A battery cell and a method of manufacturing the same
By applying an acid-responsive microcapsule protective coating to the surface of lithium-ion battery cells, acidic gases are captured and decomposed, releasing endothermic, adsorbent, and flame-retardant materials. This solves the problem of insufficient early chemical signal detection in lithium-ion battery thermal runaway, enabling early and precise intervention and multiple protections against thermal runaway, thus improving battery safety.
Patent Information
- Application Number
- CN202611092085.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-22
- Publication Date
- 2026-11-24
AI Technical Summary
Existing lithium-ion batteries lack the means to detect and effectively suppress early chemical signals of acidic gas generation during thermal runaway, making it difficult to interrupt the thermal runaway chain reaction in time and posing a risk of combustion and explosion.
An acid-responsive protective coating is applied to the surface of the separator, inner liner, shell, or safety valve of the battery cell. The acid-responsive microcapsules release the composite core material during thermal runaway, forming a cascade response mechanism of active capture-local enrichment-acid-responsive decomposition-multiple protection, including functions such as heat absorption, adsorption, flame retardancy, and fire extinguishing.
It enables early and precise intervention and multiple blocking of thermal runaway chain reactions, improves battery safety performance, and avoids the response lag and performance loss of traditional methods.
Smart Images

Figure CN123162273A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery technology, and in particular to a battery cell and its preparation method. Background Technology
[0002] Lithium-ion batteries are widely used in new energy vehicles, energy storage power stations, and consumer electronics due to their high energy density and long cycle life. However, the frequent battery combustion and explosion accidents in recent years have made battery safety a core bottleneck restricting the industry's development. Although lithium iron phosphate (LiFePO4) batteries have good thermal stability due to the stable structure of their cathode materials, they can still experience thermal runaway under thermal abuse conditions, releasing flammable and explosive gases such as hydrogen (H2), carbon monoxide (CO), methane (CH4), and ethylene (C2H4), as well as highly toxic gases such as hydrofluoric acid (HF). Studies have shown that the upper limit of explosion of gases generated during thermal runaway can reach 73.77%, while the lower limit of explosion of mixed gases can be as low as 4.83%.
[0003] Thermal runaway in lithium-ion batteries is a complex chain reaction process. When localized overheating occurs inside the battery, it first triggers the decomposition of lithium salts, generating acidic gases. For the currently mainstream lithium hexafluorophosphate (LiPF6) electrolyte system, LiPF6 begins to thermally decompose above 80°C, generating phosphorus pentafluoride (PF5) and hydrofluoric acid (HF). These acidic gases corrode the positive electrode material, dissolve transition metal ions, and damage the solid electrolyte interphase (SEI) film at the negative electrode, initiating more severe side reactions. Simultaneously, the acidic environment accelerates the decomposition of the electrolyte, producing large amounts of flammable gases, ultimately leading to thermal runaway, combustion, or even explosion. Studies have shown that the generation of acidic gases is a key initiation signal for the thermal runaway chain reaction, appearing earlier than a significant increase in temperature.
[0004] Existing technologies for improving battery safety mainly fall into the following categories: The first category is physical protection technologies, such as thermal management systems, explosion-proof valves, and positive temperature coefficient thermistors (PTCs). These measures are passive protections, relying on temperature conduction for response, exhibiting hysteresis, and unable to chemically suppress the root cause of thermal runaway. The second category is separator modification technologies, such as coating the separator with a ceramic layer to improve its heat shrinkage resistance. This method can prevent direct short circuits between the positive and negative electrodes, but cannot suppress electrolyte decomposition, gas generation, and combustion. The third category is electrolyte additive technology, adding flame retardants or film-forming additives to the electrolyte. However, traditional flame retardants significantly reduce the electrolyte's conductivity and negatively impact the battery's cycle life and rate performance. These additives persist under normal battery operation, representing a compromise of "sacrificing electrochemical performance for safety." The fourth category is external sensing triggering technology, using sensors to monitor battery temperature or voltage and injecting flame retardants or cutting off circuits through an external control system. The solution is complex in structure, expensive, and occupies a large space. Furthermore, its sensing and response speed is insufficient to cope with instantaneous thermal runaway.
[0005] In recent years, researchers have proposed the concept of smart responsive microcapsules, such as temperature-responsive microcapsules. Under thermal runaway conditions, the microcapsules rupture and release the substances encapsulated within. However, the trigger signal is temperature, and the response exhibits a hysteresis—by the time the temperature reaches the trigger threshold, thermal runaway has often already occurred. In contrast, the generation of acidic gases is an early chemical signal of thermal runaway, appearing much earlier than the increase in temperature.
[0006] Therefore, developing an effective strategy that can sense early chemical signals of thermal runaway inside a battery and suppress the chain reaction of thermal runaway from the source is a technical problem that urgently needs to be solved in this field. Summary of the Invention
[0007] To address the aforementioned technical problems, this invention provides a battery cell and its preparation method. The battery cell provided by this invention has an acid-responsive protective coating disposed at at least at one of the following locations: the surface of the separator, the inner or outer surface of the inner cladding, the inner surface of the casing, and the inner or outer surface of the safety valve. The acid-responsive protective coating includes acid-responsive microcapsules. When the battery is operating normally, the acid-responsive microcapsules remain intact. When the battery experiences thermal runaway, acidic gas triggers the decomposition of the cross-linked shell of the acid-responsive microcapsules, and the composite core material is precisely released, forming a cascade response mechanism of "active capture - local enrichment - acid-responsive decomposition - multiple protection". This achieves early and precise intervention and multiple blocking of the thermal runaway chain reaction, thereby effectively improving the safety performance of the battery.
[0008] In a first aspect, the present invention provides a battery cell, the battery cell comprising an electrode assembly, an electrolyte, a casing, and an acid-responsive protective coating; The electrode assembly includes a positive electrode, a negative electrode, and a separator, wherein the separator is disposed between the positive electrode and the negative electrode; The housing has an internal cavity in which the electrode assembly and electrolyte are housed, and the electrode assembly is immersed in the electrolyte. The acid-responsive protective coating comprises acid-responsive microcapsules and a binder, wherein the acid-responsive microcapsules comprise a composite core material and a cross-linked shell encapsulating the composite core material; The composite core material includes at least two of the following: heat-absorbing material, gas adsorbent, flame retardant, fire extinguishing agent, and pore-closing agent. The cross-linked shell includes a cross-linked acid-responsive polymer material having a trapping group and an acid-sensitive group. The trapping group is a group capable of undergoing an acid-base neutralization reaction or hydrogen bonding with an acidic gas, and the acid-sensitive group is a group capable of breaking chemical bonds in an acidic environment, causing the cross-linked shell to disintegrate.
[0009] The present invention provides a battery cell with an acid-responsive protective coating comprising acid-responsive microcapsules. During normal battery operation, the acid-responsive microcapsules remain intact. In the event of thermal runaway, acidic gas triggers the decomposition of the cross-linked shell of the acid-responsive microcapsules, precisely releasing the composite core material. This forms a cascade response mechanism of "active capture - local enrichment - acid-responsive decomposition - multiple protection," achieving early and precise intervention and multiple blocking of the thermal runaway chain reaction, thereby effectively improving battery safety performance. Specifically: The battery cell provided by this invention incorporates an acid-responsive protective coating, which includes acid-responsive microcapsules. Each microcapsule comprises a composite core material and a cross-linked shell encapsulating the composite core material. The cross-linked shell consists of a cross-linked acid-responsive polymer material, possessing both acid gas capture and acid-responsive decomposition functions. On one hand, it actively captures acidic gases through capturing groups, forming enrichment zones locally within the cross-linked shell, significantly increasing local acid intensity. On the other hand, the acid-sensitive groups undergo chemical bond breakage in the acidic microenvironment, accelerating the shell decomposition reaction. This cascade mechanism of "active capture-local enrichment-accelerated response" makes the response speed of the acid-responsive microcapsules of this invention several times faster than traditional acid-responsive microcapsules, enabling precise intervention during the critical window before thermal runaway occurs. Simultaneously, this invention encapsulates a composite core material within the cross-linked shell, including at least two of the following: endothermic material, gas adsorbent, flame retardant, fire extinguishing agent, and pore-closing agent, constructing a "endothermic-adsorption-flame retardant-pore-closing" quadruple protection system, achieving a comprehensive solution to the chain reaction of thermal runaway. When the battery is operating normally, the cross-linked shell remains intact, and the composite core material does not come into contact with the electrolyte, thus not negatively affecting the battery's rate performance and cycle life. In the event of thermal runaway, acidic gas triggers the decomposition of the cross-linked shell, precisely releasing the composite core material. This "release-on-demand" design completely solves the problem of traditional electrolyte additives sacrificing performance for safety. Especially when the acid-responsive protective coating is applied to the inner and outer surfaces of the safety valve, at the instant the safety valve opens due to battery thermal runaway, the internal high-pressure gas carries acid-responsive microcapsules out. These microcapsules rupture under the impact of the high-speed airflow, instantly releasing the composite core material within, achieving rapid response.
[0010] The release mechanism of the acid-responsive microcapsules of this invention is illustrated in the following diagram. Figure 2As shown, the cross-linked shell remains intact during normal battery operation. However, when a lithium-ion battery experiences thermal abuse, the LiPF6 in the electrolyte decomposes upon heating, producing acidic gases such as hydrofluoric acid (HF). HF diffuses to the surface of the acid-responsive microcapsules in the acid-responsive protective coating. The capturing groups of the acid-responsive polymer material in the cross-linked shell actively capture HF through acid-base neutralization reactions or hydrogen bonding with the acidic gases, forming a high-concentration acidic microenvironment locally within the shell. This acidic microenvironment triggers the chemical bond breaking of the acid-sensitive groups (chemical bond breaking, network decrosslinking, etc.), causing the shell structure to collapse and releasing the composite core material encapsulated within. Among these mechanisms, the heat-absorbing material absorbs a large amount of heat through phase change, reducing the temperature peak and buying time for other protective materials to respond; the gas adsorbent actively captures harmful gases such as HF, CO, CO2, and C2H4, reducing the risk of combustion, explosion, and toxicity at the source; the flame retardant inhibits electrolyte combustion, breaks the combustion chain, and prevents the spread of thermal runaway; the fire extinguishing agent extinguishes any existing open flames; and the pore-closing agent melts at high temperatures, flows to the pores of the separator, and solidifies upon cooling to block the pores, thus terminating the electrochemical reaction at a physical level. This cascaded response mechanism of "active capture - local enrichment - acid response decomposition - multiple protections" achieves early and precise intervention and multiple blocking of the thermal runaway chain reaction, thereby effectively improving the battery's safety performance.
[0011] As a preferred embodiment of the present invention, the battery cell further includes an inner cladding film, which wraps around at least a portion of the outer surface of the electrode assembly; and / or, a safety valve is provided on the housing; The acid-responsive protective coating is disposed at at least one of the following: the surface of the diaphragm, the inner or outer surface of the inner diaphragm, the inner surface of the housing, and the inner or outer surface of the safety valve.
[0012] The battery cell provided by the present invention has an acid-responsive protective coating at at least one of the following: the surface of the separator, the inner or outer surface of the inner cladding, the inner surface of the casing, and the inner or outer surface of the safety valve. This coating enables early and precise intervention and multiple blocking of the thermal runaway chain reaction when the battery experiences thermal runaway, effectively improving the battery's safety performance.
[0013] As a preferred embodiment of the present invention, the capturing group is selected from at least one of amino, carboxylate, sulfonate, amide, and phosphate groups.
[0014] As a preferred embodiment of the present invention, the acid-sensitive group is selected from at least one of acetal, ketal, hydrazone, imino, phosphate ester, carbonate, glycosidic bond, and peptide bond.
[0015] When the battery experiences thermal runaway, the LiPF6 in the electrolyte decomposes upon heating to produce acidic gases such as hydrofluoric acid (HF). The trapping groups in the acid-responsive polymer material of this invention can actively trap the acidic gases, forming enrichment zones in the cross-linked shell, significantly increasing the local acidity intensity. This causes the acid-sensitive groups to break chemical bonds in the acidic microenvironment, leading to the disintegration of the cross-linked shell and the release of the composite core material.
[0016] As a preferred embodiment of the present invention, the acid-responsive polymer material is selected from at least one of sodium alginate, sodium hyaluronate, pectin, Schiff base crosslinked chitosan, Schiff base crosslinked gelatin, poly(1,4-butanediamine-terephthalaldehyde imine), chitosan, carboxylated modified polyvinyl butyral, and amino-modified poly(cyclohexanediethanol-acetone ketal).
[0017] As a preferred embodiment of the present invention, when the acid-responsive protective coating is disposed on the surface of the diaphragm, the composite core material includes a heat-absorbing material, a pore-closing agent, a gas adsorbent, a flame retardant, and a fire extinguishing agent; the mass ratio of the heat-absorbing material, the pore-closing agent, the gas adsorbent, the flame retardant, and the fire extinguishing agent is (15-25):(25-40):(20-30):(10-20):(5-10), for example, 15:25:20:10:5, 20:30:25:15:8, 25:40:30:20:10, 15:35:25:15:5, etc.
[0018] As a preferred embodiment of the present invention, the diaphragm is selected from at least one of ceramic diaphragms, aramid diaphragms, polyimide diaphragms, polyacrylonitrile nanofiber diaphragms, and cellulose nanofiber diaphragms.
[0019] As a preferred embodiment of the present invention, when the acid-responsive protective coating is disposed on the inner surface of the housing or the inner or outer surface of the safety valve, the composite core material includes a heat-absorbing material, a gas adsorbent, a flame retardant, and a fire extinguishing agent; the mass ratio of the heat-absorbing material, the gas adsorbent, the flame retardant, and the fire extinguishing agent is (10-20):(25-35):(25-35):(20-30), for example, 10:25:25:20, 15:30:30:25, 20:35:35:30, 10:30:30:30, etc.
[0020] As a preferred embodiment of the present invention, when the acid-responsive protective coating is disposed on the inner or outer surface of the inner membrane, the composite core material includes a heat-absorbing material, a gas adsorbent, a flame retardant, and a fire extinguishing agent, wherein the mass ratio of the heat-absorbing material, the gas adsorbent, the flame retardant, and the fire extinguishing agent is (10-20):(25-35):(25-35):(15-28), for example, 10:25:25:15, 15:30:30:20, 20:35:35:25, 10:30:30:28, etc.
[0021] As a preferred embodiment of the present invention, the heat-absorbing material includes at least one of paraffin wax, polyethylene glycol, hydrated salt, and aluminum hydroxide.
[0022] The heat-absorbing material provided by this invention absorbs a large amount of heat through phase change, reducing the temperature peak and buying time for other protective materials to respond.
[0023] As a preferred embodiment of the present invention, the gas adsorbent is selected from metal oxides and / or porous materials capable of adsorbing at least one of hydrogen fluoride, carbon dioxide, ethylene, and carbon monoxide, preferably at least one of activated alumina, magnesium oxide, molecular sieve, ZIF-8, and flower-shaped cerium dioxide microspheres.
[0024] The gas adsorbent provided by this invention can actively adsorb harmful gases such as HF, CO, CO2, and C2H4, reducing the risk of combustion and explosion and the risk of poisoning from the source.
[0025] As a preferred embodiment of the present invention, the flame retardant is selected from organophosphorus flame retardants, preferably at least one of triethyl phosphate, trimethyl phosphate, and dimethyl methylphosphonate.
[0026] The flame retardant provided by this invention can inhibit electrolyte combustion, break the combustion chain, and prevent the spread of thermal runaway.
[0027] As a preferred embodiment of the present invention, the extinguishing agent is selected from perfluorohexanone and / or heptafluoropropane, which can extinguish existing open flames.
[0028] As a preferred embodiment of the present invention, the closing agent is selected from at least one of polyethylene wax, ethylene-ethyl acrylate copolymer, ethylene-vinyl acetate copolymer, Fischer-Tropsch wax, and oxidized polyethylene wax.
[0029] The pore-closing agent provided by this invention has a melting point of 85-115℃. It melts at this temperature, flows to the pores of the membrane, and solidifies after cooling to block the pores, thereby blocking ion transport and terminating the electrochemical reaction from a physical level.
[0030] As a preferred embodiment of the present invention, the acid-responsive microcapsules have a particle size of 1-50 μm, such as 1 μm, 5 μm, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, etc., and the appropriate particle size can be selected according to the different application locations.
[0031] As a preferred embodiment of the present invention, the thickness of the shell of the acid-responsive microcapsule is 0.2-10 μm, for example, 0.2 μm, 0.5 μm, 1 μm, 2 μm, 5 μm, 8 μm, 10 μm, etc.
[0032] As a preferred embodiment of the present invention, the adhesive is selected from at least one of polyvinylidene fluoride, polyacrylate, polyacrylamide, aramid fiber, polyimide, styrene-butadiene rubber, polyacrylate, polyvinyl alcohol, polyacrylic acid, polyurethane, and epoxy resin.
[0033] As a preferred embodiment of the present invention, the mass ratio of the acid-responsive microcapsules to the binder is (20-40):(1-10), for example, 20:1, 20:5, 20:10, 25:10, 30:1, 35:10, 40:1, etc.
[0034] As a preferred embodiment of the present invention, the thickness of the acid-responsive protective coating is 2-100 μm, such as 2 μm, 5 μm, 10 μm, 20 μm, 50 μm, 80 μm, 100 μm, etc., and the appropriate thickness can be selected according to the different application locations.
[0035] In a second aspect, the present invention provides a method for preparing a battery cell as described in the first aspect, the method comprising the following steps: (1) Mix the composite core material to obtain a composite core material mixture; (2) An acid-responsive polymer material is encapsulated on the surface of the composite core material mixture using a microencapsulation method to obtain acid-responsive microcapsules; (3) The acid-responsive microcapsules and the binder are mixed in a solvent to obtain a coating slurry. The coating slurry is then applied to the target substrate and dried to form an acid-responsive protective coating. (4) Assemble the target substrate coated with the acid-responsive protective coating with other components of the battery cell to obtain the battery cell.
[0036] The preparation method provided by this invention is simple and mature, requires no development of new equipment, and has good prospects for industrialization.
[0037] As a preferred embodiment of the present invention, the solvent is selected from water, NAt least one of methylpyrrolidone and ethanol.
[0038] As a preferred embodiment of the present invention, the content of the acid-responsive microcapsules is 20-40% based on the total mass of the coating slurry as 100%, for example, 20%, 25%, 30%, 35%, 40%, etc.
[0039] As a preferred embodiment of the present invention, the content of the binder is 1-10% based on the total mass of the coating slurry as 100%, for example, 1%, 3%, 5%, 7%, 10%, etc.
[0040] As a preferred embodiment of the present invention, dispersants and other additives are also added to the solvent.
[0041] As a preferred embodiment of the present invention, the microencapsulation method is selected from at least one of the following: emulsification-internal gelation, coaxial extrusion-coagulation bath, emulsion-solvent evaporation, interfacial polymerization, in-situ polymerization, and spray drying.
[0042] As a preferred embodiment of the present invention, the microencapsulation method is an emulsion-solvent evaporation method, comprising the following steps: (a) Dissolve the acid-responsive polymer material in a first organic solvent to obtain a shell solution; (b) Dispersing the composite core material mixture in the shell solution to form a primary emulsion; (c) The primary emulsion is transferred to an aqueous phase containing an emulsifier and emulsified to form a secondary emulsion; (d) The first organic solvent is removed by evaporation under reduced pressure, followed by washing and drying to obtain the acid-responsive microcapsules.
[0043] As a preferred embodiment of the present invention, the first organic solvent includes at least one of dichloromethane, ethyl acetate, and aqueous acetic acid.
[0044] As a preferred embodiment of the present invention, the emulsifier includes at least one of polyvinyl alcohol, gelatin, Tween, Span, sodium dodecyl sulfate, and poloxamer.
[0045] As a preferred embodiment of the present invention, when the acid-responsive polymer material is carboxylated modified polyvinyl butyral, aminated poly(cyclohexanediol-acetone ketal), poly(1,4-butanediamine-terephthalaldehyde imine), Schiff base crosslinked gelatin, or Schiff base crosslinked chitosan, a crosslinking agent is also added to the shell solution in step (a). The crosslinking agent is selected from at least one of glutaraldehyde, genipin, terephthalaldehyde, and adipate dihydrazide.
[0046] As a preferred embodiment of the present invention, when the acid-responsive polymer material is sodium alginate, chitosan, sodium hyaluronate or pectin, the microencapsulation method can be a coaxial extrusion-coagulation bath method or an emulsification-internal gelation method.
[0047] As a preferred embodiment of the present invention, the coaxial extrusion-coagulation bath method includes the following steps: (A) Dissolve the acid-responsive polymer material in water or an acid solution to obtain a shell solution; (B) The composite core material mixture and the shell solution are coaxially extruded to form microcapsule precursor droplets; (C) Drop the microcapsule precursor liquid into a coagulation bath to solidify and crosslink, thereby obtaining the acid-responsive microcapsules.
[0048] As a preferred embodiment of the present invention, when the acid-responsive polymer material is sodium alginate, the coagulation bath contains Ca²⁺. + An aqueous solution.
[0049] As a preferred embodiment of the present invention, when the acid-responsive polymer material is chitosan or pectin, the coagulation bath is an aqueous solution containing tripolyphosphate ions.
[0050] As a preferred embodiment of the present invention, step (B) includes extruding the composite core material mixture through an inner nozzle and coaxially extruding the shell solution through an outer nozzle to form microcapsule precursor droplets.
[0051] As a preferred embodiment of the present invention, the emulsification-internal gelation method includes the following steps: (A) Disperse the acid-responsive polymer material with an insoluble calcium or barium salt in water to obtain an aqueous phase; (B) Add the composite core material mixture to the aqueous phase and mix evenly to obtain an aqueous suspension containing the core; (C) Emulsify the aqueous suspension in the oil phase to form a water-in-oil emulsion; (D) Add acid to the emulsion and adjust the pH to 4.5-6.0 to release cations from insoluble calcium or barium salts, thereby crosslinking and curing acid-responsive polymer materials in situ to form microcapsules; (E) Separate, wash, and dry to obtain the acid-responsive microcapsules.
[0052] As a preferred embodiment of the present invention, when the acid-responsive polymer material is sodium alginate, the insoluble calcium salt is nano-calcium carbonate, the oil phase is liquid paraffin or mineral oil, and the acid is glacial acetic acid.
[0053] The technical solution provided by the embodiments of the present invention has the following advantages compared with the prior art: The battery cell provided by this invention has an acid-responsive protective coating, which includes acid-responsive microcapsules. When the battery is operating normally, the acid-responsive microcapsules remain intact. When the battery experiences thermal runaway, acidic gas triggers the decomposition of the cross-linked shell of the acid-responsive microcapsules, and the composite core material is precisely released, forming a cascade response mechanism of "active capture - local enrichment - acid-responsive decomposition - multiple protection". This achieves early and precise intervention and multiple blocking of the thermal runaway chain reaction, thereby effectively improving the safety performance of the battery. Attached Figure Description
[0054] The accompanying drawings, which are incorporated in and form part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.
[0055] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0056] Figure 1 This is a schematic diagram of the structure of the acid-responsive microcapsule described in Example 1 of the present invention; Among them, 1-crosslinked shell, 2-composite core material.
[0057] Figure 2 This is a schematic diagram illustrating the release mechanism of the acid-responsive microcapsules of the present invention.
[0058] Figure 3 The diagram shows the nail penetration test phenomena of lithium batteries in Example 1 and Comparative Example 1.
[0059] Figure 4 The results show the DC internal resistance of the lithium batteries in Example 1 and Comparative Example 1 under different states of charge.
[0060] Figure 5 The results show the discharge energy retention rate of the lithium batteries in Example 1 and Comparative Example 1 after 500 cycles. Detailed Implementation
[0061] To better understand the above-mentioned objectives, features, and advantages of the present invention, the solutions of the present invention will be further described below. It should be noted that, unless otherwise specified, the embodiments of the present invention and the features thereof can be combined with each other.
[0062] Many specific details are set forth in the following description in order to provide a full understanding of the invention, but the invention may also be practiced in other ways different from those described herein; obviously, the embodiments in the specification are only some embodiments of the invention, and not all embodiments.
[0063] Example 1 This embodiment provides a battery cell and its preparation method. The battery cell includes an electrode assembly, an electrolyte, an acid-responsive protective coating, a shell, and an inner cladding. The electrode assembly includes a positive electrode, a negative electrode, and a separator, wherein the separator is disposed between the positive electrode and the negative electrode; The housing has an internal cavity in which the electrode assembly and electrolyte are housed, and the electrode assembly is immersed in the electrolyte. A safety valve is provided on the housing; The inner cladding film wraps around at least a portion of the outer surface of the electrode assembly. The inner cladding film is a biaxially oriented polyester film (Mylar film), and its main component is polyethylene terephthalate (PET). The acid-responsive protective coating is disposed on one side surface of the diaphragm, the inner and outer surfaces of the inner membrane, the inner surface of the safety valve, and the inner surface of the shell. The acid-responsive protective coating comprises acid-responsive microcapsules and a binder. Each acid-responsive microcapsule includes a composite core material and a cross-linked shell encapsulating the composite core material. The particle size of the acid-responsive microcapsules is 1-30 μm, and the thickness of the shell is 0.2-5 μm. A schematic diagram of the acid-responsive microcapsule structure is shown below. Figure 1 As shown; The specific composition of the composite core material in the acid-responsive protective coatings placed at different locations is shown in Table 1: Table 1. Formulation of composite core materials
[0064] The cross-linked shell layer comprises a cross-linked acid-responsive polymer material, wherein the acid-responsive polymer material is sodium alginate.
[0065] The preparation method includes the following steps: 1. Preparation of acid-responsive microcapsules (1) Preparation of the shell solution: Dissolve 3 g of sodium alginate in 97 mL of deionized water, stir until completely dissolved, add 0.5 g of nano-calcium carbonate powder, disperse evenly at high speed, filter to remove bubbles, and obtain sodium alginate solution. Sodium alginate molecules contain a large number of carboxyl (-COOH) functional groups, which can capture acidic gases such as HF through hydrogen bonding. At the same time, under acidic conditions, the Ca²⁺ in the calcium alginate cross-linked network... + H +Displacement causes the shell to rapidly undergo a sol-gel transition and disintegrate. The glycosidic bonds in the polysaccharide chains can undergo acid-catalyzed hydrolysis, accelerating shell destruction and achieving acid-responsive decomposition.
[0066] (2) Preparation of composite core material mixtures: Four composite core material mixtures were prepared according to Table 1. Among them, paraffin wax is an endothermic material with a phase change temperature of about 55℃; activated alumina is a gas adsorbent used to adsorb thermally runaway gases such as HF, CO2, and C2H4; triethyl phosphate is a flame retardant; polyethylene wax is a pore-closing agent with a melting point of 105℃; and perfluorohexanone is a fire extinguishing agent. After weighing each component according to the proportion, paraffin wax and polyethylene wax (containing polyethylene wax when used in diaphragms) were preheated to 110℃ to melt, and slowly dripped into an aqueous solution containing an emulsifier under high-speed stirring to form a stable emulsion at the nano / micron level. After cooling, a suspension of solid particles was obtained, which was then mixed evenly with the remaining components at room temperature to obtain four composite core material mixtures. Paraffin absorbs a large amount of heat through solid-liquid phase transition during thermal runaway; activated alumina efficiently adsorbs harmful gases such as HF through its porous structure and high specific surface area; triethyl phosphate inhibits electrolyte combustion; polyethylene wax melts and flows at high temperatures, blocking the pores of the diaphragm; and perfluorohexanone can extinguish any open flames that have already been generated.
[0067] (3) Preparation of acid-responsive microcapsules: The composite core material suspension obtained in step (2) is thoroughly mixed with the sodium alginate solution containing nano-calcium carbonate prepared in step (1) as the aqueous phase.
[0068] (4) Add 1 g of Span 80 to 100 mL of mineral oil as the oil phase. Add 0.1 g of Tween 80 to the aqueous phase and mix thoroughly. Under high-speed homogenization or stirring, slowly add the aqueous phase to the oil phase to form a stable water-in-oil (W / O) emulsion. Control the target particle size by adjusting the homogenization / stirring speed. For microcapsules used for diaphragm coating, high-speed homogenization (15,000-20,000 rpm) is used to obtain a particle size of 1-3 μm (shell thickness 0.2-0.6 μm); for microcapsules used for inner membrane coating, medium-speed stirring (8,000-12,000 rpm) is used to obtain a particle size of 5-8 μm (shell thickness 0.2-1.2 μm); for microcapsules used for coating the inner surface of the shell, low-speed stirring (1,000-2,000 rpm) is used to obtain a particle size of 10-30 μm (shell thickness 1-5 μm); for microcapsules used for coating the inner surface of safety valves, medium-low speed stirring (3,000-5,000 rpm) is used to obtain a particle size of 8-15 μm (shell thickness 0.8-3 μm).
[0069] (5) Subsequently, glacial acetic acid was slowly added to the emulsion to adjust the pH to 5.0-5.5, and the reaction was maintained with stirring for 2-3 hours. Under these acidic conditions, the nano-calcium carbonate inside the aqueous droplets slowly released Ca²⁺. +The microcapsules underwent in-situ cross-linking and curing with sodium alginate. After the reaction was completed, the microcapsules were separated by centrifugation, washed three times alternately with isopropanol and deionized water, and dried at 30°C under normal pressure for 24 hours to obtain four types of acid-responsive microcapsules.
[0070] 2. Preparation of coating slurry Diaphragm coating slurry: 20 g of acid-responsive microcapsules for the diaphragm, 5 g of aqueous polyacrylate binder, 0.3 g of dispersant sodium polyacrylate, and 0.1 g of wetting agent fatty alcohol polyoxyethylene ether were added to 74.6 g of deionized water and dispersed at high speed to obtain the diaphragm coating slurry.
[0071] Inner surface coating slurry for the shell: 20 g of acid-responsive microcapsules for the shell, 5 g of polyvinylidene fluoride, 0.5 g of high molecular weight polyurethane wetting and dispersing agent, and... N 75g of methylpyrrolidone was dispersed at high speed to obtain a coating slurry for the inner surface of the shell.
[0072] Safety valve inner surface coating slurry: 20 g of acid-responsive microcapsules for safety valves, 4 g of polyvinylidene fluoride, and 1 g of polyurethane are added to... N The safety valve coating slurry was obtained by high-speed and uniform dispersion of 75g of methylpyrrolidone.
[0073] Inner coating slurry: 20 g of acid-responsive microcapsules for inner coating, 5 g of polyvinylidene fluoride, 1 g of chlorinated polypropylene, and... N 74 g of methylpyrrolidone was dispersed at high speed and uniformly to obtain an inner coating slurry.
[0074] 3. Coating preparation Separator coating: The above-mentioned corresponding coating slurry is coated onto the uncoated side surface of a polyethylene separator (7 μm thick) coated with ceramic on one side using a micro-gravure process. After coating and drying at 45°C, a coating with a thickness of 3 μm is formed. After winding, a battery separator coated with an acid-responsive protective coating is obtained.
[0075] Inner surface coating of the shell: The above-mentioned corresponding slurry is sprayed onto the inner surface of the square aluminum shell, with a coating thickness of 80 μm, and dried at 45℃ for 72 hours.
[0076] Safety valve inner surface coating: The above-mentioned corresponding slurry is sprayed onto the inner surface of the safety valve, with a coating thickness of 20 μm, and dried at 45℃ for 36 hours.
[0077] Inner coating: The above-mentioned slurry is sprayed onto the inner and outer surfaces of the polyethylene terephthalate inner coating, with a single-sided coating thickness of 8 μm, and dried at 45°C for 24 hours.
[0078] 4. Assembly of lithium-ion batteries Preparation of the positive electrode: Lithium iron phosphate (LiFePO4) was used as the positive electrode active material, Super-P as the conductive agent, and polyvinylidene fluoride (PVDF) as the binder. These were mixed at a mass ratio of 96:2:2. N A uniform positive electrode slurry was prepared using NMP as a solvent. The slurry was coated on both sides of an aluminum foil current collector, with a double-sided surface density of 3.62 g / 100cm². After drying at 140℃, rolling, and cutting, the positive electrode sheet was obtained.
[0079] Preparation of the negative electrode sheet: Artificial graphite was used as the negative electrode active material, Super-P as the conductive agent, and styrene-butadiene rubber (SBR) and sodium carboxymethyl cellulose (CMC) as binders. They were mixed in a mass ratio of 95:1.5:1.5:2 and prepared into a uniform negative electrode slurry using deionized water as the solvent. The slurry was coated on both sides onto a copper foil current collector, with a double-sided surface density of 2.09 g / 100cm². After drying at 110℃, rolling, and cutting, the negative electrode sheet was obtained.
[0080] Electrolyte: The lithium salt is 1M LiPF6, the solvent is a mixed solvent of ethylene carbonate / dimethyl carbonate / ethyl methyl carbonate in a volume ratio of 1:1:1, and the additives are 2wt% vinylene carbonate and 1wt% fluoroethylene carbonate.
[0081] An electrode assembly is formed by winding the positive electrode, the separator coated with the acid-responsive protective coating, and the negative electrode. The cover plate of the safety valve coated with the acid-responsive protective coating is welded to the electrode assembly. The outer surface of the electrode assembly is wrapped with the inner cladding coated with the acid-responsive protective coating and then placed in a square aluminum shell coated with the acid-responsive protective coating. After liquid injection, baking, high-temperature settling, formation, and capacity testing, a 280Ah square aluminum-shell lithium iron phosphate battery is obtained.
[0082] Example 2 This embodiment provides a battery cell and its preparation method. The battery cell is the same as that in Embodiment 1. The difference from Embodiment 1 is that the acid-responsive protective coating is only applied to one side of the separator, and there is no acid-responsive protective coating on the inner liner, safety valve, or shell. The preparation method is as described in Example 1.
[0083] Example 3 This embodiment provides a battery cell and its preparation method. The battery cell is the same as that in Embodiment 1. The difference from Embodiment 1 is that the acid-responsive protective coating is only set on the inner surface of the shell, the separator is a polyethylene separator with ceramic coated on one side (thickness 7 μm), and there is no acid-responsive protective coating on the inner cladding and the safety valve. The preparation method is as described in Example 1.
[0084] Example 4 This embodiment provides a battery cell and its preparation method. The battery cell is the same as that in Embodiment 1. The difference from Embodiment 1 is that the acid-responsive protective coating is only set on the inner surface of the safety valve, the separator is a polyethylene separator with ceramic coating on one side (thickness 7 μm), and there is no acid-responsive protective coating on the inner cladding and the shell. The preparation method is as described in Example 1.
[0085] Example 5 This embodiment provides a battery cell and its preparation method. The battery cell is the same as that in Embodiment 1. The difference from Embodiment 1 is that the acid-responsive protective coating is only set on the inner and outer surfaces of the inner cladding, the separator is a polyethylene separator with ceramic coating on one side (thickness 7μm), and there is no acid-responsive protective coating on the safety valve and the shell. The preparation method is as described in Example 1.
[0086] Example 6 This embodiment provides a battery cell and its preparation method. The battery cell is the same as that in Embodiment 1, except that the composite core material formulation in this embodiment is shown in Table 2. Table 2
[0087] The preparation method is as described in Example 1.
[0088] Example 7 This embodiment provides a battery cell and its preparation method. The battery cell is the same as that in Embodiment 1. The difference from Embodiment 1 is that sodium alginate is replaced with sodium hyaluronate, paraffin is replaced with aluminum hydroxide, activated alumina is replaced with molecular sieve, triethyl phosphate is replaced with dimethyl methylphosphonate, and polyethylene wax is replaced with Fischer-Tropsch wax. The preparation method is as described in Example 1.
[0089] Example 8 This embodiment provides a battery cell and its preparation method. The battery cell is the same as that in Embodiment 2. The difference from Embodiment 2 is that the acid-responsive polymer material in this embodiment is replaced by Schiff base crosslinked chitosan instead of sodium alginate. The preparation method is the same as in Example 2, except that: The acid-responsive microcapsules were prepared using an emulsion-solvent evaporation method, and the specific preparation method is as follows: (1) Preparation of shell solution: Dissolve 2g of chitosan in 98mL of 1% acetic acid aqueous solution, add 0.5g of glutaraldehyde as crosslinking agent, stir evenly to obtain shell solution, the amino groups on chitosan react with the aldehyde groups of glutaraldehyde to form Schiff base crosslinking network.
[0090] (2) Prepare a composite core material mixture according to the diaphragm formulation of Example 2.
[0091] (3) Preparation of acid-responsive microcapsules: The composite core material mixture is dispersed in the shell solution and ultrasonically emulsified in an ice bath to form a primary emulsion; the primary emulsion is then transferred to an aqueous phase containing 1 wt% polyvinyl alcohol and homogenized at high speed to form a secondary emulsion.
[0092] (4) Stirring at room temperature under reduced pressure to evaporate the solvent, centrifuging, washing and drying to obtain acid-responsive microcapsules. The shell of the microcapsules contains Schiff base imine bonds (-C=N-) as acid-sensitive groups, and the amino groups on chitosan are used as capturing groups.
[0093] Comparative Example 1 This comparative example provides a battery cell and its preparation method. The battery cell is the same as that in Example 2, except that the acid-responsive protective coating is not applied to one side surface of the separator, the inner and outer surfaces of the inner membrane, the inner surface of the safety valve, and the inner surface of the casing in this comparative example. The cells are directly assembled to obtain a lithium-ion battery.
[0094] Comparative Example 2 This comparative example provides a battery cell and its preparation method. The battery cell is the same as that in Example 2, except that the acid-responsive microcapsules are replaced with temperature-responsive microcapsules. The temperature-responsive microcapsules include a core material and a shell layer encapsulating the core material. The shell layer is melamine-urea-formaldehyde resin, and the core material is triethyl phosphate. The shell layer undergoes thermal shrinkage and rupture at about 100°C, releasing the core material. The method for preparing the temperature-responsive microcapsules includes: (1) Mix 10g of triethyl phosphate, 50mL of deionized water and 0.5g of sodium dodecyl sulfate and homogenize to obtain an O / W emulsion.
[0095] (2) Dissolve 3g of melamine, 1g of urea and 8mL of 37% formaldehyde in 20mL of water, adjust the pH to 8-9, and react at 70℃ for 30min to obtain MUF prepolymer.
[0096] (3) The prepolymer was dropped into the emulsion, the pH was adjusted to 3-4, and the shell was solidified by reacting at 60°C for 3 hours. After centrifugation, washing and drying, temperature-responsive microcapsules were obtained with a shell thermal response temperature of 100°C.
[0097] The remaining preparation steps are carried out in accordance with Example 2.
[0098] Comparative Example 3 This comparative example provides a battery cell and its preparation method. The battery cell is the same as that in Example 2, except that the sodium alginate in the cross-linked shell is replaced with polystyrene, which has no acid-responsive decomposition function. Methods for preparing microcapsules include: 5g of polystyrene was dissolved in 50mL of dichloromethane to form the shell solution. The composite core material was the same as in Example 2. Microcapsules were prepared using the emulsion-solvent evaporation method, referring to Example 8. The resulting microcapsule shell was stable under acidic conditions and could not be chemically disintegrated; the core could only be released through mechanical rupture.
[0099] The remaining preparation steps are carried out in accordance with Example 2.
[0100] Comparative Example 4 This comparative example provides a battery cell and its preparation method. The battery cell is the same as that in Example 2, except that the sodium alginate in the cross-linked shell is replaced with poly(cyclohexanediethanol-acetone ketal). The polymer main chain contains ketal groups, which can be hydrolyzed and broken under acidic conditions to disintegrate the shell (it has an acid-responsive function). However, it does not have a capturing group in the molecule and cannot actively capture acidic gases. It only has an acid-responsive decomposition function and no active acidic gas adsorption function.
[0101] Methods for preparing microcapsules include: 5 g of poly(cyclohexanediol-acetone ketal) was dissolved in 50 mL of dichloromethane, and 0.3 g of crosslinking agent terephthalaldehyde was added. The mixture was stirred and dissolved to form the shell solution. The composite core material was the same as in Example 2. Microcapsules were prepared using the emulsion-solvent evaporation method as described in Example 8.
[0102] The remaining preparation steps are carried out in accordance with Example 2.
[0103] Performance Test 1 Safety tests were conducted on the battery cells provided in the embodiments and comparative examples.
[0104] 1. Needle Penetration Test: Referring to GB / T 43854-2024, a needle penetration test was conducted on the batteries provided in the examples and comparative examples. The battery cells were clamped in a stainless steel fixture, the needle penetration speed was 25 mm / s, and the diameter of the steel needle was 6 mm (the steel needle surface was free of contamination, and the needle tip was clean). The samples were observed for any smoke, leakage, rupture of the explosion-proof valve, fire, or explosion. The test results are shown in Table 3 and... Figure 3 , Figure 3 The diagram shows the nail penetration test phenomena of lithium batteries in Example 1 and Comparative Example 1.
[0105] The results are shown in Table 3: Table 3
[0106] Comparing Examples 1-5 with Comparative Example 1, it can be seen that placing an acid-responsive protective coating at any location defined by this invention can significantly improve the safety performance of the battery. Among them, the synergistic effect of all elements (Example 1) is the best, with a maximum surface temperature of only 95°C, which is much lower than that of individual location solutions (Examples 2-5), indicating that there is a synergistic effect of multi-location coatings. In Example 6, the composite core material does not contain a gas adsorbent and still achieves non-flammability, but the temperature is higher than that of Example 1 and there is slight smoke, indicating that a gas adsorbent can further improve safety, but it is not an absolutely necessary component to achieve a basic suppression effect.
[0107] Depend on Figure 3 It can be observed that the lithium battery in Example 1 did not emit smoke, leak liquid outside the puncture point, catch fire, explode, or have its explosion-proof valve ruptured during the test. In contrast, the battery in Comparative Example 1 caught fire, indicating that the acid-responsive protective coating improved the battery's safety performance.
[0108] A comparison of Example 2 and Comparative Example 2 reveals that the temperature-responsive microcapsule failed to prevent thermal runaway due to its delayed response to the acidic gas, and its ignition temperature was close to that of Comparative Example 1, demonstrating the necessity of the acid response mechanism.
[0109] A comparison of Example 2 and Comparative Example 3 reveals that the inert shell cannot actively disintegrate in an acidic environment, the core cannot be released in time, and the battery performance is close to that of Comparative Example 1 without coating, proving that the release triggered by the acid-sensitive group is the core.
[0110] A comparison of Example 2 and Comparative Example 4 reveals that although the cross-linked shell microcapsules without trapping groups can release the core through acid decomposition, they cannot actively trap the initial acidic gas, resulting in a reduced thermal runaway inhibition effect and ultimately ignition. This demonstrates the importance of trapping groups in blocking the chain reaction from the source.
[0111] The present invention also conducted overcharge tests, adiabatic temperature rise characteristic tests, and short-circuit tests on the batteries provided in the embodiments and comparative examples. The test results were basically consistent with those of the nail penetration test. The application of the acid-responsive protective coating can significantly improve the safety performance of the battery.
[0112] Performance Test 2 The batteries provided in the examples and comparative examples were subjected to electrical performance tests.
[0113] 1. DCR (DC Internal Resistance) Test: DCR tests were conducted at different SOCs in a 25℃ ambient chamber. The test procedure was as follows: The battery at 100% SOC was allowed to stand for 30 minutes to eliminate polarization. Using a DC internal resistance tester, a 1C DC pulse was applied between the positive and negative terminals for 10ms, and the voltage drop ΔV was recorded. The DCR at 100% SOC was calculated as: R = ΔV / I. The battery was then gradually discharged to the target SOC (90%, 80%, 70%, 60%, 50%, 40%, 30%, 20%, 10%, 0%) with a 1C current. After each step, the battery was allowed to stand for 30 minutes to reach equilibrium. The pulse test was repeated, and the ΔV at each SOC was recorded to obtain the DCR value at each SOC point, and a DCR-SOC curve was plotted.
[0114] Figure 4 The results of DC internal resistance (DCR) of lithium batteries in Example 1 and Comparative Example 1 under different states of charge (SOC) show that the DCR values of Example 1 and Comparative Example 1 are not significantly different, indicating that the acid-responsive protective coating of the present invention does not have an adverse effect on the battery internal resistance.
[0115] 2. Cyclic performance test: Referring to GB / T36276-2023, charge and discharge cycle test is carried out in an ambient chamber at 45℃ at a rate of 0.5C, and the energy retention rate is recorded after 500 cycles.
[0116] Figure 5 The results show the discharge energy retention rates of the lithium batteries in Example 1 and Comparative Example 1 after 500 cycles. It can be observed that the discharge energy retention rate of Example 1 after 500 cycles is 96.05%, which is not lower than that of Comparative Example 1 (95.37%). This indicates that the acid-responsive protective coating does not adversely affect the cycle performance of the battery and may even improve its cycle stability.
[0117] In summary, the acid-responsive protective coating of this invention can be widely applied to the safety protection of secondary batteries such as lithium-ion batteries and sodium-ion batteries in the lithium iron phosphate / graphite system. The preparation method of this acid-responsive protective coating is simple, the process is mature, and the raw materials are widely available, allowing for large-scale industrial production. Applying this acid-responsive protective coating to battery separators, inner battery films, battery casings, or battery safety valves can significantly improve battery safety under abuse conditions such as overcharging, puncture, and thermal shock. This has significant practical value for applications with extremely high safety requirements, such as new energy vehicles and energy storage power stations.
[0118] It should be noted that, in this document, relational terms such as "first" and "second" are used merely to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitations, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element.
[0119] The above description is merely a specific embodiment of the present invention, enabling those skilled in the art to understand or implement the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the present invention is not to be limited to the embodiments described herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A battery cell, characterized by, The battery cell includes an electrode assembly, an electrolyte, a casing, and an acid-responsive protective coating; The electrode assembly includes a positive electrode, a negative electrode, and a separator, wherein the separator is disposed between the positive electrode and the negative electrode; The housing has an internal cavity in which the electrode assembly and electrolyte are housed, and the electrode assembly is immersed in the electrolyte. The acid-responsive protective coating comprises acid-responsive microcapsules and a binder, wherein the acid-responsive microcapsules comprise a composite core material and a cross-linked shell encapsulating the composite core material; The composite core material includes at least two of the following: heat-absorbing material, gas adsorbent, flame retardant, fire extinguishing agent, and pore-closing agent. The cross-linked shell includes a cross-linked acid-responsive polymer material having a trapping group and an acid-sensitive group. The trapping group is a group capable of undergoing an acid-base neutralization reaction or hydrogen bonding with an acidic gas, and the acid-sensitive group is a group capable of breaking chemical bonds in an acidic environment, causing the cross-linked shell to disintegrate.
2. The battery cell of claim 1, wherein, The battery cell further includes an inner cladding membrane that wraps around at least a portion of the outer surface of the electrode assembly; and / or, a safety valve is provided on the housing; The acid-responsive protective coating is disposed at at least one of the following: the surface of the diaphragm, the inner or outer surface of the inner diaphragm, the inner surface of the housing, and the inner or outer surface of the safety valve.
3. The battery cell according to claim 1 or 2, characterized in that, The capturing group is selected from at least one of amino, carboxylate, sulfonate, amide, and phosphate groups; And / or, the acid-sensitive group is selected from at least one of acetal, ketal, hydrazone, imino, phosphate, carbonate, glycosidic, and peptide bonds.
4. The battery cell according to claim 1 or 2, characterized in that, The acid-responsive polymer material is selected from at least one of sodium alginate, sodium hyaluronate, pectin, Schiff base crosslinked chitosan, Schiff base crosslinked gelatin, poly(1,4-butanediamine-terephthalaldehyde imine), chitosan, carboxylated modified polyvinyl butyral, and amino-modified poly(cyclohexanediethanol-acetone ketal).
5. The battery cell of claim 2, wherein, When the acid-responsive protective coating is applied to the surface of the diaphragm, the composite core material comprises a heat-absorbing material, a pore-closing agent, a gas adsorbent, a flame retardant, and a fire extinguishing agent; the mass ratio of the heat-absorbing material, the pore-closing agent, the gas adsorbent, the flame retardant, and the fire extinguishing agent is (15-25):(25-40):(20-30):(10-20):(5-10); And / or, when the acid-responsive protective coating is disposed on the inner surface of the housing or the inner or outer surface of the safety valve, the composite core material includes a heat-absorbing material, a gas absorbent, a flame retardant, and a fire extinguishing agent; the mass ratio of the heat-absorbing material, the gas absorbent, the flame retardant, and the fire extinguishing agent is (10-20):(25-35):(25-35):(20-30); And / or, when the acid-responsive protective coating is disposed on the inner or outer surface of the inner membrane, the composite core material includes a heat-absorbing material, a gas adsorbent, a flame retardant, and a fire extinguishing agent, wherein the mass ratio of the heat-absorbing material, the gas adsorbent, the flame retardant, and the fire extinguishing agent is (10-20):(25-35):(25-35):(15-28).
6. The battery cell according to claim 1 or 2, characterized in that, The heat-absorbing material includes at least one of paraffin wax, polyethylene glycol, hydrated salt, and aluminum hydroxide; And / or, the gas adsorbent is selected from metal oxides and / or porous materials capable of adsorbing at least one of hydrogen fluoride, carbon dioxide, ethylene, and carbon monoxide, preferably at least one of activated alumina, magnesium oxide, molecular sieve, ZIF-8, and flower-shaped cerium dioxide microspheres; And / or, the flame retardant is selected from organophosphorus flame retardants, preferably at least one of triethyl phosphate, trimethyl phosphate, and dimethyl methylphosphonate; And / or, the extinguishing agent is selected from perfluorohexanone and / or heptafluoropropane; And / or, the closing agent is selected from at least one of polyethylene wax, ethylene-ethyl acrylate copolymer, ethylene-vinyl acetate copolymer, Fischer-Tropsch wax, and oxidized polyethylene wax.
7. The battery cell according to claim 1 or 2, characterized in that, The acid-responsive microcapsules have a particle size of 1-50 μm; And / or, the shell thickness of the acid-responsive microcapsule is 0.2-10 μm.
8. The battery cell according to claim 1 or 2, characterized in that, The adhesive is selected from at least one of polyvinylidene fluoride, polyacrylate, polyacrylamide, aramid fiber, polyimide, styrene-butadiene rubber, polyacrylate, polyvinyl alcohol, polyacrylic acid, polyurethane, and epoxy resin; And / or, the mass ratio of the acid-responsive microcapsules to the binder is (20-40):(1-10); And / or, the thickness of the acid-responsive protective coating is 2-100 μm.
9. A method for preparing a battery cell according to any one of claims 1-8, characterized in that, The preparation method includes the following steps: The composite core material is mixed evenly to obtain a composite core material mixture; Acid-responsive polymer materials are encapsulated on the surface of the composite core material mixture using a microencapsulation method to obtain acid-responsive microcapsules; The acid-responsive microcapsules and binder are mixed in a solvent to obtain a coating slurry. The coating slurry is then applied to the target substrate and dried to form an acid-responsive protective coating. The target substrate coated with the acid-responsive protective coating is assembled with other components of the battery cell to obtain the battery cell.
10. The preparation method according to claim 9, characterized in that, The microencapsulation method is selected from at least one of the following: emulsification-internal gelation, coaxial extrusion-coagulation bath, emulsion-solvent evaporation, interfacial polymerization, in-situ polymerization, and spray drying.