Solid-state battery cell, battery device, power consuming device, method for producing interface layer material

By designing a core-shell structure interface layer material in solid-state battery cells, the problem of dendrite growth in the negative electrode was solved, improving cycle performance and rate performance, while reducing costs and achieving stability of the negative electrode and electrolyte layer.

CN123162298APending Publication Date: 2026-11-24CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510677580.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-23
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Dendrite growth in the negative electrode of solid-state battery cells limits their practical application. Existing interface modification technologies are complex and costly, with limited performance improvement.

Method used

The design employs an interface layer material with a core-shell structure. The core is an insulating, electronic, or ionic conductor, while the shell is an electronic or ionic conductor with an electronic conductivity of 1×10⁻²S·cm⁻¹~5×10²S·cm⁻¹. This provides a rigid framework and uniform electron distribution, reduces local current density differences, and the shell material exhibits excellent electronic conduction and ion transport properties.

Benefits of technology

It improves the cycle performance and rate performance of solid-state battery cells, reduces the risk of lithium or sodium dendrite formation, enhances the interfacial stability between the anode and electrolyte layers, and reduces manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123162298A_ABST
    Figure CN123162298A_ABST
Patent Text Reader

Abstract

This disclosure provides a method for preparing a solid-state battery cell, a battery device, an electrical device, and an interface layer material. The solid-state battery cell includes a positive electrode, an electrolyte layer, and a negative electrode. The electrolyte layer is located between the positive and negative electrodes. The negative electrode includes a negative electrode current collector and an interface layer located on at least one side of the negative electrode current collector. The interface layer includes an interface layer material, which includes a core and a shell layer located on at least a portion of the surface of the core. The electronic conductivity of the interface layer material is 1×10⁻⁶. ‑2 S·cm ‑1 ~5×10 2 S·cm ‑1 Solid-state battery cells exhibit good cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to a method for preparing a solid-state battery cell, a battery device, an electrical device, and an interface layer material. Background Technology

[0002] Compared to battery cells using liquid electrolytes, solid-state battery cells use solid electrolyte materials, making them less prone to combustion and explosion, and thus offering high reliability and high energy density. Solid-state battery cells using metal anodes typically have even higher energy density; however, these cells suffer from dendrite growth, which limits their practical applications. Summary of the Invention

[0003] This disclosure provides a method for preparing a solid-state battery cell, a battery device, an electrical device, and an interface layer material. The solid-state battery cell has good cycle performance.

[0004] In a first aspect, this disclosure provides a solid-state battery cell, comprising a positive electrode, an electrolyte layer, and a negative electrode. The electrolyte layer is located between the positive and negative electrodes. The negative electrode includes a negative electrode current collector and an interface layer located on at least one side of the negative electrode current collector. The interface layer includes an interface layer material, which comprises a core and a shell layer located on at least a portion of the surface of the core. The electronic conductivity of the interface layer material is 1×10⁻⁶. -2 S·cm -1 ~5×10 2 S·cm -1 .

[0005] In the solid-state battery cell disclosed herein, the interface layer of the negative electrode includes an interface layer material with a core-shell structure. The core provides a rigid framework, maintaining the structural integrity of the interface layer material during cycling. This helps maintain the stability of the ion transport channels in the negative electrode and improves the cycle performance of the solid-state battery cell. The electronic conductivity of this interface layer material is 1×10⁻⁶. -2 S·cm -1 ~5×10 2 S·cm -1 Within this range, it is beneficial to achieve a uniform electron distribution on the surface of the negative electrode current collector, reducing local current density differences. This homogenizes lithium or sodium nucleation sites, allowing lithium or sodium ions to deposit uniformly on the surface of the negative electrode current collector, thereby reducing the risk of lithium or sodium dendrite formation. Furthermore, with the electronic conductivity of the interface layer material within the aforementioned range, it can also transfer some electron flow, reducing the reduction tendency of lithium or sodium metal to the solid electrolyte, thus improving the interfacial stability between the negative electrode and the electrolyte layer. Therefore, the solid-state battery cell of this disclosure exhibits excellent cycle performance.

[0006] In some embodiments, the core includes at least one of an insulating material, an electronic conductor material, or an ionic conductor material.

[0007] In some embodiments, the core includes at least one of metal oxide, polymer insulating material, metal, carbon material, electron-ion dual-conducting positive electrode active material, electron-ion dual-conducting negative electrode active material, and solid electrolyte material, wherein the solid electrolyte material includes one or more of sulfide solid electrolyte material, halide solid electrolyte material, oxide solid electrolyte material, and polymer solid electrolyte material.

[0008] The core is an insulating material, which possesses high mechanical strength, thus providing a rigid framework to maintain the structural integrity of the interface layer material during cycling. This helps maintain the stability of the ion transport channels in the negative electrode, improving the cycle performance of the solid-state battery cell. Furthermore, compared to electronic and ion-conducting materials, insulating materials are less expensive, reducing the cost of the interface layer material and consequently lowering the manufacturing cost of the solid-state battery cell.

[0009] The core material is an electronic conductor, which can further assist electron transport in the interface layer material, making it easier to achieve a uniform electron distribution on the surface of the negative electrode current collector and reducing local current density differences. This, in turn, helps to homogenize lithium or sodium nucleation sites, allowing lithium or sodium ions to be deposited uniformly on the surface of the negative electrode current collector, thereby further reducing the risk of lithium or sodium dendrite formation.

[0010] The core is an ion-conducting material, which can further assist the active ion transport of the interface layer material, thus improving the ion transport kinetics of the negative electrode. In this case, the solid-state battery cell can still maintain a high discharge capacity at high current densities, thereby improving the rate performance of the solid-state battery cell. Good negative electrode ion transport kinetics make it easier for active ions to deposit and strip away on the negative electrode, thereby reducing capacity decay during cycling and improving the cycle stability of the solid-state battery cell.

[0011] In some embodiments, the shell layer includes at least one of an electronic conductor material, an ionic conductor material, and an electronic-ionic dual conductor material.

[0012] In some embodiments, the shell layer comprises one or more of the following: conductive carbon black, amorphous carbon, lithium transition metal oxides and their modified forms, lithium phosphates and their modified forms, lithium titanate, lithium niobate, sulfur, selenium, tellurium, sodium transition metal oxides, polyanionic materials, Prussian blue materials, natural graphite, artificial graphite, mesophase microcarbon spheres, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, and metal oxides.

[0013] The aforementioned shell material possesses excellent electronic conductivity and / or ion transport properties. Good electronic conductivity facilitates a uniform electron distribution on the surface of the negative electrode current collector, reducing local current density differences. This homogenizes lithium or sodium nucleation sites, allowing lithium or sodium ions to deposit uniformly on the surface of the negative electrode current collector, thereby reducing the risk of lithium or sodium dendrite formation. Good ion transport properties enhance the ion transport kinetics on the interface layer material surface, resulting in favorable ion transport kinetics at the negative electrode. This allows the solid-state battery cell to maintain a high discharge capacity even at high current densities, thus enabling good rate performance. Furthermore, favorable negative electrode ion transport kinetics facilitate easier deposition and stripping of lithium or sodium ions, reducing capacity decay during cycling and improving the cycle stability of the solid-state battery cell.

[0014] In some embodiments, the core comprises an insulating material, and the shell comprises at least one of an electronic conductor material and an electronic-ion dual conductor material.

[0015] In some embodiments, the core comprises an ionic conductor material, and the shell comprises at least one of an electronic conductor material and an electronic-ionic dual conductor material.

[0016] In some embodiments, the core comprises an electronic conductor material, and the shell comprises at least one of an electronic conductor material, an ionic conductor material, and an electronic-ionic dual conductor material.

[0017] The inclusion of the aforementioned materials in the core and shell layers allows the interface layer material to possess excellent electronic conductivity. Good electronic conductivity facilitates a uniform electron distribution on the surface of the negative electrode current collector, reducing local current density differences. This homogenizes lithium or sodium nucleation sites, ensuring uniform deposition of lithium or sodium ions on the surface of the negative electrode current collector, thereby reducing the risk of lithium or sodium dendrite formation.

[0018] In some embodiments, the shell comprises at least one of an electronic conductor material and an electronic-ion dual conductor material, and the electronic conductivity of the shell is 10. -4 S·cm -1 The above can be selected as 10. -4 S·cm -1 ~100S·cm -1 This helps to make the electron distribution on the surface of the negative electrode current collector more uniform and reduce the difference in local current density.

[0019] In some embodiments, the shell comprises at least one of an ion-conducting material and an electron-ion dual-conducting material, and the ionic conductivity of the shell is 10. -6 S·cm -1 The above can be selected as 10. -6 S·cm-1 ~10 -2 S·cm -1 This can improve the ion transport kinetics on the surface of the interface layer material, giving the negative electrode good ion transport kinetics, thereby improving the rate performance and cycle stability of solid-state battery cells.

[0020] In some embodiments, the core comprises an electronically conductive material, and the shell comprises at least one of an electronically conductive material and an electron-ion dual-conductor material, wherein the ratio of the electronic conductivity of the shell to the electronic conductivity of the core is 1:1 to 10. 11 1. This facilitates the uniform three-dimensional growth of lithium or sodium metal, reducing the risk of lithium or sodium dendrite formation.

[0021] In some embodiments, the core comprises an ionic conductor material, and the shell comprises at least one of an ionic conductor material and an electron-ion dual conductor material, wherein the ratio of the ionic conductivity of the shell to the ionic conductivity of the core is 0.1:1 to 10. 3 1. This is beneficial for improving the rate performance of solid-state battery cells.

[0022] In some embodiments, the core comprises an insulating material or an electronically conductive material, and the shell comprises an electronically conductive material. When the solid-state battery cell is fully charged, the ionic conductivity of the interface layer material is 10. -6 S·cm -1 ~10 -2 S·cm -1 .

[0023] In some embodiments, the core comprises an ion-conducting material, and / or the shell comprises an ion-conducting material or an electron-ion dual-conductor material, and the ionic conductivity of the interface layer material is 10. -6 S·cm -1 ~10 -2 S·cm -1 .

[0024] This allows the negative electrode to have good ion transport kinetics, improving the rate performance and cycle stability of solid-state battery cells.

[0025] In some embodiments, the shell comprises a carbon material, the core comprises a carbon material, and the shell I D / I G Greater than kernel I D / I G I D This indicates that the Raman spectrum is at 1350±50 cm⁻¹. -1 D peak intensity at I G This indicates that the Raman spectrum is at 1580±50 cm⁻¹. -1 The intensity of the G peak at that location.

[0026] In some embodiments, the shell I D / I G It ranges from 1.62 to 1.72.

[0027] In some embodiments, the kernel's I D / I G It ranges from 1.60 to 1.65.

[0028] I of the shell and kernel D / I G Meeting the above conditions allows the shell to have a higher defect rate than the core, thus enabling a higher ion diffusion rate. This facilitates the rapid transport of lithium or sodium ions to the surface of the negative electrode current collector, improving the ion transport kinetics of the negative electrode. This, in turn, leads to better improvement in the ion transport kinetics of the negative electrode and more uniform lithium or sodium ion deposition, thereby further enhancing the rate performance of solid-state battery cells.

[0029] In some embodiments, the shell layer comprises a carbon material containing non-carbon elements, including O and / or F elements.

[0030] The core consists of carbon materials, which contain non-carbon elements, including O and / or F elements.

[0031] Furthermore, the ratio of carbon content to non-carbon content in the shell is less than that in the kernel.

[0032] In some embodiments, the shell comprises a carbon material containing non-carbon elements, and the ratio of the mass content of carbon elements to the mass content of non-carbon elements in the shell is 40 to 800.

[0033] In some embodiments, the core comprises a carbon material containing non-carbon elements, and the ratio of the mass content of carbon elements to the mass content of non-carbon elements in the core is 600 to 1500.

[0034] This can improve the ion transport dynamics of the negative electrode and enhance the rate performance and cycle stability of solid-state battery cells.

[0035] In some embodiments, the porosity of the shell is greater than that of the core. This greater porosity allows the shell to have a higher ion diffusion rate. This facilitates the rapid transport of lithium ions to the surface of the negative electrode current collector, improving the ion transport kinetics of the negative electrode. This, in turn, can better enhance the ion transport kinetics of the negative electrode and achieve more uniform lithium or sodium ion deposition, thereby further improving the rate performance of the solid-state battery cell.

[0036] In some embodiments, the porosity of the shell is 1% to 20%.

[0037] In some embodiments, the porosity of the kernel is 0–5%.

[0038] This can improve the ion transport kinetics of the negative electrode while reducing the irreversible loss of active ions, thereby reducing the irreversible capacity loss of solid-state battery cells.

[0039] In some embodiments, the shell thickness is 2 nm to 50 nm. This facilitates the uniform deposition of active ions and improves the cycle performance of solid-state battery cells.

[0040] In some embodiments, the volumetric particle size Dv50 of the interface layer material is 20 nm to 2 μm. This can further improve the rate performance and cycle performance of solid-state battery cells.

[0041] In some embodiments, the ratio of the shell thickness to the volumetric particle size Dv50 of the interface layer material is 2.5:100 to 45:100. This maintains the structural integrity of the interface layer material during cycling, thereby maintaining the stability of the ion transport channels in the negative electrode, while also providing good ion and electron transport channels and reducing the risk of lithium or sodium dendrite formation.

[0042] In some embodiments, the NP ratio of a solid-state battery cell is 0.01 to 0.05, where the NP ratio is the ratio of the negative electrode capacity per unit area to the positive electrode capacity per unit area.

[0043] In a second aspect, this disclosure provides a battery device comprising a plurality of solid-state battery cells as described in the first aspect.

[0044] Thirdly, this disclosure provides an electrical device that includes a solid-state battery cell (as described in the first aspect) or a battery device (as described in the second aspect).

[0045] Fourthly, this disclosure provides a method for preparing an interface layer material, comprising the following steps: providing a core; forming a shell on the surface of the core to obtain the interface layer material, the interface layer material comprising a core and a shell located on at least a portion of the surface of the core, and the electronic conductivity of the interface layer material being 1×10⁻⁶. -2 S·cm -1 ~5×10 2 S·cm -1 .

[0046] In some embodiments, the step of forming a shell on the surface of the core includes the following steps: providing a shell material; and coating the core surface with the shell material to obtain an interface layer material.

[0047] In some embodiments, the core comprises carbon material and the shell comprises carbon material;

[0048] The steps for forming a shell on the surface of the core include the following: acid washing the core with an acid solution to form a shell on the core surface, thereby obtaining an interface layer material. Attached Figure Description

[0049] To more clearly illustrate the technical solutions of the embodiments of this disclosure, the accompanying drawings used in the embodiments of this disclosure will be briefly described below. Obviously, the drawings described below are merely some embodiments of this disclosure. For those skilled in the art, other drawings can be obtained based on the drawings without creative effort.

[0050] Figure 1 A schematic diagram of a solid-state battery cell provided in some embodiments of this disclosure is shown.

[0051] Figure 2 A schematic diagram of an electrical device provided in some embodiments of this disclosure is shown.

[0052] Figure 3 The diagram shows a structural schematic of the interface layer material provided in some embodiments of this disclosure.

[0053] The accompanying drawings are not necessarily drawn to scale. Detailed Implementation

[0054] The following detailed description, with appropriate reference to the accompanying drawings, discloses embodiments of the solid-state battery cell, battery device, power-consuming device, and method for preparing the interface layer material of this disclosure. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of practically identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided to enable those skilled in the art to fully understand this disclosure and are not intended to limit the subject matter of the claims.

[0055] The "range" disclosed in this disclosure is defined by a lower limit and an upper limit, whereby a given range is defined by selecting a lower limit and an upper limit, which define the boundaries of the particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also expected. Furthermore, if minimum range values ​​1 and 2 are listed, and if maximum range values ​​3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this disclosure, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0056] Unless otherwise specified, all embodiments and optional embodiments of this disclosure may be combined with each other to form new technical solutions, and such technical solutions should be considered as included in the disclosure of this disclosure.

[0057] Unless otherwise specified, all technical features and optional technical features of this disclosure can be combined to form new technical solutions, and such technical solutions should be considered as included in the disclosure of this disclosure.

[0058] Unless otherwise specified, all steps in this disclosure may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order; for example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.

[0059] Unless otherwise specified, in this disclosure, the terms "first," "second," etc., are used to distinguish different objects, rather than to describe a specific order or primary / secondary relationship.

[0060] In this disclosure, the terms "multiple" or "a variety" refer to two or more kinds.

[0061] In the description of the embodiments of this disclosure, unless otherwise specified, "above" or "below" the second feature can mean that the first feature is in direct contact with the second feature, or that the first feature is in indirect contact with the second feature through an intermediate medium. Furthermore, "above," "over," and "on top" of the second feature can mean that the first feature is directly above or diagonally above the second feature, or simply that the first feature is at a higher horizontal level than the second feature. "Below," "below," and "under" the second feature can mean that the first feature is directly below or diagonally below the second feature, or simply that the first feature is at a lower horizontal level than the second feature.

[0062] Unless otherwise stated, the test temperature for all parameters mentioned in this disclosure is 25°C.

[0063] The solid-state battery cells mentioned in the embodiments of this disclosure are capable of charging and discharging independently. Solid-state battery cells may be cylindrical, cuboid, or other shapes, and the embodiments of this disclosure are not limited in this respect. Figure 1 This is an example of a rectangular solid-state battery cell 5.

[0064] The battery apparatus mentioned in the embodiments of this disclosure may include one or more battery cell assemblies for providing voltage and capacity. The battery cell assembly may include multiple solid-state battery cells, which are connected in series, parallel, or mixed connections via busbars.

[0065] In some embodiments, a battery cell assembly is typically formed by arranging multiple solid-state battery cells.

[0066] As an example, a battery cell assembly can be a battery module, which is formed by arranging and fixing multiple solid-state battery cells together to form an independent module. As another example, a battery module can be formed by bundling multiple solid-state battery cells together with cable ties.

[0067] In some embodiments, the battery device may be a battery pack, which includes a housing and one or more individual battery cells housed within the housing.

[0068] As an example, the battery cell assembly can be a battery module, which can be housed in a housing by fixing the battery module in the housing.

[0069] As an example, battery cell assemblies can also be housed in a housing by directly fixing multiple solid-state battery cells to the housing.

[0070] As an example, the enclosure may include a first enclosure and a second enclosure. The first enclosure and the second enclosure are fastened together to form a closed space inside the enclosure to house the individual battery cells. Here, "closed" refers to covering or closing, and can be either sealed or unsealed. The first enclosure may be a top cover or a bottom plate.

[0071] As an example, the enclosure may include a top cover, a frame, and a bottom plate. The top cover and bottom plate are connected to the frame, creating an enclosed space inside the enclosure to house the individual battery cells.

[0072] In some embodiments, the housing may be part of the vehicle's chassis structure. For example, a portion of the housing may be at least a part of the vehicle's floor, or a portion of the housing may be at least a part of the vehicle's crossbeams and longitudinal beams.

[0073] The technical solutions described in this disclosure are applicable to various electrical devices that use solid-state battery cells or battery devices, such as, but not limited to, mobile devices (e.g., mobile phones, tablets, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc. Solid-state battery cells and battery devices are used to store or provide electrical energy.

[0074] Figure 2 This is a schematic diagram of an example electrical device. The device could be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc.

[0075] The solid-state battery cells disclosed herein may include coin cells, molded cells, hard-case cells, pouch cells, etc.

[0076] The battery cells provided in the embodiments of this disclosure can be negative electrode-free metal solid-state battery cells, such as negative electrode-free lithium metal solid-state battery cells.

[0077] A cathodeless lithium metal solid-state battery cell typically refers to a battery cell in which no negative electrode active material layer is actively placed on the negative electrode side during the manufacturing process. For example, during the manufacturing process, a negative electrode active material layer formed of carbon-based active materials such as graphite is not applied or deposited at the negative electrode, and a lithium-based metal layer is not actively placed on the negative electrode side. During the first charge, lithium ions gain electrons on the negative electrode side and deposit on the surface of the negative electrode current collector to form lithium metal. During discharge, the lithium metal can be converted back into lithium ions and return to the positive electrode, achieving cyclic charging and discharging.

[0078] Lithium metal possesses a high theoretical specific capacity (3860 mAh / g) and a low reduction potential (-3.04 V vs. SHE), making it a highly promising anode material. Compared to other solid-state battery cells, anode-free lithium metal solid-state battery cells exhibit higher volumetric and gravimetric energy densities, better reliability, and require no free lithium metal during assembly, thus simplifying the manufacturing process.

[0079] Currently, the main challenges facing single-cell lithium metal solid-state batteries without anodes are: the high reducibility of lithium metal, the large volume expansion of the anode caused by lithium metal deposition during charging and discharging, the dendrite growth problem caused by uneven lithium metal deposition, and the internal short circuit problem caused by dendrite growth.

[0080] To address these issues, modifying the interface between the anode and electrolyte layers is an excellent strategy. However, existing interface modification techniques suffer from complex processes, high costs, and limited performance improvements.

[0081] Therefore, this disclosure provides a solid-state battery cell with good cycle performance.

[0082] The solid-state battery cell provided in this embodiment includes a positive electrode, an electrolyte layer, and a negative electrode, with the electrolyte layer located between the positive and negative electrodes.

[0083] The negative electrode includes a negative electrode current collector and an interface layer located on at least one side of the negative electrode current collector. The interface layer includes an interface layer material, which includes a core and a shell located on at least a portion of the surface of the core. The electronic conductivity of the interface layer material is 1 × 10⁻⁶. -2 S·cm -1 ~5×10 2 S·cm -1 .

[0084] The solid-state battery cells disclosed herein may include lithium metal solid-state battery cells and / or sodium metal solid-state battery cells.

[0085] In the solid-state battery cell disclosed herein, the interface layer of the negative electrode includes an interface layer material with a core-shell structure. The core provides a rigid framework, maintaining the structural integrity of the interface layer material during cycling. This helps maintain the stability of the ion transport channels in the negative electrode and improves the cycle performance of the solid-state battery cell. The electronic conductivity of this interface layer material is 1×10⁻⁶. -2 S·cm -1 ~5×10 2 S·cm -1Within this range, it is beneficial to achieve a uniform electron distribution on the surface of the negative electrode current collector, reducing local current density differences. This homogenizes lithium or sodium nucleation sites, allowing lithium or sodium ions to deposit uniformly on the surface of the negative electrode current collector, thereby reducing the risk of lithium or sodium dendrite formation. Furthermore, with the electronic conductivity of the interface layer material within the aforementioned range, it can also transfer some electron flow, reducing the reduction tendency of lithium or sodium metal to the solid electrolyte, thus improving the interfacial stability between the negative electrode and the electrolyte layer. Therefore, the solid-state battery cell of this disclosure exhibits excellent cycle performance.

[0086] The electronic conductivity of the interface layer material can be tested using the four-probe method, referring to GB / T 30835-2014.

[0087] In some embodiments, the core may include at least one of an insulating material, an electronic conductor material, or an ionic conductor material.

[0088] In this embodiment of the disclosure, the insulating material refers to a material with an electronic conductivity of less than 10⁻¹⁰ S·cm. -1 Materials with an electronic conductivity of 10⁻⁶. Electronic conductor materials refer to materials with an electronic conductivity of 10⁻⁶. -4 S·cm -1 The above materials. Ionic conductor materials refer to materials with an ionic conductivity of 10. -6 S·cm -1 The above materials. Electron-ion biconductor materials refer to materials with an electronic conductivity of 10. -4 S·cm -1 The above, and the ionic conductivity is 10. -6 S·cm -1 The above materials.

[0089] In some embodiments, the insulating material may include at least one of metal oxides (e.g., Al2O3, ZrO2, etc.) and polymer insulating materials.

[0090] In some embodiments, the electronic conductor material may include at least one of metal, carbon material, electron-ion dual-conducting positive electrode active material, and electron-ion dual-conducting negative electrode active material.

[0091] In some embodiments, the ion conductor material may include a solid electrolyte material, which may include one or more of sulfide solid electrolyte materials, halide solid electrolyte materials, oxide solid electrolyte materials, and polymer solid electrolyte materials.

[0092] In some embodiments, the core may include at least one of metal oxides, polymer insulating materials, metals, carbon materials, electron-ion dual-conducting positive electrode active materials, electron-ion dual-conducting negative electrode active materials, and solid electrolyte materials. The solid electrolyte materials include one or more of sulfide solid electrolyte materials, halide solid electrolyte materials, oxide solid electrolyte materials, and polymer solid electrolyte materials.

[0093] The core is an insulating material, which possesses high mechanical strength, thus providing a rigid framework to maintain the structural integrity of the interface layer material during cycling. This helps maintain the stability of the ion transport channels in the negative electrode, improving the cycle performance of the solid-state battery cell. Furthermore, compared to electronic and ion-conducting materials, insulating materials are less expensive, reducing the cost of the interface layer material and consequently lowering the manufacturing cost of the solid-state battery cell.

[0094] The core material is an electronic conductor, which can further assist electron transport in the interface layer material, making it easier to achieve a uniform electron distribution on the surface of the negative electrode current collector and reducing local current density differences. This, in turn, helps to homogenize lithium or sodium nucleation sites, allowing lithium or sodium ions to be deposited uniformly on the surface of the negative electrode current collector, thereby further reducing the risk of lithium or sodium dendrite formation.

[0095] The core is an ion-conducting material, which can further assist the transport of active ions (such as lithium ions or sodium ions) in the interface layer material, thus improving the ion transport kinetics of the negative electrode. In this case, the solid-state battery cell can still maintain a high discharge capacity at high current densities, thereby improving the rate performance of the solid-state battery cell. Good ion transport kinetics at the negative electrode make it easier for active ions to deposit and strip away, thereby reducing capacity decay during cycling and improving the cycle stability of the solid-state battery cell.

[0096] In some embodiments, the shell may include at least one of an electronic conductor material, an ionic conductor material, and an electronic-ionic dual conductor material.

[0097] In some embodiments, the solid-state battery cell may be a lithium metal solid-state battery cell, and the shell may include at least one of carbon material, positive electrode active material capable of lithium ion insertion / extraction, and negative electrode active material capable of lithium ion insertion / extraction.

[0098] In some embodiments, the solid-state battery cell may be a sodium metal solid-state battery cell, and the shell may include at least one of carbon material, positive electrode active material capable of lithium ion insertion / extraction, and negative electrode active material capable of sodium ion insertion / extraction.

[0099] In some embodiments, the carbon material may include one or more of hard carbon, soft carbon, graphite, conductive carbon black, and amorphous carbon.

[0100] In some embodiments, the positive electrode active material capable of lithium ion intercalation / deintercalation may include one or more of lithium transition metal oxides and their modified forms, lithium phosphates and their modified forms, lithium titanate, lithium niobate, sulfur, selenium, and tellurium.

[0101] In some embodiments, the negative electrode active material capable of lithium ion intercalation / deintercalation may include one or more of the following: natural graphite, artificial graphite, mesophase microcarbon spheres, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, and metal oxides.

[0102] In some embodiments, the positive electrode active material capable of deintercalating and intercalating sodium ions may include one or more of sodium transition metal oxides, polyanionic materials, and Prussian blue materials.

[0103] In some embodiments, the negative electrode active material capable of deintercalating and deintercalating sodium ions may include hard carbon.

[0104] In some embodiments, the shell layer may include one or more of the following: conductive carbon black, amorphous carbon, lithium transition metal oxides and their modified forms, lithium phosphates and their modified forms, lithium titanate, lithium niobate, sulfur, selenium, tellurium, sodium transition metal oxides, polyanionic materials, Prussian blue materials, natural graphite, artificial graphite, mesophase microcarbon spheres, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, and metal oxides.

[0105] The aforementioned shell material possesses excellent electronic conductivity and / or ion transport properties. Good electronic conductivity facilitates a uniform electron distribution on the surface of the negative electrode current collector, reducing local current density differences. This homogenizes lithium or sodium nucleation sites, allowing lithium or sodium ions to deposit uniformly on the surface of the negative electrode current collector, thereby reducing the risk of lithium or sodium dendrite formation. Good ion transport properties enhance the ion transport kinetics on the interface layer material surface, resulting in favorable ion transport kinetics at the negative electrode. This allows the solid-state battery cell to maintain a high discharge capacity even at high current densities, thus enabling good rate performance. Furthermore, favorable negative electrode ion transport kinetics facilitate easier deposition and stripping of lithium or sodium ions, reducing capacity decay during cycling and improving the cycle stability of the solid-state battery cell.

[0106] In some embodiments, the core may include an insulating material, and the shell may include at least one of an electronic conductor material and an electronic-ion dual conductor material.

[0107] In some embodiments, the core may include an ionic conductor material, and the shell may include at least one of an electronic conductor material and an electronic-ionic dual conductor material.

[0108] In some embodiments, the core may include an electronic conductor material, and the shell may include at least one of an electronic conductor material, an ionic conductor material, and an electronic-ionic dual conductor material.

[0109] The inclusion of the aforementioned materials in the core and shell layers allows the interface layer material to possess excellent electronic conductivity. Good electronic conductivity facilitates a uniform electron distribution on the surface of the negative electrode current collector, reducing local current density differences. This homogenizes lithium or sodium nucleation sites, ensuring uniform deposition of lithium or sodium ions on the surface of the negative electrode current collector, thereby reducing the risk of lithium or sodium dendrite formation.

[0110] In some embodiments, the shell layer comprises at least one of an electronic conductor material and an electronic-ion dual conductor material, and the electronic conductivity of the shell layer may be 10. -4 S·cm -1 That's all. Optionally, in some embodiments, the electronic conductivity of the shell can be 10. -4 S·cm -1 ~100S·cm -1 For example, it can be 10 -4 S·cm -1 10 -3 S·cm -1 10 -2 S·cm -1 10 -1 S·cm -1 A range consisting of 1, 10, 100, or any of the above values.

[0111] The electronic conductivity of the shell is 10 -4 S·cm -1 The above allows the interface layer material to possess suitable electronic conductivity, improving its electronic conduction performance. This, in turn, facilitates a more uniform electron distribution on the surface of the negative electrode current collector, reducing local current density differences. This, in turn, homogenizes lithium or sodium nucleation sites, ensuring uniform deposition of lithium or sodium ions on the surface of the negative electrode current collector, thereby reducing the risk of lithium or sodium dendrite formation. Furthermore, maintaining the electronic conductivity of the shell within the aforementioned range can also reduce the reduction tendency of lithium or sodium metal to the solid electrolyte, thereby improving the interfacial stability between the negative electrode and the electrolyte layer, and ultimately enhancing the cycle performance of the solid-state battery cell.

[0112] In some embodiments, the shell layer comprises at least one of an ion-conducting material and an electron-ion dual-conducting material, and the ionic conductivity of the shell layer can be 10. -6 S·cm -1 That's all. Optionally, in some embodiments, the ionic conductivity of the shell can be 10. -6 S·cm -1 ~10-2 S·cm -1 For example, it can be 10 -6 S·cm -1 10 -5 S·cm -1 10 -4 S·cm -1 10 -3 S·cm -1 10 -2 S·cm -1 or a range consisting of any of the above values.

[0113] The ionic conductivity of the shell is 10. -6 S·cm -1 The above can improve the ion transport kinetics on the surface of the interface layer material, giving the negative electrode good ion transport kinetics. In this case, the solid-state battery cell can still have a high discharge capacity at high current densities, thus enabling the solid-state battery cell to have good rate performance. Good negative electrode ion transport kinetics make it easier for lithium or sodium ions to deposit and be stripped from the negative electrode, thereby reducing capacity decay during cycling and improving the cycle stability of the solid-state battery cell.

[0114] In some embodiments, the core comprises an electronically conductive material, and the shell comprises at least one of an electronically conductive material and an electron-ion dual-conductor material, wherein the ratio of the electronic conductivity of the shell to the electronic conductivity of the core can be 1:1 to 10. 11 :1, for example, can be 1:1, 10:1, 100:1, 1000:1, 10 4 1, 10 5 1, 10 6 1, 10 7 1, 10 8 1, 10 9 1, 10 10 1, 10 11 :1, or any range of the above ratios.

[0115] The ratio of the electronic conductivity of the shell to that of the core is 1:1 to 10. 11 1. At this point, the core has equal or lower electronic conductivity than the shell. Lithium or sodium ions tend to deposit on the shell surface or in the structural pores rather than penetrating into the core. This facilitates the three-dimensional uniform growth of lithium or sodium metal and reduces the risk of lithium or sodium dendrite formation.

[0116] In some embodiments, the core comprises an ionic conductor material, and the shell comprises at least one of an ionic conductor material and an electron-ion dual conductor material, wherein the ratio of the ionic conductivity of the shell to the ionic conductivity of the core can be 0.1:1 to 10. 3 :1, for example, can be 0.1:1, 0.5:1, 1:1, 10:1, 50:1, 100:1, 500:1, 1000:1 or any range of the above ratios.

[0117] When the ratio of the ionic conductivity of the shell to that of the core is within the aforementioned range, the transport impedance of active ions at the negative electrode interface is lower, and the ion migration path is shorter, thereby improving the rate performance of the solid-state battery cell. This ratio also facilitates rapid dispersion of active ions, avoids local concentration gradients, promotes uniform nucleation of lithium or sodium in three-dimensional space, and delays the growth of lithium or sodium dendrites.

[0118] The electronic conductivity of the shell, the ratio of the electronic conductivity of the shell to that of the core, the ionic conductivity of the shell, and the ratio of the ionic conductivity of the shell to that of the core can be measured using atomic force microscopy (AFM).

[0119] In some embodiments, the core comprises an insulating material or an electronically conductive material, and the shell comprises an electronically conductive material. When the solid-state battery cell is fully charged, the ionic conductivity of the interface layer material can be 10. -6 S·cm -1 ~10 - 2 S·cm -1 For example, it can be 10 -6 S·cm -1 10 -5 S·cm -1 10 -4 S·cm -1 10 -3 S·cm -1 10 -2 S·cm -1 or a range consisting of any of the above values.

[0120] In some embodiments, the core comprises an ion-conducting material, and / or the shell comprises an ion-conducting material or an electron-ion dual-conducting material; the ionic conductivity of the interface layer material is 10. -6 S·cm -1 ~10 -2 S·cm -1 .

[0121] In this embodiment, a solid-state battery cell being in a fully charged state means: at 25°C, the solid-state battery cell is charged at a constant current rate of 1 / 3C to the upper limit cutoff voltage, and then charged at a constant voltage at the upper limit cutoff voltage until the current drops to 0.05C. At this point, the solid-state battery cell is in a fully charged state. The upper limit cutoff voltage is known in the art, and the voltage recommended in the product specification can be used. For example, the positive electrode active material is a lithium transition metal oxide, such as LiNi. 1 / 3 Co 1 / 3Mn 1 / 3 O2 (abbreviated as NCM333), LiNi 0.5 Co 0.2 Mn 0.3 O2 (abbreviated as NCM523), LiNi 0.5 Co 0.25 Mn 0.25 O2 (abbreviated as NCM211), LiNi 0.6 Co 0.2 Mn 0.2 O2 (abbreviated as NCM622), LiNi 0.8 Co 0.1 Mn 0.1 O2 (abbreviated as NCM811), LiNi 0.96 Co 0.02 Mn 0.02 O2 (abbreviated as Ni96), LiNi 0.80 Co 0.15 Al 0.05 O2, the upper limit cutoff voltage can be 4.25V (vs. Li). + For example, the positive electrode active material is LiFePO4, and the upper limit cutoff voltage can be 3.65V (vs. Li). + / Li).

[0122] The ionic conductivity of the interface layer material is 10. -6 S·cm -1 ~10 -2 S·cm -1 This allows the negative electrode to possess favorable ion transport kinetics, enabling the solid-state battery cell to maintain a high discharge capacity even at high current densities, thus resulting in excellent rate performance. Good negative electrode ion transport kinetics also facilitate the deposition and stripping of lithium or sodium ions, reducing capacity decay during cycling and improving the cycle stability of the solid-state battery cell.

[0123] The ionic conductivity of the interface layer material can be determined by impedance spectroscopy. For example, in a glove box environment, a fully charged solid-state battery cell can be disassembled, and the interface layer material on the negative electrode surface can be scraped off with a knife. The scraped interface layer material powder can be ground thoroughly in a mortar for 10 minutes to obtain sample powder. 150 mg of sample powder can be pressed into a 10 mm diameter mold under a pressure of 4 tons to prepare an electrolyte disc with a diameter of 10 mm. The conductive agent VGCF can be spread on both sides of the electrolyte disc as a blocking electrode, and a pressure of 1 ton can be applied to form it. The blocking electrode and an electrochemical impedance workstation can be connected for testing. The temperature during the test is 25℃, the pressure is 150 MPa, the test bias is 10 mV, and the frequency range is 1 MHz-10 Hz. The resistance value R is obtained by reading the intersection of the test impedance spectrum curve with the horizontal axis. The ionic conductivity σ of the sample can be calculated according to the formula σ=D / (R×S), where σ is the ionic conductivity, D is the thickness of the electrolyte disc, and S is the contact area between the blocking electrode and the electrolyte disc.

[0124] In some embodiments, the shell layer comprises a carbon material, and the core layer comprises a carbon material, which may include one or more of hard carbon, soft carbon, graphite, conductive carbon black, and amorphous carbon. The shell layer I D / I G It can be greater than the kernel's I. D / I G I D This indicates that the Raman spectrum is at 1350±50 cm⁻¹. -1 D peak intensity at I G This indicates that the Raman spectrum is at 1580±50 cm⁻¹. -1 The intensity of the G peak at that location.

[0125] In some embodiments, the shell I D / I G It can be between 1.62 and 1.72.

[0126] In some embodiments, the kernel's I D / I G It can be 1.60 to 1.65.

[0127] I of the shell and kernel D / I G Meeting the above conditions allows the shell to have a higher defect rate than the core, thus enabling a higher ion diffusion rate. This facilitates the rapid transport of lithium or sodium ions to the surface of the negative electrode current collector, improving the ion transport kinetics of the negative electrode. This, in turn, leads to better improvement in the ion transport kinetics of the negative electrode and more uniform lithium or sodium ion deposition, thereby further enhancing the rate performance of solid-state battery cells.

[0128] Material I D / I GThe test can be performed using a Raman spectrometer. D This indicates that the Raman spectrum of the material is at 1350±50 cm⁻¹. -1 D peak intensity at I G This indicates that the Raman spectrum of the material is at 1580±50 cm⁻¹. -1 The intensity of the G peak at the location was measured. The test conditions were: excitation wavelength 532 nm, grating 600 lines, objective lens 50x, integration time 10 s, cumulative scan 3 times, area scan, obtaining the D and G peak intensities at 100 points, and calculating the I at 100 points. D / I G Remove the largest and smallest 30 I's. D / I G The average of the remaining 40 points is the material's I. D / I G The testing instrument can be a Horiba LabRAM HR800 Raman spectrometer.

[0129] In some embodiments, the shell may include a carbon material containing non-carbon elements, including oxygen (O) and / or sulfur (F). The core may include a carbon material containing non-carbon elements, including oxygen (O) and / or sulfur (F). Furthermore, the ratio of the mass content of carbon to the mass content of non-carbon elements in the shell is less than the ratio of the mass content of carbon to the mass content of non-carbon elements in the core.

[0130] In some embodiments, the shell layer comprises a carbon material containing non-carbon elements, and the ratio of the mass content of carbon elements to the mass content of non-carbon elements in the shell layer can be 40 to 800.

[0131] In some embodiments, the core comprises carbon material containing non-carbon elements, and the ratio of the mass content of carbon elements to the mass content of non-carbon elements in the core can be 600 to 1500.

[0132] During the initial charging of a solid-state battery cell, F atoms can form a LiF or NaF coating layer on the surface of the interface material. This coating layer has good ion conductivity, thereby forming ion permeation channels along the thickness direction within the interface layer, improving the transport kinetics within the negative electrode. An appropriate amount of oxygen-containing functional groups can improve the ion transport kinetics of the negative electrode and contribute to high initial coulombic efficiency and high capacity retention in the solid-state battery cell. Compared to the core, the shell layer contains more of the aforementioned non-carbon elements, resulting in better ion transport kinetics at the negative electrode. This allows the solid-state battery cell to maintain a high discharge capacity even at high current densities, thus enabling good rate performance. Good ion transport kinetics at the negative electrode also facilitate the deposition and stripping of lithium or sodium ions, reducing capacity decay during cycling and improving the cycle stability of the solid-state battery cell.

[0133] The ratio of the mass content of carbon to the mass content of non-carbon elements in the shell and core can be obtained by inductively coupled plasma optical emission spectrometry (ICP-OES).

[0134] In some embodiments, the porosity of the shell is greater than that of the core.

[0135] The shell has a higher porosity than the core, allowing for a higher ion diffusion rate. This facilitates rapid lithium-ion transport to the negative electrode current collector surface, improving ion transport kinetics. Consequently, it enhances negative electrode ion transport kinetics and promotes more uniform lithium-ion deposition, ultimately improving the rate performance of solid-state battery cells.

[0136] In some embodiments, the porosity of the shell can be 1% to 20%.

[0137] In some embodiments, the porosity of the kernel can be 0 to 5%. 0% indicates that the kernel is non-porous.

[0138] Optionally, the porosity of the core can be 0.5% to 5%.

[0139] When the porosity of the shell and core is within the above range, it can improve the ion transport kinetics of the negative electrode while reducing the irreversible loss of active ions, thereby reducing the irreversible capacity loss of solid-state battery cells.

[0140] In some embodiments, the thickness of the shell can be 2nm to 50nm, for example, it can be 2nm, 5nm, 10nm, 20nm, 30nm, 40nm, 50nm, or any of the above values.

[0141] The shell thickness ranges from 2nm to 50nm, which facilitates uniform coating of the core. Provided with good ion and electron transport channels, it guides lithium or sodium ions into the shell for deposition, forming a three-dimensional uniform lithium or sodium layer, thereby reducing the risk of lithium or sodium dendrite formation. Appropriate shell thickness can also reduce irreversible loss of active ions, thus mitigating irreversible capacity loss in solid-state battery cells and improving their cycle performance.

[0142] The thickness of the shell can be measured using methods and equipment known in the art. For example, it can be measured using transmission electron microscopy (TEM). As an example, the thickness of the shell can be measured by the following steps: first, turn on the transmission electron microscope, measure the thickness of the sample shell, test the thickness at five points, and take the average value as the thickness of the shell.

[0143] In some embodiments, the volume distribution particle size Dv50 of the interface layer material can be 20 nm to 2 μm, for example, it can be 20 nm, 50 nm, 80 nm, 100 nm, 500 nm, 800 nm, 1 μm, 1.2 μm, 1.5 μm, 1.8 μm, 2 μm, or any combination of the above values.

[0144] A volume distribution particle size Dv50 of 20nm to 2μm for the interface layer material is beneficial for the interface layer to have a suitable packing density. This can not only enable the negative electrode to have good ion transport kinetics, but also reduce the volume expansion of the negative electrode and reduce the internal short circuit problem caused by dendrite growth, thereby further improving the rate performance and cycle performance of solid-state battery cells.

[0145] Dv50 represents the particle size corresponding to a cumulative volumetric distribution percentage of 50% for the material. It can be measured using a laser particle size analyzer, referring to GB / T19077-2016. During testing, add 1g of the sample to a clean small beaker and 20ml of deionized water. Sonicate at 53kHz / 120W for 5 minutes to ensure complete dispersion. Turn on the laser particle size analyzer, clean the optical path system, and automatically test the background. Stir the sonicated solution to ensure uniform dispersion, place it in the sample cell as required, and begin measuring the particle size. A MasterSizer 3000 laser particle size analyzer can be used as the testing instrument.

[0146] In some embodiments, the ratio of the shell thickness to the volumetric particle size Dv50 of the interface layer material can be 2.5:100 to 45:100, for example, it can be 2.5:100, 5:100, 10:100, 20:100, 30:100, 40:100, 45:100, or any range of the above ratios. Optionally, the ratio of the shell thickness to the volumetric particle size Dv50 of the interface layer material can be 2.5:100 to 15:100, for example, it can be 2.5:100, 3:100, 5:100, 8:100, 10:100, 12:100, 15:100, or any range of the above ratios.

[0147] Figure 3 This is an example of an interface layer material in an embodiment of this disclosure. For example... Figure 3 As shown, the interface layer material 10 may include a core 11 and a shell 12. The ratio of the shell thickness d to the volume distribution particle size Dv50 of the interface layer material may be 2.5:100 to 45:100.

[0148] The ratio of the shell thickness to the radius of the interface layer material is between 2.5:100 and 45:100. This can maintain the structural integrity of the interface layer material during cycling, thereby maintaining the stability of the ion transport channel of the negative electrode, and can also provide good ion transport channels and electron transport channels, reducing the risk of lithium dendrites or sodium dendrites forming.

[0149] In some embodiments, the NP ratio of a solid-state battery cell can be 0.01 to 0.05, where the NP ratio is the ratio of the unit area capacity of the negative electrode (i.e., the interface layer) to the unit area capacity of the positive electrode.

[0150] The NP ratio can be tested using the following method.

[0151] The negative electrode was removed from a solid-state battery cell and placed in a solid-state battery mold for testing. The counter electrode was a lithium-indium alloy sheet separated by an electrolyte layer. The battery was discharged to 0.01V (vs. Li) at a current density of 0.1C. + / Li), and then charged to 2V at a current density of 0.1C (vs. Li). + The resulting charging capacity ( / Li) is the negative electrode capacity. Negative electrode capacity per unit area = negative electrode capacity / negative electrode area.

[0152] The positive electrode is extracted from a solid-state battery cell and placed in a solid-state battery mold for testing. A lithium-indium alloy sheet is used as the counter electrode, separated by an electrolyte layer. The battery is charged at a current density of 0.1C to the upper cutoff voltage, and then discharged at a current density of 0.1C to the lower cutoff voltage. The resulting discharge capacity is the positive electrode capacity. Positive electrode capacity per unit area = Positive electrode capacity / Positive electrode area.

[0153] The NP ratio of a solid-state battery cell = negative electrode unit area capacity / positive electrode unit area capacity.

[0154] Both the upper and lower cutoff voltages are known in the art, and the voltages recommended in the product specifications can be used. For example, the positive electrode active material is a lithium transition metal oxide or its modified form, such as LiNi. 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (abbreviated as NCM333), LiNi 0.5 Co 0.2 Mn 0.3 O2 (abbreviated as NCM523), LiNi 0.5 Co 0.25 Mn 0.25 O2 (abbreviated as NCM211), LiNi 0.6 Co 0.2 Mn 0.2 O2 (abbreviated as NCM622), LiNi 0.8 Co0.1 Mn 0.1 O2 (abbreviated as NCM811), LiNi 0.96 Co 0.02 Mn 0.02 O2 (abbreviated as Ni96), LiNi 0.80 Co 0.15 Al 0.05 O2, the upper limit cutoff voltage can be 4.3V (vs. Li). + / Li), the lower cutoff voltage can be 2V (vs.Li). + / Li).

[0155] In some embodiments, the negative current collector may be a conductive negative current collector, such as a metal foil or a composite current collector. The metal foil may be a pure metal, an alloy, or a surface-treated metal, for example, including but not limited to stainless steel foil, copper foil, nickel foil, and titanium foil. The composite current collector may include a polymer material substrate and a metal material layer formed on at least one surface of the polymer material substrate. As an example, the metal material may include, but is not limited to, one or more of copper, copper alloys, nickel, nickel alloys, titanium, titanium alloys, silver, and silver alloys. As an example, the polymer material substrate may include, but is not limited to, one or more of polypropylene, polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene, and polyethylene.

[0156] It should be noted that the above-mentioned tests on various parameters of the interface layer material can be performed by sampling from the prepared solid-state battery cell according to the following steps: Discharge the solid-state battery cell (for safety reasons, the solid-state battery cell is generally left in a fully discharged state); after disassembling the solid-state battery cell, remove the negative electrode, and then sample from the negative electrode to test the various parameters related to the interface layer material.

[0157] [positive electrode]

[0158] The positive electrode can be prepared by either a dry process or a wet process.

[0159] In some embodiments, the positive electrode includes a positive electrode current collector and a positive electrode active material layer located on at least one side of the positive electrode current collector, wherein the positive electrode active material layer includes a solid electrolyte material and a positive electrode active material.

[0160] In some embodiments, the positive current collector may be a metal foil or a composite current collector. The metal foil may be a pure metal, an alloy, or a surface-treated metal, such as, but not limited to, stainless steel foil, carbon-coated aluminum foil, or aluminum foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. As an example, the metal material may include, but is not limited to, one or more of aluminum, aluminum alloys, nickel, nickel alloys, titanium, titanium alloys, silver, and silver alloys. As an example, the polymer substrate may include, but is not limited to, one or more of polypropylene, polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene.

[0161] In some embodiments, the positive electrode may not require an additional positive current collector; for example, the stainless steel sheet of the mold battery can be directly used as the positive current collector.

[0162] In some embodiments, the positive electrode active material may include one or more of lithium transition metal oxides and their modified forms, lithium phosphates and their modified forms, lithium titanate, lithium niobate, sulfur, selenium, and tellurium.

[0163] Optionally, examples of lithium transition metal oxides may include, but are not limited to, one or more of lithium cobalt oxides, lithium nickel oxides, lithium manganese oxides, lithium nickel cobalt oxides, lithium manganese cobalt oxides, lithium nickel manganese oxides, lithium nickel cobalt manganese oxides, lithium nickel cobalt aluminum oxides, and lithium-rich manganese-based materials.

[0164] Optionally, examples of lithium phosphates may include, but are not limited to, one or more of lithium iron phosphate, lithium iron phosphate and carbon composites, lithium manganese phosphate, lithium manganese phosphate and carbon composites, lithium manganese iron phosphate, and lithium manganese iron phosphate and carbon composites.

[0165] In some embodiments, to further improve the energy density of a solid-state battery cell, the positive electrode active material may include materials of the general formula Li. a Ni b Co c M d O e A f One or more of lithium transition metal oxides and their modified materials. 0.8≤a≤1.2, 0.5≤b<1, 0<c<1, 0<d<1, 1≤e≤2, 0≤f≤1, M may include one or more of Mn, Al, Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, and B, and A may include one or more of N, F, S, and Cl. Optionally, 0.6≤b<1, 0.8≤b<1.

[0166] As an example, the positive electrode active material may include, but is not limited to, LiCoO2, LiNiO2, LiMnO2, LiMn2O4, and LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (abbreviated as NCM333), LiNi 0.5 Co 0.2 Mn 0.3 O2 (abbreviated as NCM523), LiNi 0.5 Co 0.25 Mn 0.25 O2 (abbreviated as NCM211), LiNi 0.6 Co 0.2 Mn 0.2 O2 (abbreviated as NCM622), LiNi 0.8 Co 0.1 Mn 0.1 O2 (abbreviated as NCM811), LiNi 0.96 Co 0.02 Mn 0.02 O2 (abbreviated as Ni96), LiNi 0.80 Co 0.15 Al 0.05 One or more of O2, LiFePO4, LiMnPO4 and their respective modified materials.

[0167] In some embodiments, the positive electrode active material may include one or more of sodium transition metal oxides, polyanionic materials (such as phosphates, fluorophosphates, pyrophosphates, sulfates, etc.), and Prussian blue materials.

[0168] As an example, positive electrode active materials may include NaFeO2, NaCoO2, NaCrO2, NaMnO2, NaNiO2, and NaNi 1 / 2Ti 1 / 2 O2, NaNi 1 / 2 Mn 1 / 2 O2, Na 2 / 3 Fe 1 / 3 Mn 2 / 3 O2, NaNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, NaFePO4, NaMnPO4, NaCoPO4, Prussian blue materials and materials with the general formula X p M' q (PO4) r O x Y 3-x One or more of the materials. In general formula X p M' q (PO4)r O x Y 3-x In the given condition, 0 < p ≤ 4, 0 < q ≤ 2, 1 ≤ r ≤ 3, 0 ≤ x ≤ 2, and X includes elements selected from H. + Li + Na + K + and NH4 + One or more of the following, M' is a transition metal cation, which may be selected from one or more of V, Ti, Mn, Fe, Co, Ni, Cu and Zn, and Y is a halide anion, which may be selected from one or more of F, Cl and Br.

[0169] The modified materials for the above-mentioned positive electrode active materials can be the positive electrode active materials through doping modification and / or surface coating modification.

[0170] During the charging and discharging process, solid-state battery cells undergo the intercalation and deintercalation of Li or Na, resulting in varying molar contents of Li or Na at different discharge states. In the examples of positive electrode active materials in this disclosure, the molar contents of Li or Na represent the initial state of the material, i.e., the state before feeding. When the positive electrode active material is applied to a solid-state battery cell, the molar contents of Li or Na will change after charge-discharge cycles. Similarly, in the examples of positive electrode active materials in this disclosure, the molar contents of O are only theoretical values. Oxygen release from the crystal lattice will cause changes in the molar contents of O, and the actual molar contents of O will also fluctuate.

[0171] In some embodiments, the solid electrolyte material in the positive electrode may include one or more of the following: sulfide solid electrolyte material, halide solid electrolyte material, oxide solid electrolyte material, and polymer solid electrolyte material.

[0172] Optionally, the sulfide solid electrolyte material may include one or more of the following: silver-germanium sulfide type, LGPS type, Li2S-GeS2 type, Li2S-P2S5 type, Li2S-SiS2 type, and Li2S-MeS-P2S5 type sulfide solid electrolyte materials. Me may include one or more of Si, Ge, Sn, and Al.

[0173] Optionally, the sulfide solid electrolyte material of the silver-germanium sulfide type may include Li 6±s P 1-j A j S 5±s- t B t X 1±sThe material has the following properties: 0≤j<1, 0≤t<1, 0≤s<1, A includes one or more elements from Ge, Si, Sn and Sb, B includes one or more elements from O, Se and Te, and X includes one or more elements from Cl, Br, I and F.

[0174] Optionally, LGPS-type sulfide solid electrolyte materials may include those with the chemical formula Li 10±δ5 Ge 1-g G g P 2-q Q q S 12- w W w The material has the following properties: 0≤δ5<1, 0≤g≤1, 0≤q≤2, 0≤w<1, G includes one or two elements from Si and Sn, Q includes Sb, and W includes one or more elements from O, Se, Te, Cl, Br, I, and F.

[0175] Optionally, as an example, sulfide solid electrolyte materials may include Li6PS5Cl, Li6PS5Br, Li 10 GeP2S 12 Li3PS4, Li7P3S 11 One or more of them.

[0176] Optionally, the sulfide solid electrolyte material may include, but is not limited to, one or more of Na3PS4, Na3SnS4, and Na3SbS4.

[0177] Optionally, the halide solid electrolyte material may be one or more of Li3YCl6, Li3YBr6, Li3ErCl6, Li3InCl6, and Li3InBr6, including but not limited to.

[0178] Optionally, the halide solid electrolyte material may include, but is not limited to, Na2ZrCl6 and / or Na3YCl6.

[0179] Optionally, the oxide solid electrolyte material may include one or more of the following: NASICON type solid electrolyte, LISICON type solid electrolyte, perovskite type solid electrolyte, and garnet type solid electrolyte.

[0180] As an example, oxide solid electrolyte materials may include, but are not limited to, Li5La3Ti2O 12 Li7La3Zr2O 12 Li4Ti5O 12 Li 14 Zn(GeO4)4, LiTi2(PO4)3, Li 1+x Al x Ti2-x (PO4)3, Li 1+y Al y Ge 2-y One or more of (PO4)3, 0 < x < 2, 0 < y < 2.

[0181] Optionally, the oxide solid electrolyte material may include, but is not limited to, Na. 3.2 Hf2Si 2.2 P 0.8 O 12 Na 3.4 Zr 1.6 Sc 0.4 Si2PO 12 Na 3.1 Zr 1.9 La 0.1 Si2PO 12 One or more of them.

[0182] Optionally, the polymer solid electrolyte material can be formed by complexing a polymer matrix material with a lithium salt. Optionally, the polymer matrix material can be one or more of, but not limited to, polyethylene oxide (PEO) and its derivatives, polypropylene oxide (PPO) and its derivatives, polycarbonate (PPC), polyacrylonitrile (PAN), polysiloxane (PDMS), polyvinylidene fluoride (PVDF), and polymethyl methacrylate (PMMA). Optionally, the lithium salt can be one or more of, but not limited to, LiClO4, LiAsF4, LiPF6, LiBF4, LiTFSI, and LiFSI.

[0183] Optionally, the polymer solid electrolyte material can be formed by complexing a polymer matrix material with a sodium salt. Optionally, the polymer matrix material can be one or more of, but not limited to, polyethylene oxide (PEO) and its derivatives, polypropylene oxide (PPO) and its derivatives, polycarbonate (PPC), polyacrylonitrile (PAN), polysiloxane (PDMS), polyvinylidene fluoride (PVDF), and polymethyl methacrylate (PMMA). Optionally, the sodium salt can be one or more of, but not limited to, NaAsF4, NaPF6, NaBF4, NaTFSI, and NaFSI.

[0184] Optionally, the polymer solid electrolyte material may also include an inert filler, which can reduce the crystallinity of the polymer and improve its mechanical properties. Optionally, the inert filler may include, but is not limited to, one or more of TiO2, Al2O3, ZrO2, and SiO2.

[0185] In some embodiments, the positive electrode active material layer may further include a positive electrode conductive agent.

[0186] Optionally, the positive electrode conductive agent may be one or more of the following, including but not limited to superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes (CNTs), graphene, carbon nanofibers, and vapor-grown carbon fibers (VGCF).

[0187] In some embodiments, the positive electrode active material layer may or may not include a positive electrode binder, and can be adjusted according to the positive electrode composition and the preparation process of the solid-state battery cell.

[0188] Optionally, the positive electrode binder may include, but is not limited to, one or more of the following: polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), ethylene-tetrafluoroethylene-propylene terpolymer, ethylene-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, styrene-butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, methyl vinyl silicone rubber, nitrile rubber (NBR), hydrogenated nitrile rubber (HNBR), thermoplastic styrene-butadiene rubber (SBS), isoprene rubber, cis-butadiene rubber (BR), ethyl cellulose, fluororubber, and acrylate rubber.

[0189] [Electrolyte layer]

[0190] The electrolyte layer can be prepared by a dry process or a wet process.

[0191] In some embodiments, the electrolyte layer comprises a solid electrolyte material. Optionally, the solid electrolyte material may include one or more of sulfide solid electrolyte materials, halide solid electrolyte materials, oxide solid electrolyte materials, and polymer solid electrolyte materials.

[0192] Optionally, the sulfide solid electrolyte material may include one or more of the following: silver-germanium sulfide type, LGPS type, Li2S-GeS2 type, Li2S-P2S5 type, Li2S-SiS2 type, and Li2S-MeS-P2S5 type sulfide solid electrolyte materials. Me may include one or more of Si, Ge, Sn, and Al.

[0193] Optionally, the sulfide solid electrolyte material of the silver-germanium sulfide type may include Li 6±s P 1-j A j S 5±s- t B t X 1±s The material has the following properties: 0≤j<1, 0≤t<1, 0≤s<1, A includes one or more elements from Ge, Si, Sn and Sb, B includes one or more elements from O, Se and Te, and X includes one or more elements from Cl, Br, I and F.

[0194] Optionally, LGPS-type sulfide solid electrolyte materials may include those with the chemical formula Li 10±δ5 Ge 1-g G g P 2-q Q q S 12- w W w The material has the following properties: 0≤δ5<1, 0≤g≤1, 0≤q≤2, 0≤w<1, G includes one or two elements from Si and Sn, Q includes Sb, and W includes one or more elements from O, Se, Te, Cl, Br, I, and F.

[0195] Optionally, as an example, sulfide solid electrolyte materials may include Li6PS5Cl, Li6PS5Br, Li 10 GeP2S 12 Li3PS4, Li7P3S 11 One or more of them.

[0196] Optionally, the sulfide solid electrolyte material may include, but is not limited to, one or more of Na3PS4, Na3SnS4, and Na3SbS4.

[0197] Optionally, the halide solid electrolyte material may be one or more of Li3YCl6, Li3YBr6, Li3ErCl6, Li3InCl6, and Li3InBr6, including but not limited to.

[0198] Optionally, the halide solid electrolyte material may include, but is not limited to, Na2ZrCl6 and / or Na3YCl6.

[0199] Optionally, the oxide solid electrolyte material may include one or more of the following: NASICON type solid electrolyte, LISICON type solid electrolyte, perovskite type solid electrolyte, and garnet type solid electrolyte.

[0200] Optionally, the oxide solid electrolyte material may include, but is not limited to, Na. 3.2 Hf2Si 2.2 P 0.8 O 12 Na 3.4 Zr 1.6 Sc 0.4 Si2PO 12 Na 3.1 Zr 1.9 La 0.1 Si2PO 12 One or more of them.

[0201] As an example, oxide solid electrolyte materials may include, but are not limited to, Li5La3Ti2O 12 Li7La3Zr2O 12 Li4Ti5O 12 Li 14 Zn(GeO4)4, LiTi2(PO4)3, Li 1+x Al x Ti 2-x (PO4)3, Li 1+y Al y Ge 2-y One or more of (PO4)3, 0 < x < 2, 0 < y < 2.

[0202] Optionally, the polymer solid electrolyte material can be formed by complexing a polymer matrix material with a lithium salt. Optionally, the polymer matrix material can be one or more of, but not limited to, polyethylene oxide (PEO) and its derivatives, polypropylene oxide (PPO) and its derivatives, polycarbonate (PPC), polyacrylonitrile (PAN), polysiloxane (PDMS), polyvinylidene fluoride (PVDF), and polymethyl methacrylate (PMMA). Optionally, the lithium salt can be one or more of, but not limited to, LiClO4, LiAsF4, LiPF6, LiBF4, LiTFSI, and LiFSI.

[0203] Optionally, the polymer solid electrolyte material can be formed by complexing a polymer matrix material with a sodium salt. Optionally, the polymer matrix material can be one or more of, but not limited to, polyethylene oxide (PEO) and its derivatives, polypropylene oxide (PPO) and its derivatives, polycarbonate (PPC), polyacrylonitrile (PAN), polysiloxane (PDMS), polyvinylidene fluoride (PVDF), and polymethyl methacrylate (PMMA). Optionally, the sodium salt can be one or more of, but not limited to, NaAsF4, NaPF6, NaBF4, NaTFSI, and NaFSI.

[0204] Optionally, the polymer solid electrolyte material may also include an inert filler, which can reduce the crystallinity of the polymer and improve its mechanical properties. Optionally, the inert filler may include, but is not limited to, one or more of TiO2, Al2O3, ZrO2, and SiO2.

[0205] In some embodiments, the electrolyte layer may or may not include a binder, depending on the manufacturing process of the solid-state battery cell. Optionally, the binder may include, but is not limited to, one or more of the following: polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), ethylene-tetrafluoroethylene-propylene terpolymer, ethylene-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, styrene-butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, methyl vinyl silicone rubber, nitrile rubber (NBR), hydrogenated nitrile rubber (HNBR), thermoplastic styrene-butadiene rubber (SBS), isoprene rubber, butadiene rubber (BR), ethyl cellulose, fluororubber, and acrylate rubber.

[0206] In some embodiments, the solid-state battery cell may further include an outer packaging for accommodating the electrode assembly formed by assembling the negative electrode, electrolyte layer, and positive electrode. The outer packaging may be a rigid shell, such as a hard plastic shell, aluminum shell, or steel shell. The outer packaging may also be a flexible package, such as a pouch. The material of the flexible package may be plastic, such as one or more of aluminum-plastic film, polypropylene, polybutylene terephthalate (PBT), and polybutylene succinate (PBS).

[0207] [Preparation methods for solid-state battery cells]

[0208] The methods for preparing solid-state battery cells are well known. For example, the assembly methods of solid-state battery cells include, but are not limited to, coin cells, mold cells, hard-case cells, and pouch cells.

[0209] This disclosure also provides a method for preparing an interface layer material.

[0210] The preparation method of the interface layer material includes the following steps: providing a core; forming a shell on the surface of the core to obtain the interface layer material, the interface layer material comprising a core and a shell located on at least a portion of the surface of the core, and the electronic conductivity of the interface layer material is 10. -2 S·cm -1 ~5×10 2 S·cm -1 .

[0211] By adjusting parameters such as the material composition of the core, the material composition of the shell, and the ratio of the core to the shell, an interface layer material that meets the given electronic conductivity can be prepared.

[0212] In some embodiments, the step of forming a shell on the surface of the core includes the following steps: providing a shell material; and coating the core surface with the shell material to obtain an interface layer material.

[0213] The above-mentioned coating can be carried out in a variety of ways, such as chemical vapor deposition (CVD), magnetron sputtering, etc., to deposit shell materials on the core surface, but is not limited to these methods.

[0214] In some embodiments, the core comprises carbon material and the shell comprises carbon material.

[0215] The steps for forming a shell on the surface of the core include the following: acid washing the core with an acid solution to form a shell on the core surface, thereby obtaining an interface layer material.

[0216] The type of acid, the concentration of the acid solution, the temperature of the pickling treatment, and the pickling time can be adjusted according to actual needs, and the embodiments disclosed herein do not limit these.

[0217] In some embodiments, the solution used for pickling may include aqueous solutions of hydrochloric acid, sulfuric acid, nitric acid, hydrofluoric acid, or a mixture of at least two of the foregoing.

[0218] In some embodiments, the concentration of the solution used for pickling can be 0.5 mol / L to 1 mol / L.

[0219] In some embodiments, the pickling temperature can be 25°C-30°C.

[0220] In some embodiments, the pickling process can last for 6-12 hours.

[0221] Example

[0222] The following embodiments describe the disclosure of this disclosure in more detail. These embodiments are merely illustrative, as various modifications and variations will be apparent to those skilled in the art within the scope of this disclosure. Unless otherwise stated, all parts, percentages, and ratios reported in the following embodiments are based on mass, and all reagents used in the embodiments are commercially available or synthesized by conventional methods and can be used directly without further processing, and the instruments used in the embodiments are commercially available.

[0223] Example 1

[0224] Preparation of interface layer materials

[0225] Al₂O₃ cores with a Dv₅₀ of 50 nm were placed in the reaction chamber of a CVD apparatus and sealed. The heating temperature was set to 850 °C. Acetylene (carbon source gas) and argon (carrier gas) were introduced at a ratio of 1:5 and a flow rate of 3 L / min. Under the influence of the high temperature and gaseous atmosphere, the carbon source gas decomposed or reacted, depositing an amorphous carbon layer on the core to obtain the interface layer material. The parameters of the interface layer material are detailed in Table 1.

[0226] Preparation of negative electrode

[0227] The interface layer material prepared above is mixed with the binder polyvinylidene fluoride (PVDF) at a mass ratio of 95:5, and the solvent N-methylpyrrolidone (NMP) is added. The mixture is stirred and mixed thoroughly to obtain an interface layer slurry. The interface layer slurry is coated on the copper foil of the negative electrode current collector, dried, cold-pressed, cut to a suitable size, and the tabs are welded to obtain the negative electrode.

[0228] Preparation of positive electrode

[0229] LiNi, the positive electrode active material 0.8 Co 0.1 Mn 0.1 O2, solid electrolyte material Li6PS5Cl, positive electrode conductive agent vapor-grown carbon fiber (VGCF), and positive electrode binder polytetrafluoroethylene (PTFE) are mixed evenly in a mass ratio of 70:26:3:1. The mixture is heated on a heating table at 80°C and rolled back and forth to form a dry positive electrode active material layer. Then, it is combined with the positive electrode current collector aluminum foil hot roller, cut to the appropriate size, and welded with tabs to obtain the positive electrode.

[0230] Preparation of electrolyte layer

[0231] The solid electrolyte material Li6PS5Cl and the binder polytetrafluoroethylene (PTFE) were mixed evenly at a mass ratio of 99:1, heated on a heating table at 80°C, and rolled back and forth to form a dry electrolyte layer.

[0232] Preparation of solid-state battery cells

[0233] The negative electrode, electrolyte layer and positive electrode are stacked in order from bottom to top to obtain the electrode assembly. After being subjected to 600MPa isostatic pressing, the electrode assembly is encapsulated in an aluminum-plastic bag to obtain a soft-pack solid-state battery cell.

[0234] Example 2

[0235] Except for the following differences, the preparation of the pouch solid-state battery cells is the same as in Example 1.

[0236] Preparation of interface layer materials

[0237] Al₂O₃ cores with a Dv₅₀ of 50 nm were placed in the reaction chamber of a CVD apparatus and sealed. The heating temperature was set to 850 °C. Acetylene (carbon source gas) and argon (carrier gas) were introduced at a ratio of 1:5 and a flow rate of 3 L / min. Under the influence of the high temperature and gaseous atmosphere, the carbon source gas decomposed or reacted, depositing an amorphous carbon layer on the core to obtain the interface layer material. The parameters of the interface layer material are detailed in Table 1.

[0238] Example 3

[0239] Except for the following differences, the preparation of the pouch solid-state battery cells is the same as in Example 1.

[0240] Preparation of interface layer materials

[0241] Al₂O₃ cores with a Dv₅₀ of 900 nm were placed in the reaction chamber of a CVD apparatus and sealed. The heating temperature was set to 850 °C. Acetylene (carbon source gas) and argon (carrier gas) were introduced at a ratio of 1:5 and a flow rate of 3 L / min. Under the influence of the high temperature and gaseous atmosphere, the carbon source gas decomposed or reacted, depositing an amorphous carbon layer on the core to obtain the interface layer material. The parameters of the interface layer material are detailed in Table 1.

[0242] Example 4

[0243] Except for the following differences, the preparation of the pouch solid-state battery cells is the same as in Example 1.

[0244] Preparation of interface layer materials

[0245] A core Al₂O₃ with a Dv₅₀ of 16 nm was placed in the reaction chamber of a CVD apparatus and sealed. The heating temperature was set to 850 °C. Acetylene (carbon source gas) and argon (carrier gas) were introduced at a ratio of 1:5 and a flow rate of 3 L / min. Under the influence of the high temperature and gaseous atmosphere, the carbon source gas decomposed or reacted, depositing an amorphous carbon layer on the core to obtain the interface layer material. The parameters of the interface layer material are detailed in Table 1.

[0246] Example 5

[0247] Except for the following differences, the preparation of the pouch solid-state battery cells is the same as in Example 1.

[0248] Preparation of interface layer materials

[0249] Conductive carbon black (Super P, SP) with a core density of 35 nm was magnetically stirred in 1 mol / L dilute hydrochloric acid at 25 °C for 10 h, then filtered. The material was then washed with deionized water and dried in a vacuum oven at 80 °C for 12 h to obtain the interface layer material. The parameters of the interface layer material are detailed in Table 1.

[0250] Example 6

[0251] Except for the following differences, the preparation of the pouch solid-state battery cells is the same as in Example 1.

[0252] Preparation of interface layer materials

[0253] An interface layer material was obtained by forming a LiFePO4 shell on the surface of a core Al2O3 with a Dv50 of 50 nm using magnetron sputtering. The parameters of the interface layer material are detailed in Table 1.

[0254] Example 7

[0255] Except for the following differences, the preparation of the pouch solid-state battery cells is the same as in Example 1.

[0256] Preparation of interface layer materials

[0257] The negative electrode active material Li4Ti5O was formed on the surface of an Al2O3 core with a Dv50 of 50 nm by magnetron sputtering. 12 The shell layer is then used to obtain the interface layer material. Parameters of the interface layer material are detailed in Table 1.

[0258] Example 8

[0259] Except for the following differences, the preparation of the pouch solid-state battery cells is the same as in Example 1.

[0260] Preparation of interface layer materials

[0261] The core ion conductor material with a Dv50 of 90nm is lithium lanthanum zirconium oxide (Li7La3Zr2O). 12 LLZO was placed in the reaction chamber of the CVD equipment and sealed, and the heating temperature was set to 850℃. Acetylene (carbon source gas) and argon (carrier gas) were introduced, with a carbon source gas to carrier gas ratio of 1:5 and a flow rate of 3 L / min. Under the influence of high temperature and gas atmosphere, the carbon source gas decomposed or reacted, depositing an amorphous carbon layer in the core to obtain the interface layer material. The parameters of the interface layer material are detailed in Table 1.

[0262] Comparative Example 1

[0263] Except for the following differences, the preparation of the pouch solid-state battery cells is the same as that of Comparative Example 1.

[0264] Preparation of negative electrode layer

[0265] Al2O3 with a Dv50 of 50 nm and polyvinylidene fluoride (PVDF) binder were mixed at a mass ratio of 95:5. N-methylpyrrolidone (NMP) solvent was added and the mixture was stirred thoroughly to obtain an interface layer slurry. The interface layer slurry was coated onto the copper foil of the negative electrode current collector, dried, cold-pressed, cut to a suitable size, and the tabs were welded to obtain the negative electrode layer.

[0266] Comparative Example 2

[0267] Except for the following differences, the preparation of the pouch solid-state battery cells is the same as that of Comparative Example 1.

[0268] Preparation of negative electrode layer

[0269] SP with a Dv50 of 35nm and polyvinylidene fluoride (PVDF) binder were mixed at a mass ratio of 95:5. N-methylpyrrolidone (NMP) solvent was added and the mixture was stirred thoroughly to obtain an interface layer slurry. The interface layer slurry was coated onto the copper foil of the negative electrode current collector, dried, cold-pressed, cut to a suitable size, and the tabs were welded to obtain the negative electrode layer.

[0270] Comparative Example 3

[0271] Except for the following differences, the preparation of the pouch solid-state battery cells is the same as that of Comparative Example 1.

[0272] Preparation of negative electrode layer

[0273] LLZO with a Dv50 of 100 nm and polyvinylidene fluoride (PVDF) binder were mixed at a mass ratio of 95:5. N-methylpyrrolidone (NMP) solvent was added and the mixture was stirred thoroughly to obtain an interface layer slurry. The interface layer slurry was coated onto the copper foil of the negative electrode current collector, dried, cold-pressed, cut to a suitable size, and the tabs were welded to obtain the negative electrode layer.

[0274] Performance testing

[0275] (1) First coulombic efficiency test of solid-state battery cell

[0276] At 25°C, solid-state battery cells were charged to 4.3V (vs. Li) at a current density of 0.1C. + / Li), let stand for 10 minutes, then discharge to 2.5V at a current density of 0.1C (vs. Li). + / Li), to obtain the specific capacity of the first charge and the specific capacity of the first discharge.

[0277] The initial coulombic efficiency (%) of a solid-state battery cell = first discharge specific capacity / first charge specific capacity × 100%.

[0278] (2) Rate performance test of solid-state battery cells

[0279] At 25°C, the solid-state battery cell was first charged to 4.3V (vs. Li) at a current density of 0.1C. + / Li), let stand for 10 minutes, then discharge to 2.5V at a current density of 0.1C (vs. Li). + The solid-state battery cell was charged and discharged 5 times, and the resulting capacity was recorded as the discharge specific capacity at a rate of 0.1C. Then, the solid-state battery cell was charged to 4.3V (vs. Li) at a current density of 0.1C. + / Li), let stand for 10 minutes, then discharge to 2.5V at a current density of 2C (vs. Li). + The capacity obtained by 5 cycles of charge and discharge ( / Li) is recorded as the discharge specific capacity at a 2C rate.

[0280] (3) Cyclic performance test of solid-state battery cells

[0281] At 25°C, the solid-state battery cells were first charged to 4.3V (vs. Li) at a current density of 0.5C. + / Li), let stand for 10 minutes, then discharge at a current density of 0.5C to 2.5V (vs. Li). + / Li), the discharge specific capacity at this time is recorded as C1. The solid-state battery cell is cycled 200 times at a current density of 0.5C, and the discharge capacity at this time is recorded as C2.

[0282] The capacity retention rate of a solid-state battery cell after 200 cycles at a current density of 0.5C is calculated as C2 / C1 × 100%.

[0283] During the above test, a pressure of 5 MPa was applied to the solid-state battery cell.

[0284] The performance test results of Examples 1-8 and Comparative Examples 1-3 are detailed in Table 2.

[0285] Table 1

[0286]

[0287] Table 2

[0288]

[0289] In Table 1, " / " indicates that the corresponding structure is not present or the corresponding parameter cannot be measured.

[0290] The test results in Tables 1 and 2 show that the interface layer material has a core-shell structure and its electronic conductivity is within a suitable range, which can improve the cycle performance of electrodeless lithium metal solid-state battery cells. By adjusting the composition and structure of the interface layer material, the initial coulombic efficiency and rate performance of the solid-state battery cells can be further improved.

[0291] It should be noted that this disclosure is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this disclosure are included within the technical scope of this disclosure. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, are also included within the scope of this disclosure without departing from the spirit of this disclosure.

Claims

1. A solid-state battery cell, comprising a positive electrode, an electrolyte layer, and a negative electrode, wherein the electrolyte layer is located between the positive electrode and the negative electrode, characterized in that, The negative electrode includes a negative electrode current collector and an interface layer located on at least one side of the negative electrode current collector. The interface layer includes an interface layer material, which includes a core and a shell located on at least a portion of the surface of the core. The electronic conductivity of the interface layer material is 1×10⁻⁶. -2 S·cm -1 ~5×10 2 S·cm -1 .

2. The solid-state battery cell according to claim 1, characterized in that, The core comprises at least one of an insulating material, an electronic conductor material, or an ionic conductor material; and / or, The shell layer includes at least one of electronic conductor materials, ionic conductor materials, and electronic-ionic dual conductor materials.

3. The solid-state battery cell according to claim 2, characterized in that, The shell layer comprises one or more of the following: conductive carbon black, amorphous carbon, lithium transition metal oxides and their modified forms, lithium phosphates and their modified forms, lithium titanate, lithium niobate, sulfur, selenium, tellurium, sodium transition metal oxides, polyanionic materials, Prussian blue materials, natural graphite, artificial graphite, mesophase microcarbon spheres, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, and metal oxides; and / or, The core includes at least one of metal oxides, polymer insulating materials, metals, carbon materials, electron-ion dual-conducting positive electrode active materials, electron-ion dual-conducting negative electrode active materials, and solid electrolyte materials. The solid electrolyte materials include one or more of sulfide solid electrolyte materials, halide solid electrolyte materials, oxide solid electrolyte materials, and polymer solid electrolyte materials.

4. The solid-state battery cell according to claim 2, characterized in that, The core comprises an insulating material, and the shell comprises at least one of an electronic conductor material and an electronic-ion dual conductor material; Alternatively, the core may comprise an ionic conductor material, and the shell may comprise at least one of an electronic conductor material and an electronic-ionic dual conductor material; Alternatively, the core may comprise an electronic conductor material, and the shell may comprise at least one of an electronic conductor material, an ionic conductor material, and an electronic-ionic dual conductor material.

5. The solid-state battery cell according to any one of claims 1-4, characterized in that, The shell comprises at least one of an electronic conductor material and an electronic-ion dual conductor material, and the electronic conductivity of the shell is 10. -4 S·cm -1 The above can be selected as 10. -4 S·cm -1 ~100S·cm -1 .

6. The solid-state battery cell according to any one of claims 1-4, characterized in that, The shell layer comprises at least one of an ion-conducting material and an electron-ion dual-conducting material, and the ionic conductivity of the shell layer is 10. -6 S·cm -1 The above can be selected as 10. -6 S·cm -1 ~10 -2 S·cm -1 .

7. The solid-state battery cell according to any one of claims 1-6, characterized in that, The core comprises an electronically conductive material, and the shell comprises at least one of an electronically conductive material and an electron-ion dual-conductor material, wherein the ratio of the electronic conductivity of the shell to the electronic conductivity of the core is 1:1 to 10. 11 :

1.

8. The solid-state battery cell according to any one of claims 1-7, characterized in that, The core comprises an ionic conductor material, and the shell comprises at least one of an ionic conductor material and an electron-ion dual conductor material, wherein the ratio of the ionic conductivity of the shell to the ionic conductivity of the core is 0.1:1 to 10. 3 :

1.

9. The solid-state battery cell according to any one of claims 1-8, characterized in that, The core comprises an insulating material or an electronically conductive material, and the shell comprises an electronically conductive material. When the solid-state battery cell is fully charged, the ionic conductivity of the interface layer material is 10. -6 S·cm -1 ~10 -2 S·cm -1 .

10. The solid-state battery cell according to any one of claims 1-8, characterized in that, The core comprises an ion-conducting material, and / or the shell comprises an ion-conducting material or an electron-ion dual-conductor material, wherein the ionic conductivity of the interface layer material is 10. -6 S·cm -1 ~10 -2 S·cm -1 .

11. The solid-state battery cell according to any one of claims 1-10, characterized in that, The shell layer comprises carbon material, the core layer comprises carbon material, and the shell layer I D / I G Greater than the kernel's I D / I G I D This indicates that the Raman spectrum is at 1350±50 cm⁻¹. -1 D peak intensity at I G This indicates that the Raman spectrum is at 1580±50 cm⁻¹. -1 The intensity of the G peak at that location.

12. The solid-state battery cell according to any one of claims 1-11, characterized in that, The shell layer comprises carbon material, the core layer comprises carbon material, and the shell layer I D / I G The value is 1.62 to 1.72, and / or the I of the kernel is... D / I G It is 1.60 to 1.65, I D This indicates that the Raman spectrum is at 1350±50 cm⁻¹. -1 D peak intensity at I G This indicates that the Raman spectrum is at 1580±50 cm⁻¹. -1 The intensity of the G peak at that location.

13. The solid-state battery cell according to any one of claims 1-12, characterized in that, The shell layer comprises a carbon material, which contains non-carbon elements, including O and / or F elements. The core comprises a carbon material, which contains non-carbon elements, including O and / or F elements. Furthermore, the ratio of the mass content of carbon elements to the mass content of non-carbon elements in the shell is less than the ratio of the mass content of carbon elements to the mass content of non-carbon elements in the core.

14. The solid-state battery cell according to any one of claims 1-13, characterized in that, The shell comprises a carbon material containing non-carbon elements, and the ratio of the mass content of carbon elements to the mass content of non-carbon elements in the shell is 40 to 800; and / or, The shell layer comprises carbon material containing non-carbon elements, and the ratio of the mass content of carbon elements to the mass content of non-carbon elements in the core is 600 to 1500.

15. The solid-state battery cell according to any one of claims 1-14, characterized in that, The porosity of the shell is greater than that of the core.

16. The solid-state battery cell according to any one of claims 1-15, characterized in that, The porosity of the shell is 1% to 20%; and / or, The porosity of the core is 0-5%.

17. The solid-state battery cell according to any one of claims 1-16, characterized in that, The thickness of the shell layer is 2 nm to 50 nm; and / or, The volumetric particle size Dv50 of the interface layer material is 20 nm to 2 μm; and / or; The ratio of the thickness of the shell layer to the volume distribution particle size Dv50 of the interface layer material is 2.5:100 to 45:

100.

18. The solid-state battery cell according to any one of claims 1-17, characterized in that, The NP ratio of the solid-state battery cell is 0.01 to 0.05, where the NP ratio is the ratio of the negative electrode capacity per unit area to the positive electrode capacity per unit area.

19. A battery device, characterized in that, It includes any one of the solid-state battery cells according to claims 1-18.

20. An electrical appliance, characterized in that, Includes the solid-state battery cell according to any one of claims 1-18 or the battery device according to claim 19.

21. A method for preparing the interface layer material according to any one of claims 1-18, characterized in that, The process includes the following steps: providing a core; forming a shell on the surface of the core to obtain an interface layer material, the interface layer material comprising the core and a shell located on at least a portion of the surface of the core, and the interface layer material having an electronic conductivity of 1 × 10⁻⁶. -2 S·cm -1 ~5×10 2 S·cm -1 .

22. The method according to claim 21, characterized in that, The step of forming a shell on the surface of the core includes the following steps: providing a shell material; and coating the surface of the core with the shell material to obtain the interface layer material.

23. The method according to claim 21, characterized in that, The core comprises carbon material, and the shell comprises carbon material; The step of forming a shell on the surface of the core includes the following steps: acid washing the core with an acid solution to form a shell on the surface of the core, thereby obtaining the interface layer material.