Sodium ion solid-state composite electrolyte membrane, preparation method thereof and solid-state sodium ion battery

By constructing a three-phase synergistic structure of oxide continuous phase + polymer binder phase + glass fiber reinforcing phase on a glass fiber skeleton, the problem of balancing conductivity and mechanical properties in NASICON-type sodium ion solid electrolytes is solved, and the large-scale production of sodium ion solid composite electrolyte membranes with high ionic conductivity and mechanical strength is realized.

CN123162292APending Publication Date: 2026-11-24HCB BATTERY CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611376662.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-07
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing NASICON-type sodium-ion solid electrolytes suffer from difficulties in achieving synergistic growth in conductivity and mechanical properties, poor processing performance of oxide electrolyte slurries, and complex processes, making it impossible to overcome the challenges of achieving high ionic conductivity, high mechanical strength, low production cost, and scalable mass production.

Method used

A three-phase synergistic structure of oxide continuous phase + polymer binder phase + glass fiber reinforced phase was constructed by using glass fiber as the skeleton and solid electrolyte filler inside and on the surface. Sodium ion solid composite electrolyte membrane was prepared by stepwise ball milling and slit coating process.

Benefits of technology

It achieves good particle dispersion under high oxide filling, while also possessing excellent ionic conductivity and mechanical strength, reducing manufacturing costs, making it suitable for large-scale production, and exhibiting high film density and excellent thickness uniformity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The application relates to a sodium ion solid-state composite electrolyte film and a preparation method thereof and a solid-state sodium ion battery. The sodium ion solid-state composite electrolyte film comprises a glass fiber framework and a solid-state electrolyte filler; the solid-state electrolyte filler is filled in the pores of the glass fiber framework and adheres to at least one side surface of the glass fiber framework; and the solid-state electrolyte filler comprises an oxide solid-state electrolyte, a dispersing agent, a nano inorganic material, a polymer material, a film-forming additive, a plasticizer and a sodium salt. The sodium ion solid-state composite electrolyte film prepared by taking the glass fiber as the framework and filling the solid-state electrolyte filler on the glass fiber has excellent ionic conductivity, meanwhile, has excellent film layer strength and flexibility, and the preparation process has low energy consumption, can be fully adapted to an existing process production line, and has the feasibility of large-scale landing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of solid-state battery technology, specifically to composite solid-state electrolyte membranes, and more particularly to a sodium-ion solid-state composite electrolyte membrane, its preparation method, and a solid-state sodium-ion battery. Background Technology

[0002] Solid-state sodium-ion batteries, with their core advantages of abundant sodium resources, low cost, and inherent safety, have become the most promising next-generation electrochemical energy storage technology in the field of large-scale energy storage. Sodium-ion solid electrolytes, as the core component of solid-state sodium-ion batteries, directly determine the battery's electrochemical performance, safety performance, and manufacturing cost. Among them, NASICON-type oxide electrolytes (such as sodium zirconium silicon phosphate) are the mainstream research direction for oxide-based sodium-ion solid electrolytes due to their high room-temperature ionic conductivity, wide electrochemical window, and excellent thermal stability.

[0003] Currently, NASICON-type sodium-ion solid electrolytes mainly include three mainstream technical solutions: pure oxide ceramic electrolytes, oxide-polymer composite electrolytes, and porous oxide framework composite solutions. Pure ceramic electrolytes have high room temperature conductivity, but the material is inherently brittle, making ultra-thin processing extremely difficult and preventing continuous roll-to-roll production. Furthermore, the interface with the electrode is a hard contact with high interfacial impedance. Pure ceramic electrolytes also suffer from high sintering costs and processing difficulties. Traditional composite electrolytes have good flexibility and are easy to process, but the oxide filling amount is low, failing to reach the ion conduction percolation threshold, and the room temperature ion conductivity is generally only 10. -6 ~10 -5 The S / cm ratio cannot meet the rate performance requirements of power batteries, and the particle agglomeration is serious under high oxide filling, which deteriorates the slurry processing performance. The porous oxide skeleton solution relies on high-temperature sintering to prepare a three-dimensional skeleton, which has a long process flow, high energy consumption, low yield of large-area preparation, and poor flexibility of ceramic skeleton, making it unsuitable for continuous roll-to-roll production lines.

[0004] CN118367223A discloses a Na 3+ax M x Zr 2-x Si2PO 12 Nanofiber ceramic electrolytes are prepared by electrospinning precursor fibers, followed by high-temperature crystallization. This preparation method offers advantages such as low sintering temperature and adjustable nanofiber aspect ratio, resulting in nanofiber ceramic electrolytes with high sodium ion conductivity.

[0005] CN115189014A discloses a composite electrolyte membrane based on a sodium ion sulfide solid electrolyte. The composite electrolyte membrane is obtained by uniformly mixing a polymer, sodium salt, and sodium ion sulfide solid electrolyte in a solvent, followed by heating to evaporate the solvent. This composite electrolyte membrane combines an inorganic electrolyte with a polymer electrolyte, reducing the interfacial impedance of the solid-state battery. However, it exhibits low ionic conductivity at room temperature and can only be produced in small batches, raising concerns about its industrial feasibility.

[0006] CN116207339A discloses a solid electrolyte membrane. A solid electrolyte is coated onto ceramic fibers, vacuum dried, and then pressurized to obtain the solid electrolyte membrane. This solid electrolyte membrane has a low interfacial impedance, but the process remains cumbersome.

[0007] The existing NASICON-type sodium-ion solid electrolyte still suffers from problems such as difficulty in achieving synergistic growth in conductivity and mechanical properties, poor processing performance of oxide electrolyte slurry, and complex processes, making it impossible to break through the four core indicators of "high ionic conductivity, high mechanical strength, low production cost, and scalable mass production".

[0008] Therefore, there is an urgent need to develop a sodium-ion solid electrolyte membrane with excellent electrical conductivity and mechanical properties, good particle dispersion under high oxide filling, and a process suitable for mass production. Summary of the Invention

[0009] To address the shortcomings of existing technologies, the purpose of this application is to provide a sodium-ion solid-state composite electrolyte membrane, its preparation method, and a solid-state sodium-ion battery. This application uses glass fiber as a skeleton and sets solid electrolyte fillers inside and on its surface to construct a three-phase synergistic structure of "oxide continuous phase + polymer binder phase + glass fiber reinforced phase", which makes the sodium-ion solid-state composite electrolyte membrane have excellent ionic conductivity, while also having excellent membrane strength and flexibility.

[0010] To achieve this objective, the present application adopts the following technical solution: In a first aspect, this application provides a sodium ion solid-state composite electrolyte membrane, the sodium ion solid-state composite electrolyte membrane comprising a glass fiber skeleton and a solid electrolyte filler; the solid electrolyte filler fills the pores of the glass fiber skeleton and is attached to at least one side surface of the glass fiber skeleton; the solid electrolyte filler comprises an oxide solid electrolyte, a dispersant, a nano-inorganic material, a polymer material, a film-forming additive, a plasticizer, and a sodium salt.

[0011] This application uses glass fiber with high porosity as a skeleton, and sets solid electrolyte fillers inside and on the surface to construct a three-phase synergistic structure of "oxide continuous phase + polymer binder phase + glass fiber reinforced phase". The closely packed submicron oxide particles serve as the continuous main pathway for ion conduction, the polymer only fills the gaps between particles to play a binding role, and the three-dimensional skeleton of glass fiber penetrates the membrane to provide mechanical support. This makes the sodium ion solid composite electrolyte membrane have excellent ionic conductivity, while also having excellent membrane strength and flexibility.

[0012] In some embodiments, the oxide solid electrolyte includes any one or a combination of at least two of NZSP, NATP, or NAGP.

[0013] In some embodiments, the oxide solid electrolyte includes any one or a combination of at least two of Mg-Nb co-doped NZSP, Al-doped NZSP, or Y-doped NZSP.

[0014] In some embodiments, the dispersant includes any one or a combination of at least two of phosphate ester dispersants, block copolymer dispersants, silane coupling dispersants, or nonionic auxiliary dispersants. Typical but non-limiting combinations include combinations of phosphate ester dispersants and block copolymer dispersants, or combinations of silane coupling dispersants and nonionic auxiliary dispersants.

[0015] In some embodiments, the phosphate ester type dispersant includes, but is not limited to, any one or a combination of at least two of alkyl phosphate esters, polyoxyethylene ether phosphate esters, or phosphate ester modified acrylate oligomers.

[0016] In some embodiments, the block copolymer dispersant includes, but is not limited to, any one or a combination of at least two of polyurethane block copolymers, acrylate block copolymers, or styrene-maleic anhydride copolymers and their derivatives.

[0017] In some embodiments, the silane coupling dispersant includes, but is not limited to, any one or a combination of at least two of γ-aminopropyltriethoxysilane, γ-(methacryloyloxy)propyltrimethoxysilane, epoxysilane, and phenylsilane.

[0018] In some embodiments, the nonionic auxiliary dispersant includes, but is not limited to, any one or a combination of at least two of polyvinylpyrrolidone (PVP), polyethylene glycol (PEG), and sorbitan trioleate (Span-85).

[0019] In some embodiments, the nano-inorganic material includes any one or a combination of at least two of nano-alumina, nano-silica, or nano-boron nitride.

[0020] In some embodiments, the polymer material includes any one or a combination of at least two of polyvinylidene fluoride-hexafluoropropylene copolymer, polyvinylidene fluoride, polyethylene oxide, or polyacrylonitrile.

[0021] In some embodiments, the film-forming additive includes any one or a combination of at least two of sodium difluorooxalate borate, fluoroethylene carbonate, or vinylene carbonate.

[0022] In some embodiments, the plasticizer includes any one or a combination of at least two of succinic anhydride, ethylene carbonate, or propylene carbonate.

[0023] In some embodiments, the sodium salt includes any one or a combination of at least two of sodium bis(fluorosulfonyl)imide, sodium bis(trifluoromethanesulfonyl)imide, or sodium hexafluorophosphate.

[0024] In some embodiments, the mass ratio of the oxide solid electrolyte, dispersant, nano-inorganic material, polymer material, film-forming additive, plasticizer, and sodium salt in the solid electrolyte filler is (70~80):(0.5~3):(1~5):(5~15):(0.1~1):(2~10):(2~10), wherein (70~80) can be, for example, 70, 72, 75, 78, or 80; wherein (0.5~3) can be, for example, 0.5, 1, 1.5, 2, 2.5, or 3; wherein (1~5) can be, for example, 1, 2, 3, 4, or 5; wherein (5~15) can be, for example, 5, 7, 10, 12, or 15; wherein (0.1~1) can be, for example, 0.1, 0.3, 0.5, 0.7, or 1; and wherein (2~10) can be, for example, 2, 4, 6, 8, or 10.

[0025] In some embodiments, the D50 particle size of the oxide solid electrolyte is 0.4 μm to 0.8 μm, for example, it can be 0.4 μm, 0.45 μm, 0.5 μm, 0.55 μm, 0.6 μm, 0.65 μm, 0.7 μm, 0.75 μm or 0.8 μm.

[0026] In some embodiments, the D50 particle size of the nano-inorganic material is 20nm~50nm, for example, it can be 20nm, 21nm, 22nm, 23nm, 24nm, 25nm, 26nm, 27nm, 28nm, 29nm, 30nm, 35nm, 40nm, 45nm or 50nm, etc.

[0027] In some embodiments, the density of the sodium ion solid composite electrolyte membrane is ≥90%, for example, the density can be 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98% or 99%, etc.

[0028] In this application, the density of the sodium ion solid composite electrolyte membrane refers to the ratio of the apparent density to the true density of the sodium ion solid composite electrolyte membrane. The higher the density of the sodium ion solid composite electrolyte membrane, the lower the porosity.

[0029] In some embodiments, the total thickness of the solid electrolyte filler attached to both sides of the glass fiber skeleton is 1μm to 4μm, for example, it can be 1μm, 1.5μm, 2.0μm, 2.5μm, 3.0μm, 3.5μm or 4μm, etc.

[0030] Secondly, this application provides a method for preparing a sodium ion solid composite electrolyte membrane as described in the first aspect, the method comprising the following steps: (1) Mix oxide solid electrolyte powder, nano-inorganic material, dispersant and first solvent, and wet ball mill to obtain oxide solid electrolyte slurry; (2) The polymer material, plasticizer, sodium salt, film-forming additive and second solvent are mixed to obtain polymer solution; (3) The oxide solid electrolyte slurry described in step (1) and the polymer solution described in step (2) are mixed and dispersed in sequence in the first dispersion and the second dispersion to obtain a composite electrolyte slurry; the rotation speed of the first dispersion is less than the rotation speed of the second dispersion. (4) The composite electrolyte slurry described in step (3) is coated on the first and second surfaces opposite to the glass fiber membrane, and the resulting wet membrane is dynamically dried to obtain a sodium ion solid composite electrolyte membrane precursor. (5) The sodium ion solid composite electrolyte membrane precursor described in step (4) is subjected to hot rolling treatment to obtain the sodium ion solid composite electrolyte membrane.

[0031] This application uses NASICON-type oxide solid electrolyte as the core raw material. Through stepwise ball milling with precise particle size control, the oxide solid electrolyte is ground to a submicron-level narrow particle size distribution. The high-intensity shear of the ball mill simultaneously refines the oxide and deagglomerates the nanofillers, allowing the nanofillers to uniformly fill the gaps between oxide particles, optimizing particle size distribution and packing density. This avoids the problem of easy agglomeration of nanofillers during subsequent mixing and improves the film density and interfacial compatibility, improving the dispersion stability of high-solids slurry from the source. Combined with a low-proportion polymer binder formulation, the polymer material fills only the gaps between oxide particles to play a binding role, ensuring that the oxide forms a continuous ion-conducting network. Finally, a high-porosity glass fiber membrane is used as a three-dimensional reinforcing skeleton. A double-sided slit coating process is used to completely fill the pores of the skeleton with low-viscosity slurry. After curing, a three-phase synergistic integrated structure of "oxide continuous ion-conducting phase + polymer binder phase + glass fiber mechanical reinforcement phase" is formed. This achieves ultra-high oxide solid electrolyte filling content while also possessing excellent mechanical strength, processability, and low cost, solving the industry problem of balancing high conductivity and mass production in existing technologies.

[0032] This application involves hot rolling of the sodium-ion solid composite electrolyte membrane precursor. The hot-pressing process slightly plasticizes the polymer material, causing oxide particles to rearrange for closer packing. This further eliminates tiny residual pores within the membrane layer, improving the pore filling density of the glass fiber and the overall membrane density. Simultaneously, it corrects thickness deviations caused by coating and drying, optimizing surface smoothness. After rolling, the membrane is cooled to room temperature by cooling rollers and then wound under constant tension to obtain the final glass fiber reinforced sodium-ion solid composite electrolyte membrane. The total thickness deviation of the finished product is ≤±1μm, and the membrane density is ≥90%.

[0033] Furthermore, the preparation method provided in this application adopts a mature mass production process in this industry, which does not require the addition of special equipment, greatly reduces manufacturing costs, and has the feasibility of large-scale implementation.

[0034] In some embodiments, the first solvent in step (1) and the second solvent in step (2) each independently comprise any one or a combination of at least two of N-methylpyrrolidone, N,N-dimethylformamide, or N,N-dimethylacetamide.

[0035] In some implementations, the mixing method in step (2) includes: First, the polymer is dissolved in a second solvent and stirred for the first time. Then, a plasticizer is added and stirred for the second time. Next, a sodium salt is added and stirred for the third time. Finally, a film-forming additive is added and stirred for the fourth time.

[0036] In some embodiments, the first stirring time is 4h to 6h, for example, it can be 4h, 4.5h, 5h, 5.5h or 6h.

[0037] In some embodiments, the second stirring time is 2h to 3h, for example, it can be 2h, 2.2h, 2.5h, 2.7h or 3h.

[0038] In some embodiments, the third stirring time is 2h to 6h, for example, it can be 2h, 3h, 4h, 5h or 6h.

[0039] In some embodiments, the fourth stirring time is 1h to 2h, for example, it can be 1h, 1.2h, 1.5h, 1.7h or 2h.

[0040] In some embodiments, the temperature of the first stirring, the second stirring, the third stirring and the fourth stirring is 45°C to 65°C, for example, it can be 45°C, 50°C, 55°C, 60°C or 65°C.

[0041] This application adds a plasticizer to the polymer liquid. The purpose of this application is to use the plasticizer to insert between the polymer molecular chains, thereby weakening the intermolecular forces and increasing the upper limit of polymer solubility.

[0042] In some embodiments, the mass ratio of the mixed oxide solid electrolyte slurry to the polymer solution in step (3) is (70~85):(15~30), where (70~85) can be, for example, 70, 72, 75, 77, 80, 82 or 85; and (15~30) can be, for example, 15, 18, 20, 23, 25, 28 or 30.

[0043] In some embodiments, the D50 particle size of the oxide solid electrolyte powder in step (1) is 3μm to 5μm, for example, it can be 3μm, 3.2μm, 3.5μm, 3.7μm, 4μm, 4.2μm, 4.5μm, 4.7μm or 5μm, etc.

[0044] In some embodiments, the D50 particle size of the powder in the oxide solid electrolyte slurry of step (1) is 0.4μm~0.8μm, for example, it can be 0.4μm, 0.45μm, 0.5μm, 0.55μm, 0.6μm, 0.65μm, 0.7μm, 0.75μm or 0.8μm, etc.

[0045] In some embodiments, the solid content of the oxide solid electrolyte slurry in step (1) is 65wt% to 85wt%, for example, it can be 65wt%, 69wt%, 73wt%, 77wt%, 81wt% or 85wt%, etc.

[0046] In some embodiments, in the oxide solid electrolyte slurry of step (1), the mass ratio of oxide solid electrolyte powder, nano-inorganic material, dispersant and first solvent is (60~80):(1~5):(1~5):(15~35), wherein (60~80) can be, for example, 60, 65, 70, 75 or 80; wherein (1~5) can be, for example, 1, 2, 3, 4 or 5; wherein (15~35) can be, for example, 15, 20, 25, 30 or 35.

[0047] In some embodiments, the solid content of the polymer solution in step (2) is 45wt% to 55wt%, for example, it can be 45wt%, 46wt%, 47wt%, 48wt%, 49wt%, 50wt%, 51wt%, 52wt%, 53wt%, 54wt%, or 55wt%.

[0048] In some embodiments, in the polymer solution of step (2), the mass ratio of polymer material, plasticizer, sodium salt, film-forming additive and second solvent is (15~25):(10~20):(10~20):(0.2~2):(45~55), wherein (15~25) can be, for example, 15, 18, 20, 22 or 25; wherein (10~20) can be, for example, 10, 12, 15, 18 or 20; wherein (0.2~2) can be, for example, 0.2, 0.5, 0.8, 1, 1.2, 1.5, 1.8 or 2; wherein (45~55) can be, for example, 45, 47, 50, 52 or 55.

[0049] In some embodiments, the solid content of the composite electrolyte slurry in step (3) is 60wt% to 80wt%, for example, it can be 60wt%, 62wt%, 65wt%, 67wt%, 70wt%, 72wt%, 75wt%, 77wt% or 80wt%, etc.

[0050] In some embodiments, the first dispersion time in step (3) is 0.3h to 1h, for example, it can be 0.3h, 0.4h, 0.5h, 0.6h, 0.7h, 0.8h, 0.9h or 1h, etc., the purpose of which is to avoid the secondary agglomeration of oxide particles caused by excessively high local polymer concentration. The first dispersion speed is 500rpm to 1000rpm, for example, it can be 500rpm, 600rpm, 700rpm, 800rpm, 900rpm or 1000rpm, etc.

[0051] In some embodiments, the second dispersion time in step (3) is 1h to 4h, for example, it can be 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, or 4h, etc., and the first dispersion speed is 2000rpm to 5000rpm, for example, it can be 2000rpm, 2500rpm, 3000rpm, 3500rpm, 4000rpm, 4500rpm, or 5000rpm, etc. The purpose of the second dispersion is to uniformly coat the oxide and nanofiller particles with the polymer slurry to form a stable slurry system.

[0052] In some embodiments, the viscosity of the composite electrolyte slurry in step (3) is 100 mPa•s to 1000 mPa•s, for example, it can be 100 mPa•s, 150 mPa•s, 200 mPa•s, 250 mPa•s, 300 mPa•s, 350 mPa•s, 400 mPa•s, 450 mPa•s, 500 mPa•s, 550 mPa•s, 600 mPa•s, 650 mPa•s, 700 mPa•s, 750 mPa•s, 800 mPa•s, 850 mPa•s, 900 mPa•s, 950 mPa•s or 1000 mPa•s, etc.

[0053] This application overcomes the viscosity bottleneck of slurry with high oxide content by designing a low-proportion polymer binder formulation, allowing the polymer to fill the gaps between particles and play a binding role, ensuring that the oxides form a continuous ion conduction network, which is beneficial to ion conduction.

[0054] In some embodiments, the thickness of the glass fiber membrane in step (4) is 10μm to 60μm, for example, it can be 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, 16μm, 17μm, 18μm, 19μm, 20μm, 25μm, 30μm, 35μm, 40μm, 45μm, 50μm, 55μm or 60μm, etc.

[0055] In some embodiments, the porosity of the glass fiber membrane in step (4) is 90% to 98%, for example, it can be 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97% or 98%.

[0056] In some embodiments, the average pore size of the glass fiber membrane in step (4) is 2μm to 15μm, for example, it can be 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm or 15μm, etc.

[0057] In some embodiments, the thickness of the sodium ion solid composite electrolyte membrane precursor in step (4) is 18 μm to 65 μm, for example, it can be 18 μm, 19 μm, 20 μm, 21 μm, 22 μm, 23 μm, 24 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 55 μm, 60 μm or 65 μm, etc.

[0058] In some embodiments, the pore filling rate of the sodium ion solid composite electrolyte membrane precursor in step (4) is ≥94%, for example, the pore filling rate can be 94%, 94.5%, 95%, 95.5%, 96%, 96.5%, 97%, 97.5%, 98%, 98.5%, 99% or 99.5%, etc.

[0059] This application achieves a high pore filling rate through a slot coating process, avoiding the problem of internal pore defects in sodium ion solid composite electrolyte membranes.

[0060] In some embodiments, the thickness of the residual film on the surface of the sodium ion solid composite electrolyte membrane precursor in step (4) is 1 μm to 4 μm, for example, it can be 1 μm, 1.5 μm, 2.0 μm, 2.5 μm, 3.0 μm, 3.5 μm or 4 μm.

[0061] In some embodiments, the coating in step (4) includes slot coating.

[0062] In this application, the slit coating method includes simultaneously or sequentially coating both sides of the glass fiber membrane to obtain a wet film, followed by dynamic drying to obtain the sodium ion solid composite electrolyte membrane precursor.

[0063] This application involves coating both sides of a glass fiber membrane to obtain a wet film. The slurry from both sides penetrates into the glass fiber skeleton and merges inside the pores, completely eliminating gas-sealed bubble defects. Combined with dynamic drying, surface skinning is avoided, solvent evaporation is ensured in an orderly manner, and the crystallization and precipitation of additives and sodium salts are inhibited. Ultimately, the glass fiber pore filling rate is ≥98%, and the residual thickness on both sides is precisely controlled within 1μm~4μm, resulting in excellent membrane uniformity.

[0064] In some embodiments, during the slit coating process in step (4), the speed of the glass fiber membrane is 3m / min to 35m / min, for example, it can be 3m / min, 4m / min, 5m / min, 6m / min, 7m / min, 8m / min, 9m / min, 10m / min, 15m / min, 20m / min, 25m / min, 30m / min or 35m / min, etc.

[0065] In some embodiments, the roll surface temperature of the hot rolling process in step (5) is 70°C to 100°C, for example, it can be 70°C, 75°C, 80°C, 85°C, 90°C, 95°C or 100°C.

[0066] In some embodiments, the inter-roll linear pressure of the hot rolling process in step (5) is 0.5kN / cm to 2.5kN / cm, for example, it can be 0.5kN / cm, 0.6kN / cm, 0.7kN / cm, 0.8kN / cm, 0.9kN / cm, 1.0kN / cm, 1.1kN / cm, 1.2kN / cm, 1.3kN / cm, 1.4kN / cm, 1.5kN / cm, 1.7kN / cm, 2.0kN / cm, 2.2kN / cm or 2.5kN / cm, etc.

[0067] In some embodiments, during the hot rolling process described in step (5), the speed of the sodium ion solid composite electrolyte membrane precursor is 3m / min to 35m / min, for example, it can be 3m / min, 4m / min, 5m / min, 6m / min, 7m / min, 8m / min, 9m / min, 10m / min, 15m / min, 20m / min, 25m / min, 30m / min or 35m / min, etc.

[0068] In some embodiments, after the hot rolling treatment in step (5), the film thickness compression rate of the sodium ion solid composite electrolyte membrane precursor is 5% to 12%, for example, it can be 5%, 6%, 7%, 8%, 9%, 10%, 11% or 12%, etc.

[0069] In some implementations, the dynamic drying method described in step (4) includes: After the composite electrolyte slurry described in step (3) is coated on the first and / or second surfaces of the glass fiber membrane, the wet membrane passes through at least the first, second, third, fourth, fifth and sixth drying zones with different temperatures in sequence.

[0070] In some implementations, during the dynamic drying in step (4), the temperature of the first drying zone is 55°C to 65°C, for example, it can be 55°C, 57°C, 60°C, 62°C or 65°C.

[0071] In some embodiments, during the dynamic drying in step (4), the temperature of the second drying zone is 65°C to 75°C, for example, it can be 65°C, 67°C, 70°C, 72°C or 75°C.

[0072] In some embodiments, during the dynamic drying in step (4), the temperature of the third drying zone is 85°C to 90°C, for example, it can be 85°C, 86°C, 87°C, 88°C, 89°C or 90°C.

[0073] In some embodiments, during the dynamic drying in step (4), the temperature of the fourth drying zone is 90℃~95℃, for example, it can be 90℃, 91℃, 92℃, 93℃, 94℃ or 95℃, etc.

[0074] In some embodiments, during the dynamic drying in step (4), the temperature of the fifth drying zone is 75°C to 80°C, for example, it can be 75°C, 76°C, 77°C, 78°C, 79°C or 80°C.

[0075] In some embodiments, during the dynamic drying in step (4), the temperature of the sixth drying zone is 55°C to 60°C, for example, it can be 55°C, 56°C, 57°C, 58°C, 59°C or 60°C.

[0076] Thirdly, this application provides a solid-state sodium-ion battery, which includes a sodium-ion solid-state composite electrolyte membrane as described in the first aspect, or a sodium-ion solid-state composite electrolyte membrane prepared by the preparation method described in the second aspect.

[0077] Compared with the prior art, this application has the following advantages: (1) In this application, a glass fiber membrane is used as a skeleton, and solid electrolyte filler is filled in the pores of the skeleton. The tensile strength of the sodium ion solid composite electrolyte membrane can reach 6MPa~22MPa, which is due to the reinforcing effect of the glass fiber skeleton.

[0078] (2) The sodium ion solid composite electrolyte membrane prepared in this application exhibits excellent electrochemical performance and excellent room temperature ionic conductivity, reaching 8.9 × 10⁻⁶. -5 S / cm ~ 2.0 × 10 -4 S / cm; the electrochemical stability window is suitable for high-voltage sodium cathode materials, reaching 4.4V~4.8V; the critical current density can effectively suppress sodium dendrite growth, and the interfacial impedance is stable over a long period of time, with a critical current density of up to 0.6mA / cm. 2 ~1.3mA / cm 2 .

[0079] (3) This application achieves a pore filling rate of ≥94% through slit coating process and has no internal pore defects. The sodium ion solid composite electrolyte membrane prepared by this process has a double-sided surface thickness deviation of ≤±2.2μm and excellent membrane uniformity, which can effectively avoid sodium ion flux distortion caused by uneven thickness.

[0080] (4) The preparation method provided in this application has low energy consumption, low cost, high product yield, low solvent residue rate, and uses mature equipment in the lithium battery industry throughout the process. It is easy to modify existing production lines and is suitable for large-scale production. Detailed Implementation

[0081] The technical solution of this application will be further described below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely to help understand this application and should not be regarded as specific limitations on this application.

[0082] The scope of this application can be defined by lower and upper limits. The selected lower and upper limits define the boundaries of a specific range. The range defined in this way can be defined by the inclusion or exclusion of endpoints. Any endpoint can be independently selected for inclusion or exclusion, and all lower and upper limits can be arbitrarily combined to form new ranges. That is, any lower limit can be combined with any upper limit to form a valid range. For example, if the ranges of 60~120 and 80~110 are listed for specific parameters, it should be understood that the ranges of 60~110 and 80~120 also fall within the scope of this application. In addition, if the minimum range values ​​1 and 2 are listed, and the maximum range values ​​3, 4 and 5 are also listed, then all ranges of 1~3, 1~4, 1~5, 2~3, 2~4 and 2~5 fall within the scope of this application. In this application, the numerical range "a~b" represents a shortened representation of any combination of real numbers between a and b, where a and b are both real numbers. For example, the numerical range "0~5" means that all real numbers between 0 and 5 have been fully listed in this document, and "0~5" is only a shortened representation of this set of numerical combinations. When a parameter is expressed as an integer ≥2, it is equivalent to listing positive integers that meet the requirements, such as 2, 3, 4, 5, 6, 7, 8, 9, and 10. When a parameter is expressed as an integer selected from "2~10", it is equivalent to listing any integer among 2, 3, 4, 5, 6, 7, 8, 9, and 10.

[0083] In this application, "a combination of at least two" refers to a quantity greater than or equal to 2, unless otherwise specified. For example, "any one or a combination of at least two" means any one of the listed items can be selected, or a combination of at least two of the listed items formed in a manner that does not conflict and enables the implementation of this application. In this application, unless otherwise specified, the features or solutions corresponding to "and / or" cover any one of two or more related listed items, as well as any and all combinations of the related listed items. The arbitrary and all combinations include any two related listed items, any more related listed items, or a combination of all related listed items. For example, "A and / or B" means a set consisting of A, B, and combinations of A and B, where "containing A and / or B" can be understood, depending on the context of the statement, as containing A, containing B, or containing both A and B. In this application, "optional" means that the corresponding feature, component, step or solution is not necessary, that is, it is selected from either "with" or "without". If there are multiple "optional" limitations in a technical solution, unless otherwise specified and there is no technical conflict or mutual constraint, each "optional" limitation is independent and does not affect the others.

[0084] In this application, technical features or solutions described using open-ended terms such as "comprising" or "including" do not exclude additional non-conflicting elements beyond those listed unless otherwise specified. They are considered to disclose both closed-ended features or solutions consisting solely of the listed elements and open-ended features or solutions that may include additional non-conflicting elements beyond the listed elements. For example, if A includes a1, a2, and a3, unless otherwise specified, this means that A can consist only of a1, a2, and a3, or it can include other non-conflicting elements based on a1, a2, and a3. This corresponds to the disclosure of technical solutions such as "A consists of a1, a2, and a3," "A is selected from a1, a2, and a3," and "A not only includes a1, a2, and a3, but may also include other non-conflicting elements." All embodiments and optional embodiments of this application, unless otherwise specified and without technical conflict, can be combined to form new technical solutions, and such combinations fall within the scope of this application. The term "embodiment" as used in this application means that a specific feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment or implementation of this application. The appearance of this phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment mutually exclusive with other embodiments. Those skilled in the art can explicitly and implicitly understand that the embodiments described in this application can be combined with other embodiments that do not conflict with existing technologies. The ordinal numbers "first," "second," "third," and "fourth" used in this application to describe "first aspect," "second aspect," "third aspect," and "fourth aspect" are for descriptive purposes only and should not be construed as indicating or implying relative importance or quantity, nor should they be construed as implicitly specifying the importance or quantity of the indicated technical features. They serve only as a non-exhaustive enumeration and do not constitute a closed limitation on quantity.

[0085] In this application, the order in which the steps are written in the methods described in the various embodiments does not imply a strict execution order. The actual execution order of each step should be determined according to its function and possible internal logic. Unless otherwise specified, all steps in this application can be executed in the order they are written, or in any order without technical conflict. For example, if the method includes steps (a) and (b), it means that the method may include steps (a) and (b) executed sequentially, or it may include steps (b) and (a) executed sequentially. If the method also includes step (c), then step (c) can be added to the method in any order without conflict, including but not limited to the execution order of steps (a), (b), and (c), steps (a), (c), and (b).

[0086] The numerical range described in this application includes not only the point values ​​listed above, but also any point values ​​within the numerical ranges not listed above. Due to space limitations and for the sake of brevity, this application will not exhaustively list the specific point values ​​included in the range.

[0087] Example 1 This embodiment provides a sodium ion solid composite electrolyte membrane, comprising a glass fiber skeleton and a solid electrolyte filler. The solid electrolyte filler fills the pores of the glass fiber skeleton and is attached to both sides of the glass fiber skeleton. The solid electrolyte filler includes oxide solid electrolyte, dispersant, nano-inorganic material, polymer material, film-forming additive, plasticizer and sodium salt.

[0088] This embodiment also provides a method for preparing the above-mentioned sodium ion solid composite electrolyte membrane, including the following steps: (1) In the oxide solid electrolyte slurry, the mass ratio of dispersant, nano-inorganic material, oxide solid electrolyte powder and first solvent is 2:4:66:28. NMP is used as the first solvent. Zirconia grinding balls are used to add Mg-Nb co-doped NZSP powder, nano alumina and dispersant BYK-110 into a planetary liquid phase ball mill. The D50 particle size of the powder after grinding is controlled to be 0.55μm. Liquid phase pulverization and mixing are carried out at 25℃~30℃ for 8h to obtain an oxide solid electrolyte slurry with a solid content of 72%. The initial D50 particle size of Mg-Nb co-doped NZSP powder is 4.5μm and the D50 particle size of nano alumina is 30nm.

[0089] (2) According to the mass ratio of polymer material, plasticizer, sodium salt, film-forming additive and second solvent in the polymer solution, which is 18:16:15:0.5:50.5, and using NMP as the second solvent, PVDF-HFP was first added to the stirred tank and pre-swelled for 5 hours under constant temperature stirring at 60°C; then the plasticizer succinate was added and the mixture was kept warm and stirred for 2.5 hours; sodium salt NaFSI was added and the mixture was kept warm and stirred for 4 hours until completely dissolved; finally, film-forming additive NaDFOB was added and the mixture was kept warm and stirred for 1.5 hours until uniformly dissolved, resulting in a uniform, transparent, gel-free polymer solution with a solid content of 49.5%.

[0090] (3) Preparation of composite electrolyte slurry: The oxide solid electrolyte slurry of step (1) and the polymer liquid of step (2) are mixed in a mass ratio of 75:25. First, it is pre-dispersed at a low speed of 700 rpm for 0.5 h, and then homogenized at a high speed of 4000 rpm for 2 h. Then, it is transferred to a vacuum degassing tank and degassed for 25 min under a vacuum degree ≥ -0.095 MPa and 25℃ to obtain a uniform low viscosity composite electrolyte slurry.

[0091] The solid content of the composite electrolyte slurry at 25℃ is 66.4wt%, and the viscosity is 480mPa•s.

[0092] In the solid electrolyte filler, the mass ratio of Mg-Nb co-doped NZSP, BYK-110, PVDF-HFP, NaFSI, nano-alumina, succinic acid, and NaDFOB is 74.6:2.3:6.8:5.6:4.5:6:0.2.

[0093] (4) Coating and film formation: Electronic grade alkali-free glass fiber membrane is used as a three-dimensional reinforcing skeleton. The composite electrolyte slurry prepared in step (3) is filtered through a 300-mesh filter and sent to a slot coating equipment to be coated on the upper and lower surfaces of the glass fiber membrane. The coating speed is controlled at 6m / min. After coating, the wet film is dynamically dried for 12min to remove organic solvents and residual moisture step by step. Finally, the sodium ion solid composite electrolyte membrane precursor is obtained by winding.

[0094] The total thickness of the sodium ion solid composite electrolyte membrane precursor is 30 μm, and the total thickness of the solid electrolyte fillers attached to both sides of the glass fiber skeleton is controlled at 2.5 μm, with a glass fiber porosity of 98.3%. The glass fiber membrane itself is an electronic-grade alkali-free glass fiber membrane with a thickness of 25 μm, a porosity of 92%, and an average pore size of 5 μm. Dynamic drying parameters: 60℃→70℃→88℃→92℃→78℃→58℃.

[0095] (5) Hot rolling treatment: The sodium ion solid composite electrolyte membrane precursor dried in step (4) is fed into a twin-roll hot rolling mill for online rolling and compaction. The roll surface temperature is controlled at 85℃, the inter-roll linear pressure is 1.5kN / cm, the rolling speed is 4m / min, and the film thickness compression rate is controlled at 8%. After rolling, the membrane is cooled to room temperature by a cooling roller and then wound up under constant tension to obtain the sodium ion solid composite electrolyte membrane.

[0096] The sodium ion solid composite electrolyte membrane provided in this embodiment has a total thickness deviation of ≤ ±0.8 μm and a membrane density of 96.5%.

[0097] Example 2 This embodiment provides a sodium ion solid composite electrolyte membrane, comprising a glass fiber skeleton and a solid electrolyte filler. The solid electrolyte filler fills the pores of the glass fiber skeleton and is attached to both sides of the glass fiber skeleton. The solid electrolyte filler includes oxide solid electrolyte, dispersant, nano-inorganic material, polymer material, film-forming additive, plasticizer and sodium salt.

[0098] This embodiment also provides a method for preparing the above-mentioned sodium ion solid composite electrolyte membrane, including the following steps: (1) In the oxide solid electrolyte slurry, the mass ratio of dispersant, nano-inorganic material, oxide solid electrolyte powder and first solvent is 2:2:76:20. DMF is used as the first solvent. Al-doped NZSP powder, nano-silica and dispersant BYK-163 are added to a planetary liquid phase ball mill to control the D50 particle size of the powder after grinding to be 0.50μm. Liquid phase pulverization and mixing are carried out at 25℃~30℃ for 10h to obtain an oxide solid electrolyte slurry with a solid content of 80%. The initial D50 particle size of Al-doped NZSP powder is 4.0μm and the D50 particle size of nano-silica is 25nm.

[0099] (2) According to the mass ratio of polymer material, plasticizer, sodium salt, film-forming additive and second solvent in the polymer solution, it is 18:16:15:0.5:50.5. DMF is used as the second solvent. First, PEO is added to the stirring tank and pre-swelled for 6 hours under constant temperature stirring at 65°C. Then, plasticizer EC is added and the temperature is maintained and stirred for 3 hours. Sodium salt NaTFSI is added and the temperature is maintained and stirred for 4 hours until completely dissolved. Finally, film-forming additive FEC is added and the temperature is maintained and stirred for 1.5 hours until uniformly dissolved, resulting in a uniform, transparent, gel-free polymer solution with a solid content of 49.5%.

[0100] (3) Preparation of composite electrolyte slurry: The oxide solid electrolyte slurry of step (1) and the polymer liquid of step (2) are mixed in a mass ratio of 75:25. First, it is pre-dispersed at a low speed of 700 rpm for 0.5 h, and then homogenized at a high speed of 4000 rpm for 2 h. Then, it is transferred to a vacuum degassing tank and degassed for 20 min under a vacuum degree ≥ -0.095 MPa and 25℃ to obtain a uniform low viscosity composite electrolyte slurry.

[0101] The solid content of the composite electrolyte slurry at 25℃ is 72.4wt%, and the viscosity is 550mPa•s.

[0102] In the solid electrolyte filler, the mass ratio of Al-doped NZSP, BYK-163, PEO, NaTFSI, nano-silica, EC and FEC is 78.8:2.1:6.2:5.2:2.1:5.4:0.2.

[0103] (4) Coating and film formation: Electronic grade alkali-free glass fiber membrane is used as a three-dimensional reinforcing skeleton. The composite electrolyte slurry prepared in step (3) is filtered through a 300-mesh filter and sent to a slot coating equipment to be coated on the upper and lower surfaces of the glass fiber membrane. The coating speed is controlled at 5m / min. After coating, the wet film is dynamically dried for 13min to remove organic solvents and residual moisture step by step. Finally, the sodium ion solid composite electrolyte membrane precursor is obtained by winding.

[0104] The total thickness of the sodium-ion solid composite electrolyte membrane precursor is 36 μm, and the total thickness of the solid electrolyte fillers attached to both sides of the glass fiber skeleton is controlled at 3.0 μm, with a glass fiber porosity of 97.6%. The glass fiber membrane itself is an electronic-grade alkali-free glass fiber membrane with a thickness of 30 μm, a porosity of 90%, and an average pore size of 6 μm. Dynamic drying parameters: 58℃→68℃→86℃→91℃→77℃→56℃.

[0105] (5) Hot rolling treatment: The sodium ion solid composite electrolyte membrane precursor dried in step (4) is fed into a twin-roll hot rolling mill for online rolling and compaction. The roll surface temperature is controlled at 80℃, the inter-roll linear pressure is 1.2kN / cm, the rolling speed is 5m / min, and the film thickness compression rate is controlled at 7%. After rolling, the membrane is cooled to room temperature by a cooling roller and then wound up under constant tension to obtain the sodium ion solid composite electrolyte membrane.

[0106] The sodium ion solid composite electrolyte membrane provided in this embodiment has a total thickness deviation of ≤ ±0.9 μm and a membrane density of 95.8%.

[0107] Example 3 This embodiment provides a sodium ion solid composite electrolyte membrane, comprising a glass fiber skeleton and a solid electrolyte filler. The solid electrolyte filler fills the pores of the glass fiber skeleton and is attached to both sides of the glass fiber skeleton. The solid electrolyte filler includes oxide solid electrolyte, dispersant, nano-inorganic material, polymer material, film-forming additive, plasticizer and sodium salt.

[0108] This embodiment also provides a method for preparing the above-mentioned sodium ion solid composite electrolyte membrane, including the following steps: (1) In the oxide solid electrolyte slurry, the mass ratio of dispersant, nano-inorganic material, oxide solid electrolyte powder and first solvent is 2:4:63:31. DMAc is used as the first solvent. With alumina grinding balls, NATP powder, nano-boron nitride and dispersant PAA are added to a planetary liquid phase ball mill. The D50 particle size of the powder after grinding is controlled to be 0.65μm. Liquid phase pulverization and mixing are carried out at 25℃~30℃ for 7h to obtain an oxide solid electrolyte slurry with a solid content of 69%. The initial D50 particle size of NATP powder is 5.0μm and the D50 particle size of nano-boron nitride is 40nm.

[0109] (2) According to the mass ratio of polymer material, plasticizer, sodium salt, film-forming additive and second solvent in the polymer solution, which is 22:16:15:1:46, DMAc is used as the second solvent. First, PAN is added to the stirring tank and pre-swelled for 4.5h under constant temperature stirring at 55℃. Then, plasticizer PC is added and the temperature is kept warm and stirred for 2h. Sodium salt NaPF6 is added and the temperature is kept warm and stirred for 4.5h until completely dissolved. Finally, film-forming additive VC is added and the temperature is kept warm and stirred for 1h until uniformly dissolved, resulting in a uniform, transparent, gel-free polymer solution with a solid content of 54%.

[0110] (3) Preparation of composite electrolyte slurry: The oxide solid electrolyte slurry of step (1) and the polymer liquid of step (2) are mixed in a mass ratio of 78:22. First, it is pre-dispersed at a low speed of 700 rpm for 0.5 h, and then homogenized at a high speed of 4000 rpm for 1.5 h. Then it is transferred to a vacuum degassing tank and degassed for 15 min under vacuum degree ≥ -0.095 MPa and 25℃ to obtain a uniform low viscosity composite electrolyte slurry.

[0111] The solid content of the composite electrolyte slurry at 25℃ is 65.7wt%, and the viscosity is 390mPa•s.

[0112] In the solid electrolyte packing, the mass ratio of NATP, PAA, PAN, NaPF6, nano boron nitride, PC and VC is 74.8:2.4:7.4:5:4.7:5.4:0.3.

[0113] (4) Coating and film formation: Electronic grade alkali-free glass fiber membrane is used as a three-dimensional reinforcing skeleton. The composite electrolyte slurry prepared in step (3) is filtered through a 300-mesh filter and sent to a slot coating equipment to be coated on the upper and lower surfaces of the glass fiber membrane. The coating speed is controlled at 8m / min. After coating, the wet film is dynamically dried for 9min to remove organic solvents and residual moisture step by step. Finally, the sodium ion solid composite electrolyte membrane precursor is obtained by winding.

[0114] The total thickness of the sodium-ion solid composite electrolyte membrane precursor is 20 μm, and the total thickness of the solid electrolyte fillers attached to both sides of the glass fiber skeleton is controlled at 2.5 μm, with a glass fiber porosity of 97.2%. The glass fiber membrane itself is an electronic-grade alkali-free glass fiber membrane with a thickness of 15 μm, a porosity of 95%, and an average pore size of 4 μm. Dynamic drying parameters: 62℃→72℃→89℃→94℃→79℃→59℃.

[0115] (5) Hot rolling treatment: The sodium ion solid composite electrolyte membrane precursor dried in step (4) is fed into a twin-roll hot rolling mill for online rolling and compaction. The roll surface temperature is controlled at 90°C, the inter-roll linear pressure is 2.0 kN / cm, the rolling speed is 2 m / min, and the film thickness compression rate is controlled at 10%. After rolling, the membrane is cooled to room temperature by a cooling roller and then wound up under constant tension to obtain the sodium ion solid composite electrolyte membrane.

[0116] The sodium ion solid composite electrolyte membrane provided in this embodiment has a total thickness deviation of ≤ ±0.7 μm and a membrane density of 97.2%.

[0117] Example 4 This embodiment provides a sodium ion solid composite electrolyte membrane, comprising a glass fiber skeleton and a solid electrolyte filler. The solid electrolyte filler fills the pores of the glass fiber skeleton and is attached to both sides of the glass fiber skeleton. The solid electrolyte filler includes oxide solid electrolyte, dispersant, nano-inorganic material, polymer material, film-forming additive, plasticizer and sodium salt.

[0118] This embodiment also provides a method for preparing the above-mentioned sodium ion solid composite electrolyte membrane, including the following steps: (1) In the oxide solid electrolyte slurry, the mass ratio of dispersant, nano-inorganic material, oxide solid electrolyte powder and first solvent is 2:3:68:27. NMP is used as the first solvent. NZSP powder, nano-alumina and dispersant PVP are added to a planetary liquid phase ball mill and ground to control the D50 particle size of the powder to be 0.60μm. The mixture is liquid-phase pulverized and mixed at 25℃~30℃ for 9h to obtain an oxide solid electrolyte slurry with a solid content of 73%. The initial D50 particle size of NZSP powder is 4.2μm and the D50 particle size of nano-alumina is 30nm.

[0119] (2) According to the mass ratio of polymer material, plasticizer, sodium salt, film-forming additive and second solvent in the polymer solution, which is 25:14:14:0.5:46.5, and using NMP as the second solvent, PVDF-HFP was first added to the stirred tank and pre-swelled for 5.5 h under constant temperature stirring at 60℃; then the plasticizer succinate was added and the mixture was kept warm and stirred for 2.5 h; sodium salt NaFSI was added and the mixture was kept warm and stirred for 4.5 h until completely dissolved; finally, film-forming additive NaDFOB was added and the mixture was kept warm and stirred for 1.5 h until uniformly dissolved, resulting in a uniform, transparent, gel-free polymer solution with a solid content of 53.5%.

[0120] (3) Preparation of composite electrolyte slurry: The oxide solid electrolyte slurry of step (1) and the polymer liquid of step (2) are mixed in a mass ratio of 75:25. First, it is pre-dispersed at a low speed of 700 rpm for 0.5 h, and then homogenized at a high speed of 4000 rpm for 2 h. Then, it is transferred to a vacuum degassing tank and degassed for 22 min under vacuum degree ≥ -0.095 MPa and 25℃ to obtain a uniform low viscosity composite electrolyte slurry.

[0121] The solid content of the composite electrolyte slurry at 25℃ is 68.1wt%, and the viscosity is 520mPa•s.

[0122] In the solid electrolyte packing, the mass ratio of NZSP, PVP, PVDF-HFP, NaFSI, nano-alumina, succinic acid, and NaDFOB is 74.9:2.2:9.2:5.1:3.3:5.1:0.2.

[0123] (4) Coating and film formation: Electronic grade alkali-free glass fiber membrane is used as a three-dimensional reinforcing skeleton. The composite electrolyte slurry prepared in step (3) is filtered through a 300-mesh filter and sent to a slot coating equipment to be coated on the upper and lower surfaces of the glass fiber membrane. The coating speed is controlled at 7m / min. After coating, the wet film is dynamically dried for 11min to remove organic solvents and residual moisture step by step. Finally, the sodium ion solid composite electrolyte membrane precursor is obtained by winding.

[0124] The total thickness of the sodium ion solid composite electrolyte membrane precursor is 28 μm, and the total thickness of the solid electrolyte fillers attached to both sides of the glass fiber skeleton is controlled at 2.0 μm, with a glass fiber porosity of 97.9%. The glass fiber membrane itself is an electronic-grade alkali-free glass fiber membrane with a thickness of 24 μm, a porosity of 93%, and an average pore size of 4.5 μm. Dynamic drying parameters: 60℃→69℃→87℃→93℃→78℃→57℃.

[0125] (5) Hot rolling treatment: The sodium ion solid composite electrolyte membrane precursor dried in step (4) is fed into a twin-roll hot rolling mill for online rolling and compaction. The roll surface temperature is controlled at 88℃, the inter-roll linear pressure is 1.8kN / cm, the rolling speed is 3m / min, and the film thickness compression rate is controlled at 9%. After rolling, the membrane is cooled to room temperature by a cooling roller and then wound up under constant tension to obtain the sodium ion solid composite electrolyte membrane.

[0126] The sodium ion solid composite electrolyte membrane provided in this embodiment has a total thickness deviation of ≤ ±0.8 μm and a membrane density of 96.8%.

[0127] Example 5 This embodiment provides a sodium ion solid composite electrolyte membrane, comprising a glass fiber skeleton and a solid electrolyte filler. The solid electrolyte filler fills the pores of the glass fiber skeleton and is attached to both sides of the glass fiber skeleton. The solid electrolyte filler includes oxide solid electrolyte, dispersant, nano-inorganic material, polymer material, film-forming additive, plasticizer and sodium salt.

[0128] This embodiment also provides a method for preparing the above-mentioned sodium ion solid composite electrolyte membrane, including the following steps: (1) In the oxide solid electrolyte slurry, the mass ratio of dispersant, nano-inorganic material, oxide solid electrolyte powder and first solvent is 2:3:70:25. NMP / DMF mixed solvent (mass ratio 1:1) is used as the first solvent. Alumina grinding balls are used. Y-doped NZSP powder, nano-silica and dispersant BYK-110 are added to a planetary liquid phase ball mill. The D50 particle size of the powder after grinding is controlled to be 0.52μm. Liquid phase pulverization and mixing are carried out at 25℃~30℃ for 8.5h to obtain an oxide solid electrolyte slurry with a solid content of 75%. The initial D50 particle size of Y-doped NZSP powder is 4.8μm and the D50 particle size of nano-silica is 25nm.

[0129] (2) According to the mass ratio of polymer material, plasticizer, sodium salt, film-forming additive and second solvent in the polymer solution, the mass ratio is 18:20:12:0.5:49.5. Using NMP / DMF mixed solvent (mass ratio 1:1) as the second solvent, the PVDF-HFP / PEO mixed matrix (mass ratio 7:3) is first added to the stirred tank and pre-swelled for 5.5h under constant temperature stirring at 62℃; then the plasticizer succinate / EC mixture (mass ratio 1:1) is added and the mixture is kept warm and stirred for 2.5h; the sodium salt NaFSI is added and the mixture is kept warm and stirred for 4.5h until completely dissolved; finally, the film-forming additive FEC is added and the mixture is kept warm and stirred for 1.5h until uniformly dissolved, resulting in a uniform, transparent, gel-free high solids polymer solution with a solids content of 50.5%.

[0130] (3) Preparation of composite electrolyte slurry: The oxide solid electrolyte slurry of step (1) and the polymer liquid of step (2) are mixed in a mass ratio of 70:30. First, it is pre-dispersed at low speed of 600 rpm for 0.5 h, and then homogenized at high speed of 3500 rpm for 2.2 h. Then it is transferred to a vacuum degassing tank and degassed for 24 min under vacuum degree ≥ -0.095 MPa and 25℃ to obtain a uniform low viscosity composite electrolyte slurry.

[0131] The solid content of the composite electrolyte slurry at 25℃ is 67.7wt%, and the viscosity is 500mPa•s.

[0132] In the solid electrolyte filler, the mass ratio of Y-doped NZSP, BYK-110, mixed polymer material, NaFSI, nano-silica, mixed plasticizer and FEC is 72.4:2.1:8:5.3:3.1:8.9:0.2.

[0133] (4) Coating and film formation: Electronic grade alkali-free glass fiber membrane is used as a three-dimensional reinforcing skeleton. The composite electrolyte slurry prepared in step (3) is filtered through a 300-mesh filter and sent to a slot coating equipment to be coated on the upper and lower surfaces of the glass fiber membrane. The coating speed is controlled at 8m / min. After coating, the wet film is dynamically dried for 11.5min to remove organic solvents and residual moisture step by step. Finally, the sodium ion solid composite electrolyte membrane precursor is obtained by winding.

[0134] The total thickness of the sodium-ion solid composite electrolyte membrane precursor is 29 μm, and the total thickness of the solid electrolyte fillers attached to both sides of the glass fiber skeleton is controlled at 2.0 μm, with a glass fiber porosity of 98.1%. The glass fiber membrane itself is an electronic-grade alkali-free glass fiber membrane with a thickness of 25 μm, a porosity of 92%, and an average pore size of 5 μm. Dynamic drying parameters: 61℃→71℃→88℃→92℃→78℃→58℃.

[0135] (5) Hot rolling treatment: The sodium ion solid composite electrolyte membrane precursor dried in step (4) is fed into a twin-roll hot rolling mill for online rolling and compaction. The roll surface temperature is controlled at 83°C, the inter-roll linear pressure is 1.4 kN / cm, the rolling speed is 5 m / min, and the film thickness compression rate is controlled at 7.5%. After rolling, the membrane is cooled to room temperature by a cooling roller and then wound up under constant tension to obtain the sodium ion solid composite electrolyte membrane.

[0136] The sodium ion solid composite electrolyte membrane provided in this embodiment has a total thickness deviation of ≤ ±0.8 μm and a membrane density of 96.2%.

[0137] Example 6 This embodiment provides a sodium ion solid composite electrolyte membrane, comprising a glass fiber skeleton and a solid electrolyte filler. The solid electrolyte filler fills the pores of the glass fiber skeleton and is attached to both sides of the glass fiber skeleton. The solid electrolyte filler includes oxide solid electrolyte, dispersant, nano-inorganic material, polymer material, film-forming additive, plasticizer and sodium salt.

[0138] This embodiment also provides a method for preparing the above-mentioned sodium ion solid composite electrolyte membrane, including the following steps: (1) In the oxide solid electrolyte slurry, the mass ratio of dispersant, nano-inorganic material, oxide solid electrolyte powder and first solvent is 2:2:72:24. NMP is used as the first solvent. Zirconia grinding balls are used to add Mg-Nb co-doped NZSP powder, nano-alumina / nano-boron nitride mixed filler and dispersant BYK-163 into a planetary liquid phase ball mill. The D50 particle size of the powder after grinding is controlled to be 0.58μm. Liquid phase pulverization and mixing are carried out at 25℃~30℃ for 7.5h to obtain an oxide solid electrolyte slurry with a solid content of 76%. The initial D50 particle size of Mg-Nb co-doped NZSP powder is 4.5μm. The mass ratio of nano-alumina / nano-boron nitride mixed filler is 2:1, and the D50 particle sizes are 30nm and 40nm, respectively.

[0139] (2) According to the mass ratio of polymer material, plasticizer, sodium salt, film-forming additive and second solvent in the polymer solution, which is 15:13:20:0.5:51.5, and using NMP as the second solvent, PVDF-HFP was first added to the stirred tank and pre-swelled for 5 hours under constant temperature stirring at 60°C; then the plasticizer succinate was added and the mixture was kept warm and stirred for 2.5 hours; sodium salt NaTFSI was added and the mixture was kept warm and stirred for 4 hours until completely dissolved; finally, film-forming additive NaDFOB was added and the mixture was kept warm and stirred for 1.5 hours until uniformly dissolved, resulting in a uniform, transparent, gel-free polymer solution with a solid content of 48.5%.

[0140] (3) Preparation of composite electrolyte slurry: The oxide solid electrolyte slurry of step (1) and the polymer liquid of step (2) are mixed in a mass ratio of 70:30. First, it is pre-dispersed at low speed of 800 rpm for 0.5 h, and then homogenized at high speed of 4500 rpm for 2.5 h. Then it is transferred to a vacuum degassing tank and degassed for 28 min under vacuum degree ≥ -0.095 MPa and 25℃ to obtain a uniform low viscosity composite electrolyte slurry.

[0141] The solid content of the composite electrolyte slurry at 25℃ is 67.8wt%, and the viscosity is 620mPa•s.

[0142] In the solid electrolyte filler, the mass ratio of Mg-Nb co-doped NZSP, BYK-163, PVDF-HFP, NaTFSI, mixed nanofiller, succinic acid and NaDFOB is 74.4:2.1:6.6:8.8:2.1:5.8:0.2.

[0143] (4) Coating and film formation: Electronic grade alkali-free glass fiber membrane is used as a three-dimensional reinforcing skeleton. The composite electrolyte slurry prepared in step (3) is filtered through a 300-mesh filter and sent to a slot coating equipment to be coated on the upper and lower surfaces of the glass fiber membrane. The coating speed is controlled at 6m / min. After coating, the wet film is dynamically dried for 12.5min to remove organic solvents and residual moisture step by step. Finally, the sodium ion solid composite electrolyte membrane precursor is obtained by winding.

[0144] The total thickness of the sodium-ion solid composite electrolyte membrane precursor is 32 μm, and the total thickness of the solid electrolyte fillers attached to both sides of the glass fiber skeleton is controlled at 2.5 μm, with a glass fiber porosity of 98.5%. The glass fiber membrane itself is an electronic-grade alkali-free glass fiber membrane with a thickness of 27 μm, a porosity of 94%, and an average pore size of 5.5 μm. Dynamic drying parameters: 59℃→69℃→87℃→92℃→77℃→57℃.

[0145] (5) Hot rolling treatment: The sodium ion solid composite electrolyte membrane precursor dried in step (4) is fed into a twin-roll hot rolling mill for online rolling and compaction. The roll surface temperature is controlled at 87°C, the inter-roll linear pressure is 1.7 kN / cm, the rolling speed is 6 m / min, and the film thickness compression rate is controlled at 8.5%. After rolling, the membrane is cooled to room temperature by a cooling roller and then wound up under constant tension to obtain the sodium ion solid composite electrolyte membrane.

[0146] The sodium ion solid composite electrolyte membrane provided in this embodiment has a total thickness deviation of ≤±0.7μm and a membrane density of 97.0%.

[0147] Example 7 This embodiment provides a sodium ion solid composite electrolyte membrane, comprising a glass fiber skeleton and a solid electrolyte filler. The solid electrolyte filler fills the pores of the glass fiber skeleton and is attached to both sides of the glass fiber skeleton. The solid electrolyte filler includes oxide solid electrolyte, dispersant, nano-inorganic material, polymer material, film-forming additive, plasticizer and sodium salt.

[0148] This embodiment also provides a method for preparing the above-mentioned sodium ion solid composite electrolyte membrane, including the following steps: (1) In the oxide solid electrolyte slurry, the mass ratio of dispersant, nano-inorganic material, oxide solid electrolyte powder and first solvent is 2:4:67:27. DMAc is used as the first solvent. With zirconia grinding balls, NZSP / NATP mixed oxide powder, nano alumina and dispersant PAA are added to a planetary liquid phase ball mill. The D50 particle size of the powder after grinding is controlled to be 0.56μm. Liquid phase pulverization and mixing are carried out at 25℃~30℃ for 8h to obtain an oxide solid electrolyte slurry with a solid content of 73%. The mass ratio of NZSP / NATP mixed oxide powder is 7:3, the initial D50 particle size is 4.6μm, and the D50 particle size of nano alumina is 30nm.

[0149] (2) According to the mass ratio of polymer material, plasticizer, sodium salt, film-forming additive and second solvent in the polymer solution, which is 18:16:15:0.8:50.2, DMAc is used as the second solvent. First, PAN is added to the stirring tank and pre-swelled for 5 hours under constant temperature stirring at 58°C. Then, plasticizer PC is added and the temperature is maintained and stirred for 2.5 hours. Sodium salt NaPF6 is added and the temperature is maintained and stirred for 5 hours until completely dissolved. Finally, film-forming additive VC is added and the temperature is maintained and stirred for 1.5 hours until uniformly dissolved, resulting in a uniform, transparent, gel-free polymer solution with a solid content of 49.8%.

[0150] (3) Preparation of composite electrolyte slurry: The oxide solid electrolyte slurry of step (1) and the polymer liquid of step (2) are mixed in a mass ratio of 75:25. First, it is pre-dispersed at low speed of 650 rpm for 0.5 h, and then homogenized at high speed of 3000 rpm for 2 h. Then it is transferred to a vacuum degassing tank and degassed for 20 min under vacuum degree ≥ -0.095 MPa and 25℃ to obtain a uniform low viscosity composite electrolyte slurry.

[0151] The solid content of the composite electrolyte slurry at 25℃ is 67.2wt%, and the viscosity is 450mPa•s.

[0152] In the solid electrolyte filler, the mass ratio of mixed oxides, PAA, PAN, NaPF6, nano alumina, PC and VC is 74.8:2.2:6.7:5.6:4.5:5.9:0.3.

[0153] (4) Coating and film formation: Electronic grade alkali-free glass fiber membrane is used as a three-dimensional reinforcing skeleton. The composite electrolyte slurry prepared in step (3) is filtered through a 300-mesh filter and sent to a slot coating equipment to be coated on the upper and lower surfaces of the glass fiber membrane. The coating speed is controlled at 8m / min. After coating, the wet film is dynamically dried for 10min to remove organic solvents and residual moisture step by step. Finally, the sodium ion solid composite electrolyte membrane precursor is obtained by winding.

[0154] The total thickness of the sodium-ion solid composite electrolyte membrane precursor is 26 μm, and the total thickness of the solid electrolyte fillers attached to both sides of the glass fiber skeleton is controlled at 2.0 μm, with a glass fiber porosity of 97.8%. The glass fiber membrane itself is an electronic-grade alkali-free glass fiber membrane with a thickness of 22 μm, a porosity of 91%, and an average pore size of 4 μm. Dynamic drying parameters: 61℃→70℃→88℃→93℃→79℃→58℃.

[0155] (5) Hot rolling treatment: The sodium ion solid composite electrolyte membrane precursor dried in step (4) is fed into a twin-roll hot rolling mill for online rolling and compaction. The roll surface temperature is controlled at 92℃, the inter-roll linear pressure is 1.6kN / cm, the rolling speed is 4m / min, and the film thickness compression rate is controlled at 7%. After rolling, the membrane is cooled to room temperature by a cooling roller and then wound up under constant tension to obtain the sodium ion solid composite electrolyte membrane.

[0156] The sodium ion solid composite electrolyte membrane provided in this embodiment has a total thickness deviation of ≤ ±0.9 μm and a membrane density of 96.0%.

[0157] Example 8 This embodiment provides a sodium ion solid composite electrolyte membrane, comprising a glass fiber skeleton and a solid electrolyte filler. The solid electrolyte filler fills the pores of the glass fiber skeleton and is attached to both sides of the glass fiber skeleton. The solid electrolyte filler includes oxide solid electrolyte, dispersant, nano-inorganic material, polymer material, film-forming additive, plasticizer and sodium salt.

[0158] This embodiment also provides a method for preparing the above-mentioned sodium ion solid composite electrolyte membrane, including the following steps: (1) In the oxide solid electrolyte slurry, the mass ratio of dispersant, nano-inorganic material, oxide solid electrolyte powder and first solvent is 2.5:3:69.5:25. NMP is used as the first solvent. Zirconia grinding balls are used to add Mg-Nb co-doped NZSP powder, nano-alumina and dispersant BYK-110 into a planetary liquid phase ball mill. The D50 particle size of the powder after grinding is controlled to be 0.45μm. Liquid phase pulverization and mixing are carried out at 25℃~30℃ for 6h to obtain an oxide solid electrolyte slurry with a solid content of 75%. The initial D50 particle size of Mg-Nb co-doped NZSP powder is 4.0μm and the D50 particle size of nano-alumina is 30nm.

[0159] (2) According to the mass ratio of polymer material, plasticizer, sodium salt, film-forming additive and second solvent in the polymer solution, which is 18:16:15:0.5:50.5, and using NMP as the second solvent, PVDF-HFP was first added to the stirred tank and pre-swelled for 5 hours under constant temperature stirring at 60°C; then the plasticizer succinate was added and the mixture was kept warm and stirred for 2 hours; sodium salt NaFSI was added and the mixture was kept warm and stirred for 4 hours until completely dissolved; finally, film-forming additive NaDFOB was added and the mixture was kept warm and stirred for 1 hour until uniformly dissolved, resulting in a uniform, transparent, gel-free polymer solution with a solid content of 49.5%.

[0160] (3) Preparation of composite electrolyte slurry: The oxide solid electrolyte slurry of step (1) and the polymer liquid of step (2) are mixed in a mass ratio of 75:25. First, it is pre-dispersed at low speed of 800 rpm for 0.5 h, and then homogenized at high speed of 5000 rpm for 1.5 h. Then it is transferred to a vacuum degassing tank and degassed for 18 min under vacuum degree ≥ -0.095 MPa and 25℃ to obtain a uniform low viscosity composite electrolyte slurry.

[0161] The solid content of the composite electrolyte slurry at 25℃ is 68.6wt%, and the viscosity is 380mPa•s.

[0162] In the solid electrolyte filler, the mass ratio of Mg-Nb co-doped NZSP, BYK-110, PVDF-HFP, NaFSI, nano-alumina, succinic acid and NaDFOB is 76:2.7:6.6:5.4:3.3:5.8:0.2.

[0163] (4) Coating and film formation: Electronic grade alkali-free glass fiber membrane is used as a three-dimensional reinforcing skeleton. The composite electrolyte slurry prepared in step (3) is filtered through a 300-mesh filter and sent to a slot coating equipment to be coated on the upper and lower surfaces of the glass fiber membrane. The coating speed is controlled at 12m / min. After coating, the wet film is dynamically dried for 8.5min to remove organic solvents and residual moisture step by step. Finally, the sodium ion solid composite electrolyte membrane precursor is obtained by winding.

[0164] The total thickness of the sodium-ion solid composite electrolyte membrane precursor is 18 μm, and the total thickness of the solid electrolyte fillers attached to both sides of the glass fiber skeleton is controlled at 1.5 μm, with a glass fiber porosity of 97.5%. The glass fiber membrane itself is an electronic-grade alkali-free glass fiber membrane with a thickness of 15 μm, a porosity of 97%, and an average pore size of 3 μm. Dynamic drying parameters: 62℃→72℃→89℃→94℃→79℃→59℃.

[0165] (5) Hot rolling treatment: The sodium ion solid composite electrolyte membrane precursor dried in step (4) is fed into a twin-roll hot rolling mill for online rolling and compaction. The roll surface temperature is controlled at 82℃, the inter-roll linear pressure is 1.0kN / cm, the rolling speed is 2m / min, and the film thickness compression rate is controlled at 6%. After rolling, the membrane is cooled to room temperature by a cooling roller and then wound up under constant tension to obtain the sodium ion solid composite electrolyte membrane.

[0166] The sodium ion solid composite electrolyte membrane provided in this embodiment has a total thickness deviation of ≤ ±0.6 μm and a membrane density of 95.7%.

[0167] Example 9 This embodiment provides a sodium ion solid composite electrolyte membrane, comprising a glass fiber skeleton and a solid electrolyte filler. The solid electrolyte filler fills the pores of the glass fiber skeleton and is attached to both sides of the glass fiber skeleton. The solid electrolyte filler includes oxide solid electrolyte, dispersant, nano-inorganic material, polymer material, film-forming additive, plasticizer and sodium salt.

[0168] This embodiment also provides a method for preparing the above-mentioned sodium ion solid composite electrolyte membrane, including the following steps: (1) In the oxide solid electrolyte slurry, the mass ratio of dispersant, nano-inorganic material, oxide solid electrolyte powder and first solvent is 2:2:78:18. NMP is used as the first solvent. Zirconia grinding balls are used to add Mg-Nb co-doped NZSP powder, nano-alumina and dispersant BYK-110 into a planetary liquid phase ball mill. The D50 particle size of the powder after grinding is controlled to be 0.45μm. Liquid phase pulverization and mixing are carried out at 25℃~30℃ for 6h to obtain an oxide solid electrolyte slurry with a solid content of 82%. The initial D50 particle size of Mg-Nb co-doped NZSP powder is 4.0μm and the D50 particle size of nano-alumina is 30nm.

[0169] (2) According to the mass ratio of polymer material, plasticizer, sodium salt, film-forming additive and second solvent in the polymer solution, which is 18:16:15:0.5:50.5, and using NMP as the second solvent, PVDF-HFP was first added to the stirred tank and pre-swelled for 5 hours under constant temperature stirring at 60°C; then the plasticizer succinate was added and the mixture was kept warm and stirred for 2 hours; sodium salt NaFSI was added and the mixture was kept warm and stirred for 4 hours until completely dissolved; finally, film-forming additive NaDFOB was added and the mixture was kept warm and stirred for 1 hour until uniformly dissolved, resulting in a uniform, transparent, gel-free polymer solution with a solid content of 49.5%.

[0170] (3) Preparation of composite electrolyte slurry: The oxide solid electrolyte slurry of step (1) and the polymer liquid of step (2) are mixed in a mass ratio of 75:25. First, it is pre-dispersed at low speed of 800 rpm for 0.5 h, and then homogenized at high speed of 5000 rpm for 1.5 h. Then it is transferred to a vacuum degassing tank and degassed for 18 min under vacuum degree ≥ -0.095 MPa and 25℃ to obtain a uniform low viscosity composite electrolyte slurry.

[0171] The solid content of the composite electrolyte slurry at 25℃ is 68.6wt%, and the viscosity is 760mPa•s.

[0172] In the solid electrolyte filler, the mass ratio of Mg-Nb co-doped NZSP, BYK-110, PVDF-HFP, NaFSI, nano-alumina, succinic acid and NaDFOB is 79.2:2:6.1:5.1:2:5.4:0.2.

[0173] (4) Coating and film formation: Electronic grade alkali-free glass fiber membrane is used as a three-dimensional reinforcing skeleton. The composite electrolyte slurry prepared in step (3) is filtered through a 300-mesh filter and sent to a slot coating equipment to be coated on the upper and lower surfaces of the glass fiber membrane. The coating speed is controlled at 12m / min. After coating, the wet film is dynamically dried for 8.5min to remove organic solvents and residual moisture step by step. Finally, the sodium ion solid composite electrolyte membrane precursor is obtained by winding.

[0174] The total thickness of the sodium-ion solid composite electrolyte membrane precursor is 18 μm, and the total thickness of the solid electrolyte fillers attached to both sides of the glass fiber skeleton is controlled at 1.5 μm, with a glass fiber porosity of 97.5%. The glass fiber membrane itself is an electronic-grade alkali-free glass fiber membrane with a thickness of 15 μm, a porosity of 97%, and an average pore size of 3 μm. Dynamic drying parameters: 62℃→72℃→89℃→94℃→79℃→59℃.

[0175] (5) Hot rolling treatment: The sodium ion solid composite electrolyte membrane precursor dried in step (4) is fed into a twin-roll hot rolling mill for online rolling and compaction. The roll surface temperature is controlled at 82℃, the inter-roll linear pressure is 1.0kN / cm, the rolling speed is 2m / min, and the film thickness compression rate is controlled at 6%. After rolling, the membrane is cooled to room temperature by a cooling roller and then wound up under constant tension to obtain the sodium ion solid composite electrolyte membrane.

[0176] The sodium ion solid composite electrolyte membrane provided in this embodiment has a total thickness of 3.0 μm for the solid electrolyte filler attached to both sides of the glass fiber skeleton, a glass fiber pore filling rate of 94.8%, a membrane thickness compression rate of 5%, a total thickness deviation of ≤±1.5 μm for the finished sodium ion solid composite electrolyte membrane, and a membrane density of 95.3%.

[0177] Example 10 This embodiment provides a sodium ion solid composite electrolyte membrane. Except that in the preparation method of the sodium ion solid composite electrolyte membrane, step (4) dynamic drying is adjusted to the same temperature drying, the drying time is 10 min, and the drying temperature is 85℃. All other steps are the same as in Example 1.

[0178] The sodium ion solid composite electrolyte membrane provided in this embodiment has a total thickness of 2.8 μm for the solid electrolyte filler attached to both sides of the glass fiber skeleton, a glass fiber pore filling rate of 95.1%, a membrane thickness compression rate of 6.5%, a total thickness deviation of ≤±1.8 μm for the finished sodium ion solid composite electrolyte membrane, and a membrane density of 90.5%.

[0179] Example 11 This embodiment provides a sodium ion solid composite electrolyte membrane. Except that step (5) in the preparation method of the sodium ion solid composite electrolyte membrane is not hot rolling, the rest is the same as in embodiment 1.

[0180] In this embodiment, the total thickness of the solid electrolyte filler attached to both sides of the glass fiber skeleton in the sodium ion solid composite electrolyte membrane becomes 3.0 μm, the glass fiber pore filling rate becomes 95.5%, the membrane thickness compression rate becomes 0%, the total thickness deviation of the finished sodium ion solid composite electrolyte membrane becomes ≤±2.2 μm, and the membrane density becomes 88.7%.

[0181] Comparative Example 1 This comparative example provides a sodium ion solid composite electrolyte membrane. Except for the preparation method of the sodium ion solid composite electrolyte membrane, in step (3), the mass ratio of the oxide solid electrolyte slurry and the polymer adhesive is 50:50. All other aspects are the same as in Example 1.

[0182] The sodium-ion solid composite electrolyte membrane provided in this comparative example has a total thickness of 2.8 μm for the solid electrolyte filler attached to both sides of the glass fiber skeleton, a glass fiber pore filling rate of 94.7%, a membrane thickness compression rate of 8.9%, a total thickness deviation of ≤±2.2 μm for the finished sodium-ion solid composite electrolyte membrane, and a membrane density of 90.7%.

[0183] Comparative Example 2 This comparative example provides a sodium ion solid composite electrolyte membrane, comprising a PET release film and a solid electrolyte filler, wherein the solid electrolyte is attached to the release side surface of the PET release film; the solid electrolyte filler comprises oxide solid electrolyte, dispersant, nano-inorganic material, polymer material, film-forming additive, plasticizer and sodium salt.

[0184] Except for the preparation method of sodium ion solid composite electrolyte membrane, in step (4) the glass fiber membrane is changed to PET release membrane and in step (5) hot rolling treatment is not performed, the rest are the same as in Example 1.

[0185] The sodium ion solid composite electrolyte membrane provided in this comparative example has a total thickness of 30 μm, a pore filling rate of 0%, a membrane thickness compression rate of 5%, a membrane density of 91.8%, and a total thickness deviation of ≤±1.2 μm.

[0186] Performance testing The following properties of the sodium-ion solid composite electrolyte membranes provided in all the above embodiments and comparative examples were tested, including: Room temperature ionic conductivity test: The room-temperature ionic conductivity was measured using electrochemical impedance spectroscopy (EIS). A sodium-ion solid-state composite electrolyte membrane was sandwiched between two stainless steel blocking electrodes to assemble a stainless steel / electrolyte membrane / stainless steel symmetrical blocking cell. EIS measurements were performed on an electrochemical workstation at room temperature (25±1℃) with a frequency scan range of 1MHz to 0.1Hz and an AC amplitude of 10mV. The bulk resistance Rb of the electrolyte was obtained by fitting the Nyquist plot to the equivalent circuit. The ionic conductivity was calculated using the formula σ=L / (Rb×S), where L is the thickness of the electrolyte membrane and S is the effective area of ​​the electrode. At least three parallel samples were tested for each sample, and the average value was taken as the final result.

[0187] Tensile strength test: Tensile strength testing was conducted according to the Test Method for Tensile Properties of Plastic Films (GB / T1040.3). Sodium-ion solid composite electrolyte membranes were cut into dumbbell-shaped or strip-shaped standard specimens, with a specimen width of 15 mm and a gauge length of 50 mm. A universal testing machine was used to apply a uniaxial tensile load to the specimens at a tensile rate of 50 mm / min until the specimens fractured. The stress-strain curves during the tensile process were recorded, and the tensile strength was calculated using the formula σ = F. max / A calculation, where F max The maximum tensile force that the specimen can withstand before fracture is given by , and A is the initial cross-sectional area of ​​the specimen. At least five parallel samples should be tested for each formulation, and the average value should be taken as the final result.

[0188] Pore ​​filling rate test: The pore filling rate was determined by comparing the original porosity of the glass fiber skeleton with the residual porosity of the composite electrolyte membrane. The original porosity of the glass fiber skeleton was tested using the mercury intrusion porosimetry (MIP) or the gas displacement method (helium specific gravity bottle method).

[0189] Residual porosity test of composite electrolyte membrane: The sample was placed in a pore size and specific surface area analyzer, and the total pore volume and apparent density of the sample were determined by mercury intrusion porosimetry or gas adsorption. The results were calculated using the formula P=(1-ρ). app / ρ true The porosity is calculated as ρ × 100%, where ρ app For apparent density, ρ true This is the true density. The pore filling rate is calculated using the formula F = (Pskeleton - Pcomposite membrane) / Pskeleton × 100%, where Pskeleton is the original porosity of the glass fiber skeleton, and Pcomposite membrane is the residual porosity of the composite electrolyte membrane. At least three parallel samples are tested for each sample, and the average value is taken.

[0190] Electrochemical window testing: The electrochemical window was measured using linear sweep voltammetry (LSV). A sodium-ion solid-state composite electrolyte membrane was assembled into a stainless steel / electrolyte membrane / sodium metal blocked battery, with stainless steel serving as the working electrode and sodium metal as the counter and reference electrodes. A linear potential scan was performed at room temperature at a scan rate of 1 mV / s from the open-circuit potential to higher potentials on an electrochemical workstation. The current-potential response curve was recorded, and the inflection point where the current rises sharply was used to determine the oxidative decomposition potential of the electrolyte; this inflection point potential is the upper limit of the electrolyte's electrochemical window. At least three parallel samples were tested for each sample, and the average value was taken.

[0191] Critical current density test: The critical current density (CCD) was tested using a symmetrical cell method with progressively increasing current. Sodium-ion solid-state composite electrolyte membranes were assembled into sodium metal / electrolyte membrane / sodium metal symmetrical cells. Cyclic tests were performed at room temperature using a constant current charge-discharge tester, with current density increased in a stepwise manner. Each current density was cycled for 10 cycles, followed by a gradual increase in current density until a sudden voltage drop (towards 0V) or obvious signs of a short circuit appeared. The maximum current density the cell could withstand before a short circuit was defined as the critical current density. At least three parallel samples were tested for each sample, and the average value was taken.

[0192] The test results are shown in Table 1.

[0193] Table 1 The test results show that: (1) A comparison of Example 1 with Examples 2-4 and Example 9 shows that the type and content of the oxide solid electrolyte affect the room temperature ionic conductivity. In Example 9, when the oxide solid electrolyte is Mg-Nb co-doped NZSP and the oxide mass ratio is 79.2, the room temperature ionic conductivity can reach 2.0 × 10⁻⁶. -4The room temperature ionic conductivity of Example 1, with an oxide mass ratio of 74.6 and a S / cm, is 1.7 × 10⁻⁶. -4 S / cm, the room temperature ionic conductivity of Example 9 was 18% higher than that of Example 1; while in Example 4, when the oxide solid electrolyte was NZSP and the oxide mass ratio was 74.9, the room temperature ionic conductivity was 1.0 × 10⁻⁶. -4 The room temperature ionic conductivity was 8.9 × 10⁻⁶ S / cm, which was 41% lower than that in Example 1. In Example 3, when the oxide solid electrolyte was NATP and the oxide mass ratio was 74.8, the room temperature ionic conductivity was 8.9 × 10⁻⁶ S / cm. -5 The room temperature ionic conductivity was reduced by 48% compared to Example 1, with a concentration of S / cm. These results indicate that oxide solid electrolytes are the main ion conduction channel, and higher concentrations result in higher room temperature ionic conductivity. Mg-Nb co-doping modification of the oxide solid electrolyte NZSP significantly improves its room temperature ionic conductivity. Undoped NZSP and NATP systems exhibit lower room temperature ionic conductivity due to intrinsic conductivity or interface issues.

[0194] (2) A comparison between Example 1 and Example 4 shows that the polymer content has a trade-off relationship with tensile strength and room-temperature ionic conductivity. In Example 4, when the polymer material is PVDF-HFP and the polymer mass ratio is 9.2, the tensile strength can reach 22 MPa, while the tensile strength of Example 1 with a polymer mass ratio of 6.8 is 15 MPa. The tensile strength of Example 4 is 47% higher than that of Example 1; however, its critical current density is 1.2 mA / cm², which is higher than that of Example 1. 2 It decreased to 0.8 mA / cm in Example 4. 2 The above results indicate that the polymer phase is the main contributor to mechanical strength, and increasing its content can significantly enhance tensile strength. However, excessive polymer can dilute the ceramic ion conduction channels, leading to a decrease in room temperature ionic conductivity and dendrite suppression ability. Therefore, the polymer content needs to be controlled within a reasonable range.

[0195] (3) A comparison between Example 1 and Example 5 shows that increasing the plasticizer content improves ionic conductivity. In Example 5, when the plasticizer mass ratio is 8.9, the ionic conductivity reaches 1.5 × 10⁻⁶. -4 The ionic conductivity of Example 1, with a plasticizer mass ratio of 6.0 and a S / cm, is 1.7 × 10⁻⁶. -4 In Example 5, the ionic conductivity (S / cm) decreased by 12% compared to Example 1; however, its tensile strength was only 9 MPa, a decrease of 40% compared to Example 1. These results indicate that the plasticizer SN / EC can promote sodium salt dissociation and improve the ionic conductivity of the polymer phase, but excessive plasticizer softens the polymer matrix, leading to a significant decrease in room temperature mechanical strength.

[0196] (4) A comparison between Example 1 and Example 6 shows that increasing the sodium salt content and introducing the mixed nanofiller can optimize the overall electrochemical performance. In Example 6, when the NaTFSI mass ratio is 8.8 and the nano-inorganic material is a nano-alumina / nano-boron nitride mixed filler, the pore filling rate can reach 98.5%, and the room temperature ionic conductivity is 1.4 × 10⁻⁶. -4 The current density is 1.3 mA / cm, the electrochemical window is 4.7 V, and the critical current density can reach 1.3 mA / cm. 2 Example 1 showed an A / cm² value of 1.2 mA / cm². 2 The critical current density of Example 6 was increased by 8% compared to Example 1. The above results indicate that the high sodium salt content provides sufficient charge carriers, and the mixed nanofillers with different particle sizes and morphologies achieve dense filling. The two work synergistically to improve the pore filling rate, density, and interfacial contact, thereby optimizing the dendrite suppression ability and improving the electrochemical performance.

[0197] (5) A comparison between Example 1 and Example 7 shows that the NZSP / NATP mixed oxide system and PAN polymer material can broaden the electrochemical window. In Example 7, when the mass ratio of NZSP / NATP mixed oxide powder is 7:3 and the polymer material is PAN matrix, the electrochemical window can reach 4.8V. The electrochemical window of Example 1, where the polymer material is PVDF-HFP matrix, is 4.6V. The electrochemical window of Example 7 is 0.2V wider than that of Example 1. The tensile strength of Example 7 is 16MPa, which is 7% higher than that of Example 1. However, the room temperature ionic conductivity of Example 7 is 1.2×10⁻⁶. -4 The S / cm decreased by 29% compared to Example 1. The above results indicate that the nitrile groups (-C≡N) in the PAN matrix have better oxidation resistance than the CF bonds in PVDF-HFP, which can broaden the electrochemical window; the room temperature ionic conductivity of the mixed oxide system decreased due to the slight increase in the interfacial impedance between the two phases.

[0198] (6) A comparison between Example 1 and Example 8 shows that the synergistic effect of ultrafine powder grinding and high dispersant can significantly improve room temperature ionic conductivity. In Example 8, when the D50 particle size of the ground powder is 0.45 μm and the dispersant mass ratio is 2.7, the room temperature ionic conductivity can reach 1.8 × 10⁻⁶. -4 The room temperature ionic conductivity of Example 1, with a particle size D50 of 0.45 μm after grinding and a dispersant mass ratio of 2.7, is 1.7 × 10⁻⁶ S / cm. -4In Example 8, the room-temperature ionic conductivity (S / cm) was 6% higher than that of Example 1; however, Example 8 used glass fibers with a porosity of 97% and a thickness of 15 μm, resulting in a tensile strength of only 11 MPa, a 27% decrease compared to Example 1. These results indicate that ultrafine grinding increases ceramic-ceramic contact points, shortens the ion transport path, and the high dispersant reduces agglomeration. These two factors synergistically improve density and interfacial contact, thereby increasing room-temperature ionic conductivity. The reduced glass fiber thickness leads to a decrease in the mechanical load-bearing cross-section.

[0199] (7) A comparison between Example 1 and Example 9 shows that high solids content slurry can improve room temperature ionic conductivity. In Example 9, when the solids content of the oxide solid electrolyte slurry is 82% and the oxide mass ratio is 79.2, the room temperature ionic conductivity can reach 2.0 × 10⁻⁶. -4 The room temperature ionic conductivity of Example 1, with an oxide solid electrolyte slurry solid content of 66.4% and a flux ratio (S / cm), is 1.7 × 10⁻⁶. -4 In Example 9, the room-temperature ionic conductivity (S / cm) was 18% higher than that of Example 1; however, the pore filling rate of Example 9 was only 94.8%, a decrease of 3.5% compared to Example 1, the tensile strength was only 9 MPa, a decrease of 40% compared to Example 1, and the electrochemical window was only 4.4 V. These results indicate that increasing the oxide content in the high-solids slurry can lead to a tighter ceramic-ceramic contact, thereby increasing the room-temperature ionic conductivity; however, excessively high solids content in the slurry results in insufficient glass fiber pore penetration, leading to a decrease in pore filling rate, density, and mechanical properties, indicating a balance between conductivity and processability.

[0200] (8) A comparison between Example 1 and Example 10 shows that the gradient temperature drying process is crucial for density, mechanical strength, and dendrite suppression. In Example 10, after drying at 85°C for 10 min, the film density was only 90.5%, while the film density of Example 1 after gradient drying was 96.5%, a decrease of 6.2% compared to Example 1; the pore filling rate of Example 10 was 95.1%, a decrease of 3.2% compared to Example 1; the tensile strength of Example 10 was only 8 MPa, a decrease of 47% compared to Example 1; and the critical current density of Example 10 was only 0.7 mA / cm². 2 The conductivity was 42% lower than that of Example 1; the room temperature ionic conductivity of Example 10 was 1.5 × 10⁻⁶. -4 The S / cm decreased by 12% compared to Example 1. The above results indicate that isothermal drying leads to rapid skin formation on the wet film surface and internal solvent residue, resulting in a significant decrease in film density and interfacial bonding. Its impact on mechanical strength and dendrite suppression ability is far greater than its impact on bulk ionic conductivity, verifying the irreplaceable nature of gradient temperature drying.

[0201] (9) A comparison between Example 1 and Example 11 shows that hot rolling is the core process for ensuring the density, mechanical strength, and dendrite suppression ability of the composite film. The film density of Example 11 without hot rolling is only 88.7%, while the film density of Example 1 with hot rolling is 96.5%, representing a decrease of 8.1% in film density compared to Example 1. The tensile strength of Example 11 is only 6 MPa, a decrease of 60% compared to Example 1. The critical current density of Example 11 is only 0.6 mA / cm². 2 The ionic conductivity of Example 11 decreased by 50% compared to Example 1; the room temperature ionic conductivity of Example 11 was 1.4 × 10⁻⁶. -4 The S / cm decreased by 18% compared to Example 1. These results indicate that hot rolling treatment tightly bonds the glass fiber, oxide solid electrolyte, and polymer material, eliminating interfacial porosity and significantly improving density and stress transfer efficiency. Without hot rolling treatment, interfacial porosity increases, and mechanical strength and dendrite suppression ability decrease significantly, verifying the necessity of hot rolling treatment.

[0202] (10) A comparison between Example 1 and Comparative Example 1 shows that the mixing ratio of oxide slurry to polymer solution directly determines the ceramic phase content and is a key process parameter affecting overall performance. In Comparative Example 1, when the mass ratio of oxide solid electrolyte slurry to polymer solution is 50:50, the room temperature ionic conductivity is only 5.0 × 10⁻⁶. -5 The room temperature ionic conductivity of Example 1, where the mass ratio of oxide solid electrolyte slurry to polymer solution is 75:25 (S / cm), is 1.7 × 10⁻⁶. -4 The room temperature ionic conductivity of Comparative Example 1 was 71% lower than that of Example 1; the critical current density of Comparative Example 1 was only 0.5 mA / cm. 2 Compared to Example 1, the pore filling rate of Comparative Example 1 was 94.7%, a decrease of 3.6% compared to Example 1; however, the tensile strength of Comparative Example 1 reached 25 MPa, an increase of 67% compared to Example 1. The above results indicate that when the mass ratio of oxide solid electrolyte slurry to polymer solution is reduced to 50:50, the ceramic phase falls below the critical content, the main ion conduction channel breaks, and the ionic conductivity and dendrite suppression ability decrease significantly. Although the increase in polymer phase improves mechanical strength, it comes at the cost of sacrificing electrochemical performance. This verifies the rationality of the process when the mass ratio of mixed oxide solid electrolyte slurry to polymer solution is (70~85):(15~30).

[0203] (11) A comparison between Example 1 and Comparative Example 2 shows that the three-dimensional glass fiber skeleton provides dual protection for mechanical properties and ion transport. In Comparative Example 2, when the glass fiber skeleton was adjusted to a PET release film, the tensile strength was only 4 MPa, while the tensile strength of Example 1 using the glass fiber skeleton was 15 MPa. The tensile strength of Comparative Example 2 decreased by 73% compared to Example 1; the room temperature ionic conductivity of Comparative Example 2 was 1.0 × 10⁻⁶. -4 The current density (S / cm) was 41% lower than that of Example 1; the critical current density of Comparative Example 2 was 0.6 mA / cm. 2 The pore filling rate was 50% lower than that of Example 1; the pore filling rate of Comparative Example 2 was 0%. These results indicate that without a glass fiber skeleton, ceramic particles are randomly dispersed in the polymer, making it difficult to form continuous three-dimensional ion channels, and significantly reducing ionic conductivity and dendrite suppression ability. Simultaneously, without fiber reinforcement, the mechanical strength of the pure ceramic-polymer composite layer collapses, verifying the necessity of a three-dimensional glass fiber reinforced skeleton structure. In this application, the glass fiber skeleton, oxide electrolyte, and polymer material have clearly defined functions and synergistic effects, simultaneously achieving high room temperature ionic conductivity and high mechanical strength.

[0204] The applicant declares that the above description is only a specific implementation of this application, but the protection scope of this application is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in this application fall within the protection and disclosure scope of this application.

Claims

1. A sodium-ion solid composite electrolyte membrane, characterized in that, The sodium ion solid composite electrolyte membrane comprises a glass fiber skeleton and a solid electrolyte filler. The solid electrolyte filler fills the pores of the glass fiber skeleton and adheres to at least one side surface of the glass fiber skeleton; The solid electrolyte filler includes oxide solid electrolyte, dispersant, nano-inorganic material, polymer material, film-forming additive, plasticizer and sodium salt.

2. The sodium ion solid composite electrolyte membrane as described in claim 1, characterized in that, The oxide solid electrolyte includes any one or a combination of at least two of NZSP, NATP, or NAGP. And / or, the dispersant includes any one or a combination of at least two of the following: phosphate ester type dispersant, block copolymer type dispersant, silane coupling type dispersant, or nonionic auxiliary dispersant; And / or, the nano-inorganic material includes any one or a combination of at least two of nano-alumina, nano-silica, or nano-boron nitride; And / or, the polymer material includes any one or a combination of at least two of polyvinylidene fluoride-hexafluoropropylene copolymer, polyvinylidene fluoride, polyethylene oxide, or polyacrylonitrile; And / or, the film-forming additive includes any one or a combination of at least two of sodium difluorooxalate borate, fluoroethylene carbonate, or vinylene carbonate; And / or, the plasticizer includes any one or a combination of at least two of succinic anionyl succinate, ethylene carbonate, or propylene carbonate; And / or, the sodium salt comprises any one or a combination of at least two of sodium bis(fluorosulfonyl)imide, sodium bis(trifluoromethanesulfonyl)imide, or sodium hexafluorophosphate; And / or, in the solid electrolyte filler, the mass ratio of oxide solid electrolyte, dispersant, nano-inorganic material, polymer material, film-forming additive, plasticizer and sodium salt is (70~80):(0.5~3):(1~5):(5~15):(0.1~1):(2~10):(2~10).

3. The sodium ion solid-state composite electrolyte membrane as described in claim 1 or 2, characterized in that, The D50 particle size of the oxide solid electrolyte is 0.4 μm to 0.8 μm; And / or, the D50 particle size of the nano-inorganic material is 20nm~50nm; And / or, the density of the sodium ion solid composite electrolyte membrane is ≥90%; And / or, the total thickness of the solid electrolyte filler attached to both sides of the glass fiber skeleton is 1μm~4μm.

4. A method for preparing a sodium ion solid composite electrolyte membrane as described in any one of claims 1 to 3, characterized in that, The preparation method includes the following steps: (1) Mix oxide solid electrolyte powder, nano-inorganic material, dispersant and first solvent, and wet ball mill to obtain oxide solid electrolyte slurry; (2) The polymer material, plasticizer, sodium salt, film-forming additive and second solvent are mixed to obtain polymer solution; (3) The oxide solid electrolyte slurry described in step (1) and the polymer solution described in step (2) are mixed and dispersed in sequence in the first dispersion and the second dispersion to obtain a composite electrolyte slurry; the rotation speed of the first dispersion is less than the rotation speed of the second dispersion. (4) The composite electrolyte slurry described in step (3) is coated on the first and second surfaces opposite to the glass fiber membrane, and the resulting wet membrane is dynamically dried to obtain a sodium ion solid composite electrolyte membrane precursor. (5) The sodium ion solid composite electrolyte membrane precursor described in step (4) is subjected to hot rolling treatment to obtain the sodium ion solid composite electrolyte membrane.

5. The preparation method according to claim 4, characterized in that, The first solvent in step (1) and the second solvent in step (2) each independently comprise any one or a combination of at least two of N-methylpyrrolidone, N,N-dimethylformamide or N,N-dimethylacetamide; And / or, the mass ratio of the mixed oxide solid electrolyte slurry to the polymer solution in step (3) is (70~85):(15~30).

6. The preparation method according to claim 4 or 5, characterized in that, The D50 particle size of the oxide solid electrolyte powder in step (1) is 3μm~5μm; And / or, in the oxide solid electrolyte slurry of step (1), the D50 particle size of the powder is 0.4μm~0.8μm; And / or, the solid content of the oxide solid electrolyte slurry in step (1) is 65wt%~85wt%; And / or, in the oxide solid electrolyte slurry of step (1), the mass ratio of oxide solid electrolyte powder, nano-inorganic material, dispersant and first solvent is (60~80):(1~5):(1~5):(15~35); And / or, the solid content of the polymer solution in step (2) is 45wt%~55wt%; And / or, in the polymer solution described in step (2), the mass ratio of polymer material, plasticizer, sodium salt, film-forming additive and second solvent is (15~25):(10~20):(10~20):(0.2~2):(45~55); And / or, the solid content of the composite electrolyte slurry in step (3) is 60wt%~80wt%; And / or, the viscosity of the composite electrolyte slurry in step (3) is 100 mPa•s to 1000 mPa•s.

7. The preparation method according to any one of claims 4 to 6, characterized in that, The thickness of the glass fiber membrane in step (4) is 10 μm to 60 μm; And / or, the porosity of the glass fiber membrane in step (4) is 90%~98%; And / or, the average pore size of the glass fiber membrane in step (4) is 2 μm to 15 μm; And / or, the thickness of the sodium ion solid composite electrolyte membrane precursor in step (4) is 18 μm to 65 μm; And / or, the pore filling rate of the sodium ion solid composite electrolyte membrane precursor in step (4) is ≥94%.

8. The preparation method according to any one of claims 4 to 7, characterized in that, The coating in step (4) includes slot coating; And / or, the roll surface temperature of the hot rolling process in step (5) is 70℃~100℃; And / or, the inter-roll linear pressure of the hot rolling process described in step (5) is 0.5 kN / cm to 2.5 kN / cm; And / or, after the hot rolling treatment described in step (5), the film thickness compression rate of the sodium ion solid composite electrolyte membrane precursor is 5%~12%.

9. The preparation method according to any one of claims 4 to 8, characterized in that, The dynamic drying method described in step (4) includes: After the composite electrolyte slurry described in step (3) is coated on the first and / or second surfaces of the glass fiber membrane, the wet membrane passes through at least the first drying zone, the second drying zone, the third drying zone, the fourth drying zone, the fifth drying zone and the sixth drying zone with different temperatures in sequence. The temperature of the first drying zone is 55℃~65℃, the temperature of the second drying zone is 65℃~75℃, the temperature of the third drying zone is 85℃~90℃, the temperature of the fourth drying zone is 90℃~95℃, the temperature of the fifth drying zone is 75℃~80℃, and the temperature of the sixth drying zone is 55℃~60℃.

10. A solid-state sodium-ion battery, characterized in that, The solid sodium-ion battery includes a sodium-ion solid composite electrolyte membrane as described in any one of claims 1 to 3, or the solid sodium-ion battery includes a sodium-ion solid composite electrolyte membrane prepared by the preparation method described in any one of claims 4 to 9.

Citation Information

Patent Citations

  • Preparation and application of composite electrolyte membrane based on sodium ion sulfide solid electrolyte