A lithium battery

By adjusting the micropore area ratio, sphericity, and carboxylic acid ester solvent content of the positive electrode sheet of lithium-ion batteries, the problem of insufficient liquid retention capacity of the positive electrode sheet was solved, thereby improving the low-temperature fast charging performance and cycle stability of the battery.

CN123162276APending Publication Date: 2026-11-24CALB GROUP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611131621.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-28
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

The existing positive electrode of lithium-ion batteries has a weak liquid retention capacity, which makes it difficult for the electrolyte to be fully retained. During long-term cycling, local liquid shortage is likely to occur, affecting lithium-ion transport and battery cycle performance.

Method used

By synergistically regulating the average area ratio of micropores in the positive electrode active material layer, the sphericity of micropores, and the content of carboxylic acid ester solvents in the electrolyte, the full wetting of the electrolyte and lithium-ion transport are ensured, thereby improving the low-temperature fast charging performance and cycle life of the battery.

Benefits of technology

This achieves high-efficiency liquid retention of the positive electrode, reduces the adverse effects of electrolyte viscosity on lithium-ion diffusion, ensures full utilization of the internal pore structure of the positive electrode active material layer, and improves lithium-ion transport kinetics and overall electrochemical performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

This invention provides a lithium battery, belonging to the field of battery technology. By simultaneously controlling the average area ratio and micropore sphericity of the positive electrode active material layer, as well as the content of carboxylic acid ester solvents in the electrolyte, this invention improves the electrolyte retention capacity of the positive electrode, reduces the adverse effects of increased electrolyte viscosity caused by the dissolution of pore-forming agents on lithium-ion diffusion, and ensures that the internal pore structure of the positive electrode active material layer is fully utilized, resulting in high electrolyte wetting and improved lithium-ion transport kinetics and low-temperature stability. Ultimately, this achieves superior low-temperature fast-charging performance and cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of battery technology, and in particular to a battery. Background Technology

[0002] In existing lithium-ion batteries, the positive electrode has a weak liquid retention capacity. During long-term cycling, as the electrolyte is continuously consumed, the positive electrode can hardly maintain effective retention and continuous wetting of the electrolyte, which can easily lead to local liquid shortage, thereby restricting lithium-ion transport and accelerating capacity decay, affecting the cycle performance and service life of the battery.

[0003] Therefore, improving the cycle performance of lithium-ion batteries has become a pressing technical problem to be solved in this field. Summary of the Invention

[0004] The purpose of this application is to overcome the shortcomings of the existing technology and provide a battery that improves the liquid retention capacity of the positive electrode by synergistically regulating the average area ratio (a) of micropores in the positive electrode active material layer, the micropore sphericity (b), and the content of carboxylic acid ester solvents (c) in the electrolyte. This reduces the adverse effects of increased electrolyte viscosity caused by the dissolution of pore-forming agents on lithium-ion diffusion, while ensuring the full utilization of the electrolyte by the internal pore structure of the positive electrode active material layer, improving the electrolyte wetting degree and lithium-ion transport kinetics, and improving the battery's low-temperature fast charging performance and cycle life.

[0005] To achieve the above objectives, in a first aspect of this application, the present invention provides a lithium battery, comprising a positive electrode and an electrolyte, wherein the positive electrode comprises a positive active material layer containing micropores, and the electrolyte comprises an organic solvent, wherein the organic solvent comprises a carboxylic acid ester solvent. Wherein, the percentage of the micropores to the area of ​​the positive electrode active material layer is a; The average major axis length L of the micropore max The length is 0.01–1 μm, and the average minor axis length L min The value is 0.01–1 μm, and L max ≥L min ; The circularity of the micropore is b, where b = L max / L min ; The mass percentage of the carboxylic acid ester solvent in the organic solvent is c; The lithium battery satisfies the following condition: a / (b×c) = 0.11~2.22.

[0006] In summary, compared with the prior art, the present invention achieves the following technical effects: This application provides a battery that improves the liquid retention capacity of the positive electrode by simultaneously controlling the average area ratio of micropores in the positive electrode active material layer, the sphericity of micropores, and the content of carboxylic acid ester solvents in the electrolyte. This reduces the adverse effects of increased electrolyte viscosity caused by the dissolution of pore-forming agents on lithium-ion diffusion, while ensuring that the internal pore structure of the positive electrode active material layer can be fully utilized. This results in high electrolyte wetting, improved lithium-ion transport kinetics and low-temperature stability, and ultimately, superior low-temperature fast charging performance and cycle performance. Detailed Implementation

[0007] To enable those skilled in the art to better understand the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of the present invention.

[0008] In this application, the technical features described in an open-ended manner include both closed technical solutions consisting of the listed features and open technical solutions that include the listed features.

[0009] In this application, numerical ranges are referred to as continuous unless otherwise specified, and include the minimum and maximum values ​​of the range, as well as every value between the minimum and maximum values. Furthermore, when the range refers to integers, it includes every integer between the minimum and maximum values ​​of the range. Additionally, when multiple ranges are provided to describe a feature or characteristic, the ranges may be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges to which they are incorporated.

[0010] Unless otherwise specified, the experimental methods used in the following examples are conventional methods. Unless otherwise specified, all materials and reagents used are commercially available.

[0011] The present application is further illustrated below with specific embodiments: A lithium battery includes a positive electrode sheet and an electrolyte, wherein the positive electrode sheet includes a positive active material layer containing micropores, and the electrolyte includes an organic solvent, wherein the organic solvent includes a carboxylic acid ester solvent. Wherein, the percentage of the micropores to the area of ​​the positive electrode active material layer is a; The average major axis length L of the micropore max The length is 0.01–1 μm, and the average minor axis length L min The value is 0.01–1 μm, and L max ≥L min; The circularity of the micropore is b, where b = L max / L min ; The mass percentage of the carboxylic acid ester solvent in the organic solvent is c; The lithium battery satisfies the following condition: a / (b×c) = 0.11~2.22.

[0012] Existing lithium-ion battery cathode electrodes have weak electrolyte retention capacity, making it difficult for the electrolyte to remain sufficiently within the electrode. This leads to localized electrolyte shortages during long-term cycling, thus affecting the battery's cycle life. To improve electrolyte retention, this application increases the average area ratio 'a' of micropores in the positive electrode active material layer, creating more electrolyte storage space within the electrode and thereby improving electrolyte adsorption and retention performance. However, these micropores are formed after the pore-forming agent dissolves. As the micropore area ratio 'a' increases, the amount of pore-forming agent added also increases, leading to subsequent dissolution into the electrolyte. This increases the viscosity of the electrolyte system and reduces the lithium-ion diffusion rate, especially at low temperatures, causing kinetic deterioration and affecting the battery's low-temperature fast-charging performance. To avoid the aforementioned problems caused by simply increasing the number of micropores, this application further controls the micropore sphericity 'b' (b=L). max / L min When the roundness b decreases, the micropore morphology becomes more regular and the edges more rounded, resulting in more uniform capillary action of the micropores. This allows for maintaining high liquid retention performance even with a lower micropore area ratio, reducing the amount of pore-forming agent and minimizing its impact on electrolyte viscosity. However, when the roundness b is too low, the micropores tend to become overly regular, leading to excessive retention of pore structures during rolling, reduced electrode compaction density, and weakened particle contact, thus affecting electron conduction and volumetric energy density. This application further increases the content of carboxylic acid ester solvent c in the electrolyte to improve the lithium-ion diffusion rate and thus improve low-temperature performance; however, when the content of carboxylic acid ester solvent c is too high, electrolyte side reactions intensify, which in turn reduces cycle life. Therefore, this application synergistically controls the micropore area ratio a, micropore roundness b, and carboxylic acid ester solvent content c to satisfy the relationship a / (b×c) = 0.11~2.22, thereby balancing the cycle life and low-temperature kinetic performance of the positive electrode.

[0013] In some implementations, the battery satisfies the range of a / (b×c) = 0.11, 0.35, 0.55, 0.75, 0.95, 1, 1.35, 1.55, 1.75, 1.95, 2, 2.15, 2.22, or any two of these values.

[0014] In some embodiments, the battery satisfies: a / (b×c) = 0.2~1.11.

[0015] In this application, adjusting the average area ratio 'a' of micropores in the positive electrode active material layer can improve the electrolyte retention capacity of the positive electrode, enabling the electrolyte to remain stably within the positive electrode during cycling, reducing the risk of interfacial side reactions caused by localized electrolyte shortages, thereby improving the cycle stability of the battery. However, it is also necessary to consider the impact of pore-forming agent dissolution on the electrolyte system viscosity, avoiding the problem that excessively high micropore area ratio leads to increased pore-forming agent dissolution, resulting in increased electrolyte viscosity, decreased lithium-ion diffusion rate, and consequently affecting the low-temperature performance of the battery. To ensure electrolyte retention while reducing the adverse effects of pore-forming agent addition on kinetic performance, the sphericity 'b' of the micropores also needs to be controlled simultaneously. Circularity reflects the regularity of micropore morphology and the uniformity of capillary force distribution. Lower circularity indicates more regular and rounded micropore morphology, more uniform electrolyte binding at the micropore edges, and easier formation of a stable electrolyte distribution within the pores, thus maintaining superior electrolyte retention even with a lower micropore area ratio. However, excessively low circularity can lead to excessive pore retention during electrode compaction, reducing electrode compaction density, increasing electron transport impedance, and consequently affecting battery kinetic performance and volumetric energy density. Further improvements can be made by increasing the content (c) of carboxylic acid ester solvents in the electrolyte to enhance ion transport kinetics under low-temperature conditions. However, excessively high carboxylic acid ester solvent content can increase side reactions in the electrolyte system, decrease electrode / electrolyte interface stability, and consequently affect battery cycle life.

[0016] When the regulation satisfies the preferred range of a / (b×c), the positive electrode can maintain a high liquid retention capacity and avoid excessive electrolyte viscosity caused by excessive dissolution of pore-forming agent. At the same time, it ensures that the electrolyte fully wets the pores inside the positive electrode active material layer, resulting in a more uniform lithium-ion transport path and higher diffusion efficiency. This balances better low-temperature fast charging performance and cycle stability, enabling the battery to achieve better overall electrochemical performance.

[0017] In this application, when a / (b×c) is less than 0.11, it indicates that a is relatively low, and / or b is high, and / or c is high. At this time, the effective pore space inside the positive electrode sheet for storing electrolyte is insufficient, weakening the adsorption and retention capacity of the micropores for electrolyte. This easily leads to localized electrolyte shortages during cycling, resulting in insufficient wetting of the positive electrode active material particles by the electrolyte, thereby increasing the risk of side reactions at the electrode / electrolyte interface, reducing lithium-ion transport channels, decreasing ion transport uniformity, and shortening battery life. Furthermore, when b is too high, the micropore morphology tends to be elongated or irregular, and the capillary force distribution is uneven, further weakening the electrolyte retention capacity of the positive electrode sheet. When a / (b×c) is greater than 2.22, it indicates that a is high, and / or b is low, and / or c is low. At this time, more pore-forming agents need to be added, leading to increased viscosity of the electrolyte system and increased lithium-ion migration resistance. Especially under low-temperature conditions, the lithium-ion diffusion rate decreases more significantly, easily causing a reduction in battery kinetic performance. Meanwhile, when the content of carboxylic acid ester solvents is insufficient, it is difficult to effectively compensate for the kinetic loss caused by the dissolution of pore-forming agents, which leads to a decrease in lithium-ion transport efficiency and ultimately limits the fast-charging performance of the battery.

[0018] In some embodiments, 'a' is 10% to 40%, for example, a range of one or both of 10%, 13%, 15%, 17%, 19%, 20%, 23%, 25%, 27%, 29%, 30%, 33%, 35%, 37%, 39%, and 40%, preferably 20% to 30%. If 'a' is too high, the pore-forming agent used to form micropores dissolves into the electrolyte, increasing the electrolyte viscosity and slowing the lithium-ion diffusion rate, thus affecting the battery's low-temperature performance. Controlling 'a' within 10% to 40% can improve the liquid retention performance of the positive electrode while also considering lithium-ion transport kinetics, thereby achieving better cycle stability and low-temperature fast-charging performance.

[0019] In some embodiments, b = 1.5~8.0, for example, a value within the range of one or both of 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, and 8, preferably 1.8~4.0; if the roundness b is too low, it will lead to insufficient positive electrode compaction. Controlling b within the range of 1.5~8.0 can balance the ability of micropores to retain electrolyte with the electrode compaction performance, achieving better electrolyte wetting effect and kinetic performance.

[0020] In some embodiments, c = 10%~30%, for example, a range of one or any two of 10%, 13%, 15%, 17%, 19%, 20%, 23%, 25%, 27%, 29%, and 30%, preferably 15%~25%. When c is too high, side reactions in the system intensify, which deteriorates the battery's lifespan. Controlling c within the range of 10%~30% can balance the low-temperature lithium-ion diffusion rate with electrolyte interface stability, thereby achieving superior low-temperature fast-charging performance and cycle stability.

[0021] This invention does not impose any particular limitation on the method for controlling the average area ratio 'a' of micropores in the positive electrode active material layer. Those skilled in the art can use any method that can achieve the adjustment of 'a', such as adjusting the particle size distribution width of the positive electrode active material (e.g., LFP); or adjusting the compaction density, preferably by reducing the compaction density, to achieve the adjustment of the average area ratio 'a', but are not limited to the above methods.

[0022] This invention addresses the circularity b (i.e., L) of micropores in the positive electrode active material layer. max / L min The method of adjusting b is not particularly limited. Those skilled in the art can use any method that can achieve the adjustment of b, such as adjusting the content of the pore-forming agent; or adjusting the perforation density of the electrode sheet to achieve the adjustment of the roundness b, but are not limited to the above methods.

[0023] This invention does not impose any particular limitation on the method of controlling the content c of carboxylic acid ester solvents. Those skilled in the art can use any method that can achieve the adjustment of c, such as adjusting the content of ethyl acetate in the electrolyte; or adjusting the content of methyl propionate in the electrolyte, but are not limited to the above methods.

[0024] In some implementations, the L max Preferably 0.02~0.8μm, and / or, the L min The preferred size is 0.02~0.8μm; this balances the positive electrode's liquid retention capacity, electrolyte wetting performance, and lithium-ion transport efficiency, thereby achieving superior cycle performance and kinetic performance.

[0025] In some embodiments, the carboxylic acid ester solvent includes at least one selected from ethyl acetate, propyl acetate, methyl formate, methyl acetate, methyl butyrate, ethyl propionate, and methyl propionate. These carboxylic acid ester solvents have low viscosity and strong dissolving power, which can effectively reduce electrolyte viscosity, increase electrolyte ionic conductivity, and improve the migration rate of lithium ions in the electrolyte and electrode pores, thus contributing to improved battery kinetic performance at low temperatures.

[0026] In some embodiments, the carboxylic acid ester solvent is ethyl acetate; ethyl acetate has low viscosity, low melting point and good fluidity, which can effectively reduce the viscosity of the electrolyte system, especially at low temperatures, which is beneficial for maintaining the high ion migration ability of the electrolyte, improving the diffusion rate of lithium ions and improving the low-temperature performance of the battery.

[0027] In some embodiments, the organic solvent further includes a carbonate solvent, which accounts for 70-90% by mass of the electrolyte, for example, a range of one or any two of 70%, 72%, 74%, 76%, 78%, 80%, 82%, 84%, 86%, 88%, and 90%.

[0028] In some embodiments, the carbonate solvent includes at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, and methyl propyl carbonate. Carbonate solvents have good lithium salt dissolving ability and electrochemical stability, and can be used as the main solvent in the electrolyte system to provide a stable transport medium for lithium ions and maintain the interface stability during battery charging and discharging.

[0029] In some embodiments, the carbonate solvent is ethylene carbonate; carboxylic acid ester solvents typically have lower viscosity, which is beneficial for improving low-temperature fluidity and lithium-ion diffusion performance.

[0030] In some embodiments, when the carboxylic acid ester solvent is ethyl acetate, the mass ratio of ethylene carbonate to ethyl acetate in the organic solvent is 1:(0.5~1.5), for example, a range of one or both of 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4, and 1:1.5; this can balance the low-temperature kinetic performance, interfacial stability, and cycle life of the electrolyte, thereby obtaining better overall electrochemical performance.

[0031] In some embodiments, the organic solvent further includes at least one selected from ether solvents, tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane, dimethoxymethane, and 1,2-dimethoxyethane.

[0032] In some embodiments, the electrolyte further includes a lithium salt and additives, the lithium salt including lithium hexafluorophosphate (LiPF6). At least one of lithium perchlorate (LiClO4), lithium tetrafluoroborate (LiBF4), lithium dioxolaneborate (LiBOB), lithium bis(trifluoromethanesulfonylimide) (LiTFSI), and lithium hexafluoroarsenate (LiAsF6), and / or, The additive includes at least one of vinylene carbonate, 4-methylvinyl sulfite, and butylene sulfite; the additive helps to promote the formation of a stable interface film on the electrode surface, reduce the degree of side reactions between the electrolyte and the electrode material, and improve the stability of lithium-ion transport.

[0033] In some embodiments, the lithium salt accounts for 10% to 20% of the electrolyte by mass, for example, a range of one or any two of 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, and 20%.

[0034] And / or, The additive accounts for 2% to 10% of the electrolyte by mass, for example, one or any two of the following ranges: 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%. Controlling the mass percentage of the additive within the range of 2% to 10% can balance interfacial stability, side reaction suppression ability, and lithium-ion transport efficiency, thereby obtaining better cycle performance and kinetic performance.

[0035] In some embodiments, the positive electrode active material layer includes a positive electrode active material, which includes at least one of lithium iron phosphate, lithium cobalt oxide, lithium manganese iron phosphate, ternary materials, and lithium manganese oxide. All of the above positive electrode active materials can realize the charging and discharging process of the battery through the insertion and extraction of lithium ions. The solution of this application is not only applicable to a single positive electrode active material system, but also to a battery system in which multiple positive electrode active materials are used alone or in combination, and has good applicability and compatibility.

[0036] In some embodiments, when the positive electrode active material is lithium iron phosphate, a = 20%~30%, for example, a range of one or any two of 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, and 30%. Lithium iron phosphate materials typically have high compaction density and relatively low electronic conductivity, and their electrochemical reaction process is quite sensitive to the degree of electrolyte wetting and the uniformity of lithium-ion transport. Therefore, there is a higher demand for the electrolyte retention performance of the electrode. Controlling a within the range of 20%~30% can balance the electrolyte retention capacity of the positive electrode, lithium-ion transport kinetics, and cycle stability, thereby obtaining better low-temperature performance and rate performance.

[0037] In some embodiments, the particle size D of the lithium iron phosphate 50The particle size ranges from 0.02 to 15 μm, for example, one or any two of the following values: 0.02 μm, 0.05 μm, 0.1 μm, 0.5 μm, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, and 15 μm. The particle size of lithium iron phosphate particles affects the particle packing state of the positive electrode active material layer. When the particle size of lithium iron phosphate particles is too small, although the lithium-ion diffusion path is shortened, which is beneficial to rate capability... While increasing the specific surface area of ​​lithium iron phosphate particles can improve performance, it also increases the likelihood of side reactions between the electrode and electrolyte. Simultaneously, reduced interparticle porosity can restrict ion transport channels after electrode compaction, increasing electrolyte consumption and negatively impacting long-term cycle stability. Conversely, excessively large lithium iron phosphate particle size lengthens the diffusion path of lithium ions within the particles, potentially affecting rate performance and low-temperature kinetics. Furthermore, larger interparticle voids may reduce the uniformity of wetting within the electrode, hindering electrolyte retention and stable transport during long-term cycling. Therefore, the particle size D of lithium iron phosphate... 50 By controlling the size within the range of 0.02–15 μm, the structural stability of the positive electrode, lithium-ion transport efficiency, and cycle stability can be balanced, thereby achieving better overall electrochemical performance.

[0038] In some embodiments, the lithium iron phosphate comprises large particles and small particles, wherein the particle size D of the large particles is... 50 The particle size is 0.8~4μm, for example, a value within the range of one or any two of 0.8μm, 1μm, 1.5μm, 2μm, 2.5μm, 3μm, 3.5μm, and 4μm; the particle size D of the small particles is... 50 The particle size is 0.2~0.8μm, for example, one or any two of 0.2μm, 0.3μm, 0.4μm, 0.5μm, 0.6μm, 0.7μm, 0.8μm; the combination of large and small particles is beneficial to improve the particle packing state of the positive electrode active material layer.

[0039] In some embodiments, the lithium iron phosphate further includes ultra-small particles and ultra-large particles, wherein the particle size D of the ultra-small particles is... 50 The value is 20~80 nm, for example, a value within the range of one or any two of 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, and 80 nm; the particle size D of the ultra-large particles is... 50The particle size is 4~15μm, for example, values ​​within the range of one or any two of 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, and 15μm. By introducing ultra-small and ultra-large particles in combination with large and small particles, a multi-level particle size distribution structure can be formed. Smaller particles can fill the gaps between larger particles, resulting in a tighter stacking of the positive electrode active material particles, improving electrode compaction and reducing the interparticle void size. However, with reduced interparticle voids, the electrolyte wetting path within the electrode becomes narrower, reducing electrolyte storage space. During long-term cycling, localized insufficient wetting or electrolyte deficiency is more likely to occur due to continuous electrolyte consumption, thus affecting the continuous lithium-ion transport efficiency and the utilization rate of the active material. Therefore, when using the above-mentioned multi-level particle size compound system, the positive electrode sheet has higher requirements for electrolyte retention performance, and it is necessary to improve the electrode sheet's ability to adsorb and retain electrolyte by adjusting the microporous structure in the positive electrode active material layer. Preferably, a = 20%~30%, for example, a range of one or any two of 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, and 30%. Controlling a within the range of 20%~30% can better adapt to the multi-level particle size lithium iron phosphate system, maintaining a high degree of compaction while taking into account electrolyte wetting and electrolyte retention performance, thereby improving the battery's cycle performance and service life.

[0040] In some embodiments, the particle size D of the ternary material 50 The value is 2~20μm, for example, one or any two of the following: 2μm, 5μm, 7μm, 9μm, 10μm, 12μm, 14μm, 16μm, 18μm, 20μm.

[0041] In some embodiments, when the ternary material is nickel-cobalt-manganese ternary material (MCN), a = 5%~15%, for example, a range of one or any two of 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, and 15%. The chemical formula for nickel-cobalt-manganese ternary materials can be represented as LiNi. x Co y Mn z O2, x, y, and z represent the molar ratios of nickel, cobalt, and manganese, respectively. Nickel-cobalt-manganese ternary materials have high operating voltage and high ion transport efficiency, with relatively low dependence on electrode liquid retention capacity. By controlling a within the range of 5% to 15%, electrolyte wetting ability, lithium-ion transport efficiency, and interface stability can be balanced, thereby achieving superior rate performance and cycle stability.

[0042] In some embodiments, the method for preparing the positive electrode sheet includes the following steps: The binder, conductive agent and positive electrode active material are mixed, and solvent, pore-forming agent and dispersing agent are added. The mixture is then impregnated, kneaded and dispersed at high speed to obtain the positive electrode slurry. The positive electrode slurry is coated onto the surface of the current collector, dried, and rolled to obtain the positive electrode sheet.

[0043] In some embodiments, the pore-forming agent includes any one or more of ethylene carbonate, polyethylene glycol, tributyl phosphate, triethylhexyl phosphate, methyl palmitate, and dioctyl adipate.

[0044] In some embodiments, the pore-forming agent is ethylene carbonate, and the particle size D50 of the ethylene carbonate is 50 μm to 500 μm, for example, a range of one or any two of 50 μm, 100 μm, 150 μm, 200 μm, 250 μm, 300 μm, 350 μm, 400 μm, 450 μm, and 500 μm.

[0045] In some embodiments, the pore-forming agent accounts for 0.1% to 3% of the positive electrode slurry by mass, for example, a range of one or any two of 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, and 3%.

[0046] In this invention, the conductive agent is used to provide conductivity, and any conductive agent can be used without particular limitation, as long as it has suitable electronic conductivity and does not significantly cause adverse chemical changes in the battery. Exemplarily, the conductive agent includes, but is not limited to, at least one of carbon nanotubes, carbon black, graphite, activated carbon, carbon fibers, mesoporous carbon, and fullerenes, wherein carbon fibers are, for example, carbon nanofibers; and carbon black is, for example, acetylene black, SP, Ketjen black, etc.

[0047] In this invention, the binder is used to improve the adhesion between positive electrode active material particles and the adhesion between the positive electrode active material and the positive electrode current collector. Any binder can be used without particular limitation, as long as it has suitable adhesive properties and does not significantly cause adverse chemical changes in the battery. Exemplarily, the binder includes, but is not limited to, fluorinated polyolefin binders, including, but not limited to, polyvinylidene fluoride (PVDF), PVDF copolymers, or their modified derivatives (e.g., modified with carboxylic acids, acrylic acid, acrylonitrile, etc.).

[0048] In some embodiments, the areal density of the positive electrode active material layer is 300 g / m³. 2 ~600g / m 2 For example, 300g / m 2 350 g / m 2 400 g / m 2 450 g / m2 500 g / m 2 550 g / m 2 600 g / m 2 The value is within the range of one or both of the following. This application improves the electrolyte retention capacity of the positive electrode, enabling the electrode to maintain a good electrolyte wetting state during long-term cycling, which is especially suitable for high areal density and thick electrode systems, and is beneficial to improving the long-term cycle stability and life performance of the battery.

[0049] Furthermore, the compaction density of the positive electrode active material layer is 2.5 g / cm³. 3 ~2.8g / cm 3 For example, 2.5 g / cm 3 2.55 g / cm 3 2.6 g / cm 3 2.65 g / cm 3 2.7 g / cm 3 2.75 g / cm 3 2.8 g / cm 3 The value is within the range of one or both of these parameters. Controlling the compaction density of the positive electrode active material layer within a certain range promotes rapid lithium-ion transport and avoids excessive gaps between positive electrode active material particles, reducing side reactions at the positive electrode interface and thus ensuring the cycle life of the lithium-ion battery.

[0050] In some embodiments, the battery includes a negative electrode sheet, the negative electrode sheet includes a negative electrode active material layer, the negative electrode active material layer includes a negative electrode active material, and the negative electrode active material includes any one or more of graphite, silicon oxide, and silicon carbon.

[0051] In some embodiments, the areal density of the negative electrode active material layer is 120 g / m³. 2 ~280 g / m 2 For example, 120g / m 2 150 g / m 2 180 g / m 2 200 g / m 2 220 g / m 2 250 g / m 2 280 g / m 2 The range of one or any two of them.

[0052] In some embodiments, the compaction density of the negative electrode active material layer is 1.5 g / cm³. 3 ~1.8 g / cm 3 For example, 1.5 g / cm 3 1.52 g / cm 31.54 g / cm 3 1.56 g / cm 3 1.58 g / cm 3 1.6 g / cm 3 1.65 g / cm 3 1.7 g / cm 3 1.75 g / cm 3 1.8 g / cm 3 The range of one or any two of them.

[0053] In this invention, the lithium-ion battery further includes a separator disposed between the positive electrode and the negative electrode to separate them and prevent short circuits. The separator can be at least one of polyethylene (PE) and polypropylene (PP); a coating can also be provided on the surface of the separator, which can be an inorganic coating and / or an organic coating. The inorganic coating material includes at least one of alumina, silicon oxide, titanium oxide, magnesium oxide, zirconium oxide, and boehmite; the organic coating includes at least one of aramid coating and polyvinylidene fluoride (PVDF) coating.

[0054] To enable those skilled in the art to better understand the present application, the technical solutions in the embodiments of the present application will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present application, and not all embodiments.

[0055] Unless otherwise specified, all components and raw materials used in the embodiments and comparative examples of this application are commercially available, and the same type of components and raw materials are used in each parallel experiment.

[0056] Test methods 1. The average area ratio of micropores in the 5 detection areas a: (1) Pretreatment: Discharge the battery to 2.75V at a rate of 0.33C, disassemble and remove the positive electrode, rinse with dimethyl carbonate (DMC), soak for 24 hours and dry for later use. (2) SEM imaging: Five detection areas were selected on the surface of the positive electrode active material layer for scanning electron microscopy (SEM) imaging. The specific sampling locations are as follows: Sampling point 1: 5 cm from the top edge and 5 cm from the left edge of the electrode; Sampling point 2: 5 cm from the top edge and 5 cm from the right edge of the electrode; Sampling point 3: 5 cm from the lower edge and 5 cm from the left edge of the electrode; Sampling point 4: 5 cm from the lower edge and 5 cm from the right edge of the electrode; Sampling point 5: At the intersection of half the length and half the width of the electrode.

[0057] The sampling point should be a flat area free of material loss, with a selected area width of 15mm and a magnification of 5000.

[0058] (3) Processing: Open the original SEM image using ImageJ software, adjust the threshold, and distinguish between the dark areas of the pores and the light-colored solid matrix of the electrode. Set the measurement parameters: area and equivalent diameter. Screen and retain closed pores with an equivalent pore diameter ≤1μm.

[0059] Micropore area ratio = S p / S t ×100%, where S p S represents the total area of ​​all pores with a diameter < 1 μm. t =Total SEM field of view × 100%. The average value of 5 different test areas is recorded as parameter a. 2. Major axis length L of the micropore. max minor axis length L min : Open the original SEM image in ImageJ and adjust the threshold. Set the measurement parameters: fit the major axis of the ellipse, fit the minor axis of the ellipse, and automatically calculate AR = Major / Minor. Take the average value of 5 different test regions as parameter b.

[0060] 3. The mass percentage of carboxylic acid esters in the electrolyte, c: (1) Pretreatment: Discharge the battery to 2.75V at 0.33C and remove the electrolyte; (2) GC-FID test: Take 0.5g of electrolyte, dilute it 100 times with acetone solvent, and filter it with an organic filter membrane. Chromatographic column TG-5ms (30m×0.2mm×0.25μm); injection port 250℃, split ratio 30:1; column temperature 40℃ (3min) → 10℃ / min → 180℃ (5min); FID detector 280℃; quantify using fluorobenzene as internal standard and external standard method to obtain the content of ethyl propionate (wt%) as c. 4. Low temperature DCR of battery: The batteries were cycled three times at 0.33C at 25℃, and then brought to 50% SOC. They were then placed in a high-low temperature chamber, with -10℃ set as the target low temperature, and kept at this temperature for 4 hours. The open-circuit voltage U0 was recorded. A constant current discharge of 0.3C was applied for 18 seconds, and the voltage U1 at the end of the pulse and the current I were recorded. The DCR was recorded as (U0-U1) / I. Three batteries were tested per group, and the average value was taken. 5. Battery lifespan (capacity retention rate after a certain number of cycles): Three batteries were taken after formation and capacitation. They were discharged at 1C constant current to 2.75V, rested for 10 minutes, then charged at 1C constant current to 3.65V, then charged at constant voltage to 0.05C cutoff, rested for 10 minutes, and then the 1C constant current charging was repeated. The discharge capacity of the third cycle was recorded as C0. After 600 cycles, the discharge capacity C1 was recorded. The capacity retention rate was C1 / C0×100%, and the average value of each group was taken.

[0061] 6. Compacted density of the positive electrode active material layer: The thickness of the electrode coating area was measured using a micrometer at 10 points, and the average value 'a' was taken. After wiping the coating area, the average thickness of the foil was measured as 'b'. The compaction density is: c = C / (ab).

[0062] 7. Areal density of the positive electrode active material layer: Take a complete, unblemished positive electrode sheet and use a slicing machine to cut out five small discs with a diameter of 40 mm. Weigh the small discs and calculate the average value A. Wipe the coated area on the surface of the small discs with N-methylpyrrolidone (NMP), and after drying, obtain foil. Weigh the small discs and calculate the average value B. The areal density is: C = (AB) / (3.14) 0.022) g / m 2 .

[0063] 8. Particle size D 50 : Take a complete, unblemished electrode sheet, dissolve it in NMP solvent, and collect the solution. Centrifuge the solution at 2000 rpm for 5 min. Remove the lower precipitate, repeatedly wash and filter the solid with ultrapure water, and dry it at 80℃ to obtain the positive electrode active material (such as LFP) powder. Measure the powder using a Malvern particle size analyzer to obtain the D... 50 .

[0064] Example Example 1 (1) Preparation of positive electrode sheet: PVDF binder, acetylene black conductive agent, and positive electrode active material were mixed, with the positive electrode active material being lithium iron phosphate (LFP). The LFP particle size distribution width was adjusted to 1.52. NMP solvent and ethylene carbonate pore-forming agent were added, and the mixture was impregnated and kneaded. High-speed dispersion was then performed to obtain a positive electrode slurry. The mass ratio of positive electrode active material, conductive agent, binder, and pore-forming agent was 96:1.8:2:0.2, and the solid content of the slurry was 58 wt%. The positive electrode slurry was coated onto the surface of a current collector aluminum foil, dried, and rolled to obtain a positive electrode sheet with an areal density of 450 g / m². 2 The compacted density is 2.6 g / cm³. 3 By controlling the electrode perforation density to 50 holes / cm 2 (2) Preparation of negative electrode sheet: A negative electrode slurry is prepared by mixing graphite (anode active material), SP (conductive agent), styrene-butadiene rubber (SBR) (binder), and sodium carboxymethyl cellulose (CMC) (dispersant) with water as a solvent. The ratio of negative electrode active material: conductive agent: binder: dispersant is 96:1.8:2:0.2. The negative electrode slurry is coated onto both surfaces of the negative electrode current collector, dried, rolled, and slit to obtain the negative electrode sheet with an areal density of 200 g / m³. 2 The compacted density is 1.6 g / cm³. 3 .

[0065] (3) Preparation of electrolyte: The thoroughly dried lithium salt was dissolved in a mixed organic solvent to prepare an electrolyte with a concentration of 1 mol / L.

[0066] Organic solvent: Ethyl carbonate (EC): Ethyl methyl carbonate (EMC): Dimethyl carbonate (DMC): Ethyl acetate (EA): Methyl propionate (MP) = 2.4:4:1.6:1:1.

[0067] Lithium salt: LiPF6 addition amount 12wt%; Additives: 4 wt% vinylene carbonate (VC), 1 wt% propane sulfonate lactone (PS), 1 wt% trimethyl phosphate (TMP). (4) Assembly and formation The positive electrode, separator, and negative electrode are stacked in sequence, with the separator positioned between the positive and negative electrodes to provide isolation. The separator is made of PE. The cells are then wound to obtain a bare cell. The bare cell is placed in an outer packaging shell, dried, and then injected with electrolyte. After vacuum sealing, settling, formation, and shaping, a lithium-ion battery is obtained.

[0068] Example 2 The preparation method of the battery in this embodiment is basically the same as that in Example 1, except that in step (1), the LFP particle size distribution width is adjusted to 1.82; the mass ratio of positive electrode active material, conductive agent, binder and pore-forming agent is 95.9:1.8:2:0.3; and the electrode perforation density is 100 per cm. 2 .

[0069] In step (3), ethyl acetate 5 wt%, methyl propionate 10 wt%, and the remaining organic solvents are adjusted proportionally.

[0070] Example 3 The preparation method of the battery in this embodiment is basically the same as that in Example 1, except that in step (1), the LFP particle size distribution width is adjusted to 1.82; the pore-forming agent is tributyl phosphate; and the mass ratio of positive electrode active material, conductive agent, binder, and pore-forming agent is 96.1:1.8:2:0.1; the electrode sheet is not perforated. The compaction density of the positive electrode sheet is 2.65 g / cm³.3 .

[0071] In step (3), ethyl acetate 10 wt%, methyl propionate 15 wt%, and the remaining organic solvents are adjusted proportionally.

[0072] Example 4 The preparation method of the battery in this embodiment is basically the same as that in Example 1, except that in step (1), the mass ratio of positive electrode active material, conductive agent, binder and pore-forming agent is 95.8:1.8:2:0.4; and the electrode perforation density is 150 per cm. 2 The compacted density of the positive electrode sheet is 2.55 g / cm³. 3 .

[0073] In step (3), ethyl acetate is 5 wt%, methyl propionate is 8 wt%, and the remaining organic solvents are adjusted proportionally.

[0074] Example 5 The preparation method of the battery in this embodiment is basically the same as that in Example 1, except that in step (1), the positive electrode active material is MCN. The particle size distribution width of MCN is adjusted to 1.82; the mass ratio of positive electrode active material, conductive agent, binder and pore-forming agent is 95.8:1.8:2:0.4; and the electrode perforation density is 150 holes / cm. 2 The compacted density of the positive electrode sheet is 2.7 g / cm³. 3 .

[0075] In step (3), ethyl acetate is 30 wt%, methyl propionate is not included, and the remaining organic solvents are adjusted proportionally.

[0076] Example 6 The preparation method of the battery in this embodiment is basically the same as that in Example 1, except that in step (1), the LFP particle size distribution width is adjusted to 1.72; the mass ratio of positive electrode active material, conductive agent, binder and pore-forming agent is 96.15:1.8:2:0.05; and the electrode perforation density is 10 holes / cm. 2 The compacted density of the positive electrode sheet is 2.67 g / cm³. 3 .

[0077] In step (3), ethyl acetate 10 wt%, methyl propionate 2.5 wt%, and the remaining organic solvents are adjusted proportionally.

[0078] Example 7 The preparation method of the battery in this embodiment is basically the same as that in Example 1. The difference is that in step (1), the LFP particle size distribution width is adjusted to 1.63; the mass ratio of positive electrode active material, conductive agent, binder and pore-forming agent is 96.15:1.8:2:0.05; and the electrode is not perforated.

[0079] In step (3), ethyl acetate is 12 wt%, methyl propionate is 13 wt%, and the remaining organic solvents are adjusted proportionally.

[0080] Example 8 The preparation method of the battery in this embodiment is basically the same as that in Example 1, except that in step (1), the positive electrode active material is MCN. The particle size distribution width of MCN is adjusted to 1.88; the mass ratio of positive electrode active material, conductive agent, binder and pore-forming agent is 95.8:1.8:2:0.4; and the electrode perforation density is 200 per cm. 2 The compacted density of the positive electrode sheet is 2.8 g / cm³. 3 .

[0081] In step (3), ethyl acetate 20 wt%, methyl propionate 10 wt%, and the remaining organic solvents are adjusted proportionally.

[0082] Example 9 The preparation method of the battery in this embodiment is basically the same as that in Example 1, except that in step (1), the LFP particle size distribution width is adjusted to 1.25; the mass ratio of positive electrode active material, conductive agent, binder, and pore-forming agent is 96.18:1.8:2:0.02; and the electrode sheet is not perforated. The compaction density of the positive electrode sheet is 2.55 g / cm³. 3 .

[0083] In step (3), ethyl acetate 25 wt%, methyl propionate 20 wt%, and the remaining organic solvents are adjusted proportionally.

[0084] Comparative Example 1 The preparation method of the battery in this comparative example is basically the same as that in Example 1, except that in step (1), the LFP particle size distribution width is adjusted to 1.88; the mass ratio of positive electrode active material, conductive agent and binder is 96.2:1.8:2:0.3; and the electrode perforation density is 20 holes / cm. 2 The compacted density of the positive electrode sheet is 2.7 g / cm³. 3 .

[0085] In step (3), ethyl acetate is 17 wt%, methyl propionate is 20 wt%, and the remaining organic solvents are adjusted proportionally.

[0086] Comparative Example 2 The preparation method of the battery in this comparative example is basically the same as that in Example 1, except that in step (1), the LFP particle size distribution width is adjusted to 1.45; the mass ratio of positive electrode active material, conductive agent, binder and pore-forming agent is 95.7:1.8:2:0.5; and the electrode perforation density is 150 per cm. 2The compacted density of the positive electrode sheet is 2.55 g / cm³. 3 .

[0087] In step (3), ethyl acetate is 5 wt%, methyl propionate is not included, and the remaining organic solvents are adjusted proportionally.

[0088] Comparative Example 3 The preparation method of the battery in this comparative example is basically the same as that in Example 1, except that in step (1), the LFP particle size distribution width is adjusted to 1.78; the mass ratio of positive electrode active material, conductive agent, and binder is 96.2:1.8:2:0.3; and the electrode sheet is not perforated. The compaction density of the positive electrode sheet is 2.75 g / cm³. 3 .

[0089] In step (3), ethyl acetate 20 wt%, methyl propionate 20 wt%, and the remaining organic solvents are adjusted proportionally.

[0090] Comparative Example 4 The preparation method of the battery in this comparative example is basically the same as that in Example 1, except that in step (1), the LFP particle size distribution width is adjusted to 1.23; the mass ratio of positive electrode active material, conductive agent, binder and pore-forming agent is 95.6:1.8:2:0.6; and the electrode perforation density is 100 per cm. 2 The compacted density of the positive electrode sheet is 2.5 g / cm³. 3 .

[0091] In step (3), ethyl acetate is 6 wt%, methyl propionate is not included, and the remaining organic solvents are adjusted proportionally.

[0092] Comparative Example 5 The preparation method of this comparative example battery is basically the same as that of Example 1, except that in step (1), the LFP particle size distribution width is adjusted to 1.78; the pore-forming agent is tributyl phosphate; and the mass ratio of positive electrode active material, conductive agent, binder, and pore-forming agent is 95.6:1.8:2:0.6; the electrode sheet is not perforated. The compaction density of the positive electrode sheet is 2.75 g / cm³. 3 .

[0093] In step (3), ethyl acetate 10 wt%, methyl propionate 20 wt%, and the remaining organic solvents are adjusted proportionally.

[0094] Comparative Example 6 The preparation method of the battery in this comparative example is basically the same as that in Example 1, except that the organic solvent of the electrolyte is selected as EC:EMC:DMC=3:5:2.

[0095] Table 1

[0096] As shown in Table 1, this invention achieves a lithium-ion battery with both excellent cycle stability and low-temperature kinetic performance by controlling the average area ratio of micropores in the positive electrode active material layer, the sphericity of the micropores, and the content of carboxylic acid ester solvents in the electrolyte.

[0097] When the value of a / (b×c) in Comparative Example 1 is too low, the effective liquid storage space inside the positive electrode is insufficient, the irregular micropore morphology leads to a significant decrease in electrolyte retention capacity, local liquid shortage is prone to occur during long-term cycling, the interfacial side reactions are aggravated, the cycle stability shows a significant downward trend, and the battery life is greatly shortened.

[0098] In Comparative Example 2, the a / (b×c) value was too high, resulting in a significant increase in the dissolution of the pore-forming agent, leading to an increase in electrolyte viscosity, increased lithium-ion transport resistance, and a sharp deterioration in low-temperature kinetic performance. In Comparative Example 3, the a / (b×c) value was too low, resulting in the most significant decrease in cycle stability and the most severe degradation in overall battery performance. In Comparative Example 4, the a / (b×c) value was too high, leading to a significant increase in electrolyte viscosity due to the large amount of pore-forming agent dissolution, hindering lithium-ion migration, significantly increasing low-temperature impedance, and drastically reducing low-temperature fast-charging capability, with a prominent trend of deteriorating kinetic performance. In Comparative Example 5, insufficient liquid storage space, poor micropore regularity, weak liquid retention capacity, significantly decreased cycle stability, increased interfacial side reactions, and an overall downward trend in performance. Comparative Example 6 lacked carboxylic acid ester solvents, resulting in a sharp increase in electrolyte viscosity at low temperatures and hindered lithium-ion transport. Simultaneously, it could not offset the viscosity increase caused by the dissolution of the pore-forming agent, causing severe liquid shortage in the positive electrode during long-term cycling, exacerbating interfacial side reactions, and ultimately significantly deteriorating both battery cycle stability and low-temperature fast-charging performance.

[0099] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A lithium battery, characterized in that, The device includes a positive electrode sheet and an electrolyte. The positive electrode sheet includes a positive active material layer containing micropores. The electrolyte includes an organic solvent, which includes a carboxylic acid ester solvent. Wherein, the percentage of the micropores to the area of ​​the positive electrode active material layer is a; The average major axis length L of the micropore max The length is 0.01–1 μm, and the average minor axis length L min The value is 0.01–1 μm, and L max ≥L min ; The circularity of the micropore is b, where b = L max / L min ; The mass percentage of the carboxylic acid ester solvent in the organic solvent is c; The lithium battery satisfies the following condition: a / (b×c) = 0.11~2.

22.

2. The lithium battery according to claim 1, characterized in that, The lithium battery satisfies: a / (b×c) = 0.2~1.

11.

3. The lithium battery according to claim 1, characterized in that, The a = 10%~40%, and / or, The value of b is 1.5 to 8.0, and / or, The value of c is 10% to 30%.

4. The lithium battery according to claim 1, characterized in that, The carboxylic acid ester solvent includes at least one of ethyl acetate, propyl acetate, methyl formate, methyl acetate, methyl butyrate, ethyl propionate, and methyl propionate.

5. The lithium battery according to claim 4, characterized in that, The carboxylic acid ester solvent is ethyl acetate.

6. The lithium battery according to claim 1, characterized in that, The organic solvent also includes carbonate solvents, which account for 70-90% of the total organic solvent by mass.

7. The lithium battery according to claim 6, characterized in that, The carbonate solvents include at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, and methyl propyl carbonate.

8. The lithium battery according to claim 7, characterized in that, The carbonate solvent is ethylene carbonate.

9. The lithium battery according to claim 7, characterized in that, When the carboxylic acid ester solvent is ethyl acetate, the mass ratio of ethylene carbonate to ethyl acetate in the organic solvent is 1:(0.5~1.5).

10. The lithium battery according to claim 1, characterized in that, The electrolyte further includes lithium salts and additives, wherein the lithium salts include at least one of lithium hexafluorophosphate, lithium perchlorate, lithium tetrafluoroborate, lithium dioxaborate, lithium bis(trifluoromethanesulfonyl)imide, and lithium hexafluoroarsenate, and / or, The additive includes at least one of vinylene carbonate, 4-methylvinyl sulfite, and butene sulfite.

11. The lithium battery according to claim 10, characterized in that, The lithium salt accounts for 10% to 20% of the mass percentage of the electrolyte, and / or, The additive accounts for 2% to 10% of the mass of the electrolyte.

12. The lithium battery according to claim 1, characterized in that, The positive electrode active material layer includes a positive electrode active material, which includes at least one of lithium iron phosphate, lithium cobalt oxide, lithium manganese iron phosphate, ternary materials, and lithium manganese oxide.

13. The lithium battery according to claim 12, characterized in that, When the positive electrode active material is lithium iron phosphate, a = 20%~30%.

14. The lithium battery according to claim 12, characterized in that, The particle size D of the lithium iron phosphate 50 The range is 0.02~15μm.

15. The lithium battery according to claim 12, characterized in that, The lithium iron phosphate comprises large particles and small particles, wherein the particle size D of the large particles is... 50 The particle size D of the small particles is 0.8~4μm. 50 The thickness is 0.2~0.8μm.

16. The lithium battery according to claim 15, characterized in that, The lithium iron phosphate also includes ultra-small particles and ultra-large particles, wherein the particle size D of the ultra-small particles is... 50 The particle size D of the ultra-large particles is 20~80nm. 50 The size is 4~15μm.

17. The lithium battery according to claim 16, characterized in that, The value of a is 20% to 30%.

18. The lithium battery according to claim 12, characterized in that, The particle size D50 of the ternary material is 2~20μm.

19. The lithium battery according to claim 12, characterized in that, When the ternary material is a nickel-cobalt-manganese ternary material, a = 5%~15%.

20. The lithium battery according to claim 1, characterized in that, The method for preparing the positive electrode sheet includes the following steps: The binder, conductive agent and positive electrode active material are mixed, and solvent, pore-forming agent and dispersing agent are added. The mixture is then impregnated, kneaded and dispersed at high speed to obtain the positive electrode slurry. The positive electrode slurry is coated onto the surface of the current collector, dried, and rolled to obtain the positive electrode sheet.

21. The lithium battery according to claim 20, characterized in that, The pore-forming agent includes any one or more of ethylene carbonate, polyethylene glycol, tributyl phosphate, triethylhexyl phosphate, methyl palmitate, and dioctyl adipate.

22. The lithium battery according to claim 20, characterized in that, The pore-forming agent is ethylene carbonate, and the particle size D50 of the ethylene carbonate is 50 μm to 500 μm.

23. The lithium battery according to claim 20, characterized in that, The pore-forming agent accounts for 0.1% to 3% of the mass of the positive electrode slurry.

24. The lithium battery according to claim 1, characterized in that, The lithium battery includes a negative electrode sheet, the negative electrode sheet includes a negative electrode active material layer, the negative electrode active material layer includes a negative electrode active material, and the negative electrode active material includes any one or more of graphite, silicon oxide, and silicon carbon.