Low-gas lithium iron manganese phosphate battery and preparation method thereof

By adding sodium phytate to the electrolyte to chelate manganese ions, the problem of gas generation during the formation of lithium manganese iron phosphate batteries is solved, achieving low gas generation and maintaining battery performance, making it suitable for large-scale industrial applications.

CN123162274APending Publication Date: 2026-11-24HUBEI DONGYU XINSHENG NEW ENERGY CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611094683.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-22
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

The severe gas generation problem in the formation stage of lithium manganese iron phosphate batteries leads to cell swelling, damage to the SEI film structure, and shortened battery life. Existing suppression solutions are costly to modify or have complex processes, making them difficult to apply on a large scale.

Method used

Adding a small amount of sodium phytate as a functional additive to the electrolyte allows it to chelate with manganese ions through its multiple phosphate groups, preventing manganese ion migration and inhibiting gas production at both the positive and negative electrodes, thus blocking the dual gas production pathways.

Benefits of technology

It significantly reduces the gas production during the formation of lithium manganese iron phosphate batteries, maintains battery performance, is suitable for large-scale production, has low cost, and a simple process, making it suitable for large-scale industrial promotion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention discloses a low-gas-yielding lithium manganese iron phosphate battery and its preparation method, belonging to the field of lithium-ion battery technology. The low-gas-yielding lithium manganese iron phosphate battery includes a positive electrode, a negative electrode, a separator, and an electrolyte. The active material of the positive electrode is lithium manganese iron phosphate, and sodium phytate is added to the electrolyte as a functional additive. This invention only requires adding a small amount of sodium phytate to a conventional electrolyte, without modifying the positive electrode material or adjusting the production process, and can utilize the "active site occupancy + Mn²" properties of sodium phytate. + The "chelation" dual-action mechanism significantly suppresses gas production during formation, resulting in a low-gas-producing lithium manganese iron phosphate battery. Examples show that adding 0.3 wt% sodium phytate can reduce gas production by more than 75%, a superior effect compared to traditional coating modification methods. This invention has the advantages of simple process, low cost, and ease of industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of lithium-ion battery technology, specifically relating to a low-gas-yielding lithium manganese iron phosphate battery and its preparation method. Background Technology

[0002] Lithium manganese iron phosphate (LMFP) has become a highly competitive cathode material in the fields of power batteries for new energy vehicles and energy storage batteries due to its higher energy density (voltage platform of about 4.1V, which is about 10% to 15% higher than that of lithium iron phosphate), lower raw material cost, and excellent safety performance.

[0003] However, the severe gas generation problem during the formation stage of lithium manganese iron phosphate batteries has been a core bottleneck hindering their large-scale application. Lithium manganese iron phosphate materials have a high content of transition metal ions, and the generation of transition metal ions (especially Mn) is inevitable during charge and discharge processes. 2+ Dissolution leads to instability in the material structure. Some dissolved transition metal ions migrate to the negative electrode and are reduced, causing damage to the negative electrode structure and generating large amounts of flammable gases such as hydrogen and carbon monoxide. This not only causes the cell to swell and deform, damaging the solid electrolyte interphase (SEI) membrane structure and reducing battery cycle life, but also poses serious safety hazards. This phenomenon is more pronounced under high-temperature environments.

[0004] Currently, a major reason why lithium manganese iron phosphate (LFP) batteries have not yet been officially commercialized in the electric vehicle sector is that their lifespan degrades rapidly and gas production is significant under high-temperature conditions. Existing gas production suppression solutions for LFP batteries mainly fall into the following categories: One approach involves adjusting the synthesis process of cathode materials, such as improving the structural stability of lithium manganese iron phosphate through coating modification or doping. This type of approach requires significant adjustments to existing material synthesis routes, resulting in high costs and long development cycles.

[0005] Second, there are modifications to the electrode manufacturing process, such as improving the electrode / electrolyte interface stability by optimizing the electrode formulation or preparation process. These solutions involve adjustments to existing production line processes and are complex to implement.

[0006] Thirdly, the formation process can be optimized, such as by setting up a separate film-forming charge-discharge stage to improve the film-forming effect. Although this type of solution does not require changing the material system, it requires adjusting the formation process parameters and cannot fundamentally solve the problem of chemical gas generation caused by manganese ion dissolution.

[0007] Fourthly, there are electrolyte additive formulation schemes, such as adding multiple functional additives to form stable electrolyte interface films on the surfaces of the positive and negative electrodes, inhibiting the dissolution and deposition of transition metal manganese ions. These schemes involve the formulation of multiple additives, resulting in complex formulations, and compatibility issues may exist between different additives.

[0008] Therefore, there is an urgent need for a solution that can suppress gas production simply by adding a component, without requiring any changes to the existing production process and material synthesis route, to significantly reduce the gas production during the formation of lithium manganese iron phosphate, and to be compatible with existing large-scale production. Summary of the Invention

[0009] This invention addresses the technical shortcomings of existing lithium manganese iron phosphate (LFP) batteries, such as severe gas production during formation and high costs or complex processes associated with modifying existing suppression methods. It provides a low-gas-producing LFP battery and its preparation method. This invention only requires adding a small amount of sodium phytate as a functional additive to a conventional electrolyte, without any modification to the cathode material or adjustment to the cell manufacturing process. This significantly reduces the formation gas production of LFP batteries, resulting in a low-gas-producing LFP battery.

[0010] To achieve the above objectives, the present invention provides the following technical solution: A low-gas-producing lithium manganese iron phosphate battery includes a positive electrode, a negative electrode, a separator, and an electrolyte. The active material of the positive electrode is lithium manganese iron phosphate, and sodium phytate is added to the electrolyte as a functional additive.

[0011] The principle behind sodium phytate's ability to reduce gas production is as follows: Sodium phytate molecules contain six phosphate groups, possessing multiple strong coordination sites and exhibiting extremely high coordination affinity for manganese ions. When a small amount of manganese ions dissolve from the surface of lithium manganese iron phosphate and enter the electrolyte, sodium phytate molecules rapidly chelate and capture the dissolved Mn. 2+ Ions, inhibiting Mn 2+ Ions migrate to the negative electrode to catalyze the decomposition of the SEI membrane and generate gas, thus blocking the secondary gas generation pathway initiated by manganese ions at the source. At the same time, sodium phytate molecules preferentially adsorb onto the defective active sites on the surface of lithium manganese iron phosphate particles. After occupying the sites, they prevent the electrolyte carbonate solvent from undergoing oxidative decomposition and gas generation at the active sites, thus suppressing primary gas generation from the positive electrode side. Gas generation reactions on both the positive and negative electrodes can be suppressed simultaneously with just one additive, eliminating the need for multiple additives and making the process extremely simple.

[0012] In a preferred embodiment, the sodium phytate in the electrolyte has a mass fraction of 0.1% to 0.5%.

[0013] In a further preferred embodiment, the sodium phytate in the electrolyte has a mass fraction of 0.2% to 0.4%.

[0014] In a further preferred embodiment, the sodium phytate in the electrolyte has a mass fraction of 0.3%.

[0015] In a preferred embodiment, the electrolyte is a carbonate-based electrolyte, wherein LiPF6 is 1 mol / L, and the volume ratio of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) is 1:1:1.

[0016] In a further preferred embodiment, the electrolyte also contains vinylene carbonate (VC), and the amount of VC added is 1 wt% of the total mass of the electrolyte.

[0017] The preparation method of the low-gas-yielding lithium manganese iron phosphate battery includes the following steps: S1. Preparation of positive electrode sheet: Lithium manganese iron phosphate, conductive agent and binder are mixed to prepare positive electrode slurry, which is coated on current collector, and then dried, cold pressed and cut to obtain positive electrode sheet; S2. Electrolyte preparation: Add sodium phytate to the electrolyte and stir until completely dissolved to obtain a functional electrolyte containing sodium phytate. S3. Cell assembly: Assemble the positive electrode, negative electrode, and separator to obtain a bare cell, inject the functional electrolyte, encapsulate, and then perform formation and venting sealing to obtain a low-gas-yielding lithium manganese iron phosphate battery.

[0018] In the preferred embodiment, the conductive agent in step S1 is conductive carbon black, the binder is polyvinylidene fluoride (PVDF) binder, and the current collector is aluminum foil.

[0019] In the preferred embodiment, the mass ratio of lithium manganese iron phosphate, conductive agent and binder in step S1 is 97:1:2.

[0020] In the preferred embodiment, the stirring in step S2 is carried out under an inert gas atmosphere, and the stirring time is 10-60-30 min.

[0021] In the preferred embodiment, the formation in step S3 has the following specific parameters: after standing for 5 minutes, charge at 0.1C for 7 minutes, then stand for 30 minutes, charge at 0.33C for 28 minutes, and finally stand for 10 minutes to complete the formation.

[0022] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. This invention only requires the addition of a small amount of sodium phytate as an additive to a conventional electrolyte. It does not require any modification to the existing lithium manganese iron phosphate cathode material synthesis process, nor does it require adjustments to the battery production process. Any lithium manganese iron phosphate battery manufacturer can directly implement this invention using its existing production lines, making it suitable for large-scale industrial application.

[0023] 2. This invention achieves the dual functions of "occupying the positive electrode active site to inhibit solvent decomposition + chelating and capturing dissolved manganese ions in the electrolyte to prevent gas generation at the negative electrode" using only sodium phytate as an additive. This single-agent, dual-effect inhibition blocks two formation gas generation pathways simultaneously. It eliminates the need for multiple functional additives, avoiding the compatibility issues associated with compound additives.

[0024] 3. This invention exhibits excellent gas generation suppression effects, resulting in a low-gas-generating battery. Examples show that adding only 0.3 wt% sodium phytate can reduce gas generation during lithium manganese iron phosphate formation by more than 75%, demonstrating superior gas generation suppression compared to traditional coating modification methods. The resulting battery exhibits extremely low gas generation during formation.

[0025] 4. The amount of sodium phytate added in this invention is extremely low (only 0.2% to 0.5%), which will not significantly change the viscosity and ionic conductivity of the electrolyte, nor will it increase the proportion of inactive components in the battery cell. Examples show that this invention maintains the original discharge specific capacity and cycle performance of lithium manganese iron phosphate while reducing gas production.

[0026] 5. Sodium phytate is a natural extract that has been industrially produced on a large scale. It is widely found in plants such as cereals, beans and oil crops, and is widely used in the food and pharmaceutical industries. The raw material supply is stable and the price is low.

[0027] 6. This invention only requires adding sodium phytate to the conventional electrolyte in proportion and stirring to dissolve it during electrolyte preparation. All other processes adopt the existing conventional lithium manganese iron phosphate battery production process, without any additional processing steps. Detailed Implementation

[0028] The technical solution of the present invention will be further described and illustrated below through examples. All raw materials used in the examples are commercially available or prepared using conventional methods.

[0029] Example 1 A low-gas-yielding lithium manganese iron phosphate battery is prepared by the following steps: S1. Preparation of the positive electrode: Commercially available unmodified lithium manganese iron phosphate was mixed at a mass ratio of lithium manganese iron phosphate: conductive carbon black: PVDF = 97:1:2. NMP (N-methylpyrrolidone) was used as the solvent to prepare a positive electrode slurry with a solid content of 60%. This slurry was coated onto a 13 μm carbon-coated aluminum foil, dried, and cold-pressed to a compaction density of 2.35 g / cm³. 3 The positive electrode sheet is obtained by cutting. S2. Electrolyte preparation: In an argon glove box, add 0.3 g of sodium phytate powder to 100 g of conventional electrolyte (1 mol / L LiPF6, EC:EMC:DMC=1:1:1, with 1 wt% VC added), and stir magnetically for 30 min until the sodium phytate is completely dissolved to obtain the functional electrolyte. S3. Cell Assembly: The positive electrode sheet, artificial graphite negative electrode, and PE separator obtained in step S1 are stacked to prepare a 3 Ah soft-pack bare cell. 1.1 g of the functional electrolyte obtained in step S2 is injected, and the cell is sealed after standing for 12 h. After standing for 5 min, it is charged at 0.1 C for 7 min, then stood for 30 min, and then charged at 0.33 C for 28 min. Finally, it is left to stand for 10 min to complete the formation. The vent is then sealed to obtain the finished battery.

[0030] Example 2 A low-gas-yielding lithium manganese iron phosphate battery is prepared by the following steps: S1. Preparation of the positive electrode: Commercially available unmodified lithium manganese iron phosphate was mixed with conductive carbon black and PVDF at a mass ratio of 97:1:2. NMP was used as the solvent to prepare a positive electrode slurry with a solid content of 60%. This slurry was coated onto a 13 μm carbon-coated aluminum foil, dried, and cold-pressed to a compaction density of 2.35 g / cm³. 3 The positive electrode sheet is obtained by cutting. S2. Electrolyte preparation: In an argon glove box, add 0.1 g of sodium phytate powder to 100 g of conventional electrolyte (1 mol / L LiPF6, EC:EMC:DMC=1:1:1, with 1 wt% VC added), and stir magnetically for 30 min until the sodium phytate is completely dissolved to obtain the functional electrolyte. S3. Cell Assembly: The positive electrode sheet, artificial graphite negative electrode and PE separator obtained in step S1 are stacked to prepare a 3 Ah soft-pack bare cell. 1.1 g of the functional electrolyte obtained in step S2 is injected, and after standing for 12 h, it is packaged. It is then charged and formed at 0.33 C according to conventional process. After degassing and sealing, the finished battery is obtained.

[0031] Example 3 A low-gas-yielding lithium manganese iron phosphate battery is prepared by the following steps: S1. Preparation of the positive electrode: Commercially available unmodified lithium manganese iron phosphate was mixed with conductive carbon black and PVDF at a mass ratio of 97:1:2. NMP was used as the solvent to prepare a positive electrode slurry with a solid content of 60%. This slurry was coated onto a 13 μm carbon-coated aluminum foil, dried, and cold-pressed to a compaction density of 2.35 g / cm³. 3 The positive electrode sheet is obtained by cutting. S2. Electrolyte preparation: In an argon glove box, add 0.2 g of sodium phytate powder to 100 g of conventional electrolyte (1 mol / L LiPF6, EC:EMC:DMC=1:1:1, with 1 wt% VC added), and stir magnetically for 30 min until the sodium phytate is completely dissolved to obtain the functional electrolyte. S3. Cell Assembly: The positive electrode sheet, artificial graphite negative electrode and PE separator obtained in step S1 are stacked to prepare a 3 Ah soft-pack bare cell. 1.1 g of the functional electrolyte obtained in step S2 is injected, and after standing for 12 h, it is packaged. It is then charged and formed at 0.33 C according to conventional process. After degassing and sealing, the finished battery is obtained.

[0032] Example 4 A low-gas-yielding lithium manganese iron phosphate battery is prepared by the following steps: S1. Preparation of the positive electrode: Commercially available unmodified lithium manganese iron phosphate was mixed with conductive carbon black and PVDF at a mass ratio of 97:1:2. NMP was used as the solvent to prepare a positive electrode slurry with a solid content of 60%. This slurry was coated onto a 13 μm carbon-coated aluminum foil, dried, and cold-pressed to a compaction density of 2.35 g / cm³. 3 The positive electrode sheet is obtained by cutting. S2. Electrolyte preparation: In an argon glove box, add 0.4 g of sodium phytate powder to 100 g of conventional electrolyte (1 mol / L LiPF6, EC:EMC:DMC=1:1:1, with 1 wt% VC added), and stir magnetically for 30 min until the sodium phytate is completely dissolved to obtain the functional electrolyte. S3. Cell Assembly: The positive electrode sheet, artificial graphite negative electrode and PE separator obtained in step S1 are stacked to prepare a 3 Ah soft-pack bare cell. 1.1 g of the functional electrolyte obtained in step S2 is injected, and after standing for 12 h, it is packaged. It is then charged and formed at 0.33 C according to conventional process. After degassing and sealing, the finished battery is obtained.

[0033] Example 5 A low-gas-yielding lithium manganese iron phosphate battery is prepared by the following steps: S1. Preparation of the positive electrode: Commercially available unmodified lithium manganese iron phosphate was mixed with conductive carbon black and PVDF at a mass ratio of 97:1:2. NMP was used as the solvent to prepare a positive electrode slurry with a solid content of 60%. This slurry was coated onto a 13 μm carbon-coated aluminum foil, dried, and cold-pressed to a compaction density of 2.35 g / cm³. 3 The positive electrode sheet is obtained by cutting. S2. Electrolyte preparation: In an argon glove box, add 0.5 g of sodium phytate powder to 100 g of conventional electrolyte (1 mol / L LiPF6, EC:EMC:DMC=1:1:1, with 1 wt% VC added), and stir magnetically for 30 min until the sodium phytate is completely dissolved to obtain the functional electrolyte. S3. Cell Assembly: The positive electrode sheet, artificial graphite negative electrode and PE separator obtained in step S1 are stacked to prepare a 3 Ah soft-pack bare cell. 1.1 g of the functional electrolyte obtained in step S2 is injected, and after standing for 12 h, it is packaged. It is then charged and formed at 0.33 C according to conventional process. After degassing and sealing, the finished battery is obtained.

[0034] Comparative Example 1 A lithium iron phosphate battery is prepared by the following steps: S1. Preparation of the positive electrode: Commercially available unmodified lithium manganese iron phosphate was mixed with conductive carbon black and PVDF at a mass ratio of 97:1:2. NMP was used as the solvent to prepare a positive electrode slurry with a solid content of 60%. This slurry was coated onto a 13 μm carbon-coated aluminum foil, dried, and cold-pressed to a compaction density of 2.35 g / cm³. 3 The positive electrode sheet is obtained by cutting. S2. Electrolyte preparation: Prepare 100 g of conventional electrolyte (1 mol / L LiPF6, EC:EMC:DMC=1:1:1, with 1 wt% VC added) in an argon glove box. S3. Cell Assembly: The positive electrode sheet, artificial graphite negative electrode and PE separator obtained in step S1 are stacked to prepare a 3 Ah soft-pack bare cell. 1.1 g of conventional electrolyte obtained in step S2 is injected, and after standing for 12 h, it is packaged. It is then charged and formed at 0.33 C according to conventional process. After degassing and sealing, the finished battery is obtained.

[0035] Comparative Example 2 The difference between this comparative example and Example 1 is that carbon-coated modified lithium manganese iron phosphate (LMFP@C) is used instead of the unmodified lithium manganese iron phosphate in Example 1 as the positive electrode active material, and sodium phytate is not added to the electrolyte. The remaining steps and parameters are the same as in Example 1. The preparation method of the carbon-coated modified lithium manganese iron phosphate is as follows: commercial lithium manganese iron phosphate (LiMn) is used... 0.6 Fe 0.4 PO4) and glucose were mixed at a mass ratio of 100:5, and an appropriate amount of deionized water was added. The mixture was then ball-milled for 4 h to obtain a precursor slurry. The precursor slurry was spray-dried at 120 °C to obtain a precursor powder. The precursor powder was placed in a tube furnace and heated to 650 °C at a heating rate of 5 °C / min under an argon atmosphere. The temperature was held for 4 h and then naturally cooled to room temperature to obtain carbon-coated modified lithium manganese iron phosphate (LMFP@C), wherein the carbon coating layer thickness was 3–5 nm and the carbon content was 2.5 wt%.

[0036] Comparative Example 3 The difference between this comparative example and Example 1 is that a nitrogen-containing heterocyclic oxazolone manganese complex additive is used instead of sodium phytate as the electrolyte functional additive, and the amount added is also 0.3 wt% of the total electrolyte mass. The remaining steps and parameters are the same as in Example 1. Representative compounds of this type of additive can be found in Chinese patent application publication number CN117895080A.

[0037] Comparative Example 4 The difference between this comparative example and Example 1 is that ethylene sulfate (DTD) is used instead of sodium phytate as the electrolyte functional additive, and the amount added is also 0.3 wt% of the total mass of the electrolyte. The remaining steps and parameters are the same as in Example 1.

[0038] Vinyl sulfate (1,3,2-Dioxathiolane-2,2-dioxide, abbreviated as DTD), CAS number 1072-53-3, chemical formula C2H4O4S, appears as white crystals. Comparative Example 5 The difference between this comparative example and Example 1 is that a multi-additive compound system is used instead of sodium phytate as the electrolyte functional additive. The compound system consists of 0.2 wt% 1,3-propanesulfonyl lactone (PS) + 0.2 wt% tris(trimethylsilyl)phosphate (TMSP) (both based on the total mass of the electrolyte). The remaining steps and parameters are the same as in Example 1.

[0039] Performance testing The performance of the batteries prepared in Examples 1-5 and the comparative examples was tested, and the results are shown in Table 1: Table 1 Comparison of Battery Performance

[0040] The test results show that: (1) The present invention is optimal or tied for optimal in all three evaluation dimensions. The gas production of Example 1 (0.3% sodium phytate) was 1.17 mL / Ah (75.4% lower than the blank control group), the specific capacity at 1C rate was 152.3 mAh / g, and the capacity retention rate after 500 cycles at 1C was 94.8%. It ranked first in both gas production suppression and cycle retention rates, and tied for first place in the rate capacity dimension.

[0041] (2) The "direct coordination + site occupancy" mechanism of sodium phytate is superior to the "indirect film formation" or "ring-opening reaction" mechanisms of other technical routes. Sodium phytate molecules contain six phosphate ester groups, which can rapidly chelate Mn through direct coordination. 2+ Furthermore, it preferentially adsorbs onto the positive electrode active site through polar groups, resulting in fast reaction kinetics and high efficiency. In contrast, oxazolones require ring-opening reactions (with moderate efficiency), and DTD only forms a film indirectly (with low efficiency). Compound formulations also suffer from complex ratio optimization and insufficient addition amounts.

[0042] (3) 0.3% is the optimal amount of sodium phytate to be added. At this amount, the optimal balance is achieved between gas generation suppression, rate capacity and cycle retention. Below 0.3%, gas generation suppression and cycle improvement are insufficient, while above 0.3%, the electrolyte viscosity increases, leading to a decrease in rate capacity and cycle retention.

[0043] (4) The present invention has significant industrialization advantages. In terms of performance, the present invention is superior to four mainstream industry solutions: carbon coating modification (Comparative Example 2), oxazolone additives (Comparative Example 3), DTD (Comparative Example 4), and PS+TMSP compound (Comparative Example 5). In terms of process, the present invention only requires the addition of a single sodium phytate additive to the conventional electrolyte, without modifying the cathode material or adjusting the existing production process, and the modification cost is almost zero. In terms of cost, sodium phytate is a natural extract that has been produced on a large scale industrially, with a stable supply of raw materials and a low price.

[0044] In summary, this invention utilizes a single sodium phytate additive to achieve "positive electrode active site occupancy + electrolyte chelation of Mn". 2 + The dual direct action mechanism of this invention outperforms the four mainstream industry technologies in terms of gas production suppression, rate capacity utilization, and cycle stability. It also has significant industrialization advantages such as extremely simple formulation, unchanged process, and low cost, which fully demonstrates the technological advancement and practical value of the invention.

[0045] The present invention is simple and easy to implement, requiring no process modification. It only requires the addition of a low-cost additive to solve the gas generation problem in the formation of lithium manganese iron phosphate. Sodium phytate is a widely available and inexpensive raw material, making it suitable for large-scale promotion and application.

[0046] It should be understood that the above embodiments are for illustrative purposes only and are not intended to limit the scope of protection of the present invention. Furthermore, it should be understood that after reading the teachings of this invention, those skilled in the art can make various alterations or modifications to the invention, and these equivalent forms also fall within the scope defined by the appended claims.

Claims

1. A low-gas-producing lithium manganese iron phosphate battery, comprising a positive electrode, a negative electrode, a separator, and an electrolyte, characterized in that, The active material of the positive electrode is lithium manganese iron phosphate, and sodium phytate is added to the electrolyte as a functional additive.

2. The low-gas-producing lithium manganese iron phosphate battery according to claim 1, characterized in that, The sodium phytate in the electrolyte has a mass fraction of 0.1% to 0.5%.

3. The low-gas-producing lithium manganese iron phosphate battery according to claim 2, characterized in that, The sodium phytate in the electrolyte has a mass fraction of 0.2% to 0.4%.

4. The low-gas-producing lithium manganese iron phosphate battery according to claim 3, characterized in that, The sodium phytate in the electrolyte has a mass fraction of 0.3%.

5. The low-gas-producing lithium manganese iron phosphate battery according to claim 1, characterized in that, The electrolyte is a carbonate-based electrolyte, wherein LiPF6 is 1 mol / L, and the volume ratio of ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate is 1:1:

1.

6. The low-gas-producing lithium manganese iron phosphate battery according to claim 5, characterized in that, The electrolyte also contains vinylene carbonate, and the amount of vinylene carbonate added is 1 wt% of the total mass of the electrolyte.

7. A method for preparing a low-gas-producing lithium manganese iron phosphate battery as described in any one of claims 1 to 6, characterized in that, Includes the following steps: S1. Preparation of positive electrode sheet: Lithium manganese iron phosphate, conductive agent and binder are mixed to prepare positive electrode slurry, which is coated on current collector, and then dried, cold pressed and cut to obtain positive electrode sheet; S2. Electrolyte preparation: Add sodium phytate to the electrolyte and stir until completely dissolved to obtain a functional electrolyte containing sodium phytate. S3. Cell assembly: Assemble the positive electrode, negative electrode, and separator to obtain a bare cell, inject the functional electrolyte, encapsulate, and then perform formation and venting sealing to obtain a low-gas-yielding lithium manganese iron phosphate battery.

8. The method for preparing a low-gas-yielding lithium manganese iron phosphate battery according to claim 7, characterized in that, The conductive agent in step S1 is conductive carbon black, the binder is polyvinylidene fluoride binder, and the current collector is aluminum foil; the mass ratio of lithium manganese iron phosphate, conductive agent and binder in step S1 is 97:1:

2.

9. The method for preparing a low-gas-yielding lithium manganese iron phosphate battery according to claim 7, characterized in that, The stirring in step S2 is carried out under an inert gas atmosphere for 10 to 60 minutes.

10. The method for preparing a low-gas-yielding lithium manganese iron phosphate battery according to claim 7, characterized in that, The formation process described in step S3 has the following specific parameters: after standing for 5 minutes, charge at 0.1C for 7 minutes, then stand for 30 minutes, charge at 0.33C for 28 minutes, and finally stand for 10 minutes to complete the formation.

Citation Information

Patent Citations

  • Additive, electrolyte containing additive and secondary battery

    CN117895080A