Method for preparing oxide-based flexible composite solid electrolyte membrane with island structure
The oxide-based flexible composite solid electrolyte membrane with an island-reef structure is formed by high-temperature sintering and ultrafast laser cutting. The inorganic-organic interface is bridged by silane coupling agent, which solves the problems of brittleness and interface compatibility of oxide solid electrolyte and realizes high conductivity and flexible production.
Patent Information
- Application Number
- CN202610806762.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-06-05
- Publication Date
- 2026-11-24
AI Technical Summary
Oxide solid electrolytes exhibit extremely high ceramic rigidity and brittleness after high-temperature sintering, making them unable to withstand bending stress. Furthermore, the inorganic/organic interface suffers from severe contact problems and poor compatibility, limiting their application in the flexibility and large-scale production of all-solid-state lithium batteries.
A flexible composite solid electrolyte membrane with an oxide-based structure is formed by combining high-temperature sintering with ultrafast laser cutting and chemical bridging with silane coupling agent. Through-slits are formed on the oxide ceramic substrate by ultrafast laser cutting, and chemical bridging is formed between the silane coupling agent and the oxide and polymer in the slits.
It achieves high conductivity, macroscopic flexibility and excellent interfacial compatibility of oxide electrolyte, can withstand large-angle bending, is suitable for flexible mass production of all-solid-state batteries, reduces interfacial impedance and improves mechanical tensile strength.
Smart Images

Figure CN123162299A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of new energy solid-state battery manufacturing technology, and in particular to a process for preparing an oxide-based flexible composite solid-state electrolyte membrane with an island-reef structure by combining high-temperature sintering, laser precision cutting and silane coupling agent interface modification. Background Technology
[0002] Oxide solid electrolytes (such as garnet-type LLZO and NASICON-type LATP) have excellent chemical stability to lithium metal, a wide electrochemical window, and high room temperature ionic conductivity. They are also relatively stable in air, making them extremely important electrolyte materials for all-solid-state lithium batteries.
[0003] However, oxide solid electrolytes typically require high-temperature sintering (600℃~1200℃) to achieve densification and eliminate grain boundary resistance. The sintered oxides exhibit extremely high ceramic rigidity and brittleness. This inherently "hard and brittle" physical characteristic makes them unable to withstand any bending stress, severely limiting their application in the large-scale roll-to-roll production of power batteries. Furthermore, to impart flexibility, polymer materials are often introduced to prepare composite electrolytes. However, the significant difference in surface energy between inorganic oxide ceramics and organic polymers leads to severe contact problems and poor compatibility at the interface, resulting in a sharp increase in the interfacial ion transport impedance of the composite film.
[0004] Therefore, how to not only endow oxide solid-state batteries with macroscopic flexibility while retaining their high electrical conductivity in high-temperature sintered dense bodies, but also effectively solve the high impedance problem at the inorganic / organic interface is a key technological bottleneck currently facing the industrialization of oxide solid-state batteries. Summary of the Invention
[0005] To address the problems in the prior art, the present invention aims to provide a method for preparing an oxide-based flexible composite solid electrolyte membrane with an island-reef structure. This method ingeniously combines the intrinsic properties of oxides, and through a combined process of "high-temperature sintering - ultrafast laser cutting - silane coupling agent chemical bridging - polymer filling," perfectly achieves the high conductivity, macroscopic flexibility, and excellent interfacial compatibility of the oxide electrolyte.
[0006] A method for preparing an oxide-based flexible composite solid electrolyte membrane with an island-reef structure includes the following steps:
[0007] Step S1: Sintering of ceramic green body. After pressing the oxide solid electrolyte powder into shape, it is sintered at high temperature at 600℃~1200℃ to fully densify it, thereby obtaining a continuous dense oxide ceramic substrate with a preset thickness, and then fixing it on the processing stage.
[0008] Step S2: Ultrafast laser mesh cutting. An ultrafast laser is used to perform mesh scanning and cutting on the fixed ceramic substrate, forming crisscrossing through-slits, thereby dividing the originally continuous ceramic substrate into several independent, highly conductive ceramic island units arranged in an array.
[0009] Step S3: Coupling agent interface modification. A surface treatment liquid containing a silane coupling agent is introduced into the gap. The naturally occurring free hydroxyl groups (-OH) on the cut cross-section of the oxide ceramic react with the silanol groups generated by the hydrolysis of the silane coupling agent through a dehydration condensation reaction. After drying, an interface modification layer is firmly bonded to the cut sidewall of the high-conductivity ceramic island unit.
[0010] Step S4: Polymer Casting and Filling. A flexible polymer is dissolved in a solvent to prepare a casting slurry. Using a casting coating process, the slurry is applied to the cut substrate surface, allowing it to penetrate and fill the gaps.
[0011] Step S5: Drying and curing. The solvent evaporates at a preset temperature, and the organic functional groups of the flexible polymer and the silane coupling agent undergo physical entanglement or chemical bonding. The molding and curing process forms a flexible polymer network that connects all the ceramic island units into a whole. After demolding, a flexible composite solid electrolyte membrane is obtained.
[0012] The beneficial effects of this application are:
[0013] 1. High-temperature sintering ensures high conductivity, and ultrafast laser breaks through processing limits: Only through high-temperature sintering can the high ionic conductivity of oxide electrolytes be brought into play; for extremely brittle and hard ceramic sheets after sintering, ultrafast laser (picosecond / femtosecond) is used for "cold ablation" cutting, avoiding the fatal defect of ceramic sheet breakage caused by traditional mechanical cutting, and realizing the non-destructive construction of micro-nano structures for hard and brittle materials.
[0014] 2. Silane coupling agents achieve "inorganic-organic" chemical bridging, significantly reducing interfacial impedance: Taking full advantage of the hydroxyl-rich surface of oxide ceramics, silane coupling agents are introduced as "chemical bridges." One end is firmly anchored to the sidewall of the oxide ceramic via covalent bonds, while the other end is tightly bonded to the flexible polymer network. This molecular-level interfacial modification completely eliminates interfacial gaps and repulsion between inorganic islands and organic polymers, significantly reducing interfacial impedance and greatly enhancing the mechanical tensile strength of the composite film.
[0015] 3. Excellent flexibility and roll-to-roll (R2R) production potential: The rigid oxide islands arranged in an array are isolated and connected by a flexible polymer network (reef chain), which gives the originally extremely brittle ceramic sheet a macroscopic flexibility similar to "chainmail". It can withstand large-angle bending and is extremely suitable for the large-scale flexible mass production of all-solid-state batteries. Attached Figure Description
[0016] Figure 1 This is a flowchart illustrating the preparation process of the flexible oxide composite solid electrolyte membrane for island and reef structures according to the present invention.
[0017] Figure 2 This is a schematic diagram of the preparation process of the flexible oxide composite solid electrolyte membrane for island and reef structures according to the present invention.
[0018] Figure 3 This is a photograph of the flexible composite solid electrolyte membrane prepared according to Example 1 of this application.
[0019] Figure 4 Impedance diagrams of flexible composite solid electrolyte membranes prepared according to Example 1 and Comparative Example 1 of this application.
[0020] Figure 5 This is a constant current charge-discharge cycle voltage-time curve of the symmetrical battery in Example 1. Detailed Implementation Plan
[0021] The embodiments of this application are described in detail below, and the technical solutions in the embodiments are clearly and completely described.
[0022] like Figure 1 , Figure 2 As shown, this invention relates to a method for preparing an oxide-based flexible composite solid electrolyte membrane with an island-reef structure, comprising the following steps:
[0023] Step S1: Sintering of ceramic green body. After pressing the oxide solid electrolyte powder into shape, it is sintered at high temperature at 600℃~1200℃ to fully densify it, thereby obtaining a continuous dense oxide ceramic substrate with a preset thickness, and then fixing it on the processing stage.
[0024] Step S2: Ultrafast laser mesh cutting. An ultrafast laser is used to perform mesh scanning and cutting on the fixed ceramic substrate, forming crisscrossing through-slits, thereby dividing the originally continuous ceramic substrate into several independent, highly conductive ceramic island units arranged in an array.
[0025] Step S3: Coupling agent interface modification. A surface treatment liquid containing a silane coupling agent is introduced into the gap. The naturally occurring free hydroxyl groups (-OH) on the cut cross-section of the oxide ceramic react with the silanol groups generated by the hydrolysis of the silane coupling agent through a dehydration condensation reaction. After drying, an interface modification layer is firmly bonded to the cut sidewall of the high-conductivity ceramic island unit.
[0026] Step S4: Polymer Casting and Filling. A flexible polymer is dissolved in a solvent to prepare a casting slurry. Using a casting coating process, the slurry is applied to the cut substrate surface, allowing it to penetrate and fill the gaps.
[0027] Step S5: Drying and curing. The solvent evaporates at a preset temperature, and the organic functional groups of the flexible polymer and the silane coupling agent undergo physical entanglement or chemical bonding. The molding and curing process forms a flexible polymer network that connects all the ceramic island units into a whole. After demolding, a flexible composite solid electrolyte membrane is obtained.
[0028] In some embodiments, in step S2, the ultrafast laser is preferably a picosecond laser or a femtosecond laser. These types of cold-processing lasers can induce "cold ablation" of materials through multiphoton absorption, controlling the heat-affected zone at the sub-micron level and avoiding damage to the crystalline phase at the sulfide edges.
[0029] In some embodiments, in step S2, the width of the slit formed by cutting is controlled between 1 μm and 200 μm, and the maximum lateral feature size of the formed highly conductive island unit is controlled between 0.5 mm and 5 mm. In some embodiments, in step S3, in order to protect the sulfide electrolyte which is sensitive to polar environments, the non-polar solvent is strictly selected from at least one of toluene, xylene, n-hexane, n-heptane, or cyclohexane; the non-polar elastomer is selected from at least one of styrene-ethylene-butene-styrene block copolymer (SEBS), polyisobutylene (PIB), and styrene-butadiene rubber (SBR).
[0030] Example 1: High-temperature sintering of oxides and preparation of ceramic substrates, including weighing Li 6.4 La3Zr 1.4 Ta 0.6 O 12 (LLZO) tantalum-doped garnet-type solid electrolyte powder was pressed into a preform in a 50 mm diameter mold under a pressure of 300 MPa. The preform was then placed in a muffle furnace, buried in an alumina crucible with master powder, and sintered at 1150 °C for 12 h. After natural cooling, the surface was polished to obtain a dense LLZO ceramic substrate with a thickness of approximately 80 μm and a relative density greater than 95%.
[0031] Ultrafast laser mesh cutting involves fixing the obtained LLZO dense ceramic substrate onto a processing platform; performing mesh scanning cutting using a femtosecond laser (wavelength 1030nm, pulse width 300fs, repetition frequency 100kHz); setting the cutting spacing to 1.5mm and the kerf width to approximately 80μm; and using laser pulses to ablate the LLZO ceramic without thermal damage, ultimately forming a regularly arranged island-shaped LLZO ceramic array.
[0032] The silane coupling agent interface modification involves preparing a 2% (v / v) KH560 (γ-(2,3-epoxypropoxy)propyltrimethoxysilane) ethanol / water mixed solution; spraying this solution into the laser-cut slits; and then vacuum baking at 80°C for 2 hours. During this process, the methoxy groups of KH560 hydrolyze and undergo a condensation reaction with the hydroxyl groups (-OH) on the cut surface of the LLZO ceramic to form a strong Si-O-metal bond layer, while the epoxy groups at the other end face outwards for subsequent bonding with polymers.
[0033] The preparation of a flexible polymer-filled composite membrane involves weighing 0.8 g of PVDF-HFP and an appropriate amount of LiTFSI lithium salt, dissolving them in DMF solvent, and stirring at 60°C until homogeneous. The resulting casting liquid is then coated onto the surface of a modified ceramic substrate, allowing the liquid to completely penetrate the gaps using capillary action. The substrate is then dried under vacuum at 60°C for 24 hours, and demolded after solvent evaporation. The coupling agent on the modified layer surface tightly binds to PVDF-HFP, ultimately forming a highly flexible "island-reef structure" LLZO / PVDF-HFP composite electrolyte membrane. Figure 3 As shown.
[0034] Comparative Example 1: Without silane coupling agent modification, the cut LLZO ceramic substrate was prepared using the same method as in Example 1, but the interface modification step was skipped, and PVDF-HFP polymer filling and drying curing were performed directly.
[0035] Testing and verification.
[0036] Interfacial Impedance Testing (EIS): The composite membranes obtained in Example 1 and Comparative Example 1 were subjected to AC impedance testing. The results showed that the composite membrane of Example 1, modified with KH560 silane coupling agent, had an interfacial impedance of only 85 Ω·cm²; while the unmodified composite membrane of Comparative Example 1, due to microscopic delamination and poor contact between the polymer and ceramic, had an interfacial impedance as high as 310 Ω·cm². This proves that the silane coupling agent achieves effective "chemical bridging".
[0037] Mechanical flexibility test: The composite membrane obtained in Example 1 can withstand more than 100 continuous 180° bends around a 5mm radius cylinder without breaking. SEM cross-sectional images show that after repeated bending, the PVDF-HFP polymer and LLZO ceramic interface remain densely bonded, and no delamination occurs.
[0038] Battery cycle performance: The Li|Li symmetric battery assembled using the composite solid electrolyte membrane prepared in Example 1 can stably achieve more than 800 hours of lithium deposition / stripping cycle at a current density of 0.5 mA / cm², with stable polarization voltage and no lithium dendrite penetration short circuit.
[0039] Figure 4 and Figure 5 The EIS impedance spectra of the composite solid electrolyte membranes of Example 1 and Comparative Example 1 are presented, along with the cycle performance test results of the Li|Li symmetric battery assembled using the membrane of Example 1. Figure 4 As can be seen, the interfacial impedance of Example 1 after silane coupling agent interface modification is significantly lower than that of the unmodified Comparative Example 1; Figure 5 As can be seen, the symmetrical battery using the electrolyte membrane of Example 1 can cycle stably for over 800 hours at a current density of 0.5 mA / cm², with stable polarization voltage and no significant decay. These results collectively demonstrate that the method for preparing the oxide-based flexible composite solid electrolyte membrane with an island-reef structure of the present invention effectively solves the problems of high interfacial impedance and mechanical brittleness of oxide solid electrolytes by constructing the island-reef structure through ultrafast laser cutting and utilizing a silane coupling agent to achieve inorganic-organic interfacial chemical bonding, significantly improving the interfacial stability and long-term cycling performance of the composite electrolyte membrane.
[0040] Example 2: Preparation of an oxide-based flexible composite solid electrolyte membrane using KH570 silane coupling agent and PEO polymer.
[0041] Weigh Li 6.4 La3Zr 1.4 Ta 0.6 O 12 (LLZO) tantalum-doped garnet-type solid electrolyte powder was pressed into a preform in a 50mm diameter mold under a pressure of 300MPa. The preform was then placed in a muffle furnace, buried in an alumina crucible with master powder, and sintered at 1150℃ for 12 hours. After natural cooling, the surface was polished to obtain a dense LLZO ceramic substrate with a thickness of approximately 80μm and a relative density greater than 95%.
[0042] The obtained LLZO dense ceramic substrate was fixed on the processing platform; a femtosecond laser was used for grid scanning and cutting, with a wavelength of 1030nm, a pulse width of 300fs, and a repetition frequency of 100kHz; the cutting spacing was set to 1.2mm, and the gap width was about 70μm, forming a regularly arranged island-shaped LLZO ceramic array.
[0043] A 1.5% (v / v) KH570 (γ-methacryloyloxypropyltrimethoxysilane) ethanol / water mixed solution was prepared; this solution was sprayed into the laser-cut kerf and then vacuum-baked at 80°C for 2 hours. During this process, the methoxy groups of KH570 hydrolyzed and then condensed with the hydroxyl groups on the surface of the LLZO ceramic cut section to form a strong Si-O-metal bond layer.
[0044] Weigh 1.0 g of polyethylene oxide (PEO) and an appropriate amount of lithium LiTFSI, dissolve them in acetonitrile solvent, and stir at 60 °C until homogeneous. Apply the resulting casting liquid to the surface of a modified ceramic substrate, utilizing capillary action to allow the liquid to completely penetrate the gaps. Dry under vacuum at 60 °C for 24 h, and demold after solvent evaporation. The coupling agent on the surface of the modified layer tightly binds with PEO, ultimately forming an "island-reef structure" LLZO / PEO composite electrolyte membrane with excellent flexibility.
[0045] Testing and Verification: EIS testing showed that the interfacial impedance of the composite membrane of Example 2 modified with KH570 was 92 Ω·cm², significantly lower than that of the unmodified control group (approximately 280 Ω·cm²). The membrane could withstand more than 100 continuous 180° bends around a 5 mm radius cylinder without breaking. SEM cross-sections showed a dense adhesion between the polymer and LLZO ceramic interface, with no obvious delamination. A Li|Li symmetric cell assembled using the composite membrane prepared in Example 2 could cycle stably for over 700 hours at a current density of 0.5 mA / cm², with stable polarization voltage.
[0046] Example 3: Preparation of an oxide-based flexible composite solid electrolyte membrane using LATP oxide and picosecond laser
[0047] Weigh Li 1.3 Al 0.3 Ti 1.7 (PO4)3 (LATP) sodium superionic conductor solid electrolyte powder was pressed into a preform in a 50 mm diameter mold under a pressure of 280 MPa; then sintered at 900 °C for 8 h in an alumina crucible. After natural cooling, the surface was polished to obtain a dense LATP ceramic substrate with a thickness of about 100 μm (relative density >92%).
[0048] The obtained LATP dense ceramic substrate was fixed on the processing platform; a picosecond laser was used for grid scanning and cutting, for example, with a wavelength of 1064nm, a pulse width of 10ps, and a repetition frequency of 200kHz; the cutting spacing was set to 1.0mm, and the slit width was about 90μm, forming a regularly arranged island-shaped LATP ceramic array.
[0049] Prepare a 2% (v / v) KH560 ethanol / water mixed solution; spray it into the laser-cut crevices and bake it under vacuum at 80°C for 2 hours to allow KH560 to undergo a condensation reaction with the hydroxyl groups of the LATP ceramic cutting section, forming an interface modification layer.
[0050] Weigh 0.7g of PVDF-HFP and an appropriate amount of LiTFSI lithium salt, dissolve them in DMF solvent, and stir at 60℃ until homogeneous; coat the resulting casting solution onto the surface of a modified ceramic substrate, utilizing capillary action to allow the liquid to completely penetrate the gaps; dry under vacuum at 60℃ for 24h, and demold after solvent evaporation. This ultimately forms a highly flexible "island-reef structure" LATP / PVDF-HFP composite electrolyte membrane.
[0051] Testing and Validation: EIS testing showed that the interfacial impedance of the composite membrane of Example 3 modified with KH560 was 78 Ω·cm², significantly lower than that of the unmodified control group (approximately 265 Ω·cm²). The membrane could withstand more than 100 continuous 180° bends around a 6 mm radius cylinder without breakage. SEM cross-sections showed good bonding between the polymer and LATP ceramic interface, with no obvious porosity or delamination. A Li|Li symmetric battery assembled using the composite membrane prepared in Example 3 could be stably cycled for over 650 hours at a current density of 0.4 mA / cm², with stable polarization voltage, verifying the universality of the process for different oxide systems (garnet and NASICON types).
[0052] This invention proposes an oxide-based flexible composite solid-state electrolyte membrane with an island-reef structure and its preparation method. This method cleverly utilizes high-temperature sintering to ensure the intrinsic high conductivity of the oxide, overcomes the processing challenges of hard and brittle ceramics using ultrafast lasers, and completely solves the core problem of poor inorganic / organic interface compatibility through chemical modification with a silane coupling agent. This opens up a highly promising new path for the flexible mass production of high-safety, high-energy-density oxide all-solid-state batteries.
Claims
1. A method for preparing an oxide-based flexible composite solid electrolyte film having an atoll structure, characterized by, Includes the following steps: S1: After pressing the oxide solid electrolyte powder into shape, sinter it at a preset high temperature to obtain a continuous dense oxide ceramic substrate with a preset thickness, and fix it. S2: The ceramic substrate is cut into a grid pattern using an ultrafast laser device to form a gap that penetrates the thickness of the substrate and an array of oxide ceramic islands divided by the gap; S3: Introduce a surface treatment liquid containing a silane coupling agent into the gap, and after drying, form an interface modification layer on the sidewall of the cut section of the oxide ceramic island; S4: Prepare a flexible polymer casting solution using a solvent, and use a solution casting method to penetrate and fill the gaps that have been modified by the interface; S5: Evaporate the solvent in the casting solution to allow the flexible polymer to solidify and form in the gaps, thereby obtaining the flexible composite solid electrolyte membrane.
2. The production method according to claim 1, characterized by, In step S1, the temperature range of the high-temperature sintering is 600℃ to 1200℃, and the sintering time is 2h to 24h; the preset thickness is 20μm to 200μm.
3. The preparation method according to claim 1, characterized in that, In step S1, the oxide solid electrolyte powder is selected from one of the following: garnet type (such as LLZO), sodium superionic conductor type (such as LATP, LAGP), perovskite type (such as LLTO), or lanthanum-doped lithium silicon zirconium phosphate (such as LLZSP) solid electrolyte.
4. The method of claim 1, wherein, In step S2, the ultrafast laser device is a picosecond laser or a femtosecond laser; the maximum feature size of the cross-section of the oxide ceramic island formed by cutting is 0.5mm to 5mm, and the width of the gap is 1μm to 200μm.
5. The preparation method according to claim 1, characterized in that, In step S3, the silane coupling agent contains an alkoxy group capable of undergoing a condensation reaction with hydroxyl groups on the oxide surface; the silane coupling agent is selected from at least one of KH550, KH560, KH570 or KH792.
6. The preparation method according to claim 1, characterized in that, In step S4, the flexible polymer is selected from at least one of polyethylene oxide (PEO), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), polymethyl methacrylate (PMMA), or styrene-ethylene-butene-styrene block copolymer (SEBS).