A short-time mechanically-chemically prepared zirconium-based halide solid-state electrolyte, a preparation method thereof, and a full solid-state battery

By introducing LiCl into the zirconium-based halide solid electrolyte and adopting a one-time feeding process, the problem of long synthesis time of zirconium-based chlorides is solved, and high ionic conductivity and electrochemical performance are maintained in a short time, making it suitable for large-scale production and battery applications.

CN123162302APending Publication Date: 2026-11-24GUANGDONG UNIV OF TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611297367.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-25
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

The mechanochemical synthesis of zirconium-based chloride Li₂ZrCl₆ in the existing technology is time-consuming and difficult to meet the practical application requirements of all-solid-state batteries. Furthermore, the long-term high-energy ball milling results in slow reaction kinetics, which restricts large-scale application.

Method used

Additional LiCl is introduced to adjust the stoichiometric composition, and a one-time feeding process is adopted to avoid the intermediate processing of step feeding, thus shortening the total ball milling time to less than 7 hours, including the pre-ball milling and high-energy ball milling processes.

Benefits of technology

It significantly shortens the synthesis time of zirconium-based halide solid electrolytes, maintains high ionic conductivity, improves preparation efficiency, is suitable for large-scale production, and broadens the electrochemical window to improve battery application performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123162302A_ABST
    Figure CN123162302A_ABST
Patent Text Reader

Abstract

The application relates to the technical field of solid-state batteries and discloses a short-time mechanically-chemically-prepared zirconium-based halide solid-state electrolyte, a preparation method thereof and a full solid-state battery, the chemical general formula of the electrolyte is Li x ZrX 6‑m‑n (SO4) m (PO4) n wherein X is Cl, Br or I, m+n=1, x=2+m+2n, 0.3<=m<=0.7, 0.3<=n<=0.7. During preparation, ZrX4, LiX, Li2SO4 and Li3PO4 are added at one time in a stoichiometric ratio under an inert atmosphere, pre-milling and high-energy ball milling are sequentially performed, and annealing is not performed. In the application, ZrX4, LiX, Li2SO4 and Li3PO4 are added at one time, the product can be obtained through pre-milling, high-energy ball milling and sieving, no step-by-step feeding, no intermediate system prepared in sequence, no annealing treatment are needed, the technological process is obviously simplified, and the processing time required for obtaining a zirconium-based halide electrolyte with high ionic conductivity can be obviously shortened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of solid-state battery technology, specifically to a zirconium-based halide solid electrolyte prepared by short-time mechanochemical methods and an all-solid-state battery. Background Technology

[0002] All-solid-state batteries are widely considered the core direction of next-generation energy storage technology due to their combination of high safety and high energy density potential. Halide solid electrolytes, with their high ionic conductivity, good cold-pressing film formation properties, and excellent compatibility with high-voltage cathode materials, have attracted widespread attention in recent years.

[0003] Among various halide systems, zirconium chloride Li₂ZrCl₆ (LZC) is favored due to its relatively low raw material cost, relatively simple preparation process, and good compatibility with oxide cathode materials. However, LZC's room temperature ionic conductivity (typically around 0.4 mS·cm) is limited. -1 However, this still falls short of meeting the practical application requirements of all-solid-state batteries. Researchers have made numerous attempts to improve their conductivity. For example, some studies have obtained modified LZC materials with higher conductivity by replacing chlorine sites with oxygen or sulfur, but the ball milling time for their mechanochemical synthesis still varies from several hours to 24 hours. Other studies have used Al³⁺… + For Zr 4+ The heterovalent substitution increased the ionic conductivity of the LZC-based electrolyte to 1.13 mS·cm. -1 However, the synthesis process still requires up to 12 hours of high-energy ball milling.

[0004] In recent years, polyanion doping strategies have emerged as promising approaches in the field of halide solid electrolytes. Recent studies have introduced carbonate ions into zirconium chloride frameworks, validating the feasibility of polyanion engineering in improving the performance of LZC-based halide electrolytes. However, its mechanochemical synthesis process still requires high-energy ball milling treatment lasting over 12 hours.

[0005] The above studies indicate that while anion substitution, cation substitution, and polyanion doping can effectively improve the ionic conductivity of LZC-based halide electrolytes, their mechanochemical synthesis processes are generally time-consuming, becoming a significant bottleneck restricting large-scale applications. Existing synthetic routes mostly employ direct reaction strategies involving long-duration high-energy ball milling, or rely on complex processes involving stepwise feeding and intermediate pretreatment, resulting in slow reaction kinetics and difficulty in reducing overall processing time.

[0006] Therefore, how to shorten the mechanochemical synthesis time of zirconium-based halide solid electrolytes by designing a reasonable raw material system and optimizing the feeding path while maintaining high ionic conductivity is a technical problem that has not yet been solved by existing technologies. Summary of the Invention

[0007] The purpose of this invention is to significantly shorten the mechanochemical synthesis time of zirconium-based halide solid electrolytes without significantly sacrificing ionic conductivity, while minimizing the impact on other electrochemical properties of the electrolyte itself (such as the electrochemical window), and to control the total ball milling time to within 7 hours, which is beneficial for large-scale application.

[0008] In view of this, the present invention provides a zirconium-based halide solid electrolyte prepared by mechanochemical means in a short time, its preparation method, and its application. The core of achieving the "short time" effect lies in the synergy of two aspects: first, the introduction of additional LiCl to adjust the stoichiometric composition and accelerate reaction kinetics; second, the use of a single-feed process to avoid the additional time consumption caused by intermediate processing in stepwise feeding. Neither of these aspects alone can achieve the short-time effect of this application: if only LiCl is introduced but stepwise feeding is used, the time required to achieve a similar conductivity is significantly longer than with a single-feed process; if only a single-feed process is used but LiCl is not introduced, the conductivity level of Example 1 cannot be achieved within the same time frame.

[0009] To achieve the above objectives, in a first aspect, the present invention provides a method for preparing a zirconium-based halide solid electrolyte by short-time mechanochemical preparation, comprising the following steps: S1. Under an inert atmosphere, ZrX4, Li2SO4, Li3PO4, and LiX as an additional lithium source and halogen source are added to a ball mill container in stoichiometric ratio and pre-milled at 100-300 rpm for 0.5-2 h to obtain a premixed powder. Where: X is Cl, Br or I, the molar ratio of LiX to ZrX4 is 1:1, the molar ratio of Li2SO4 to ZrX4 is m, the molar ratio of Li3PO4 to ZrX4 is n, m+n=1, 0.3≤m≤0.7, 0.3≤n≤0.7; S2. The premixed powder is ball-milled at 400-700 rpm for 2-7 hours at a ball-to-powder ratio of (20-50):1 to form electrolyte powder. The powder is then sieved to obtain the zirconium-based halide solid electrolyte, with the chemical formula Li. x ZrX 6-m-n (SO4) m (PO4) n Where m+n=1, x=2+m+2n, 0.3≤m≤0.7, 0.3≤n≤0.7; In the above steps, the total ball milling time does not exceed 7 hours, and no annealing treatment is performed.

[0010] As a further preferred technical solution of the present invention, the total ball milling time is 4 hours, wherein the pre-ball milling time in step S1 is 1 hour and the rotation speed is 150 rpm, and the high-energy ball milling time in step S2 is 3 hours, the rotation speed is 500 rpm, and the ball-to-material ratio is 30:1.

[0011] As a further preferred embodiment of the present invention, X is Cl, m=n=0.5, and the chemical formula of the zirconium-based halide solid electrolyte is Li. 3.5 ZrCl5(SO4) 0.5 (PO4) 0.5 .

[0012] In this invention, using 1 mol ZrX4 as a baseline, when m+n=1, regardless of the values ​​of m and n, the amount of LiX in the raw materials remains constant at 1 mol. Only the amounts of Li2SO4 and Li3PO4 are adjusted proportionally, resulting in a simple raw material formulation suitable for a single-feed mechanochemical process. This invention introduces LiX (X being Cl, Br, or I) into the raw material system to: firstly, provide sufficient chloride and lithium ions, allowing for greater control over the stoichiometric composition of the product; and secondly, avoid reliance on polyanionic groups to compensate for charge balance due to chloride vacancies, thereby helping to suppress the precipitation of crystalline sulfate impurities. In other words, the introduction of LiX makes SO4... 2- and PO4 3- It no longer needs to assume the role of charge compensation, thus eliminating the thermodynamic driving force for the precipitation of polyanions in crystalline form.

[0013] According to a second aspect of the present invention, a zirconium-based halide solid electrolyte is provided, which is prepared by the preparation method of the first aspect described above.

[0014] As a further preferred embodiment of the present invention, the zirconium-based halide solid electrolyte has an ionic conductivity of 1.69–2.06 mS·cm at 25°C. -1 .

[0015] According to a third aspect of the present invention, the present invention provides a composite positive electrode comprising a positive electrode active material, a conductive agent, and a zirconium halide solid electrolyte as described in the second aspect above; preferably, the zirconium halide solid electrolyte in the composite positive electrode accounts for 5wt%-30wt% by mass.

[0016] According to a fourth aspect of the present invention, an all-solid-state battery is provided, comprising a positive electrode, a negative electrode, and a solid electrolyte layer disposed between the positive electrode and the negative electrode; the solid electrolyte layer comprises the zirconium halide solid electrolyte of the second aspect described above, and / or the positive electrode is the composite positive electrode described in the third aspect.

[0017] Compared with the prior art, the present invention can achieve the following beneficial effects: (1) Preparation time is greatly shortened. By introducing the synergistic effect of LiCl and the "one-time feeding" process, the total ball milling time can be controlled within 7 hours (the preferred scheme has a total processing time of only about 4 hours after 1 hour of pre-ball milling and 3 hours of high-energy ball milling). Compared with the long ball milling time of 12 to 24 hours generally required by the prior art, the synthesis time is significantly shortened and the preparation efficiency is improved.

[0018] (2) Maintaining high ionic conductivity. With a significantly shortened preparation time, the preferred embodiment of this invention (Example 1) achieves a room-temperature ionic conductivity of 2.06 mS·cm. -1 .

[0019] (3) The composition window is clearly defined. When m:n is 3:7, 1:1 and 7:3, the room temperature ionic conductivity is 1.82, 2.06 and 1.69 mS·cm, respectively. -1 This indicates that high ionic conductivity can be obtained within the ranges of 0.3≤m≤0.7 and 0.3≤n≤0.7.

[0020] (4) The process is simple and suitable for large-scale production. The present invention adds four raw materials, ZrX4, LiX, Li2SO4 and Li3PO4, at one time, and obtains the product by pre-ball milling, high-energy ball milling and sieving. There is no need for step feeding, no need for sequential preparation of intermediate systems and no need for annealing treatment, and the process flow is significantly simplified.

[0021] (5) The electrochemical window is widened. LSV test results show that the reduction / oxidation decomposition potential of Example 1 of the present invention is 1.03-4.38 V (window 3.35 V), while that of the stepwise feeding sample (Comparative Example 4-3) is 1.67-4.01 V (window 2.34 V), and the electrochemical window is widened by about 1.01 V.

[0022] (6) Excellent battery application performance. The all-solid-state battery using the preferred electrolyte of this invention has a first discharge specific capacity of 186 mAh·g at 0.1 C. -1 The initial coulombic efficiency was 84.2%, and the capacity retention rate after 100 cycles at 0.5 C was 87.3%, which was significantly better than the undoped control cell (initial coulombic efficiency 79.7%, capacity retention rate after 100 cycles at 0.5 C 62.8%). Attached Figure Description

[0023] The present invention will now be described in further detail with reference to the accompanying drawings and specific embodiments.

[0024] Figure 1 The XRD patterns are those of Examples 1, 2, 3, Comparative Examples 3-2 and 4-3 of this application.

[0025] Figure 2 The following are linear sweep voltammetry (LSV) curves of Comparative Examples 3-2, 4-3 and Example 1 of this application; where a is the LSV curve of Comparative Example 3-2; b is the LSV curve of Comparative Example 4-3 (stepwise feeding); and c is the LSV curve of Example 1.

[0026] The objectives, features, and advantages of this invention will be further explained in conjunction with the embodiments and with reference to the accompanying drawings. Detailed Implementation

[0027] The specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings. It should be understood that the specific embodiments described herein are for illustration and explanation only and are not intended to limit the present invention.

[0028] Unless otherwise defined, the technical terms used in the following embodiments have the same meanings as commonly understood by those skilled in the art to which this invention pertains. Unless otherwise specified, the test reagents used in the following embodiments are all battery-grade high-purity raw materials; the experimental methods described are all conventional methods unless otherwise specified.

[0029] In the following procedures, weighing, ball milling, sample preparation, and testing were all performed in an argon-filled glove box with a water oxygen content of less than 0.1 ppm; the ball mill jar and grinding beads were made of zirconium oxide; and all electrochemical tests were conducted at 25 °C. Ionic conductivity was measured using the AC impedance method. The electrolyte powder was cold-pressed and sandwiched between stainless steel blocking electrodes. The testing frequency was 1 MHz to 0.1 Hz, and the ionic conductivity was calculated based on the resistance, electrolyte sheet thickness, and effective area.

[0030] Example 1: m:n=1:1 This embodiment provides a zirconium-based halide solid electrolyte, prepared by short-time mechanochemical methods, as follows: (1) One-time feeding / premixing: Weigh 1 mol ZrCl4, 1 mol LiCl, 0.5 mol Li2SO4 and 0.5 mol Li3PO4, add the four raw materials into the ball mill jar at one time under argon atmosphere, and pre-ball mill at 150 rpm for 1 h to obtain premixed powder; (2) High-energy ball milling: The premixed powder was ball-milled at 500 rpm for 3 h at a ball-to-powder ratio of 30:1. The resulting powder was then passed through a 100-mesh sieve to obtain the solid electrolyte Li. 3.5 ZrCl5(SO4) 0.5 (PO4) 0.5 .

[0031] The solid electrolyte obtained in this embodiment has a room temperature ionic conductivity of 2.06 mS·cm.- ¹, Total ball milling time: 4 hours.

[0032] Comparative Example 1: This comparative example provides an undoped electrolyte Li₂ZrCl₆, and the specific preparation method is as follows: (1) Weigh 1 mol ZrCl4 and 2 mol LiCl, mix them under an argon atmosphere, and pre-ball mill at 150 rpm for 1 h; (2) Then, according to the ball-to-material ratio of 30:1, the powder is ball-milled at 600 rpm for 30 h. The powder obtained is passed through a 100-mesh sieve to obtain Li2ZrCl6.

[0033] The resulting solid electrolyte has a room-temperature ionic conductivity of 0.42 mS·cm. -1 The total ball milling time was 31 hours.

[0034] Comparative Example 2: No pre-ball milling (containing LiCl) The raw material composition is the same as that in Example 1 (containing LiCl), except that pre-ball milling is not performed. The four raw materials are added at once and then directly ball-milled at 500 rpm for 3 h with a ball-to-material ratio of 30:1. The resulting powder is passed through a 100-mesh sieve to obtain a solid electrolyte.

[0035] The resulting solid electrolyte has a room-temperature ionic conductivity of 1.55 mS·cm. -1 The total ball milling time was 3 hours.

[0036] Comparative Example 3-1: High-energy ball milling for 3 hours (without LiCl) (1) Weigh 1 mol ZrCl4, 0.5 mol Li2SO4 and 0.5 mol Li3PO4 (without adding LiCl), add the three raw materials to the ball mill jar at once under an argon atmosphere, and pre-mill at 150 rpm for 1 h; (2) Then, the powder was ball-milled at 500 rpm for 3 h with a ball-to-material ratio of 30:1. The resulting powder was then passed through a 100-mesh sieve.

[0037] The room temperature ionic conductivity of the obtained solid electrolyte is 1.33 mS·cm. -1 The total ball milling time was 4 hours.

[0038] Comparative Example 3-2: High-energy ball milling for 6 hours (without LiCl) The only difference from Comparative Example 3-1 is that the high-energy ball milling time at 500 rpm was extended to 6 h.

[0039] The room temperature ionic conductivity of the obtained solid electrolyte is 1.86 mS·cm. -1 The total ball milling time was 7 hours.

[0040] Comparative Example 4-1: High-energy ball milling for 2 hours (step-by-step feeding) 1) Ball mill Li2SO4 separately at 200 rpm for 1 h; 2) Pre-ball mill ZrCl4, LiCl and Li3PO4 at 150 rpm for 1 h, and then ball mill at 500 rpm for 2 h at a ball-to-material ratio of 30:1; 3) Mix the powders obtained from parts 1) and 2) above, and ball mill at 200 rpm for 1 h. Pass the resulting powder through a 100-mesh sieve.

[0041] The resulting solid electrolyte has a room-temperature ionic conductivity of 0.85 mS·cm. -1 The total ball milling time was 5 hours.

[0042] Comparative Example 4-2: High-energy ball milling for 4 hours (stepwise feeding) The difference from Comparative Example 4-1 is that, in step 2), the high-energy ball milling time at 500 rpm after mixing ZrCl4, LiCl and Li3PO4 was extended from 2h to 4h.

[0043] The room temperature ionic conductivity of the obtained solid electrolyte is 1.61 mS·cm. -1 The total ball milling time was 7 hours.

[0044] Comparative Example 4-3: High-energy ball milling for 8 hours (step-by-step feeding) The difference from Comparative Example 4-1 is that in step 2), the high-energy ball milling time of 500 rpm after mixing ZrCl4, LiCl and Li3PO4 was extended to 8 h.

[0045] The room temperature ionic conductivity of the obtained solid electrolyte is 1.93 mS·cm. -1 The total ball milling time was 11 hours.

[0046] Example 2: m:n=3:7 Weigh out 1 mol ZrCl4, 1 mol LiCl, 0.3 mol Li2SO4, and 0.7 mol Li3PO4, and keep the remaining preparation conditions the same as in Example 1 to obtain Li 3.7 ZrCl5(SO4) 0.3 (PO4) 0.7 .

[0047] The room temperature ionic conductivity of the obtained solid electrolyte is 1.82 mS·cm. -1 The total ball milling time was 4 hours.

[0048] Example 3: m:n=7:3 Weigh out 1 mol ZrCl4, 1 mol LiCl, 0.7 mol Li2SO4, and 0.3 mol Li3PO4, and follow the same preparation conditions as in Example 1 to obtain Li 3.3 ZrCl5(SO4) 0.7 (PO4) 0.3 .

[0049] The room temperature ionic conductivity of the obtained solid electrolyte is 1.69 mS·cm. -1 The total ball milling time was 4 hours.

[0050] Example 4: High-energy ball milling for 2 hours The raw material composition and other preparation conditions were the same as in Example 1, except that the high-energy ball milling time was adjusted to 2 h.

[0051] The room temperature ionic conductivity of the obtained solid electrolyte is 1.31 mS·cm. -1 The total ball milling time was 3 hours.

[0052] Example 5: High-energy ball milling for 4 hours The raw material composition and other preparation conditions were the same as in Example 1, except that the high-energy ball milling time was adjusted to 4 h.

[0053] The room temperature ionic conductivity of the obtained solid electrolyte is 2.02 mS·cm. -1 The total ball milling time was 5 hours.

[0054] Example 6: High-energy ball milling for 5 hours The raw material composition and other preparation conditions were the same as in Example 1, except that the high-energy ball milling time was adjusted to 5 h.

[0055] The room temperature ionic conductivity of the obtained solid electrolyte is 1.97 mS·cm. -1 The total ball milling time was 6 hours.

[0056] In Examples 1 and 4-6 above, when the high-energy ball milling time is 2 hours (Example 4), the conductivity is 1.31 mS·cm. -1 When the time is extended to 3 hours or more, the conductivity is ≥1.69 mS·cm. -1 In Example 1 (high-energy ball milling for 3 hours), the temperature reached 2.06 mS·cm. -1 , is the optimal value.

[0057] The following is a comprehensive comparative analysis of the solid electrolyte performance of Example 1 and Comparative Example 1, as follows: (1) Table 1 lists the composition, process conditions, ionic conductivity and corresponding total synthesis time of representative samples with and without LiCl introduced in the above examples and comparative examples, in order to examine the effect of the introduction of LiCl on the synthesis efficiency.

[0058] Table 1. Effects of LiCl introduction on ionic conductivity and synthesis time As shown in Table 1, within the same 4-hour preparation time, Example 1 with the introduction of LiCl (2.06 mS·cm) showed the best results. -1 Compared to Comparative Example 3-1 (1.33 mS·cm) without LiCl, -1 The conductivity increased by approximately 55%. Samples without LiCl required a longer total ball milling time of 7 hours (Comparative Examples 3-2) to achieve 1.86 mS·cm. -1 Its conductivity is still lower than that of Example 1 at 4h (2.06 mS·cm). -1 The results indicate that the introduction of LiCl can shorten the synthesis time required to achieve similar or higher conductivity from 7 hours to 4 hours, a reduction of more than 40%. Experimental results in Examples 1-3 show that in SO4... 2- With PO4 3- As the molar ratio m:n changes from 3:7 to 7:3, the room temperature ionic conductivity first increases and then decreases, reaching its highest value of 2.06 mS·cm when m:n = 1:1. -1 This result indicates that SO4 levels are within this range. 2- With PO4 3- The synergistic effect is composition-dependent, and a moderate ratio (m:n≈1:1) is more conducive to obtaining higher ionic conductivity.

[0059] (2) Table 2 compares the effects of single-feeding and step-feeding on ionic conductivity and total synthesis time required to achieve target performance under the same raw material ratio (all containing LiCl).

[0060] Table 2. Ionic conductivity and synthesis time for different feeding methods Table 2 shows that single-feeding is superior to step-feeding at all time points, especially in Example 1 (single-feeding, 4h, 2.06 mS·cm). -1 ) vs Comparative Example 4-1 (stepwise feeding, 5 hours, 0.85 mS·cm) -1 ), shorter time and higher conductivity; Example 6 (single feeding, 7h, 1.97 mS·cm) -1 ) vs Comparative Example 4-2 (stepwise feeding, 7h, 1.61 mS·cm) -1The conductivity increased by approximately 22% with the next feeding at the same time. Comparative Example 4-3 (stepwise feeding, 11h, 1.93 mS·cm) -1 It still did not reach the 2.06 mS·cm achieved in Example 1 within 4 hours. -1 This indicates that single-feeding is superior to multi-feeding in both efficiency and performance—it can achieve higher conductivity in a shorter time.

[0061] Example 2 uses a single-feeding process, and only 1.31 mS·cm is obtained when the total ball milling time is about 3 hours. -1 The room temperature ionic conductivity; with extended high-energy ball milling, Example 1 achieved a high ionic conductivity of 2.06 mS·cm at a total ball milling time of approximately 4 h. -1 The room temperature ionic conductivity indicates that increasing the high-energy ball milling time is beneficial to improving the ionic conductivity; however, when the high-energy ball milling is further extended to 4 h (Example 5) and 6 h (Example 6), the conductivity shows a decreasing trend compared to Example 1, reaching 2.02 and 1.97 mS·cm, respectively. -1 This indicates that excessively increasing the high-energy ball milling time actually leads to a decrease in ionic conductivity.

[0062] (3) The electrochemical window of representative samples was evaluated by linear sweep voltammetry (LSV) at a scan rate of 0.1 mV / s and a test temperature of 25 ℃. Figure 2 The following are linear sweep voltammetry (LSV) curves for Comparative Examples 4-3 and Example 1 of this application, where (a) is the LSV curve for Comparative Example 4-3 (stepwise addition) and (b) is the LSV curve for Example 1. The oxidative decomposition onset potentials and electrochemical windows for Comparative Examples 4-3 and Example 1 are listed in Table 3.

[0063] Table 3. Comparison of electrochemical windows for different samples Depend on Figure 2 As shown in Table 3, the oxidation decomposition onset potential of Comparative Example 4-3, which used stepwise feeding without introducing LiCl, was 4.01 V, and the electrochemical window was 2.34 V; the oxidation decomposition onset potential of Comparative Example 3-2, which used stepwise feeding but introduced LiCl, was 4.18 V, and the electrochemical window was 2.71 V; while the oxidation decomposition onset potential of Example 1, which used a single feeding process and introduced LiCl, was significantly increased to 4.38 V, and the electrochemical window reached 3.35 V. These results indicate that both the introduction of LiCl and the single feeding process have an enhancing effect on the electrochemical window, and the two work synergistically to further broaden the window.

[0064] Application Example 1: All-solid-state battery using solid-state electrolyte from Example 1 High-nickel ternary cathode material LiNi 0.8 Co0.1 Mn 0.1 O2 (NCM811), Solid electrolyte of Example 1 (Li 3.5 ZrCl5(SO4) 0.5 (PO4) 0.5 The composite positive electrode layer is prepared by mixing the solid electrolyte powder (65:30:5 by mass) and VGCF conductive agent, grinding them evenly, and then using the mixture as the composite positive electrode layer. Approximately 80 mg of the solid electrolyte powder from Example 1 is weighed and cold-pressed in a 10 mm diameter mold at 200 MPa to obtain the solid electrolyte layer. 10-15 mg of the composite positive electrode powder is evenly spread on the surface of the electrolyte layer and cold-pressed at 300 MPa. A 60 mg Li6PS5Cl intermediate layer is placed between the electrolyte layer and the lithium indium alloy negative electrode. All the above layers are then integrally cold-pressed in a mold to assemble an all-solid-state battery.

[0065] Test results: Tested under conditions of 2.8–4.3 V and 25 °C, the initial discharge specific capacity at 0.1 C was 186 mAh·g. -1 The initial coulombic efficiency was 84.2%; the capacity retention after 100 cycles at 0.5 C was 87.3%.

[0066] Comparative Application 1: All-solid-state battery using undoped electrolyte The battery structure and test conditions were the same as in Example 7, except that the electrolyte of Example 1 was replaced with Li2ZrCl6 of Comparative Example 1.

[0067] Test results: The initial discharge specific capacity at 0.1 C is 175 mAh·g. -1 The initial coulombic efficiency was 79.7%; the capacity retention after 100 cycles at 0.5 C was 62.8%.

[0068] Table 4. Performance of all-solid-state batteries The data in Table 4 show that, under the same battery structure and test conditions, the battery using the electrolyte of Example 1 has higher initial discharge specific capacity, initial coulombic efficiency, and 100-cycle capacity retention.

[0069] While specific embodiments of the present invention have been described above, those skilled in the art should understand that these are merely illustrative examples, and various changes or modifications can be made to these embodiments without departing from the principles and essence of the present invention. The scope of protection of the present invention is defined only by the appended claims.

Claims

1. A method for preparing a zirconium-based halide solid electrolyte by short-time mechanochemical preparation, characterized in that, Includes the following steps: S1. Under an inert atmosphere, ZrX4, Li2SO4, Li3PO4, and LiX as an additional lithium source and halogen source are added to a ball mill container in stoichiometric ratio and pre-milled at 100-300 rpm for 0.5-2 h to obtain a premixed powder. Where: X is Cl, Br or I, the molar ratio of LiX to ZrX4 is 1:1, the molar ratio of Li2SO4 to ZrX4 is m, the molar ratio of Li3PO4 to ZrX4 is n, m+n=1, 0.3≤m≤0.7, 0.3≤n≤0.7; S2. The premixed powder is ball-milled at 400-700 rpm for 2-7 hours at a ball-to-powder ratio of (20-50):1 to form electrolyte powder. The powder is then sieved to obtain the zirconium-based halide solid electrolyte, with the chemical formula Li. x ZrX 6-m-n (SO4) m (PO4) n Where m+n=1, x=2+m+2n, 0.3≤m≤0.7, 0.3≤n≤0.7; In the above steps, the total ball milling time does not exceed 7 hours, and no annealing treatment is performed.

2. The method for preparing zirconium-based halide solid electrolyte by short-time mechanochemical preparation according to claim 1, characterized in that, The total ball milling time is 4 hours, of which the pre-ball milling time in step S1 is 1 hour and the rotation speed is 150 rpm, and the high-energy ball milling time in step S2 is 3 hours, the rotation speed is 500 rpm, and the ball-to-material ratio is 30:

1.

3. The method for preparing zirconium-based halide solid electrolyte by short-time mechanochemical preparation according to claim 1, characterized in that, X is Cl, m=n=0.5, and the chemical formula of the zirconium-based halide solid electrolyte is Li. 3.5 ZrCl5(SO4) 0.5 (PO4)0.

5.

4. A zirconium-based halide solid electrolyte, characterized in that, It is prepared by the preparation method according to any one of claims 1-3.

5. The zirconium-based halide solid electrolyte according to claim 4, characterized in that, The zirconium-based halide solid electrolyte has an ionic conductivity of 1.69–2.06 mS·cm at 25 °C. - ¹.

6. A composite positive electrode, characterized in that, It includes positive electrode active material, conductive agent, and zirconium-based halide solid electrolyte as described in claim 4 or 5.

7. The composite positive electrode according to claim 6, characterized in that, The zirconium-based halide solid electrolyte in the composite cathode accounts for 5wt% to 30wt% of the total mass.

8. An all-solid-state battery, characterized in that, It includes a positive electrode, a negative electrode, and a solid electrolyte layer disposed between the positive electrode and the negative electrode; the solid electrolyte layer comprises the zirconium-based halide solid electrolyte of claim 4 or 5, and / or the positive electrode is the composite positive electrode of claim 6 or 7.