Secondary battery and electric device
By preparing an undercoat containing inorganic oxides on the current collector substrate, the problem of uneven coating caused by residual oil film on the surface of the low-cost current collector substrate is solved, achieving high-quality coating of the electrode and improving battery performance, while reducing battery cost.
Patent Information
- Application Number
- CN202611397389.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-11
- Publication Date
- 2026-11-24
AI Technical Summary
In existing technologies, residual oil film on the surface of low-cost current collector substrates during manufacturing leads to uneven coating of water-based slurry, making it difficult to achieve high-quality electrode coating, especially in sodium-ion batteries.
A metal current collector substrate prepared by calendering using an inorganic oxide base coating combined with particulate binders, dispersants, conductive agents, and wetting agents improves the compatibility and coating quality between the water-based slurry and the current collector substrate.
This improved the coating quality and bonding strength of the electrode sheets, reduced the cold pressing elongation of the battery, balanced the electrochemical performance of the battery, and reduced the overall cost of the battery.
Smart Images

Figure CN123162283A_ABST
Abstract
Description
[0001] This application is a divisional application based on the invention with application number 202410437980.5, application date April 11, 2024, applicant CATL, and invention title "Secondary Battery and Power Consumption Device". Technical Field
[0002] This application relates to the field of battery technology, and more particularly to a secondary battery and an electrical device. Background Technology
[0003] With the increasing prominence of energy and environmental issues, the new energy industry has received more and more attention. Due to its high energy density and good cycle performance, rechargeable batteries have been widely used in recent years in energy storage power systems such as hydropower, thermal power, wind power and solar power plants, as well as in many fields such as power tools, electric bicycles, electric motorcycles, electric cars, military equipment, and aerospace.
[0004] Electrodes are a crucial component of rechargeable batteries. Improving electrode quality to further enhance battery performance is a pressing technical challenge in this field. Summary of the Invention
[0005] This application is made in view of the above-mentioned problems, and its purpose is to provide a secondary battery with improved performance.
[0006] A first aspect of this application provides a secondary battery, the secondary battery including an electrode, the electrode including a current collector and a film layer disposed on at least one side of the current collector, the current collector including a current collector substrate and a base coating disposed on at least one side of the current collector substrate, the base coating including an inorganic oxide, and the film layer including an aqueous binder.
[0007] Inorganic oxides have a high density and better adhesion to metal current collector substrates. Compared to commonly used active materials (such as soft or hard carbon) or conductive agents (such as conductive carbon) in film layers, they are less prone to shrinkage or displacement under the surface tension of the slurry. This can effectively improve the coating quality of the primer layer and achieve successful coating of liquid slurries with large surface energy differences from the current collector substrate. Water-based slurries, including water-based binders, often have high surface tension, leading to large surface energy differences and poor coating quality when coated on current collector substrates. Including inorganic oxides in the primer layer can particularly solve the problem of poor compatibility between water-based slurries and current collector substrates, improving the coating quality of water-based slurries on current collector substrates.
[0008] In any embodiment, the inorganic oxide includes one or more of aluminum oxide, boehmite, magnesium oxide, iron oxide, silicon oxide, and zirconium oxide.
[0009] In any embodiment, the inorganic oxide accounts for 30%-60% of the total mass of the base coating.
[0010] The inclusion of inorganic oxides within the aforementioned mass range in the base coating can improve the coating quality of the electrode, enhance the electrode bonding strength, reduce the elongation during cold pressing of the electrode, and effectively control the current collector resistance, thus taking into account the electrochemical performance of the battery.
[0011] In any embodiment, the volume distribution particle size Dv50 of the inorganic oxide is < 2 μm.
[0012] Inorganic oxides with a volume distribution particle size within the above range can adhere tightly to the metal current collector substrate, improving the forming quality of the base coating and the electrode sheet.
[0013] In any embodiment, the base coating further includes a particulate binder, which includes one or more of styrene-butadiene rubber and acrylate rubber.
[0014] Particulate binders are amphiphilic and exhibit better water resistance compared to linear binders, which have a stronger affinity for water-soluble solvents. This allows the base coat to remain stable during the application of the upper film containing active substances, further enhancing the base coat's role in improving coating quality.
[0015] In any embodiment, the particulate adhesive accounts for 10%-40% of the total mass of the base coating.
[0016] The inclusion of particulate binders within the aforementioned mass range in the base coating can improve the coating quality of the electrode sheets, enhance the bonding strength of the electrode sheets, and effectively control the current collector resistance, thus taking into account the electrochemical performance of the battery.
[0017] In any embodiment, the base coating further includes a dispersant, which includes one or more polyacrylic polymers.
[0018] Polyacrylic acid polymers are linear polymers that can be fully dispersed in solvents to coat inorganic oxides, reduce the agglomeration of inorganic oxides, effectively disperse inorganic oxides, help inorganic oxides to fully exert their performance, further improve the forming quality of the base coating, improve the coating quality and bonding strength of the electrode, and reduce the elongation of the electrode during cold pressing.
[0019] In any embodiment, the mass percentage of the dispersant is 1%-8% based on the total mass of the base coating, and can be optionally 1%-5%.
[0020] Dispersants with a mass content within this range can effectively improve the bonding strength between the film layer and the current collector, and reduce the adverse effects of excessive acrylic acid content on the reduced water resistance of the undercoat, thus comprehensively improving the forming quality of the electrode sheet.
[0021] In any embodiment, the base coating layer further includes one or more of a conductive agent, a thickener, and a wetting agent.
[0022] Conductive agents can minimize the negative impact of the undercoat on the conductivity of the current collector while also ensuring the electrochemical performance of the battery. Thickeners improve the dispersion of conductive agents and reduce the sedimentation of conductive agents and inorganic oxides, thereby improving the stability of the undercoat slurry and expanding the process window. Wetting agents enhance the wetting of the film slurry on the current collector containing the oil film, facilitating the coating of the undercoat slurry onto the metal current collector substrate.
[0023] In any embodiment, the conductive agent includes one or more of Super-P, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers; and / or the thickener includes one or more of sodium carboxymethyl cellulose, sodium alginate, xanthan gum, and carrageenan; and / or the wetting agent includes one or more of polyethoxy ether surfactants, polyether silicone surfactants, nonionic fluorocarbon polymer surfactants, and acetylene surfactants.
[0024] In any embodiment, based on the total mass of the base coating, the conductive agent accounts for 10%-40% by mass; the thickener accounts for 0.5%-4% by mass; and the wetting agent accounts for 0.2%-1% by mass.
[0025] In any embodiment, the thickness of the base coating is 0.5µm-3µm.
[0026] A base coating with a suitable thickness can balance the battery's molding quality and electrochemical performance.
[0027] In any embodiment, the current collector substrate is a metal current collector substrate, which is prepared by calendering.
[0028] Metal current collector substrates prepared by calendering have low cost, which can further reduce the overall cost of batteries. However, an oil film inevitably remains on the surface of the metal current collector substrate after calendering. This application is particularly suitable for such metal current collector substrates, and can comprehensively reduce the cost of secondary batteries.
[0029] In any embodiment, the current collector substrate has a dyne value of 20-35 mN / cm.
[0030] Water has a dyne value greater than 70 mN / cm, and the difference in dyne value between aqueous slurry and the aforementioned metal current collector substrate makes it difficult to achieve uniform coating on their surface. The embodiments of this application can effectively improve the coating quality of aqueous slurry on the aforementioned metal current collector substrate, which helps to broaden the range of selectable current collector substrates and further reduce battery costs.
[0031] In any embodiment, the current collector substrate includes a metal current collector substrate, which includes at least one of copper foil, aluminum foil, stainless steel foil, titanium foil, and nickel foil.
[0032] In any embodiment, the membrane layer further includes a negative electrode active material, which includes one or more of hard carbon, soft carbon, graphite, and silicon; and / or the aqueous binder includes one or more of styrene-butadiene rubber (SBR) and acrylate rubber.
[0033] In any embodiment, the secondary battery includes one or more of sodium secondary batteries and lithium secondary batteries.
[0034] In any embodiment, the secondary battery includes a sodium-ion battery, and each sodium-ion battery cell includes: a battery casing with an opening at its upper part; a top cover assembly disposed at the opening of the battery casing, the top cover assembly being sealed to and electrically connected to the battery casing; and an electrode assembly for electrical connection, the electrode assembly being disposed on the top cover assembly; wherein the top cover assembly includes a top cover plate, and the electrode assembly and the top cover plate are constructed as a single integral component made of aluminum or an aluminum alloy.
[0035] This sodium-ion battery achieves an optimized design of the battery top cover assembly while maintaining battery performance. By integrating the electrode assembly onto the top cover assembly, it is constructed as a single integral component made of aluminum or aluminum alloy, which reduces the number of structural parts and further reduces manufacturing costs. At the same time, it enables the battery casing and electrode assembly to be connected and energized, reducing the possibility of corrosion of the battery casing.
[0036] A second aspect of this application provides an electrical device comprising a secondary battery in any embodiment.
[0037] A third aspect of this application provides a current collector comprising a current collector substrate and a base coating disposed on at least one side of the current collector substrate, the base coating comprising an inorganic oxide.
[0038] In any embodiment, the inorganic oxide includes one or more of aluminum oxide, boehmite, magnesium oxide, iron oxide, silicon oxide, and zirconium oxide.
[0039] In any embodiment, the base coating further includes a particulate binder, which includes one or more of styrene-butadiene emulsions and acrylate emulsions.
[0040] In any embodiment, the base coating further includes a dispersant, which includes one or more polyacrylic polymers.
[0041] In any embodiment, the current collector substrate is a metal current collector substrate, and the dyne value of the metal current collector substrate is 20-35 mN / m.
[0042] In any embodiment, the current collector substrate is a metal current collector substrate, and the metal current collector substrate includes aluminum foil. Attached Figure Description
[0043] Figure 1 This is a schematic diagram of a secondary battery according to one embodiment of this application.
[0044] Figure 2 yes Figure 1 An exploded view of a secondary battery according to one embodiment of this application is shown.
[0045] Figure 3 This is a schematic diagram of a battery module according to one embodiment of this application.
[0046] Figure 4 This is a schematic diagram of a battery pack according to one embodiment of this application.
[0047] Figure 5 yes Figure 4 An exploded view of a battery pack according to one embodiment of this application is shown.
[0048] Figure 6 This is a schematic diagram of an electrical device that uses a secondary battery as a power source according to one embodiment of this application.
[0049] Explanation of reference numerals in the attached figures: 1 Battery pack; 2 Upper housing; 3 Lower housing; 4 Battery module; 5 Secondary battery; 51 Housing; 52 Electrode assembly; 53 Top cover assembly. Detailed Implementation
[0050] The embodiments of the secondary battery and electrical device of this application are hereby disclosed in detail with appropriate reference to the accompanying drawings. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of practically identical structures may be omitted. This is to avoid making the following description unnecessarily lengthy and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided to enable those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.
[0051] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way typically include endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is also expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values of 1 and 2 are listed, and if maximum range values of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" have been listed herein; "0-5" is merely a shortened representation of these numerical combinations. Furthermore, when a parameter is described as an integer greater than or equal to 2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0052] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.
[0053] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.
[0054] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.
[0055] Unless otherwise specified, the terms "comprising" and "including" as used in this application can be open-ended or closed-ended. For example, "comprising" and "including" can mean that other components not listed may also be included, or that only the listed components may be included.
[0056] Unless otherwise specified, the term "or" is inclusive in this application. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, the condition "A or B" is satisfied by any of the following conditions: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0057] With increasing demands for cost reduction in batteries, the urgency of adopting low-cost current collector substrates is constantly growing. However, low-cost current collector substrates are often manufactured using low-cost production processes, such as rolling, which involves coating the surface of the current collector substrate with an oil film during the rolling process to reduce surface damage. However, this oil film is difficult to remove, preventing aqueous slurries from fully wetting the surface of the current collector substrate, thus hindering effective coating. Taking sodium-ion batteries as an example, since sodium ions do not alloy with aluminum like lithium ions, there are more options for negative electrode current collector materials. For instance, the negative electrode of a sodium-ion battery can use low-cost foils such as aluminum foil instead of the copper foil commonly used in existing technologies to further reduce costs. As an example, if the aluminum foil is prepared by rolling, an oil film will remain on its surface, making it difficult to coat the negative electrode with aqueous slurry, thus preventing its application to the negative electrode sheet.
[0058] A first aspect of this application provides a secondary battery, the secondary battery including an electrode, the electrode including a current collector and a film layer disposed on at least one side of the current collector, the current collector including a current collector substrate and a base coating disposed on at least one side of the current collector substrate, the base coating including an inorganic oxide, and the film layer including an aqueous binder.
[0059] Inorganic oxides are inorganic compounds composed of oxygen atoms and one or more metallic or non-metallic elements.
[0060] Inorganic oxides in the undercoat can be tested using any known testing method. For example, decomposition products in the film can be analyzed using instruments such as Raman spectroscopy, X-ray diffraction, and transmission electron microscopy; or component analysis can be performed using energy dispersive spectroscopy.
[0061] Waterborne binders are binders that use an aqueous medium as a dispersant. Therefore, films containing waterborne binders are often prepared using aqueous slurries. Waterborne binders are classified into linear binders and particulate binders based on their dispersion morphology in the solvent. Linear binders exhibit a linear morphology in the solvent and can achieve polymer chain extension, thus encapsulating the active materials in the film. Examples include, but are not limited to, polyacrylic acid and polymethyl acrylate. Particulate binders are binders that exhibit a dot-like morphology in the solvent, often consisting of latex particles. Examples include, but are not limited to, styrene-butadiene rubber and styrene-acrylic rubber.
[0062] Inorganic oxides have a high density and better affinity to the current collector substrate. Compared with commonly used active materials (such as soft carbon or hard carbon) or conductive agents (such as conductive carbon) in the film layer, they are less likely to shrink or shift under the surface tension of the slurry, which can effectively improve the coating quality of the base layer.
[0063] Aqueous slurries containing water-based binders often exhibit high surface tension, leading to significant surface energy differences and poor coating quality when coated on current collector substrates. Including inorganic oxides in the undercoat layer effectively addresses the poor compatibility between the aqueous slurry and the current collector substrate, improving the coating quality. It is understood that the electrode here can be either a positive or negative electrode, and the embodiments of this application achieve corresponding technical effects for different battery systems. As an example, for positive electrode sheets using aqueous film slurries, the current collector provided in the embodiments of this application also provides improved electrode coating quality. It should be noted that the secondary battery mentioned here is not limited to sodium secondary batteries but also includes lithium secondary batteries.
[0064] It is understandable that the material of the current collector is not particularly limited, as long as it does not cause chemical changes in the secondary battery and is conductive. Current collectors include metal foils with a pure metal content of 95% or higher, such as at least one of copper foil, aluminum foil, stainless steel foil, titanium foil, and nickel foil. They also include alloy foils with at least two main metals, for example, alloy foils made from at least two main elements of copper, aluminum, nickel, titanium, and iron. Furthermore, they can include copper, aluminum-cadmium alloys, iron, or stainless steel with surface treatments using carbon, nickel, titanium, silver, copper, etc. In addition, the bonding force with the negative electrode active material can be enhanced by forming micro-uneven surfaces, and they can be used in various forms such as films, sheets, foils, meshes, porous bodies, foams, and non-woven fabrics.
[0065] In some embodiments, the inorganic oxide includes one or more of aluminum oxide, boehmite, magnesium oxide, iron oxide, silicon oxide, and zirconium oxide.
[0066] In some embodiments, the inorganic oxide includes one or more of alumina and boehmite.
[0067] The two inorganic oxides mentioned above have superior adhesion to aluminum foil, which can further improve the forming quality and bonding strength of the electrode sheet.
[0068] In some embodiments, the inorganic oxide accounts for 30%-60% of the total mass of the primer coating.
[0069] In some embodiments, based on the total mass of the primer coating, the mass percentage of the inorganic oxide can be selected as 30%, 35%, 40%, 45%, 50%, 55%, 60%, or any value range between the two.
[0070] The inclusion of inorganic oxides within the aforementioned mass range in the base coating can improve the coating quality of the electrode, enhance the electrode bonding strength, reduce the elongation during cold pressing of the electrode, and effectively control the current collector resistance, thus taking into account the electrochemical performance of the battery.
[0071] In some embodiments, the volumetric particle size Dv50 of the inorganic oxide is <2 μm.
[0072] The volume distribution particle size Dv50 refers to the particle size that, in the particle size volume distribution diagram, corresponds to a cumulative volume distribution percentage of 50%, starting from the smallest particle size.
[0073] The volume distribution particle size Dv50 can be tested using any method known in the art. As an example, it can be determined using a laser particle size analyzer such as the Mastersizer 2000E from Malvern Instruments Ltd., UK, in accordance with GB / T19077-2016 Particle Size Distribution Laser Diffraction Method.
[0074] Inorganic oxides with a volume distribution particle size within the above range can adhere tightly to the metal current collector substrate, improving the forming quality of the base coating and the electrode sheet.
[0075] In some embodiments, the base coating layer further includes a particulate adhesive, which includes one or more of styrene-butadiene rubber and acrylate rubber.
[0076] Particulate adhesives refer to adhesives that exhibit a dot-like morphology in the base layer. These adhesives generally present a granular distribution in the solvent and are mostly latex particles.
[0077] Styrene-butadiene rubber (SBR) is also known as polystyrene-butadiene copolymer.
[0078] Acrylic rubber is an elastomer obtained by copolymerization of acrylates as the main monomers. The main monomers include methyl acrylate, ethyl acrylate, butyl acrylate, and 2-ethylhexyl acrylate. In some embodiments, acrylate rubber includes styrene-acrylic rubber (SAR). SAR is also known as a styrene-acrylate copolymer.
[0079] Particulate binders are amphiphilic and exhibit better water resistance compared to linear binders, which have a stronger affinity for water-soluble solvents. This allows the base coat to remain stable during the application of the upper film containing active substances, further enhancing the base coat's role in improving coating quality.
[0080] In some embodiments, the particulate binder includes acrylate rubber.
[0081] Acrylic rubber exhibits stronger adhesion to metal current collector substrates compared to other particulate adhesives, which can further improve the coating quality and bonding strength of the electrode sheet.
[0082] In some embodiments, the particulate binder accounts for 10%-40% of the total mass of the base coating.
[0083] In some embodiments, the mass percentage of the particulate adhesive, based on the total mass of the base coating, can be selected as 10%, 15%, 20%, 25%, 30%, 35%, 40%, or any value between the two.
[0084] The inclusion of particulate binders within the aforementioned mass range in the base coating can improve the coating quality of the electrode sheets, enhance the bonding strength of the electrode sheets, and effectively control the current collector resistance, thus taking into account the electrochemical performance of the battery.
[0085] In some embodiments, the base coating further includes a dispersant, which includes one or more polyacrylic polymers.
[0086] Polyacrylic acid polymers refer to polymers obtained by polymerization of acrylic acid or acrylic acid derivatives as monomers, or by copolymerization of these monomers with other unsaturated compounds. It can be understood that polyacrylic acid polymers can include both homopolymers and copolymers.
[0087] In some embodiments, the polyacrylic polymer includes one or more of polyacrylic acid, polymethacrylic acid, polyacrylamide, poly(acrylic acid-acrylamide), poly(acrylic acid-acrylonitrile), and poly(acrylic acid-acrylonitrile-acrylamide).
[0088] Polyacrylic acid polymers are linear polymers that can be fully dispersed in solvents to coat inorganic oxides, reduce the agglomeration of inorganic oxides, effectively disperse inorganic oxides, help inorganic oxides to fully exert their performance, further improve the forming quality of the base coating, improve the coating quality and bonding strength of the electrode, and reduce the elongation of the electrode during cold pressing.
[0089] In some embodiments, the dispersant accounts for 1%-8% of the total mass of the base coating.
[0090] In some embodiments, the mass percentage of the dispersant, based on the total mass of the base coating, can be selected as 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, or any value range between the two.
[0091] Dispersants with a mass content within this range can effectively improve the bonding strength between the film layer and the current collector, and reduce the adverse effects of excessive acrylic acid content on the reduced water resistance of the undercoat, thus comprehensively improving the forming quality of the electrode sheet.
[0092] In some embodiments, the base coating layer further includes one or more of a thickener, a conductive agent, and a wetting agent.
[0093] In some embodiments, the conductive agent includes one or more of Super-P, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0094] Conductive agents can minimize the negative impact of the undercoat on the conductivity of the current collector while taking into account the electrochemical performance of the battery.
[0095] In some embodiments, the thickener includes one or more of sodium carboxymethyl cellulose, sodium alginate, xanthan gum, and carrageenan.
[0096] Thickeners can improve the dispersion of conductive agents and reduce the sedimentation of conductive agents and inorganic oxides, thereby improving the stability of the base coating slurry and expanding the process window.
[0097] In some embodiments, the wetting agent includes one or more of the following: polyethoxy ether surfactants, polyether silicone surfactants, nonionic fluorocarbon polymer surfactants, and alkyne surfactants.
[0098] Wetting agents help improve the wetting of the film slurry on the current collector containing the oil film, so that the base coating slurry can be coated on the metal current collector substrate.
[0099] In some embodiments, based on the total mass of the base coating, the conductive agent accounts for 10%-40% by mass; the thickener accounts for 0.5%-4% by mass; and the wetting agent accounts for 0.2%-1% by mass.
[0100] In some embodiments, the mass percentage of the conductive agent, based on the total mass of the base coating, can be selected as 10%, 20%, 30%, 40%, or any value between the two.
[0101] In some embodiments, the mass percentage of the thickener, based on the total mass of the base coating, can be selected as 0.5%, 1%, 2%, 3%, 4%, or any value range between the two.
[0102] In some embodiments, the mass percentage of the wetting agent may be selected as 0.2%, 0.4%, 0.6%, 0.8%, 1%, or any value range between the two.
[0103] In some embodiments, the thickness of the base coating is 0.5µm-3µm.
[0104] In some embodiments, the thickness of the base coating can be selected as 0.5µm, 1µm, 2µm, 3µm, or any value range between the two.
[0105] A base coating with a suitable thickness can balance the battery's molding quality and electrochemical performance.
[0106] In some embodiments, the primer coating can be prepared by mixing an inorganic oxide and a dispersant in an aqueous solvent, stirring until homogeneous, adding a thickener, and then adding a conductive agent, a binder, and a wetting agent in sequence to form a primer slurry; coating the primer slurry onto a metal current collector substrate, and after drying, cold pressing, and other processes, a current collector containing the primer coating can be obtained.
[0107] In some embodiments, the film layer further includes a negative electrode active material, which includes one or more of hard carbon, soft carbon, graphite, and silicon.
[0108] In some embodiments, the waterborne adhesive includes one or more of styrene-butadiene rubber (SBR) and acrylate rubber.
[0109] Unlike linear binders such as polyacrylic acid, the above-mentioned particulate binder can effectively alleviate the gelation phenomenon of the film slurry and improve the brittleness of the film. It has a particularly significant effect on improving the slurry of negative electrode active materials such as hard carbon, soft carbon, and graphite.
[0110] In some embodiments, the current collector substrate is a metal current collector substrate, which is prepared by calendering.
[0111] Metal current collector substrates prepared by calendering have low cost, which can further reduce the overall cost of batteries. However, an oil film inevitably remains on the surface of the metal current collector substrate after calendering. This application is particularly suitable for such metal current collector substrates, and can comprehensively reduce the cost of secondary batteries.
[0112] In some embodiments, the current collector substrate has a dyne value of 20-35 mN / m.
[0113] In some embodiments, the dyne value of the current collector substrate may be selected as 20 mN / m, 25 mN / m, 30 mN / m, 35 mN / m, or any value range between the two.
[0114] The dyne value, also known as the surface tension coefficient, primarily describes the magnitude of surface tension, i.e., the force exerted between two adjacent parts of a liquid surface per unit length. The dyne value reflects the wetting ability of the current collector substrate; a higher dyne value indicates better wetting ability. The dyne value can be obtained by any method known in the art. As an example, the dyne value of the current collector substrate is tested by tracing it across the surface with a dyne pen.
[0115] Water has a dyne value greater than 70 mN / m, and the difference in dyne value between the aqueous slurry and the aforementioned current collector substrate makes it difficult to achieve uniform coating on their surface. The embodiments of this application can effectively improve the coating quality of the aqueous slurry on the aforementioned current collector substrate, which is beneficial for broadening the range of selectable current collector substrates and further reducing battery costs. In some embodiments, the current collector substrate includes a metal current collector substrate, which includes at least one of copper foil, aluminum foil, stainless steel foil, titanium foil, and nickel foil.
[0116] In some embodiments, the metal current collector substrate includes aluminum foil.
[0117] The aluminum foil will spontaneously form an aluminum oxide film on its surface, which makes the oxide of the undercoat layer in this embodiment have a higher affinity for it, and can further improve the coating quality and bonding strength of the electrode sheet.
[0118] In some embodiments, the film layer may optionally include a conductive agent. The conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0119] In some embodiments, the membrane layer may also optionally include other additives, such as thickeners (e.g., sodium carboxymethyl cellulose (CMC-Na)).
[0120] In some embodiments, the electrode can be prepared by dispersing the above-mentioned components for preparing the electrode, such as active materials, conductive agents, binders and any other components, in a solvent (e.g., deionized water) to form a film slurry; coating the film slurry onto a current collector, and then obtaining the electrode after drying, cold pressing and other processes.
[0121] In some implementations, the secondary battery includes one or more of sodium secondary batteries and lithium secondary batteries.
[0122] In some implementations, the secondary battery is a sodium-ion battery, and the electrode is a negative electrode.
[0123] In some embodiments, the secondary battery is a negative electrode-free battery, which may be a sodium-based negative electrode-free battery or a lithium-based negative electrode-free battery.
[0124] A negative electrodeless rechargeable battery refers to a battery in which a negative electrode active material layer is not actively placed on the negative electrode side during the battery manufacturing process. For example, a metal or carbonaceous active material layer is not formed at the negative electrode through coating or deposition processes. During the first charge, active ions gain electrons on the anode side and deposit as a metallic phase on the surface of the current collector. During discharge, the metal can transform back into active ions and return to the positive electrode, achieving cyclic charging and discharging. Therefore, a negative electrodeless battery is also a type of metal battery. Compared to other rechargeable batteries, negative electrodeless rechargeable batteries can achieve higher energy density because they do not have a pre-placed negative electrode active material layer.
[0125] Although electrodeless secondary batteries do not require coating or deposition processes to form a negative electrode active material layer, they often include a base coating containing conductive materials to induce deposition. Due to significant differences in surface tension, the aqueous base coating for electrodeless secondary batteries faces difficulties in forming on low-dyne current collector substrates. The base coating provided in this application is also suitable for electrodeless secondary batteries, improving coating quality. Furthermore, the inorganic oxide can further induce metal deposition, which is beneficial for improving the uniformity of metal deposition.
[0126] In some embodiments, the secondary battery includes a sodium-ion battery, wherein a single sodium-ion battery cell includes: a battery casing with an opening at its upper part; a top cover assembly disposed at the opening of the battery casing, the top cover assembly being sealed to and electrically connected to the battery casing; and an electrode assembly for electrical connection, the electrode assembly being disposed on the top cover assembly; wherein the top cover assembly includes a top cover plate, and the electrode assembly and the top cover plate are constructed as a single integral component made of aluminum or an aluminum alloy.
[0127] This sodium-ion battery achieves an optimized design of the battery top cover assembly while maintaining battery performance. By integrating the electrode assembly onto the top cover assembly, it is constructed as a single integral component made of aluminum or aluminum alloy, which reduces the number of structural parts and further reduces manufacturing costs. At the same time, it enables the battery casing and electrode assembly to be connected and energized, reducing the possibility of corrosion of the battery casing.
[0128] In some embodiments, the secondary battery further includes a positive electrode sheet, which includes a positive current collector and a positive active material layer formed on at least a portion of the surface of the positive current collector. The positive active material layer includes a positive active material, which may include at least one of layered transition metal oxides, polyanionic compounds, and Prussian blue compounds.
[0129] The transition metal in the layered transition metal oxide can be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr, and Ce. Optionally, the layered transition metal oxide is, for example, NaxMO2, where M is one or more of Ti, V, Mn, Co, Ni, Fe, Cr, and Cu, and 0 < x ≤ 1.
[0130] Polyanionic compounds can contain metal ions, transition metal ions, or tetrahedral (YO4) structures. n- A class of compounds with anionic units. The metal ion may be one of sodium, lithium, potassium, or zinc; the transition metal may be at least one of Mg, Al, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Zr, Cr, Nb, Mo, In, Ge, Ga, Sn, Hf, Ta, W, and Pb; Y may be at least one of P, S, and Si; n represents (YO4). n- The price state.
[0131] As an optional implementation of this application, the general chemical formula of the polyanionic compound may be Na. x-a A a V y-b M b (PO4) 2-2c (DO4)2 c F z-d Q d, wherein the element A represents an alkali metal element doped to replace Na, the element M represents a metal element replacing V, the element D represents a doping element replacing P, and the element Q represents a doping element replacing F. The element D includes at least one of Si and S, and the element Q includes at least one of Cl and O; 3.5≤x≤4.5, 0≤a≤0.15x, 0.8≤y≤1.1, 0≤b≤0.3y, 0≤c≤0.15, 0.8≤z≤1.1, 0≤d≤0.2z. Optionally, the element A includes at least one of K and Li; the element M includes at least one of Fe, Cr, Al, Sc, Ga, In, Ti, Zr, Mn, Zn, Ni, Cu, and Co.
[0132] As an optional implementation of the present application, the general chemical formula of the polyanionic compound may be Na x R y (PO4)2P2O7, wherein x=3.5-4.5, y=2.75-3.25, and R includes at least one of Mg, Al, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Zr, Cr, Nb, Mo, In, Ga, Sn, Hf, Ta, W, and Pb.
[0133] As an optional implementation of the present application, the general chemical formula of the polyanionic compound may be Na 4+x R 3-y P 4- m O 15 / C; wherein 0<x<0.5, 0<y≤0.5, 0<m≤0.2, and R includes at least one of Mg, Al, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Zr, Cr, Nb, Mo, In, Ga, Sn, Hf, Ta, W, and Pb.
[0134] As an optional implementation of the present application, the general chemical formula of the polyanionic compound may be Na m Fe x (PO4) y P2O7 / C; wherein 3.6≤m≤4.4, 2.8≤x≤3, 2≤y≤2.1. The Prussian blue analogue may be a class of compounds having sodium ions, transition metal ions, and cyanide ions (CN-). The transition metal may be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr, and Ce. The Prussian blue analogue is, for example, Na a Me b Me’ c(CN)6, wherein Me and Me' are each independently at least one of Ni, Cu, Fe, Mn, Co and Zn, 0 < a ≤ 2, 0 < b < 1, 0 < c < 1.
[0135] In some embodiments, the positive electrode active material layer may further include a conductive agent to improve the conductivity of the positive electrode. The conductive agent may be one or more of Super P, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphite, graphene, and carbon nanofibers.
[0136] In some embodiments, the positive electrode active material layer may further include a binder to firmly bond the positive electrode active material and optionally a conductive agent to the positive electrode current collector. The binder may be at least one selected from polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyacrylic acid (PAA), polyvinyl alcohol (PVA), ethylene-vinyl acetate copolymer (EVA), styrene-butadiene rubber (SBR), carboxymethyl cellulose (CMC), sodium alginate (SA), polymethacrylic acid (PMA), and carboxymethyl chitosan (CMCS).
[0137] In some embodiments, the positive current collector can be a conductive carbon sheet, a metal foil, a carbon-coated metal foil, a porous metal plate, or a composite current collector. The conductive carbon material of the conductive carbon sheet can be selected from one or more of Super P, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphite, graphene, and carbon nanofibers. The metal material of the metal foil, carbon-coated metal foil, and porous metal plate is independently selected from at least one of copper, aluminum, nickel, and stainless steel. The composite current collector can be a composite current collector formed by combining a metal foil with a polymer base film.
[0138] In some embodiments, the positive electrode sheet can be prepared by dispersing the above-mentioned components for preparing the positive electrode sheet, such as positive active material, conductive agent, binder and any other components, in a solvent (e.g., N-methylpyrrolidone) to form a positive electrode slurry; coating the positive electrode slurry onto the positive electrode current collector, and then obtaining the positive electrode sheet after drying, cold pressing and other processes.
[0139] [Electrolytes] The electrolyte acts as a conductor of ions between the positive and negative electrodes. This application does not impose specific restrictions on the type of electrolyte; it can be selected according to requirements. For example, the electrolyte can be liquid, gel, or entirely solid.
[0140] In some embodiments, the electrolyte is an electrolyte solution. The electrolyte solution includes an electrolyte salt and a solvent.
[0141] In some embodiments, the electrolyte salt may be selected from at least one of sodium hexafluorophosphate, sodium difluorosulfonamide, sodium difluoromethanesulfonamide, sodium trifluoromethanesulfonate, sodium tetrafluoroborate, sodium difluorophosphate, sodium perchlorate, and sodium chloride.
[0142] In some embodiments, the electrolyte comprises an ester solvent, which includes at least one selected from ethylene carbonate, propylene carbonate, diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, propylene carbonate, methyl acetate, ethyl propionate, and fluoroethylene carbonate.
[0143] In some embodiments, the electrolyte comprises an ether solvent, including one or more of ethylene glycol dimethyl ether, ethylene glycol diethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, 1,3-dioxolane, tetrahydrofuran, methyltetrahydrofuran, diphenyl ether, and crown ether, optionally including one or more of ethylene glycol dimethyl ether, ethylene glycol diethyl ether, diethylene glycol dimethyl ether, and tetraethylene glycol dimethyl ether.
[0144] In some embodiments, the electrolyte may optionally include additives. For example, additives may include negative electrode film-forming additives, positive electrode film-forming additives, and may also include additives that can improve certain battery performance, such as additives that improve battery overcharge performance, additives that improve battery high-temperature or low-temperature performance, etc.
[0145] In some embodiments, the secondary battery also includes a separator. This application does not impose any particular limitation on the type of separator; any known porous separator with good chemical and mechanical stability can be selected.
[0146] In some embodiments, the material of the separator can be selected from at least one of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0147] In some implementations, the positive electrode, negative electrode, and separator can be fabricated into an electrode assembly using a winding or stacking process.
[0148] In some embodiments, the secondary battery may include an outer packaging. This outer packaging may be used to encapsulate the electrode assembly and electrolyte described above.
[0149] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. The outer packaging of the secondary battery can also be a soft pack, such as a pouch. The material of the soft pack can be plastic; examples of plastics include polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0150] This application does not impose any particular limitation on the shape of the secondary battery; it can be cylindrical, square, or any other arbitrary shape. For example, Figure 1 This is an example of a square-structured secondary battery 5.
[0151] In some implementations, refer to Figure 2 The outer packaging may include a housing 51 and a cover 53. The housing 51 may include a base plate and side plates connected to the base plate, the base plate and side plates forming a receiving cavity. The housing 51 has an opening communicating with the receiving cavity, and the cover 53 can be placed over the opening to close the receiving cavity. A positive electrode, a negative electrode, and a separator can be formed into an electrode assembly 52 using a winding or stacking process. The electrode assembly 52 is encapsulated within the receiving cavity. Electrolyte is immersed in the electrode assembly 52. The secondary battery 5 may contain one or more electrode assemblies 52, which can be selected by those skilled in the art according to specific practical needs.
[0152] In some implementations, the secondary batteries can be assembled into a battery module, and the number of secondary batteries contained in the battery module can be one or more, the specific number of which can be selected by those skilled in the art according to the application and capacity of the battery module.
[0153] Figure 3 This is battery module 4, used as an example. (See reference...) Figure 3 In battery module 4, multiple secondary batteries 5 can be arranged sequentially along the length of battery module 4. Of course, they can also be arranged in any other manner. Furthermore, these multiple secondary batteries 5 can be fixed in place using fasteners.
[0154] Optionally, the battery module 4 may also include a housing with a receiving space in which a plurality of secondary batteries 5 are received.
[0155] In some embodiments, the battery modules described above can also be assembled into a battery pack, and the number of battery modules contained in the battery pack can be one or more, the specific number of which can be selected by those skilled in the art according to the application and capacity of the battery pack.
[0156] Figure 4 and Figure 5 This is battery pack 1 as an example. (See reference...) Figure 4 and Figure 5 The battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box includes an upper body 2 and a lower body 3, with the upper body 2 covering the lower body 3 to form a closed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.
[0157] In addition, this application also provides an electrical device, which includes at least one of the secondary battery, battery module, or battery pack provided in this application. The secondary battery, battery module, or battery pack can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device may include, but is not limited to, mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc.
[0158] As the electrical device, a secondary battery, battery module, or battery pack can be selected according to its usage requirements.
[0159] Figure 6 This is an example of an electrical device. The device could be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the secondary battery for this device, a battery pack or battery module can be used.
[0160] Another example device could be a mobile phone, tablet, or laptop. These devices typically require a slim and lightweight design and can use a rechargeable battery as their power source.
[0161] Furthermore, this application also provides a current collector, which includes a metal current collector substrate and a base coating disposed on at least one side of the metal current collector substrate, the base coating comprising an inorganic oxide.
[0162] It is understood that the current collector includes the current collector features of the secondary battery in any embodiment.
[0163] Example The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.
[0164] Example 1 1) Preparation of current collectors Preparation of primer slurry: Take 40 parts of alumina and 5 parts of polyacrylic acid and mix them in an aqueous solution. After stirring evenly, add 2 parts of thickener CMC-Na to form a uniform and stable alumina dispersion. After adding 29.7 parts of Super-P and stirring evenly, add 28 parts of dot-type adhesive styrene-butadiene emulsion and disperse for 30 min. Finally, add 0.3 parts of wetting agent polyoxyethylene ether and disperse for 30 min to form a primer slurry with a solid content of 18%.
[0165] Primer coating application: The above-mentioned primer coating is uniformly applied to the aluminum metal current collector substrate, and after drying, a primer coating layer is obtained. The coating weight is 140mg / 1540.25mm. 2 The dyne value of aluminum metal current collector substrate is 20-35 mN / m.
[0166] 2) Preparation of negative electrode sheet The negative electrode active material hard carbon, conductive carbon black, water-based binder styrene-butadiene rubber (SBR), and thickener sodium carboxymethyl cellulose (CMC-Na) are thoroughly stirred in a deionized water solvent system at a mass ratio of 96:2:1:1 to obtain a negative electrode slurry. The negative electrode slurry is then uniformly coated onto the negative electrode current collector prepared in the previous step, and then dried, cold-pressed, and slit to obtain the negative electrode sheet.
[0167] The preparation methods of Examples 2-8 are basically the same as those of Example 1, except that the specific components of the base coating are adjusted, as shown in Table 1. In Example 4, the conductive agent is carbon nanotubes.
[0168] Comparative Example 1 The negative electrode active material hard carbon, conductive carbon black, binder styrene-butadiene rubber (SBR), and thickener sodium carboxymethyl cellulose (CMC-Na) are thoroughly stirred in a deionized water solvent system at a mass ratio of 96:2:1:1 to obtain a negative electrode slurry. The negative electrode slurry is then uniformly coated on the surface of aluminum foil, and then dried, cold-pressed, and slit to obtain the negative electrode sheet.
[0169] The preparation method of Comparative Example 2 is basically the same as that of Example 1, except that the specific components of the base coating are adjusted, as shown in Table 1.
[0170] Table 1
[0171] II. Battery Performance Testing 1. Water resistance test of negative electrode current collector The negative electrode current collector coated with the primer layer prepared above was stamped using a stamping machine to obtain an area of approximately 2 mm². 2The sample was prepared by uniformly applying 0.2g of water to one side of its base coating and then baking it at 120°C for 5 minutes. The sample was then observed using a CCD microscope. If the sample contained exposed current collector substrate, it was deemed unqualified; if the sample showed film tears or outward migration and diffusion of the base coating without exposing the substrate, it was deemed qualified; if the film layer did not show significant changes, it was deemed good.
[0172] 2. Coating quality test of negative electrode sheet Observe the coating quality of the prepared negative electrode sheet; if there is severe edge shrinkage and large-area missing coating, it is judged as unqualified; if there is a small amount of serrated edge shrinkage and a small amount of dotted missing coating, it is judged as qualified; if there is no edge shrinkage and missing coating, and the film surface is flat and uniform, it is judged as good.
[0173] 3. Bond strength test The peel strength between the negative electrode film and the current collector with the base coating was tested according to the test method in the national standard GB T 2791-1995.
[0174] 4. Electrode elongation test Take the negative electrode sheet, remove the tab area, and mark three points horizontally at three-meter intervals along the electrode sheet direction. The length of each mark should be accurate to 0.1mm. Record the distance between two adjacent points as 'a'. Adjust the left and right gaps and the tonnage of the pressure rollers of the cold press between 20 tons and 79 tons to adjust the cold pressing thickness so that the electrode sheet reaches the ideal compaction density. Measure the compaction density of the electrode sheet as 0.95 g / cm³. 3 The length b of the electrode marking after cold pressing. That is, the cold pressing elongation η = (b / a-1) 100%. Two segments were taken from each sample, and three samples were taken. The average of the six data points obtained from the test was used as the electrode elongation rate.
[0175] 5. Current collector resistance test The current collector with a base coating was tested using an electrode resistance meter (Yuaneng Technology). Five samples were tested in parallel, and the average value was taken as the film resistance of the current collector. III. Analysis of Test Results for Each Embodiment and Comparative Example Batteries for each embodiment and comparative example were prepared according to the above method, and various performance parameters were measured. The results are shown in Table 2 below.
[0176] Table 2
[0177] As can be seen from the comparison of the embodiments and comparative examples, the secondary battery with an inorganic oxide-based undercoating provided in this application can achieve the coating of aqueous film slurry on the aluminum foil surface, which is beneficial to further reduce the cost of sodium secondary batteries. A comparison between Examples 1, 3, and 4 shows that when the inorganic oxide content in the undercoating is 30%-60% by mass, the undercoating not only improves the coating quality of the aqueous slurry on the current collector substrate, but also enhances the mechanical interlocking force with the film layer through the riveting effect between the inorganic oxide and the negative electrode active material, thereby increasing the bonding strength between the film layer and the current collector; it can also reduce the driving effect of film layer extension on the current collector during cold pressing, and reduce the elongation rate of the current collector during cold pressing.
[0178] Table 3
[0179] As shown in Table 3, the inorganic oxide accounts for 30%-60% of the mass, and the particulate binder accounts for 10%-30% of the mass. This can improve the coating quality, bonding strength, and elongation of the electrode while taking into account the resistance. It can also reduce costs while taking into account the electrochemical performance of the secondary battery.
[0180] Although the electrode coating quality was improved in Examples 6 and 7 and was upgraded to qualified, a small number of jagged edges and a small number of spot-like omissions appeared in the coating, making it impossible to accurately measure the electrode bonding strength and elongation. Therefore, its performance was not tested.
[0181] As can be seen from the comparison of Examples 1, 2, 5 and Example 6, when the mass ratio of the dispersant is 1%-5% based on the total mass of the base coating, the interaction force between the water molecules in the aqueous negative electrode film slurry and the dispersant polyacrylic acid in the base coating is maintained at a suitable level, making it difficult for water molecules to insert between the molecules of the base coating. The base coating has good water resistance, and the coating appearance of the electrode is further improved.
[0182] As can be seen from the comparison of Examples 1, 2, 8 and Example 7, when the mass ratio of the particulate binder is greater than 10% based on the total mass of the base coating, the particulate binder can provide sufficient adhesion in the base coating, making it difficult for water molecules to insert between the molecules of the base coating. The base coating has good water resistance, and the coating appearance of the electrode is further improved.
[0183] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.
Claims
1. A secondary battery, characterized in that, The secondary battery includes an electrode, the electrode includes a current collector and a film layer disposed on at least one side of the current collector, the current collector includes a current collector substrate and a base coating disposed on at least one side of the current collector substrate, the base coating includes an inorganic oxide, and the film layer includes an aqueous binder.
2. The secondary battery according to claim 1, characterized in that, The inorganic oxides include one or more of aluminum oxide, boehmite, magnesium oxide, iron oxide, silicon oxide, and zirconium oxide.
3. The secondary battery according to claim 1 or 2, characterized in that, Based on the total mass of the base coating, the inorganic oxide accounts for 30%-60% of the total mass.
4. The secondary battery according to any one of claims 1 to 3, characterized in that, The volume distribution particle size Dv50 of the inorganic oxide is <2 μm.
5. The secondary battery according to any one of claims 1 to 4, characterized in that, The base coating also includes a particulate adhesive, which includes one or more of styrene-butadiene rubber and acrylate rubber.
6. The secondary battery according to claim 5, characterized in that, Based on the total mass of the base coating, the mass percentage of the particulate adhesive is 10%-40%.
7. The secondary battery according to any one of claims 1 to 6, characterized in that, The base coating also includes a dispersant, which includes one or more polyacrylic polymers.
8. The secondary battery according to claim 7, characterized in that, Based on the total mass of the base coating, the dispersant accounts for 1%-8% of the total mass.
9. The secondary battery according to any one of claims 1 to 8, characterized in that, Based on the total mass of the base coating, the dispersant accounts for 1%-5% of the total mass.
10. The secondary battery according to claim 8, characterized in that, The base coating further includes one or more of a conductive agent, a thickener, and a wetting agent; the conductive agent includes one or more of Super-P, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers; and / or The thickener includes one or more of sodium carboxymethyl cellulose, sodium alginate, xanthan gum, and carrageenan; and / or The wetting agent includes one or more of the following: polyoxyethylene ether surfactants, polyether silicone surfactants, nonionic fluorocarbon polymer surfactants, and acetylene surfactants.
11. The secondary battery according to claim 10, characterized in that, Based on the total mass of the base coating, the conductive agent accounts for 10%-40% of the mass; the thickener accounts for 0.5%-4% of the mass; and the wetting agent accounts for 0.2%-1% of the mass.
12. The secondary battery according to any one of claims 1 to 11, characterized in that, The thickness of the base coating is 0.5µm-3µm.
13. The secondary battery according to any one of claims 1 to 12, characterized in that, The current collector substrate is a metal current collector substrate, which is prepared by calendering.
14. The secondary battery according to any one of claims 1 to 13, characterized in that, The current collector substrate has a dyne value of 20-35 mN / m.
15. The secondary battery according to any one of claims 1 to 14, characterized in that, The current collector substrate includes a metal current collector substrate, which includes at least one of copper foil, aluminum foil, stainless steel foil, titanium foil, and nickel foil.
16. The secondary battery according to any one of claims 1 to 15, characterized in that, The film layer further includes a negative electrode active material, which includes one or more of hard carbon, soft carbon, graphite, and silicon; and / or The water-based adhesive includes one or more of styrene-butadiene rubber (SBR) and acrylate rubber.
17. The secondary battery according to any one of claims 1 to 16, characterized in that, The secondary battery includes one or more of sodium secondary batteries and lithium secondary batteries.
18. The secondary battery according to any one of claims 1 to 17, characterized in that, The secondary battery includes a sodium-ion battery, and the individual cells of the sodium-ion battery include: A battery casing, wherein an opening is provided at the top of the battery casing; A top cover assembly is disposed at the opening of the battery housing, and the top cover assembly is sealed to and electrically connected to the battery housing; as well as An electrode assembly for electrical connection, the electrode assembly being disposed on the top cover assembly; The top cover assembly includes a top cover plate, and the electrode assembly and the top cover plate are constructed as a single integral component made of aluminum or an aluminum alloy.
19. An electrical appliance, characterized in that, The electrical device includes the secondary battery as described in any one of claims 1 to 18.
20. A current collector, characterized in that, The current collector includes a current collector substrate and a base coating disposed on at least one side of the current collector substrate, the base coating comprising an inorganic oxide.
21. The current collector according to claim 20, characterized in that, The inorganic oxides include one or more of aluminum oxide, boehmite, magnesium oxide, iron oxide, silicon oxide, and zirconium oxide.
22. The current collector according to claim 20 or 21, characterized in that, The base coating also includes a particulate binder, which includes one or more of styrene-butadiene emulsions and acrylate emulsions.
23. The current collector according to any one of claims 20 to 22, characterized in that, The base coating also includes a dispersant, which includes one or more polyacrylic polymers.
24. The current collector according to any one of claims 20 to 23, characterized in that, The current collector substrate is a metal current collector substrate, and the dyne value of the metal current collector substrate is 20-35 mN / m.
25. The current collector according to any one of claims 20 to 24, characterized in that, The current collector substrate is a metal current collector substrate, and the metal current collector substrate includes aluminum foil.