Composite sulfide solid electrolyte, method for preparing the same, and battery

By coating a dense fluoropolymer layer onto the surface of a sulfide solid electrolyte in the form of chemically bonded SC, the problems of moisture sensitivity and interfacial compatibility of the sulfide electrolyte are solved, the air stability and electrochemical performance of the battery are improved, and a highly efficient battery modification effect is achieved.

CN123162291APending Publication Date: 2026-11-24TIANJIN GUOAN MGL NEW MATERIALS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611369896.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-04
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Sulfide solid electrolytes in lithium batteries suffer from problems such as sensitivity to moisture, narrow electrochemical window, and poor compatibility with lithium metal anode, resulting in insufficient safety and stability.

Method used

A dense fluorinated polymer layer is chemically bonded (SC) onto the surface of a sulfide solid electrolyte. The coating layer is formed through in-situ polymerization. The sulfur sites are activated by the mechanical force generated by ball milling, thereby achieving in-situ polymerization of the fluorinated monomers and forming a coating layer that is covalently bonded to the sulfide surface.

Benefits of technology

It improves the electrolyte's air stability, high voltage adaptability, and lithium dendrite protection, thereby enhancing the battery's performance stability and safety, and reducing production costs and environmental pressure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention provides a composite sulfide solid electrolyte, its preparation method, and a battery. The composite sulfide solid electrolyte comprises a sulfide solid electrolyte matrix and a fluoropolymer coating layer covering the surface of the sulfide solid electrolyte matrix; the fluoropolymer coating layer and the sulfide solid electrolyte matrix are connected by S-C covalent bonds. This invention coats the surface of the sulfide solid electrolyte with a dense fluoropolymer coating layer in the form of chemically bonded S-C, enabling the coated composite sulfide solid electrolyte to possess superhydrophobic properties, high-voltage oxidation resistance, and excellent lithium metal anode compatibility without significantly sacrificing the high ionic conductivity of the sulfide electrolyte itself, thereby improving battery performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of battery technology, and relates to a composite sulfide solid electrolyte, its preparation method, and a battery. Background Technology

[0002] With the rapid development of electric vehicles, portable electronic devices, and large-scale energy storage power stations, unprecedented demands have been placed on the energy density and safety of lithium batteries. Traditional liquid lithium batteries use organic liquid electrolytes, which pose inherent safety hazards such as leakage, combustion, and explosion, and their energy density is already approaching its theoretical limit. All-solid-state lithium batteries use non-flammable solid electrolytes instead of liquid electrolytes, fundamentally solving the safety issues. They are also compatible with high-energy-density lithium metal anodes and high-voltage cathodes, and are widely recognized as the core development direction of next-generation lithium battery technology.

[0003] Sulfide solid electrolytes (SEEs) have become the closest solid electrolyte system to industrialization due to their high room-temperature ionic conductivity and good machinability. However, SEEs suffer from three inherent defects that severely restrict their large-scale application in lithium metal solid-state batteries: first, they are extremely sensitive to moisture, rapidly hydrolyzing to produce toxic H2S gas upon exposure to air, while simultaneously experiencing a sharp drop in ionic conductivity; second, they have a narrow electrochemical window, easily undergoing oxidative decomposition upon contact with a high-voltage positive electrode; and third, they have poor interface compatibility with the lithium metal anode, easily forming a high-resistivity interface layer and inducing lithium dendrite growth during charging and discharging, leading to battery short-circuit failure. To overcome these defects, researchers have conducted extensive exploratory work, with main technical approaches including: modifying the composition of the sulfide bulk material through doping or alloying, controlling crystal size using nanostructure design, and constructing protective coatings on the surface of sulfide particles. Among these, surface coating modification, which can selectively construct physical / chemical barriers at the interface without altering the bulk structure of the sulfide electrolyte, is considered one of the most promising improvement strategies. However, current surface coating technology still suffers from drawbacks such as complex processes, uneven coating layers, difficulty in precisely controlling thickness, the potential introduction of high-resistivity layers, and the tendency for the coating layer to detach during cycling. Furthermore, coated products are unlikely to effectively address all three major industrialization challenges faced by sulfide solid electrolytes.

[0004] Therefore, providing a sulfide solid electrolyte and its preparation method to overcome the above-mentioned defects in the prior art is of great significance for expanding the application of batteries, especially solid-state batteries. Summary of the Invention

[0005] To address the shortcomings of existing technologies, the present invention aims to provide a composite sulfide solid electrolyte, its preparation method, and a battery thereof. The present invention coats the surface of a sulfide solid electrolyte with a dense fluoropolymer coating layer in the form of chemically bonded SC. This allows the coated composite sulfide solid electrolyte to possess superhydrophobic properties, high-voltage oxidation resistance, and excellent lithium metal anode compatibility without significantly sacrificing the high ionic conductivity of the sulfide electrolyte itself, thereby improving battery performance.

[0006] To achieve this objective, the present invention adopts the following technical solution:

[0007] In a first aspect, the present invention provides a composite sulfide solid electrolyte, the composite sulfide solid electrolyte comprising a sulfide solid electrolyte matrix and a fluoropolymer coating layer covering the surface of the sulfide solid electrolyte matrix;

[0008] The fluoropolymer coating layer and the sulfide solid electrolyte matrix have SC covalent bonds.

[0009] Preferably, the fluoropolymer in the fluoropolymer coating layer includes any one or a combination of at least two of fluoropolymers, fluoropolymers, or fluoropolyesters.

[0010] In a second aspect, the present invention provides a method for preparing a composite sulfide solid electrolyte as described in the first aspect, the method comprising the following steps:

[0011] The sulfide solid electrolyte matrix to be coated and the fluorine-containing monomer are mixed and ball-milled under a protective atmosphere. During the ball milling process, the fluorine-containing monomer completes in-situ polymerization on the surface of the sulfide solid electrolyte matrix to be coated, thus obtaining the composite sulfide solid electrolyte.

[0012] Preferably, the mass ratio of the fluorinated monomer to the sulfide solid electrolyte matrix to be coated is 1:(1~20).

[0013] Preferably, the fluorinated monomer includes a fluorinated cyclic monomer.

[0014] Preferably, the boiling point range of the fluorinated monomer is 40℃~300℃.

[0015] Preferably, the mass percentage of fluorine in the fluorinated monomer is 20% to 60%.

[0016] Preferably, the fluorinated monomer includes any one or a combination of at least two of the following: 3,3,3-trifluoropropylene carbonate, difluoroethylene carbonate, epifluoropropane, 3,3-bis(fluoromethyl)oxetane, α-(trifluoromethyl)-γ-butyrolactone, or tetrafluoroethane-β-sulfonyl lactone.

[0017] Preferably, the ball milling speed is 100 rpm to 400 rpm, and the ball milling time is 0.5 h to 10 h.

[0018] Preferably, the ball milling process includes continuous ball milling or intermittent ball milling.

[0019] Preferably, the in-situ polymerization includes in-situ ring-opening polymerization.

[0020] Preferably, after the ball milling process is completed, a drying process is performed to obtain the composite sulfide solid electrolyte.

[0021] Thirdly, the present invention also provides a battery comprising a composite sulfide solid electrolyte as described in the first aspect or a composite sulfide solid electrolyte prepared by the preparation method described in the second aspect.

[0022] Preferably, the battery comprises an all-solid-state battery, which includes an all-solid-state lithium metal battery.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] (1) In the composite sulfide solid electrolyte of the present invention, a dense fluorinated polymer coating layer is coated on the surface of the sulfide solid electrolyte in the form of chemical bonding SC. By combining the fluorinated polymer material through a special coating method, the coated composite sulfide solid electrolyte has high air stability, high voltage adaptability, superhydrophobic properties and high resistance to lithium dendrites without significantly sacrificing the high ionic conductivity of the sulfide electrolyte body. The coating modification effect has durability and long-term cycle stability, thereby improving the performance of the battery.

[0025] (2) In the preparation method provided by the present invention, under the conditions of no initiator, no solvent, and no catalyst, the in-situ polymerization of fluorine-containing monomers is achieved directly in one step during the ball milling process by utilizing the mechanical force generated by the ball mill. The coating layer grows directly from the surface of the sulfide solid electrolyte in situ, and the polymer chain is anchored to the electrolyte surface through SC covalent bonds. The particle surface of the sulfide solid electrolyte matrix to be coated has a large number of coordinatingly unsaturated nucleophilic sulfur sites (such as end groups S). 2- PS4 3-The active sulfur ends and defect-site sulfide anions in the structure inherently possess nucleophilic reactivity. The mechanical shearing and impact generated by ball milling further expose fresh surfaces and activate the nucleophilic ability of the sulfur sites. Without the need for additional initiators or catalysts, the nucleophilic sites on the particle surface of the sulfide solid electrolyte matrix to be coated can serve as initiation sites. Monomer adsorption and polymerization occur simultaneously. Nucleophilic attack on the electron-deficient centers of the fluorinated monomers triggers the polymerization mechanism, forming chain-growth active centers. Subsequent monomers continue to polymerize and add at the active chain ends, achieving directional growth of polymer chains on the sulfide surface. Finally, the starting end of the polymer chain is connected to the SC (Signal-Containing Electrolyte) system. Covalent bonds firmly bond with the sulfide surface, forming a chemically bonded coating layer. This in-situ polymerization can form molecular-level bonds between the host and the polymer layer. Compared with common physical adsorption, the coating layer formed by this in-situ polymerization is not easily detached during battery cycling. At the same time, the fluorinated monomers of this invention can achieve mild polymerization under ball milling without the need for a large amount of additional heat input. The preparation method of this invention improves the conversion rate of fluorinated monomers and the density of the coating layer, completely avoids solvent residue problems, significantly reduces production costs and environmental pressure, has high industrial feasibility, is technically mature, and is easy to scale up to ton-scale production. Detailed Implementation

[0026] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.

[0027] The "range" disclosed in this invention can be defined in the form of a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of the specific range. This type of range definition can include or exclude endpoints; any endpoint can be independently included or excluded, and they can be arbitrarily combined, meaning any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60~120 and 80~110 are listed for specific parameters, it is understood that ranges of 60~110 and 80~120 are also expected. Furthermore, if minimum range values ​​1 and 2 are listed, and maximum range values ​​3, 4, and 5 are also listed, then the following ranges are all expected: 1~3, 1~4, 1~5, 2~3, 2~4, and 2~5. In this invention, unless otherwise stated, the numerical range "a~b" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0~5" indicates that all real numbers between "0" and "5" have been listed in this article; "0~5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is described as an integer ≥2, it is equivalent to listing integers such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc. For instance, when a parameter is described as an integer selected from "2~10", it is equivalent to listing the integers 2, 3, 4, 5, 6, 7, 8, 9, and 10.

[0028] In this invention, "a combination of at least two" refers to a quantity greater than or equal to two, unless otherwise specified. For example, "any combination of one or at least two" means one or more or more items. It can be understood that when referring to "a combination of at least two," it refers to any suitable combination of multiple items, that is, a combination of "at least two" items carried out in a manner that does not conflict with and enables the implementation of this invention.

[0029] Unless otherwise specified, all embodiments and optional embodiments of the present invention can be combined with each other to form new technical solutions.

[0030] The term "embodiment" as used in this invention means that a specific feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment or implementation of the invention. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a mutually exclusive, independent, or alternative embodiment. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described in this invention can be combined with other embodiments.

[0031] In this invention, open-ended technical features or solutions described using terms such as "comprising" do not exclude additional members beyond those listed unless otherwise specified. They can be considered as providing both closed-ended features or solutions comprised of the listed members and open-ended features or solutions that include additional members beyond the listed members. For example, A includes a1, a2, and a3. Unless otherwise specified, it may also include other members or exclude additional members. This can be considered as providing both technical features or solutions where "A is composed of a1, a2, and a3" or "A is selected from a1, a2, and a3," and technical features or solutions where "A includes not only a1, a2, and a3, but also other members."

[0032] In this invention, unless otherwise specified, the features or solutions corresponding to "and / or" include any one of two or more of the related listed items, as well as any and all combinations of the related listed items. These arbitrary and all combinations include any two related listed items, any more related listed items, or a combination of all related listed items. For example, "A and / or B" represents a group consisting of A, B, and "a combination of A and B". "Containing A and / or B" can mean "containing A, containing B, and containing A and B", or "containing A, containing B, or containing A and B", and can be appropriately understood according to the context.

[0033] In this invention, the terms "first aspect," "second aspect," "third aspect," "fourth aspect," etc., are used for descriptive purposes only and should not be construed as indicating or implying relative importance or quantity, nor should they be construed as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first," "second," "third," "fourth," etc., serve only as a non-exhaustive enumeration and should be understood not to constitute a closed limitation on the quantity.

[0034] In this invention, "optional" means that something is optional, that is, it refers to either "with" or "without". If there are multiple "optional" options in a technical solution, unless otherwise specified, and there are no contradictions or mutual constraints, then each "optional" option is independent.

[0035] In this invention, "room temperature" generally refers to 4℃~35℃, and can refer to 20℃±5℃. In some embodiments of this invention, room temperature refers to 20℃~30℃.

[0036] In one embodiment, the present invention provides a composite sulfide solid electrolyte, the composite sulfide solid electrolyte comprising a sulfide solid electrolyte matrix and a fluoropolymer coating layer covering the surface of the sulfide solid electrolyte matrix;

[0037] The fluoropolymer coating layer is connected to the sulfide solid electrolyte matrix via SC covalent bonds.

[0038] In the composite sulfide solid electrolyte of the present invention, a dense fluoropolymer coating layer is coated on the surface of the sulfide solid electrolyte in the form of chemical bonding SC. By combining the fluoropolymer material through a special coating method, the coated composite sulfide solid electrolyte can have high air stability, high voltage adaptability, superhydrophobic properties and high resistance to lithium dendrites without significantly sacrificing the high ionic conductivity of the sulfide electrolyte itself. The coating modification effect has durability and long-term cycle stability, thereby improving the performance of the battery.

[0039] The fluoropolymer coating in this invention differs from conventional physical interface coating. Conventional physical interface coatings are only physically adsorbed onto the substrate, resulting in weak interfacial bonding. They are easily peeled off during electrode preparation or battery cycling, leading to a sharp increase in interfacial impedance and affecting the long-term stability of the battery. In contrast, this invention coats the surface of the sulfide solid electrolyte with a dense fluoropolymer coating in the form of chemically bonded SC, resulting in strong interfacial bonding and durable coating modification effects.

[0040] In some embodiments, the fluoropolymer in the fluoropolymer coating layer includes any one or a combination of at least two of fluoropolycarbonate, fluoropolyether, or fluoropolyester.

[0041] The fluoropolymer provided by this invention has high antioxidant properties, and in synergy with the strong electron-withdrawing effect of the CF bond, it more effectively prevents the oxidation of the positive electrode, further improving the electrochemical performance of the battery. At the same time, the hetero-chain polymer chain provided by this invention has higher flexibility than carbon-carbon chain, which is beneficial to forming a dense, uniform and flexible coating layer on the particle surface of the sulfide solid electrolyte matrix.

[0042] In one embodiment, the present invention provides a method for preparing a composite sulfide solid electrolyte as described in the above embodiments, the preparation method comprising the following steps:

[0043] The sulfide solid electrolyte matrix to be coated and the fluorine-containing monomer are mixed and ball-milled under a protective atmosphere. During the ball milling process, the fluorine-containing monomer completes in-situ polymerization on the surface of the sulfide solid electrolyte matrix to be coated, thus obtaining the composite sulfide solid electrolyte.

[0044] In the preparation method provided by this invention, under conditions of no initiator, no solvent, and no catalyst, the in-situ polymerization of fluorinated monomers is achieved directly in one step during ball milling, utilizing the mechanical force generated by the ball mill. The coating layer grows directly from the surface of the sulfide solid electrolyte in situ, and the polymer chains are anchored to the electrolyte surface through SC covalent bonds. The surface of the sulfide solid electrolyte matrix particles to be coated contains a large number of coordinatingly unsaturated nucleophilic sulfur sites (such as end groups S). 2- PS4 3- The active sulfur ends and defective sulfide anions of the structure inherently possess nucleophilic reactivity. The mechanical shearing and impact generated by ball milling further expose fresh surfaces and activate the nucleophilic ability of sulfur sites. Without the need for additional initiators or catalysts, the nucleophilic sites on the surface of the sulfide solid electrolyte matrix particles to be coated can serve as initiation sites. Monomer adsorption and polymerization occur simultaneously. Nucleophilic attack on the electron-deficient centers of the fluorinated monomers triggers the polymerization mechanism, forming chain growth active centers. Subsequently, monomers continue to polymerize and add at the active chain ends, achieving directional growth of polymer chains from the sulfide surface. Finally, the starting ends of the polymer chains are firmly bonded to the sulfide surface through SC covalent bonds, forming a chemically bonded coating layer. This in-situ polymerization can form molecular-level bonds between the host and the polymer layer. At the same time, the fluorinated monomers of this invention can achieve mild polymerization under ball milling without the need for a large amount of additional heat input. The preparation method of this invention improves the conversion rate of fluorinated monomers and the density of the coating layer, completely avoids solvent residue problems, significantly reduces production costs and environmental pressure, has high industrial feasibility, is technically mature, and is easy to scale up to ton-scale production.

[0045] Traditional fluoropolymer coating involves pre-synthesizing high-molecular-weight polymer powders via free radical polymerization. The polymerization process is completely separate from the sulfide coating, relying solely on physical action to achieve surface coverage. Furthermore, in-situ polymerization often requires solvents and external initiators and catalysts, leading to problems such as solvent residue, long reaction cycles, low efficiency, high cost, and significant environmental impact. Additionally, traditional fluoropolymers are pre-synthesized high molecules with molecular weights typically reaching hundreds of thousands, making them prone to aggregation and difficult to achieve nanoscale uniform coating. In contrast, the polymer of this invention grows in situ on the sulfide surface, forming an ultrathin, uniform nanoscale film free of free homopolymer impurities.

[0046] In some embodiments, the mass ratio of the fluorinated monomer to the sulfide solid electrolyte matrix to be coated is 1:(1~20), for example, 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, 1:16, 1:17, 1:18, 1:19 or 1:20, etc.

[0047] In the preparation process of this invention, the selection of an appropriate amount of fluorinated monomer is more conducive to obtaining a uniform and dense coating layer. In particular, adjusting the mass ratio of the fluorinated monomer to the sulfide solid electrolyte matrix to be coated to 1:(1~20) can form a continuous and dense nanoscale coating layer on the surface of the sulfide electrolyte matrix. This can effectively isolate air and moisture and suppress interfacial side reactions, while minimizing the loss of ionic conductivity.

[0048] In some embodiments, the present invention does not limit the median particle size of the sulfide solid electrolyte matrix to be coated. Without departing from the overall technical concept of the present invention, conventional particle size ranges are applicable.

[0049] For example, the median particle size Dv50 of the sulfide solid electrolyte matrix to be coated is 0.5μm to 20μm, such as 0.5μm, 1μm, 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, 16μm, 17μm, 18μm, 19μm or 20μm, etc.

[0050] It is understood that the sulfide solid electrolyte matrix to be coated in this invention can be purchased directly from commercial sources, or it can be prepared by conventional methods. Those skilled in the art can make adaptive selections and adjustments according to actual needs.

[0051] This invention does not specifically limit the type of material to be coated with sulfide solid electrolyte. Any conventional sulfide solid electrolyte to be coated is applicable without departing from the overall technical concept of this invention.

[0052] For example, but not limitingly, the sulfide solid electrolyte to be coated includes Li6PS5X (X = at least one of Cl, Br, or I), Li 10 GeP2S 12 Li7P3S 11 The sulfide solid electrolyte to be coated may include at least one of Li3PS4 or Li3PS4, and may also include conventional doping elements, including but not limited to at least one of Al, Si, Sn, Ti or Zr.

[0053] In some embodiments, the fluorinated monomer includes a fluorinated cyclic monomer.

[0054] In some embodiments, the fluorinated monomer includes any one or a combination of at least two of 3,3,3-trifluoropropylene carbonate, difluoroethylene carbonate, epifluoropropane, 3,3-bis(fluoromethyl)oxetane, α-(trifluoromethyl)-γ-butyrolactone, or tetrafluoroethane-β-sulfonyl lactone.

[0055] The fluorinated monomers provided in this invention are selected from fluorinated cyclic monomers, which can undergo ring-opening polymerization. Furthermore, the electron-deficient centers of fluorinated cyclic monomers are unique, the ring-opening breakage sites are clearly defined, and there are no additional side reactions. At the same time, cyclic monomers have inherent ring strain, and the intrinsically active sulfur anions on the ring can directly nucleophilically attack the ring-opening sites, and chain growth can start from the surface sites, without the need for additional initiators or catalysts. In contrast, non-cyclic monomers mostly rely on free radical polymerization, often requiring initiators, resulting in low polymerization efficiency and a high tendency to generate small molecule byproducts during polymerization, which limits the polymerization growth of fluorinated polymers and affects the coating effect.

[0056] In some embodiments, the boiling point range of the fluorinated monomer is 40°C to 300°C, such as 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 125°C, 150°C, 175°C, 200°C, 225°C, 250°C, 280°C, or 300°C.

[0057] This invention selects fluorinated monomers with a boiling point range of 40℃ to 300℃ for coating polymerization, which avoids the monomer volatilization caused by heat generation during ball milling due to the low boiling point of the monomer, thus affecting the polymerization and coating effect; at the same time, it avoids the damage to the sulfide material and the surface coating layer caused by the high boiling point of the monomer during the subsequent vacuum drying to remove excess monomer.

[0058] In some embodiments, the fluorine content in the fluorinated monomer is 20% to 60% by mass, for example, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, or 60%.

[0059] In selecting fluorine-containing monomers, this invention explored the mass percentage of fluorine and found that a mass percentage of fluorine of 20% to 60% can maximize the improvement of air stability, high voltage oxidation resistance, and lithium metal interface compatibility without significantly sacrificing the high ionic conductivity of the sulfide electrolyte.

[0060] In some embodiments, the ball milling process is performed at a speed of 100 rpm to 400 rpm, such as 100 rpm, 130 rpm, 150 rpm, 180 rpm, 200 rpm, 230 rpm, 250 rpm, 280 rpm, 300 rpm, 330 rpm, 350 rpm, 380 rpm, or 400 rpm.

[0061] In the ball milling process of this invention, mechanical force is used to activate the surface of the sulfide solid electrolyte to be coated through a triple action of physical crushing, lattice distortion, and selective chemical bond breaking, generating a large number of highly active unsaturated sulfur nucleophilic sites. Simultaneously, the ring strain bonds of the monomer are stretched, reducing the ring-opening activation energy, thus achieving synergistic polymerization initiation by mechanical force and the nucleophilicity of the sulfur sites. No solvents, initiators, or catalysts are required, improving monomer conversion and coating density, completely avoiding solvent residue problems, and significantly reducing production costs and environmental pressure. Furthermore, the ball milling speed does not need to be too high, and high-energy ball milling processes are not required. A relatively low ball milling speed of 100 rpm to 400 rpm provides sufficient mechanical activation energy to ensure the surface polymerization reaction proceeds fully, while avoiding problems such as excessive destruction of the sulfide crystal structure, uncontrolled particle size refinement, and excessive introduction of impurities from the milling media caused by excessively high speeds.

[0062] In some embodiments, the ball milling treatment time is 0.5h to 10h, for example, 0.5h, 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h or 10h.

[0063] It is understood that the present invention can use conventional ball milling equipment for ball milling. At the same time, the present invention does not have special requirements for the ball-to-material ratio during the ball milling process. A conventional ball-to-material ratio can be used, such as (5~25):1, for example, 5:1, 10:1, 20:1 or 25:1, etc.

[0064] In some embodiments, the ball milling process includes continuous ball milling or intermittent ball milling.

[0065] It is understood that the ball milling process of the present invention can be carried out continuously until the ball milling is completed; or it can be carried out intermittently until the ball milling is completed, depending on the boiling point of the fluorinated monomer. When the boiling point of the fluorinated monomer is relatively low, for example, 40~100℃, intermittent ball milling can be used, for example, the ball milling process can be paused for a fixed time after each ball milling period, and then the ball milling process can be continued.

[0066] In some embodiments, the in-situ polymerization includes in-situ ring-opening polymerization.

[0067] This invention uses fluorinated cyclic monomers as monomers for polymerization and completes ring-opening polymerization during ball milling, rather than free radical polymerization. The polymerization conditions are more suitable, and the polymer coating is more dense.

[0068] The core of the in-situ coating of this invention is in-situ coating without the addition of external initiators / catalysts / organic solvents, using the active sites on the surface of the sulfide solid electrolyte as the initiation center, anchoring the polymer chain ends to the electrolyte surface with covalent bonds, and completing the polymerization and coating simultaneously. Polymerization of other polymer materials generally suffers from poor mechanism compatibility, low reaction controllability, easy destruction of the electrolyte matrix, numerous side reactions, and poor coating quality. Therefore, ring-opening polymerization in this invention has the best compatibility with the sulfide solid electrolyte system, the most prominent advantages, and is the polymerization method that best achieves the core objective of modification without energy loss. Ring-opening polymerization is more suitable because: 1) cyclic monomers are sensitive to nucleophilic attack, and the cyclic structure has ring strain; its electron-deficient centers are not only easily attacked by S on the sulfide surface... 2- Nucleophilic attack can also easily induce ring-opening under mechanical force. During ring-opening polymerization, the ring structure is opened, and the ring strain is released, which is thermodynamically favorable. This means that ring-opening polymerization can proceed spontaneously under mild conditions without requiring a large amount of additional energy. However, acyclic monomers do not have ring strain, and their polymerization reaction depends entirely on the heat of chemical reaction between functional groups, usually requiring higher temperatures, longer reaction times, or external catalysts to drive it. 2) Cyclic monomers have a unique electron-deficient center, a clearly defined ring-opening breakage site, and no additional side reactions. Many acyclic monomers easily generate small molecule byproducts during polymerization. 3) Ring-opening polymerization is a chain growth process, with the polymer chain gradually extending outward from the initiation site on the sulfide surface. This surface-growing mode allows the thickness of the coating layer to be precisely controlled by adjusting parameters such as monomer concentration and reaction time, making it easy to form a uniform nanoscale thin layer. The polymerization of acyclic monomers is usually a chain reaction; once initiated, the reaction is violent and exothermic, making it difficult to confine the polymerization reaction to the particle surface. More likely, the monomers will homopolymerize in the system, forming a large number of polymer particles that precipitate, rather than forming a uniform coating layer on the sulfide surface.

[0069] Furthermore, the advantages of ring-opening polymerization for coating are as follows: 1) Coatings obtained through physical coating and in-situ polymerization with added initiators have only a weak bond with the electrolyte. Under the interfacial stress and volume changes during electrode pressing and battery cycling, they are prone to peeling, cracking, and displacement, gradually losing their protective function. In contrast, the polymer chain ends of ring-opening polymerization of cyclic monomers form covalent bonds with the electrolyte surface, resulting in a coating layer with a much stronger bonding force than the physical adsorption system. Under the stress of electrode pressing and battery cycling, it is not easily peeled off, significantly improving long-cycle stability. 2) No additional initiators or catalysts are required. Polymerization is triggered entirely by the surface activity of the sulfide itself and the mechanical force generated during ball milling, avoiding the negative impact of initiator residues and catalyst impurities on the electrochemical performance of the electrolyte. At the same time, true in-situ surface initiation is achieved, rather than physical deposition after free phase polymerization. 3) The thickness of the coating layer formed by ring-opening polymerization can be precisely controlled by adjusting parameters such as monomer concentration and reaction time, making it easy to form a uniform nanoscale thin layer. 4) After the cyclic monomer is opened, the functional polar groups (carbonate bond, ether bond, ester bond) are directly embedded in the polymer backbone. These polar groups can conduct lithium ions, so that the coating layer itself has a certain ion conduction ability.

[0070] In some embodiments, after the ball milling process is completed, a drying process is performed to obtain the composite sulfide solid electrolyte.

[0071] It is understood that after ball milling, the present invention does not require a polymerization process; that is, the polymerization process ends when ball milling is completed, and a simple drying process is sufficient, such as vacuum drying.

[0072] In some embodiments, the protective atmosphere includes a nitrogen atmosphere and / or an inert gas atmosphere, wherein the inert gas includes, but is not limited to, argon and / or helium.

[0073] In one embodiment, the present invention also provides a battery comprising a composite sulfide solid electrolyte as described in the above embodiments or a composite sulfide solid electrolyte prepared by the preparation method described in the above embodiments.

[0074] It is understood that the composite sulfide solid electrolyte provided by the present invention can be used as a modifier to modify electrode materials, or as one of the raw materials for the preparation of positive electrode sheets, negative electrode sheets, or solid electrolyte layers; that is, the composite sulfide solid electrolyte of the present invention is applicable to liquid lithium-ion batteries, solid-liquid lithium-ion batteries, and all-solid-state lithium-ion batteries. Those skilled in the art can make adaptive selections and adjustments according to actual needs.

[0075] In some embodiments, the battery includes an all-solid-state battery, which includes an all-solid-state lithium metal battery.

[0076] The composite sulfide solid electrolyte provided by this invention solves the problems of weak interfacial bonding and easy peeling off during electrode preparation and battery cycling of traditional physical coatings. By utilizing the low surface energy and high CF bond energy characteristics of the fluoropolymer layer and the unique mechanism of forming a LiF-rich stable interface layer with lithium metal in situ, the invention achieves a triple synergistic improvement in the air stability, high voltage adaptability and resistance to lithium dendrite growth of the sulfide electrolyte, thereby enhancing its application potential in all-solid-state lithium metal batteries.

[0077] The numerical range described in this invention includes not only the point values ​​listed above, but also any point values ​​within the numerical ranges not listed above. Due to space limitations and for the sake of brevity, this invention will not exhaustively list all the specific point values ​​included in the range.

[0078] Example 1

[0079] This embodiment provides a composite sulfide solid electrolyte, which includes a sulfide solid electrolyte matrix and a fluoropolymer coating layer covering the surface of the sulfide solid electrolyte matrix;

[0080] The chemical formula of the sulfide solid electrolyte matrix is ​​Li6PS5Cl, and the fluorinated polymer is fluorinated polycarbonate.

[0081] The fluoropolymer coating layer is connected to the sulfide solid electrolyte matrix via SC covalent bonds.

[0082] The preparation method of the composite sulfide solid electrolyte is as follows:

[0083] First, 10g of the sulfide solid electrolyte matrix Li6PS5Cl powder to be coated and 1.2g of fluorine-containing cyclic monomer 3,3,3-trifluoropropylene carbonate (fluorine mass percentage is 36.5%) were added to a zirconia ball mill jar with a ball-to-material ratio of 10:1. The ball mill jar was then sealed under an argon atmosphere.

[0084] The ball milling jar was placed in a planetary ball mill and milled at 300 rpm for 3 hours. After the reaction was completed, the milled product was taken out and vacuum dried at 100°C for 12 hours to remove unreacted monomers, thus obtaining the composite sulfide solid electrolyte.

[0085] Example 2

[0086] This embodiment provides a composite sulfide solid electrolyte, which includes a sulfide solid electrolyte matrix and a fluoropolymer coating layer covering the surface of the sulfide solid electrolyte matrix;

[0087] The chemical formula of the sulfide solid electrolyte matrix is ​​Li6PS5Cl, and the fluorinated polymer is a fluorinated polyether.

[0088] The fluoropolymer coating layer is connected to the sulfide solid electrolyte matrix via SC covalent bonds.

[0089] The preparation method of the composite sulfide solid electrolyte is as follows:

[0090] First, 10g of the sulfide solid electrolyte matrix Li6PS5Cl powder to be coated and 0.9g of the fluorine-containing cyclic monomer epifluoropropane (fluorine mass percentage is 25%) were added to a zirconia ball mill jar with a ball-to-material ratio of 10:1. The ball mill jar was then sealed under an argon atmosphere.

[0091] The ball milling jar was placed in a planetary ball mill and intermittently ball milled at 250 rpm. The intermittent ball milling process involved milling for 20 minutes, pausing for 10 minutes, and then continuing the milling process. The total time for pure ball milling was 3 hours. After the reaction was completed, the milled product was taken out and vacuum dried at 60°C for 5 hours to remove unreacted monomers, thus obtaining the composite sulfide solid electrolyte.

[0092] Example 3

[0093] This embodiment provides a composite sulfide solid electrolyte, which includes a sulfide solid electrolyte matrix and a fluoropolymer coating layer covering the surface of the sulfide solid electrolyte matrix;

[0094] The chemical formula of the sulfide solid electrolyte matrix is ​​Li6PS5Cl, and the fluorinated polymer is a fluorinated polyester.

[0095] The fluoropolymer coating layer is connected to the sulfide solid electrolyte matrix via SC covalent bonds.

[0096] The preparation method of the composite sulfide solid electrolyte is as follows:

[0097] First, 10g of the sulfide solid electrolyte matrix Li6PS5Cl powder to be coated and 1.2g of the fluorine-containing cyclic monomer α-(trifluoromethyl)-γ-butyrolactone (fluorine mass percentage is 37%) were added to a zirconia ball mill jar with a ball-to-material ratio of 10:1. The ball mill jar was then sealed under an argon atmosphere.

[0098] The ball milling jar was placed in a planetary ball mill and intermittently ball milled at 350 rpm. The intermittent ball milling process consisted of grinding for 20 minutes, pausing for 10 minutes, and then continuing ball milling. The total pure ball milling time was 4 hours. The mixture was then vacuum dried at 80°C for 10 hours to remove unreacted monomers, thus obtaining the composite sulfide solid electrolyte.

[0099] Example 4

[0100] The difference between this embodiment and Embodiment 1 is that the sulfide solid electrolyte matrix in this embodiment is Li. 10 GeP2S 12 .

[0101] All other conditions remain the same as in Example 1.

[0102] Example 5

[0103] The difference between this embodiment and Embodiment 1 is that the mass of the fluorinated cyclic monomer 3,3,3-trifluoropropylene carbonate in this embodiment is 0.5g, that is, the mass ratio of the fluorinated cyclic monomer to the sulfide solid electrolyte matrix to be coated is 1:20.

[0104] All other conditions remain the same as in Example 1.

[0105] Example 6

[0106] The difference between this embodiment and Embodiment 1 is that the mass of the fluorinated cyclic monomer 3,3,3-trifluoropropylene carbonate in this embodiment is 10g, that is, the mass ratio of the fluorinated cyclic monomer to the sulfide solid electrolyte matrix to be coated is 1:1.

[0107] All other conditions remain the same as in Example 1.

[0108] Example 7

[0109] The difference between this embodiment and Embodiment 1 is that the mass of the fluorinated cyclic monomer 3,3,3-trifluoropropylene carbonate in this embodiment is 0.4g, that is, the mass ratio of the fluorinated cyclic monomer to the sulfide solid electrolyte matrix to be coated is 1:25.

[0110] All other conditions remain the same as in Example 1.

[0111] Example 8

[0112] The difference between this embodiment and Embodiment 1 is that the mass of the fluorinated cyclic monomer 3,3,3-trifluoropropylene carbonate in this embodiment is 20g, that is, the mass ratio of the fluorinated cyclic monomer to the sulfide solid electrolyte matrix to be coated is 1:0.5.

[0113] All other conditions remain the same as in Example 1.

[0114] Example 9

[0115] The difference between this embodiment and Embodiment 1 is that the fluorinated monomer in this embodiment is hexafluorobutyl acrylate, and its polymerization process is free radical polymerization.

[0116] All other conditions remain the same as in Example 1.

[0117] Example 10

[0118] The difference between this embodiment and Embodiment 1 is that the fluorinated monomer in this embodiment is fluoroethylene carbonate, and the mass percentage of fluorine is 17.9%.

[0119] All other conditions remain the same as in Example 1.

[0120] Example 11

[0121] The difference between this embodiment and Embodiment 1 is that the fluorinated monomer in this embodiment is hexafluoropropylene oxide, and the mass percentage of fluorine is 68.7%.

[0122] All other conditions remain the same as in Example 1.

[0123] Example 12

[0124] The difference between this embodiment and Embodiment 1 is that the ball milling speed in this embodiment is 400 rpm.

[0125] All other conditions remain the same as in Example 1.

[0126] Example 13

[0127] The difference between this embodiment and Embodiment 1 is that the ball milling speed in this embodiment is 100 rpm.

[0128] All other conditions remain the same as in Example 1.

[0129] Example 14

[0130] The difference between this embodiment and Embodiment 1 is that the ball milling speed in this embodiment is 450 rpm.

[0131] All other conditions remain the same as in Example 1.

[0132] Example 15

[0133] The difference between this embodiment and Embodiment 1 is that the ball milling speed in this embodiment is 50 rpm.

[0134] All other conditions remain the same as in Example 1.

[0135] Comparative Example 1

[0136] The difference between this comparative example and Example 1 is that the composite sulfide solid electrolyte in this comparative example is the sulfide solid electrolyte matrix to be coated in Example 1, which is vacuum dried at 45°C for 12 hours before use.

[0137] All other conditions remain the same as in Example 1.

[0138] Comparative Example 2

[0139] The difference between this comparative example and Example 1 is that the preparation method of the composite sulfide solid electrolyte in this comparative example is as follows:

[0140] 200 mg of Li6PS5Cl sulfide solid electrolyte powder was weighed and added to a reaction flask. 4 mL of isobutyl isobutyrate was added to form a suspension system. Then, 30 μL of 3,3,3-trifluoropropylene carbonate was added. The mixture was stirred and reacted at 80 °C for 12 h. After the reaction was completed, the mixture was separated by centrifugation, washed with isobutyl isobutyrate, and vacuum dried at 50 °C for 12 h. During the stirring polymerization process, the structure of the sulfide matrix was destroyed, and the composite sulfide solid electrolyte was obtained.

[0141] Comparative Example 3

[0142] The difference between this comparative example and Example 1 is that the composite sulfide solid electrolyte in this comparative example does not contain SC covalent bonds.

[0143] In the preparation method, the fluorinated cyclic monomer 3,3,3-trifluoropropylene carbonate is directly replaced with polycarbonate formed after polymerization, that is, the ball milling treatment is a purely physical coating.

[0144] All other conditions remain the same as in Example 1.

[0145] Performance Test 1

[0146] The composite sulfide solid electrolytes provided in the examples and comparative examples were tested for room temperature ionic conductivity, electrochemical window LSV, and air stability.

[0147] Room temperature ionic conductivity: At room temperature (25°C), the composite sulfide solid electrolytes provided in the examples and comparative examples were pressed into sheets with a diameter of 10 mm under 500 MPa, and the room temperature ionic conductivity was tested by electrochemical impedance spectroscopy (EIS) using the blocked electrode method.

[0148] Electrochemical window: The composite sulfide solid electrolytes provided in the examples and comparative examples were tested using linear sweep voltammetry (LSV) to obtain the bulk antioxidant voltage value, i.e., the electrochemical window value (V).

[0149] Air stability: The room temperature ionic conductivity of the composite sulfide solid electrolytes provided in the examples and comparative examples was tested by electrochemical impedance spectroscopy (EIS) using the blocked electrode method after being exposed to closed air at a dew point of -40°C for 5 hours.

[0150] The test results are shown in Table 1.

[0151] Table 1

[0152]

[0153] From Table 1, we can obtain:

[0154] This invention coats a dense fluoropolymer coating layer on the surface of a sulfide solid electrolyte by chemical bonding (SC). Without significantly sacrificing the high ionic conductivity of the sulfide electrolyte, the coated composite sulfide solid electrolyte possesses both superhydrophobic properties and high-pressure oxidation resistance.

[0155] Performance Test 2

[0156] The composite sulfide solid electrolytes provided in the examples and comparative examples were assembled into Li / / Li symmetric model batteries in an argon-filled glove box (water content <0.1 ppm, oxygen content <0.1 ppm). Each model battery was tested using a blue electric current testing system to determine its critical current density. The test employed a constant current step-increment method, with an initial current density of 0.1 mA / cm². 2 The current density step size is 0.05 mA / cm². 2 The test results shown in Table 2 were obtained.

[0157] Table 2

[0158]

[0159] From Table 2, we can obtain:

[0160] The composite sulfide solid electrolyte provided by this invention can generate a LiF layer in situ when in contact with lithium metal, exhibiting excellent resistance to lithium dendrite formation.

[0161] Performance Test 3

[0162] Preparation method of all-solid-state lithium-ion battery: In an argon glove box, the solid electrolyte and positive electrode prepared in the examples and comparative examples are placed together.

[0163] Highly active material (lithium-rich manganese-based cathode, Li) 1.4 Ni 0.3 Mn 0.7 O 2.4The conductive agent was weighed in a weight ratio of 25:65:10, mixed, and ground evenly using an agate mortar to prepare a composite positive electrode material. In a battery mold with a diameter of 10 mm, 100 mg of modified sulfide solid electrolyte was laid flat and pressurized at 360 MPa. Then, 3.7 mg of the aforementioned composite positive electrode material was laid flat and pressurized again at 360 MPa. An aluminum foil was stacked on the positive electrode layer side, thus forming a current collector on the positive electrode side. An indium sheet with a mass of 80 mg and a diameter of 10 mm was placed on the solid electrolyte layer side, and a lithium sheet with a mass of 2.4 mg and a diameter of 8 mm was placed on the indium sheet as the negative electrode material. The mixture was pressurized at 80 MPa to create a laminate consisting of a positive electrode, a solid electrolyte layer, and a negative electrode. Stainless steel current collectors were placed above and below the laminate, and current collector leads were attached to the current collectors to obtain an all-solid-state lithium-ion battery.

[0164] The obtained mold batteries were tested using the Blue Electric testing system. Cyclic performance test conditions: room temperature 25℃, 0.1C rate, voltage range 1.5-4.3V (vs Li / Li). + The test results shown in Table 3 were obtained.

[0165] Table 3

[0166]

[0167] Combining Tables 1, 2, and 3, we can conclude that:

[0168] This invention coats a dense fluoropolymer coating layer onto the surface of a sulfide solid electrolyte in the form of chemically bonded SC. This results in a composite sulfide solid electrolyte that combines superhydrophobic properties, high-voltage oxidation resistance, and high ionic conductivity. The coating modification effect is durable and has long-term cycle stability. By utilizing the low surface energy, high CF bond energy, and unique mechanism of the fluoropolymer layer to form a stable LiF-rich interface layer in situ with lithium metal, the performance of the battery is improved.

[0169] Data analysis of Examples 1 and 5-8 shows that, during the preparation process of this invention, selecting an appropriate amount of fluorinated monomer is more conducive to obtaining a uniform and dense coating layer. In particular, adjusting the mass ratio of the fluorinated monomer to the sulfide solid electrolyte matrix to be coated to 1:(1~20) allows for precise control of in-situ polymerization to form a nanoscale uniform and dense coating layer. The coating thickness is thin and the coverage is complete. The ultrathin fluorinated coating layer does not significantly increase the migration resistance of lithium ions, thereby maximizing the maintenance of the intrinsic high ionic conductivity of the sulfide electrolyte. At the same time, the thin and dense nano-coating layer can give full play to the structural advantages of the fluorinated polymer, effectively improving the air stability, interfacial compatibility and cycle stability of the sulfide electrolyte, taking into account both ion conduction and protective modification effects.

[0170] Analysis of the data from Examples 1 and 9 shows that the ring-opening polymerization of fluorinated cyclic monomers used in this invention is more conducive to forming a uniform and dense coating layer compared to non-ring-opening polymerization. Ring-opening polymerization utilizes the nucleophilicity of the active sulfur sites on the sulfide electrolyte surface to initiate polymerization, allowing the fluorinated polymer layer to grow in situ from the surface active sites, achieving uniform coverage at the molecular level and avoiding the physical coating unevenness or agglomeration problems that may occur with non-ring-opening polymerization. Simultaneously, the ring-opening polymerization reaction conditions are mild, with no small molecule byproducts generated in condensation polymerization, making it a non-destructive surface modification strategy that can complete the coating without significantly affecting the bulk structure and ionic conductivity of the sulfide electrolyte. Compared to non-ring-opening polymerization, ring-opening polymerization is more conducive to constructing a uniform and complete ultra-thin fluorinated coating layer, effectively isolating moisture, suppressing side reactions, optimizing solid-solid interface contact, and significantly improving battery cycle stability and air resistance stability while ensuring the high ionic conductivity of the sulfide electrolyte.

[0171] Data analysis of Examples 1, 10, and 11 reveals that the present invention explored the mass percentage of fluorine in the fluorinated monomer selection. It was found that a fluorine mass percentage within the range of 20% to 60% maximizes air stability, high-voltage oxidation resistance, and lithium metal interface compatibility without significantly sacrificing the high ionic conductivity of the sulfide electrolyte. When the fluorine mass percentage is too low (Example 10), the effective fluorine content in the coating layer is insufficient to form a stable protective barrier, resulting in significantly inferior oxidation resistance, air stability, and anti-dendrying properties compared to Example 1. When the fluorine mass percentage is too high (e.g., Example 11), the organic coating layer formed by the polymerization of this monomer significantly reduces the ionic conductivity of the composite sulfide. This is mainly attributed to the strong rigidity and intermolecular interactions of the high-fluorine content segments, which restrict the migration of lithium ions within the coating layer. Meanwhile, although the introduction of fluorine-containing groups usually helps to improve the oxidation resistance and air stability of materials, this study found that when the fluorine content is too high (Example 11), its effect on improving oxidation resistance and air stability is insufficient. It is speculated that this is because the high fluorine content leads to poor interfacial compatibility between the coating layer and the sulfide matrix, resulting in uneven coating and thus weakening the protective effect. At the same time, the coating layer's ability to inhibit lithium dendrite growth also fails to meet expectations.

[0172] Comparative analysis of data from Example 1 and Comparative Example 2 reveals that the ball milling process of this invention, utilizing a solvent-free mechanical force field, achieves both uniform dispersion and appropriate surface activation of the sulfide electrolyte powder. It also triggers in-situ ring-opening polymerization of fluorinated cyclic monomers on the electrolyte particle surface, ultimately constructing a continuous and dense nanoscale polymer coating layer. The entire process is solvent-free, fundamentally avoiding the chemical erosion of the electrolyte interface by organic residues. While solvent methods can also achieve monomer ring-opening polymerization, organic solvents inevitably remain on the surface and grain boundaries of the sulfide electrolyte. Even trace amounts of these residues continuously corrode the sulfide matrix, generating high-resistivity impurity phases, damaging the intrinsic structure of the electrolyte, and significantly degrading Li. + Conduction pathways. Meanwhile, polymerization reactions in the solution phase tend towards homogeneous nucleation and growth, making it difficult to precisely control the preferential concentration of polymerization sites on the electrolyte surface. This results in a weak, unevenly distributed, and poorly compact coating layer that fails to effectively suppress interfacial side reactions. Furthermore, residual solvents continuously participate in redox decomposition during long-term electrochemical cycling, generating inactive byproducts that accumulate at the interface. This intensifies interfacial polarization and causes a continuous increase in impedance, ultimately resulting in a significantly lower coulombic efficiency in the later stages of cycling compared to the stable interface obtained by the ball milling dry method. This demonstrates the inherent limitations of solvent-based methods in terms of interfacial stability and long-term cycling reliability.

[0173] Analysis of the data from Examples 1 and 12-15 reveals that, during the ball milling process, a relatively low milling speed of 100 rpm to 400 rpm is necessary to achieve better uniform dispersion and moderate surface activation of the sulfide electrolyte powder. This allows for the activation of in-situ ring-opening polymerization of fluorinated cyclic monomers through gentle mechanical force, constructing a continuous and complete nanoscale dense coating layer on the electrolyte particle surface. Conversely, excessively high milling speeds lead to intense mechanical impact and shearing, exacerbating lattice breakage and particle pulverization of the sulfide matrix, resulting in a significant decrease in the intrinsic ionic conductivity of the electrolyte. Furthermore, it easily damages the already formed polymer coating film, causing uneven coating and increased interface defects. Conversely, excessively slow milling speeds provide insufficient mechanical activation energy, making it difficult to effectively trigger monomer ring-opening polymerization and form a complete and effective coating modification layer.

[0174] Analysis of the data from Examples 1, 1, and 3 shows that the composite sulfide solid electrolyte provided by this invention has a fluoropolymer coating layer with a special bonding method. In-situ polymerization using ball milling at the nucleophilic sites on the surface of the sulfide solid electrolyte results in a dense fluoropolymer modified layer that is firmly covalently bonded to the electrolyte matrix and uniformly and completely coated. Compared with direct physical coating of polymers, the in-situ polymerization coating of this invention achieves a tight bond between the coating layer and the matrix at the molecular level, effectively solving the problems of weak interfacial bonding, easy peeling and detachment of the coating layer, and high interfacial contact impedance associated with physical adsorption coating. During cycling, it maintains the integrity of the coating structure, more persistently blocks external moisture erosion, inhibits interfacial side reactions, and significantly improves the air stability and electrochemical cycling performance of the sulfide solid electrolyte.

[0175] The above description is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention fall within the protection and disclosure scope of the present invention.

Claims

1. A composite sulfide solid-state electrolyte, characterized by, The composite sulfide solid electrolyte includes a sulfide solid electrolyte matrix and a fluoropolymer coating layer covering the surface of the sulfide solid electrolyte matrix. The fluoropolymer coating layer is connected to the sulfide solid electrolyte matrix via SC covalent bonds.

2. The composite sulfide solid-state electrolyte according to claim 1, characterized in that, The fluoropolymer coating layer includes any one or a combination of at least two of fluoropolymers, fluoropolyethers, or fluoropolyesters.

3. A method for preparing a composite sulfide solid electrolyte as described in claim 1 or 2, characterized in that, The preparation method includes the following steps: The sulfide solid electrolyte matrix to be coated and the fluorine-containing monomer are mixed and ball-milled under a protective atmosphere. During the ball milling process, the fluorine-containing monomer completes in-situ polymerization on the surface of the sulfide solid electrolyte matrix to be coated, thus obtaining the composite sulfide solid electrolyte.

4. The preparation method according to claim 3, characterized in that, The mass ratio of the fluorine-containing monomer to the sulfide solid electrolyte matrix to be coated is 1:(1~20).

5. The preparation method according to claim 3, characterized in that, The fluorinated monomers include fluorinated cyclic monomers; And / or, the boiling point range of the fluorinated monomer is 40℃~300℃; And / or, the mass percentage of fluorine in the fluorinated monomer is 20% to 60%.

6. The preparation method according to claim 5, characterized in that, The fluorinated monomers include any one or a combination of at least two of the following: 3,3,3-trifluoropropylene carbonate, difluoroethylene carbonate, epifluoropropane, 3,3-bis(fluoromethyl)oxetane, α-(trifluoromethyl)-γ-butyrolactone, or tetrafluoroethane-β-sulfolactone.

7. The preparation method according to claim 3, characterized in that, The ball milling process is performed at a speed of 100 rpm to 400 rpm for a duration of 0.5 h to 10 h.

8. The preparation method according to claim 3, characterized in that, The ball milling process includes continuous ball milling or intermittent ball milling. And / or, the in-situ polymerization includes in-situ ring-opening polymerization; And / or, after the ball milling process is completed, a drying process is performed to obtain the composite sulfide solid electrolyte.

9. A battery, characterized in that, The battery includes the composite sulfide solid electrolyte as described in claim 1 or 2, or the composite sulfide solid electrolyte prepared by the preparation method described in any one of claims 3-8.

10. The battery according to claim 9, characterized in that, The battery includes an all-solid-state battery, which includes an all-solid-state lithium metal battery.