Secondary battery
By introducing tetracyanoborate compound A into lithium-ion batteries to generate a dense SEI layer, the problems of ionic conductivity decay and acetonitrile-based electrolyte corrosion in lithium-ion batteries under low-temperature conditions are solved. This achieves synergistic optimization of the battery's low-temperature performance and fast-charging capability, and improves the battery's cycle stability and storage performance.
Patent Information
- Application Number
- CN202611512438.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-28
- Publication Date
- 2026-11-24
AI Technical Summary
Existing lithium-ion batteries exhibit decreased ionic conductivity and high viscosity at low temperatures, hindering lithium-ion migration and resulting in insufficient fast-charging performance and low-temperature adaptability. Additionally, acetonitrile-based electrolytes readily react with lithium salts to generate HF acid, which corrodes the electrodes and current collectors, affecting battery cycle stability and long-term storage performance.
By introducing a specific additive compound A containing tetracyanoborate (TCB⁻), a dense inorganic-organic composite SEI layer is formed on the graphite surface. This layer blocks acetonitrile co-intercalation and reductive decomposition, inhibits gas generation and lithium dendrite growth, stabilizes the cathode material, captures HF, promotes full dissociation of lithium salt, improves ionic conductivity, and enhances low-temperature performance and fast-charging capability.
It significantly improves the low-temperature performance, fast-charging capability, and long-term stability of secondary batteries, suppresses electrode corrosion and side reactions, increases lithium-ion transference number and overall ionic conductivity, and synergistically optimizes the battery's low-temperature adaptability and fast-charging performance.
Smart Images

Figure CN123162287A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of energy storage device technology, and more particularly to a secondary battery. Background Technology
[0002] In the electrolyte systems of lithium-ion batteries and other electrochemical energy storage devices, carbonate compounds are the most widely used non-aqueous solvents. They possess excellent electrochemical stability and lithium-ion conductivity, making them a core component of mainstream electrolytes. However, carbonate solvents exhibit a significant decrease in ionic conductivity and a high viscosity at low temperatures, hindering lithium-ion migration and resulting in insufficient fast-charging performance and low-temperature adaptability, making it difficult to meet the requirements of extreme low-temperature scenarios.
[0003] To overcome this bottleneck, the industry has generally adopted an improvement scheme that introduces acetonitrile (AcN). Actonitrile, with its advantages of low viscosity and high dielectric constant, can significantly improve the ionic conductivity of the electrolyte, optimize interfacial contact, and improve the battery's low-temperature and fast-charging performance. However, the introduction of acetonitrile also brings new challenges: it easily reacts with lithium salts to generate HF acid, which corrodes the electrodes and current collectors; at the same time, acetonitrile is easily reduced to produce gas on the graphite anode surface and cannot form a stable SEI film, resulting in a decrease in battery cycle stability and long-term storage performance, which restricts the industrial application of acetonitrile-based electrolytes.
[0004] Therefore, there is an urgent need to develop new non-aqueous electrolyte systems to resolve the contradiction between performance improvement and application risks in existing solutions, achieve synergistic optimization of battery low-temperature performance, fast charging capability and cycle storage performance, and provide technical support for the application of electrochemical energy storage devices in extreme environments. Summary of the Invention
[0005] To address the aforementioned problems, the present invention aims to provide a secondary battery. This secondary battery, by introducing specific additives, can fundamentally suppress the reduction decomposition, side reaction gas generation, and electrode corrosion problems of acetonitrile-based electrolytes during cycling and storage. Simultaneously, it significantly improves the ion transport efficiency, high-temperature storage capacity retention, and cycle life of the secondary battery, achieving synergistic optimization of the low-temperature performance, fast-charging capability, and long-term stability of acetonitrile-based secondary batteries, thus providing a reliable technical solution for the industrial application of acetonitrile-based electrolytes.
[0006] To achieve the above objectives, the present invention provides a secondary battery comprising a positive electrode material, a negative electrode material, and an electrolyte. The negative electrode material comprises graphite, and the electrolyte comprises an electrolyte salt, a non-aqueous organic solvent, and an additive. The non-aqueous organic solvent comprises a carbonate, a carboxylic acid ester, and acetonitrile. The additive comprises compound A with the structural formula shown in Formula 1, wherein M... + Selected from alkali metal ions, substituted or unsubstituted C1~C 12Alkylammonium ions, substituted or unsubstituted pyridinium ions, substituted or unsubstituted imidazolium ions, substituted or unsubstituted pyrrolidineium ions, substituted or unsubstituted imidazolidineium ions.
[0007]
[0008] Formula 1 In the secondary battery of the present invention, an additive containing compound A is introduced into the non-aqueous organic solvent comprising carbonate, carboxylic acid ester, and acetonitrile. Compound A contains tetracyanoborate (TCB). - It has a dual structure of electron-deficient boron centers and strong adsorption sites of polycyano groups, which can preferentially adsorb acetonitrile molecules onto the surface of graphite materials and cathode materials. During the activation of secondary batteries and the first charge, selective oxidation / reduction decomposition occurs, thereby achieving multiple functions to improve the battery's low-temperature performance, fast charging capability, high-temperature cycling and storage performance.
[0009] Firstly, TCB - Preferential reduction on the graphite surface generates a dense inorganic-organic composite SEI layer containing Li3N, BN, LiF and cyano polymers. This layer exhibits high ionic conductivity and strong electronic insulation, effectively blocking acetonitrile co-intercalation and continuous reduction decomposition, inhibiting gas generation and lithium dendrite growth, preventing repeated rupture and reconstruction of the SEI film, and significantly reducing interfacial impedance.
[0010] Secondly, polycyano groups can be strongly adsorbed onto the positive electrode active sites, stabilizing lattice oxygen, reducing surface catalytic activity, and inhibiting the oxidative decomposition of acetonitrile and carbonate solvents. Simultaneously, they block HF-induced dissolution of the positive electrode transition metal, preventing the deterioration of the negative electrode SEI film.
[0011] Third, the central boron atom has strong Lewis acidity, which can quickly capture HF generated by the hydrolysis of LiPF6 through ligand exchange, neutralize acidic species, stabilize PF5 intermediates, cut off the electrolyte autocatalytic decomposition chain, significantly reduce electrode and current collector corrosion, suppress gas generation during high-temperature storage, and improve capacity retention.
[0012] Fourth, TCB - Access to Li + Solvation of the sheath promotes complete dissociation of lithium salt and increases the free Li + The concentration of Li was reduced simultaneously. + Desolvation energy barrier, enhancing Li + The mobility number and overall ionic conductivity, combined with the low viscosity advantage of acetonitrile, further enhance the low-temperature discharge and fast-charging capabilities.
[0013] As a technical solution of the present invention, compound A is selected from at least one of compounds one to three.
[0014]
[0015] As one technical solution of the present invention, compound A accounts for 0.05~3.00% of the mass of the electrolyte.
[0016] As one technical solution of the present invention, the electrolyte salt is selected from at least one of lithium hexafluorophosphate, lithium perchlorate, lithium tetrafluoroborate, lithium trifluoromethanesulfonate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(oxalate-borate), lithium difluorophosphate, lithium lower aliphatic carboxylic acids, lithium difluorodioxalate phosphate, lithium bis(fluorosulfonyl)imide, lithium chloroborane, and lithium tetraphenylborate.
[0017] As one technical solution of the present invention, the mass ratio of the carboxylic acid ester to the acetonitrile is 1.0~5.0:2.0~6.0:1.0.
[0018] As one technical solution of the present invention, the carbonate is selected from at least one of ethylene carbonate, propylene carbonate, butyl carbonate, methyl pentyl carbonate, ethylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, and propylene carbonate.
[0019] As one technical solution of the present invention, the carboxylic acid ester is selected from at least one of γ-butyrolactone, γ-valerolactone, δ-valerolactone, methyl acetate, ethyl acetate, ethyl propionate, butyl acetate, propyl propionate and butyl propionate.
[0020] As a technical solution of the present invention, the additive further comprises compound B, which comprises vinyl sulfite and / or lithium difluorooxalate borate, and the compound B accounts for 1.0 to 5.0% of the mass of the electrolyte.
[0021] As one technical solution of the present invention, compound B comprises vinyl sulfite and lithium difluorooxalate borate, and the mass ratio of vinyl sulfite to lithium difluorooxalate borate is 1~5:0.5~2.0.
[0022] As a technical solution of the present invention, the positive electrode material is selected from at least one of lithium iron phosphate materials, lithium cobalt oxide materials, lithium nickel cobalt manganese oxide materials and lithium nickel cobalt aluminum oxide materials, and the negative electrode material may further include silicon-based materials, wherein the silicon-based materials are silicon-carbon composite materials and / or silicon-oxygen composite materials. Detailed Implementation
[0023] The non-aqueous electrolyte of this invention exhibits superior low-temperature performance, fast-charging capability, high-temperature cycling performance, and storage performance. The secondary battery of this invention may comprise a positive electrode material, a negative electrode material, and a non-aqueous electrolyte.
[0024] The cathode material may include layered oxides (such as lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and lithium cobalt oxide) and olivine-type materials (lithium iron phosphate and lithium manganese iron phosphate). The electrolyte of this invention is particularly suitable for olivine-type materials (lithium iron phosphate and lithium manganese iron phosphate). Further, the lithium nickel cobalt manganese oxide material may include lithium nickel cobalt manganese oxide, doped or coated lithium nickel cobalt manganese oxide. The lithium nickel cobalt aluminum oxide material may include lithium nickel cobalt aluminum oxide, doped or coated lithium nickel cobalt aluminum oxide. The lithium cobalt oxide material may include lithium cobalt oxide, doped or coated lithium cobalt oxide. The lithium iron phosphate material may include lithium iron phosphate, doped or coated lithium iron phosphate. The lithium manganese iron phosphate material may include lithium manganese iron phosphate, doped or coated lithium manganese iron phosphate.
[0025] The negative electrode material includes at least graphite, which may be artificial graphite and / or natural graphite. Furthermore, the negative electrode material may also include silicon-based materials, including silicon-carbon composites and / or silicon-oxygen composites.
[0026] Non-aqueous electrolytes contain electrolyte salts, non-aqueous organic solvents, and additives.
[0027] The electrolyte salt constitutes 5-25% of the mass of the non-aqueous electrolyte, further comprising 8-20% of the mass, and even further comprising 10-15% of the mass. For example, the mass percentage of the electrolyte salt may be, but is not limited to, 5%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 20%, and 25%. The mass percentage of the electrolyte salt is not limited to the listed values; other unlisted values within this range also apply. The electrolyte salt is selected from at least one of lithium hexafluorophosphate (LiPF6), lithium perchlorate (LiClO4), lithium tetrafluoroborate (LiBF4), lithium trifluoromethanesulfonate (LiCF3SO3), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(oxalateborate)borate (LiBOB), lithium difluorophosphate (LiPO2F2), lower aliphatic carboxylic acids, lithium difluorodioxalate phosphate (LiDFBP), lithium bis(fluorosulfonyl)imide (LiFSI), lithium chloroborane, and lithium tetraphenylborate. As an example, lithium hexafluorophosphate (LiPF6) is used as the electrolyte salt, but it is not a limitation thereof.
[0028] The non-aqueous organic solvent includes carbonates, carboxylic acid esters, and acetonitrile, and the mass ratio of carbonates, carboxylic acid esters, and acetonitrile is 1.0~5.0:2.0~6.0:1.0. As examples, the mass ratio may be, but is not limited to, 1.0:2.0:1.0, 1.0:3.0:1.0, 1.0:4.0:1.0, 1.0:5.0:1.0, 1.0:6.0:1.0, 2.0:2.0:1.0, 2.0:3.0:1.0, 2.0:4.0:1.0, 2.0:5.0:1.0, 2.0:6.0:1.0, 3.0:2.0:1.0, and 3.0:3.0:1. 0, 3.0:4.0:1.0, 3.0:5.0:1.0, 3.0:6.0:1.0, 4.0:2.0:1.0, 4.0:3.0:1.0, 4.0:4.0:1.0, 4.0:5.0:1.0, 4.0:6.0:1.0, 5.0:2.0:1.0, 5.0:3.0:1.0, 5.0:4.0:1.0, 5.0:5.0:1.0, 5.0:6.0:1.0. The carbonate is selected from ethylene carbonate (EC), propylene carbonate (PCA), butyl carbonate (BC), methyl amyl carbonate (MPC), vinylene carbonate (VEC), dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (EMC), methyl propyl carbonate (MPC), and propylene carbonate (PC). The carboxylic acid ester is selected from at least one of γ-butyrolactone (GBL), γ-valerolactone (GVL), δ-valerolactone (DVL), methyl acetate (MA), ethyl acetate (EA), ethyl propionate (EP), butyl acetate (BAC), propyl propionate (PP), and butyl propionate (PRB).
[0029] The non-aqueous organic solvent accounts for 65-90% of the mass of the non-aqueous electrolyte, preferably 75-89%. More preferably, the non-aqueous organic solvent accounts for 78-88% of the mass of the non-aqueous electrolyte. As an example, the mass percentage of the non-aqueous organic solvent may be, but is not limited to, 65%, 68%, 70%, 73%, 75%, 78%, 80%, 83%, 85%, 87%, or 90%, but is not limited to the listed values; other unlisted values within this range are also applicable.
[0030] The additive contains compound A, which has the structural formula shown in Formula 1.
[0031]
[0032] Formula 1 Among them, M + Selected from alkali metal ions, substituted or unsubstituted C1~C 12Alkylammonium ions, substituted or unsubstituted pyridinium ions, substituted or unsubstituted imidazolium ions, substituted or unsubstituted pyrrolidineium ions, and substituted or unsubstituted imidazolidineium ions. As an example, M + Optional from Li + Na + K + Ammonium ion, methyl-substituted ammonium ion, ethyl-substituted ammonium ion, propyl-substituted ammonium ion, isopropyl-substituted ammonium ion, butyl-substituted ammonium ion, isobutyl-substituted ammonium ion, pentyl-substituted ammonium ion, isopentyl-substituted ammonium ion, vinyl-substituted ammonium ion, propenyl-substituted ammonium ion, isopropenyl-substituted ammonium ion, butenyl-substituted ammonium ion, isobutenyl-substituted ammonium ion, pentenyl-substituted ammonium ion, isopentenyl-substituted ammonium ion Ammonium ion, ethynyl-substituted ammonium ion, propynyl-substituted ammonium ion, isopropynyl-substituted ammonium ion, butynyl-substituted ammonium ion, isobutynyl-substituted ammonium ion, penynyl-substituted ammonium ion, isopentenyl-substituted ammonium ion, pyridinium ion, pyrrolemethylonium ion, pyrroleethylonium ion, pyrrolepropylonium ion, pyrroleisopropylonium ion, pyrrolebutylonium ion, pyrroleisobutylonium ion, pyrrolepentylonium ion, pyrroleisopentylonium ion, pyrrolevinylonium ion Pyrrolopropenylonium ion, pyrroloisopropenylonium ion, pyrrolobutenylonium ion, pyrroloisobutenylonium ion, pyrrolopentenylonium ion, pyrroloethynylonium ion, pyrrolopropenylonium ion, pyrrolobutenylonium ion, pyrroloisobutenylonium ion, pentyrroloethynylonium ion, pyrroloisopentenylonium ion, imidazoleonium ion, imidazolemethylonium ion, imidazoleethylonium ion, imidazolepropylonium ion, imidazole isopropylonium ion, imidazole Ion: Imidazole-butylium, Imidazole-isobutyliumium, Imidazole-pentyliumium, Imidazole-isopentyliumium, Imidazole-vinyliumium, Imidazole-propynyliumium, Imidazole-isopropynyliumium, Imidazole-butenyliumium, Imidazole-isobutylenyliumium, Imidazole-pentenyliumium, Imidazole-isopentenyliumium, Imidazole-ethynyliumium, Imidazole-propynyliumium, Imidazole-isopropynyliumium, Imidazole-butynyliumium, Imidazole-isobutynyliumium, Imidazole-pyrrolynyliumium, Imidazole-isopentynyliumium.
[0033] Furthermore, compound A is selected from at least one of compounds one through three.
[0034]
[0035] CAS No.: 261356-49-4 CAS No.: 742099-80-5 CAS No.: 623575-91-7 Compound A comprises 0.05 to 3.00% of the electrolyte by mass. Further, compound A comprises 0.1 to 3.0% of the electrolyte by mass, and even further, compound A comprises 0.5 to 2.0% of the electrolyte by mass. As examples, compound A comprises 0.05%, 0.10%, 0.20%, 0.30%, 0.40%, 0.50%, 0.60%, 0.70%, 0.80%, 0.90%, 1.00%, 1.50%, 2.00%, 2.50%, and 3.00% of the electrolyte by mass, but is not limited to the listed values; other unlisted values within this range also apply.
[0036] Furthermore, the additive also includes compound B, which comprises vinyl sulfite and / or lithium difluorooxalate borate. Compound B accounts for 1.0 to 5.0% of the electrolyte mass, and as an example, compound B may be, but is not limited to, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, and 5.0%. Compound B comprises vinyl sulfite and lithium difluorooxalate borate, wherein the mass ratio of vinyl sulfite to lithium difluorooxalate borate is 1~5:0.5~2.0. For example, the mass ratio may be, but is not limited to, 1:0.5, 1:1.0, 1:1.5, 1:2.0, 2:0.5, 2:1.0, 2:1.5, 3:0.5, 3:1.0, 3:2.0, 4:0.5, 4:1.0, 4:1.5, 5:0.5, 5:1.0, 5:1.5, and 5:2.0.
[0037] To further illustrate the purpose, technical solution, and beneficial effects of this invention, the following will provide a further description of the invention in conjunction with specific embodiments. It should be noted that, for other raw materials in the embodiments and comparative examples where specific conditions are not specified, they can be carried out under conventional conditions or conditions recommended by the manufacturer. Reagents or instruments used where the manufacturer is not specified are all commercially available conventional products.
[0038] Example 1 1.1 Preparation of Electrolyte In an argon atmosphere and a vacuum glove box with a moisture content of <1ppm, dimethyl carbonate (DMC), propylene carbonate (PC), methyl acetate (MA), and γ-butyrolactone (GBL) were mixed in a weight ratio of DMC:PC:MA:GBL=3:6:5:6 to obtain 73.5g of the first solvent. Then, 13.0g of acetonitrile (ACN) was added to obtain 86.5g of non-aqueous organic solvent. Next, 0.5g of compound one was added, dissolved, and stirred thoroughly. Then, 13.0g of LiPF6 was added and mixed evenly to obtain 100g of non-aqueous electrolyte.
[0039] 1.2 Preparation of the positive electrode sheet Lithium iron phosphate material LiFePO4, binder PVDF and conductive agent SuperP are mixed evenly at a mass ratio of 95:1:4 to prepare a lithium secondary battery positive electrode slurry with a certain viscosity. The mixed slurry is coated on both sides of aluminum foil, dried and rolled to obtain the positive electrode sheet.
[0040] 1.3 Preparation of negative electrode Artificial graphite, binder PVDF and conductive agent SuperP are mixed evenly in a mass ratio of 90:2:8 to prepare a lithium secondary battery negative electrode slurry of a certain viscosity. The mixed slurry is coated on both sides of copper foil, dried and rolled to obtain the negative electrode sheet.
[0041] 1.4 Preparation of secondary batteries The positive electrode, separator, and negative electrode are stacked in sequence, and then layered as needed. After the tabs are welded, they are placed in the aluminum-plastic film of the battery outer packaging. The prepared non-aqueous electrolyte is injected into the dried bare cell. Vacuum sealing, standing, formation (0.05C constant current charging to 3.0V, then 0.1C constant current charging to 3.3V), shaping, and capacity testing are performed sequentially to obtain a 1Ah soft-pack lithium secondary battery.
[0042] The composition and content of the electrolytes in Examples 1-11 and Comparative Examples 1-4 are shown in Table 1. The preparation processes of the secondary battery electrolytes, positive electrode plates, negative electrode plates, and secondary batteries in Examples 2-11 and Comparative Examples 1-4 are the same as those in Example 1.
[0043] Table 1. Composition of the electrolytes in Examples 1-11 and Comparative Examples 1-4
[0044] The secondary batteries prepared in Examples 1-11 and Comparative Examples 1-4 were subjected to performance tests under the following conditions, and the results are shown in Table 2.
[0045] (1) High-temperature cycling performance test The lithium-ion battery was placed in a 45°C constant temperature chamber and allowed to stand for 30 minutes to reach a constant temperature. It was then charged at a constant current of 6C until the voltage reached 3.65V, followed by constant voltage charging at 3.65V until the current reached 0.05C. Next, it was discharged at a constant current of 6C until the voltage reached 2.5V. The initial discharge capacity was recorded as C0, and the volume at this point was recorded as V0. This constitutes one charge-discharge cycle. Then, 500 cycles of 6C / 6C charging and discharging were performed at 45°C. The discharge capacity was recorded as C1, and the volume as V1. The capacity retention rate and volume growth rate of the lithium-ion battery were calculated using the following formulas.
[0046] Capacity retention rate = C1 / C0 × 100% Volume growth rate = (V1 - V0) / V0 × 100% (2) High-temperature storage performance test The lithium-ion battery was charged at a constant current of 1C to a voltage of 3.65V at a constant temperature of 25℃, then charged at a constant voltage of 3.65V to a current of 0.05C, and then discharged at a constant current of 1C to a voltage of 2.5V. The first discharge capacity of the battery was recorded as C0. The lithium-ion battery was then placed in a constant temperature chamber at 60℃ and left to stand for 30 minutes to allow the lithium-ion battery to reach a constant temperature. After being stored at 60℃ for 15 days, it was then charged at a constant current and constant voltage of 1C / 1C at a constant temperature of 25℃. Discharge to 2.5V, and record the discharge capacity as C1. Then, charge the lithium-ion battery again at a constant temperature of 25℃ with a constant current of 1C to a voltage of 3.65V. Then, charge it at a constant voltage of 3.65V to a current of 0.05C. After storing it at 60℃ for 15 days, discharge it at a constant temperature of 25℃ with a constant current and constant voltage of 1C / 1C to 2.5V, and record the discharge capacity as C2. Calculate the capacity retention rate of the lithium-ion battery after 15 days and 30 days of storage using the following formulas.
[0047] 15-day storage capacity retention rate = C1 / C0 × 100% 30-day storage capacity retention rate = C2 / C0 × 100% (3) Low-temperature discharge test Under normal temperature (25℃) conditions, a lithium-ion battery is subjected to a single 0.5C / 0.5C charge-discharge cycle (battery cutoff voltage 3.0V, discharge capacity C0), with an upper limit voltage of 4.1V (cutoff current 0.05C). The battery is then fully charged to 4.1V at 0.5C (cutoff current 0.05C) at room temperature (25℃), and then transferred to -20℃ for 4 hours. It is then discharged at 0.5C to 3.0V, with a discharge capacity of C1. The capacity retention rate is calculated.
[0048] Capacity retention rate = (C1 / C0) × 100% Table 2 Performance test results of secondary batteries in Examples 1-8 and Comparative Examples 1-3
[0049] As shown in Table 2, Examples 1-11 still exhibited good cycle performance at a high rate of 6.0C, good storage performance at a high temperature of 60°C, and high capacity retention even after being stored at -20°C for 4 hours. This is because the addition of compound A containing tetracyanoborate in Examples 1-11 can fundamentally suppress the reduction decomposition, side reaction gas generation, and electrode corrosion problems of acetonitrile-based electrolytes during cycling and storage; at the same time, it significantly improves the ion transport efficiency, high-temperature storage capacity retention, and cycle life of the secondary battery, achieving synergistic optimization of the low-temperature performance, fast charging capability, and long-term stability of the acetonitrile-based secondary battery.
[0050] Comparing Examples 1-3 and Examples 6-10, it is evident that introducing ES and LiODFB into compound A results in higher electrochemical performance of the secondary battery. This is because ES possesses excellent interfacial film-forming properties, forming a dense, stable, and extremely low-impedance organic passivation film on the electrode surface. This effectively isolates the electrolyte from continuous contact with the electrode active material, preventing the continuous occurrence of side reactions. LiODFB replenishes the boron and fluorine active ions in the electrolyte, optimizes the inorganic composition of the SEI film, and enhances the mechanical strength and high-temperature stability of the film. Together with compound A containing tetracyanoborate, these two compounds form a synergistic effect, inhibiting electrolyte decomposition, gas generation, and electrode corrosion from multiple dimensions. This significantly reduces volume expansion during battery cycling, substantially improving the battery's high-rate cycle life and high-temperature storage stability.
[0051] Comparing Examples 1-3 and Examples 6-8, it is evident that when Compound A is Compound 2, the battery exhibits superior electrochemical performance. This is because Compound 2's molecular structure possesses optimal spatial configuration and charge distribution characteristics adapted to the electrode interface. Compared to Compound 1 and Compound 3, it can not only more efficiently capture active free radicals in the electrolyte and block solvent chain decomposition reactions, but also precisely control the composition and morphology of the SEI film at the electrode interface, forming a thin, dense, flexible, and conductive interface film. Furthermore, Compound 2 significantly enhances the electrolyte's ionic conductivity, substantially reducing polarization during high-rate charge and discharge processes and minimizing energy loss. Therefore, the corresponding battery outperforms the other two compounds in high-rate cycle capacity retention, volume expansion resistance, high-temperature storage stability, and low-temperature capacity performance.
[0052] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to preferred embodiments, it is not limited to those listed in the embodiments. Those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the essence and scope of the technical solutions of the present invention.
Claims
1. A secondary battery, comprising a positive electrode material, a negative electrode material, and an electrolyte, characterized in that, The negative electrode material comprises graphite, and the electrolyte comprises an electrolyte salt, a non-aqueous organic solvent, and an additive. The non-aqueous organic solvent comprises carbonate, carboxylic acid ester, and acetonitrile. The additive comprises compound A with the structural formula shown in Formula 1, wherein M... + Selected from alkali metal ions, substituted or unsubstituted C1~C 12 Alkylammonium ions, substituted or unsubstituted pyridinium ions, substituted or unsubstituted imidazolium ions, substituted or unsubstituted pyrrolidineium ions, substituted or unsubstituted imidazolidineium ions, Formula 1.
2. The secondary battery according to claim 1, characterized in that, Compound A is selected from at least one of compounds one through three. 。 3. The secondary battery according to claim 1, characterized in that, The compound A accounts for 0.05 to 3.00% of the mass of the electrolyte.
4. The secondary battery according to claim 1, characterized in that, The electrolyte salt is selected from at least one of lithium hexafluorophosphate, lithium perchlorate, lithium tetrafluoroborate, lithium trifluoromethanesulfonate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(oxalate-borate), lithium difluorophosphate, lithium lower aliphatic carboxylic acids, lithium difluorodioxalate phosphate, lithium bis(fluorosulfonyl)imide, lithium chloroborane, and lithium tetraphenylborate.
5. The secondary battery according to claim 1, characterized in that, The mass ratio of the carbonate, the carboxylic acid ester, and the acetonitrile is 1.0~5.0:2.0~6.0:1.
0.
6. The secondary battery according to claim 1, characterized in that, The carbonate is selected from at least one of ethylene carbonate, propylene carbonate, butyl carbonate, methyl pentyl carbonate, ethylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, and propylene carbonate.
7. The secondary battery according to claim 1, characterized in that, The carboxylic acid ester is selected from at least one of γ-butyrolactone, γ-valerolactone, δ-valerolactone, methyl acetate, ethyl acetate, ethyl propionate, butyl acetate, propyl propionate, and butyl propionate.
8. The secondary battery according to claim 1, characterized in that, The additive also includes compound B, which contains vinyl sulfite and / or lithium difluorooxalate borate, and the compound B accounts for 1.0 to 5.0% of the mass of the electrolyte.
9. The secondary battery according to claim 8, characterized in that, The compound B comprises vinyl sulfite and lithium difluorooxalate borate, and the mass ratio of the vinyl sulfite to the lithium difluorooxalate borate is 1~5:0.5~2.
0.
10. The secondary battery according to claim 1, characterized in that, The positive electrode material is selected from at least one of lithium iron phosphate materials, lithium cobalt oxide materials, lithium nickel cobalt manganese oxide materials, and lithium nickel cobalt aluminum oxide materials. The negative electrode material may also include silicon-based materials, which are silicon-carbon composite materials and / or silicon-oxygen composite materials.