Non-aqueous electrolyte secondary battery and method for manufacturing the same
By forming an SEI film containing Al, Ti, and B elements on the surface of the negative electrode active material, the problems of internal short circuits and resistance characteristics caused by conductive foreign matter in non-aqueous electrolyte secondary batteries are solved, heat release suppression and resistance optimization are achieved, and high capacity performance is maintained.
Patent Information
- Application Number
- CN202610671937.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2025-05-22
- Filing Date
- 2026-05-15
- Publication Date
- 2026-11-24
AI Technical Summary
In non-aqueous electrolyte secondary batteries using lithium composite oxides with a high nickel content, internal short circuits caused by conductive foreign matter lead to heat generation and poor resistance characteristics.
An SEI film containing at least one element, Al and Ti, and element B is formed on the surface of the negative electrode active material. By controlling the amount of these elements within a certain range, the heat release during internal short circuits caused by conductive foreign matter is suppressed, and the resistance characteristics are optimized.
It effectively suppresses heat release during internal short circuits, improves the battery's resistance characteristics, and maintains high capacity performance.
Smart Images

Figure CN123162272A_ABST
Abstract
Description
Technical Field
[0001] This disclosure relates to non-aqueous electrolyte secondary batteries and methods for manufacturing the same. It should be noted that this application claims priority to Japanese Patent Application No. 2025-085889, filed May 22, 2025, the entire contents of which are incorporated herein by reference. Background Technology
[0002] In recent years, from the perspective of the SDGs (Safety, General and Technical Regulations), the demand for battery electric vehicles (BEVs) and plug-in hybrid electric vehicles (PHEVs) using non-aqueous electrolyte secondary batteries, such as lithium-ion batteries, has been continuously growing. From the perspective of extending the driving range of BEVs and PHEVs, there is a desire for further increases in the capacity of non-aqueous electrolyte secondary batteries.
[0003] Typical examples of positive electrode active materials for lithium-ion secondary batteries include lithium composite oxides (e.g., lithium nickel cobalt manganese composite oxides). It is known that when using lithium composite oxides with a high proportion of nickel, it is possible to increase the capacity of non-aqueous electrolyte secondary batteries (e.g., see Patent Document 1).
[0004] Existing technical documents
[0005] Patent documents
[0006] Patent Document 1: Japanese Patent Application Publication No. 2024-173646 Summary of the Invention
[0007] However, in non-aqueous electrolyte secondary batteries using lithium composite oxides with a high nickel content, internal short circuits caused by conductive foreign matter mixed into the battery can easily lead to heat generation. On the other hand, excellent resistance characteristics are required in non-aqueous electrolyte secondary batteries.
[0008] Therefore, the purpose of this disclosure is to provide a non-aqueous electrolyte secondary battery that suppresses heat release during internal short circuits caused by conductive foreign matter and has excellent resistance characteristics.
[0009] The non-aqueous electrolyte secondary battery disclosed herein comprises a positive electrode, a negative electrode, and a non-aqueous electrolyte. The positive electrode has a positive electrode active material layer containing a positive electrode active material. The negative electrode has a negative electrode active material layer containing a negative electrode active material. The positive electrode active material comprises a lithium composite oxide having the composition represented by the following formula (1). The negative electrode active material has an SEI film on its surface. The SEI film contains at least one element of Al and Ti, and element B. The amount of at least one element of Al and Ti contained in the SEI film is 20 μg to 200 μg per 1g of the negative electrode active material. The amount of element B contained in the SEI film is 120 μg to 380 μg per 1g of the negative electrode active material.
[0010] Li 1+a Ni x Co y Mn z M1 b1 M2 c O2 …(1)
[0011] (In the formula, M1 is at least one of Al and Ti, M2 is at least one element selected from Zr, Mo, W, Nb, Mg, Ca, Na, Fe, Cr, Zn and Sn, a satisfies 0≤a≤0.1, x satisfies 0.8≤x<1, y satisfies 0≤y≤0.15, z satisfies 0≤z≤0.15, b1 satisfies 0≤b1<0.05, and c satisfies 0≤c≤0.05.)
[0012] Based on this configuration, a non-aqueous electrolyte secondary battery can be provided, which suppresses heat generation during internal short circuits caused by conductive foreign matter and exhibits excellent resistance characteristics.
[0013] From another perspective, the method for manufacturing a non-aqueous electrolyte secondary battery disclosed herein includes: a preparation step, preparing an assembly having a positive electrode, a negative electrode, and a non-aqueous electrolyte; and an activation step, performing an activation treatment on the assembly. The positive electrode has a positive electrode active material layer containing a positive electrode active material. The negative electrode has a negative electrode active material layer containing a negative electrode active material. The positive electrode active material comprises a lithium composite oxide represented by the following formula (2). The non-aqueous electrolyte contains lithium bis(oxalato)borate. The activation step is performed by forming an SEI film from lithium bis(oxalato)borate on the surface of the negative electrode active material, the SEI film containing at least one element of Al and Ti, and element B, wherein the amount of at least one element of Al and Ti contained in the SEI film is 20 μg to 200 μg per 1g of the negative electrode active material, and the amount of element B contained in the SEI film is 120 μg to 380 μg per 1g of the negative electrode active material.
[0014] Li 1+a Ni x Co y Mn z M1 b2 M2 c O2 …(2)
[0015] (In the formula, M1 is at least one of Al and Ti, M2 is at least one element selected from Zr, Mo, W, Nb, Mg, Ca, Na, Fe, Cr, Zn and Sn, a satisfies 0≤a≤0.1, x satisfies 0.8≤x<1, y satisfies 0≤y≤0.15, z satisfies 0≤z≤0.15, b2 satisfies 0<b2≤0.05, and c satisfies 0≤c≤0.05.)
[0016] Based on this configuration, it is possible to manufacture a non-aqueous electrolyte secondary battery that suppresses heat generation during internal short circuits caused by conductive foreign matter and exhibits excellent resistance characteristics. Attached Figure Description
[0017] Figure 1 This is a schematic cross-sectional view illustrating the internal structure of a lithium-ion secondary battery according to one embodiment of the present disclosure.
[0018] Figure 2 This is an exploded schematic diagram showing the configuration of the wound electrode body of a lithium-ion secondary battery according to one embodiment of the present disclosure. Detailed Implementation
[0019] Hereinafter, embodiments of the present disclosure will be described with reference to the accompanying drawings. It should be noted that matters not mentioned in this specification but necessary for the implementation of this disclosure can be grasped as design matters by those skilled in the art based on prior art. This disclosure can be implemented based on the content disclosed in this specification and common technical knowledge in the field. Furthermore, in the following drawings, components and parts that perform the same function are labeled with the same symbols. Additionally, the dimensional relationships (length, width, thickness, etc.) in the drawings do not reflect actual dimensional relationships. It should be noted that the numerical range referred to as "A to B" in this specification includes both A and B.
[0020] It should be noted that in this manual, "secondary battery" refers to a rechargeable and rechargeable energy storage device. Additionally, in this manual, "lithium-ion secondary battery" refers to a secondary battery that uses lithium ions as charge carriers and achieves charging and discharging through the transfer of charge between the positive and negative electrodes, accompanied by lithium ions.
[0021] The present disclosure will now be described in detail using a flat square lithium-ion secondary battery having a flat-shaped wound electrode body and a flat-shaped battery casing as an example, but it is not intended to limit the present disclosure to the scope described in the above embodiments.
[0022] Figure 1The lithium-ion secondary battery 100 shown is a sealed battery constructed by housing a flat, wound electrode body 20 and a non-aqueous electrolyte 80 within a flat, square battery casing (i.e., outer container) 30. The battery casing 30 is provided with a positive terminal 42 and a negative terminal 44 for external connection, as well as a thin-walled safety valve 36, which is configured to release internal pressure when the internal pressure of the battery casing 30 rises above a predetermined level. Additionally, the battery casing 30 is provided with an injection port (not shown) for injecting the non-aqueous electrolyte 80. The positive terminal 42 is electrically connected to a positive current collector 42a. The negative terminal 44 is electrically connected to a negative current collector 44a. As the material for the battery casing 30, lightweight and thermally conductive metal materials such as aluminum can be used, for example. It should be noted that... Figure 1 This does not accurately represent the amount of non-aqueous electrolyte 80.
[0023] like Figure 1 and Figure 2 As shown, the wound electrode body 20 has a configuration in which a positive electrode sheet 50 and a negative electrode sheet 60 are overlapped and wound along their long sides, separated by two elongated insulating sheets 70. The positive electrode sheet 50 has a configuration in which a positive electrode active material layer 54 is formed on one or both sides (here, both sides) of the elongated positive electrode current collector 52 along its long side. The negative electrode sheet 60 has a configuration in which a negative electrode active material layer 64 is formed on one or both sides (here, both sides) of the elongated negative electrode current collector 62 along its long side. The non-formed portions 52a of the positive electrode active material layer (i.e., the portions of the positive electrode current collector 52 that do not form the positive electrode active material layer 54 and are exposed) and the non-formed portions 62a of the negative electrode active material layer (i.e., the portions of the negative electrode current collector 62 that do not form the negative electrode active material layer 64 and are exposed) are formed in such a way that they protrude outward from both ends of the winding axis of the wound electrode body 20 (i.e., the sheet width direction orthogonal to the aforementioned long side direction). The non-forming portion 52a of the positive electrode active material layer and the non-forming portion 62a of the negative electrode active material layer are respectively bonded to the positive electrode current collector 42a and the negative electrode current collector 44a.
[0024] As the positive current collector 52 constituting the positive electrode sheet 50, a known positive current collector used in lithium-ion secondary batteries can be used. Examples of such current collectors include sheets or foils made of metals with good conductivity (e.g., aluminum, nickel, titanium, stainless steel, etc.). Aluminum foil is preferred as the positive current collector 52.
[0025] The size of the positive current collector 52 is not particularly limited, and can be appropriately determined according to the battery design. When aluminum foil is used as the positive current collector 52, its thickness is not particularly limited, for example, it is 5μm to 35μm, preferably 7μm to 20μm.
[0026] The positive electrode active material layer 54 contains a positive electrode active material. In this disclosure, a lithium composite oxide with a high nickel content and containing at least one of Al and Ti can be used as the positive electrode active material. In the lithium composite oxide, the content of Ni relative to metal elements other than Li is 80 mol% or more.
[0027] Specifically, the positive electrode active material contains a lithium composite oxide having the composition represented by the following formula (1).
[0028] Li 1+a Ni x Co y Mn z M1 b1 M2 c O2 …(1)
[0029] (In the formula, M1 is at least one of Al and Ti. M2 is at least one element selected from Zr, Mo, W, Nb, Mg, Ca, Na, Fe, Cr, Zn and Sn. a satisfies 0 ≤ a ≤ 0.1. x satisfies 0.8 ≤ x < 1. y satisfies 0 ≤ y ≤ 0.15. z satisfies 0 ≤ z ≤ 0.15. b1 satisfies 0 ≤ b1 < 0.05. c satisfies 0 ≤ c ≤ 0.05.)
[0030] The lithium composite oxide is preferably a lithium-nickel-cobalt-manganese composite oxide. Therefore, in equation (1), preferably y satisfies 0 < y ≤ 0.15 and z satisfies 0 < z ≤ 0.15, more preferably y satisfies 0.05 ≤ y ≤ 0.15 and z satisfies 0.05 ≤ z ≤ 0.15. b1 preferably satisfies 0 ≤ b1 ≤ 0.04, more preferably 0 ≤ b1 ≤ 0.03. c can be 0.
[0031] The positive electrode active material may consist solely of a lithium composite oxide having the composition represented by the above formula (1), or may further contain compounds other than the lithium composite oxide having the composition represented by the above formula (1) to function as an active material, to the extent that it does not significantly impair the effects of this disclosure.
[0032] The average particle size (median particle size: D50) of the positive electrode active material is not particularly limited, but is, for example, 0.05 μm to 25 μm, preferably 1 μm to 20 μm, and more preferably 3 μm to 15 μm. It should be noted that the average particle size (D50) of the positive electrode active material can be determined, for example, by laser diffraction scattering.
[0033] The positive electrode active material layer 54 may also contain components other than the positive electrode active material, such as lithium triphosphate, conductive materials, binders, etc. As conductive materials, carbon black such as acetylene black (AB), carbon fibers such as vapor-grown carbon fibers (VGCF), carbon nanotubes (CNTs), and other carbon materials (such as graphite) can be appropriately used. As binders, polyvinylidene fluoride (PVdF) can be used, for example.
[0034] The content of the positive electrode active material in the positive electrode active material layer 54 (i.e., the content of the positive electrode active material relative to the total mass of the positive electrode active material layer 54) is not particularly limited, but is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 85% by mass to 99% by mass. The content of trilithium phosphate in the positive electrode active material layer 54 is not particularly limited, but is preferably 0.1% by mass to 15% by mass, more preferably 0.2% by mass to 10% by mass. The content of conductive material in the positive electrode active material layer 54 is not particularly limited, but is preferably 0.1% by mass to 20% by mass, more preferably 0.3% by mass to 15% by mass. The content of binder in the positive electrode active material layer 54 is not particularly limited, but is preferably 0.4% by mass to 15% by mass, more preferably 0.5% by mass to 10% by mass.
[0035] The thickness of the positive electrode active material layer 54 is not particularly limited, for example, it is 10μm to 400μm, preferably 20μm to 300μm or less.
[0036] The positive electrode 50 may contain an insulating layer (not shown) at the boundary between the non-forming portion 52a of the positive electrode active material layer and the positive electrode active material layer 54. This insulating layer may contain, for example, ceramic particles.
[0037] As the negative electrode current collector 62 constituting the negative electrode sheet 60, a known negative electrode current collector used in lithium-ion secondary batteries can be used. Examples of such current collectors include sheets or foils made of metals with good conductivity (e.g., copper, nickel, titanium, stainless steel, etc.). Copper foil is preferred as the negative electrode current collector 62.
[0038] The size of the negative electrode current collector 62 is not particularly limited, and can be appropriately determined according to the battery design. When copper foil is used as the negative electrode current collector 62, its thickness is not particularly limited, for example, it is 5μm to 35μm, preferably 7μm to 20μm.
[0039] The negative electrode active material layer 64 contains a negative electrode active material. Examples of such a negative electrode active material include carbon-based negative electrode active materials such as graphite, hard carbon, and soft carbon; Si-based negative electrode active materials such as Si, silicon oxide, silicon carbide, and silicon nitride; Sn-based negative electrode active materials such as tin, tin oxide, tin nitride, and tin-containing alloys; and Si-C composite materials. Among these, graphite and Si-C composite materials are preferred. The graphite can be natural graphite or artificial graphite, and can be amorphous carbon-coated graphite in the form of amorphous carbon material. Examples of Si-C composite materials include materials comprising a carbon porous body and Si particles, with the Si particles disposed within the cavities of the porous body.
[0040] The negative electrode active material has an SEI (Solid Electrolyte Interface) film on its surface. That is, an SEI film is formed on the surface of the negative electrode active material. The SEI film is a film formed on the surface of the negative electrode active material by decomposition of a non-aqueous electrolyte or the like. In this disclosure, the SEI film contains at least one element of Al and Ti, as well as element B. Moreover, in this disclosure, the amount of at least one element of Al and Ti contained in the SEI film (hereinafter, sometimes referred to as "Al and Ti elemental content") is 20 μg to 200 μg per 1g of negative electrode active material. In addition, the amount of element B contained in the SEI film is 120 μg to 380 μg per 1g of negative electrode active material.
[0041] In a non-aqueous electrolyte secondary battery, when an internal short circuit (i.e., current flow between the positive and negative electrodes) occurs due to the presence of conductive foreign matter, heat is first released through the current flow caused by the conductive foreign matter. Then, this heat release triggers a reaction between the negative electrode and the non-aqueous electrolyte, leading to further heat release through the heat of reaction. Next, the heat of reaction between the negative electrode and the non-aqueous electrolyte triggers a reaction between the positive electrode and the non-aqueous electrolyte, leading to even further heat release. Thus, when an internal short circuit occurs due to conductive foreign matter, a chain reaction is triggered by the heat release, thereby increasing the amount of heat released.
[0042] In contrast, in this disclosure, the SEI film contains at least one element of Al and Ti in specified amounts, and an element of B in specified amounts. Therefore, in the event of an internal short circuit caused by conductive foreign matter, the reaction between the negative electrode and the non-aqueous electrolyte can be suppressed. Consequently, the heat of reaction between the negative electrode and the non-aqueous electrolyte is less likely to be generated, and the reaction between the positive electrode and the non-aqueous electrolyte is also suppressed. As a result, exothermic reactions are less likely to occur. Furthermore, according to such an SEI film, the resistance of the non-aqueous electrolyte secondary battery can be significantly reduced.
[0043] The Al and Ti in the SEI film typically originate from the Al and Ti contained in the positive electrode active material, respectively. If the amount of Al and Ti in the SEI film is too low, the exothermic suppression effect will be reduced. Therefore, the amount of Al and Ti in the SEI film is 20 μg or more per 1g of negative electrode active material, preferably 30 μg or more, more preferably 60 μg or more, and even more preferably 80 μg or more. On the other hand, if the amount of Al and Ti is too high, the resistance of the lithium-ion secondary battery 100 will increase. Therefore, the amount of Al and Ti in the SEI film is 200 μg or less per 1g of negative electrode active material, preferably 180 μg or less, more preferably 150 μg or less, and even more preferably 130 μg or less.
[0044] From the perspective of achieving a high level of balance between heat suppression and resistivity, the amount of Al and Ti elements in the SEI film is preferably 30 μg to 180 μg per 1g of negative electrode active material, more preferably 60 μg to 150 μg. When resistivity is important, the amount of Al and Ti elements in the SEI film is preferably 30 μg to 100 μg per 1g of negative electrode active material. When heat suppression is important, the amount of Al and Ti elements in the SEI film is preferably 115 μg to 200 μg per 1g of negative electrode active material.
[0045] The boron (B) element in the SEI film typically originates from the film-forming agent, lithium bis(oxalatoborate) (LiBOB), contained in the non-aqueous electrolyte. If the amount of B in the SEI film is too small, the exothermic suppression effect will be diminished. Therefore, the amount of B in the SEI film is 120 μg or more per 1g of negative electrode active material, preferably 140 μg or more, more preferably 160 μg or more, and even more preferably 180 μg or more. On the other hand, if the amount of B is too large, the resistance of the lithium-ion secondary battery 100 increases. Therefore, the amount of B in the SEI film is 380 μg or less per 1g of negative electrode active material, preferably 350 μg or less, more preferably 300 μg or less, and even more preferably 250 μg or less.
[0046] SEI film can form a layer that completely covers the surface of the negative electrode active material. Alternatively, SEI film can be distributed in an island-like pattern on the surface of the negative electrode active material.
[0047] The average particle size (median particle size: D50) of the negative electrode active material is not particularly limited, for example, it is 0.1 μm to 50 μm, preferably 1 μm to 25 μm, and more preferably 5 μm to 20 μm. It should be noted that the average particle size (D50) of the negative electrode active material can be determined, for example, by laser diffraction scattering.
[0048] The negative electrode active material layer 64 may contain components other than the active material, such as binders and conductive materials. Examples of binders include styrene-butadiene rubber (SBR), carboxymethyl cellulose (CMC), polyacrylic acid, and polyvinylidene fluoride (PVDF). CMC may also function as a tackifier. Examples of conductive materials that may be contained in the positive electrode active material layer 54 include substances such as...
[0049] The content of negative electrode active material in the negative electrode active material layer 64 is preferably 90% by mass or more, more preferably 95% to 99% by mass. The content of binder in the negative electrode active material layer 64 is preferably 0.1% to 8% by mass, more preferably 0.5% to 3% by mass. The content of thickener in the negative electrode active material layer 64 is preferably 0.3% to 3% by mass, more preferably 0.5% to 2% by mass.
[0050] The thickness of the negative electrode active material layer 64 is not particularly limited, for example, it is 10μm to 400μm, preferably 20μm to 300μm.
[0051] As the separator 70, examples include porous sheets (membranes) made of resins such as polyethylene (PE), polypropylene (PP), polyester, cellulose, and polyamide. The porous sheet can be a single-layer structure or a multi-layered structure with two or more layers (for example, a three-layer structure with PP layers laminated on both sides of a PE layer). A heat-resistant layer (HRL) can be provided on the surface of the separator 70.
[0052] The thickness of the spacer 70 is not particularly limited, for example, it is 5μm to 50μm, preferably 10μm to 30μm. The air permeability of the spacer 70 obtained by the Gurley test method is not particularly limited, but preferably 350 seconds / 100cc or less.
[0053] The non-aqueous electrolyte 80 typically contains a non-aqueous solvent and a supporting salt (electrolyte salt). As the non-aqueous solvent, organic solvents commonly used in electrolytes of lithium-ion secondary batteries, such as carbonates, ethers, esters, nitriles, sulfones, and lactones, can be used without particular restriction. Among these, carbonates and esters are preferred, and specific examples include ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), ethylene monofluorocarbonate (MFEC), ethylene difluorocarbonate (DFEC), methyl monofluoromethyl difluoromethyl carbonate (F-DMC), dimethyl trifluorocarbonate (TFDMC), methyl acetate, and methyl propionate. Such non-aqueous solvents can be used alone or in appropriate combinations of two or more.
[0054] As a supporting salt, lithium salts such as LiPF6, LiBF4, and lithium bis(fluorosulfonyl)imide (LiFSI) (preferably LiPF6) can be used appropriately. The concentration of the supporting salt is preferably 0.7 mol / L to 1.3 mol / L.
[0055] Additionally, the non-aqueous electrolyte 80 may contain lithium bis(oxalatoborate) (LiBOB) as the boron source for the SEI film. LiBOB is a film-forming agent. The non-aqueous electrolyte 80 may also be completely free of LiBOB by decomposing it. The concentration of LiBOB in the non-aqueous electrolyte 80 may be 0% to 0.3% by mass, 0% to 0.1% by mass, or 0% by mass.
[0056] It should be noted that the above-mentioned non-aqueous electrolyte 80 may also contain components other than those mentioned above, such as gas-generating agents like biphenyl (BP) and cyclohexylbenzene (CHB), and various additives like thickeners, as long as it does not significantly impair the effect of this disclosure.
[0057] Next, a preferred manufacturing method for the lithium-ion secondary battery 100 will be described. However, the lithium-ion secondary battery 100 is not limited to being manufactured by the following method.
[0058] The manufacturing method includes: a preparation step, which prepares an assembly having a positive electrode, a negative electrode, and a non-aqueous electrolyte; and an activation step, which activates the assembly. Here, the positive electrode has a positive electrode active material layer containing a positive electrode active material. The negative electrode has a negative electrode active material layer containing a negative electrode active material. The positive electrode active material contains a lithium composite oxide having the composition represented by the following formula (2). On the other hand, the non-aqueous electrolyte contains LiBOB.
[0059] Li 1+a Ni x Co y Mn z M1 b2 M2 c O2 …(2)
[0060] In equation (2), M1, M2, a, x, y, z, c have the same meaning as M1, M2, a, x, y, z, c in equation (1). b2 satisfies 0 < b2 ≤ 0.05, preferably satisfies 0.01 ≤ b2 ≤ 0.05, and more preferably satisfies 0.02 ≤ b2 ≤ 0.05.
[0061] In this activation process, an SEI film derived from LiBOB is formed on the surface of the negative electrode active material. Furthermore, the activation is performed under the following conditions: the SEI film contains at least one element of Al and Ti, and element B. The amount of at least one element of Al and Ti contained in the SEI film is 20 μg to 200 μg per 1g of negative electrode active material. The amount of element B contained in the SEI film is 120 μg to 380 μg per 1g of negative electrode active material.
[0062] First, the preparation process will be explained. The assembly prepared in this preparation process is equivalent to the lithium-ion secondary battery 100 before the activation treatment.
[0063] The positive electrode can be prepared as follows. A lithium composite oxide having the composition represented by the above formula (2) is prepared as the positive electrode active material. The positive electrode active material and any component of the positive electrode active material layer 54 (e.g., conductive material, binder, etc.) are mixed in a dispersion medium (e.g., N-methylpyrrolidone, etc.) to prepare a slurry for forming the positive electrode active material layer. The slurry for forming the positive electrode active material layer is coated onto the positive electrode current collector 52 and dried to form the positive electrode active material layer. If necessary, the positive electrode active material layer is subjected to pressure treatment. A positive electrode sheet can be obtained from this. This positive electrode sheet differs from the positive electrode sheet 50 described above in that the positive electrode active material contains more of at least one element of Al and Ti. This is because at least one element of Al and Ti will dissolve in the activation process below.
[0064] The negative electrode can be prepared as follows: A slurry for forming the negative electrode active material layer 64 is prepared by mixing the negative electrode active material and any component of the negative electrode active material layer 64 (e.g., binder, thickener, etc.) in a dispersion medium (e.g., water). This slurry is then coated onto the negative electrode current collector 62 and dried to form the negative electrode active material layer 64. If necessary, the negative electrode active material layer 64 is subjected to pressure treatment. This yields a negative electrode sheet. This negative electrode sheet differs from the negative electrode sheet 60 described above in that an SEI film is not formed on the surface of the negative electrode active material. This is because an SEI film is formed on the surface of the negative electrode active material during the activation process described below.
[0065] It should be noted that in this specification, "slurry" refers to a mixture in which some or all of the solid components are dispersed in a solvent, including so-called "paste" and "ink".
[0066] On the other hand, a battery casing 30 and a non-aqueous electrolyte are prepared. The non-aqueous electrolyte contains lithium bis(oxalatoborate) (LiBOB) as the boron source for the SEI film. This non-aqueous electrolyte differs from the aforementioned non-aqueous electrolyte 80 in that it has a higher LiBOB concentration. This is because some or all of the LiBOB will decompose during the activation process below. Here, the amount of boron in the SEI film formed by the activation process can be adjusted according to the LiBOB concentration in the non-aqueous electrolyte. Specifically, the higher the LiBOB concentration in the non-aqueous electrolyte, the higher the amount of boron in the SEI film. The LiBOB concentration in the non-aqueous electrolyte is appropriately selected according to the target amount of boron in the SEI film, for example, from 0.1% to 1.0% by mass, preferably from 0.2% to 0.8% by mass.
[0067] Prepare the separator 70, and fabricate the electrode body using the positive electrode, negative electrode, and separator 70 according to known methods. Contain the fabricated electrode body and the prepared non-aqueous electrolyte in the battery casing 30.
[0068] Specifically, for example, in the case where the electrode body is a wound electrode body as shown in the example, such as... Figure 2 As shown, a laminate is formed by overlapping positive and negative electrode sheets with two separators 70. After forming a wound body by winding the laminate along its long side, the wound body is flattened by pressure treatment or the like, thereby forming an electrode body. When the electrode body is a laminated electrode body, the electrode body is formed by alternately stacking multiple positive and multiple negative electrode sheets while sandwiching separators 70 between them.
[0069] As the battery casing 30, for example, a casing body having an opening and a cover sealing the opening are prepared. The cover is provided with an injection port for injecting a non-aqueous electrolyte.
[0070] A positive terminal 42 and a positive current collector 42a, and a negative terminal 44 and a negative current collector 44a are mounted on the cover of the battery casing 30. The positive current collector 42a and the negative current collector 44a are respectively joined to the non-formed portions 52a and 62a of the positive active material layer exposed at the ends of the electrode body. Then, the electrode body is received inside the opening of the casing body of the battery casing 30, and the casing body of the battery casing 30 is welded to the cover.
[0071] Next, a non-aqueous electrolyte is injected through the injection port, and then the injection port is sealed. This yields an assembly containing a positive electrode, a negative electrode, and a non-aqueous electrolyte.
[0072] Next, the activation process will be described. In the activation process, the obtained assembly is activated. This activation process includes a step of charging at a specified voltage as an initial charge. In the activation process, the assembly is typically charged to a specified charge state at a specified temperature and maintained in this charge state for a specified time. As a result, the components contained in the non-aqueous electrolyte are decomposed, and an SEI film is formed on the surface of the negative electrode active material. At this time, at least LiBOB contained in the non-aqueous electrolyte is decomposed. As a result, the SEI film contains the decomposition products of LiBOB, and therefore, the SEI film contains element B. In addition, at least one element of Al and Ti contained in the positive electrode active material is dissolved. As a result, at least one element of Al and Ti dissolved in the positive electrode active material is introduced into the SEI film. Therefore, the SEI film contains at least one element of Al and Ti. For the decomposition of LiBOB and the dissolution of Al and Ti contained in the positive electrode active material, the activation process preferably includes a step of charging the assembly to a charge state of 4.0V or higher.
[0073] Furthermore, the activation treatment is carried out in such a way that the amount of Al and Ti elements contained in the SEI film is 20μg to 200μg per 1g of negative electrode active material, and the amount of B element is 120μg to 380μg per 1g of negative electrode active material.
[0074] Here, the higher the amount of at least one element, Al or Ti, in the positive electrode active material, the greater the amount of Al and Ti in the SEI film. Higher activation temperatures also tend to result in a greater amount of Al and Ti in the SEI film. Higher battery voltages after activation treatment also tend to result in a greater amount of Al and Ti in the SEI film. Longer activation times also tend to result in a greater amount of Al and Ti in the SEI film.
[0075] The activation treatment can be carried out at room temperature (i.e., 25°C ± 10°C) or under heat. The activation temperature can be, for example, 15°C to 40°C (especially 15°C to 35°C). The battery voltage for activation can be, for example, 4.0V to 4.5V (especially 4.1V to 4.4V). The activation time can be, for example, 30 minutes to 24 hours. Therefore, the activation time can be appropriately selected from these ranges, taking into account the aforementioned trends.
[0076] It should be noted that the amount of element B depends on the concentration of LiBOB in the non-aqueous electrolyte. Under the activation treatment conditions where the amounts of Al and Ti are adjusted, the influence of the activation treatment conditions is relatively small.
[0077] The activation process described above can be performed using a known charger, etc. A lithium-ion secondary battery 100 can be obtained by operating as described above.
[0078] In the lithium-ion secondary battery 100, heat release during internal short circuits caused by conductive foreign matter is suppressed. The lithium-ion secondary battery 100 has low internal resistance, resulting in excellent resistance characteristics. Furthermore, the lithium-ion secondary battery 100 has a high capacity because it uses a lithium composite oxide with a high nickel content in the positive electrode active material.
[0079] The lithium-ion secondary battery 100 can be used for a variety of applications. Specific applications include portable power supplies for personal computers, portable electronic devices, mobile terminals, etc.; power supplies for vehicles such as battery electric vehicles (BEVs), hybrid electric vehicles (HEVs), and plug-in hybrid electric vehicles (PHEVs); and batteries for small energy storage devices, with vehicle power supplies being the preferred option. The lithium-ion secondary battery 100 can also typically be used in the form of a battery pack consisting of multiple battery cells connected in series and / or parallel.
[0080] The above description, as an example, illustrates a square lithium-ion secondary battery 100 having a flat, wound electrode body 20. However, the lithium-ion secondary battery can also be configured as a lithium-ion secondary battery having a stacked electrode body (i.e., an electrode body formed by alternating layers of multiple positive and multiple negative electrodes). Furthermore, the lithium-ion secondary battery can also be configured as a cylindrical lithium-ion secondary battery, a laminated shell type lithium-ion secondary battery, etc.
[0081] The non-aqueous electrolyte secondary battery disclosed herein can be configured as a non-aqueous electrolyte secondary battery other than a lithium-ion secondary battery according to known methods.
[0082] The following describes in detail the embodiments related to this disclosure, but it is not intended to limit this disclosure to the manner shown in the above embodiments.
[0083] [Examples 1-6 and Comparative Examples 1-14]
[0084] A lithium nickel cobalt manganese composite oxide (NCM) with the composition shown in Table 1 was prepared as the positive electrode active material. A slurry for forming the positive electrode active material layer was prepared by mixing NCM, acetylene black (AB) as a conductive material, and polyvinylidene fluoride (PVdF) as a binder with N-methylpyrrolidone (NMP) at a mass ratio of NCM:AB:PVdF = 100:1:1. This slurry was coated onto both sides of an aluminum foil (15 μm thick) in a strip and then dried to form the positive electrode active material layer. The positive electrode active material layer was rolled to a specified thickness, and the resulting sheet was processed into a specified size to fabricate the positive electrode sheet.
[0085] Graphite particles (average particle size (D50): 15 μm) were prepared as the negative electrode active material. Then, carboxymethyl cellulose (CMC) and styrene-butadiene rubber (SBR) were prepared as binders. They were mixed with water as a solvent in a weight ratio of graphite particles:CMC:SBR = 97:1:2 to prepare a slurry for forming the negative electrode active material layer.
[0086] The preparation of the slurry for forming the negative electrode active material layer is carried out as follows: First, graphite particles and CMC are dry-mixed using a stirred granulator. Then, a solvent (water) is added for solid-phase kneading and mixing. The solid content during solid-phase kneading and mixing is 65%. SBR and solvent (water) are further added to the mixture after solid-phase kneading and mixing. Thus, the slurry for forming the negative electrode active material layer is prepared. This slurry is coated on both sides of a copper foil (10 μm thick) in strip form and then dried to form the negative electrode active material layer. After the negative electrode active material layer is rolled to a specified thickness, the resulting sheet is processed into a specified size to manufacture the negative electrode sheet.
[0087] In addition, a porous polyolefin sheet with a three-layer structure of PP / PE / PP is prepared as a separator. The fabricated positive and negative electrode sheets are stacked in between the separator to form a laminated electrode body. In this laminated electrode body, the relative area between the positive and negative active material layers is 200 cm². 2 .
[0088] Current collector leads are installed on the positive and negative electrode plates, and the laminated electrode body is inserted into an outer casing made of aluminum laminated sheet. A non-aqueous electrolyte is injected into the interior of the outer casing, and the opening of the outer casing is sealed to fabricate the assembly. A solution containing LiPF6 as the supporting salt, dissolved at a concentration of 1 mol / L, and further containing LiBOB at a specified concentration, is used as the non-aqueous electrolyte. This solution contains ethylene carbonate (EC), fluoroethylene carbonate (FEC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) in a volume ratio of EC:FEC:EMC:DMC = 15:5:40:40.
[0089] The assembled assembly was placed in a constant temperature bath set to the temperatures shown in Table 1. The assembly was charged with a constant current of 0.2C to the voltage shown in Table 1, and then charged at a constant voltage for 1.5 hours. This charging was then maintained for the time shown in Table 1. Next, it was discharged with a constant current of 0.2C to 3.0V, and then discharged at a constant voltage for 1.5 hours. This activation treatment yielded the evaluation lithium-ion secondary batteries for each embodiment and comparative example. The discharge capacity of this evaluation lithium-ion secondary battery is 500mAh.
[0090] <Evaluation of Resistance Characteristics>
[0091] Each evaluation lithium-ion secondary battery was placed in a constant temperature bath at 25°C and adjusted to a charging state of 3.7V. Then, each evaluation lithium-ion secondary battery was placed in a constant temperature bath at -10°C and discharged for 10 seconds with a current of 2.0A. The voltage drop ΔV was measured during this period, and the output resistance of each evaluation lithium-ion secondary battery was determined using the voltage drop ΔV and the current value. The relative values of the output resistances of other test examples when the output resistance value of Example 1 was set to 100 were determined as the resistance ratio. The results are shown in Table 1.
[0092] <ICP Analysis of SEI Membrane>
[0093] After evaluating the initial characteristics, each lithium-ion secondary battery was disassembled under an argon atmosphere, and the negative electrode was removed. The negative electrode active material layer was peeled off from the copper foil, and a specified amount of the negative electrode active material layer was measured. The measured negative electrode active material layer was treated with hydrochloric acid to prepare a sample solution. The sample solution was quantitatively analyzed for Al, Ti, and B using a commercially available ICP emission spectrometer. The results are shown in Table 1. It should be noted that the values in Table 1 are the mass values in ppm of the negative electrode active material layer. Since the mass ratio of the negative electrode active material in the negative electrode active material layer is 97%, the value obtained by multiplying the value in Table 1 by 0.97 is the mass value (μg) of 1g of negative electrode active material.
[0094] <Evaluation of Negative Electrode Heat Release>
[0095] After evaluating the initial characteristics, each evaluation lithium-ion secondary battery was disassembled under an argon atmosphere, and the negative electrode was removed. The negative electrode active material layer was peeled off from the copper foil to obtain the negative electrode active material layer. 4 mg of the negative electrode active material layer was measured into a sample pan, and 2 μL of non-aqueous electrolyte was added to prepare the test sample. The test sample was subjected to DSC measurement using a commercially available DSC device at a heating rate of 2 °C / min. The onset temperature of the exothermic peak was determined using the obtained DSC curve and taken as the exothermic onset temperature (°C). The results are shown in Table 1. It should be noted that, considering measurement error, the onset temperature was confirmed every 10 °C.
[0096]
[0097] As described above, when an internal short circuit is caused by a conductive foreign object, heat is generated due to the current flow. This heat then causes the negative electrode to react with the non-aqueous electrolyte, further generating heat. This heat of reaction causes the positive electrode to react with the non-aqueous electrolyte, generating even more heat. A higher exothermic onset temperature (°C) in the DSC measurement indicates a greater ability to suppress the reaction between the negative electrode and the non-aqueous electrolyte, thus meaning that the heat generated during an internal short circuit caused by a conductive foreign object can be suppressed.
[0098] According to the results in Table 1, it can be seen that when the amount of Al and Ti elements in each 1g of negative electrode active material in the SEI film is 20μg~200μg, and the amount of B element is 120μg~380μg, the exothermic onset temperature is relatively high and the resistance is relatively low. Therefore, it can be concluded that, according to the non-aqueous electrolyte secondary battery of this disclosure, the exothermic reaction caused by internal short circuit due to conductive foreign matter is suppressed, and the resistance characteristics are excellent.
[0099] While the specific examples of this disclosure have been described in detail above, these are merely illustrative and do not limit the scope of patent protection. The technology described in the scope of patent protection includes technical solutions with various modifications and alterations to the specific examples illustrated above.
[0100] That is, the non-aqueous electrolyte secondary batteries disclosed herein are the following items [1] to [8].
[0101] [1] A non-aqueous electrolyte secondary battery, comprising a positive electrode, a negative electrode, and a non-aqueous electrolyte,
[0102] The aforementioned positive electrode has a positive electrode active material layer containing positive electrode active material.
[0103] The aforementioned negative electrode has a negative electrode active material layer containing negative electrode active material.
[0104] The above-mentioned positive electrode active material comprises a lithium composite oxide having the composition represented by the following formula (1),
[0105] The above-mentioned negative electrode active material has an SEI film on its surface.
[0106] The aforementioned SEI film contains at least one element, Al and Ti, as well as element B.
[0107] The amount of at least one element, Al and Ti, contained in the SEI membrane is 20 μg to 200 μg per 1g of the above-mentioned negative electrode active material.
[0108] The amount of element B contained in the SEI membrane is greater than 100 μg and less than 400 μg per 1g of the above negative electrode active material.
[0109] Li 1+a Ni x Co y Mn z M1 b1 M2 c O2 …(1)
[0110] (In the formula, M1 is at least one of Al and Ti, M2 is at least one element selected from Zr, Mo, W, Nb, Mg, Ca, Na, Fe, Cr, Zn and Sn, a satisfies 0≤a≤0.1, x satisfies 0.8≤x<1, y satisfies 0≤y≤0.15, z satisfies 0≤z≤0.15, b1 satisfies 0≤b1<0.05, and c satisfies 0≤c≤0.05.)
[0111] [2] According to the non-aqueous electrolyte secondary battery of item [1], wherein the amount of at least one element of Al and Ti contained in the SEI film is 30 μg to 180 μg per 1g of the above negative electrode active material.
[0112] The amount of element B contained in the SEI membrane is 150 μg to 300 μg per 1g of the above negative electrode active material.
[0113] [3] The non-aqueous electrolyte secondary battery according to item [1] or [2], wherein in the above formula (1), y satisfies 0.05≤y≤0.15 and z satisfies 0.05≤z≤0.15.
[0114] [4] A method for manufacturing a non-aqueous electrolyte secondary battery, comprising:
[0115] The preparation process involves preparing an assembly with a positive electrode, a negative electrode, and a non-aqueous electrolyte, as well as...
[0116] The activation process involves activating the above-mentioned assembly.
[0117] The aforementioned positive electrode has a positive electrode active material layer containing positive electrode active material.
[0118] The aforementioned negative electrode has a negative electrode active material layer containing negative electrode active material.
[0119] The above-mentioned positive electrode active material includes a lithium composite oxide represented by the following formula (2),
[0120] The above-mentioned non-aqueous electrolyte contains lithium bis(oxalate-borate).
[0121] The activation process described above is carried out as follows: an SEI film derived from lithium bis(oxalato)borate is formed on the surface of the negative electrode active material. The SEI film contains at least one element of Al and Ti, as well as element B. The amount of at least one element of Al and Ti contained in the SEI film is 20 μg to 200 μg per 1g of the negative electrode active material, and the amount of element B contained in the SEI film is 120 μg to 380 μg per 1g of the negative electrode active material.
[0122] Li 1+a Ni x Co y Mnz M1 b2 M2 c O2 …(2)
[0123] (In the formula, M1 is at least one of Al and Ti, M2 is at least one element selected from Zr, Mo, W, Nb, Mg, Ca, Na, Fe, Cr, Zn and Sn, a satisfies 0 ≤ a ≤ 0.1, x satisfies 0.8 ≤ x < 1, y satisfies 0 ≤ y ≤ 0.15, z satisfies 0 ≤ z ≤ 0.15, b2 satisfies 0 < b2 ≤ 0.05, and c satisfies 0 ≤ c ≤ 0.05.)
[0124] [5] According to the manufacturing method described in item [4], the amount of at least one element of Al and Ti contained in the SEI film is 30 μg to 180 μg per 1g of the above-mentioned negative electrode active material.
[0125] The amount of element B contained in the SEI membrane is 150 μg to 300 μg per 1g of the above negative electrode active material.
[0126] [6] According to the manufacturing method described in item [4] or [5], in the above formula (2), y satisfies 0.05≤y≤0.15 and z satisfies 0.05≤z≤0.15.
[0127] [7] The manufacturing method according to any one of [4] to [6], wherein the activation treatment includes the step of bringing the assembly to a charging state of 4.0V or higher.
[0128] [8] The manufacturing method according to any one of [4] to [7], wherein the concentration of lithium bis(oxalato)borate in the above-mentioned non-aqueous electrolyte is 0.2% to 0.8% by mass.
Claims
1. A non-aqueous electrolyte secondary battery, comprising a positive electrode, a negative electrode, and a non-aqueous electrolyte. The positive electrode has a positive electrode active material layer containing positive electrode active material. The negative electrode has a negative electrode active material layer containing negative electrode active material. The positive electrode active material comprises a lithium composite oxide having the composition represented by the following formula (1). The negative electrode active material has an SEI film on its surface. The SEI film contains at least one element, Al and Ti, as well as element B. The amount of at least one element, Al and Ti, contained in the SEI membrane is 20 μg to 200 μg per 1g of the negative electrode active material. The amount of boron in the SEI membrane is 120 μg to 380 μg per 1g of the negative electrode active material. Li 1+a Ni x Co y Mr z M1 b1 M2 c O2 …(1) In the formula, M1 is at least one of Al and Ti, M2 is at least one element selected from Zr, Mo, W, Nb, Mg, Ca, Na, Fe, Cr, Zn and Sn, a satisfies 0≤a≤0.1, x satisfies 0.8≤x<1, y satisfies 0≤y≤0.15, z satisfies 0≤z≤0.15, b1 satisfies 0≤b1<0.05, and c satisfies 0≤c≤0.
05.
2. The non-aqueous electrolyte secondary battery according to claim 1, wherein, The amount of at least one element, Al and Ti, contained in the SEI membrane is 30 μg to 180 μg per 1g of the negative electrode active material. The amount of element B contained in the SEI membrane is 150 μg to 300 μg per 1g of the negative electrode active material.
3. The non-aqueous electrolyte secondary battery according to claim 1, wherein, In equation (1), y satisfies 0.05≤y≤0.15, and z satisfies 0.05≤z≤0.
15.
4. A method for manufacturing a non-aqueous electrolyte secondary battery, comprising: The preparation process involves preparing an assembly with a positive electrode, a negative electrode, and a non-aqueous electrolyte, as well as... The activation process involves activating the assembly. The positive electrode has a positive electrode active material layer containing positive electrode active material. The negative electrode has a negative electrode active material layer containing negative electrode active material. The positive electrode active material comprises a lithium composite oxide represented by the following formula (2), The non-aqueous electrolyte contains lithium dioxaborate. The activation process is carried out as follows: an SEI film from lithium bis(oxalato)borate is formed on the surface of the negative electrode active material. The SEI film contains at least one element of Al and Ti, and element B. The amount of at least one element of Al and Ti contained in the SEI film is 20 μg to 200 μg per 1g of the negative electrode active material, and the amount of element B contained in the SEI film is 120 μg to 380 μg per 1g of the negative electrode active material. Li 1+a Ni x Co y Mr z M1 b2 M2 c O2 …(2) In the formula, M1 is at least one of Al and Ti, M2 is at least one element selected from Zr, Mo, W, Nb, Mg, Ca, Na, Fe, Cr, Zn and Sn, a satisfies 0≤a≤0.1, x satisfies 0.8≤x<1, y satisfies 0≤y≤0.15, z satisfies 0≤z≤0.15, b2 satisfies 0<b2≤0.05, and c satisfies 0≤c≤0.
05.
5. The manufacturing method according to claim 4, wherein, The amount of at least one element, Al and Ti, contained in the SEI membrane is 30 μg to 180 μg per 1g of the negative electrode active material. The amount of element B contained in the SEI membrane is 150 μg to 300 μg per 1g of the negative electrode active material.
6. The manufacturing method according to claim 4, wherein, In equation (2), y satisfies 0.05≤y≤0.15, and z satisfies 0.05≤z≤0.
15.
7. The manufacturing method according to claim 4, wherein, The activation process includes the step of bringing the assembly to a charging state of 4.0V or higher.
8. The manufacturing method according to claim 4, wherein, The concentration of lithium bis(oxalato)borate in the non-aqueous electrolyte is 0.2% to 0.8% by mass.
Citation Information
Patent Citations
Positive electrode active material for secondary battery
JP2024173646A
Fire-resistant coated beam and floor structure