Halide solid electrolyte, method for preparing the same, and solid-state battery
Patent Information
- Application Number
- CN202510674003.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-23
- Publication Date
- 2026-11-24
AI Technical Summary
[0003]目前,典型的三元素卤化物固体电解质的结构式为LiaMbXc(其中,X=Cl、Br或I,a、b和c满足化合价平衡),但是,LiaMbXc的抗氧化性交叉,循环过程中易发生自分解现象,与高电压正极材料会发生严重的界面反应,不能满足高能量密度正极的需求,特别是X为氯元素时上述问题更为突出
Smart Images

Figure BDA0005417231610000031 
Figure BDA0005417231610000081 
Figure BDA0005417231610000151
Abstract
Description
Technical Field
[0001] This invention relates to the field of solid-state battery technology, specifically to a halide solid electrolyte, its preparation method, and a solid-state battery. Background Technology
[0002] Lithium-ion batteries have driven the rapid development of electric vehicles, with solid-state batteries, in particular, significantly improving battery safety due to the use of solid electrolytes. Among commonly used solid electrolytes, halide solid electrolytes have attracted considerable attention due to their good chemical compatibility with the vast majority of high-energy-density cathode materials currently available.
[0003] Currently, the typical structural formula of a three-element halide solid electrolyte is Li. a M b X c (Where X = Cl, Br, or I, and a, b, and c satisfy oxidation state equilibrium), however, Li a M b X c The antioxidant properties of these halogenated solid electrolytes are inconsistent, and they are prone to self-decomposition during cycling. They also exhibit severe interfacial reactions with high-voltage cathode materials, failing to meet the requirements of high-energy-density cathodes, especially when X is chlorine. Furthermore, the electrochemical windows of most halide solid electrolytes are insufficient for practical applications. When the voltage exceeds 4.3V, these halogen elements undergo severe oxidation, leading to electrolyte degradation and increased interfacial resistance between the cathode and the electrolyte.
[0004] Many studies have focused on elemental doping to address these issues. However, improper selection of doping elements can disrupt the original crystal structure and have the opposite effect, such as compromising the stability of the original structure, reducing ionic conductivity, and decreasing the electrochemical performance of the battery. Summary of the Invention
[0005] In view of the above-mentioned technical problems existing in the prior art, the purpose of this invention is to provide a halide solid electrolyte, its preparation method and solid-state battery.
[0006] In a first aspect, the present invention provides a halide solid electrolyte comprising Li, Yb, a dopant element M, and a halogen X, wherein the dopant element M at least substitutes for a Li site, and the ionic radius of M is R. M The ionic radius of X is R. X R M / R X It is in the range of 0.255 to 0.732.
[0007] In this invention, halogen X can be a single type or a combination of two or more elements. When X is a combination of two or more elements, the ionic radius of each element should satisfy the relationship with the ionic radius of M: R M / R X The value is in the range of 0.255 to 0.732. Taking an example where M contains only one element, and X is Cl or Br, with Cl having an ionic radius of R... Cl The ionic radius of Br is R. Br The ionic radius of M is R M Then R M / R Cl Within the range of 0.255 to 0.732, and R M / R Br Within the range of 0.255 to 0.732. If M is a combination of two or more elements, each element should satisfy the above relationship.
[0008] Similarly, the dopant element M can be a single type or a combination of two or more elements. When M is a combination of two or more elements, the ionic radius of each element should satisfy the relationship with the ionic radius of X: R M / R X It is in the range of 0.255 to 0.732.
[0009] This invention relates to Li a Yb b X c (Where a, b, and c satisfy valence equilibrium) A halide solid electrolyte is formed by doping with element M. This halide solid electrolyte contains Li, Yb, dopant element M, and halogen X. This is achieved by controlling M to at least replace Li sites and controlling R... M / R X Within the range of 0.255 to 0.732, Li can be maintained without damage. a Yb b X c The original crystal form of the material is preserved, maintaining its original structure, minimizing the internal energy of the material, bringing the structure to its most stable state, and improving the material's oxidation resistance and electrical conductivity.
[0010] In this invention, Li a Yb b X c As a basic material, it has a tetrahedral stacked structure, an octahedral stacked structure, or a structure where octahedrons and tetrahedrons are stacked together. The original structure is relatively stable. However, after adding a new element M, depending on the ionic radius of M, its coordination with X will differ, potentially leading to different polyhedral shapes and affecting the coordination number of the positive ion. If R... M / R XIf the dopant is not within the scope defined in this application, or if M does not substitute for Li sites, it will destroy the original crystal structure of the material, resulting in mismatch between positive and negative ion coordination and the presence of equal impurities. At the same time, many dopants that originally had a positive effect on conductivity will be unable to exert their positive effect on improving conductivity after the structure is destroyed.
[0011] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. The technical objectives and beneficial effects of the present invention can be better achieved and realized through the following preferred technical solutions.
[0012] Preferably, the chemical formula of the halide solid electrolyte is Li. a1 Yb b1 M c1 X d1 Wherein, X = at least one of Cl, Br, or I; wherein, M substitutes for the Li site, 1.5 ≤ a1 ≤ 10, 0.1 ≤ b1 ≤ 3, 0.05 ≤ c1 ≤ 4, 1 ≤ d1 ≤ 12, R M / R X It is in the range of 0.255 to 0.414.
[0013] Preferably, the chemical formula of the halide solid electrolyte is Li. a2 Yb b2 M c2 X′ d2 Wherein, X′ = at least one of Cl, Br, or I; wherein, M simultaneously substitutes for both the Li site and the Yb site, 1.5 ≤ a² ≤ 8, 0.05 ≤ b² ≤ 3, 0.05 ≤ c² ≤ 4, 1 ≤ d² ≤ 12, R M / R X Between 0.255 and 0.732.
[0014] Preferably, the doping element M includes at least one of alkali metals, alkaline earth metals, actinides, transition metals, lanthanides, and group VA elements, and more preferably at least two of alkali metals, alkaline earth metals, actinides, transition metals, lanthanides, and group VA elements.
[0015] Preferably, the configuration entropy of the molecular formula of the halide solid electrolyte is S1, and the configuration entropy of the molecular formula of the halide solid electrolyte before doping with M is S0, where S1>S0.
[0016] The configuration entropy of the molecular formula of the halide solid electrolyte is calculated according to the following formula:
[0017]
[0018] Where Sconfig is the configuration entropy of the molecular formula; x aY represents the mole fraction of Li. b M represents the mole fraction of element Yb. d The mole fraction of element M, z c Let N1 be the mole fraction of X, N2 be the number of types of element M, and N3 be the number of types of element X.
[0019] Regarding the number of types of element X, N2, for example, if X is Cl, then N2 = 1; if X is a combination of Cl and Br, then N2 = 2. The same logic applies to the number of types of element M.
[0020] The higher the configuration entropy, the more stable the electrolyte structure, the higher the conductivity, and the better the ion mobility. This invention, through the above limitations, affects the compositional disorder and ion mobility of the solid electrolyte, significantly improving the ionic conductivity of the solid electrolyte and promoting the improvement of battery performance.
[0021] In existing technologies, the selection of element doping / substitution is often determined through extensive DOE experiments, resulting in low R&D efficiency. This invention defines the doping sites of M and the ionic radius of M as R. M The ionic radius of X is R X The relationship between the two, as well as the relationship between configurational entropy, can save a lot of DOE experiments.
[0022] In a second aspect, the present invention provides a method for preparing a halide solid electrolyte as described in the first aspect, the method comprising the following steps:
[0023] The raw materials for the halide solid electrolyte are mixed and reacted under high temperature and high pressure conditions, followed by cooling to obtain the halide solid electrolyte.
[0024] In the method of the present invention, based on the ionic radius R of M M The ionic radius R of X X The relationship between M and X can determine the types of M and X. The appropriate molar mass of each raw material can be calculated based on the configuration entropy. The material is kept under high temperature and high pressure for a period of time. During this process, different elements are fully mixed uniformly through thermal energy. Finally, the material solidifies into crystals through cooling. The material will undergo two processes: uniform nucleation and growth, and finally form the desired halide solid electrolyte material.
[0025] In one embodiment, selecting raw materials with fewer impurities and higher purity is beneficial to improving the performance of the prepared halide solid electrolyte material.
[0026] Preferably, the high temperature is 100℃~400℃.
[0027] Preferably, the high pressure is 100 Pa to 20 MPa.
[0028] Preferably, the reaction time under high temperature and high pressure conditions is 4h to 20h.
[0029] Preferably, the reaction is accompanied by stirring.
[0030] Preferably, the cooling rate is 0.5℃ / min to 20℃ / min.
[0031] Thirdly, the present invention provides a solid-state battery, wherein the solid-state battery includes the halide solid electrolyte described in the first aspect.
[0032] Compared with existing technologies, the present invention has the following beneficial effects:
[0033] This invention relates to Li a Yb b X c (Where a, b, and c satisfy valence equilibrium) A halide solid electrolyte is formed by doping with element M. This halide solid electrolyte contains Li, Yb, dopant element M, and halogen X. This is achieved by controlling M to at least replace Li sites and controlling R... M / R X Within the range of 0.255 to 0.732, Li can be maintained without damage. a Yb b X c The original crystal form of the material is preserved, maintaining its original structure, minimizing the internal energy of the material, and bringing the structure to its most stable state. This improves the material's oxidation resistance and conductivity, thereby enhancing the electrochemical performance of batteries assembled using it. Detailed Implementation
[0034] The technical solution of the present invention will be further illustrated below through specific embodiments.
[0035] In one embodiment, the present invention provides a halide solid electrolyte comprising Li, Yb, a dopant element M, and a halogen X, wherein the dopant element M at least substitutes for a Li site, and the ionic radius of M is R. M The ionic radius of X is R. X R M / R X It is in the range of 0.255 to 0.732.
[0036] In one embodiment of the present invention, R M / R X It can be in the range of 0.255 to 0.732, for example, 0.255, 0.258, 0.260, 0.265, 0.300, 0.350, 0.400, 0.450, 0.500, 0.550, 0.600, 0.650, 0.700 or 0.732, etc.
[0037] In one embodiment of the present invention, halogen X can be a single type or a combination of two or more elements. When X is a combination of two or more elements, the ionic radius of each element should satisfy the relationship with the ionic radius of M: R M / R X The value is in the range of 0.255 to 0.732. Taking an example where M contains only one element, and X is Cl or Br, with Cl having an ionic radius of R... Cl The ionic radius of Br is R. Br The ionic radius of M is R M Then R M / R Cl Within the range of 0.255 to 0.732, and R M / R Br Within the range of 0.255 to 0.732. If M is a combination of two or more elements, each element should satisfy the above relationship.
[0038] Similarly, the dopant element M can be a single type or a combination of two or more elements. When M is a combination of two or more elements, the ionic radius of each element should satisfy the relationship with the ionic radius of X: R M / R X It is in the range of 0.255 to 0.732.
[0039] One embodiment of the present invention relates to Li a Yb b X c (Where a, b, and c satisfy valence equilibrium) A halide solid electrolyte is formed by doping with element M. This halide solid electrolyte contains Li, Yb, dopant element M, and halogen X. This is achieved by controlling M to at least replace Li sites and controlling R... M / R X Within the range of 0.255 to 0.732, Li can be maintained without damage. a Yb b X c The original crystal form of the material is preserved, maintaining its original structure, minimizing the internal energy of the material, bringing the structure to its most stable state, and improving the material's oxidation resistance and electrical conductivity.
[0040] In one embodiment of the present invention, Li a Yb b X cAs a basic material, it has a tetrahedral stacked structure, an octahedral stacked structure, or a structure where octahedrons and tetrahedrons are stacked together. The original structure is relatively stable. However, after adding a new element M, depending on the ionic radius of M, its coordination with X will differ, potentially leading to different polyhedral shapes and affecting the coordination number of the positive ion. If R... M / R X If the dopant is not within the scope defined in this application, or if M does not substitute for Li sites, it will destroy the original crystal structure of the material, resulting in mismatch between positive and negative ion coordination and the presence of equal impurities. At the same time, many dopants that originally had a positive effect on conductivity will be unable to exert their positive effect on improving conductivity after the structure is destroyed.
[0041] In one embodiment, the chemical formula of the halide solid electrolyte is Li. a1 Yb b1 M c1 X d1 Wherein, X = at least one of Cl, Br, or I; wherein, M substitutes for the Li site, 1.5 ≤ a1 ≤ 10, 0.1 ≤ b1 ≤ 3, 0.05 ≤ c1 ≤ 4, 1 ≤ d1 ≤ 12, R M / R X The range is from 0.255 to 0.414. For example, a1 can be 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, or 10, etc.; b1 can be 0.1, 0.3, 0.5, 0.6, 0.8, 1, 1.2, 1.5, 1.7, 1.8, 2, 2.3, 2.6, 2.8, or 3, etc.; c1 can be 0.05, 0.08, etc. 0.1, 0.12, 0.15, 0.17, 0.2, 0.23, 0.25, 0.28, 0.3, 0.32, 0.34, 0.36, 0.38, or 4, etc.; d1 can be, for example, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10, 10.5, 11, 11.5, or 12, etc.
[0042] In one embodiment, the chemical formula of the halide solid electrolyte is Li. a2 Yb b2 M c2 X′ d2 Wherein, X′ = at least one of Cl, Br, or I; wherein, M simultaneously substitutes for both the Li site and the Yb site, 1.5 ≤ a² ≤ 8, 0.05 ≤ b² ≤ 3, 0.05 ≤ c² ≤ 4, 1 ≤ d² ≤ 12, R M / R XThe range is between 0.255 and 0.732. For example, a2 can be 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, or 8, etc.; b2 can be 0.05, 0.08, 0.1, 0.13, 0.15, 0.18, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 1, 1.2, 1.3, 1.5, 1.8, 2, 2.2, 2.4, 2.6, 2.8, or 3, etc.; c2 can be 0.05, 0.08, 0.1, 0.1, etc. 3, 0.15, 0.18, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 1, 1.2, 1.3, 1.5, 1.8, 2, 2.2, 2.4, 2.6, 2.8, 3, 3.2, 3.4, 3.5, 3.7, 3.8, or 4, etc.; d2 can be, for example, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10, 10.5, 11, 11.5, or 12, etc.
[0043] In one embodiment, the doping element M includes at least one of alkali metals, alkaline earth metals, actinides, transition metals, and lanthanides, preferably at least two of alkali metals, alkaline earth metals, actinides, transition metals, and lanthanides.
[0044] In one embodiment, the configuration entropy of the molecular formula of the halide solid electrolyte is S1, and the configuration entropy of the molecular formula of the halide solid electrolyte before doping with M is S0, where S1>S0.
[0045] The configuration entropy of the molecular formula of the halide solid electrolyte is calculated according to the following formula:
[0046]
[0047] Where Sconfig is the configuration entropy of the molecular formula; x a Y represents the mole fraction of Li. b M represents the mole fraction of element Yb. d The mole fraction of element M, z c Let N1 be the mole fraction of X, N2 be the number of types of element M, and N3 be the number of types of element X.
[0048] Regarding the number of types of element X, N2, for example, if X is Cl, then N2 = 1; if X is a combination of Cl and Br, then N2 = 2. The same logic applies to the number of types of element M.
[0049] The higher the configuration entropy, the more stable the electrolyte structure, the higher the conductivity, and the better the ion mobility. This invention, through the above limitations, affects the compositional disorder and ion mobility of the solid electrolyte, significantly improving the ionic conductivity of the solid electrolyte and promoting the improvement of battery performance.
[0050] In existing technologies, the selection of element doping / substitution is often determined through extensive DOE experiments, resulting in low R&D efficiency. This invention defines the doping sites of M and the ionic radius of M as R. M The ionic radius of X is R X The relationship between the two, as well as the relationship between configurational entropy, can save a lot of DOE experiments.
[0051] In another embodiment of the present invention, a method for preparing the halide solid electrolyte as described above is provided, the method comprising the following steps:
[0052] The raw materials for the halide solid electrolyte are mixed and reacted under high temperature and high pressure conditions, followed by cooling to obtain the halide solid electrolyte.
[0053] In one embodiment of the method of the present invention, based on the ionic radius R of M M The ionic radius R of X X The relationship between M and X can determine the types of M and X. The appropriate molar mass of each raw material can be calculated based on the configuration entropy. The material is kept under high temperature and high pressure for a period of time. During this process, different elements are fully mixed uniformly through thermal energy. Finally, the material solidifies into crystals through cooling. The material will undergo two processes: uniform nucleation and growth, and finally form the desired halide solid electrolyte material.
[0054] In one embodiment, selecting raw materials with fewer impurities and higher purity is beneficial to improving the performance of the prepared halide solid electrolyte material.
[0055] In one embodiment, the high temperature is 100℃ to 400℃, for example, it can be 100℃, 120℃, 130℃, 150℃, 160℃, 180℃, 200℃, 220℃, 240℃, 260℃, 280℃, 300℃, 325℃, 350℃, 370℃ or 400℃, etc.
[0056] In one embodiment, the high pressure is 100 Pa to 20 MPa, for example, it can be 100 Pa, 200 Pa, 300 Pa, 500 Pa, 750 Pa, 1 kPa, 1.5 kPa, 2 kPa, 3 kPa, 4 kPa, 5 kPa, 6 kPa, 7 kPa, 8 kPa, 9 kPa, 10 kPa, 15 kPa, 20 kPa, 25 kPa, 30 kPa, 35 kPa, 40 kPa, 45 kPa, 50 kPa, 55 kPa, 60 kPa, 65 kPa. kPa, 70kPa, 75kPa, 80kPa, 85kPa, 90kPa, 95kPa, 100kPa, 120kPa, 150kPa, 180kPa, 200kPa, 220kPa, 250kPa, 30 0kPa, 350kPa, 400kPa, 450kPa, 500kPa, 550kPa, 600kPa, 650kPa, 750kPa, 800kPa, 850kPa, 900kPa, 950kPa, 1M Pa, 1.2MPa, 1.5MPa, 1.7MPa, 2MPa, 2.3MPa, 2.5MPa, 2.8MPa, 3MPa, 3.3MPa, 3.6MPa, 3.8MPa, 4MPa, 4.2MPa, 4.5 MPa, 4.7MPa, 5MPa, 5.2MPa, 5.5MPa, 5.8MPa, 6MPa, 6.3MPa, 6.5MPa, 6.7MPa, 7MPa, 7.3MPa, 7.5MPa, 7.7MPa, 8M Pa, 8.2MPa, 8.4MPa, 8.6MPa, 9MPa, 9.3MPa, 9.6MPa, 10MPa, 10.5MPa, 11MPa, 11.5MPa, 12MPa, 12.5MPa, 13MPa, 13.5MPa, 14MPa, 14.5MPa, 15MPa, 15.5MPa, 16MPa, 16.5MPa, 17MPa, 17.5MPa, 18MPa, 18.5MPa, 19MPa or 20MPa, etc.
[0057] In one embodiment, the reaction time under high temperature and high pressure conditions is 4h to 20h, for example, it can be 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h or 20h.
[0058] In one embodiment, the reaction is accompanied by stirring.
[0059] In one embodiment, the cooling rate is 0.5℃ / min to 20℃ / min, for example, it can be 0.5℃ / min, 1℃ / min, 1.5℃ / min, 2℃ / min, 2.5℃ / min, 3℃ / min, 3.5℃ / min, 4℃ / min, 4.5℃ / min, 5℃ / min, 6℃ / min, 7℃ / min, 8℃ / min, 9℃ / min, 10℃ / min, 11℃ / min, 12℃ / min, 13℃ / min, 14℃ / min, 15℃ / min, 16℃ / min, 17℃ / min, 18℃ / min, 19℃ / min, or 20℃ / min, etc.
[0060] In another embodiment of the present invention, a solid-state battery is provided, wherein the solid-state battery includes the above-described halide solid electrolyte.
[0061] The numerical range described in this invention includes not only the point values listed above, but also any point values within the numerical ranges not listed above. Due to space limitations and for the sake of brevity, this invention will not exhaustively list all the specific point values included in the range.
[0062] Based on the above implementation methods, the following typical but non-limiting embodiments are provided:
[0063] Example 1
[0064] This embodiment provides a halide solid electrolyte, the chemical formula of which is Li. 3.2 Yb 1.0 Mo 0.8 Cl 7.8 In this case, Mo replaces the Li site, Mo 6+ radius R Mo and Cl - radius R cl Satisfy the following relation: R Mo / R cl =62 / 181=0.3425.
[0065] The configurational entropy of the aforementioned halide solid electrolyte is -19.57R; the molecular formula of this halide solid electrolyte before doping with M is Li₄Yb. 1.0 Cl 7.8 The configurational entropy is -21.57R.
[0066] This embodiment also provides a method for preparing the above-mentioned halide solid electrolyte, including the following steps:
[0067] The raw materials for the halide solid electrolyte were mixed evenly according to the molar ratio of LiCl:MoCl2:YbCl3 of 3.2:0.8:1.0, and then reacted at 200℃ and 200Pa pressure for 12h with stirring during the reaction. After the reaction, the mixture was cooled at a rate of 2℃ / min to obtain the halide solid electrolyte.
[0068] Example 2
[0069] This embodiment provides a halide solid electrolyte, the chemical formula of which is Li. 3.9 Yb 1.2 Bi 0.2 I 8.1 In this case, M simultaneously replaces both the Li and Yb sites, and Bi... 3+ radius R Bi and I - radius R I Satisfy the following relation: R Bi / R I =108 / 216=0.5.
[0070] The configurational entropy of the aforementioned halide solid electrolyte is -22.14R; the molecular formula of this halide solid electrolyte before doping with M is Li. 4.0 Yb 1.3 I 8.1 The configuration entropy is -22.83R.
[0071] This embodiment also provides a method for preparing the above-mentioned halide solid electrolyte, including the following steps:
[0072] The raw materials for the halide solid electrolyte were mixed evenly according to the molar ratio of LiI:BiI3:YbI3 of 3.9:0.2:1.2. The raw materials for the halide solid electrolyte were then reacted at 275°C and 600Pa pressure, with stirring during the reaction. After the reaction, the mixture was cooled at a rate of 1°C / min to obtain the halide solid electrolyte.
[0073] Example 3
[0074] This embodiment provides a halide solid electrolyte, the chemical formula of which is Li. 3.5 Yb 0.5 Mg 0.5 Cl6; where Mg substitutes for Li sites and Yb sites, Mg 2+ radius R Mg and Cl - radius R cl Satisfy the following relation: R Mg / R cl =65 / 181=0.359.
[0075] The configurational entropy of the aforementioned halide solid electrolyte is -14.44R; the molecular formula of this halide solid electrolyte before doping with M is Li. 3.75 Yb 0.75 Cl6 has a configurational entropy of -15.49R.
[0076] This embodiment also provides a method for preparing the above-mentioned halide solid electrolyte, including the following steps:
[0077] The raw materials for the halide solid electrolyte were mixed evenly according to the molar ratio of LiCl:MgCl2:YbCl3 of 3.5:0.5:0.5, and then reacted at 300℃ and 5MPa pressure for 5h with stirring during the reaction. After the reaction, the mixture was cooled at a rate of 5℃ / min to obtain the halide solid electrolyte.
[0078] Example 4
[0079] This embodiment provides a halide solid electrolyte, the chemical formula of which is Li. 3.8 Yb 1.0 Hf 1.1 Br 11.2 ; where Hf replaces the Li site and the Yb site, Hf 2+ radius R Hf and Br - radius R Br Satisfy the following relationship: RH f / R Br =75 / 195=0.405.
[0080] The configurational entropy of the aforementioned halide solid electrolyte is -32.24R; the molecular formula of this halide solid electrolyte before doping with M is Li. 4.25 Yb 1.65 Br 11.2 The configuration entropy is -34.03R.
[0081] This embodiment also provides a method for preparing the above-mentioned halide solid electrolyte, including the following steps:
[0082] The raw materials for the halide solid electrolyte were mixed uniformly at a molar ratio of LiBr:HfBr4:YbBr3 of 3.8:1.1:1.0, and then reacted at 350℃ and 5kPa pressure for 7h with stirring during the reaction. After the reaction, the mixture was cooled at a rate of 2℃ / min to obtain the halide solid electrolyte.
[0083] Example 5
[0084] This embodiment provides a halide solid electrolyte, the chemical formula of which is Li. 3.3 Yb 1.0 Mo 0.4 Mg 0.4 Cl 7.9 In this case, both Mo and Mg substitute for Li sites, with Mo... 6+ radius R Mo and Cl - radius R cl Satisfy the following relation: R Mo / R cl =62 / 181=0.3425, Mg 2+ radius R Mg And the radius R of Cl- cl Satisfy the following relation: R Mg / R cl =65 / 181=0.359.
[0085] The configurational entropy of the aforementioned halide solid electrolyte is -19.54R; the molecular formula of this halide solid electrolyte before doping with M is Li. 3.7 Yb 1.4 Cl 7.9 The configurational entropy is -21.64R.
[0086] This embodiment also provides a method for preparing the above-mentioned halide solid electrolyte, including the following steps:
[0087] The raw materials for the halide solid electrolyte were mixed evenly according to the molar ratio of LiCl:MoCl2:MgCl2:YbCl3 of 3.3:0.4:0.4:1.0, and then reacted at 325℃ and 2kPa pressure for 9h with stirring during the reaction. After the reaction, the mixture was cooled at a rate of 8℃ / min to obtain the halide solid electrolyte.
[0088] Comparative Example 1
[0089] The difference from Example 1 is that Mo is replaced with Be, that is, the Li site is replaced with Be. In this case, Be2... + radius R Be and Cl - radius R cl Satisfy the following relation: R Be / R cl =31 / 181=0.171.
[0090] Comparative Example 2
[0091] The difference from Example 1 is that Mo is replaced with K, that is, the Li site is replaced with K. In this case, K... + radius RK and Cl - radius R cl Satisfy the following relation: R K / R cl =133 / 181=0.735.
[0092] Comparative Example 3
[0093] The difference from Example 1 is that Mo replaces the Yb site.
[0094] The following tests were performed on the halide solid electrolytes of Examples 1-5 and Comparative Examples 1-3:
[0095] (a) Conductivity test:
[0096] (1) Weigh 100mg of halide solid electrolyte powder and put it into the mold liner (diameter 10mm). Press it into an electrolyte sheet using a press (parameter: 400MPa). Match stainless steel blocking electrodes at both ends of the electrolyte sheet to assemble a blocking symmetric battery.
[0097] (2) The impedance value of the sample was measured by electrochemical AC impedance spectroscopy using an electrochemical workstation to obtain the resistance value R (unit: Ω) of the solid electrolyte. The test frequency was from 0.01 Hz to 1 MHz, the test disturbance voltage was 5 mV, and the test temperature was the temperature inside the glove box.
[0098] (3) Take out the electrolyte sheet and use a micrometer to measure the thickness L (in cm) of the solid electrolyte sheet;
[0099] (4) Then, the ionic conductivity of the solid electrolyte at the temperature inside the glove box is calculated using the formula.
[0100] The formula is: σLi + =L / (R*S);
[0101] In the formula σLi + —Ionic conductivity of solid electrolytes (S cm⁻¹) -1 );
[0102] L—Thickness of the solid electrolyte (cm);
[0103] R—Intrinsic resistance (Ω) of solid electrolyte;
[0104] S — Cross-sectional area of solid electrolyte (cm²) 2 ).
[0105] (II) Antioxidant Capacity Test:
[0106] (1) Weigh out 100 mg of total material according to the mass ratio of SP: halide solid electrolyte = 9:1, place it in a mortar and grind by hand for 10 min to mix it evenly;
[0107] (2) Weigh 100mg of halide solid electrolyte powder and put it into the inner liner of the mold (diameter 10mm), and press it into electrolyte sheets using a press (parameter: 400MPa);
[0108] (3) Spread 25mg of the mixture from step (1) on one end of the electrolyte, flatten it with a mold, and then press it firmly with a press (parameter: 400MPa); introduce a Li sheet into the other end;
[0109] (4) Use an electrochemical workstation to perform LSV testing, set the open circuit voltage to ~6V and the scan rate to 0.1mV / S.
[0110] (III) Solid-state battery mold battery assembly:
[0111] Its preparation method includes the following steps:
[0112] (1) Weigh 100mg of sulfide solid electrolyte and put it into the inner liner of the alumina ceramic mold (diameter 10mm). Press it into electrolyte sheet using a press (parameters: 100MPa, 30s). Remove excess electrolyte powder with a rubber bulb.
[0113] (2) LiNi 0.83 Co 0.11 Mn 0.06 O2 (abbreviated as NCM83) and the halide solid electrolytes of Examples 1-5 and Comparative Examples 1-3 were mixed at a mass ratio of 60:40 and ground in a mortar for 15 minutes to disperse them evenly, resulting in a mixture of 100 mg.
[0114] (3) Weigh 25mg of the mixture powder from step (2) and spread it evenly on the electrolyte tablet. Rotate the stainless steel electrode head to the bottom of the mold and rotate the head to spread the powder evenly.
[0115] (4) Remove the pressure head, place a piece of carbon-coated aluminum foil (10mm) on top of the powder, press at 400MPa for 2 minutes, and remove excess positive electrode powder with a rubber bulb; then weigh it a second time to obtain the actual positive electrode material load.
[0116] (5) Place a 100μm indium foil on the other side of the electrolyte sheet, and then place a 50μm lithium copper composite strip, both with a diameter of 10mm.
[0117] (6) Fasten the mold and the pressure head, tighten the nut, and you will get a solid-state mold battery; test it with Blue Electric.
[0118] (iv) Electrical performance testing:
[0119] (1) Test method for first-time efficiency: At 35±3℃, charge the battery with a constant current of 0.1C to 3.7V, and charge it with a constant voltage of 3.7V to the cutoff current of 0.05C. Record the charging capacity as C1; then discharge the battery with a constant current of 0.1C to 2.0V and record the discharge capacity as D1; calculate the first-time efficiency based on the discharge capacity and charging capacity. First-time efficiency = (D1 / C1)×100%.
[0120] (2) Test method for first-cycle discharge capacity and capacity retention: At 35±3℃, charge at a constant current of 1C to 3.7V, then charge at a constant voltage of 3.7V to the cutoff current of 0.05C, and record the charging capacity as C1. Discharge the battery at a constant current of 1C to 2.0V, and record the first-cycle discharge capacity as D1. Repeat the charge-discharge process N times to obtain the discharge capacity of the Nth cycle, which is recorded as D. N The initial efficiency is calculated based on the first discharge capacity and the first charge capacity: Initial efficiency = (D1 / C1) × 100%. The capacity retention rate for the Nth cycle is calculated based on the first discharge capacity and the Nth discharge capacity: Capacity retention rate for the Nth cycle = (D1 / C1) × 100%. N / D1)×100%.
[0121] The test results are shown in Table 1.
[0122] Table 1
[0123]
[0124] As shown in Table 1, the present invention is effective for Li a Yb b X c (Where a, b, and c satisfy valence equilibrium) A halide solid electrolyte is formed by doping with element M. This halide solid electrolyte contains Li, Yb, dopant element M, and halogen X. This is achieved by controlling M to at least replace Li sites and controlling R... M / R X Within the range of 0.255 to 0.732, Li can be maintained without damage. a Yb b X c The original crystal form of the material is preserved, maintaining its original structure and minimizing its internal energy to achieve the most stable state. This improves the material's oxidation resistance and electrical conductivity, thereby enhancing the electrochemical performance of batteries assembled using it. Example 5 uses co-doping with two elements, which significantly improves performance compared to the single-element doping used in Examples 1-4.
[0125] The applicant declares that the detailed method of the present invention is illustrated by the above embodiments, but the present invention is not limited to the above detailed method, that is, it does not mean that the present invention must rely on the above detailed method to be implemented. Those skilled in the art should understand that any improvements to the present invention, equivalent substitutions of the raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A halide solid electrolyte, characterized in that, The halide solid electrolyte contains Li, Yb, dopant element M, and halogen X. Dopant element M at least substitutes for Li sites, and the ionic radius of M is R. M The ionic radius of X is R. X R M / R X It is in the range of 0.255 to 0.
732.
2. The halide solid electrolyte according to claim 1, characterized in that, The chemical formula of the halide solid electrolyte is Li a1 Yb b1 M c1 X d1 Wherein, X = at least one of Cl, Br, or I; wherein, M substitutes for the Li site, 1.5 ≤ a1 ≤ 10, 0.1 ≤ b1 ≤ 3, 0.05 ≤ c1 ≤ 4, 1 ≤ d1 ≤ 12, R M / R X It is in the range of 0.255 to 0.
414.
3. The halide solid electrolyte according to claim 1, characterized in that, The chemical formula of the halide solid electrolyte is Li a2 Yb b2 M c2 X′ d2 Wherein, X′ = at least one of Cl, Br, or I; wherein, M simultaneously substitutes for both the Li site and the Yb site, 1.5 ≤ a² ≤ 8, 0.05 ≤ b² ≤ 3, 0.05 ≤ c² ≤ 4, 1 ≤ d² ≤ 12, R M / R X Between 0.255 and 0.
732.
4. The halide solid electrolyte according to any one of claims 1-3, characterized in that, The doping element M includes at least one of alkali metals, alkaline earth metals, actinides, transition metals, lanthanides, and group VA elements.
5. The halide solid electrolyte according to claim 4, characterized in that, The doping element M is selected from at least two of the following: alkali metals, alkaline earth metals, actinides, transition metals, lanthanides, and group VA elements.
6. The halide solid electrolyte according to any one of claims 1-5, characterized in that, The configuration entropy of the molecular formula of the halide solid electrolyte is S1, and the configuration entropy of the molecular formula of the halide solid electrolyte before doping with M is S0, where S1>S0. The configuration entropy of the molecular formula of the halide solid electrolyte is calculated according to the following formula: Where Sconfig is the configuration entropy of the molecular formula; x a Y represents the mole fraction of Li. b M represents the mole fraction of element Yb. d X is the mole fraction of element M. c Let N1 be the mole fraction of X, N2 be the number of types of element M, and N3 be the number of types of element X.
7. A method for preparing a halide solid electrolyte as described in any one of claims 1-6, characterized in that, The preparation method includes the following steps: The raw materials for the halide solid electrolyte are mixed and reacted under high temperature and high pressure conditions, followed by cooling to obtain the halide solid electrolyte.
8. The method for preparing a halide solid electrolyte according to claim 7, characterized in that, The high temperature is 100℃~400℃; The high pressure is 100Pa to 20MPa; The reaction time under high temperature and high pressure conditions is 4h to 20h.
9. The method for preparing a halide solid electrolyte according to claim 7 or 8, characterized in that, The reaction is accompanied by stirring; The cooling rate is 0.5℃ / min to 20℃ / min.
10. A solid-state battery, characterized in that, The solid-state battery includes the halide solid electrolyte as described in any one of claims 1-6.