this application. The secondary battery can be used as the power source of the electrical device or as the energy storage unit of the electrical device. The electrical device may include, but is not limited to, mobile devices, electric vehicles, electric trains, ships and satellites, energy storage systems, etc. Among them, mobile devices may be, for example, mobile phones, laptops, etc.; electric vehicles may be, for example, pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc., but are not limited to.

[0200] As an electrical device, a rechargeable battery can be selected based on its usage requirements.

[0201] Figure 7 Here is an example of an electrical device 6. This electrical device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. To meet the high power and high energy density requirements of the secondary battery for this electrical device, a battery pack or battery module can be used.

[0202] Another example device could be a mobile phone, tablet, or laptop. These devices typically require a slim and lightweight design and can use a rechargeable battery as their power source.

[0203] Example

[0204] The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where the technology or conditions are not specified in the embodiments, they are performed according to the technology or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.

[0205] Preparation of primary and secondary batteries

[0206] Example 1

[0207] 1) Preparation of negative electrode sheet

[0208] An aqueous dispersion of single-walled carbon nanotubes (CNTs) containing a one-dimensional conductive agent was taken, and SnS additive was added. The mixture was stirred at 50 rpm / min and 500 rpm / min to achieve uniform mixing. The mixture was then spray-dried to obtain SnS linearly encapsulated with CNTs, i.e., SnS@CNT. The CNTs in the aqueous dispersion comprised 3% of the total mass, the mass ratio of the one-dimensional conductive agent CNTs to the additive SnS was 5:100, the Dv50 of the additive SnS was 8 μm, and the Dv99 was 30 μm. The CNTs had a diameter of 3 nm and a length of 60 μm.

[0209] Artificial graphite, natural graphite, styrene-butadiene rubber (SBR) binder, and acetylene black (HBL) conductive agent were thoroughly mixed and ball-milled in a deionized water solvent system at a mass ratio of 48.5:48.5:1.5:1.5 to obtain the first negative electrode slurry.

[0210] The first graphite particles, natural graphite, styrene-butadiene rubber (SBR) binder, acetylene black (acetylene black) conductive agent, and SnS@CNT were thoroughly mixed and ball-milled in a deionized water solvent system at a mass ratio of 57.09:38.06:2.5:0.35:2 to obtain the second negative electrode slurry. The first graphite particles had a Dv50 of 12 μm and a specific surface area of ​​2.4 m². 2 / g, OI value 3; the mass percentage of the first graphite particles relative to the total mass of the first graphite particles and natural graphite is 60%. The mass percentage of SnS@CNT in the second negative electrode slurry is 2%.

[0211] A first negative electrode slurry is uniformly coated onto both sides of a copper foil to form a first negative electrode active material layer. A second negative electrode slurry is then coated onto the surface of the first negative electrode active material layer. The copper foil is then dried in an oven at 110°C for 1 hour, and compacted to a density of PD = 1.75 g / cm³. 3 The negative electrode sheet is obtained by rolling.

[0212] 2) Preparation of positive electrode sheet

[0213] LiNi, the positive electrode active material 0.86 C 0.06 Mn 0.08Conductive carbon black SP and binder PVDF were mixed at a weight ratio of 98:1:1, and solvent NMP was added. The mixture was stirred under vacuum until the system was homogeneous to obtain the positive electrode slurry. The positive electrode slurry was uniformly coated on both sides of the positive electrode current collector aluminum foil, air-dried at room temperature, and then transferred to an oven for further drying. Finally, it was cold-pressed to obtain a compaction density PD = 3.6 g / cm³. 3 Positive electrode sheet.

[0214] 3) Separating membrane

[0215] A 6μm thick polyethylene separator film was selected.

[0216] 4) Preparation of electrolyte

[0217] The organic solvent is a mixture containing ethylene carbonate (EC), diethyl carbonate (DEC), and dimethyl carbonate (DMC), wherein the volume ratio of EC, DEC, and DMC is 1:1:1. Thoroughly dried lithium salt LiPF6 is dissolved in the organic solvent and mixed thoroughly in an argon-atmosphere glove box with a water content of <10 ppm to obtain the electrolyte. The concentration of the lithium salt is 1 mol / L.

[0218] 5) Battery manufacturing

[0219] The electrodes are arranged in the following order: separator - negative electrode sheet - separator - positive electrode sheet. One end of the positive electrode sheet, negative electrode sheet, and two separators is fixed to the discharge roller, and the other end is stacked together and fixed to the winding shaft. The winding shaft is rotated by a motor to wind the positive electrode sheet, negative electrode sheet, and two separators to obtain the electrode assembly. The electrode assembly is placed in the battery casing, dried, and then injected with electrolyte. After vacuum sealing, settling, formation, and shaping, a lithium-ion battery is obtained.

[0220] Example 2

[0221] The secondary battery of Example 2 is prepared in a similar manner to the secondary battery of Example 1, except that: in Example 2, the mass percentage of SnS@CNT in the second negative electrode slurry prepared is 1%, and the mass ratio of the first graphite particles, natural graphite, styrene-butadiene rubber binder, acetylene black conductive agent and SnS@CNT is 57.69:38.46:2.5:0.35:1; all other aspects are the same.

[0222] Example 3

[0223] The secondary battery of Example 3 is prepared in a similar manner to that of Example 1, except that: in Example 3, the mass percentage of SnS@CNT in the second negative electrode slurry prepared is 5%, and the mass ratio of the first graphite particles, natural graphite, styrene-butadiene rubber binder, acetylene black conductive agent and SnS@CNT is 55.29:36.86:2.5:0.35:5; all other aspects are the same.

[0224] Example 4

[0225] The secondary battery in Example 4 is prepared in a similar manner to the secondary battery in Example 1, except that: in Example 4, the mass percentage of SnS@CNT in the second negative electrode slurry prepared is 10%, and the mass ratio of the first graphite particles, natural graphite, styrene-butadiene rubber binder, acetylene black conductive agent, and SnS@CNT is 52.29:34.86:2.5:0.35:10; all other aspects are the same.

[0226] Example 5

[0227] The secondary battery of Example 5 is prepared in a similar manner to the secondary battery of Example 1, except that: in Example 5, the mass percentage of SnS@CNT in the second negative electrode slurry prepared is 0.2%, and the mass ratio of the first graphite particles, natural graphite, styrene-butadiene rubber binder, acetylene black conductive agent and SnS@CNT is 58.17:38.78:2.5:0.35:0.2; all other aspects are the same.

[0228] Example 6

[0229] The secondary battery of Example 6 is prepared in a similar manner to that of the secondary battery of Example 1, except that: in Example 6, the mass ratio of SnS@CNT in the second negative electrode slurry prepared is 11%, and the mass ratio of the first graphite particles, natural graphite, styrene-butadiene rubber binder, acetylene black conductive agent and SnS@CNT is 51.69:34.46:2.5:0.35:11; all other aspects are the same.

[0230] Example 7

[0231] The secondary battery of Example 7 is prepared in a similar manner to the secondary battery of Example 1, except that: in Example 7, the mass percentage of SnS@CNT in the second negative electrode slurry prepared is 0.1%, and the mass ratio of the first graphite particles, natural graphite, styrene-butadiene rubber binder, acetylene black conductive agent and SnS@CNT is 58.23:38.82:2.5:0.35:0.1; all other aspects are the same.

[0232] Electron electron microscopy was performed on the SnS@CNTs prepared in Example 1, and the results are as follows: Figure 1 As shown. By Figure 1It can be seen that the one-dimensional conductive agent CNT is uniformly dispersed on the surface of the additive SnS, achieving effective linear encapsulation of the additive.

[0233] The mass percentage of SnS@CNT in the second negative electrode active material layer of each secondary battery negative electrode sheet in Examples 1-7 and the dosage ratio of each component in the second negative electrode active material layer were tested. The test results are shown in Table 1.

[0234] The secondary batteries prepared in Examples 1-7 were subjected to negative electrode rebound / expansion tests and low-temperature charge-discharge capacity retention tests, respectively. The test methods are as follows:

[0235] The test methods for low-temperature charge-discharge capacity retention are as follows:

[0236] Low-temperature charging capacity retention test: Place the battery cell on the electrochemical test channel, charge it to 4.25V at 0.33C at 25℃, and then discharge it to 2.8V at 0.33C. Record the capacity C0. After standing in a -10℃ environment for 2 hours, charge it at 0.33C in a -10℃ environment and record the capacity to 4.3V, which is denoted as C. The low-temperature discharge capacity retention rate at -10℃ is: C / C0×100%.

[0237] Low-temperature discharge capacity retention test: Place the battery cell on the electrochemical test channel at 25°C, fully charge it to 4.25V with a current of 0.33C, and then fully discharge it to 2.8V with a current of 0.33C, recording the capacity C0; charge it to 4.25V with a current of 0.33C0, place it at a low temperature of -10°C for 2 hours, and then discharge it at 0.33C, recording the discharge capacity C1. The low-temperature discharge capacity retention rate at -10°C is: C1 / C0×100%.

[0238] Negative electrode rebound / expansion test: Take different cells and adjust them to the same SOC. Disassemble the cells, take the electrode sheets, and measure the thickness of the electrode sheets with vernier calipers.

[0239] Take the anodes of different cells in the fully discharged state and the anodes adjusted to the fully charged state, and measure the thickness of the electrode sheets D0 and D1 with vernier calipers. Calculate the full-charge anode expansion rate (D1-D0) / D0. The results are shown in Table 1.

[0240] The differences between Examples 1-7 and the test results are shown in Table 1.

[0241] Table 1

[0242]

[0243] Here, mass percentage refers to the mass percentage of SnS@CNT in the second negative electrode active material layer.

[0244] Example 8

[0245] The secondary battery of Example 8 is prepared in a similar manner to that of the secondary battery of Example 1, except that: when preparing the negative electrode sheet in Example 8, the mass ratio of the one-dimensional conductive agent CNT to the additive SnS is 2:100 when linearly coating the surface of the additive SnS with the one-dimensional conductive agent CNT. All other aspects are the same.

[0246] Example 9

[0247] The secondary battery of Example 9 is prepared in a similar manner to the secondary battery of Example 1, except that: when preparing the negative electrode sheet in Example 9, the mass ratio of the one-dimensional conductive agent CNT to the additive SnS when linearly coating the surface of the additive SnS is 10:100; all other aspects are the same.

[0248] Example 10

[0249] The secondary battery of Example 10 is prepared in a similar manner to that of the secondary battery of Example 1, except that: when preparing the negative electrode sheet in Example 10, the mass ratio of the one-dimensional conductive agent CNT to the additive SnS is 50:100 when linearly coating the surface of the additive SnS; all other aspects are the same.

[0250] Example 11

[0251] The secondary battery of Example 11 is prepared in a similar manner to that of the secondary battery of Example 1, except that: when preparing the negative electrode sheet in Example 11, the mass ratio of the one-dimensional conductive agent CNT to the additive SnS when linearly coating the surface of the additive SnS is 100:100; all other aspects are the same.

[0252] Example 12

[0253] The secondary battery of Example 12 is prepared in a similar manner to the secondary battery of Example 1, except that: when preparing the negative electrode sheet in Example 12, the mass ratio of the one-dimensional conductive agent CNT to the additive SnS when linearly coating the surface of the additive SnS is 105:100; all other aspects are the same.

[0254] Example 13

[0255] The secondary battery of Example 13 is prepared in a similar manner to the secondary battery of Example 1, except that: when preparing the negative electrode sheet in Example 13, the mass ratio of the one-dimensional conductive agent CNT to the additive SnS is 1:100 when linearly coating the surface of the additive SnS with the one-dimensional conductive agent CNT. All other aspects are the same.

[0256] The percentage of the mass of the one-dimensional conductive agent CNT relative to the mass of the additive SnS in the SnS@CNT contained in each secondary battery in Test Examples 8-13 is shown in Table 2.

[0257] The secondary batteries prepared in Examples 8-13 were subjected to negative electrode rebound / expansion tests and low-temperature charge-discharge capacity retention tests, using the same methods as in Examples 1-7. The test results are shown in Table 2.

[0258] Table 2

[0259]

[0260] In Table 2, the percentage refers to the percentage of the mass of the one-dimensional conductive agent CNT in the SnS@CNT contained in the secondary battery relative to the mass of the additive SnS.

[0261] Example 14

[0262] The secondary battery in Example 14 is prepared in a similar manner to the secondary battery in Example 1, except that the first graphite particles used in the preparation of the second negative electrode active material layer of the negative electrode sheet in Example 14 have a Dv50 of 10 μm and a specific surface area of ​​2 m². 2 / g, OI value is 3.5; all others are the same.

[0263] Example 15

[0264] The secondary battery in Example 15 is prepared in a similar manner to the secondary battery in Example 1, except that the first graphite particles used in the preparation of the second negative electrode active material layer of the negative electrode sheet in Example 15 have a Dv50 of 16 μm and a specific surface area of ​​6 m². 2 / g, OI value is 2.5; all others are the same.

[0265] The Dv50, specific surface area BET, and OI value of the first graphite particles used in the second negative electrode active material layer of the negative electrode sheet in each of the secondary batteries in Examples 14-15 were tested. The test results are shown in Table 3.

[0266] The secondary batteries prepared in Examples 14-15 were subjected to negative electrode rebound / expansion tests and low-temperature charge-discharge capacity retention tests, using the same methods as in Examples 1-7. The test results are shown in Table 3.

[0267] Table 3

[0268]

[0269] Example 16

[0270] The secondary battery of Example 16 is prepared in a similar manner to the secondary battery of Example 1, except that: when preparing the second negative electrode slurry of the negative electrode sheet in Example 16, the mass percentage of the first graphite particles relative to the total mass of the first graphite particles and natural graphite is 25%, and all other aspects are the same.

[0271] Example 17

[0272] The secondary battery of Example 17 is prepared in a similar manner to the secondary battery of Example 1, except that: when preparing the second negative electrode slurry of the negative electrode sheet in Example 17, the mass of the first graphite particles is 50% of the total mass of the first graphite particles and natural graphite, and all other aspects are the same.

[0273] Example 18

[0274] The secondary battery of Example 18 is prepared in a similar manner to the secondary battery of Example 1, except that: when preparing the second negative electrode slurry of the negative electrode sheet in Example 18, the mass percentage of the first graphite particles relative to the total mass of the first graphite particles and natural graphite is 75%, and all other aspects are the same.

[0275] The percentage of the mass of the first graphite particles used in the second negative electrode active material layer of the negative electrode sheet in each of the test examples 16-18 relative to the total mass of the first graphite particles and natural graphite, as well as the ratio of the amount of each component in the second negative electrode active material layer, are shown in Table 4.

[0276] The secondary batteries prepared in Examples 16-18 were subjected to negative electrode rebound / expansion tests and low-temperature charge-discharge capacity retention tests, using the same methods as in Examples 1-7. The test results are shown in Table 4.

[0277] Table 4

[0278]

[0279] In Table 4, the percentage refers to the percentage of the mass of the first graphite particles contained in the second negative electrode active material layer of the secondary battery relative to the total mass of the first graphite particles and natural graphite.

[0280] Example 19

[0281] The secondary battery in Example 19 is prepared using a method similar to that in Example 1, except that: in preparing the second negative electrode slurry for the negative electrode sheet in Example 19, the mass ratio of the first graphite particles, natural graphite, styrene-butadiene rubber binder, acetylene black conductive agent, and SnS@CNT is 57:38:2.5:0.5:2; and the positive electrode active material used in preparing the positive electrode sheet is LiNi. 0.65 C 0.15 Mn 0.2 Everything else is the same.

[0282] Example 20

[0283] The secondary battery of Example 20 is prepared using a method similar to that of Example 1, except that: in preparing the second negative electrode slurry for the negative electrode sheet in Example 20, the negative electrode active materials used include first graphite particles, natural graphite, and silicon-based materials; the mass ratio of the first graphite particles, natural graphite, silicon-based materials, styrene-butadiene rubber binder, acetylene black conductive agent, and SnS@CNT in the second negative electrode slurry is 55.89:37.26:2:2.5:0.35:2; all other aspects are the same. The silicon-based material is carbon-coated silicon, with a coating weight of 30% by mass of silicon.

[0284] Example 21

[0285] The secondary battery in Example 21 is prepared using a method similar to that in Example 1, except that: in Example 21, the negative electrode active material used in preparing the second negative electrode slurry includes first graphite particles, natural graphite, and silicon-based materials; the mass ratio of first graphite particles, natural graphite, silicon-based materials, styrene-butadiene rubber binder, acetylene black conductive agent, and SnS@CNT in the second negative electrode slurry is 55.89:37.26:2:2.5:0.35:2; and the positive electrode active material used in preparing the positive electrode is LiNi. 0.65 C 0.15 Mn 0.2 Everything else is the same. Among them, the silicon-based material is carbon-coated silicon, with a coating weight of 30% by mass of silicon.

[0286] The secondary batteries prepared in Examples 19-21 were subjected to negative electrode rebound / expansion tests and low-temperature charge-discharge capacity retention tests, using the same methods as in Examples 1-7. The test results are shown in Table 5.

[0287] Table 5

[0288]

[0289] Example 22

[0290] The secondary battery of Example 22 is prepared in a similar manner to the secondary battery of Example 1, except that: when preparing the negative electrode sheet in Example 22, the same amount of one-dimensional conductive agent carbon fiber is used instead of one-dimensional conductive agent CNT to obtain carbon fiber coated SnS, i.e. SnS@carbon fiber; all other aspects are the same.

[0291] Example 23

[0292] The secondary battery of Example 23 is prepared in a similar manner to the secondary battery of Example 1, except that: when preparing the negative electrode sheet in Example 23, the same amount of iron fiber is used to replace the one-dimensional conductive agent CNT to obtain SnS coated with iron fiber, i.e., SnS@iron fiber; all other aspects are the same.

[0293] Example 24

[0294] The secondary battery of Example 24 is prepared in a similar manner to the secondary battery of Example 1, except that: when preparing the negative electrode sheet in Example 24, the same amount of polythiophene is used to replace the one-dimensional conductive agent CNT to obtain polythiophene-coated SnS, i.e., SnS@polythiophene; all other aspects are the same.

[0295] The types of one-dimensional conductive agents contained in the second negative electrode active material layer of each secondary battery negative electrode sheet in Test Examples 22-24 are shown in Table 6.

[0296] The secondary batteries prepared in Examples 22-24 were subjected to negative electrode rebound / expansion tests and low-temperature charge-discharge capacity retention tests, using the same methods as in Examples 1-7. The test results are shown in Table 6.

[0297] Table 6

[0298]

[0299] Comparative Example 1

[0300] The secondary battery of Comparative Example 1 is prepared in a similar manner to the secondary battery of Example 1, except that SnS@CNT was not added when preparing the second negative electrode slurry of the negative electrode sheet in Comparative Example 1, and the mass ratio of the first graphite particles, natural graphite, styrene-butadiene rubber binder and acetylene black conductive agent in the second negative electrode slurry is 58.29:38.86:2.5:0.35; all other aspects are the same.

[0301] Comparative Example 2

[0302] The secondary battery of Comparative Example 2 is similar to the secondary battery of Example 1 in that the one-dimensional conductive agent CNT is not pre-coated linearly on the surface of the additive SnS when preparing the second negative electrode slurry of the negative electrode sheet in Comparative Example 2, but is added to the second negative electrode slurry at the same time; all of the above are the same.

[0303] Comparative Example 3

[0304] The secondary battery of Comparative Example 3 is similar to the secondary battery of Example 20 in that the one-dimensional conductive agent CNT is not pre-coated linearly on the surface of the additive SnS when preparing the second negative electrode slurry of the negative electrode sheet in Comparative Example 3, but is added to the second negative electrode slurry at the same time; all of the above are the same.

[0305] Comparative Example 4

[0306] The secondary battery of Comparative Example 4 is prepared in a similar manner to the secondary battery of Example 19, except that SnS@CNT was not added when preparing the second negative electrode slurry of the negative electrode sheet in Comparative Example 4, and the mass ratio of the first graphite particles, natural graphite, styrene-butadiene rubber binder and acetylene black conductive agent in the second negative electrode slurry is 58.2:38.8:2.5:0.5; all other aspects are the same.

[0307] Comparative Example 5

[0308] The secondary battery of Comparative Example 5 is prepared in a similar manner to the secondary battery of Example 19, except that: when preparing the second negative electrode slurry of the negative electrode sheet in Comparative Example 5, the one-dimensional conductive agent CNT was not pre-coated linearly on the surface of the additive SnS, but was added to the coating slurry at the same time; all of these are the same.

[0309] Comparative Example 6

[0310] The secondary battery of Comparative Example 6 is prepared in a similar manner to the secondary battery of Example 21, except that: when preparing the second negative electrode slurry of the negative electrode sheet in Comparative Example 6, the one-dimensional conductive agent CNT was not pre-coated linearly on the surface of the additive SnS, but was added to the coating slurry at the same time; all of these are the same.

[0311] Comparative Example 7

[0312] The secondary battery of Comparative Example 7 is similar to the secondary battery of Example 1 in that the first negative electrode slurry is not prepared when preparing the negative electrode sheet of Comparative Example 7. Instead, the second negative electrode slurry is directly applied to the surface of the negative electrode current collector, and the second negative electrode active material layer replaces the first negative electrode active material layer; all other aspects are the same.

[0313] Comparative Example 8

[0314] The secondary battery of Comparative Example 8 is prepared in a similar manner to the secondary battery of Example 1, except that: when preparing the second negative electrode slurry of the negative electrode sheet in Comparative Example 8, the one-dimensional conductive agent CNT was not linearly coated on the surface of the additive SnS, but the same amount of additive SnS without linear coating was directly added to replace it; everything else is the same.

[0315] The secondary batteries prepared in Comparative Examples 1-8 were subjected to negative electrode rebound / expansion tests and low-temperature charge-discharge capacity retention tests, using the same methods as in Examples 1-7. The test results are shown in Table 7.

[0316] Table 7

[0317]

[0318] As can be seen from the comparison of the results of the above embodiments and comparative examples, this application improves the low-temperature charging capability of the secondary battery by setting a second negative electrode active material layer in the negative electrode sheet, and the second negative electrode active material layer contains an additive with a one-dimensional conductive agent on its surface. At the same time, it can also reduce the impact of the introduction of additives on the cell capacity decay.

[0319] The description of the various embodiments above tends to emphasize the differences between the various embodiments. The similarities or similarities between them can be referred to, and for the sake of brevity, they will not be repeated here.

[0320] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.

Claims

1. A secondary battery, characterized in that, Includes a negative electrode sheet, wherein the negative electrode sheet comprises: Negative electrode current collector; A first negative electrode active material layer is located on at least one side surface of the negative electrode current collector, and the first negative electrode active material layer comprises a first negative electrode active material; and The second negative electrode active material layer is located on the surface of the first negative electrode active material layer away from the negative electrode current collector. The second negative electrode active material layer includes a second negative electrode active material and an additive. A one-dimensional conductive agent is disposed on the surface of the additive. The lithium intercalation potentials of the first and second negative electrode active materials at 25°C are each independently < 1.2V (Vs. Li). + / Li), the additive includes one or more of elemental tin, tin compounds and tin-containing alloys.

2. The secondary battery as described in claim 1, characterized in that, The one-dimensional conductive agent includes one or more of carbon nanotubes, carbon fibers, metal fibers, and conductive polymer fibers.

3. The secondary battery as described in claim 2, characterized in that, The carbon nanotubes include one or more of single-walled carbon nanotubes and multi-walled carbon nanotubes; and / or The carbon nanotubes have a diameter of 0.5 nm to 100 nm and a length of 10 μm to 1000 μm.

4. The secondary battery according to any one of claims 1 to 3, characterized in that, The tin compound includes one or more of SnO2, SnO, SnS, and SnF; and / or The tin-containing alloys include one or more of the following: tin-bismuth alloy, lithium-tin alloy, tin-copper alloy, tin-silver alloy, tin-selenium alloy, tin-tellurium alloy, and sodium-tin alloy.

5. The secondary battery according to any one of claims 1 to 4, characterized in that, The mass percentage of the one-dimensional conductive agent relative to the mass of the additive is 2%-100%; and / or The sum of the mass percentages of the additive and the one-dimensional conductive agent in the second negative electrode active material layer is 0.2%-10%, and can be selected as 1%-10%.

6. The secondary battery according to any one of claims 1 to 5, characterized in that, The second negative electrode active material includes one or more of graphite negative electrode materials and silicon-based negative electrode materials.

7. The secondary battery according to any one of claims 1 to 6, characterized in that, The second negative electrode active material includes graphite negative electrode material and silicon-based negative electrode material, and the graphite negative electrode material has a mass percentage content of ≥80% based on the total mass of the graphite negative electrode material and the silicon-based negative electrode material.

8. The secondary battery according to any one of claims 6 to 7, characterized in that, The graphite anode material includes first graphite particles, the first graphite particles having a Dv50 of 10μm-16μm and a specific surface area of ​​2m². 2 / g-6m 2 / g, OI value ≤3.

5.

9. The secondary battery as described in claim 8, characterized in that, The first graphite particles account for 25%-75% of the mass of the graphite anode material, and can be selected as 50%-75%.

10. The secondary battery according to any one of claims 6 to 9, characterized in that, The silicon-based anode material has a Dv50 of 15μm-20μm and a specific surface area of ​​1m². 2 / g-5m 2 / g.

11. The secondary battery according to any one of claims 1 to 10, characterized in that, The first negative electrode active material and the second negative electrode active material may be the same or different.

12. The secondary battery according to any one of claims 1 to 11, characterized in that, The secondary battery includes a positive electrode sheet, the positive electrode sheet includes a positive active material layer, the positive active material layer contains a positive active material, and the initial coulombic efficiency of the positive active material in a lithium metal half-cell is ≤90% at 25°C.

13. The secondary battery as described in claim 12, characterized in that, The positive electrode active material includes one or more of lithium nickel cobalt manganese oxide, lithium nickel oxide, and lithium manganese oxide.

14. The secondary battery as described in claim 13, characterized in that, The general chemical formula of the positive electrode active material is Li. 1+d [Ni x Co y Mn z M1 e O2, where 0.5≤x≤1, 0<y<0.3, 0<z≤1, 0<d<0.2, 0<e<0.2, x+y+z+e=1, and M1 is one or more of Mg, Ca, Sb, Ce, Ti, Zr, Sr, Al, Zn, Mo and B.

15. The secondary battery according to any one of claims 1 to 14, characterized in that, The secondary battery is a lithium-ion battery.

16. A method for preparing a secondary battery, characterized in that, The preparation method includes the step of preparing a negative electrode sheet, wherein the preparation of the negative electrode sheet includes: A first negative electrode active material layer is formed on at least one side surface of the negative electrode current collector, the first negative electrode active material layer comprising a first negative electrode active material; A one-dimensional conductive agent is linearly coated on the surface of an additive, wherein the additive includes one or more of elemental tin, tin compounds, and tin-containing alloys; A second negative electrode slurry is prepared, the second negative electrode slurry comprising a second negative electrode active material and the additive having the one-dimensional conductive agent linearly coated on its surface; The second negative electrode slurry is applied to the surface of the first negative electrode active material layer on the side away from the negative electrode current collector to form the second negative electrode active material layer; The lithium intercalation potentials of the first and second negative electrode active materials at 25°C are each independently < 1.2V (Vs. Li). + / Li).

17. The preparation method according to claim 16, characterized in that, The mass ratio of the one-dimensional conductive agent to the additive is (2-100):100; and / or The additive has a Dv50 of 1μm-15μm and a Dv99 of <40μm.

18. The preparation method according to any one of claims 16 to 17, characterized in that, The step of linearly coating a one-dimensional conductive agent onto the surface of the additive includes: The dispersion containing the one-dimensional conductive agent is mixed with the additive and then spray-dried to linearly coat the one-dimensional conductive agent on the surface of the additive.

19. The preparation method according to claim 18, characterized in that, The solvent for the dispersion includes one or more of water, polyvinyl alcohol, polyacrylic acid, such as polyethylene glycol, polyvinylpyrrolidone, N-methylpyrrolidone, and dimethyl sulfoxide; and / or The one-dimensional conductive agent accounts for 0.2%-5% of the mass of the dispersion.

20. A negative electrode sheet, characterized in that, include: Negative electrode current collector; A first negative electrode active material layer is located on at least one side surface of the negative electrode current collector, and the first negative electrode active material layer contains a first negative electrode active material; as well as The second negative electrode active material layer is located on the surface of the first negative electrode active material layer away from the negative electrode current collector. The second negative electrode active material layer includes a second negative electrode active material and an additive. A one-dimensional conductive agent is disposed on the surface of the additive. The lithium intercalation potentials of the first and second negative electrode active materials at 25°C are each independently < 1.2V (Vs. Li). + / Li), the additive includes one or more of elemental tin, tin compounds and tin-containing alloys.

21. The negative electrode sheet as described in claim 20, characterized in that, The negative electrode sheet in the secondary battery according to any one of claims 2 to 11.

22. An electrical appliance, characterized in that, It includes one or more of the secondary batteries described in any one of claims 1 to 15 and the secondary batteries prepared by the preparation method described in any one of claims 16 to 19.