A rapid amorphous halide oxide solid electrolyte material and a preparation method and application thereof

By combining an alkaline sodium source, tantalum compounds, transition metal chlorides, and B₂O₃, and employing high-temperature pretreatment and ball milling methods, the problems of long amorphization time and high energy consumption of sodium ion halide solid electrolytes were solved, achieving a highly efficient and safe amorphization process, improving ionic conductivity, and making it suitable for the industrial production of various central metal elements.

CN123162301APending Publication Date: 2026-11-24SHENZHEN GUYAN NEW MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611235746.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-14
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

The existing amorphization process of sodium-ion halide solid electrolytes requires long-term high-energy ball milling, which is energy-intensive and has low production efficiency. In addition, the sodium dopant introduces additional Na⁺ to interfere with the optimization of ion conductivity, which poses a risk of gas generation and is not conducive to industrial preparation.

Method used

By employing a combination of alkaline sodium source, tantalum-containing compounds, transition metal chlorides, and B₂O₃, and utilizing high-temperature pretreatment and ball milling, rapid amorphization is achieved by taking advantage of the sodium-free nature and high reactivity of B₂O₃, avoiding the introduction of additional Na⁺, and constructing an amorphous network with high ionic conductivity.

Benefits of technology

It significantly shortens the amorphization time, improves ionic conductivity, reduces energy consumption, and reduces the risk of gas generation. It is suitable for a variety of central metal elements and meets the requirements of industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123162301A_ABST
    Figure CN123162301A_ABST
Patent Text Reader

Abstract

The invention relates to a rapidly amorphized oxyhalide solid electrolyte material, its preparation method and application. The preparation method includes grinding and initially mixing an alkaline sodium source, a tantalum-containing compound, a transition metal chloride, and B2O3 to obtain an initially mixed material; then pre-treating to obtain a pre-treated precursor; followed by ball milling to obtain the rapidly amorphized oxyhalide solid electrolyte material. Its general formula is: Na(Ta 1‑x M x )OCl4-yB2O3, where M is a transition metal; 0<x<1; 0<y≤0.5. The pre-treatment is responsible for chemical activation and gas discharge, and the ball milling is responsible for complete structural amorphization. The pre-treatment constructs an amorphous prototype to reduce the subsequent amorphization energy barrier. The alkaline sodium source makes the O / Cl exchange more sufficient during the pre-treatment stage, and the gas discharge in the pre-treatment stage provides more favorable thermodynamic conditions for the reaction of the alkaline sodium source; and ensures the efficient utilization of Na + within an extremely short ball milling time. Incorporating B2O3 results in high ionic conductivity (3.5 mS / cm), no additional Na + , reduced formation of NaCl impurity phases, and maintenance of a more continuous amorphous ion conduction network.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of new energy battery materials, and in particular to a fast amorphous halide oxide solid electrolyte material, its preparation method, and its application. Background Technology

[0002] With the global energy structure transformation and the advancement of "dual-carbon" goals, large-scale energy storage technology has become a key link in supporting the consumption of renewable energy and grid stability. Sodium-ion batteries are considered an ideal choice for large-scale energy storage due to the abundance, widespread distribution, and low cost of sodium resources (sodium salts are only 1 / 10 the price of lithium salts). Compared to traditional liquid electrolyte batteries, all-solid-state sodium-ion batteries use a non-flammable solid electrolyte, fundamentally eliminating safety hazards such as electrolyte leakage and thermal runaway. They are also compatible with high-voltage positive electrodes and metallic sodium negative electrodes, achieving higher energy density.

[0003] Among numerous solid-state electrolyte materials, halide solid-state electrolytes have attracted widespread attention in recent years due to their unique comprehensive properties. Halide solid-state electrolytes combine the high voltage stability of oxide electrolytes with the good mechanical deformability of sulfide electrolytes—they exhibit high oxidation stability (typically >4V vs. Na). + Sodium halide electrolytes (Na) are soft and can form good solid-solid interface contacts with electrode materials under room temperature cold pressing conditions, achieving tight interfacial bonding without high-temperature sintering. Furthermore, halide electrolytes exhibit better chemical stability than sulfides and are less prone to hydrolysis to produce toxic H2S gas, thus being considered one of the most promising electrolyte candidates for next-generation all-solid-state sodium batteries. However, the development of sodium halide solid-state electrolytes faces a core bottleneck: extremely low synthesis efficiency, long amorphization time, and high energy consumption.

[0004] To achieve high ionic conductivity, sodium halide electrolytes typically require amorphization—that is, disrupting the long-range ordered structure of crystalline materials to form an amorphous phase with numerous defects and free volumes. In the amorphous structure, the migration channels of sodium ions are no longer confined to regular lattice sites, but instead form an isotropic continuous diffusion network; simultaneously, the disordered arrangement of the polyhedral framework activates the "paddle wheel effect," where the rotation of anion polyhedra synergistically promotes cation transitions, thereby significantly increasing ionic conductivity. Taking the representative NaTaCl6 system as an example, traditional mechanical ball milling requires high-energy ball milling for more than 40 hours to induce polyhedral orientation disorder, activate the paddle wheel mechanism, and obtain a high ionic conductivity >3 mS / cm. Similarly, Na… 2.5 Cr 0.5 Zr 0.5Cl6 requires 20 hours of ball milling to achieve a conductivity of approximately 0.1 mS / cm. This long synthesis time severely restricts the production efficiency and large-scale preparation capability of halide electrolytes, significantly increasing manufacturing costs.

[0005] However, current research still has the following shortcomings: ① The volatile gases such as CO2 generated during the high-energy ball milling process require timely depressurization, which poses certain risks and is not conducive to industrial-scale preparation; ② The price of Ta raw materials is relatively high, and it is necessary to explore the feasibility of partially or completely replacing Ta with cheaper elements (such as Nb, Hf, Zr); ③ Existing sodium-containing dopants (such as Na2B4O7) inevitably introduce additional Na while introducing oxygen-containing anionic groups. + This interferes with the precise control of Na content in the formulation and the optimization of ionic conductivity; ④ The structure-property relationship between the optimal doping amount, ball milling parameters, degree of amorphization, and ionic conductivity has not yet been systematically established.

[0006] Therefore, developing an efficient amorphization strategy based on oxygen-containing anion dopants applicable to a variety of central metal elements is of great significance for promoting the practical application of sodium halide solid electrolytes.

[0007] Therefore, existing technologies need to be improved. Summary of the Invention

[0008] In view of the shortcomings of the prior art, the purpose of this invention is to provide a rapidly amorphous halide oxide solid electrolyte material, its preparation method, and its application. This aims to solve the problems of long ball milling time, high energy consumption, and low production efficiency required for amorphization in the preparation of existing sodium-based halide solid electrolytes, as well as the introduction of additional Na+ by existing sodium-containing dopants. + This leads to technical problems such as limited optimization of ionic conductivity and gas generation during the preparation process.

[0009] The technical solution of the present invention is as follows: In a first aspect, the present invention provides a method for preparing a rapid amorphous halide oxide solid electrolyte material, comprising the following steps: Take an alkaline sodium source, tantalum compounds, transition metal chlorides, and B2O3; The alkaline sodium source, tantalum-containing compound, transition metal chloride, and B2O3 are ground and initially mixed to obtain a pre-mixed material; The initial mixed material is pretreated to obtain a pretreated precursor. The pretreated precursor was ball-milled to obtain the rapidly amorphous halide oxide solid electrolyte material. The transition metal is not tantalum.

[0010] Optionally, the alkaline sodium source is at least one selected from Na₂O, Na₂O₂, and NaOH. The purity is ≥99.99%, used as the Na₂O source. + Carrier source. Before use, it needs to be dried in a vacuum drying oven at 120°C for 12 hours to remove any possible adsorbed water.

[0011] Optionally, the tantalum-containing compound is TaCl5, TaCl4, TaCl3, TaCl2, TaO2, or Ta2O5.

[0012] Optionally, the transition metal chloride is at least one of NbCl5, HfCl4, and ZrCl4. The purity is ≥99%. These chlorides are all strong Lewis acids and can undergo ligand exchange reactions with the O atom in B2O3.

[0013] Optionally, the molar ratio of alkaline sodium source, tantalum-containing compound, transition metal chloride, and B2O3 is 1:1-x:x:y, where 0 <x<1,0<y≤0.5。

[0014] Optionally, B2O3 with a purity ≥99.9% can be used as a sodium-free amorphization promoter. During storage, B2O3 may absorb moisture from the air to form boric acid; therefore, it needs to be dried at 300°C for 4 hours under vacuum before use. The particle size of B2O3 is preferably ≤100 mesh (after prior ball milling) to ensure rapid refining and uniform dispersion in the initial stages of ball milling.

[0015] Optionally, the pretreatment is to keep the temperature at 100-400℃ for 0.5-4 hours under an inert atmosphere.

[0016] Preferably, the pretreatment involves holding the product at 250-350°C for 1-2 hours under an inert atmosphere. After the holding period, the inert atmosphere is maintained, and the product is cooled to room temperature with the furnace. The pretreated precursor is then collected in a glove box.

[0017] Optionally, the ball milling is performed at a speed of 550-650 rpm for 10-30 minutes. A preferred speed is 600 rpm. Excessive speed (>700 rpm) may cause overheating and increased wear of the milling jar; excessive speed (<400 rpm) will significantly reduce amorphization efficiency.

[0018] Optionally, the ball milling is a circulating ball milling process, wherein each ball milling session lasts 5-10 minutes, followed by a 5-10 minute pause.

[0019] It should be noted that the grinding jar is made of zirconium oxide (ZrO2). Zirconia has high hardness, high density, and excellent wear resistance, and can effectively transfer mechanical energy. The grinding balls are also made of zirconium oxide, with a diameter range of 2-10 mm. A mixture of diameters is recommended to improve grinding efficiency.

[0020] The ball-to-material mass ratio (ratio of the total mass of grinding balls to the total mass of powder raw materials) is (20-80):1, preferably (40-60):1, more preferably 50:1. An excessively small ball-to-material ratio (<15:1) results in insufficient impact energy and a slow amorphization process; an excessively large ball-to-material ratio (>100:1) causes the volume occupied by balls in the ball milling jar to be too large, which affects the effective contact between balls and powder and the movement trajectory of the balls.

[0021] Recommended loading scheme (45 mL ball milling jar, total feeding amount 1.5 g): the total mass of zirconia balls is 75 g (corresponding to a ball-to-material ratio of 50:1), among which 5 mm balls are about 45 g, and 10 mm balls are about 30 g. After loading, the volume of grinding balls accounts for about 40%-50% of the internal volume of the jar.

[0022] In a second aspect, the present invention provides a rapidly amorphized oxyhalide solid electrolyte material prepared by the aforementioned preparation method, Alternatively, the general formula of the rapidly amorphized oxyhalide solid electrolyte material is: Na(Ta 1-x M x )OCl4-yB2O3 (abbreviated as Na-TM-BOCl), Wherein: M is a transition metal, and the transition metal is not tantalum; it is selected from at least one of Nb, Hf, and Zr, preferably Nb; x is the doping amount of the transition metal M, 0 < x < 1; y is the effective substitution amount of B2O3, satisfying 0 < y ≤ 0.5, preferably 0.15 ≤ y ≤ 0.35, more preferably 0.18 ≤ y ≤ 0.25.

[0023] An excessively small y value (<0.10) leads to insufficient amorphization driving force, requiring a prolonged ball milling time; an excessively large y value (>0.40) may introduce excessive B2O3, and unreacted B2O3 residual phases hinder ion conduction.

[0024] In a third aspect, the present invention provides the application of the aforementioned rapidly amorphized oxyhalide solid electrolyte material in solid-state batteries.

[0025] In a fourth aspect, the present invention provides a solid-state battery comprising the aforementioned rapidly amorphized oxyhalide solid electrolyte material.

[0026] Beneficial Effects: This invention provides a rapidly amorphous halide oxide solid electrolyte material, its preparation method, and its applications. The invention involves premixing an alkaline sodium source, tantalum-containing compounds, transition metal chlorides, and B₂O₃, followed by high-temperature pretreatment and ball milling. The high-temperature pretreatment is responsible for chemical activation and gas removal, while ball milling ensures complete amorphization. Pre-treatment gas removal and high-temperature pretreatment to construct an amorphous prototype lower the energy barrier for subsequent amorphization. The high reactivity of the alkaline sodium source ensures more complete O / Cl exchange during the pretreatment stage, and gas removal during the pretreatment stage provides more favorable thermodynamic conditions for the alkaline sodium source reaction. The alkaline sodium source ensures Na₂O₃ formation within a very short ball milling time. + The invention also creatively incorporates B2O3, which has high ionic conductivity (3.5 mS / cm) and contains no additional Na. + This reduces the formation of NaCl impurity phases and maintains a more continuous amorphous ion conduction network.

[0027] This invention also constructs a multi-center metal-B2O3 doped system including tantalum and transition metal elements, which on the one hand activates the paddlewheel effect driven by polyanion rotation, and on the other hand weakens the Na... + Electrostatic interactions with the anionic framework reduce Na + The activation energy for migration. Multiple mechanisms work together to achieve higher levels of ionic conductivity. Attached Figure Description

[0028] Figure 1 This is a process flow diagram for preparing rapidly amorphous halide oxide solid electrolyte materials according to an embodiment of the present invention.

[0029] Figure 2 This is a scanning electron microscope image of Example 1.

[0030] Figure 3 This is a scanning electron microscope image of Comparative Example 2.

[0031] Figure 4 The following are comparative powder diffraction patterns for each embodiment and comparative example. Detailed Implementation

[0032] This invention provides a rapidly amorphous halide oxide solid electrolyte material, its preparation method, and its applications. To make the objectives, technical solutions, and effects of this invention clearer and more explicit, the invention is further described in detail below. It should be understood that the specific embodiments described herein are merely illustrative of the invention and are not intended to limit the invention.

[0033] Currently, the main methods for preparing sodium ion halide solid electrolytes include the following categories: (1) Traditional long-term high-energy ball milling method Using NaCl and transition metal chlorides (such as TaCl5, HfCl4, ZrCl4, etc.) as raw materials, high-energy ball milling is carried out for a long time (20-40 hours or more) under an inert atmosphere. For example, NaTaCl6 requires 40 hours of ball milling to reach >3mS / cm.

[0034] Disadvantages: ① The ball milling time is extremely long (20-40 hours), resulting in high energy consumption and extremely low production efficiency; ② Prolonged ball milling leads to severe wear on the grinding balls and jars, introducing impurities that contaminate the product; ③ Excessive ball milling may cause NaCl raw materials to re-precipitate, reducing conductivity; ④ Batch consistency is difficult to guarantee.

[0035] (2) High-temperature melting-quenching method The raw material is heated above its melting point and then rapidly quenched to maintain its amorphous state. For example, the Na2O2-TaCl5 system can achieve a high ionic conductivity of >2 mS / cm by sintering followed by quenching.

[0036] Disadvantages: ① High-temperature processing (>400℃) consumes extremely high energy and volatile components are easily lost; ② The quenching process is difficult to control precisely; ③ High equipment requirements make it inconvenient for large-scale production.

[0037] (3) Liquid phase synthesis method The raw materials are dissolved in an organic solvent, mixed evenly, and then dried and heat-treated.

[0038] Disadvantages: ① Halides are sensitive to polar solvents, and liquid-phase processing may lead to hydrolysis or solvation side reactions; ② Solvent residues are difficult to remove completely; ③ Increased cost and environmental burden.

[0039] Oxygen anion doping accelerated amorphization technology The amorphization process can be accelerated by introducing oxygen-containing anions (such as Na₂CO₃ and Na₂B₄O₇) into sodium-based halide electrolytes. For example, the TaCl₅-Na₂CO₃ system can amorphize within 10-20 minutes, with an ionic conductivity of 1.2 mS / cm; Na 1+x Ta(B4O7) x Cl 6-x The system can be amorphized within 10 minutes, with an electrical conductivity of 1.1 mS / cm.

[0040] However, the above technologies still have shortcomings: ① Sodium-containing dopants introduce additional Na + When Na₂B₄O₇ (molecular formula Na₂O·2B₂O₃) dopants introduce oxygen-containing anionic groups, they inevitably introduce additional Na₂O₃. + This limits the precise control of sodium content in the formulation—the amount of boron doping is "tied" to the sodium content and cannot be optimized independently. Excessive Na... +It readily precipitates as NaCl crystals with low electrical conductivity in amorphous matrices, hindering ion conduction. Although it can rapidly amorphize within 10 minutes, its electrical conductivity is only 1.1 mS / cm.

[0041] ②When introducing oxygen-containing anionic groups, Na2CO3 and other similar products inevitably introduce additional carbon. The volatile gases such as CO2 generated during the high-energy ball milling process require timely depressurization by opening the tank midway. This process poses certain risks and is not conducive to industrial preparation.

[0042] ③ Limited system coverage: Existing studies mainly focus on Ta-based systems. For systems with cheaper elements such as Nb, Hf, and Zr as the core metal, there is a lack of systematic verification and comparison of the effect of oxygen-containing anion doping on accelerating amorphization.

[0043] In summary, existing technologies cannot simultaneously meet the following requirements: ① Even with rapid amorphization, the ionic conductivity is only 1.1 mS / cm, which is relatively low; ② Applicability to various central metal elements (Ta, Nb, Hf, Zr, etc.); ③ Avoiding the adverse effects of introducing additional cations by dopants on ionic conductivity; ④ Establishing a clear process-structure-performance structure-property relationship; ⑤ Gas generation during ball milling, which cannot meet the requirements for industrial production. Therefore, there is an urgent need to develop an efficient and rapid amorphization strategy using oxygen-containing anion dopants without additional cations.

[0044] Based on this, this embodiment provides a method for preparing a rapid amorphous halide oxide solid electrolyte material, such as... Figure 1 As shown, it includes the following steps: S1, take an alkaline sodium source, containing tantalum compounds, transition metal chlorides and B2O3; S2. Grind and initially mix the alkaline sodium source, tantalum-containing compound, transition metal chloride, and B2O3 to obtain a preliminary mixed material; S3. Pre-treat the initial mixed material to obtain a pre-treated precursor; S4. The pretreated precursor is ball-milled to obtain the rapidly amorphized halide oxide solid electrolyte material. The transition metal is not tantalum.

[0045] It should be noted that this embodiment uses sodium-free B2O3 as an amorphization promoter. Utilizing its strong glass network forming ability and the characteristic of not introducing additional cations, byproduct gases are released through high-temperature pretreatment, followed by ball milling to achieve rapid amorphization and high ionic conductivity of the sodium-ion halide electrolyte. Specifically: The high reactivity of the alkaline sodium source allows for more complete O / Cl exchange during the pretreatment stage, providing a more ideal precursor structure for subsequent ball milling. Gas removal during the pretreatment stage provides more favorable thermodynamic conditions for the alkaline sodium source to participate in the reaction (gas escape drives the reaction in the forward direction). The alkaline sodium source chemically drives the reaction of Na... + Embedded amorphous network ensures Na within an extremely short ball milling time. + The pretreatment stage allows for more complete acid-base neutralization reactions between the alkaline sodium source and the tantalum-containing compound under heating conditions, reducing reliance on the mechanical energy of the ball mill. The synergistic effect of these two processes significantly reduces the ball milling time from the traditional 40 hours to minutes.

[0046] B₂O₃ is one of the most fundamental network-forming structures in classical glass science. Its structural unit is a planar [BO₃] triangle (BO bond length approximately 1.37 Å, OBO angle 120°). Molten B₂O₃ readily forms a disordered network of [BO₃] units connected by shared O atoms at their vertices. During high-energy ball milling, B₂O₃ particles undergo an O / Cl ligand exchange reaction with transition metal chlorides: O atoms in B₂O₃ partially replace Cl atoms in the transition metal-centered coordination layer, forming a highly distorted mixed [TMCl] network. 6-x O x [BO3] Polyhedron. Due to the significant size difference between O atoms (covalent radius 0.66 Å) and Cl atoms (covalent radius 0.99 Å), and the completely different coordination geometry between the [BO3] triangle and the [TaO6] octahedron, strong local structural stress and orientation disorder are generated. This structural perturbation at the chemical bond level propagates rapidly with the aid of mechanical ball milling, causing the long-range ordered structure to collapse in a very short time, forming an amorphous state.

[0047] Using B2O3 does not introduce additional cations, resulting in a lower proportion of NaCl residual phase in the amorphous electrolyte and maintaining a continuous ion conduction network.

[0048] The orientation disorder of the mixed TaM-Cl-O coordination polyhedra introduced by B2O3 activates the paddlewheel effect driven by the rotation of polyanions on the one hand, and weakens the Na+-coordination on the other. + Electrostatic interactions with the anionic framework reduce Na + The activation energy for migration. Multiple mechanisms work together to achieve higher levels of ionic conductivity.

[0049] The reaction mechanism in this embodiment is as follows: B2O3 is the most classic glass network-forming material. Its structural unit is a planar [BO3] triangle. Key physicochemical properties include: melting point of approximately 450℃ and softening point of approximately 300℃; easy breakage and recombination of BO bonds under mechanical force; high charge density and strong coordination ability of the [BO3] unit; no additional cations such as Na, making it a pure covalent network-forming material; low price, with industrial-grade B2O3 being the most cost-effective.

[0050] During high-energy ball milling: Step 1: Particle Refinement and Mixing. The particles of each component are broken down to the nanoscale, generating numerous fresh surfaces and high-density lattice defects. Because B2O3 has a relatively low softening temperature (approximately 300℃), it may undergo localized softening in the high-temperature micro-regions generated by ball milling, effectively coating the surface of tantalum-containing particles (such as TaCl5) and increasing the O / Cl exchange reaction interface.

[0051] Step 2: Interfacial reaction and O / Cl exchange. In the high-temperature, high-pressure micro-zone of ball milling, the [BO3] units in B2O3 undergo an O / Cl ligand exchange reaction with tantalum compounds (such as TaCl5): B2O3 + 2n[TaCl6] - →2[B(Cl,O)3] (3-x) +2n[TaCl 6-x O x ] (n-x) O atoms partially replace Cl atoms in the Ta coordination layer, forming a mixed-coordinated [TaCl] 6-x O x Polyhedron (x=1-3). The Ta-O bond length (approximately 1.88 Å) is significantly shorter than the Ta-Cl bond length (approximately 2.36 Å), and the octahedron is significantly distorted.

[0052] Step 3: Local distortion and long-range order disruption. The size difference between O and Cl and the coordination geometry difference between [BO3] and [TaO6] lead to polyhedral orientation disorder, which is transmitted through BO-Ta oxygen bridges to form associated disordered structures.

[0053] Step 4: Construction and stabilization of the amorphous network. [TaCl] 6-x O x The polyhedra are connected by BO-Ta bridging oxygen bonds to form disordered clusters or network segments. The [BO3] units provided by B2O3 can self-polymerize to form boron-oxygen rings and segments, forming an extended disordered mixed network with the Ta polyhedra.

[0054] The system in this embodiment is a B2O3 doped system, and the Na in the formula... + All from alkaline sodium sources (such as NaCl), total Na + The amount can be precisely controlled near the stoichiometric ratio. The O atoms introduced by B₂O₃ react with Cl…- Competitive coordination occurs, but the total amount of cations remains unchanged. Therefore, the proportion of residual NaCl is lower after amorphization, the NaCl peak intensity is significantly weakened in XRD, and the ion conduction network in the amorphous matrix is ​​more continuous. In contrast, the Na₂B₄O₇-doped system contains more Na₂B₄O₇. + Add Na from the NaCl raw material + Total Na in the system + The amount is too high. Some Na... + It is difficult for amorphous networks to completely absorb it, and it precipitates as NaCl microcrystals during ball milling. XRD analysis shows visible NaCl diffraction peaks in the Na₂B₄O₇ doped product. NaCl is a poorly distributed Na₂Cl crystal. + Conductor (room temperature conductivity approximately 10) -18 The microcrystals of B₂O₃, dispersed within the amorphous matrix, impede ion conduction. Experiments show that, under the same ball milling conditions, the ionic conductivity of the B₂O₃-doped system is 3.5 mS / cm, while that of the Na₂B₄O₇-doped system is 1.1 mS / cm, demonstrating a significant improvement in conductivity. The activation energy of the doped system is 0.27 eV, lower than the 0.29 eV of the Na₂B₄O₇-doped system. This confirms the superior ionic conductivity resulting from the "no additional cations" characteristic of B₂O₃.

[0055] In some embodiments, the alkaline sodium source is at least one selected from Na₂O, Na₂O₂, and NaOH. The purity is ≥99.99%, and it is used as the Na₂O source. + Carrier source. Before use, it needs to be dried in a vacuum drying oven at 120°C for 12 hours to remove any possible adsorbed water.

[0056] In some embodiments, the tantalum-containing compound is TaCl5, TaCl4, TaCl3, TaCl2, TaO2, or Ta2O5.

[0057] In some embodiments, the transition metal chloride is at least one of NbCl5, HfCl4, and ZrCl4. The purity is ≥99%. These chlorides are all strong Lewis acids and can undergo ligand exchange reactions with the O atoms in B2O3.

[0058] In some embodiments, the molar ratio of alkaline sodium source, tantalum-containing compound, transition metal chloride, and B2O3 is 1:1-x:x:y, where 0 <x<1,0<y≤0.5。

[0059] In some embodiments, B2O3 has a purity of ≥99.9% and is used as a sodium-free amorphization promoter. During storage, B2O3 may absorb moisture from the air to form boric acid; therefore, it needs to be dried at 300°C for 4 hours under vacuum before use. The particle size of B2O3 is preferably ≤100 mesh (after prior ball milling) to ensure rapid refining and uniform dispersion in the initial stages of ball milling.

[0060] In some embodiments, the pretreatment is performed by holding the temperature at 100-400°C for 0.5-4 hours under an inert atmosphere.

[0061] In some embodiments, the pretreatment involves holding the product at 250-350°C for 1-2 hours under an inert atmosphere. After the holding period, the inert atmosphere is maintained, and the product is cooled to room temperature with the furnace. The pretreated precursor is then collected in a glove box.

[0062] In some embodiments, the ball mill is operated at a speed of 550-650 rpm for 10-30 minutes for effective milling. A preferred speed is 600 rpm. Excessive speed (>700 rpm) may lead to overheating of the milling jar and accelerated wear; excessive speed (<400 rpm) will significantly reduce amorphization efficiency.

[0063] In some embodiments, the ball milling is a circulating ball milling process, wherein each ball milling session lasts 5-10 minutes, followed by a 5-10 minute pause.

[0064] It should be noted that the grinding jar is made of zirconium oxide (ZrO2). Zirconia has high hardness, high density, and excellent wear resistance, and can effectively transfer mechanical energy. The grinding balls are also made of zirconium oxide, with a diameter range of 2-10 mm. A mixture of diameters is recommended to improve grinding efficiency.

[0065] The ball-to-powder mass ratio (the ratio of the total mass of grinding balls to the total mass of powder raw materials) is (20-80):1, preferably (40-60):1, and more preferably 50:1. If the ball-to-powder ratio is too small (<15:1), the impact energy is insufficient, and the amorphization process is slow; if the ball-to-powder ratio is too large (>100:1), the volume occupied by the balls in the grinding jar is too large, which affects the effective contact between the balls and the powder and the trajectory of the balls.

[0066] Recommended filling method (45mL ball mill jar, total feed amount 1.5g): 75g total mass of zirconia balls (corresponding to a ball-to-material ratio of 50:1), of which approximately 45g are 5mm balls and approximately 30g are 10mm balls. After filling, the grinding balls will occupy approximately 40%-50% of the jar's internal volume.

[0067] This embodiment also provides a rapidly amorphous halide oxide solid electrolyte material, prepared by the aforementioned preparation method. Alternatively, the general formula of the rapidly amorphous halide oxide solid electrolyte material is: Na(Ta 1-x M x )OCl4-yB2O3 (abbreviated as Na-TM-BOCl), wherein: M is a transition metal, selected from at least one of Nb, Hf and Zr, preferably Nb; x is the doping amount of the transition metal M, 0 < x < 1; y is the effective substitution amount of B2O3, satisfying 0 < y ≤ 0.5, preferably 0.15 ≤ y ≤ 0.35, more preferably 0.18 ≤ y ≤ 0.25.

[0068] If the y value is too small (<0.10), the driving force for amorphization is insufficient, and the ball milling time needs to be extended; if the y value is too large (>0.40), excessive B2O3 may be introduced, and unreacted residual B2O3 phase hinders ion conduction.

[0069] This embodiment further provides the application of the rapidly amorphizable oxyhalide solid electrolyte material in solid-state batteries.

[0070] This embodiment further provides a solid-state battery comprising the rapidly amorphizable oxyhalide solid electrolyte material.

[0071] The present invention will be further described below through specific examples.

[0072] Example 1 A method for preparing a rapidly amorphizable oxyhalide solid electrolyte material (B2O3 doped, x=1, y=0.20, 10 min ball milling) NaOH was vacuum-dried at 120°C for 12 h, B2O3 was vacuum-dried at 300°C for 4 h, and TaCl5 was used directly.

[0073] In an Ar atmosphere glove box (H2O content ≤0.1 ppm, O2 content ≤0.1 ppm), the mass of each raw material was calculated according to the target composition NaTaOCl4-yB2O3. The molar ratio of NaOH:TaCl5:B2O3 = 1.0:1.0:0.20, which was weighed with an electronic balance with an accuracy of 0.1 mg.

[0074] The three weighed powders were placed in an agate mortar for grinding and preliminary mixing, manually ground for 8 min until the powder color and texture were uniform, to obtain a preliminarily mixed material.

[0075] The preliminarily mixed material was transferred to an alumina crucible with a gas outlet for pretreatment. It was placed in a tube furnace, and high-purity Ar gas (80 mL / min) was introduced. The temperature was raised to 300°C at a rate of 5°C / min and held for 1 h. After the heat preservation was completed, Ar gas was continuously introduced, and the material was cooled to room temperature along with the furnace, and the pretreated precursor was collected.

[0076] Transfer the pretreated precursor to a 45 mL zirconia ball mill jar. Add zirconia grinding balls: 45 g of 5 mm balls and 30 g of 10 mm balls, for a total ball weight of 75 g (ball-to-material ratio 50:1). Seal the ball mill jar.

[0077] Install the grinding jar onto the planetary ball mill and set the speed to 600 rpm. Use a cycle mode: 5 minutes of grinding followed by a 5-minute pause constitutes one cycle, and run for a total of 2 cycles (total effective grinding time 10 minutes).

[0078] After ball milling, allow the milling jar to cool to room temperature. Open the jar in a glove box, collect the powder using a stainless steel scraper, and seal it in a glass sample vial. The product is labeled "NTBOC-B2O3-0.20-10min". The scanning electron microscope image of Example 1 is shown below. Figure 2 As shown.

[0079] Example 2 A rapid method for preparing amorphous halide oxide solid electrolyte materials (B2O3 doping, x=1, y=0.05, ball milling for 10 min). NaOH was dried under vacuum at 120℃ for 12 hours, B2O3 was dried under vacuum at 300℃ for 4 hours, and TaCl5 was used directly.

[0080] In an Ar atmosphere glove box (H2O content ≤ 0.1 ppm, O2 content ≤ 0.1 ppm), calculate the mass of each raw material according to the target composition NaTaOCl4-0.05B2O3, and weigh them using an electronic balance with an accuracy of 0.1 mg. The molar ratio NaOH:TaCl5:B2O3 = 1.0:1.0:0.05, weighed using an electronic balance with an accuracy of 0.1 mg.

[0081] The three weighed powders were placed in an agate mortar and ground and mixed initially. The mixture was ground by hand for 8 minutes until the powder was uniform in color and texture, thus obtaining the initial mixed material.

[0082] The initial mixture was transferred to an alumina crucible with a gas outlet for pretreatment. It was placed in a tube furnace, and high-purity Ar gas (80 mL / min) was introduced. The temperature was increased to 300°C at 5°C / min and held for 1 hour. After the holding period, Ar gas was continued to flow through the furnace, and the furnace was cooled to room temperature. The pretreated precursors were then collected.

[0083] Transfer the pretreated precursor to a 45 mL zirconia ball mill jar. Add zirconia grinding balls: 45 g of 5 mm balls and 30 g of 10 mm balls, for a total ball weight of 75 g (ball-to-material ratio 50:1). Seal the ball mill jar.

[0084] Install the grinding jar onto the planetary ball mill and set the speed to 600 rpm. Use a cycle mode: 5 minutes of grinding followed by a 5-minute pause constitutes one cycle, and run for a total of 2 cycles (total effective grinding time 10 minutes).

[0085] After ball milling, allow the milling jar to cool to room temperature. Open the milling jar in a glove box, collect the powder with a stainless steel scraper, and seal it in a glass sample vial. The product is labeled "NTBOC-B2O3-0.05-10min".

[0086] Example 3 A rapid method for preparing amorphous halide oxide solid electrolyte materials (B2O3 doping, x=0.5, Nb partially replacing Ta, Ta:Nb=1:1, y=0.20, ball milling for 30 min) NaOH was dried under vacuum at 120℃ for 12 hours, B2O3 was dried under vacuum at 300℃ for 4 hours, and TaCl5 was used directly. NbCl5 was used directly in a glove box.

[0087] In an Ar atmosphere glove box (H2O content ≤ 0.1 ppm, O2 content ≤ 0.1 ppm), according to the target composition Na (Ta 0.5 Nb 0.5 Calculate the mass of each raw material using OCl4-0.50B2O3. The molar ratio is NaOH:TaCl5:NbCl5:B2O3 = 1.0:0.50:0.50:0.20. Weigh the raw materials using an electronic balance with an accuracy of 0.1 mg.

[0088] The three weighed powders are placed in an agate mortar and ground and mixed initially. The mixture is ground by hand for 10 minutes until the powder has a uniform color and texture, thus obtaining the initial mixed material.

[0089] The initial mixture was transferred to an alumina crucible with a gas outlet for pretreatment. It was placed in a tube furnace, and high-purity Ar gas (80 mL / min) was introduced. The temperature was increased to 300°C at 5°C / min and held for 1 hour. After the holding period, Ar gas was continued to flow through the furnace, and the furnace was cooled to room temperature. The pretreated precursors were then collected.

[0090] Transfer the pretreated precursor to a 45 mL zirconia ball mill jar. Add zirconia grinding balls: 45 g of 5 mm balls and 30 g of 10 mm balls, for a total ball weight of 75 g (ball-to-material ratio 50:1). Seal the ball mill jar.

[0091] Install the grinding jar onto the planetary ball mill and set the speed to 600 rpm. Use a cycle mode: 5 minutes of grinding followed by a 5-minute pause constitutes one cycle, and run for a total of 2 cycles (total effective grinding time 10 minutes).

[0092] After ball milling, allow the milling jar to cool to room temperature. Open the jar in a glove box, collect the powder with a stainless steel scraper, and seal it in a glass sample vial. The product is labeled "NTNBOC-B2O3-0.20-10min".

[0093] Comparative Example 1 A method for preparing a halide oxide solid electrolyte material (Na2B4O7 doping, equivalent B content, ball milling for 10 min). NaOH was dried under vacuum at 120℃ for 12 hours, and Na₂B₄O₇ was dried under vacuum at 300℃ for 4 hours (to remove water of crystallization and adsorbed water). TaCl₅ was used directly.

[0094] In an Ar atmosphere glove box (H2O content ≤ 0.1 ppm, O2 content ≤ 0.1 ppm), calculate the mass of each raw material according to the target composition NaTaOCl4-yNa2B4O7. The molar ratio of NaOH:TaCl5:Na2B4O7 = 1.0:1.0:0.20, and weigh using an electronic balance with an accuracy of 0.1 mg.

[0095] The three weighed powders were placed in an agate mortar and ground and mixed initially. The mixture was ground by hand for 8 minutes until the powder was uniform in color and texture, thus obtaining the initial mixed material.

[0096] The initial mixture was transferred to an alumina crucible with a gas outlet for pretreatment. It was placed in a tube furnace, and high-purity Ar gas (80 mL / min) was introduced. The temperature was increased to 300°C at 5°C / min and held for 1 hour. After the holding period, Ar gas was continued to flow through the furnace, and the furnace was cooled to room temperature. The pretreated precursors were then collected.

[0097] Transfer the pretreated precursor to a 45 mL zirconia ball mill jar. Add zirconia grinding balls: 45 g of 5 mm balls and 30 g of 10 mm balls, for a total ball weight of 75 g (ball-to-material ratio 50:1). Seal the ball mill jar.

[0098] Install the grinding jar onto the planetary ball mill and set the speed to 600 rpm. Use a cycle mode: 5 minutes of grinding followed by a 5-minute pause constitutes one cycle, and run for a total of 2 cycles (total effective grinding time 10 minutes).

[0099] After ball milling, allow the milling jar to cool to room temperature. Open the milling jar in a glove box, collect the powder with a stainless steel scraper, and seal it in a glass sample vial. The product is labeled "NTBOC-Na2B4O7-0.20-10min".

[0100] Comparative Example 2 A method for preparing a solid electrolyte material (boron-free source, ball milling for 10 min). NaOH was dried under vacuum at 120℃ for 12 hours, and TaCl5 was used directly.

[0101] In an Ar atmosphere glove box (H2O content ≤ 0.1 ppm, O2 content ≤ 0.1 ppm), calculate the mass of each raw material according to the target composition NaTaOCl4. The molar ratio of NaOH:TaCl5 = 1.0:1.0, and weigh using an electronic balance with an accuracy of 0.1 mg.

[0102] The three weighed powders were placed in an agate mortar and ground and mixed initially. The mixture was ground by hand for 8 minutes until the powder was uniform in color and texture, thus obtaining the initial mixed material.

[0103] The initial mixture was transferred to an alumina crucible with a gas outlet for pretreatment. It was placed in a tube furnace, and high-purity Ar gas (80 mL / min) was introduced. The temperature was increased to 300°C at 5°C / min and held for 1 hour. After the holding period, Ar gas was continued to flow through the furnace, and the furnace was cooled to room temperature. The pretreated precursors were then collected.

[0104] Transfer the pretreated precursor to a 45 mL zirconia ball mill jar. Add zirconia grinding balls: 45 g of 5 mm balls and 30 g of 10 mm balls, for a total ball weight of 75 g (ball-to-material ratio 50:1). Seal the ball mill jar.

[0105] Install the grinding jar onto the planetary ball mill and set the speed to 600 rpm. Use a cycle mode: 5 minutes of grinding followed by a 5-minute pause constitutes one cycle, and run for a total of 2 cycles (total effective grinding time 10 minutes).

[0106] After ball milling, allow the milling jar to cool to room temperature. Open the jar in a glove box, collect the powder using a stainless steel scraper, and seal it in a glass sample vial. Label the product "NTBOC-10min". The scanning electron microscope image of Comparative Example 2 is shown below. Figure 3 As shown.

[0107] Comparative Example 3 A rapid method for preparing amorphous halide oxide solid electrolyte materials (B2O3 overdoping, x=1, y=0.60, ball milling for 10 min). NaOH was dried under vacuum at 120℃ for 12 hours, B2O3 was dried under vacuum at 300℃ for 4 hours, and TaCl5 was used directly.

[0108] In an Ar atmosphere glove box (H2O content ≤ 0.1 ppm, O2 content ≤ 0.1 ppm), calculate the mass of each raw material according to the target composition NaTaOCl4-yB2O3. The molar ratio of NaOH:TaCl5:B2O3 = 1.0:1.0:0.60, and weigh using an electronic balance with an accuracy of 0.1 mg.

[0109] The three weighed powders were placed in an agate mortar and ground and mixed initially. The mixture was ground by hand for 8 minutes until the powder was uniform in color and texture, thus obtaining the initial mixed material.

[0110] The initial mixture was transferred to an alumina crucible with a gas outlet for pretreatment. It was placed in a tube furnace, and high-purity Ar gas (80 mL / min) was introduced. The temperature was increased to 300°C at 5°C / min and held for 1 hour. After the holding period, Ar gas was continued to flow through the furnace, and the furnace was cooled to room temperature. The pretreated precursors were then collected.

[0111] Transfer the pretreated precursor to a 45 mL zirconia ball mill jar. Add zirconia grinding balls: 45 g of 5 mm balls and 30 g of 10 mm balls, for a total ball weight of 75 g (ball-to-material ratio 50:1). Seal the ball mill jar.

[0112] Install the grinding jar onto the planetary ball mill and set the speed to 600 rpm. Use a cycle mode: 5 minutes of grinding followed by a 5-minute pause constitutes one cycle, and run for a total of 2 cycles (total effective grinding time 10 minutes).

[0113] After ball milling, allow the milling jar to cool to room temperature. Open the milling jar in a glove box, collect the powder with a stainless steel scraper, and seal it in a glass sample vial. The product is labeled "NTBOC-B2O3-0.60-10min".

[0114] Comparative Example 4 A method for preparing fast solid-state electrolyte materials (no high-temperature pretreatment, 10-min ball milling) NaOH was dried under vacuum at 120℃ for 12 hours, B2O3 was dried under vacuum at 300℃ for 4 hours, and TaCl5 was used directly.

[0115] In an Ar atmosphere glove box (H2O content ≤ 0.1 ppm, O2 content ≤ 0.1 ppm), calculate the mass of each raw material according to the target composition NaTaOCl4-yB2O3. The molar ratio of NaOH:TaCl5:B2O3 = 1.0:1.0:0.20, and weigh using an electronic balance with an accuracy of 0.1 mg.

[0116] The three weighed powders were placed in an agate mortar and ground and mixed initially. The mixture was ground by hand for 8 minutes until the powder was uniform in color and texture, thus obtaining the initial mixed material.

[0117] Transfer the initial mixture to a 45mL zirconia ball mill jar. Add zirconia grinding balls: 45g of 5mm balls and 30g of 10mm balls, for a total ball weight of 75g (ball-to-material ratio 50:1). Seal the ball mill jar.

[0118] Install the grinding jar onto the planetary ball mill and set the speed to 600 rpm. Use a cycle mode: 5 minutes of grinding followed by a 5-minute pause constitutes one cycle, and run for a total of 2 cycles (total effective grinding time 10 minutes).

[0119] After ball milling, allow the milling jar to cool to room temperature. Open the jar in a glove box, collect the powder with a stainless steel scraper, and seal it in a glass sample vial. The product is labeled "NTBOC-B2O3-0.20-10min (no pretreatment)".

[0120] Table 1 shows a performance comparison table of each embodiment and comparative example.

[0121] Table 1. Performance Comparison of Various Embodiments and Comparative Examples

[0122] As can be seen from Table 1: (1) Optimization of B2O3 doping amount - Comparison of Examples 1 and 2 with Comparative Examples 2 and 3 As shown in Table 1, Example 1 (x=0.20), Example 2 (x=0.05), Comparative Example 2 (x=0, no boron source) and Comparative Example 3 (x=0.60, excessive doping) constitute a complete set of B2O3 doping gradient comparisons, which clearly reveal the influence of B2O3 doping amount on the material structure and performance.

[0123] Comparative Example 2 (NaTaOCl4, without B2O3 doping) exhibits an ionic conductivity of only 0.18 mS / cm and an activation energy as high as 0.45 eV. For example... Figure 4 As shown, the XRD pattern reveals obvious crystallization diffraction peaks, indicating that the pure NaTaOCl4 matrix is ​​far from amorphous under 10-minute ball milling conditions—the NaTaOCl4 generated by the reaction of NaOH and TaCl5 still exists in crystalline form, and the long-range ordered lattice structure restricts the Na… + The migration pathway. Meanwhile, the NaCl residual peak intensity of Comparative Example 2 is the highest. This is because, under the condition of no B2O3-assisted amorphization, some NaOH did not fully participate in the reaction, and the generated low-conductivity NaCl remained in the product as an independent crystalline phase.

[0124] In Example 2 (x=0.05), the introduction of a small amount of B₂O₃ resulted in a jump in ionic conductivity to 3.85 mS / cm, approximately 21 times higher than in Comparative Example 2. The activation energy decreased significantly from 0.45 eV to 0.26 eV. The residual NaCl peak intensity plummeted from 100% to 12%, indicating that B₂O₃ participates in the O / Cl exchange reaction, effectively embedding Na⁺ into the amorphous network by constructing BO-Ta bridging oxygen bonds, thus suppressing the precipitation of the NaCl crystalline phase at its source. However, the amount of B₂O₃ at x=0.05 is insufficient to construct a completely continuous amorphous network, as... Figure 4 As shown, a small amount of NaCl remains in the product, which limits further improvement in ionic conductivity.

[0125] In Example 1 (x=0.20), further increasing the B₂O₃ doping amount resulted in a maximum ionic conductivity of 4.32 mS / cm and a minimum activation energy of 0.24 eV. XRD patterns showed completely amorphous characteristics. Figure 4 As shown, the residual NaCl peak intensity further decreased to 8%, indicating that the amount of B2O3 had reached the optimal ratio for constructing a complete amorphous network. Figure 2 , Figure 3 As shown, compared to Comparative Example 2, at x=0.20, the [BO3] structural units and O atoms provided by B2O3 are sufficient to undergo sufficient O / Cl ligand exchange with TaCl5 to form a continuous BO-Ta amorphous network. + Uniformly distributed within this network, the ion transport pathways are continuous and efficient. Simultaneously, an appropriate amount of B₂O₃ effectively widens the free volume and ion transport bottleneck size in the amorphous network, allowing Na₂O₃ to... + Both the geometric constraints and energy barriers for migration are significantly reduced.

[0126] In contrast, the ionic conductivity of Comparative Example 3 (x=0.60, overdoped) decreased significantly to 1.85 mS / cm, while the activation energy rebounded to 0.34 eV. For example... Figure 4 As shown, although the XRD pattern still shows a predominantly amorphous state, the presence of characteristic diffraction signals from a small amount of B2O3 indicates that the excess B2O3 did not fully participate in the construction of the amorphous network, with some remaining as free boron oxide phase in the product. While this free B2O3 itself does not hinder ion transport, its volume dilutes the effective content of the NaTaOCl4 active matrix. Simultaneously, the excessive B2O3 leads to an excessively high density of [BO3] units in the amorphous network, potentially causing over-crosslinking of the BO-Ta network and thus limiting the Na... + Long-distance migration in the network.

[0127] Based on the four sets of data, the effect of B2O3 doping concentration on ionic conductivity exhibits a typical "first increase, then decrease" trend: as x increases from 0 to 0.20, the ionic conductivity continuously rises from 0.18 mS / cm to 4.32 mS / cm; after x exceeds 0.20, the ionic conductivity begins to decrease. The optimal B2O3 doping concentration is x = 0.20. At this ratio, the [BO3] units provided by B2O3 react fully with TaCl5 to construct a complete amorphous network, with extremely low residual NaCl phase.

[0128] (2) Effect of Nb partially replacing Ta – Comparison of Example 1 and Example 3 Example 3, based on Example 1, replaced Ta with 50% Nb. The ionic conductivity was 3.45 mS / cm, lower than the 4.32 mS / cm of the pure Ta system in Example 1. The activation energy increased from 0.24 eV to 0.28 eV. Figure 4As shown, XRD indicates that the product is still amorphous, and the residual NaCl peak intensity is 10%, slightly higher than 8% in Example 1.

[0129] The decrease in ionic conductivity is mainly caused by the following factors: Nb 5+ Although its ionic radius (0.64 Å) is similar to that of Ta 5+ The Nb-O bond energy (approximately 0.64 Å) is similar, but the bond energy of the Nb-O bond (approximately 680 kJ / mol) is slightly lower than that of the Ta-O bond (approximately 700 kJ / mol). This results in a slightly weaker local structural rigidity of the Nb-O polyhedron compared to the Ta-O polyhedron, which slightly affects the geometric stability of the Na+ transport channels in the amorphous network. Furthermore, the reactivity of NbCl5 is slightly lower than that of TaCl5. Under the same pretreatment and ball milling conditions, the O / Cl exchange reaction is slightly less complete, resulting in a slightly higher residual NaCl phase.

[0130] The performance of Example 3 remains at a high level—the ionic conductivity of 3.45 mS / cm is still superior to Comparative Example 1 (3.12 mS / cm) and Comparative Example 4 (without pretreatment, 2.85 mS / cm). The raw material cost of NbCl5 is approximately 1 / 5 to 1 / 10 of that of TaCl5. The 50% Nb substitution halves the amount of Ta in the raw material, reducing the cost of the electrolyte material by approximately 30%-40%. The ionic conductivity of 3.45 mS / cm meets the application requirements of most all-solid-state sodium batteries (typically ≥1 mS / cm is sufficient). This approach achieves a good balance between performance and cost, and has high practical value in cost-sensitive applications such as large-scale energy storage.

[0131] (3) Comparison of doping effects of B2O3 and Na2B4O7 - Comparison of Example 1 and Comparative Example 1 Comparative Example 1 used Na₂B₄O₇ as the boron source (equivalent boron, i.e., the same number of B atoms). Its ionic conductivity was 3.12 mS / cm, significantly lower than the 4.32 mS / cm of Example 1, a decrease of approximately 28%. The activation energy was 0.30 eV, higher than the 0.24 eV of Example 1. Figure 4 As shown, the residual peak intensity of NaCl in Comparative Example 1 (35%) is significantly higher than that in Example 1 (8%). The molecular formula of Na₂B₄O₇ is Na₂O·2B₂O₃, with each introduction of 4 B atoms (i.e., 1 [B₄O₇]) 2- (group), while introducing 2 Na groups. + Under the condition of equal boron equivalence (x=0.20), the Na2B4O7 scheme introduces an additional 0.10 mol of Na compared to the B2O3 scheme. + (Relative to a 1 mol NaTaOCl4 matrix). These additional Na + Given the limited absorbability of amorphous networks, some of the Cl... -It combines and precipitates from the amorphous matrix as NaCl microcrystals. NaCl is a poorly distributed Na... + Conductor (room temperature conductivity approximately 10) -18 (S / cm), whose microcrystals are dispersed in the amorphous matrix, blocking the continuous ion conduction path.

[0132] (4) The necessity of high temperature pretreatment - comparison between Example 1 and Comparative Example 4 Comparative Example 4 used the exact same formulation as Example 1 (NaTaOCl4-0.20B2O3), but without high-temperature pretreatment, and was directly subjected to high-energy ball milling for 10 minutes. Its ionic conductivity was only 2.85 mS / cm, far lower than the 4.32 mS / cm of Example 1. The activation energy was as high as 0.33 eV, significantly higher than the 0.24 eV of Example 1.

[0133] The residual NaCl peak intensity of Comparative Example 4 (28%) was much higher than that of Example 1 (8%). The HCl gas generated by the O / Cl exchange reaction was retained in the closed ball mill jar—adsorbed on the powder surface to form a gas film buffer layer, which reduced the mechanical energy transfer efficiency of the grinding balls. At the same time, the gas pressure inhibited the forward progress of the O / Cl exchange reaction.

[0134] In summary, this invention provides a rapidly amorphous halide oxide solid electrolyte material, its preparation method, and its applications. This invention involves premixing an alkaline sodium source, a tantalum-containing compound, a transition metal chloride, and B₂O₃, followed by high-temperature pretreatment and ball milling. The high-temperature pretreatment is responsible for chemical activation and gas removal, while ball milling ensures complete amorphization. Pre-treatment gas removal and high-temperature pretreatment to construct an amorphous prototype lower the energy barrier for subsequent amorphization. The high reactivity of the alkaline sodium source ensures more complete O / Cl exchange during the pretreatment stage, and the gas removal during the pretreatment stage provides more favorable thermodynamic conditions for the alkaline sodium source reaction. The alkaline sodium source ensures Na₂O₃ production within an extremely short ball milling time. + The invention also creatively incorporates B2O3, which has high ionic conductivity (3.5 mS / cm) and contains no additional Na. + This reduces the formation of NaCl impurity phases and maintains a more continuous amorphous ion conduction network.

[0135] This invention also constructs a multi-center metal-B2O3 doped system including tantalum and transition metal elements, which on the one hand activates the paddlewheel effect driven by polyanion rotation, and on the other hand weakens the Na... + Electrostatic interactions with the anionic framework reduce Na + The activation energy for migration. Multiple mechanisms work together to achieve higher levels of ionic conductivity.

[0136] It should be understood that the application of the present invention is not limited to the examples above. Those skilled in the art can make improvements or modifications based on the above description, and all such improvements and modifications should fall within the protection scope of the appended claims.

Claims

1. A method for preparing a rapidly amorphous halide oxide solid electrolyte material, characterized in that, Includes the following steps: Take an alkaline sodium source, tantalum compounds, transition metal chlorides, and B2O3; The alkaline sodium source, tantalum-containing compound, transition metal chloride, and B2O3 are ground and initially mixed to obtain a pre-mixed material; The initial mixed material is pretreated to obtain a pretreated precursor. The pretreated precursor was ball-milled to obtain the rapidly amorphous halide oxide solid electrolyte material. The transition metal is not tantalum.

2. The method for preparing a rapid amorphous halide oxide solid electrolyte material according to claim 1, characterized in that, The alkaline sodium source is at least one of Na2O, Na2O2, and NaOH.

3. The method for preparing a rapid amorphous halide oxide solid electrolyte material according to claim 1, characterized in that, The tantalum-containing compounds are TaCl5, TaCl4, TaCl3, TaCl2, TaO2, and Ta2O5.

4. The method for preparing a rapid amorphous halide oxide solid electrolyte material according to claim 1, characterized in that, The transition metal chloride is at least one of NbCl5, HfCl4, and ZrCl4.

5. The method for preparing a rapid amorphous halide oxide solid electrolyte material according to claim 1, characterized in that, The molar ratio of alkaline sodium source, tantalum-containing compound, transition metal chloride, and B₂O₃ is 1:1-x:x:y, where 0 <x<1,0<y≤0.5。 6. The method for preparing a rapid amorphous halide oxide solid electrolyte material according to claim 1, characterized in that, The pretreatment is as follows: under an inert atmosphere, heat at 100-400℃ for 0.5-4 hours.

7. The method for preparing a rapid amorphous halide oxide solid electrolyte material according to claim 1, characterized in that, The ball milling speed is 550-650 rpm, and the effective ball milling time is 10-30 minutes.

8. A rapidly amorphous halide oxide solid electrolyte material, characterized in that, Prepared by the preparation method according to any one of claims 1-7, Alternatively, the general formula of the rapidly amorphous halide oxide solid electrolyte material is: Na(Ta 1-x M x )OCl4-yB2O3, Wherein: M is a transition metal; the transition metal is not tantalum; x represents the doping amount of the transition metal M, 0 <x<1; y is the effective substitution amount of B2O3, 0 <y≤0.5。 9. The application of the fast amorphous halide oxide solid electrolyte material according to claim 8 in solid-state batteries.

10. A solid-state battery, characterized in that, Including the fast amorphous halide oxide solid electrolyte material as described in claim 8.