Battery and method of manufacture
By using a protective coating designed with conjugated conductive polymers and dual dopants on the positive electrode of a ternary lithium-ion battery, a graded response to the battery's internal resistance is achieved, solving the problems of hysteresis and poor early warning in existing protective coatings, and providing precise safety protection inside the battery.
Patent Information
- Application Number
- CN202611347278.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-01
- Publication Date
- 2026-11-24
AI Technical Summary
The existing positive electrode protective coating of ternary lithium-ion batteries lacks a graded response mechanism, resulting in delayed protection and poor early warning effect. Commercial battery management systems cannot accurately identify internal battery anomalies, posing a risk of delayed monitoring response.
The protective coating, designed with a conjugated conductive polymer matrix and dual dopants, achieves a graded response of internal resistance across different voltage and temperature ranges through the difference in binding forces of weak electrostatic interactions and strong ionic bonds. The coating is stably conductive under normal conditions, but exhibits a stepwise abrupt change when overcharged or at high temperatures, providing precise early warning and blocking.
It enables early warning of abnormal internal battery voltage and temperature, keeps internal resistance stable within the normal operating range, and accurately blocks overcharging or high temperature, making up for the shortcomings of external BMS monitoring and ensuring battery safety.
Smart Images

Figure SMS_4
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery technology, and in particular to a battery and its preparation method. Background Technology
[0002] Ternary lithium-ion batteries have achieved large-scale application due to their high energy density. However, with the increase in energy density, the risk of thermal runaway caused by overcharging and high temperature has increased. Within the cutoff voltage range of 4.25~4.45V, the ternary cathode is prone to interface failure, which eventually triggers thermal runaway. The problem is more prominent in high-nickel ternary cathodes.
[0003] Currently, commercial battery management systems (BMS) can only collect external temperature and voltage data, failing to capture the true internal temperature and pressure conditions. This results in shortcomings such as delayed monitoring response and difficulty in identifying localized anomalies, hindering the ability to predict internal safety hazards at their source. Therefore, there is an urgent need to introduce early warning strategies based on internal resistance that can characterize the battery's internal state. Among various modification schemes, doped and modified conjugated polymers, used as protective coatings for ternary cathodes, can directly sense changes in internal temperature and pressure, enabling early fault warnings. They can form a synergistic protection system with external BMS monitoring, compensating for the limitations of single external monitoring. However, current cathode protective coatings generally lack a graded response mechanism, leading to delayed protection and poor early warning effects. Summary of the Invention
[0004] Therefore, it is necessary to address the problem that existing positive electrode protective coatings lack graded response, resulting in delayed protection and poor early warning effects, and to provide a positive electrode current collector protective coating, positive electrode current collector, and battery that has excellent ion transport performance at room temperature and is compatible with thermal runaway.
[0005] On the one hand, this application provides a battery with an internal resistance of <5mΩ when the voltage is ≤4.2V and the temperature is ≤60℃; When 4.2 < voltage < 4.3V and temperature < 110℃, or when voltage < 4.3V and 60℃ < temperature < 110℃, the internal resistance is 5~20mΩ; When the voltage is ≥4.3V and / or the temperature is ≥110℃, the internal resistance is >20mΩ.
[0006] According to an embodiment of this application, the battery includes a positive electrode sheet, the positive electrode sheet including a positive current collector and a protective coating coated on at least one surface of the positive current collector along the thickness direction; The protective coating comprises a substrate material, a first dopant, and a second dopant; the substrate material is a conjugated conductive polymer, and the bonding force between the first dopant and the molecular chain of the substrate material is less than the bonding force between the ions formed by the second dopant and the molecular chain of the substrate material.
[0007] According to embodiments of this application, the matrix material includes at least one of poly(3-octylthiophene), poly(3-hexylthiophene), poly(3-octylthiophene-co-3,4-ethylenedioxythiophene), and poly(3-dodecylthiophene), and / or; The first dopant includes at least one of methanesulfonic acid, ethanesulfonic acid, and hydroxymethanesulfonic acid, and / or; The second dopant includes at least one of lithium bis(fluorosulfonyl)imide, lithium trifluoromethanesulfonate, and lithium bis(trifluoromethanesulfonyl)imide.
[0008] According to embodiments of this application, the mass of the first dopant is 1 wt% to 5 wt% of the mass of the matrix material, and / or; The mass of the second dopant is 0.5wt% to 3wt% of the mass of the matrix material.
[0009] According to embodiments of this application, the protective coating further includes an oxidizing agent, which includes cerium ammonium nitrate and / or ferric perchlorate.
[0010] According to an embodiment of this application, the protective coating includes a central region and an edge region distributed along the width direction of the positive current collector, wherein the coating thickness of the central region is less than the coating thickness of the edge region.
[0011] According to embodiments of this application, the coating thickness of the edge region is 5~10μm, and / or the coating thickness of the middle region is 2~6μm.
[0012] According to an embodiment of this application, the battery includes an electrolyte, which includes a solute and a solvent. The solute includes at least one of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, and lithium bis(trifluoromethanesulfonyl)imide, and the solvent includes at least one of ethylene carbonate, dimethyl carbonate, and diethyl carbonate.
[0013] On the other hand, this application also provides a method for preparing the above-mentioned battery, comprising the following steps: A protective coating is formulated by comprising a monomer, a first dopant, a second dopant, and a solvent; wherein the monomer comprises at least one of 3-octylthiophene, 3-hexylthiophene, 3-octylthiophene-co-3,4-ethylenedioxythiophene, and 3-dodecylthiophene, and / or; The first dopant includes at least one of methanesulfonic acid, ethanesulfonic acid, and hydroxymethanesulfonic acid, and / or; The second dopant includes at least one of lithium bis(fluorosulfonyl)imide, lithium trifluoromethanesulfonate, and lithium bis(fluoromethanesulfonyl)imide; The protective coating is applied to at least one surface of the positive current collector along the thickness direction to form a protective coating.
[0014] A positive electrode active material layer is disposed on the surface of the protective coating away from the positive current collector to form a positive electrode sheet, and then assembled into a battery.
[0015] According to an embodiment of this application, the viscosity of the protective coating is: , and / or; The coating thickness of the protective coating is 2~10μm.
[0016] Compared with the prior art, this application has the following beneficial effects: The battery of this invention exhibits different internal resistances across different voltage and temperature ranges. Within the normal operating range, the internal resistance remains essentially stable with no significant change, only experiencing two step-like abrupt changes when specific voltage / temperature thresholds are reached. This enables early warning of internal voltage and temperature anomalies, forming a dual protection mechanism in conjunction with the Battery Management System (BMS). It proactively provides internal safety protection, compensating for the lag in detection by the external BMS. Detailed Implementation
[0017] To make the above-mentioned objects, features, and advantages of the present invention more apparent and understandable, specific embodiments of the present invention are described in detail below. Many specific details are set forth in the following description to provide a thorough understanding of the present invention. However, the present invention can be practiced in many other ways different from those described herein, and those skilled in the art can make similar modifications without departing from the spirit of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0018] In the description of this invention, it should be understood that the terms "center," "longitudinal," "lateral," "length," "width," "thickness," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," "outer," "clockwise," "counterclockwise," "axial," "radial," and "circumferential" are used only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this invention.
[0019] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one of that feature. In the description of this invention, "a plurality of" means at least two, such as two, three, etc., unless otherwise explicitly specified.
[0020] In this invention, unless otherwise explicitly specified and limited, the terms "installation," "connection," "linking," and "fixing," etc., should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral part; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; they can refer to the internal communication of two components or the interaction between two components, unless otherwise explicitly limited. Those skilled in the art can understand the specific meaning of the above terms in this invention according to the specific circumstances.
[0021] In this invention, unless otherwise explicitly specified and limited, "above" or "below" the second feature can mean that the first feature is in direct contact with the second feature, or that the first feature is in indirect contact with the second feature through an intermediate medium. Furthermore, "above," "over," and "on top" of the second feature can mean that the first feature is directly above or diagonally above the second feature, or simply that the first feature is at a higher horizontal level than the second feature. "Below," "below," and "under" the second feature can mean that the first feature is directly below or diagonally below the second feature, or simply that the first feature is at a lower horizontal level than the second feature.
[0022] It should be noted that when an element is referred to as being "fixed to" or "set on" another element, it can be directly on the other element or there may be an intervening element. When an element is considered to be "connected to" another element, it can be directly connected to the other element or there may be an intervening element. The terms "vertical," "horizontal," "upper," "lower," "left," "right," and similar expressions used herein are for illustrative purposes only and do not represent the only possible implementation.
[0023] On the one hand, embodiments of this application provide a battery with an internal resistance of <5mΩ when the voltage is ≤4.2V and the temperature is ≤60℃; When 4.2 < voltage < 4.3V and temperature < 110℃, or when voltage < 4.3V and 60℃ < temperature < 110℃, the internal resistance is 5~20mΩ; When the voltage is ≥4.3V and / or the temperature is ≥110℃, the internal resistance is >20mΩ.
[0024] Specifically, voltage is a core electrical performance parameter of a battery and one of the key factors triggering sudden changes in battery internal resistance. This invention divides the battery into three voltage ranges (≤4.2V, 4.2V~4.3V, ≥4.3V) to correspond to different internal resistance ranges, thereby achieving graded early warning of voltage anomalies. In particular, it detects the risk of overcharging at 4.3V and above, which is close to the critical voltage for oxygen release from the ternary cathode lattice.
[0025] The core environmental parameter during battery operation refers to the actual internal temperature of the battery (rather than the external temperature of the casing), which is another key factor triggering sudden changes in the battery's internal resistance. This invention divides the battery into three temperature ranges (≤60℃, 60℃~110℃, ≥110℃), corresponding to different internal resistance ranges, and can detect high temperature anomalies above 60℃, especially the early risk of thermal runaway above 110℃ (a temperature of 110℃ is close to the critical temperature for electrolyte decomposition and SEI film failure).
[0026] Thus, the battery in this embodiment maintains a relatively stable internal resistance with no significant change within its normal operating range, only experiencing two step-like abrupt changes when reaching specific voltage / temperature thresholds. The internal resistance thresholds corresponding to different voltage and temperature ranges precisely match the battery's safety risk level. 1. Normal operating range: voltage ≤ 4.2V and temperature ≤ 60℃. Under these conditions, the battery is in a safe operating state and its internal resistance is less than 5mΩ.
[0027] Low internal resistance does not increase the ohmic polarization of the battery, does not affect the normal charge and discharge performance and cycle life of the battery, and ensures that the battery has excellent charge and discharge efficiency and rate performance to meet daily use needs.
[0028] 2. First risk range: When either the voltage is 4.2V~4.3V (overcharge warning threshold range) and the temperature is <110℃, or the voltage is <4.3V and the temperature is 60℃~110℃ (thermal runaway warning threshold range), abnormalities begin to appear inside the battery, such as abnormal positive electrode interface reaction or slight electrolyte decomposition, and the corresponding internal resistance rises stepwise to 5~20mΩ.
[0029] The signal generated by this change in internal resistance can serve as an early warning signal. If an early risk signal is fed back to the BMS, the BMS can adjust its charging and discharging strategy in a timely manner (such as reducing the charging current or stopping charging) to avoid escalation of the risk.
[0030] 3. Second risk zone: When any phenomenon occurs, or both occur simultaneously, such as voltage ≥ 4.3V (overcharge blocking threshold) or temperature ≥ 110℃ (thermal runaway blocking threshold), the internal abnormality of the battery intensifies, such as lattice oxygen release, transition metal dissolution, and internal resistance significantly increases to greater than 20mΩ.
[0031] The signal generated by this change in internal resistance can serve as a safety signal, such as triggering an emergency shutdown command from the BMS to prevent thermal runaway and ensure battery safety.
[0032] The batteries in the above embodiments have different internal resistances in different voltage and temperature ranges. Within the normal operating range, the internal resistance remains basically stable with no significant change, only experiencing two step-like abrupt changes when specific voltage / temperature thresholds are reached. This enables early warning of internal voltage and temperature anomalies within the cell, forming a dual protection system in conjunction with the BMS. It can proactively achieve internal safety protection, compensating for the shortcomings of external BMS detection lag.
[0033] In some embodiments, the positive electrode of the battery includes a positive current collector and a protective coating applied to at least one surface of the positive current collector along its thickness direction.
[0034] The protective coating comprises a substrate material, a first dopant, and a second dopant. The substrate material is a conjugated conductive polymer, and the bonding force between the first dopant and the molecular chains of the substrate material is less than the bonding force between the ions formed by the second dopant and the molecular chains of the substrate material.
[0035] Taking a ternary lithium-ion battery as an example, a ternary lithium-ion battery includes a positive electrode, a negative electrode, a separator, an electrolyte, and a casing. The stepwise change in internal resistance is achieved by the protective coating on the positive electrode.
[0036] The protective coating comprises a substrate material, a first dopant, and a second dopant. The coating exhibits an intrinsic positive temperature coefficient (PTC) effect and a temperature-voltage synergistic graded response, enabling step-by-step protection including normal conductivity, low-voltage overcharge warning, and high-temperature / high-voltage blocking.
[0037] The first dopant can also be called a warning dopant. Its binding force with the substrate material is weak; for example, it forms weak electrostatic interactions and reversible proton bonds with the substrate. When the voltage increases to 4.2V~4.3V and / or the temperature increases to 60℃~110℃, it easily desorbs from the substrate material, leading to a decrease in the overall conductivity of the protective coating and an increase in internal resistance.
[0038] The second dopant is also known as a blocking dopant. The ions formed by the second dopant have a stronger binding force with the matrix material; for example, they form strong ionic bonds. Desorption only occurs at voltages ≥4.3V and / or temperatures ≥110℃, further reducing the overall conductivity of the protective coating and significantly increasing the internal resistance. By designing the difference in binding forces between the two dopants, a graded response to internal resistance can be achieved, ensuring accurate early warning for different risk levels.
[0039] The specific principle is as follows: Under normal conditions (i.e., within the aforementioned normal operating range), the conjugated conductive polymer of the matrix material forms a stable electron transport channel through regular π-π stacking. The warning dopants and blocking dopants are firmly bonded to the matrix material through weak electrostatic interactions and strong ionic bonds, respectively. Both are in a stable bonded state and will not desorb. The conductive network is complete and stable, so the battery internal resistance remains basically constant and does not affect the normal charge and discharge performance.
[0040] When the aforementioned first risk range is reached, the weak interaction between the warning dopant and the substrate is disrupted and preferentially desorbed, resulting in local damage to the conductive network and a first step-like small jump in internal resistance, thus forming a warning response.
[0041] When the aforementioned second risk range is reached, the strong ionic bonds between the blocking dopant and the matrix break and desorb, the conductive network is completely destroyed, and the internal resistance undergoes a second step-like leap, achieving complete blocking.
[0042] Traditional cathode protective coatings (such as coatings formed solely from the substrate material) lack a graded response mechanism. Single PTC materials are prone to false triggering or protection hysteresis, and their internal resistance gradually increases with temperature, making precise step-wise protection impossible. The protective coating in this application relies on the conjugated substrate π-π stacked structure and the differentiated desorption behavior of dual dopants to achieve a double-threshold step-wise internal resistance mutation. Thus, it maintains stable conductivity at low temperature and low pressure without compromising battery performance, and exhibits a step-like increase in resistance during overcharging / overheating, which neither affects normal charging and discharging nor hinders cathode thermal runaway from the source.
[0043] In some embodiments, the matrix material includes at least one of poly(3-octylthiophene) (P3OT), poly(3-hexylthiophene) (P3HT), poly(3-octylthiophene-co-3,4-ethylenedioxythiophene) (P3OT-co-PEDOT), and poly(3-dodecylthiophene) (P3DT).
[0044] All of the above matrix materials meet the selection requirement of a main chain thermal decomposition temperature ≥230℃, and can be adapted to the normal operating temperature range of the battery.
[0045] In some specific embodiments, the matrix material is poly(3-octylthiophene) (P3OT). This matrix material has a main chain thermal decomposition temperature >230°C, exhibits no conformational collapse at high temperatures, and its oxidation potential precisely matches the 3.0~4.4V electrochemical window of the ternary cathode. The matrix material provides the coating with efficient electron transport channels and stable binding sites for dopants. The octyl side chain enhances the interfacial adhesion with the aluminum foil and the cathode active material. The coating exhibits a micro-nano porous structure, and the alkyl side chains do not block ion transport channels, allowing lithium ions to freely penetrate. Furthermore, this matrix material exhibits optimal π-π stacking regularity and the highest accuracy in hierarchical response.
[0046] In some embodiments, the first dopant includes at least one of methanesulfonic acid (MSA), ethanesulfonic acid (ESA), and hydroxymethanesulfonic acid (HMSA).
[0047] The aforementioned first dopants all include sulfonic acid groups, which can form weak electrostatic interactions and reversible proton bonds with the matrix material. These weak interactions allow for preferential desorption under low-voltage overcharge, resulting in a slight increase in trigger resistance and providing an early warning signal for the BMS.
[0048] In some specific embodiments, the first dopant is methanesulfonic acid. The molecule contains sulfonic acid groups (-SO3H), which can form weak electrostatic interactions and reversible proton bonds with the matrix. MSA molecules are small in size and have excellent alcohol solubility, allowing them to be uniformly embedded in the interstitial spaces of the matrix backbone. Desorption occurs without side reactions and does not damage the internal structure of the battery. Furthermore, MSA has the most stable response threshold, making it suitable for the conventional operating range of ternary cathodes.
[0049] In some embodiments, the second dopant includes at least one of lithium bis(fluorosulfonyl)imide (LiFSI), lithium trifluoromethanesulfonate (LiOTF), and lithium bis(trifluoromethanesulfonyl)imide (LiTFSI).
[0050] The aforementioned second dopants are all ionic dopants, which form a structure with strong bonding with the matrix material.
[0051] In some specific embodiments, the second dopant is lithium bis(fluorosulfonyl)imide (LiFSI). After dissociation, Li + FSI forms strong ionic bonds with the sulfur atoms in the main chain of the matrix material (such as P3OT). - Rigid groups are stably embedded in the interstitial space of the matrix. Within the normal operating temperature and voltage range, LiFSI is ionicly anchored to the main chain of the matrix, in a non-free state, and does not dissolve into the electrolyte.
[0052] Strong ionic bonds ensure the stability of the conductive network under normal conditions, and desorption only occurs under high voltage / high temperature, triggering a sharp increase in resistance and completely cutting off the electron transport channel.
[0053] In some embodiments, the mass of the first dopant is 1 wt% to 5 wt% of the mass of the matrix material.
[0054] For example, the mass of the first dopant is any one of 1wt%, 2wt%, 3wt%, 4wt%, 5wt% of the mass of the matrix material, or any one of the ranges formed by any two of the above values.
[0055] Taking P3OT as the matrix material and MSA as the first dopant as an example, if the doping amount of the first dopant is too low (below 1wt%), the carrier introduction is insufficient, the P3OT matrix is still in a low conductivity state, the internal resistance of electron transport is too high, and the warning response signal is weak, so it cannot trigger the resistance jump in time.
[0056] If the doping amount of the first dopant is too high (above 5wt%), the excess MSA will occupy the interstitial space of the P3OT main chain, destroy the π-π stacking regularity of the conjugated main chain, increase the electron jumping barrier, and thus significantly increase the internal resistance of normal electron transport. At the same time, it will destroy the reversibility of weak interactions and affect the accuracy of the early warning response.
[0057] In some specific embodiments, the mass of the first dopant is 2wt% to 3wt% of the mass of the matrix material.
[0058] At this mass ratio, the amount of charge carriers introduced is more moderate, which will not disrupt the π-π stacking regularity of the matrix conjugated main chain. This ensures a low internal resistance of electron transport under normal conditions, and can stably trigger the first-order internal resistance jump when the first risk range is reached. The warning signal is clearer and more stable, and the response threshold is more accurate.
[0059] In some embodiments, the mass of the second dopant is 0.5wt% to 3wt% of the mass of the matrix material.
[0060] For example, the mass of the second dopant is any one of the following values of the mass of the matrix material: 0.5wt%, 0.6wt%, 1.0wt%, 1.2wt%, 2.0wt%, 2.3wt%, 2.7wt%, 3wt%, or any value within the range of any two of the above values.
[0061] Taking P3OT as the matrix material and LiFSI as the second dopant as an example, when the doping amount of the second dopant is too low (below 0.5wt%), the ionic bonding is insufficient, the carrier density is low, the electron transport network is unstable, the normal electron conduction efficiency is low, and the electron transport channel cannot be completely destroyed when triggering blocking, resulting in protection failure; when the doping amount is too high (above 3wt%), the excess Li + Excessive coordination with sulfur atoms in the P3OT main chain disrupts the π-π stacking structure of the conjugated main chain, leading to distortion of the electron transport channels. This, in turn, causes an abnormally high internal resistance to normal electron transport, while excessive FSI... - This can cause the desorption threshold to shift, making it prone to false triggering under normal operating conditions.
[0062] In some specific embodiments, the mass of the second dopant is 1wt% to 2wt% of the mass of the matrix material.
[0063] For example, the mass of the second dopant is any one of 1wt%, 1.2wt%, 1.5wt%, 1.8wt%, or 2wt% of the mass of the matrix material, or any one of the ranges formed by any two of the above values.
[0064] At this mass ratio, Li + The coordination with sulfur atoms in the matrix backbone is more moderate. It will not disrupt the π-π stacking regularity of the conjugated backbone, ensuring the stability and integrity of the conductive network under normal conditions and maintaining a low internal resistance to electron transport. At the same time, it can fully desorb and completely destroy the electron transport channel when the second risk interval threshold is reached, achieving more reliable safety blocking and a more stable desorption threshold.
[0065] In some embodiments, the protective coating further includes an oxidizing agent, which includes cerium ammonium nitrate and / or ferric perchlorate (Fe(ClO4)3).
[0066] The above-mentioned oxidant is a single-electron mild oxidant with an oxidation potential that matches the polymerization requirements of 3-octylthiophene monomer. It has excellent alcohol solubility, and the by-product is water-soluble nitrate, which can be completely removed by centrifugation and washing with ethanol. There are no impurities or battery cell hazards.
[0067] In some embodiments, the oxidant is cerium ammonium nitrate (CAN). This oxidant enables controlled polymerization of monomers, avoiding over-oxidation leading to conjugated chain breakage, or under-oxidation leading to incomplete polymerization, thus ensuring the PTC effect and cycle stability of the coating. Furthermore, it offers optimal polymerization controllability and minimizes impurity residues.
[0068] In some embodiments, the protective coating includes a central region and an edge region distributed along the width direction of the positive current collector, wherein the coating thickness of the central region is less than the coating thickness of the edge region.
[0069] In the width direction of the positive current collector, the central region is surrounded by the edge regions on both sides. Since the edge regions are prone to overcharging / localized overheating and are high-risk areas for voltage and temperature anomalies, a thicker coating is required to ensure thermal stability and blocking strength. This means a thicker coating design to improve the response sensitivity of the edge regions and ensure timely detection of abnormal signals. The central region, being the main charging and discharging area, can have a slightly thinner coating to reduce impedance and avoid the coating thickness affecting the amount of positive electrode active material and battery energy density. This balances protection performance with ion / electron transport efficiency.
[0070] In some specific embodiments, the coating thickness of the edge region is 5~10μm.
[0071] For example, the coating thickness of the edge region is any value of 5μm, 6μm, 7μm, 8μm, 9μm, 10μm or any value within the range of any two of the above values.
[0072] At this coating thickness, accurate response to abnormal signals in the edge region can be ensured.
[0073] In some specific embodiments, the coating thickness in the intermediate region is 2~6 μm. This coating thickness allows for a better balance between protective performance and ion / electron transport efficiency.
[0074] In some embodiments, the electrolyte of the battery includes a solute and a solvent, wherein the solute includes at least one of lithium hexafluorophosphate (LiPF6), lithium bisfluorosulfonylimide (LiFSI), and lithium bis(trifluoromethanesulfonylimide) (LiTFSI), and the solvent includes at least one of ethylene carbonate (EC), dimethyl carbonate (DMC), and diethyl carbonate (DEC).
[0075] In some specific embodiments, the solute is lithium hexafluorophosphate (LiPF6), and the solvent is ethylene carbonate (EC). This ensures optimal compatibility between the electrolyte and the coating, allowing for stable formation of the SEI film and guaranteeing battery cycle life and the stability of the protective coating response.
[0076] On the other hand, embodiments of this application also provide a method for preparing the above-mentioned battery, comprising the following steps: S100: A protective coating is formulated by combining a monomer, a first dopant, a second dopant, and a solvent.
[0077] Furthermore, the monomer, the first dopant, and the second dopant must satisfy at least one of the following conditions (1) to (3): (1) The monomer includes at least one of 3-octylthiophene, 3-hexylthiophene, 3-octylthiophene-co-3,4-ethylenedioxythiophene, and 3-dodecylthiophene.
[0078] (2) The first dopant includes at least one of methanesulfonic acid, ethanesulfonic acid, and hydroxymethanesulfonic acid, and / or; (3) The second dopant includes at least one of lithium bis(fluorosulfonyl)imide, lithium trifluoromethanesulfonate, and lithium bis(trifluoromethanesulfonyl)imide.
[0079] In this step, a conjugated conductive polymer monomer is selected as the matrix material and mixed evenly with the first dopant, the second dopant and the solvent. If an oxidant is required, it is added to obtain a protective coating.
[0080] Moreover, there is a corresponding relationship between the matrix material and the monomer mentioned above. Specifically, when the matrix material is poly(3-octylthiophene), the corresponding monomer is 3-octylthiophene.
[0081] When the matrix material is poly(3-hexylthiophene), the corresponding monomer is 3-hexylthiophene.
[0082] When the matrix material is poly(3-octylthiophene-co-3,4-ethylenedioxythiophene), the corresponding monomer is 3-octylthiophene-co-3,4-ethylenedioxythiophene.
[0083] When the matrix material is poly(3-dodecylthiophene), the corresponding monomer is 3-dodecylthiophene.
[0084] In some embodiments, the solvent is a mixed solvent composed of an alcohol and a chloroalkane. The alcohol includes at least one of anhydrous ethanol, anhydrous methanol, and anhydrous isopropanol. The chloroalkane includes one or more of chloroform, dichloromethane, and 1,2-dichloroethane. Exemplarily, in the mixed solvent, the volume ratio of the alcohol to the chloroalkane is (8.5~9.5):(0.5~1.5).
[0085] Mixed solvents can improve the uniformity of hydrophobic monomer dispersion, achieving uniform dispersion of each component and avoiding localized uneven doping in the coating that could lead to a shift in the response threshold. In some specific embodiments, the solvent is a mixed solvent composed of anhydrous ethanol and chloroform.
[0086] In some embodiments, the protective coating includes an oxidizing agent. The process of formulating the protective coating includes: S110: The monomer and oxidant of the matrix material are dissolved in a portion of an alcohol to prepare a monomer solution and an oxidant solution, respectively.
[0087] S120: The first dopant and the second dopant are dissolved in a portion of an alcohol to form a composite dopant solution.
[0088] S130: The monomer solution, oxidant solution, and composite dopant solution are mixed to carry out a polymerization reaction. In some specific embodiments, the polymerization reaction is carried out under nitrogen protection at a reaction temperature of 25~50°C. Exemplarily, the reaction temperature is any value among 25°C, 30°C, 35°C, 40°C, 45°C, and 50°C, or any value within a range formed by any pair of the above values.
[0089] Polymerization in the alcohol phase at a medium temperature of 25-50°C can improve monomer conversion.
[0090] Taking 3-octylthiophene as the monomer and cerium ammonium nitrate (CAN) solution as the oxidant solution as an example, the polymerization reaction of octylthiophene occurs in this step.
[0091] Reaction equation: n C 12 H 20 S (C) 12 H 20 S)n The two dopants intercalate into the interstices of the poly(3-octylthiophene) molecular chains during the polymerization reaction and establish preliminary interactions.
[0092] S140: The slurry obtained from the polymerization reaction is heated for curing. A segmented curing method is used to ensure strong binding of the dopants and optimize the graded response effect. In some specific embodiments, the curing temperature is 60~80℃. Exemplarily, the curing temperature is any value among 60℃, 65℃, 70℃, 75℃, and 80℃, or any value within a range formed by any two of the above values.
[0093] Taking 3-octylthiophene as an example, the ripening process is only a physical process of heating and holding at 60~80℃, without chemical bond breaking / generation. Its function is to make the π-π stacking of the P3OT conjugated chain of the product more regular, and to fully embed the two dopants into the molecular chain gaps and complete the anchoring. It is only a physical arrangement reconstruction, and finally achieves bonding with the matrix through weak electrostatic interaction and strong ionic bond, respectively.
[0094] S150: The slurry, after maturation, is washed with an alcohol and dried to prepare a protective coating of suitable viscosity. In some specific embodiments, washing is performed until the supernatant has a pH of 6.5-7.0 and a SO42- content of 0.5%. 2- The test result was negative, with no free mesylate residue.
[0095] The above embodiments are examples of pre-mixing the dopant and monomer solutions and then carrying out a polymerization reaction with the oxidant solution. In other embodiments, the monomer solution and oxidant solution may be mixed to carry out a polymerization reaction before being mixed with the dopant.
[0096] In some specific embodiments, the viscosity of the protective coating is .
[0097] For example, the viscosity of the protective coating is any value among 5500 mPa·s, 5600 mPa·s, 5800 mPa·s, 6000 mPa·s, 6200 mPa·s, 6300 mPa·s, and 6500 mPa·s, or any value within the range of any two of the above values.
[0098] At this viscosity, the coating can be made to have good flowability and formability during the coating process, avoiding problems such as sagging and uneven coating. If the viscosity is too high, coating will be difficult and the coating will be prone to cracking. If the viscosity is too low, the coating will be too thin and cannot achieve accurate internal resistance response.
[0099] After preparing the protective coating, perform the following coating steps.
[0100] S200: The protective coating is applied to at least one surface of the positive current collector along the thickness direction to form a protective coating.
[0101] In some embodiments, the coating thickness of the protective coating is 2~10μm.
[0102] For example, the coating thickness of the protective coating is any value among 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, and 10μm, or any value within the range of any two of the above values.
[0103] In some embodiments, the coating thickness of different regions of the positive current collector can be adjusted by gradient coating, so that the coating thickness in the edge region is greater than that in the middle region, to meet differentiated protection requirements. For example, the coating thickness in the edge region is 5~10μm, and the coating thickness in the middle region is 2~6μm.
[0104] S300: A positive electrode active material layer is disposed on the surface of the protective coating away from the positive current collector to form a positive electrode sheet, and the electrode is assembled into a battery.
[0105] In this step, the positive electrode current collector coated with the protective coating is dried to remove residual solvent from the coating. Then, the positive electrode active material slurry is uniformly coated on the surface of the protective coating according to conventional processes. After rolling, drying and slitting, a positive electrode sheet that meets the specifications is obtained. The obtained positive electrode sheet is then assembled with the negative electrode sheet and the separator according to conventional stacking or winding processes to obtain a bare cell. After the bare cell is placed in the casing, the electrolyte with the aforementioned ratio is injected. After standing, formation, sealing and sorting, the final finished battery is obtained. The overall preparation process is compatible with existing battery production processes, does not require additional special equipment, and is feasible for large-scale production.
[0106] The technical solution of this application will be described below with reference to specific embodiments.
[0107] Example 1: Battery-level temperature-pressure synergistic PTC resistance response characteristics test (including coating preparation + coating process) I. This embodiment discloses a method for preparing a battery, which includes the following steps: 1.1 Preparation of protective coating slurry (P3OT-MSA-LiFSI dual-doped system) Monomer dispersion: 0.1 mol (19.6 g) of 3-octylthiophene (3OT) monomer was used as the monomer of the matrix material and dispersed in 250 mL of anhydrous ethanol + chloroform in a volume ratio of 9:1. The dispersion was ultrasonically dispersed for 15 min and placed in a constant temperature water bath at 35℃. The mixture was stirred at 400 r / min to obtain the monomer dispersion.
[0108] Preparation of composite dopant: Weigh 0.0045 mol (0.432 g) methanesulfonic acid (MSA) as the first dopant and 0.0016 mol (0.294 g) lithium bis(fluorosulfonyl)imide (LiFSI) as the second dopant, dissolve them together in 65 mL of anhydrous ethanol, and stir until completely dissolved to obtain a homogeneous composite dopant solution.
[0109] Oxidizing agent preparation: Take 0.055 mol (30.14 g) of cerium ammonium nitrate (CAN), dissolve it in 100 mL of anhydrous ethanol, stir to dissolve, and prepare an oxidizing agent solution.
[0110] Polymerization reaction: The composite dopant solution was added to the monomer dispersion and stirred at 600 rpm for 15 min; then the oxidant solution was added dropwise at a rate of 1.1 mL / min, with nitrogen gas purging at 75 mL / min throughout the process, and the reaction was carried out in a 35℃ water bath with stirring at 1200 rpm; after the dropwise addition was completed, stirring was continued for 25 min to obtain a dark reddish-brown homogeneous slurry.
[0111] Washing and slurry preparation: Wash three times with anhydrous ethanol at 6500 r / min until the supernatant has a pH of 6.5-7.0 and SO42- content. 2- The test result was negative, with no free methanesulfonic acid residue. After drying, anhydrous ethanol was added and stirred until the slurry viscosity reached 6000 mPa·s. The slurry was then sealed and kept away from light for later use.
[0112] 1.2 Positive current collector coating application Using a comma-shaped doctor blade coating method, the above-mentioned protective slurry was uniformly coated on both sides of a 12μm thick aluminum foil current collector. The thickness of the protective coating on the aluminum foil current collector was controlled to be 6μm at the edge area and 4μm in the middle area. After coating, it was dried at 65℃ and 0.011 MPa vacuum for 1.5 h to obtain a positive electrode current collector with a protective coating.
[0113] 1.3 Preparation of positive electrode sheet Using NCM622 as the positive electrode active material, a positive electrode slurry was prepared and uniformly coated on the surface of the aluminum foil current collector with the above-mentioned protective coating. The ternary positive electrode sheet was obtained by rolling and slitting.
[0114] 1.4 Pouch Battery Assembly Negative electrode: Commercial graphite negative electrode; Separator: PE separator; Electrolyte: 1 mol / L LiPF6-EC / DMC (volume ratio 1:1). Following conventional lithium-ion battery assembly methods, alternating layers of separator, negative electrode, positive electrode, separator… form a 5Ah ternary soft-pack lithium-ion battery.
[0115] II. Battery Parameters In this embodiment, the thickness of the protective coating on the edge region of the positive electrode current collector on the pouch cell is 6 μm, and the thickness of the middle region is 4 μm.
[0116] The first dopant (MSA) has a doping amount of 2.20 wt%.
[0117] The second dopant (LiFSI) has a doping concentration of 1.5 wt%.
[0118] Example 2 Compared to Example 1, the only difference in Example 2 is that in step 1.1, the monomer of the matrix material is changed from 3-octylthiophene (3OT) to 3-hexylthiophene (3HT); the doping amount of the first dopant MSA is changed to 2.5wt% and the doping amount of the second dopant LiFSI is changed to 1.5wt%.
[0119] The remaining steps are the same as in Example 1.
[0120] Accordingly, in Example 2, the thickness of the protective coating on the positive current collector of the pouch battery is 5 μm.
[0121] The first dopant (MSA) has a doping amount of 2.5 wt%.
[0122] The second dopant (LiFSI) has a doping concentration of 1.5 wt%.
[0123] Example 3 Compared to Example 1, Example 3 differs only in that: in step 1.1, the oxidant cerium ammonium nitrate (CAN) is replaced with ferric perchlorate (Fe(ClO4)3); the first dopant is replaced with ESA and the doping amount is changed to 2.2wt%; and the second dopant is replaced with LiOTF and the doping amount is changed to 1.2wt%.
[0124] The remaining steps are the same as in Example 1.
[0125] Accordingly, in Example 3, the thickness of the protective coating on the positive current collector of the pouch battery is 5 μm.
[0126] The first dopant (MSA) has a doping amount of 2.2 wt%.
[0127] The second dopant (LiFSI) has a doping concentration of 1.2 wt%.
[0128] Example 4 Compared to Example 1, the only difference in Example 4 is that in step 1.1, the monomer of the substrate material is changed to 3DT; the first dopant is replaced with HMSA and the doping amount is changed to 2.8wt%; the second dopant is replaced with LiTFSI and the doping amount is changed to 1.8wt%.
[0129] The remaining steps are the same as in Example 1.
[0130] Accordingly, in Example 4, the thickness of the protective coating on the positive current collector of the pouch battery is 5 μm.
[0131] The first dopant (MSA) has a doping amount of 2.8 wt%.
[0132] The second dopant (LiFSI) has a doping concentration of 1.8 wt%.
[0133] Example 5 (One-sided application) Compared to Example 1, the only difference in Example 5 is that in step 1.2, when the positive electrode current collector coating is applied, the protective slurry is only uniformly coated on one side of the aluminum foil current collector.
[0134] The remaining steps are the same as in Example 1.
[0135] Accordingly, in Example 5, the thickness of the protective coating on the positive current collector of the pouch battery is 5 μm.
[0136] The first dopant (MSA) has a doping amount of 2.20 wt%.
[0137] The second dopant (LiFSI) has a doping concentration of 1.5 wt%.
[0138] Comparative Example 1 (Blank control, original baseline) Compared to Example 1, the only difference in Comparative Example 1 is that the protective coating slurry preparation in step 1.1 and the positive current collector coating in step 1.2 were not performed. Instead, the positive electrode sheet was prepared by directly coating the positive electrode slurry onto a 12μm bare aluminum foil (without any protective coating).
[0139] The remaining steps are the same as in Example 1.
[0140] Comparative Example 2 (single matrix, without first or second dopant) Compared to Example 1, the only difference in Comparative Example 2 is that in step 1.1, the protective coating slurry preparation contains only the substrate P3OT, without the first dopant and the second dopant, and the oxidant is still CAN.
[0141] The remaining steps are the same as in Example 1.
[0142] Comparative Example 3 (matrix + first dopant, no second dopant) Compared to Example 1, the only difference in Comparative Example 3 is that in step 1.1, the protective coating slurry preparation contains only the first dopant MSA (2.5 wt%), and no second dopant.
[0143] The remaining steps are the same as in Example 1.
[0144] Comparative Example 4 (matrix + second dopant, no first dopant) Compared to Example 1, the only difference in Comparative Example 4 is that in step 1.1, the protective coating slurry preparation only contains the second dopant LiFSI (1.5wt%), and there is no first dopant.
[0145] The remaining steps are the same as in Example 1.
[0146] Test case The testing instruments used include: Battery charge and discharge test system (CT-4008), high and low temperature constant temperature chamber, DC internal resistance (DCR) tester, multi-channel data acquisition unit.
[0147] The testing method is in-situ testing at the battery level. The specific testing methods include: taking the battery DC internal resistance (DCR) as the core evaluation index, in-situ testing the internal resistance change under different voltage-temperature coupling conditions to verify the temperature-pressure synergistic PTC graded response characteristics; after each set of operating parameters stabilizes for 10 minutes, the internal resistance is read, and the test is repeated 3 times to take the average value.
[0148] Voltage setting method: Under specified constant temperature conditions, the battery is charged at a constant current of 0.33C to the specified voltage value, then the constant voltage is maintained until 0.05C is cut off. After standing for 30 minutes to achieve electrical balance, the internal resistance is tested.
[0149] Temperature setting method: Set the temperature of the high and low temperature constant temperature chamber to the specified temperature, place the battery in it and let it stand for 2±0.5 hours. After confirming that the internal and external temperatures of the battery cell have reached thermal equilibrium, conduct the test.
[0150] Four test conditions were set up to cover all scenarios including normal performance, single voltage triggering, single temperature triggering, and temperature-pressure combined triggering, supplementing the verification under low-pressure and high-temperature extreme conditions, and fully covering all triggering conditions of the claims: Operating Condition 1 (Normal Performance Verification): Two voltage nodes, 3.8V and 4.2V, and two temperature nodes, 25℃ and 60℃, were selected for cross-testing to verify that the internal resistance is consistently below 5mΩ within the normal operating range and that the protective coating does not impair the battery's normal charge and discharge performance.
[0151] Operating Condition 2 (Verification of Single Voltage Triggered Graded Response): The temperature is constant at 60℃, and the voltage is increased in steps from 4.2V to 4.25V to 4.3V to 4.4V to verify the two-stage step response when the voltage increases alone, matching the warning and blocking thresholds in the voltage dimension.
[0152] Operating Condition 3 (Verification of Stepped Response Triggered by Single Temperature): Constant voltage 4.2V, temperature increased in steps from 60℃ to 85℃ to 110℃ to 120℃, verifying the two-stage step response when the temperature increases alone, and verifying the blocking effect under the extreme condition of "voltage ≤ 4.2V and temperature ≥ 110℃".
[0153] Operating Condition 4 (Verification of Graded Response Triggered by Temperature and Pressure): Set three sets of coupling parameters: coordinated early warning point, coordinated blocking point, and deep anomaly point. Verify the coordinated response effect when voltage and temperature are simultaneously abnormal, and confirm the reliability of graded protection under coupled operating conditions.
[0154] V. Test Result Comparison Table Comparing the test results of each embodiment and comparative example under different operating conditions, it can be seen that: The internal resistance of the batteries in Examples 1-5 is consistently controlled within 5mΩ under all operating conditions (voltage ≤ 4.2V, temperature ≤ 60℃), which is basically the same as that of conventional batteries and does not affect normal charging and discharging. Although the increase in internal resistance of Example 5 with single-sided coating is lower than that of Example 1 with double-sided coating, it still meets the basic safety protection requirements.
[0155] When the batteries in Examples 1 to 5 reach the warning threshold (voltage 4.2 to 4.3V or temperature 60 to 110℃), the internal resistance increases stepwise to 5 to 20mΩ. When they reach the blocking threshold (voltage ≥ 4.3V or temperature ≥ 110℃), the internal resistance is ≥ 20mΩ, thus achieving precise graded protection.
[0156] In contrast, Comparative Example 1 showed no increase in internal resistance under all operating conditions, exhibiting no warning or blocking capability whatsoever. Comparative Example 2 lacked a warning range of 5-20mΩ, directly entering the blocking state, posing a serious risk of false triggering. Comparative Example 3 lacked a stable blocking range, with a severely deviated response threshold under high-temperature conditions. Comparative Example 4 had no warning stage, only showing an increase in internal resistance under high-risk conditions, exhibiting a serious response lag problem.
[0157] It is evident that the battery of the present invention, due to its dual-doped protective coating, can effectively achieve temperature and pressure synergistic safety protection, taking into account both the battery's normal performance and its ability to block abnormal operating conditions.
[0158] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0159] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.
Claims
1. A battery, characterized in that, When the voltage is ≤4.2V and the temperature is ≤60℃, the internal resistance is <5mΩ; When 4.2 < voltage < 4.3V and temperature < 110℃, or when voltage < 4.3V and 60℃ < temperature < 110℃, the internal resistance is 5~20mΩ; When the voltage is ≥4.3V and / or the temperature is ≥110℃, the internal resistance is >20mΩ.
2. The battery according to claim 1, characterized in that, The battery includes a positive electrode sheet, which includes a positive current collector and a protective coating applied to at least one surface of the positive current collector along its thickness direction. The protective coating includes a substrate material, a first dopant, and a second dopant; the substrate material is a conjugated conductive polymer, and the bonding force between the first dopant and the molecular chain of the substrate material is less than the bonding force between the ions formed by the second dopant and the molecular chain of the substrate material.
3. The battery according to claim 2, characterized in that, The matrix material includes at least one of poly(3-octylthiophene), poly(3-hexylthiophene), poly(3-octylthiophene-co-3,4-ethylenedioxythiophene), and poly(3-dodecylthiophene), and / or; The first dopant includes at least one of methanesulfonic acid, ethanesulfonic acid, and hydroxymethanesulfonic acid, and / or; The second dopant includes at least one of lithium bis(fluorosulfonyl)imide, lithium trifluoromethanesulfonate, and lithium bis(trifluoromethanesulfonyl)imide.
4. The battery according to claim 2, characterized in that, The mass of the first dopant is 1 wt% to 5 wt% of the mass of the matrix material, and / or; The mass of the second dopant is 0.5wt% to 3wt% of the mass of the matrix material.
5. The battery according to claim 2, characterized in that, The protective coating also includes an oxidizing agent, which includes cerium ammonium nitrate and / or ferric perchlorate.
6. The battery according to claim 2, characterized in that, The protective coating includes a central region and an edge region distributed along the width direction of the positive current collector, wherein the coating thickness of the central region is less than that of the edge region.
7. The battery according to claim 6, characterized in that, The coating thickness in the edge region is 5~10μm, and / or the coating thickness in the middle region is 2~6μm.
8. The battery according to any one of claims 1 to 7, characterized in that, The battery includes an electrolyte, which includes a solute and a solvent. The solute includes at least one of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, and lithium bis(trifluoromethanesulfonyl)imide. The solvent includes at least one of ethylene carbonate, dimethyl carbonate, and diethyl carbonate.
9. A method for preparing a battery according to any one of claims 1 to 8, characterized in that, Includes the following steps: A protective coating is formulated by comprising a monomer, a first dopant, a second dopant, and a solvent; wherein the monomer comprises at least one of 3-octylthiophene, 3-hexylthiophene, 3-octylthiophene-co-3,4-ethylenedioxythiophene, and 3-dodecylthiophene, and / or; The first dopant includes at least one of methanesulfonic acid, ethanesulfonic acid, and hydroxymethanesulfonic acid, and / or; The second dopant includes at least one of lithium bis(fluorosulfonyl)imide, lithium trifluoromethanesulfonate, and lithium bis(fluoromethanesulfonyl)imide; The protective coating is applied to at least one surface of the positive current collector along the thickness direction to form a protective coating. A positive electrode active material layer is disposed on the surface of the protective coating away from the positive current collector to form a positive electrode sheet, and then assembled into a battery.
10. The preparation method according to claim 9, characterized in that, The viscosity of the protective coating is , and / or; The coating thickness of the protective coating is 2~10μm.