Cylindrical lithium-ion battery and electric device
By setting the cooperative relationship between the weld and the connecting piece, the main bottleneck of current flow in the weld group inside the battery is transferred to the connecting piece area, which solves the problem of increased internal resistance and Joule heat accumulation in cylindrical lithium-ion batteries during high-rate discharge, and improves the cycle life and safety of the battery.
Patent Information
- Application Number
- CN202611202745.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-10
- Publication Date
- 2026-11-24
AI Technical Summary
When existing cylindrical lithium-ion batteries are discharged at high rates, the weld seams become the main bottleneck for current flow, causing the contact resistance to increase over time, the AC internal resistance and DC internal resistance to rise, Joule heat to accumulate, and affecting the battery cycle life.
By setting the synergistic relationship between the number of welds, their width, and the thickness of the collector plate, the equivalent flow cross-section of the weld group is made to be no less than 0.3 times the flow cross-section of the connecting piece. This transfers the main bottleneck of the flow to the detectable connecting piece area, reduces internal resistance, and suppresses Joule heat accumulation.
It effectively reduces the AC and DC internal resistance of the battery, suppresses the temperature rise during high-rate discharge, and improves the cycle life and safety of the battery.
Smart Images

Figure CN123162277A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery technology, and more particularly to a cylindrical lithium-ion battery and an electrical device. Background Technology
[0002] In recent years, to achieve the performance goals of high energy density and high-rate discharge, it is necessary to construct a current-carrying channel with extremely low AC / DC internal resistance to effectively control Joule heat accumulation, discharge temperature rise, and ensure long cycle life of the battery. Full-tab cells, by fully extending the tabs along the edge of the electrode sheet, shorten the electron transport path and significantly reduce the distributed resistance of the electrode bulk phase and the tabs. However, the current must still flow sequentially through the "current collector—connector—terminal" series channel to be finally discharged. The current collector and the negative electrode full tab are usually electrically connected by multiple laser welds. The number and width of the welds and the thickness of the current collector directly determine the equivalent current-carrying cross-section and contact resistance of this stage; the width and thickness of the connecting piece also limit its own current-carrying capacity.
[0003] Therefore, it is crucial to obtain a cylindrical lithium-ion battery that can achieve a balance between low internal resistance, low temperature rise, and long cycle life while ensuring high assembly reliability and safety. Summary of the Invention
[0004] In view of this, the present invention aims to at least partially solve one of the technical problems in the related art. To this end, the present invention provides a cylindrical lithium-ion battery and an electrical device that can prevent the contact resistance from continuously increasing over time, thereby effectively reducing the battery's AC and DC internal resistance, suppressing Joule heat accumulation and temperature rise during high-rate discharge, and providing a reliable current collector structure to ensure the battery's cycle life.
[0005] To solve the above-mentioned technical problems, the present invention is implemented as follows: According to one aspect of the present invention, a cylindrical lithium-ion battery is provided, comprising: a battery cell, the battery cell including a cylindrical housing, and a cell, a current collector and a connecting piece disposed in the housing; The cylindrical shell has an opening at one end along its axial direction; the battery cell includes an electrode assembly, which includes a positive electrode plate, a separator, and a negative electrode plate stacked together, and the electrode assembly is wound along its length to form the battery cell; in the axial direction, the battery cell has tabs at both ends respectively; The electrode tab and the current collector are welded together to form multiple weld seams; the connecting piece is connected to the current collector; the battery cell satisfies: Aw≥0.3×Ac; Among them, Aw=a b c, Ac=x y; a is the number of welds, in units of: welds; b is the width of any weld in the direction perpendicular to the axial direction, in units of: mm; c is the thickness of the manifold in the axial direction, in units of: mm; x is the width of the connecting piece, in units of: mm; y is the thickness of the connecting piece, in units of: mm.
[0006] In some of these implementations, the value of 'a' is 8 to 16.
[0007] In some of these embodiments, the value of b is 0.25mm to 0.35mm.
[0008] In some of these embodiments, the value of c is 0.15mm to 0.25mm.
[0009] In some of these embodiments, the value of x is 6mm to 10mm.
[0010] In some of these embodiments, the value of y is 0.15mm to 0.30mm.
[0011] In some of these embodiments, the weld seam on the manifold is curved.
[0012] In some embodiments, the device further includes a pole connected to the connecting piece, the pole being at least partially located outside the cylindrical housing; the diameter of the pole is 7mm to 9mm in the direction perpendicular to the axial direction.
[0013] In some of these implementations, the following condition is also satisfied: Ac≥I / J; Wherein, I is the discharge current of the battery cell under a constant current discharge of 10C, in A; J is the upper limit of the current density of the connecting piece under the constant current discharge condition of 10C, and the value of J is in the range of 18A / mm. 2 ~30A / mm 2 .
[0014] In some embodiments, the collector plate is further provided with an annular welding ring, which is located in the middle of the geometric plane of the collector plate; Multiple weld seams are distributed around the circumferential weld ring.
[0015] In some embodiments, the diameter D of the annular weld ring is 4.8 mm to 5.4 mm.
[0016] In some embodiments, the width W of the annular weld ring is 0.28 mm to 0.38 mm.
[0017] In some embodiments, an electrolyte is also included, which comprises a lithium salt, a solvent, and additives; The additives include fluoroethylene carbonate, ethylene sulfate, ethylene carbonate, and lithium nitrate; In the electrolyte, the mass percentage of fluoroethylene carbonate is 3-12 wt%, the mass percentage of ethylene sulfate is 0.3-2.5 wt%, the mass percentage of ethylene carbonate is 0.2-1.8 wt%, and the mass percentage of lithium nitrate is 0.3-2.0 wt%.
[0018] In some embodiments, the lithium salt comprises lithium bis(fluorosulfonyl)imide and lithium difluorooxalate borate; Wherein, based on the total mass of the lithium salt, the molar percentage of the lithium difluorosulfonylimide is 10%~30%, and the molar percentage of the lithium difluorooxalateborate is 0.1%~0.5%.
[0019] In some of these embodiments, the AC internal resistance of the battery cell is 2mΩ to 4mΩ.
[0020] In some of these embodiments, the DC internal resistance of the battery cells is 2 to 4 mΩ.
[0021] In some of these embodiments, the battery cell has a temperature rise rate of less than or equal to 4°C / min and a peak temperature of less than or equal to 80°C under 10C discharge conditions.
[0022] According to another aspect of the present invention, an electrical device is provided, comprising: a cylindrical lithium-ion battery as described in any of the above embodiments.
[0023] Implementing the technical solution of the present invention has at least the following beneficial effects: In this invention, by ensuring that a single battery cell satisfies Aw ≥ 0.3 × Ac, meaning that the equivalent current-carrying cross-section of the weld group (defined by the number of welds, weld width, and current collector thickness) is not less than 0.3 times the current-carrying cross-section of the connecting piece (defined by the width and thickness of the connecting piece), the main bottleneck of current flow is shifted from the internal and difficult-to-detect weld group to the connecting piece link, which can be easily inspected non-destructively. The collaborative criterion avoids localized erosion, incomplete welding, or weld cracking due to thermo-mechanical coupling during cycling caused by excessively high current density in a single weld, preventing the contact resistance from continuously increasing over time. This effectively reduces the battery's AC and DC internal resistance, suppresses Joule heat accumulation and temperature rise during high-rate discharge, and provides a reliable current collector structure guarantee for the battery's cycle life.
[0024] Additional aspects and advantages of the invention will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of the invention. Attached Figure Description
[0025] The accompanying drawings, which are incorporated in and form part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.
[0026] Figure 1 The diagram shown is a schematic diagram of the collector disk structure provided by the present invention.
[0027] Explanation of reference numerals in the attached figures: 10 – manifold; 20 – weld; 30 – circumferential weld ring.
[0028] The accompanying drawings have illustrated specific embodiments of the invention, which will be described in more detail below. These drawings and descriptions are not intended to limit the scope of the invention in any way, but rather to illustrate the concept of the invention to those skilled in the art through reference to particular embodiments. Detailed Implementation
[0029] The present invention will be further illustrated below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention.
[0030] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges or individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0031] Unless otherwise specified, all embodiments and optional embodiments of the present invention can be combined with each other to form new technical solutions.
[0032] Unless otherwise specified, all technical features and optional technical features of this invention can be combined to form new technical solutions.
[0033] Unless otherwise specified, all steps of the present invention may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.
[0034] Unless otherwise specified, the terms "comprising" and "including" as used in this invention can be open-ended or closed-ended. For example, "comprising" and "including" can mean that other components not listed may also be included, or that only the listed components may be included.
[0035] Currently, in the field of cylindrical lithium-ion batteries, especially for the 21650 all-tab, negative-electrode battery configuration, to achieve high-current discharge and low ohmic internal resistance, related technologies commonly employ all-tabs formed by extending the edges of the positive and negative electrode plates at both ends of the cell. These all-tabs are then laser-welded to a metal current collector to achieve current convergence, and a connecting piece connects the current collector to the terminal post, thus forming a complete current outflow channel. Utilizing the two-dimensional current convergence characteristic of the all-tabs in the radial direction shortens the electron transport distance within the electrode bulk phase, and multiple laser welds increase the electrical contact area between the current collector and the tabs, thereby reducing contact resistance. Because this design can significantly reduce the electrode bulk phase resistance, it is considered a promising approach for balancing low internal resistance and high energy density.
[0036] However, in specific assembly and high-rate discharge scenarios, the above solutions, on the one hand, require increasing the number or width of welds to expand the effective welding cross-section in order to ensure sufficient current carrying capacity. This increases laser heat input, easily burning through thin tab foil or causing overlapping heat-affected zones, resulting in welding defects. On the other hand, if the number and size of welds are limited to control process risks, the equivalent current carrying cross-section formed by multiple welds may be insufficient, resulting in a loss of coordination with the current carrying cross-section of the downstream connecting piece. In this case, the minimum cross-section of the entire current carrying channel will appear in the weld group section located inside the shell. Once the weld becomes the main bottleneck for current carrying, the current density at the weld point increases sharply during high-current discharge, easily causing local erosion, incomplete welding, and weld point cracking due to thermo-mechanical coupling during cycling, causing the contact resistance to continuously increase over time. For example, under high discharge conditions such as 10C, even if the connecting plate and the electrode are designed to be robust enough, if the equivalent cross-section of the weld group between the current collector and the full electrode is much smaller than the cross-section of the connecting plate, the internal resistance will still increase significantly, the Joule heat will be highly concentrated, the discharge temperature rise rate and peak temperature will exceed the allowable range, and the cycle life will be severely shortened.
[0037] Researchers in this invention have discovered that the design of the current flow channel did not treat the weld group and the connecting piece as a series conductive link, thus failing to establish a quantitative criterion for cross-parameter collaborative matching. The welds are located inside the battery casing, and their quality is difficult to fully assess using conventional non-destructive testing methods. Once they become a current flow bottleneck, they constitute a latent failure point. In contrast, the connecting piece is located in a more easily detectable area, and its current flow cross-section is easily measured and verified. Therefore, if the main current flow bottleneck can be shifted from the undetectable internal welds to the detectable external connecting piece through parameter coordination, the risk of latent failure can be effectively avoided while considering process fluctuations. In view of this, this invention proposes a cylindrical lithium-ion battery and power supply device. By establishing a cross-parameter collaborative criterion between the equivalent current flow cross-section of multiple laser welds between the current collector and the tabs and the current flow cross-section of the connecting piece, specifically limiting the number of welds, the width of any weld perpendicular to the axial direction, and the product of the current collector's axial thickness to be no less than 0.3 times the product of the connecting piece's width and thickness, the main current flow bottleneck is shifted from the weld area to the connecting piece area. Under this criterion, by coordinating parameters such as the number of welds, weld width, current collector thickness, connecting plate width, connecting plate thickness, and electrode diameter, it is possible to effectively reduce the AC and DC internal resistance of the battery while maintaining assembly reliability and structural compactness. This suppresses Joule heat accumulation and temperature rise during high-rate discharge and provides a reliable current collector structure guarantee for cycle life. In other words, the structural design approach centered on the coordinated matching of weld and connecting plate cross-sections solves the problems of high internal resistance, localized overheating, and cycle degradation caused by the current bottleneck falling within the undetectable weld. This achieves the technical effect of making current safety detectable and improving high-rate performance.
[0038] The specific technical solution of the present invention is as follows: Cylindrical lithium-ion batteries In some embodiments of the present invention, a cylindrical lithium-ion battery is provided, comprising: a battery cell, the battery cell including a cylindrical housing, and a cell, a current collector and a connecting piece disposed in the housing.
[0039] The cylindrical shell has an open end along its axial direction; the cell includes an electrode assembly, which includes a positive electrode, a separator, and a negative electrode stacked together, and the electrode assembly is wound along its length to form the cell; in the axial direction, the two ends of the cell are respectively provided with tabs; the tabs and the current collector are welded together to form multiple welds, and the connecting piece is connected to the current collector; the battery cell satisfies: Aw≥0.3×Ac.
[0040] Among them, Aw=a b c, Ac=x y; a is the number of welds, unit: welds; b is the width of any weld in the direction perpendicular to the axial direction, unit: mm; x is the width of the connecting piece, unit: mm; c is the thickness of the collector plate in the axial direction, unit: mm; y is the thickness of the connecting piece, unit: mm.
[0041] As an example, refer to Figure 1 A battery cell comprises a cylindrical casing, a cell, a current collector, and connecting tabs. The cylindrical casing houses the cell, current collector, connecting tabs, and electrolyte, providing mechanical protection and encapsulation space. The cylindrical casing extends axially, with one axial end forming an opening. This opening allows the cell, current collector, and connecting tabs to be inserted into the casing during assembly, and subsequently sealed by a cap, seal, or terminal assembly. The cell can be formed by winding an electrode assembly, which includes a positive electrode, a separator, and a negative electrode. The positive and negative electrodes are separated by the separator to reduce the risk of internal short circuits. The electrode assembly, wound along its length, forms a generally cylindrical structure. At each axial end of the cell are tabs, which collect the current from the electrode to the current collector. The current collector and tabs are welded together, and connecting tabs connect the current collector to the external output structure, thus forming a current path from the electrode, tabs, current collector, connecting tabs to the external terminals. It is understandable that the axial direction refers to the direction of the extension of the central axis of the cylindrical shell; the direction perpendicular to the axial direction can be the radial direction or any direction within the cross-section; the dimensions such as width, thickness, and diameter are all based on the actual measurement direction of the corresponding component in the assembled state.
[0042] The cylindrical casing can be made of steel, nickel-plated steel, aluminum, or other metals suitable for cylindrical battery packaging. The cell can be a full-tab wound core, or a partially full-tab or multi-tab wound core; when the cell uses a full-tab construction, the tabs are continuously or intermittently unfolded along the edge of the electrode sheet, forming an end-face tab layer at the end of the cell after winding. The current collector is a disc-shaped conductive component that is attached to the end face of the tab and used for current collection; it can be made of aluminum, copper, nickel, nickel-plated copper, nickel-plated aluminum, or composite metal materials. The connecting piece is a bridging conductive component that connects the current collector to the terminal post, cap terminal, or shell terminal; its width x is the lateral dimension of the connecting piece in the main current-carrying cross-section, and its thickness y is the dimension of the connecting piece in the direction perpendicular to its main plane. Welds can be formed by laser welding, resistance welding, ultrasonic welding, or a combination of these methods; when using laser welding, the weld width b is the width of the weld molten zone or effective conductive zone in the direction perpendicular to the axial direction. Aw is used to characterize the equivalent flow cross-section of a weld group consisting of multiple welds, while Ac is used to characterize the flow cross-section of the connecting piece. By establishing a proportional relationship between Aw and Ac, it is possible to achieve cross-sectional matching between the weld group and the connecting piece, rather than simply defining individual dimensions separately.
[0043] When Aw ≥ 0.3 × Ac, the weld group has an equivalent conductivity matching that of the connecting piece. The current collected by the tabs enters the current collector through multiple welds and is then discharged by the connecting piece. The weld is less likely to become a hidden weak point with poor current coverage that is difficult to detect. If Aw is less than 0.3 × Ac, the equivalent current-carrying cross-section of the weld group is too small relative to the connecting piece. The current density borne by a single weld increases, and the welding area is prone to local heating, resistance amplification at the cold weld, thermal fatigue cracking of the weld, and continuous increase in contact resistance during the cycle. Setting the lower limit of the ratio to 0.3 is beneficial to ensure the utilization of the welding process window and the internal space of the shell while making the heat distribution in the current path more uniform and reducing the temperature rise under high-rate discharge conditions. The above relationship does not require that the cross-section of the weld group must be equal to or greater than the cross-section of the connecting piece, thereby avoiding excessive increase in the number or width of welds to increase the cross-section of the weld group and reducing thermal damage to the tab foil.
[0044] It is also understandable that the battery cell can adopt a negative electrode-less system, that is, the negative electrode sheet includes a copper current collector without a negative electrode active material, or a conventional negative electrode sheet with a negative electrode active layer. The current collector can be set at the positive terminal, negative terminal, or both ends; the connecting piece can be directly welded to the current collector, or it can be connected to the current collector via an intermediate conductive component. The weld seams can be uniformly distributed circumferentially, or non-uniformly distributed according to the tab stack density, connecting piece position, or current collector opening position, as long as the equivalent current-carrying cross-section Aw of the weld seam group satisfies the aforementioned relationship.
[0045] In some embodiments, the value of 'a' is 8 to 16. For example, 'a' can be 8, 9, 10, 11, 12, 13, 14, 15, or 16 welds. If the number of welds 'a' is less than 8, the current shared by a single weld increases, and the coverage area of the weld on the current collector plate decreases, which can easily lead to insufficient current collection in the end face tabs. If the number of welds 'a' is greater than 16, the heat-affected zones of adjacent welds are likely to overlap, the welding cycle time is prolonged, and it may cause ablation or local embrittlement of the tab foil.
[0046] In some embodiments, the value of b is 0.25mm to 0.35mm. Exemplarily, b can be any value among 0.25mm, 0.255mm, 0.265mm, 0.275mm, 0.285mm, 0.295mm, 0.305mm, 0.315mm, 0.325mm, 0.335mm, 0.345mm, or 0.35mm, or any value between any two points. If the weld width b is less than 0.25mm, the effective fusion width is insufficient, and both the welding contact area and the flow area are small; if the weld width b is greater than 0.35mm, the heat input required to form that width increases, easily causing spatter, burn-through, or expansion of the heat-affected zone.
[0047] In some embodiments, the value of c is 0.15mm to 0.25mm. Exemplarily, c can be any value among 0.15mm, 0.155mm, 0.165mm, 0.175mm, 0.185mm, 0.195mm, 0.205mm, 0.215mm, 0.225mm, 0.235mm, 0.245mm, or 0.25mm, or any value between any two points. If the current collector thickness c is less than 0.15mm, the conductive cross-section and mechanical rigidity of the current collector are insufficient, making it prone to overheating and deformation under high current. If the current collector thickness c is greater than 0.25mm, it occupies more internal height space in the battery, and the energy required for welding increases.
[0048] In some embodiments, x is taken as 6mm to 10mm. For example, x can be any point value or any point value between any two points from 6mm, 6.2mm, 6.5mm, 6.8mm, 7.2mm, 7.5mm, 7.8mm, 8.2mm, 8.5mm, 8.8mm, 9.2mm or 10mm.
[0049] In some embodiments, the value of y is 0.15mm to 0.30mm. Exemplarily, y can be any value among 0.15mm, 0.16mm, 0.17mm, 0.185mm, 0.195mm, 0.205mm, 0.215mm, 0.225mm, 0.235mm, 0.255mm, 0.275mm, or 0.30mm, or any value between any two points. If the width x of the connecting piece is less than 6mm or the thickness y is less than 0.15mm, the cross-section of the connecting piece 14 is insufficient, easily becoming a bottleneck for flow. If the width x of the connecting piece is greater than 10mm or the thickness y is greater than 0.30mm, the space occupied by the connecting piece within the shell increases, bending stress and welding heat input rise, which is detrimental to assembly consistency. It can also be understood that the connecting piece can be a straight piece, a bent piece, a bent piece with a stress-relieving arc, or a multi-layered stacked piece; the collector plate can be a disc, a notched disc, a disc with folded ears, or a partially hollowed-out disc. The selection of each parameter can be adjusted according to the battery capacity, the inner diameter of the casing, the thickness of the electrode tabs, and the energy distribution of the welding equipment.
[0050] In some embodiments, the weld seam on the manifold is curved. Exemplarily, a curved weld seam refers to a weld seam that extends non-linearly in the plane projection of the manifold, such as a wavy, arc-shaped, serpentine, smoothly transitioned bend, or a curve formed by connecting multiple arc segments. Curved weld seams can increase the actual welding path length within a limited disk area and reduce stress concentration at the weld ends. Furthermore, curved weld seams provide greater deformation release capability during thermal cycling, current surges, and slight axial springback of the core, reducing the risk of crack propagation at the weld ends; simultaneously, the curved trajectory increases the effective contact area between the electrode tab and the manifold, helping to reduce contact resistance. It is understood that curved weld seams can be formed by galvanometer scanning laser or by a combination of workpiece rotation and linear laser head feed.
[0051] In some embodiments, the following condition is also satisfied: Ac≥I / J; where I is the discharge current of a single battery cell at 10C, in A; and J is the upper limit of the design current density of the connecting piece under specified high-rate discharge conditions. When the battery cell is discharged at a constant current of 10C to the cutoff voltage at 25℃±1℃, J can be determined based on the conductive material of the connecting piece, its effective conductive cross-section, surface treatment, connection interface, internal heat dissipation conditions, and allowable temperature rise; J is 18A / mm². 2 ~30A / mm 2 As can be seen from Ac≥I / J, the actual current density I / Ac of the connector during 10C discharge does not exceed J, thereby reducing the risk of local Joule heat concentration and thermal degradation of the connector interface.
[0052] For example, the discharge current I at 10C refers to the current when the battery cell is discharged at a rate of 10 times its nominal capacity. For instance, a battery cell with a capacity of C0Ah can have a 10C discharge current of 10 × C0A. J is the allowable current density to pass through the connector material under short-term high-current discharge conditions, and its value is related to the material resistivity, heat dissipation conditions, surface treatment, allowable temperature rise, and duration. For copper, nickel, aluminum, or composite connectors, J can be determined according to the effective cross-section of the conductive layer in the material. J can be 18 A / mm². 2 19A / mm 2 20A / mm 2 21A / mm 2 22A / mm 2 23A / mm 2 24A / mm 2 25A / mm 2 26A / mm 2 27A / mm 2 29A / mm 2 Or 30A / mm 2Ac can be any point value or any point value between any two points. Optionally, Ac can be determined according to I / 19, I / 20, I / 21, I / 22, I / 23, I / 24, I / 25, I / 26, I / 27 or I / 28, in mm. 2 .
[0053] When Ac≥I / J and J≤30A / mm 2 The actual current density of the connector during 10C discharge will not exceed the short-term allowable capacity of the material, thus reducing Joule heat concentration in the connector area. If Ac is less than I / J, the connector becomes a high-temperature region in the current path under high-rate discharge, which may lead to localized heating, discoloration, surface oxidation, softening of the weld interface, or further increase in resistance. If J is greater than 30A / mm... 2 While the calculated cross-section of the connecting piece can be reduced, the limited heat dissipation conditions in the enclosed environment of the battery casing result in insufficient temperature rise margin for the connecting piece, which is detrimental to safety and reliability after long-term cycling. Therefore, directly associating Ac with I and J allows the cross-section of the connecting piece to be enlarged according to the battery capacity and rate requirements, avoiding inconsistencies in overcurrent capacity between batteries of different capacities caused by relying solely on a fixed width or thickness. It is understandable that the connecting piece can be obtained by multi-layer thin-sheet lamination to achieve an equivalent Ac, or by locally thickening, widening, or adding reinforced conductive areas to increase the overcurrent cross-section. For battery cells used at different rate rates, I can be re-determined based on the highest continuous discharge rate or peak pulse rate, and the width x and thickness y of the connecting piece can be selected accordingly.
[0054] In some embodiments, the collector plate is further provided with an annular weld ring, which is located in the middle of the geometric plane of the collector plate; multiple welds are distributed around the annular weld ring.
[0055] For example, to further improve the connection stability between the root region of the electrode tab and the collector plate, an annular weld ring is also provided on the collector plate, located in the middle of the geometric plane of the collector plate; multiple welds are distributed around the annular weld ring. The annular weld ring is a ring-shaped welding area located in the middle of the plane of the collector plate, which can be a continuous closed ring or an approximately annular weld ring formed by multiple arc-shaped weld segments spaced end to end. The middle of the geometric plane of the collector plate refers to the central region of the collector plate in the plane projection perpendicular to the axial direction. This central region can be concentric with the axis of the cylindrical shell, or it can be slightly eccentric due to the need to avoid connecting pieces, electrode posts, or exhaust structures. Multiple welds distributed around the annular weld ring means that the welds are located radially outside the annular weld ring or arranged along the outer periphery of the annular weld ring, so that the annular weld ring and the plate surface welds together form a welded structure with central reinforcement and circumferential convergence.
[0056] The annular weld ring forms a continuous or near-continuous connecting band at the root of the tab, enabling the current collector and tab to conduct through not only discrete plate welds but also enhanced mechanical bonding via a central annular region. During the winding of the battery cell, minor axial or radial stresses are generated during casing insertion, grooving, sealing, and cyclic expansion. The annular weld ring can share the peel load of the plate welds, reducing the risk of a sudden increase in contact resistance due to root cracking. Without the annular weld ring, the plate welds can still conduct, but under vibration, thermal cycling, or core springback conditions, the connection strength and peel resistance at the tab root are relatively reduced. The annular weld ring can be formed continuously in the same welding process as the plate welds, or it can be formed first and then the plate welds, or vice versa. Understandably, the annular weld ring can be circular, elliptical, a polygonal rounded-corner ring, or a ring pattern composed of multiple concentric short arcs, as long as it is located in the center of the current collector and reinforces the root of the tab.
[0057] In some embodiments, the battery cell further includes a terminal post connected to a connecting piece, and the terminal post is at least partially located outside the cylindrical housing; the diameter of the terminal post is 7mm to 9mm in the direction perpendicular to the axial direction.
[0058] For example, the electrode diameter can be any value among 7mm, 7.1mm, 7.2mm, 7.4mm, 7.6mm, 7.8mm, 8.0mm, 8.2mm, 8.4mm, 8.6mm, 8.8mm, or 9mm, or any value between any two points. If the electrode diameter is less than 7mm, the electrode's own conductive cross-section is insufficient, increasing the contact interface resistance between the electrode and the connecting piece or external terminal, easily forming hot spots in the terminal area during high-rate discharge. If the electrode diameter is greater than 9mm, the electrode occupies too much space in the middle of the cap, potentially affecting the arrangement of the sealing structure, pressure relief structure, or insulation structure, and increasing the risk of assembly interference. It is understood that the electrode can be a copper electrode, aluminum electrode, nickel electrode, copper-aluminum composite electrode, or a surface-plated nickel electrode. The connecting piece and the electrode can be joined by laser welding, riveting welding, ultrasonic welding, or conductive riveting to form a low-contact-resistance connection.
[0059] In some embodiments, the diameter D of the annular weld ring is 4.8 mm to 5.4 mm. Exemplarily, the diameter D can be any value among 4.8 mm, 4.86 mm, 4.92 mm, 4.98 mm, 5.04 mm, 5.08 mm, 5.12 mm, 5.16 mm, 5.22 mm, 5.28 mm, 5.34 mm, or 5.4 mm, or any value between any two points. If the diameter D of the annular weld ring is less than 4.8 mm, the annular weld ring is too close to the central region, providing insufficient support for the outer side of the electrode root and the inner end of the plate weld; if the diameter D is greater than 5.4 mm, the annular weld ring may be too close to the dense area of the plate weld or affect the arrangement of the connecting piece, the current collector opening, and the insulation structure. It is understood that the annular weld ring can be formed using single-pass laser scanning or double-pass overlapping scanning. For thinner tabs, a lower power and a higher scanning speed can be used for the annular weld ring; for multi-layer tabs with thicker stacks, pulsed lasers or oscillating lasers can be used to improve the consistency of the weld penetration.
[0060] In some embodiments, the width W of the annular weld ring is 0.28 mm to 0.38 mm. Exemplarily, W can be any value among 0.28 mm, 0.285 mm, 0.295 mm, 0.305 mm, 0.315 mm, 0.325 mm, 0.335 mm, 0.345 mm, 0.355 mm, 0.365 mm, 0.375 mm, or 0.38 mm, or any value between any two points. If the width W of the annular weld ring is less than 0.28 mm, its effective fusion area is insufficient, reducing its reinforcement and conductivity; if the width W is greater than 0.38 mm, the welding heat input increases, and the tab foil may overheat, burn through, or have an excessively wide heat-affected zone. Limiting D and W within the above ranges ensures that the annular weld ring falls within the effective tab root region while avoiding excessive heat input.
[0061] In some embodiments, an electrolyte is also included, comprising a lithium salt, a solvent, and additives; the additives include fluoroethylene carbonate, ethylene sulfate, vinylene carbonate, and lithium nitrate; wherein the fluoroethylene carbonate accounts for 3-12 wt% by mass, the ethylene sulfate accounts for 0.3-2.5 wt% by mass, the vinylene carbonate accounts for 0.2-1.8 wt% by mass, and the lithium nitrate accounts for 0.3-2.0 wt% by mass.
[0062] Exemplarily, the electrolyte is used to conduct lithium ions between the positive and negative electrodes and participates in the formation of the electrode interface film during charging and discharging. Fluoroethylene carbonate (FEC) can participate in the formation of fluorine-containing interface components; ethylene sulfate (DTD) can provide sulfur-containing film-forming species; vinylene carbonate (VC) is beneficial for forming polymeric interface films; and lithium nitrate can provide nitrogen-containing interface components. Fluoroethylene carbonate is preferably 5 wt% to 10 wt%; optionally, its mass percentage can be 3.5 wt%, 4.0 wt%, 4.8 wt%, 5.6 wt%, 6.4 wt%, 7.2 wt%, 8.0 wt%, 8.8 wt%, 9.6 wt%, or 10.8 wt%. Ethylene sulfate is preferably from 0.8 wt% to 1.8 wt%; alternatively, its mass percentage can be 0.45 wt%, 0.65 wt%, 0.85 wt%, 1.05 wt%, 1.25 wt%, 1.45 wt%, 1.65 wt%, 1.85 wt%, 2.05 wt%, or 2.25 wt%. Ethylene carbonate is preferably from 0.5 wt% to 1.4 wt%; alternatively, its mass percentage can be 0.3 wt%, 0.45 wt%, 0.6 wt%, 0.75 wt%, 0.9 wt%, 1.05 wt%, 1.2 wt%, 1.35 wt%, 1.5 wt%, or 1.65 wt%. Lithium nitrate is preferably from 0.6 wt% to 1.5 wt%; alternatively, its mass percentage can be 0.4 wt%, 0.55 wt%, 0.7 wt%, 0.85 wt%, 1.0 wt%, 1.15 wt%, 1.3 wt%, 1.45 wt%, 1.65 wt%, or 1.85 wt%.
[0063] When the content of fluoroethylene carbonate is below 3 wt%, the fluorinated interfacial film component is insufficient, leading to decreased stability of the negative electrode interface during cycling. When its content is above 12 wt%, electrolyte viscosity and the risk of side reactions increase, and gas generation may increase. When the content of ethylene sulfate is below 0.3 wt%, its contribution to the flexibility of the interfacial film and sulfur-containing components is insufficient; when it is above 2.5 wt%, the film-forming reaction is too strong, which may result in an excessively thick interfacial film and increased impedance. When the content of ethylene carbonate is below 0.2 wt%, polymerization film formation is insufficient; when it is above 1.8 wt%, the interfacial film thickens and the risk of gas generation increases. When the content of lithium nitrate is below 0.3 wt%, the nitrogen-containing interfacial component is insufficient; when it is above 2.0 wt%, dissolution stability and the difficulty of controlling side reactions increase. When the four additives are combined within the above ranges, a more stable interfacial film can be formed on the electrode surface, reducing charge transfer impedance. Combined with a low-resistance current collector structure, this suppresses heat generation during high-rate discharge and improves cycle stability.
[0064] In some embodiments, the lithium salt includes lithium bis(fluorosulfonyl)imide and lithium difluorooxalate borate; wherein, based on the total mass of the lithium salt, the molar percentage of lithium bis(fluorosulfonyl)imide is 10% to 30%, and the molar percentage of lithium difluorooxalate borate is 0.1% to 0.5%.
[0065] Optionally, the solvent may include ethylene carbonate, ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate, fluoroether, carboxylic acid ester, or a combination thereof.
[0066] For example, lithium bisfluorosulfonylimide (LiFSI) can co-form a dual-salt or multi-salt system with a main salt such as lithium hexafluorophosphate to improve ion migration and low-temperature conductivity. Lithium difluorooxalate borate (LiDFOB) can provide boron- and fluorine-containing film-forming species and improve the compactness of the interfacial film. The molar percentage of LiFSI is preferably 15% to 25%; alternatively, the molar percentage of LiFSI can be 11%, 13%, 15.5%, 17%, 18.5%, 20%, 21.5%, 23%, 25.5%, or 28%. The molar percentage of LiDFOB is preferably 0.2% to 0.4%; alternatively, the molar percentage of LiDFOB can be 0.12%, 0.16%, 0.20%, 0.24%, 0.28%, 0.32%, 0.36%, 0.40%, 0.44%, or 0.48%. When preparing the solution, LiFSI and LiDFOB can coexist, or one of them can be selected to be compounded with the main salt depending on the battery system. When they coexist, the total salt concentration, solubility and electrolyte viscosity should be taken into account.
[0067] When the molar proportion of LiFSI is below 10%, its improvement on ionic conductivity and interfacial film formation is insufficient. When the molar proportion of LiFSI is above 30%, the corrosion control of the electrolyte 16 on aluminum current collectors or other metal components becomes more difficult, and may lead to increased costs and viscosity. When the molar proportion of LiDFOB is below 0.1%, the contribution of boron-containing film formation is insufficient; when it is above 0.5%, it may cause excessively thick interfacial films, salting-out risks, or decreased low-temperature performance. Controlling LiFSI and LiDFOB within the above ranges can reduce interfacial impedance and maintain a stable interfacial film, thereby synergizing with the low-resistance current flow structure formed by the current collector 13, weld 131, connecting piece 14, and electrode post 15.
[0068] In some embodiments, the AC internal resistance of a single battery cell is 2mΩ to 4mΩ.
[0069] In some embodiments, the DC internal resistance of the battery cells is 2 to 4 mΩ.
[0070] In some embodiments, the battery cell has a temperature rise rate of less than or equal to 4°C / min and a peak temperature of less than or equal to 80°C under 10C discharge conditions.
[0071] For example, the AC internal resistance can be measured using the 1kHz AC impedance method, and the DC internal resistance can be measured using the HPPC pulse method or the specified rate pulse discharge method. The temperature rise rate can be obtained from the surface temperature curve of the battery cell under constant temperature of 25°C and constant current discharge at 10C; the peak temperature can be the highest temperature measured on the surface of the casing or near the terminal during the entire discharge process. The AC internal resistance is preferably 2.3mΩ to 3.5mΩ; optionally, the AC internal resistance can be 2.1mΩ, 2.2mΩ, 2.4mΩ, 2.6mΩ, 2.8mΩ, 3.0mΩ, 3.2mΩ, 3.4mΩ, 3.6mΩ, or 3.8mΩ. The DC internal resistance is preferably between 2.5 mΩ and 3.6 mΩ; alternatively, the DC internal resistance can be 2.1 mΩ, 2.3 mΩ, 2.5 mΩ, 2.7 mΩ, 2.9 mΩ, 3.1 mΩ, 3.3 mΩ, 3.5 mΩ, 3.7 mΩ, or 3.9 mΩ. The temperature rise rate is preferably no greater than 3.5 °C / min; alternatively, the temperature rise rate can be 2.2 °C / min, 2.4 °C / min, 2.6 °C / min, 2.8 °C / min, 3.0 °C / min, 3.2 °C / min, 3.4 °C / min, 3.6 °C / min, 3.8 °C / min, or 3.9 °C / min. The peak temperature is preferably no greater than 75 °C; alternatively, the peak temperature can be 62 °C, 64 °C, 66 °C, 68 °C, 70 °C, 72 °C, 74 °C, 76 °C, 78 °C, or 79 °C.
[0072] When the AC or DC internal resistance is below 2 mΩ, a larger metal cross-section or a higher welding area is typically required, which may sacrifice energy density or assembly reliability under the limited internal space of a cylindrical casing. When the AC or DC internal resistance is above 4 mΩ, Joule heating increases significantly during 10C discharge, and both voltage drop and temperature rise increase. When the temperature rise rate is greater than 4 °C / min, the temperature of the battery cell accumulates too quickly under continuous high-rate discharge, which is detrimental to thermal management. When the peak temperature is greater than 80 °C, the risk of electrolyte side reactions, interfacial film decomposition, and safety valve activation increases. Limiting the above performance parameters within this range allows for measurable indicators to reflect the fit between the current collector, weld, connecting piece, electrode, and electrolyte.
[0073] Optionally, the battery may further include a positive electrode, a negative electrode, and a separator. As an example, the positive electrode includes a positive current collector and an active coating disposed on at least one surface of the positive current collector along its thickness direction. The aforementioned "active coating disposed on at least one surface of the positive current collector" means that the positive active layer can be disposed on one surface of the positive current collector along its thickness direction, or on two surfaces of the positive current collector along its thickness direction. Here, "surface" can be the entire area of the positive current collector or a portion of the positive current collector; this application does not have any particular limitation, as long as the purpose of this application is achieved. In this invention, the separator is not particularly limited, as long as the purpose of this invention is achieved. Optionally, the separator includes, but is not limited to, a polymer separator of at least one of polyethylene, polypropylene, polyacrylonitrile, polysulfonyl, polyarylethersulfone, polyvinyl alcohol, and polyvinylidene fluoride.
[0074] Optionally, the battery may include an outer packaging that can be used to encapsulate the aforementioned electrode assembly and electrolyte. The outer packaging of the battery may be a rigid shell, such as a hard plastic shell, aluminum shell, steel shell, etc. Specifically, the rigid shell may include a housing and a cover plate, wherein the housing may include a bottom plate and a side plate connected to the bottom plate, the bottom plate and the side plate forming a receiving cavity, the housing having an opening communicating with the receiving cavity, and the cover plate being able to cover the opening to close the receiving cavity, the electrode assembly being encapsulated in the aforementioned receiving cavity, and the electrolyte in any of the above embodiments being immersed in the electrode assembly; it may also be a soft pack, such as a pouch soft pack; the material of the soft pack may be plastic, and examples of plastics include polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0075] <Electrical Appliances> In some embodiments of the present invention, an electrical device is also provided, comprising: the cylindrical lithium-ion battery of any of the above embodiments.
[0076] Optionally, the electrical devices can be vehicles, mobile phones, portable devices, laptops, ships, spacecraft, electric toys, power tools, energy storage devices, amusement equipment, elevators and lifting equipment, etc. Electric toys include stationary or mobile electric toys, such as game consoles, electric car toys, electric ship toys, or electric airplane toys, etc.; power tools include metal cutting power tools, grinding power tools, assembly power tools, and railway power tools, such as electric drills, electric grinders, electric wrenches, electric screwdrivers, electric hammers, impact drills, concrete vibrators, and electric planers, etc.; energy storage devices can be energy storage walls, base station energy storage, container energy storage, etc.; amusement equipment can be carousels, drop towers, etc. The aforementioned vehicles can be fuel-powered vehicles, natural gas vehicles, or new energy vehicles. New energy vehicles can be pure electric vehicles, hybrid electric vehicles, or range-extended electric vehicles, etc. A battery is installed inside the vehicle, which can be located at the bottom, front, or rear of the vehicle. The battery can be used to power the vehicle; for example, the battery can serve as the vehicle's operating power source. The vehicle may also include a controller and a motor. The controller controls the battery's power supply to the motor, for example, to meet the vehicle's power needs during starting, navigation, and driving. The battery can serve not only as the vehicle's operating power source but also as its driving power source, replacing or partially replacing fuel or natural gas to provide propulsion.
[0077] Since the battery provided in this embodiment of the invention adopts all the technical solutions of the above embodiments, it has at least all the beneficial effects brought about by the technical solutions of the above embodiments, and will not be described in detail here.
[0078] The present invention will be described in detail below with reference to the accompanying drawings and embodiments. However, the implementation and protection of the present invention are not limited thereto. The following embodiments are only some embodiments of the present invention and are not intended to limit the present invention.
[0079] Structural assembly and welding preparation methods 1. Assembly of the current collector and the current collector: The positive electrode uses NCM811 double-sided coated aluminum foil, and the negative electrode is a bare copper current collector (6μm bright copper foil or three-dimensional porous copper with a porosity of 30-40%) without any active material coating. The separator is a ceramic-coated PP / PE / PP three-layer composite film. The current collector is wound into a core (outer diameter approximately 20.4mm) in the order of "copper foil, separator, positive electrode, separator". The upper and lower ends of the core form full-tab end faces. An aluminum current collector with a thickness of 0.15-0.25mm (outer diameter 18.2mm, folded ear width 8mm, no fuse design) is attached to the full-tab end face of the negative electrode.
[0080] 2. Laser welding of the manifold: A fiber laser is used to weld the manifold and the tabs. (a) Surface weld: Four groups of wavy radial welds are arranged circumferentially, with three welds in each group, for a total of 12 welds. Each weld is 0.25–0.35 mm wide and 5–7 mm long, with a wavy / corrugated shape to increase the effective welding area and release thermal stress; (b) Root ring weld: A continuous circumferential weld (outer diameter D = 4.8–5.4 mm, preferably 5.1 mm, weld width W = 0.28–0.38 mm, preferably 0.33 mm) is added to the root of the manifold to strengthen the electrical connection and mechanical bonding force at the root. The welding power and scanning speed must be matched to ensure appropriate penetration depth, avoiding both incomplete welding and burning through the tab foil. After welding, Aw ≥ 0.3 × Ac must be met.
[0081] 3. Connection between connecting plate and pole: The current collector and the pole (7-9mm in diameter) are welded together with aluminum / copper connecting plates that are 6-10mm wide and 0.15-0.30mm thick; stress relief arcs are reserved at the bending points of the connecting plates to avoid stress concentration during assembly.
[0082] 4. Insertion into the shell, grooving and sealing: After the core is inserted into the 21650 steel shell, it is positioned by grooving.
[0083] 5. Liquid injection and formation: The multifunctional composite electrolyte of this invention is injected at an injection coefficient of 1.8 to 2.3 g / Ah. After standing and soaking, a two-step formation method is adopted: the first step is to precharge to 3.8V at 0.02C, the second step is to charge to 4.2V at 0.05C and then keep the voltage constant at 0.01C, followed by discharge at 0.1C to 3.0V. The formation is carried out at 35±3℃.
[0084] Example 1 The current collector is 0.20mm thick, with 12 corrugated welds (4 groups × 3), each weld being 0.30mm wide and 6mm long. The connecting piece is 8mm wide and 0.20mm thick, and the electrode diameter is 9mm. The electrolyte uses an optimal quaternary formulation (1.0MLiPF6 / EC (ethylene carbonate):EMC (ethyl methyl carbonate):DMC (dimethyl carbonate) = 30:50:20, FEC 7.0 / DTD 1.2 / VC 1.0 / LiNO3 1.0wt%). The calculated cross-sectional area of the weld group, Aw, is 12 × 0.30 × 0.20 = 0.72mm. 2 The cross-sectional area of the connecting piece, Ac, is 8 × 0.20 = 1.60 mm. 2 , Aw / Ac=0.45≥0.3.
[0085] Example 2 Compared to Example 1, only the number of welds was reduced from 12 to 8, while the remaining structural parameters and electrolyte were exactly the same as in Example 1.
[0086] Example 3 The only difference is that the number of welds is increased from 12 to 16, and the rest is the same as in Example 1.
[0087] Example 4 The only difference is that the single seam width Ww is reduced from 0.30 to 0.25 mm, while the rest is the same as in Example 1.
[0088] Example 5 The only difference is that the thickness of the connecting piece is increased from 0.30 to 0.35 mm, and the rest is the same as in Example 1.
[0089] Example 6 The only difference is that the width of the connecting piece is reduced from 8 mm to 6 mm, and the rest is the same as in Example 1.
[0090] Example 7 The only difference is that the connecting piece is increased from 8mm to 10mm, and the rest is the same as in Example 1.
[0091] Example 8 The thickness of the connecting piece was reduced from 0.20 mm to 0.15 mm, and the rest was the same as in Example 1.
[0092] Example 9 The only difference is that the thickness of the collector plate is increased from 0.20 to 0.25 mm, and the rest is the same as in Example 1.
[0093] Example 10 The only difference is that the diameter of the pole post is reduced from 9 mm to 7 mm, and everything else is the same as in Example 1.
[0094] Example 11 The structure is the same as in Example 1, but the negative electrode current collector is changed from 6μm light copper foil to three-dimensional porous copper (porosity ≈35%, specific surface area increased by about 4 times), which improves the lithium plating morphology and reduces the local current density.
[0095] Example 12 The structure is the same as in Example 1, but 10 vol% of fluorinated ether TTE is introduced into the electrolyte to partially replace DMC, which improves the uniformity of wetting of bare copper and reduces the local internal resistance caused by uneven wetting of the inner winding.
[0096] Example 13 The structure is the same as in Example 1, except that the electrolyte is changed from 1.0M LiPF6 to a double salt of 0.8M LiPF6 and 0.2M LiFSI. - It participates in film formation to enhance ionic conductivity and reduce interfacial impedance.
[0097] Example 14 The structure is the same as in Example 1, but the formation temperature is increased from 35°C to 45°C to accelerate SEI densification.
[0098] Comparative Example 1 The total number of weld seams on the panel is reduced to 4 (1 seam / group × 4 groups), and the rest is the same as in Example 1.
[0099] Comparative Example 2 The width Wcp of the connecting piece is reduced to 3mm, and the rest is the same as in Example 1.
[0100] Comparative Example 3 With a single seam width of 0.20mm and 8 seams, Aw = 8 × 0.20 × 0.20 = 0.32mm 2 The rest is the same as in Example 1.
[0101] Comparative Example 4 The thickness of the manifold was reduced to 0.10 mm, and the rest was the same as in Example 1.
[0102] Comparative Example 5 The structure is the same as in Example 1, but the electrolyte used is a blank basic electrolyte without any functional additives (only 1.0M LiPF6 / 30:50:20).
[0103] Comparative Example 6 The structure is the same as in Example 1, but the electrolyte uses a high EC and high viscosity system (EC:EMC:DMC=50:30:20).
[0104] The only difference between Examples 1 to 14 is as shown in Table 1.
[0105] Table 1 Performance testing 1. Internal resistance characterization: AC internal resistance (ACR) is measured using the 1kHz AC impedance method (internal resistance meter); DC internal resistance (DCIR) is calculated using the HPPC pulse method (e.g., 10C, 10s pulse) based on the ratio of voltage step to current step. The contact / overcurrent resistance of the weld and connecting piece is calibrated separately using a four-wire micro-ohmmeter.
[0106] 2. High-rate temperature rise characterization: Discharged at a constant current of 10C under a constant temperature environment of 25±1℃, the temperature-time curve was recorded using a K-type thermocouple attached to the middle of the battery surface and near the terminal post (sampling interval 1s). The maximum temperature rise rate dT / dt (℃ / min) in the initial stage of discharge and the peak temperature Tmax (℃) throughout the process were taken.
[0107] 3. Welding quality characterization: X-ray / industrial CT was used to inspect the weld penetration, incomplete welds and burn-through; peel force test was used to evaluate the weld strength of the manifold-electrode; SEM was used to observe the weld morphology and heat-affected zone.
[0108] 4. Cycle life characterization: At 25℃, constant current and constant voltage charge and discharge cycles were performed at 1C / 1C, and the number of cycles when the capacity retention dropped to 80% was recorded; internal resistance and temperature rise were retested every 100 cycles to track structural degradation.
[0109] 5. Safety characterization: Conduct needle penetration (Φ3mm steel needle, 80mm / s) and overcharge (1C to 130% SOC) tests according to standards such as GB / T31485, and observe whether there is fire, explosion and bulging.
[0110] The test results are shown in Tables 2 and 3.
[0111] Table 2 Table 3 The parts of this invention not described in detail are techniques known to those skilled in the art.
[0112] The basic principles of the present invention have been described above with reference to specific embodiments. However, it should be noted that the advantages, benefits, and effects mentioned in the present invention are merely examples and not limitations, and should not be considered as essential features of each embodiment of the present invention. Furthermore, the specific details disclosed above are for illustrative and facilitative purposes only, and are not limitations. These details do not limit the present invention to the necessity of employing the aforementioned specific details.
[0113] It should be noted that the terms "and / or" or " / " used herein are merely descriptions of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, or B existing alone. The singular forms "a," "described," and "the" used in the embodiments of the invention and the appended claims are also intended to include the plural forms, unless the context clearly indicates otherwise.
[0114] In the detailed description and claims, a list of items connected by the terms "at least one of," "at least one of," "at least one of," or other similar terms may mean any combination of the listed items. For example, if items A and B are listed, then the phrase "at least one of A and B" means only A; only B; or A and B. In another example, if items A, B, and C are listed, then the phrase "at least one of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may contain a single element or multiple elements. Item B may contain a single element or multiple elements. Item C may contain a single element or multiple elements.
[0115] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A cylindrical lithium-ion battery, characterized in that, include: A battery cell, the battery cell comprising a cylindrical housing, and a cell, a current collector and a connecting piece disposed in the housing; The cylindrical shell has an opening at one end along its axial direction; the battery cell includes an electrode assembly, which includes a positive electrode plate, a separator, and a negative electrode plate stacked together, and the electrode assembly is wound along its length to form the battery cell; in the axial direction, the battery cell has tabs at both ends respectively; The electrode tab and the current collector are welded together to form multiple weld seams; the connecting piece is connected to the current collector; the battery cell satisfies: Aw≥0.3×Ac; Among them, Aw=a b c, Ac=x y; a is the number of welds, in units of: welds; b is the width of any weld in the direction perpendicular to the axial direction, in units of: mm; c is the thickness of the manifold in the axial direction, in units of: mm; x is the width of the connecting piece, in units of: mm; y is the thickness of the connecting piece, in units of: mm.
2. The cylindrical lithium-ion battery according to claim 1, characterized in that, The value of 'a' can be 8 to 16. And / or, the value of b is 0.25mm~0.35mm; And / or, the value of c is 0.15mm~0.25mm; And / or, the value of x is 6mm to 10mm; And / or, the value of y is 0.15mm~0.30mm.
3. The cylindrical lithium-ion battery according to claim 1 or 2, characterized in that, The weld seam on the manifold is curved; And / or, it also includes a pole post connected to the connecting piece, the pole post being at least partially located outside the cylindrical housing; the diameter of the pole post is 7mm to 9mm in the direction perpendicular to the axial direction.
4. The cylindrical lithium-ion battery according to claim 1, characterized in that, It also satisfies: Ac≥I / J; Wherein, I is the discharge current of the battery cell under a constant current discharge of 10C, in A; J is the upper limit of the current density of the connecting piece under the constant current discharge condition of 10C, and the value of J is in the range of 18A / mm. 2 ~30A / mm 2 .
5. The cylindrical lithium-ion battery according to claim 1, characterized in that, The collector plate is also provided with an annular welding ring, which is located in the middle of the geometric plane of the collector plate; Multiple weld seams are distributed around the circumferential weld ring.
6. The cylindrical lithium-ion battery according to claim 5, characterized in that, The diameter D of the annular weld ring is 4.8 mm to 5.4 mm; And / or, the width W of the annular weld ring is 0.28mm~0.38mm.
7. The cylindrical lithium-ion battery according to any one of claims 1 to 6, characterized in that, It also includes an electrolyte, which comprises lithium salt, solvent, and additives; The additives include fluoroethylene carbonate, ethylene sulfate, ethylene carbonate, and lithium nitrate; In this electrolyte, the mass percentage of fluoroethylene carbonate is 3-12 wt%, the mass percentage of ethylene sulfate is 0.3-2.5 wt%, the mass percentage of ethylene carbonate is 0.2-1.8 wt%, and the mass percentage of lithium nitrate is 0.3-2.0 wt%.
8. The cylindrical lithium-ion battery according to claim 7, characterized in that, The lithium salts include lithium bis(fluorosulfonyl)imide and lithium difluorooxalate borate. Wherein, based on the total mass of the lithium salt, the molar percentage of the lithium difluorosulfonylimide is 10%~30%, and the molar percentage of the lithium difluorooxalateborate is 0.1%~0.5%.
9. The cylindrical lithium-ion battery according to claim 1, characterized in that, The AC internal resistance of the battery cell is 2mΩ~4mΩ; And / or, the DC internal resistance of each battery cell is 2 to 4 mΩ; And / or, the battery cell, under 10C discharge conditions, has a temperature rise rate of less than or equal to 4℃ / min and a peak temperature of less than or equal to 80℃.
10. An electrical device, characterized in that, include: The cylindrical lithium-ion battery according to any one of claims 1 to 9.