Modified electrolyte, battery and electric device
By introducing additives with a COOR₁-Ar-OSO₂R₂ structure into the electrolyte, the problems of oxidative decomposition of the electrolyte under high voltage and insufficient lithium salt dissociation are solved, forming a dense CEI film, which improves the battery's high voltage stability, long cycle performance and rate performance, and enhances thermal stability.
Patent Information
- Application Number
- CN202611316199.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-27
- Publication Date
- 2026-11-24
AI Technical Summary
Existing electrolytes are prone to oxidation and decomposition under high voltage, leading to cell expansion, increased internal pressure, dissolution of transition metals that damage the SEI film, insufficient lithium salt dissociation, low conductivity, and inability to meet the requirements of high-rate charging and discharging. Additives have single or antagonistic functions, and the density of the interface film and ionic conductivity cannot be achieved simultaneously, affecting battery performance.
The first additive, containing the COOR₁-Ar-OSO₂R₂ structure, is combined with lithium salt and non-aqueous solvent. Through haloalkyl sulfonate groups, carboxylic acid alkyl groups and unsaturated nitrogen-indene heterocyclic groups, lithium salt dissociation is synergistically promoted, the solvation structure is optimized, the interfacial impedance is reduced, a dense CEI film is formed, and the high voltage stability and rate performance of the battery are improved.
It achieves efficient lithium salt dissociation under high voltage, strengthens interface protection, reduces interface impedance, and improves the battery's high-voltage stability, long-cycle performance, and rate performance, while also enhancing thermal stability.
Smart Images

Figure SMS_17 
Figure SMS_18 
Figure SMS_19
Abstract
Description
Technical Field
[0001] This application belongs to the field of battery technology and relates to a modified electrolyte, a battery, and an electrical device. Background Technology
[0002] As lithium-ion batteries rapidly develop towards higher energy density, faster charging rates, and longer cycle life, existing electrolyte and additive technologies have many inherent defects under high-voltage conditions of 4.4V and above, which has become a key bottleneck restricting the improvement of high-voltage battery performance.
[0003] In existing electrolyte systems, conventional carbonate electrolyte systems readily undergo catalytic oxidation and decomposition reactions on the surface of high-nickel cathodes at high potentials above 4.4V, continuously generating polar byproducts such as carboxylic acids, esters, and alcohols, as well as gases such as CO2 and CO. This directly leads to abnormal expansion of the cell thickness and increased internal pressure. Simultaneously, transition metal ions (nickel, cobalt, manganese, etc.) in the cathode material continuously dissolve under the combined effects of high voltage and electrolyte side reactions. After the dissolved metal ions migrate to the anode interface, they disrupt the integrity of the anode solid electrolyte interphase (SEI) film, causing irreversible consumption of active lithium and lithium plating at the anode, ultimately resulting in rapid capacity decay and significantly shortened cycle life. Furthermore, mainstream lithium salts such as LiPF6 do not fully dissociate in conventional carbonate solvents, resulting in low electrolyte ionic conductivity. Additionally, the strong binding force between lithium ions and solvent molecules and the high desolvation energy lead to severe interface polarization under high-current fast charging, failing to meet the demands of high-rate charging and discharging, thus compromising both fast charging performance and energy density.
[0004] To address these issues, additives are often added for modification. However, existing additives have limited functionality. For instance, current high-voltage film-forming additives can only form films on the cathode surface and cannot simultaneously address lithium salt dissociation and ion conduction performance. Conductive additives can only improve conductivity and cannot suppress electrolyte oxidation and decomposition under high voltage. Even when multiple functional additives are combined, the direct antagonistic effects of the additives can lead to problems such as oxidation / reduction potential mismatch, film competition, and poor solvent compatibility. This not only fails to achieve synergistic performance but also results in increased interfacial impedance and deterioration of battery cycle performance, severely impacting battery performance under high voltage. Furthermore, existing additives generally present a contradiction between "density and ion conductivity." Inorganic-phase-dominated films have high impedance and poor rate performance, while organic-phase-dominated films have insufficient mechanical strength and are prone to rupture under high voltage, failing to achieve long-term interfacial protection during long cycles.
[0005] Therefore, how to enable the electrolyte to simultaneously promote lithium salt dissociation, protect the high-voltage interface, optimize the solvation structure, and reduce interfacial impedance under high voltage and high rate conditions, without affecting the use of the electrolyte in the battery, and effectively improve battery performance, is an urgent technical problem to be solved. Summary of the Invention
[0006] To address the shortcomings of existing technologies, the purpose of this application is to provide a modified electrolyte, battery, and electrical device. The electrolyte provided in this application, under the action of a first additive, simultaneously promotes lithium salt dissociation, protects the high-voltage interface, optimizes the solvation structure, and reduces interfacial impedance, thereby improving the electrochemical performance of the corresponding battery under high voltage and high rate conditions.
[0007] To achieve the purpose of this application, the following technical solution is adopted:
[0008] In a first aspect, this application provides a modified electrolyte comprising a non-aqueous solvent, a lithium salt, and a first additive, wherein the first additive has the following structure:
[0009] COOR1-Ar-OSO2R2;
[0010] Wherein, R1 is selected from C1-C4 straight-chain or branched alkyl groups, Ar is selected from unsaturated nitrogen-containing indene groups, and R2 is selected from C1-C4 fully haloalkyl groups.
[0011] In one embodiment of this application, the unsaturated nitrogen-indene group is selected from 5-oxo-1,2,3,5-tetrahydro-nitrogen-indene.
[0012] In one embodiment of this application, COOR1 is attached to the 3-position of the unsaturated nitrogen-indene group.
[0013] In one embodiment of this application, the OSO2R2 is attached to the 7-position of the unsaturated nitrogen indene group.
[0014] In one embodiment of this application, R2 is selected from C1-C4 perfluoroalkyl groups.
[0015] In one embodiment of this application, the first additive has the formula... To the style At least one of the following structural formulas:
[0016] .
[0017] In one embodiment of this application, based on the total mass of the non-aqueous solvent, the lithium salt, and the first additive being 100wt%, the mass percentage of the first additive is 0.05wt% to 3wt%, preferably 0.2wt% to 1.5wt%.
[0018] In one embodiment of this application, based on a total mass of 100wt% for the non-aqueous solvent, the lithium salt, and the first additive, the mass percentage of the non-aqueous solvent is 80wt% to 90wt%.
[0019] In one embodiment of this application, the non-aqueous solvent includes carbonate organic solvents.
[0020] In one embodiment of this application, the total viscosity of the non-aqueous solvent is ≤1.8 mPa·s, and the total dielectric constant of the non-aqueous solvent is ≥35.
[0021] In one embodiment of this application, the concentration of the lithium salt in the modified electrolyte is 0.8 mol / L to 1.5 mol / L, preferably 1.2 mol / L to 1.5 mol / L.
[0022] In one embodiment of this application, the modified electrolyte further includes at least one of a second additive, a third additive, or a fourth additive that is different from the first additive, wherein the second additive is a high-voltage antioxidant additive, the third additive is a low-resistance additive, and the fourth additive is a film-forming additive.
[0023] In one embodiment of this application, the second additive includes at least one of 1,3-propanesulfonate lactone, vinyl sulfate, or adiponitrile.
[0024] In one embodiment of this application, the total mass of the non-aqueous solvent, the lithium salt, and the first additive is 100 wt%, and the mass of the second additive added is 0.1 wt% to 3 wt%.
[0025] In one embodiment of this application, the third additive includes lithium difluorophosphate and / or lithium tetrafluoroborate.
[0026] In one embodiment of this application, the total mass of the non-aqueous solvent, the lithium salt, and the first additive is 100 wt%, and the mass of the third additive added is 0.1 wt% to 2 wt%.
[0027] In one embodiment of this application, the fourth additive includes fluoroethylene carbonate and / or vinylene carbonate.
[0028] In one embodiment of this application, the total mass of the non-aqueous solvent, the lithium salt, and the first additive is 100 wt%, and the mass of the fourth additive is 0.5 wt% to 8 wt%.
[0029] In a second aspect, this application provides a battery comprising the modified electrolyte as described in the first aspect.
[0030] Thirdly, this application also provides an electrical device, characterized in that the electrical device includes a battery as described in the second aspect.
[0031] Compared with the prior art, this application has the following advantages:
[0032] To address the problems of existing electrolyte systems, this application provides a modified electrolyte by incorporating a first additive. The first additive, with its haloalkyl sulfonate groups, carboxylic acid alkyl groups, and unsaturated nitrogen-indene heterocyclic groups as core functional units, simultaneously solves the problems of severe oxidative decomposition of electrolytes in high-voltage systems and rapid capacity decay caused by transition metal dissolution. It also addresses issues such as insufficient lithium salt dissociation, low electrolyte conductivity, and poor rate performance due to high lithium-ion desolvation energy. Furthermore, it resolves the problems of single-function additives and antagonistic effects arising from multiple additive combinations, while simultaneously addressing the trade-off between interfacial film density and ionic conductivity. This improves the high-voltage stability, long-cycle performance, and rate performance of the corresponding battery, as well as its thermal stability. Detailed Implementation
[0033] The technical solution of this application will be further described below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely to help understand this application and should not be regarded as specific limitations on this application.
[0034] In this application, technical features or solutions described using open-ended terms such as "comprising" do not exclude additional non-conflicting elements beyond those listed unless otherwise specified. They are considered to disclose both closed-ended features or solutions consisting solely of the listed elements and open-ended features or solutions that may include additional non-conflicting elements beyond those listed. For example, if A includes a1, a2, and a3, unless otherwise specified, it means that A may consist only of a1, a2, and a3, or it may include other non-conflicting elements based on a1, a2, and a3. This corresponds to the disclosure of technical solutions such as "A consists of a1, a2, and a3" and "A not only includes a1, a2, and a3, but may also include other non-conflicting elements."
[0035] The above description is only a specific embodiment of this application, but the protection scope of this application is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in this application fall within the protection and disclosure scope of this application.
[0036] In one embodiment, this application provides a modified electrolyte comprising a non-aqueous solvent, a lithium salt, and a first additive, wherein the first additive has the following structure:
[0037] COOR1-Ar-OSO2R2;
[0038] Wherein, R1 is selected from C1-C4 straight-chain or branched alkyl groups, Ar is selected from unsaturated nitrogen-containing indene groups, and R2 is selected from C1-C4 fully haloalkyl groups.
[0039] It should be noted that C1-C4 in this application refers to the number of carbon atoms in the corresponding substituents, which can be any one of 1, 2, 3 or 4.
[0040] To address the problems of existing electrolyte systems, this application provides a modified electrolyte by incorporating a first additive. The first additive, with its haloalkyl sulfonate groups, carboxylic acid alkyl groups, and unsaturated nitrogen-indene heterocyclic groups as core functional units, simultaneously solves the problems of severe oxidative decomposition of electrolytes in high-voltage systems and rapid capacity decay caused by transition metal dissolution. It also addresses issues such as insufficient lithium salt dissociation, low electrolyte conductivity, and poor rate performance due to high lithium-ion desolvation energy. Furthermore, it resolves the problems of single-function additives and antagonistic effects arising from multiple additive combinations, while simultaneously addressing the trade-off between interfacial film density and ionic conductivity. This improves the high-voltage stability, long-cycle performance, and rate performance of the corresponding battery, as well as its thermal stability.
[0041] The modified electrolyte of this application, when modified with the first additive, has the following advantages: the first additive uses an unsaturated nitrogen-indene group as the parent structure. This heterocyclic conjugated unsaturated structure can significantly improve the antioxidant stability of the additive molecule, increase the oxidative decomposition potential of the electrolyte, and perfectly adapt to high-voltage positive electrode systems of 4.4V and above. Furthermore, the nitrogen atom in the heterocyclic ring has a lone pair of electrons, which can react with Li... +The additive forms weak coordination, synergistically optimizing the lithium-ion solvation structure with ester and trifluoromethanesulfonate groups, reducing interfacial polarization. Furthermore, the unsaturated nitrogen-indene group, a rigid heterocyclic structure, enhances the mechanical strength of the interfacial film, improving its structural stability during cycling and achieving long-term interfacial protection. The COOR1 in the first additive, an alkyl carboxylic acid ester group, has a similar chemical structure to non-aqueous solvents, especially carbonate organic solvents, exhibiting excellent compatibility. This promotes uniform dispersion of the first additive in the electrolyte, preventing additive precipitation at high concentrations. The carbonyl oxygen atom in the ester group possesses lone pairs of electrons, which can also synergistically form weak coordination bonds with Li⁺, participating in the reconstruction of the lithium-ion solvation sheath, weakening the strong binding between lithium ions and solvent molecules, reducing desolvation energy, and further improving ion transport rate and rate performance. Simultaneously, this group can participate in the construction of the positive and negative electrode interfacial films, introducing a flexible organic phase into the interfacial film, enhancing… The mechanical strength and flexibility of the membrane prevent membrane structure rupture during cycling, achieving the goal of achieving both density and ionic conductivity in the CEI / SEI membrane. The OSO2R2 group in the first additive, namely the haloalkyl sulfonate group, has strong polarity, and both the fully haloalkyl and sulfonyl groups are strong electron-withdrawing groups, which synergistically produce a strong electron-withdrawing inductive effect, significantly improving the dielectric constant of the electrolyte, breaking the ion pair binding in lithium salts, promoting the efficient dissociation of lithium salts, and greatly improving the ionic conductivity of the electrolyte. The group has a matching oxidation potential, which can preferentially undergo directional oxidation and decomposition on the surface of the high-voltage positive electrode before carbonate solvents, forming a dense CEI protective film containing inorganic phases such as SO and LiF, further enhancing the density of the interfacial film, isolating the catalytic active sites of the positive electrode, and inhibiting the oxidative decomposition of the electrolyte and the dissolution of transition metals. At the same time, the synergistic effect of halogen atoms and sulfonyl groups also improves the thermal stability and flame retardancy of the electrolyte and inhibits thermal runaway chain reactions.
[0042] This application achieves the integration of four core functions—promoting lithium salt dissociation, high-voltage interface film formation, solvation structure regulation, and reducing interface impedance—through the separation design and synergistic effect of specific multi-groups in a single molecule. It also provides a flame-retardant effect, thereby improving the battery's high-voltage stability, rate performance, long cycle life, and thermal stability.
[0043] In some embodiments, the unsaturated nitrogen-indene group is selected from 5-oxo-1,2,3,5-tetrahydro-nitrogen-indene.
[0044] In some embodiments, the COOR1 is attached to the 3-position of the unsaturated nitrogen-indene group.
[0045] In some embodiments, the OSO2R2 is attached to the 7-position of the unsaturated nitrogen indene group.
[0046] In the first additive of this application, the site occupancy relationship between the functional groups is crucial. Using an unsaturated nitrogen-indene group as the parent nucleus, OSO2R2 is confined to the 7-position, COOR1 to the 3-position, and an oxocarbonyl group at the 5-position, a superior site occupancy combination is formed. This combination has significant advantages: the group at the 7-position and the group at the 3-position are located on opposite sides of the parent nucleus, and their steric hindrances do not interfere with each other, avoiding functional group competition and ensuring that the functions of the two major groups can be performed independently; at the same time, it can also maximize the conjugation effect. The group substituted at the 7-position forms p-π conjugation with the conjugated unsaturated structure of the parent nucleus, further enhancing the oxidation activity of the group and enabling it to form a film on the cathode surface preferentially over the solvent; this site combination can also precisely match the sites, making the oxidation potential of the first additive more suitable for the film formation window of the 4.4V high-voltage system, so that it will not oxidize and fail prematurely, and can preferentially decompose and form a film over the carbonate solvent, resulting in a dense and high-performance CEI / SEI film.
[0047] In some embodiments, R2 is selected from C1-C4 perfluoroalkyl groups.
[0048] This application selects fluorine atoms as the halogen atom of R2. Compared with other halogen atoms, it significantly broadens the electrochemical window of the electrolyte, improves the antioxidant effect, and can further enhance lithium salt dissociation and ionic conductivity, strengthen thermal stability, and optimize electrode interface film formation, thereby improving the overall cycle life and safety of high-voltage batteries.
[0049] In some embodiments, the first additive has the formula To the style At least one of the following structural formulas:
[0050] .
[0051] It is understandable that, in addition to the above ( )to( Besides the structural formula of ), there are many other structural formulas with various combinations. Those skilled in the art can make adaptive selections and adjustments according to the specific scheme.
[0052] It is understood that the first additive provided in this application can be purchased directly through commercial means; or it can be synthesized by itself using conventional synthesis methods according to the specific concept. This application does not limit the specific source of the first additive. Under the premise of not violating the overall technical concept of this application, reasonable sources are applicable.
[0053] For example, in the structural formula ( ), namely methyl 5-oxo-7-(((trifluoromethyl)sulfonyl)oxy)-1,2,3,5-tetrahydro-indene-3-carboxylic acid (CAS No.: 1956310-54-5).
[0054] In some embodiments, based on a total mass of 100wt% of the non-aqueous solvent, the lithium salt, and the first additive, the mass percentage of the first additive is 0.05wt% to 3wt%, for example, 0.05wt%, 0.1wt%, 0.2wt%, 0.5wt%, 1.0wt%, 1.5wt%, 2.0wt%, 2.5wt%, or 3.0wt%.
[0055] Further, based on the total mass of the non-aqueous solvent, the lithium salt, and the first additive being 100wt%, the mass percentage of the first additive is preferably 0.2wt% to 1.5wt%, for example, 0.2wt%, 0.25wt%, 0.3wt%, 0.35wt%, 0.4wt%, 0.45wt%, 0.5wt%, 0.55wt%, 0.6wt%, 0.65wt%, 0.7wt%, 0.75wt%, 0.8wt%, 0.85wt%, 0.9wt%, 0.95wt%, 1.0wt%, 1.05wt%, 1.1wt%, 1.15wt%, 1.2wt%, 1.25wt%, 1.3wt%, 1.35wt%, 1.4wt%, 1.45wt%, or 1.5wt%, etc.
[0056] In the modified electrolyte of this application, the mass percentage of the first additive directly affects its effectiveness. When the mass percentage is adjusted to 0.05wt%~3wt%, the effect of the first additive in the modified electrolyte is more significant. More preferably, it is 0.2wt%~1.5wt%, which will not affect the viscosity of the electrolyte itself, thus avoiding excessive viscosity that would limit the use of the electrolyte. At the same time, it can give full play to the synergistic effect of various groups and linkage sites, greatly improving the high voltage stability, long cycle performance, rate performance and thermal stability of the battery.
[0057] In some embodiments, based on the total mass of the non-aqueous solvent, the lithium salt, and the first additive being 100wt%, the mass percentage of the non-aqueous solvent is 80wt% to 90wt%, for example, 80wt%, 81wt%, 82wt%, 83wt%, 84wt%, 85wt%, 86wt%, 87wt%, 88wt%, 89wt%, or 90wt%.
[0058] In some embodiments, the non-aqueous solvent includes carbonate organic solvents.
[0059] In the modified electrolyte of this application, carbonate organic solvents are selected as non-aqueous solvents, which have higher compatibility with the first additive and can take into account both lithium salt dissociation and ion transport effects, thereby achieving precise control of the solvation structure.
[0060] It is understood that the carbonate organic solvents used in this application may be selected from cyclic carbonates and / or chain carbonates.
[0061] For example, but not limitingly, the cyclic carbonate includes ethylene carbonate (EC) and / or propylene carbonate (PC) having high dielectric constants, preferably EC, which has better lithium salt dissociation performance.
[0062] For example, but not in a limiting sense, the chain carbonate includes at least one of dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), or diethyl carbonate (DEC), preferably an EMC+DMC combination, which further reduces electrolyte viscosity and improves lithium-ion transport rate; wherein EMC and DMC can be added in equal mass ratio or in any other arbitrary ratio, and can be adaptively selected and adjusted according to actual needs.
[0063] More specifically: the mass ratio of the cyclic carbonate to the chain carbonate is (20~40):(60~80), for example 20:80, 25:75, 30:70, 35:65 or 40:60, etc.
[0064] In some embodiments, the total viscosity of the non-aqueous solvent is ≤1.8 mPa·s, for example 1.8 mPa·s, 1.7 mPa·s, 1.6 mPa·s, 1.5 mPa·s, 1.4 mPa·s, 1.3 mPa·s, 1.2 mPa·s, 1.1 mPa·s, 1.0 mPa·s, 0.9 mPa·s, 0.8 mPa·s, 0.7 mPa·s, 0.6 mPa·s, 0.5 mPa·s, 0.4 mPa·s, 0.3 mPa·s, 0.2 mPa·s, or 0.1 mPa·s.
[0065] In some embodiments, the total dielectric constant of the non-aqueous solvent is ≥35, for example 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, 52, 54, 56, 58, 60, 65, 70, 75, 80, 85, 90, 100.
[0066] The testing methods for viscosity and dielectric constant in this application are mainly based on HG / T 4067 (lithium hexafluorophosphate electrolyte) and SJ / T 11568 (electrolyte solvent for lithium-ion batteries).
[0067] As an example: Viscosity test: Using a rotational viscometer (or capillary viscometer), determine the steady-state shear viscosity of non-aqueous solvents (or electrolytes) under isothermal conditions of 25.0℃ ± 0.1℃ (or other specified temperature). Measure each sample three times and take the average value.
[0068] As an example, dielectric constant testing: Using a dielectric constant meter (or a precision LCR meter), measure the capacitance value of the sample at 1 kHz (or other specified frequency) under constant temperature conditions of 25.0℃ ± 0.1℃, and convert it to the relative dielectric constant according to the instrument constant. Measure each sample three times and take the average value.
[0069] The non-aqueous solvent provided in this application has low viscosity and high dielectric constant, and works synergistically with the first additive and lithium salt to better improve the performance of the electrolyte.
[0070] In some embodiments, the concentration of the lithium salt in the modified electrolyte is 0.8 mol / L to 1.5 mol / L, for example, 0.8 mol / L, 0.85 mol / L, 0.9 mol / L, 0.95 mol / L, 1.0 mol / L, 1.05 mol / L, 1.1 mol / L, 1.15 mol / L, 1.2 mol / L, 1.25 mol / L, 1.3 mol / L, 1.35 mol / L, 1.4 mol / L, 1.45 mol / L, or 1.5 mol / L.
[0071] Furthermore, the concentration of the lithium salt in the modified electrolyte is preferably 1.2 mol / L to 1.5 mol / L, such as 1.2 mol / L, 1.25 mol / L, 1.3 mol / L, 1.35 mol / L, 1.4 mol / L, 1.45 mol / L, or 1.5 mol / L.
[0072] This application does not limit the specific types of lithium salts. Any conventional type of lithium salt that can be used in electrolyte systems is applicable, provided it does not depart from the overall technical concept of this application.
[0073] For example, but not limitingly, the lithium salt includes one or more of lithium hexafluorophosphate (LiPF6), lithium bisfluorosulfonylimide (LiFSI), or lithium difluorooxalate borate (LiDFOB), preferably a combination of lithium hexafluorophosphate (LiPF6) and lithium bisfluorosulfonylimide (LiFSI), which improves the battery performance at high rates.
[0074] In the modified electrolyte of this application, compared with the existing electrolyte system, a relatively higher lithium salt concentration can be selected, especially 1.2mol / L~1.5mol / L, which better balances lithium salt dissociation efficiency, hydrolysis stability and cost, and has higher compatibility with the first additive.
[0075] In some embodiments, the modified electrolyte further includes at least one of a second, third, or fourth additive different from the first additive, wherein the second additive is a high-voltage antioxidant, the third additive is a low-impedance additive, and the fourth additive is a film-forming additive.
[0076] In some embodiments, the second additive includes at least one of 1,3-propanesulfonate lactone (PS), vinyl sulfate (DTD), or adiponitrile (ADN).
[0077] In some embodiments, based on a total mass of 100 wt% of the non-aqueous solvent, the lithium salt, and the first additive, the mass of the second additive is 0.1 wt% to 3 wt%, for example, 0.1 wt%, 0.2 wt%, 0.3 wt%, 0.4 wt%, 0.5 wt%, 0.6 wt%, 0.7 wt%, 0.8 wt%, 0.9 wt%, 1.0 wt%, 1.1 wt%, 1.2 wt%, 1.3 wt%, 1.4 wt%, 1.5 wt%, 1.6 wt%, 1.7 wt%, 1.8 wt%, 1.9 wt%, 2.0 wt%, 2.2 wt%, 2.4 wt%, 2.6 wt%, 2.8 wt%, or 3.0 wt%.
[0078] In the modified electrolyte of this application, a second additive can be added in addition to the first additive to synergistically construct a double-layer CEI film. The first additive forms an inner layer of inorganic phase containing S / F, while the second additive, especially PS / DTD, forms a dense outer layer of organic phase, further blocking the oxidative decomposition of the electrolyte under high voltage and inhibiting the dissolution of transition metals, thus achieving the goal of adapting to high voltage systems above 4.6V. Furthermore, adjusting the addition mass of the second additive to 0.1wt%~3wt% enhances the synergistic effect.
[0079] In some embodiments, the third additive includes lithium difluorophosphate (LiPO2F2) and / or lithium tetrafluoroborate (LiBF4).
[0080] In some embodiments, based on a total mass of 100 wt% of the non-aqueous solvent, the lithium salt, and the first additive, the added mass of the third additive is 0.1 wt% to 2 wt%, for example, 0.1 wt%, 0.2 wt%, 0.3 wt%, 0.4 wt%, 0.5 wt%, 0.6 wt%, 0.7 wt%, 0.8 wt%, 0.9 wt%, 1.0 wt%, 1.1 wt%, 1.2 wt%, 1.3 wt%, 1.4 wt%, 1.5 wt%, 1.6 wt%, 1.7 wt%, 1.8 wt%, 1.9 wt%, or 2.0 wt%.
[0081] This application adds a third additive to the modified electrolyte, which plays an auxiliary role. This additive works synergistically with the first additive to promote lithium salt dissociation and further improve the ionic conductivity of the electrolyte. At the same time, it participates in interfacial film formation, further reducing the interfacial impedance of the CEI / SEI film and optimizing the battery rate and low-temperature performance. The addition of 0.1wt% to 2wt% will not affect the normal performance of the modified electrolyte and can greatly promote the improvement of battery performance.
[0082] In some embodiments, the fourth additive includes fluoroethylene carbonate and / or vinylene carbonate.
[0083] In some embodiments, based on a total mass of 100 wt% of the non-aqueous solvent, the lithium salt, and the first additive, the mass of the fourth additive is 0.5 wt% to 8 wt%, for example, 0.5 wt%, 0.6 wt%, 0.7 wt%, 0.8 wt%, 0.9 wt%, 1.0 wt%, 1.2 wt%, 1.4 wt%, 1.6 wt%, 1.8 wt%, 2.0 wt%, 2.5 wt%, 3.0 wt%, 3.5 wt%, 4.0 wt%, 4.5 wt%, 5.0 wt%, 5.5 wt%, 6.0 wt%, 6.5 wt%, 7.0 wt%, 7.5 wt%, or 8.0 wt%.
[0084] This application introduces a fourth additive, which, in addition to its film-forming effect, can also work synergistically with the first additive without significant antagonistic effects. Together, they construct a protective film on both the positive and negative electrode interfaces. The first additive optimizes the positive electrode CEI film, while FEC / VC and other additives form a stable SEI film on the negative electrode, preventing dissolved transition metals from damaging the negative electrode interface. At the same time, it reduces the overall interface impedance and improves cycle stability. The fourth additive is added at a mass of 0.5wt%~8wt%, resulting in a more superior synergistic effect.
[0085] In one embodiment, this application does not specifically limit the preparation method of the modified electrolyte in the above embodiments. Without violating the overall technical concept of this application, conventionally applicable preparation methods for electrolytes are all applicable to this application.
[0086] For example, but not in a limiting sense, this application provides a method for preparing the modified electrolyte described in the above embodiments, the preparation method comprising:
[0087] According to a preset ratio, in a protective atmosphere with a water and oxygen content of <1ppm, an organic solvent is mixed, and then a lithium salt is added to obtain a basic electrolyte. Then, a first additive and optional high-voltage antioxidant additive and / or optional low-impedance additive and / or optional film-forming additive are added to the basic electrolyte according to a preset ratio. After dissolution and mixing, the modified electrolyte is obtained.
[0088] Optionally, the protective atmosphere includes a nitrogen atmosphere, an argon atmosphere, or a helium atmosphere, etc.
[0089] In one embodiment, this application also provides a battery comprising the modified electrolyte as described in the above embodiments.
[0090] The modified electrolyte provided in this application is suitable for battery systems with operating voltages ≥4.4V (e.g., 4.4V, 4.45V, 4.5V, 4.55V, 4.6V, 4.65V, or 4.7V, etc.). It effectively solves problems such as oxidative decomposition of electrolytes at high voltages, poor lithium salt dissociation, poor solvation, and difficulty in meeting film formation requirements, thereby improving the electrochemical performance of batteries at high voltages and high rates.
[0091] It should be noted that the battery operating voltage ≥4.4V in this application refers to the battery charging cut-off voltage not being lower than 4.4V.
[0092] Apart from the modified electrolyte specified in this application, the other raw materials and preparation processes in the battery provided in this application are all conventional technical solutions, which can be adapted and adjusted by those skilled in the art according to actual needs.
[0093] In some embodiments, the lithium-ion battery includes a positive electrode, a negative electrode, a separator, and an electrolyte.
[0094] This application does not impose any particular limitation on the positive electrode, as long as it achieves the purpose of this application. In some embodiments, the positive electrode sheet includes a positive current collector and a positive active material layer. The positive active material layer is disposed on one or both surfaces of the positive current collector. The aforementioned "surface" can be a portion of the surface of the positive current collector or the entire surface of the positive current collector. This application does not impose any particular limitation on the positive current collector, as long as it achieves the purpose of this application. For example, the positive current collector can contain aluminum foil or aluminum alloy foil, etc. The positive active material layer of this application contains a positive active material. This application does not impose any particular limitation on the type of positive active material, as long as it achieves the purpose of this application. For example, the positive active material can contain at least one of lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate, lithium-rich manganese-based materials, lithium cobalt oxide, lithium manganese oxide, lithium manganese iron phosphate, or lithium titanate, etc. In this application, the positive active material can also contain non-metallic elements, which can include at least one of fluorine, phosphorus, boron, chlorine, silicon, or sulfur. These elements can further improve the stability of the positive active material. In this application, there are no particular limitations on the thickness of the positive electrode current collector and the positive electrode active material layer, as long as the purpose of this application can be achieved. For example, the thickness of the positive electrode current collector is 5 μm to 20 μm. The thickness of the single-layer positive electrode active material layer is 30 μm to 120 μm. Optionally, the positive electrode active material layer may also include at least one of a conductive agent or a binder. This application does not particularly limit the types of conductive agents and binders in the positive electrode active material layer, as long as the purpose of this application can be achieved. This application does not particularly limit the mass ratio of the positive electrode active material, conductive agent, and binder in the positive electrode active material layer; those skilled in the art can choose according to actual needs, as long as the purpose of this application can be achieved.
[0095] In some embodiments, the positive electrode active material accounts for 85wt% to 98wt% of the mass of the positive electrode active material layer, for example, 80wt%, 81wt%, 82wt%, 83wt%, 84wt%, 85wt%, 86wt%, 87wt%, 88wt%, 89wt%, 90wt%, 91wt%, 92wt%, 93wt%, 94wt%, 95wt%, 96wt%, 97wt%, or 98wt%.
[0096] The separator of this application is disposed between the positive electrode and the negative electrode to separate them. This application does not impose any particular limitation on the separator, as long as it achieves the purpose of this application. For example, the separator material may include, but is not limited to, at least one of polyethylene (PE), polyolefins (PO) primarily composed of polypropylene (PP), polyester (e.g., polyethylene terephthalate (PET) film), cellulose, polyimide (PI), polyamide (PA), spandex, or aramid. The separator type may include at least one of woven membrane, nonwoven membrane, microporous membrane, composite membrane, rolled membrane, or spun membrane. This application does not impose any particular limitation on the separator thickness, as long as it achieves the purpose of this application.
[0097] This application does not impose any particular limitation on the negative electrode, as long as the purpose of this application can be achieved. In some embodiments, the negative electrode includes a negative electrode current collector and a negative electrode active material layer, the negative electrode active material layer being disposed on one or both surfaces of the negative electrode current collector. The aforementioned "surface" can be a portion of the surface of the negative electrode current collector or the entire surface of the negative electrode current collector. For example, the negative electrode current collector may contain copper foil or copper alloy foil, etc. The negative electrode active material layer of this application contains a negative electrode active material. The negative electrode active material includes at least one of artificial graphite, natural graphite, soft carbon, hard carbon, mesophase microcarbon spheres, silicon-based materials, and tin-based materials. Optionally, the negative electrode active material layer may also include at least one of conductive agent or binder. This application does not impose any particular limitation on the types of conductive agent and binder in the negative electrode active material layer, as long as the purpose of this application can be achieved. This application does not impose any particular limitation on the mass ratio of negative electrode active material, conductive agent, and binder in the negative electrode active material layer; those skilled in the art can choose according to actual needs, as long as the purpose of this application can be achieved.
[0098] In some embodiments, the negative electrode active material accounts for 80wt% to 98wt% of the mass of the negative electrode active material layer, for example, 80wt%, 81wt%, 82wt%, 83wt%, 84wt%, 85wt%, 86wt%, 87wt%, 88wt%, 89wt%, 90wt%, 91wt%, 92wt%, 93wt%, 94wt%, 95wt%, 96wt%, 97wt%, or 98wt%.
[0099] In some embodiments, the negative electrode active material includes at least a silicon-based material; the electrolyte provided in this application better solves the problem of volume expansion of silicon-based materials; this application does not have any particular limitation on the specific substance of the silicon-based material, and those skilled in the art can choose according to actual needs, as long as the purpose of this application can be achieved.
[0100] In some embodiments, the silicon-based material includes at least one of silicon-carbon materials, silicon-oxygen materials, nano-silicon materials, porous silicon materials, or silicon alloy materials; the silicon content in the silicon-based material is ≥5 wt%.
[0101] As an example, the silicon-carbon material includes a composite material formed by embedding nano-silicon particles in a carbon matrix, wherein the carbon matrix includes, but is not limited to, at least one of porous carbon, graphite, hard carbon, soft carbon, or mesophase carbon microspheres; the silicon mass percentage in the silicon-carbon material is 5wt% to 50wt%, for example, 5wt%, 10wt%, 15wt%, 20wt%, 25wt%, 30wt%, 35wt%, 40wt%, 45wt%, or 50wt%.
[0102] As an example, the general chemical formula of the silicon-oxygen material is SiOx, where 0 < x < 2, such as 0.3, 0.5, 1, 1.5 or 1.8, etc.; the mass percentage of silicon in the silicon-oxygen material is 30wt% to 70wt%, such as 30wt%, 35wt%, 40wt%, 45wt%, 50wt%, 55wt%, 60wt%, 65wt% or 70wt%, etc.
[0103] As an example, the particle size range of the nano-silicon material is 10nm to 500nm, such as 10nm, 50nm, 100nm, 150nm, 200nm, 250nm, 300nm, 350nm, 400nm, 450nm or 500nm, etc.
[0104] As an example, the silicon alloy material includes an alloy material formed of silicon and metal M, wherein the metal M includes, but is not limited to, at least one of Fe, Al, Sn, Mg or Ti; the mass percentage of silicon in the silicon alloy material is 20wt% to 80wt%, for example, 30wt%, 35wt%, 40wt%, 45wt%, 50wt%, 55wt%, 60wt%, 65wt%, 70wt%, 75wt% or 80wt%, etc.
[0105] In some embodiments, the negative electrode active material includes a silicon-based material, and the silicon-based material accounts for 80wt% to 95wt% of the mass of the negative electrode active material layer, for example, 80wt%, 81wt%, 82wt%, 83wt%, 84wt%, 85wt%, 86wt%, 87wt%, 88wt%, 89wt%, 90wt%, 91wt%, 92wt%, 93wt%, or 94wt%, 95wt%, etc.
[0106] Furthermore, whether it is the conductive agent and binder of the positive electrode or the conductive agent and binder of the negative electrode, the conductive agent includes, but is not limited to, conductive carbon black and carbon nanotubes; the binder includes at least one of polytetrafluoroethylene, sodium carboxymethyl cellulose, styrene-butadiene rubber, polyvinylidene fluoride, nitrile rubber, styrene-ethylene-butene-styrene copolymer, styrene-butadiene-styrene copolymer, lithium polyacrylate, sodium polyacrylate, sodium alginate or lithium alginate; the conductive agent includes at least one of acetylene black, Ketjen black, Super-P, carbon nanotubes, carbon fibers or graphene.
[0107] In some embodiments, in addition to the positive electrode, separator, electrolyte, and negative electrode described above, the lithium-ion battery also includes a casing. The casing houses the positive electrode, negative electrode, separator, electrolyte, and other components known in batteries, which are not limited in this application. This application does not impose any particular limitation on the casing; it can be any casing known in the art, as long as it achieves the purpose of this application.
[0108] In some embodiments, this application provides an electrical device that includes a battery as described in the above embodiments.
[0109] The numerical range described in this application includes not only the point values listed above, but also any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of brevity, this application will not exhaustively list the specific point values included in the range.
[0110] Example 1
[0111] This embodiment provides an electrolyte comprising a non-aqueous solvent, a lithium salt, and a first additive; the non-aqueous solvent is a carbonate organic solvent with a mass ratio of EC:EMC:DMC of 30:40:30.
[0112] The lithium salt is LiPF6, and the first additive is methyl 5-oxo-7-(((trifluoromethyl)sulfonyl)oxy)-1,2,3,5-tetrahydro-indene-3-carboxylic acid (CAS No.: 1956310-54-5).
[0113] In the electrolyte, the first additive accounts for 1 wt% of the total mass of the electrolyte, and the organic solvent accounts for 85 wt% of the total mass of the electrolyte; the concentration of the lithium salt in the electrolyte is 1.2 mol / L.
[0114] The method for preparing the electrolyte includes:
[0115] In a glove box with an argon atmosphere containing less than 1 ppm of water and oxygen, carbonate organic solvents are mixed in a predetermined ratio and stirred at room temperature for 40 minutes until completely homogeneous to obtain an organic solvent mixture system.
[0116] The lithium salt was slowly added to the above organic solvent mixture and stirred continuously for 50 minutes until completely dissolved to obtain the basic electrolyte.
[0117] The first additive, methyl 5-oxo-7-(((trifluoromethyl)sulfonyl)oxy)-1,2,3,5-tetrahydroindene-3-carboxylic acid (CAS No.: 1956310-54-5), was added to the basic electrolyte at a predetermined ratio and stirred at room temperature for 35 minutes until completely dissolved to obtain the electrolyte.
[0118] Example 2
[0119] This embodiment provides an electrolyte comprising a non-aqueous solvent, a lithium salt, and a first additive; the non-aqueous solvent is a carbonate organic solvent with a mass ratio of EC:EMC:DMC of 30:40:30.
[0120] The lithium salt is LiPF6 and LiFSI, and the first additive is 5-oxo-7-(((trifluoromethyl)sulfonyl)oxy)-1,2,3,5-tetrahydro-nitrogen indene-3-carboxylic acid methyl ester (CAS No.: 1956310-54-5).
[0121] In the electrolyte, the first additive accounts for 1 wt% of the total mass of the electrolyte, and the organic solvent accounts for 90 wt% of the total mass of the electrolyte; the concentration of the lithium salt in the electrolyte is 1.2 mol / L, of which LiPF6 is 1 mol / L and LiFSI is 0.2 mol / L.
[0122] The method for preparing the electrolyte includes:
[0123] In a glove box with an argon atmosphere containing less than 1 ppm of water and oxygen, carbonate organic solvents are mixed in a predetermined ratio and stirred at room temperature for 40 minutes until completely homogeneous to obtain an organic solvent mixture system.
[0124] The lithium salt was slowly added to the above organic solvent mixture and stirred continuously for 50 minutes until completely dissolved to obtain the basic electrolyte.
[0125] The first additive, methyl 5-oxo-7-(((trifluoromethyl)sulfonyl)oxy)-1,2,3,5-tetrahydroindene-3-carboxylic acid (CAS No.: 1956310-54-5), was added to the basic electrolyte at a predetermined ratio and stirred at room temperature for 35 minutes until completely dissolved to obtain the electrolyte.
[0126] Example 3
[0127] The difference between this embodiment and Embodiment 1 is that in this embodiment, the mass percentage of the first additive is 0.2 wt% of the total mass of the electrolyte, and the corresponding mass percentage of the non-aqueous solvent is 85.8 wt%.
[0128] All other conditions remain the same as in Example 1.
[0129] Example 4
[0130] The difference between this embodiment and Embodiment 1 is that in this embodiment, the mass percentage of the first additive is 1.5 wt% of the total mass of the electrolyte, and the corresponding mass percentage of the non-aqueous solvent is 84.5 wt%.
[0131] All other conditions remain the same as in Example 1.
[0132] Example 5
[0133] The difference between this embodiment and Embodiment 1 is that in this embodiment, the mass percentage of the first additive is 3 wt% of the total mass of the electrolyte, and the corresponding mass percentage of the non-aqueous solvent is 83 wt%.
[0134] All other conditions remain the same as in Example 1.
[0135] Example 6
[0136] The difference between this embodiment and Embodiment 1 is that in this embodiment, the mass percentage of the first additive is 0.05 wt% of the total mass of the electrolyte, and the corresponding mass percentage of the non-aqueous solvent is 85.95 wt%.
[0137] All other conditions remain the same as in Example 1.
[0138] Example 7
[0139] The difference between this embodiment and Embodiment 1 is that in this embodiment, the mass percentage of the first additive is 5 wt% of the total mass of the electrolyte, and the corresponding mass percentage of the non-aqueous solvent is 81 wt%.
[0140] All other conditions remain the same as in Example 1.
[0141] Example 8
[0142] The difference between this embodiment and Embodiment 1 is that the first additive in this embodiment has the following structural formula, namely, non-7-position substitution:
[0143] .
[0144] All other conditions remain the same as in Example 1.
[0145] Example 9
[0146] The difference between this embodiment and Example 1 is that the first additive in this embodiment has the following structural formula, that is, it is not an oxo-substituted, but an alkenyl-substituted:
[0147] .
[0148] All other conditions remain the same as in Example 1.
[0149] Example 10
[0150] The difference between this embodiment and Example 1 is that the first additive in this embodiment has the following structural formula, namely, trichloromethyl:
[0151] .
[0152] All other conditions remain the same as in Example 1.
[0153] Example 11
[0154] The difference between this embodiment and Embodiment 1 is that the non-aqueous solvent in this embodiment also includes the ether solvent DME (dimethyl ether), and the mass ratio of the ether solvent to the carbonate solvent is 30:70.
[0155] All other conditions remain the same as in Example 1.
[0156] Example 12
[0157] The difference between this embodiment and Embodiment 1 is that the concentration of lithium salt in this embodiment is 1 mol / L.
[0158] All other conditions remain the same as in Example 1.
[0159] Comparative Example 1
[0160] The difference between this comparative example and Example 1 is that the electrolyte in this comparative example is the basic electrolyte.
[0161] All other conditions remain the same as in Example 1.
[0162] Comparative Example 2
[0163] The difference between this comparative example and Example 1 is that the first additive in this comparative example is methyl 7-hydroxy-5-oxo-1,2,3,5-tetrahydroindene-3-carboxylate (… CAS No.: 2197422-77-6.
[0164] All other conditions remain the same as in Example 1.
[0165] Comparative Example 3
[0166] The difference between this comparative example and Example 1 is that the first additive in this comparative example is methyl 5-oxo-7-((methanesulfonyl)oxy)-1,2,3,5-tetrahydro-indene-3-carboxylic acid, with the following structural formula:
[0167] .
[0168] All other conditions remain the same as in Example 1.
[0169] Comparative Example 4
[0170] The difference between this comparative example and Example 1 is that it contains 5-oxo-7-(((trifluoromethyl)sulfonyl)oxy)-1,2,3,5-tetrahydro-nitrogen indene, with the structural formula shown below:
[0171] .
[0172] All other conditions remain the same as in Example 1.
[0173] Comparative Example 5
[0174] The difference between this comparative example and Example 1 is that the first additive in this comparative example is methyl 3-(trifluoromethylsulfonyloxy)-2-naphthoic acid ester ( CAS No.: 288402-18-6.
[0175] All other conditions remain the same as in Example 1.
[0176] Application Example 1
[0177] This application example provides a lithium-ion battery, which includes a positive electrode, a negative electrode, a separator, and the electrolyte provided in Example 1.
[0178] The method for preparing the lithium-ion battery includes:
[0179] Preparation of positive electrode sheet
[0180] Ternary material NCM (LiNi) 0.8 Co 0.1 Mn 0.1 O2) positive electrode active material, binder PVDF (polyvinylidene fluoride), conductive agent SP (conductive carbon black Super-P) are mixed at a mass ratio of 96:1.8:2.2, and N-methylpyrrolidone (NMP) is added. The mixture is stirred evenly to obtain a positive electrode slurry with a solid content of 65%. The positive electrode slurry is then coated onto aluminum foil through a coating process, and after drying and cold pressing, a positive electrode sheet is obtained.
[0181] (2) Preparation of negative electrode sheet
[0182] Silicon-carbon anode material (silicon content of 10 wt%), conductive agent SP (Super-P conductive carbon black), SWCNT (single-walled carbon nanotubes), and binder PAA (polyacrylic acid) are mixed in a mass ratio of 83.5:8:0.5:8, and deionized water is added. The mixture is stirred evenly to obtain an anode slurry with a solid content of 30%. The solid content is controlled at 30%. The anode slurry is then coated onto a copper foil current collector through a coating process. After vacuum drying and cold pressing, the anode sheet is obtained.
[0183] (3) Selection of electrolyte
[0184] The electrolyte provided in Example 1.
[0185] (4) Selection of separator membrane
[0186] Polyethylene (PE) + ceramic was chosen as the separator for lithium-ion batteries.
[0187] (5) Preparation of lithium-ion batteries
[0188] The positive electrode, separator, and negative electrode are stacked in sequence, with the separator positioned between the positive and negative electrodes to provide isolation, resulting in a bare cell. The bare cell is then placed in an outer packaging shell, dried, and injected with electrolyte. After vacuum sealing, settling, formation, and shaping, a lithium-ion battery is obtained.
[0189] Application Example 2-12 and Comparison Application Example 1-5
[0190] The difference between Application Examples 2-12 and Comparative Application Examples 1 and Application Example 2-12 is that the electrolytes provided in Examples 2-12 and Comparative Examples 1-5 are used respectively.
[0191] All other conditions remain the same as in Application Example 1.
[0192] Performance testing
[0193] The performance of the lithium-ion battery provided in the above application example was then compared with that of the application example. The test conditions were as follows: the rate performance of the battery was tested under the test conditions of a soft-pack battery, and the test was conducted at room temperature (25°C) on the LAND battery test system of Wuhan Jinno Electronics Co., Ltd. The charge and discharge voltage was limited to 2.5V~4.4V.
[0194] (1) Capacity retention rate after 1000 cycles at room temperature 1C / 1C
[0195] At 25°C, the lithium-ion battery was charged at a constant current and constant voltage of 1C to 4.2V, with a cutoff current of 0.05C. After resting for 10 minutes, the lithium-ion battery was discharged at a constant current of 1C to 2.5V and then rested for 10 minutes. This constitutes one charge-discharge cycle. The lithium-ion battery was subjected to 1000 charge-discharge cycles using the above method. The capacity retention rate of the lithium-ion battery after 1000 charge-discharge cycles at 1C / 1C was calculated.
[0196] The capacity retention rate (%) of a lithium-ion battery after N cycles = (discharge capacity of the Nth cycle / initial discharge capacity) × 100%, where N is the number of cycles of the lithium-ion battery.
[0197] (2) (5) Capacity retention rate at room temperature 1C / 10C discharge
[0198] The lithium-ion battery, after capacity gradation, was charged at 25℃ using a 1C rate with constant current and constant voltage to 4.2V, with a cutoff current of 0.05C; it was then allowed to stand for 10 minutes; next, the lithium-ion battery was discharged at a 1C rate with constant current to 2.5V, and its discharge capacity Q1C was recorded as the initial discharge capacity; then, the lithium-ion battery was charged at 25℃ using a 1C rate with constant current and constant voltage to 4.2V, with a cutoff current of 0.05C; it was allowed to stand for 10 minutes; then, the fully charged battery was discharged at a 10C rate with constant current to 2.5V, and its discharge capacity Q10C was recorded; the discharge capacity retention rate (%) of the lithium-ion battery at 1C / 10C rate was calculated as: discharge capacity Q10C at 10C rate / discharge capacity Q1C at 1C rate × 100%.
[0199] (3) High-temperature storage performance at 60℃
[0200] ① Standard charge and discharge: At 25℃, charge the lithium-ion battery at a constant current and constant voltage rate of 0.33C to 4.2V, let it stand for 10 minutes, then discharge the lithium-ion battery at a constant current rate of 0.33C to 2.5V, and let it stand for 10 minutes.
[0201] ② Initial performance test: The sample battery performance was tested using battery testing equipment at room temperature (25℃). Three standard charge-discharge cycles at 0.33C were performed, and the capacity after the third discharge was recorded. The initial capacity C0 was stored.
[0202] ③ High-temperature storage: At room temperature (25℃), the lithium-ion battery was charged to 4.2V at a constant current and constant voltage rate of 0.33C, left to stand for 30 minutes, and the cell thickness t1 was measured; then the cell was placed in a 60℃ oven for high-temperature storage for 7 days.
[0203] ④ Post-storage performance test: After the storage time is reached, the battery is removed from the high-temperature test chamber and left at room temperature for 2-4 hours to allow the battery temperature to return to room temperature. The cell thickness is measured and recorded as t2. The lithium-ion battery is then discharged at a constant current rate of 0.33C to 2.5V and left to stand for 10 minutes. The discharge capacity is the retention capacity C1. The battery is then subjected to 3 standard charge-discharge cycles at 0.33C, and the capacity of the third discharge is recorded as C2 after storage. The capacity recovery rate after 7 days of storage at 60℃ is calculated as C2 / C0×100%.
[0204] (4) Cell thermal runaway ARC test
[0205] Begin the ARC adiabatic thermal runaway test (the test sample is heated from room temperature to 45±2℃ in the chamber, and after resting for 90 minutes, the change in battery temperature rise rate is detected. If the temperature rise exceeds 0.2℃ within 10 minutes (i.e., SHR>0.02℃ / min), it is considered that a self-heating reaction has occurred inside the battery. Maintain the adiabatic environment until the battery experiences thermal runaway; if the temperature rise does not exceed 0.2℃ within 10 minutes (i.e., SHR≤0.02℃ / min), continue to the next step temperature rise test; each temperature step is 5℃, and the steps are repeated on each step. The ARC test temperature range is 45℃~300℃, the self-heating start temperature is T1 (temperature rise rate SHR>0.02℃ / min), and the thermal runaway start temperature is T2 (temperature rise rate SHR>1℃ / min). Note: Self-heating rate (SHR).
[0206] The test results are shown in Table 1.
[0207] Table 1
[0208]
[0209]
[0210] From Table 1, we can obtain:
[0211] The electrolyte provided in this application, under the action of the first additive, simultaneously promotes lithium salt dissociation, protects the high-voltage interface, optimizes the solvation structure, and reduces the interfacial impedance, thereby improving the electrochemical performance of the corresponding battery under high voltage and high rate conditions.
[0212] Data analysis of Examples 1 and 3-7 shows that the mass percentage of the first additive directly affects its effectiveness. When adjusted to 0.05wt%~3wt%, the effect of the first additive in the modified electrolyte is more significant. More preferably, it is 0.2wt%~1.5wt%, which will not affect the viscosity of the electrolyte itself, thus avoiding excessive viscosity that would limit the use of the electrolyte, and can also give full play to the synergistic effect of various groups and linkage sites, greatly improving the high voltage stability, long cycle performance, rate performance and thermal stability of the battery.
[0213] Data analysis of Examples 1 and 8-10 shows that the site occupancy relationship between groups is crucial in the first additive of this application. Using an unsaturated nitrogen-indene group as the parent nucleus, OSO2R2 is confined to position 7, COOR1 to position 3, and an oxocarbonyl group at position 5, a superior site occupancy combination is formed, which has more prominent advantages. Furthermore, the use of fluorine atoms as the halogen atom of R2 significantly broadens the electrochemical window of the electrolyte compared to other halogen atoms, improves the antioxidant effect, and can further enhance lithium salt dissociation and ionic conductivity, strengthen thermal stability, and optimize electrode interface film formation, thereby improving the overall cycle life and safety of high-voltage batteries.
[0214] Data analysis of Examples 1 and 11-12 shows that using carbonate-based organic solvents as non-aqueous solvents results in higher compatibility with the first additive and can balance lithium salt dissociation and ion transport effects, achieving precise control of the solvation structure. Compared with existing electrolyte systems, relatively higher lithium salt concentrations can be selected, especially 1.2 mol / L to 1.5 mol / L, which better balances lithium salt dissociation efficiency, hydrolysis stability, and cost, and has higher compatibility with the first additive.
[0215] Analysis of the data from Example 1 and Comparative Examples 1-5 shows that in the modified electrolyte of this application, the haloalkyl sulfonate group, carboxylic acid alkyl group and unsaturated nitrogen-indene heterocyclic group are the core functional units. They are all indispensable and must work together to simultaneously achieve the integration of four core functions: promoting lithium salt dissociation, high-voltage interface film formation, solvation structure regulation, and reducing interface impedance, and also achieve the effect of flame retardancy.
[0216] Example 13
[0217] The difference between this embodiment and Embodiment 1 is that a second additive is added to the electrolyte in this embodiment. The second additive is PS and DTD in a mass ratio of 1:1. Based on the total mass of the non-aqueous solvent, the lithium salt and the first additive being 100wt%, the mass of the second additive added is 3wt%.
[0218] All other conditions remain the same as in Example 1.
[0219] Example 14
[0220] The difference between this embodiment and Embodiment 1 is that a third additive, lithium difluorophosphate (LiPO2F2), is added to the electrolyte in this embodiment; based on the total mass of the non-aqueous solvent, the lithium salt, and the first additive being 100wt%, the added mass of the third additive is 2wt%.
[0221] All other conditions remain the same as in Example 1.
[0222] Example 15
[0223] The difference between this embodiment and Embodiment 1 is that a fourth additive is added to the electrolyte in this embodiment. The fourth additive is FEC and VC in a mass ratio of 1:1. Based on the total mass of the non-aqueous solvent, the lithium salt and the first additive being 100wt%, the mass of the fourth additive added is 5wt%.
[0224] All other conditions remain the same as in Example 1.
[0225] Application Example 13-15
[0226] The difference between Application Examples 13-15 and Application Example 1 is that the electrolytes provided in Examples 13-15 are used respectively.
[0227] All other conditions remain the same as in Application Example 1.
[0228] Application Examples 13-15 were tested under the exact same conditions as Application Example 1. The test results are shown in Table 2.
[0229] Table 2
[0230]
[0231] From Table 2, we can obtain:
[0232] The modified electrolyte of this application can be compounded with a second and / or a third and / or a fourth additive on the basis of the first additive. Not only will it not produce antagonistic effects, but it also has excellent synergistic effects.
[0233] The above description is only a specific embodiment of this application, but the protection scope of this application is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in this application fall within the protection and disclosure scope of this application.
Claims
1. A modified electrolyte, characterized in that, The modified electrolyte comprises a non-aqueous solvent, a lithium salt, and a first additive, wherein the first additive has the following structure: COOR1-Ar-OSO2R2; Wherein, R1 is selected from C1-C4 straight-chain or branched alkyl groups, Ar is selected from unsaturated nitrogen-containing indene groups, and R2 is selected from C1-C4 fully haloalkyl groups.
2. The modified electrolyte according to claim 1, characterized in that, The unsaturated nitrogen-indene group is selected from 5-oxo-1,2,3,5-tetrahydro-nitrogen-indene; And / or, the COOR1 is attached to the 3-position of the nitrogen-indene group in the unsaturated nitrogen; And / or, the OSO2R2 is attached to the 7-position of the unsaturated nitrogen indene group; And / or, the R2 is selected from C1-C4 perfluoroalkyl groups.
3. The modified electrolyte according to claim 2, characterized in that, The first additive has the formula To the style At least one of the following structural formulas: 。 4. The modified electrolyte according to claim 1, characterized in that, Based on a total mass of 100 wt% for the non-aqueous solvent, the lithium salt, and the first additive, the mass percentage of the first additive is 0.05 wt% to 3 wt%. And / or, based on a total mass of 100 wt% of the non-aqueous solvent, the lithium salt, and the first additive, the mass percentage of the non-aqueous solvent is 80 wt% to 90 wt%; And / or, the non-aqueous solvent includes carbonate organic solvents; And / or, the total viscosity of the non-aqueous solvent is ≤1.8 mPa·s, and the total dielectric constant of the non-aqueous solvent is ≥35; And / or, the concentration of the lithium salt in the modified electrolyte is 0.8 mol / L to 1.5 mol / L.
5. The modified electrolyte according to claim 4, characterized in that, Based on a total mass of 100 wt% for the non-aqueous solvent, the lithium salt, and the first additive, the mass percentage of the first additive is 0.2 wt% to 1.5 wt%. And / or, the concentration of the lithium salt in the modified electrolyte is 1.2 mol / L to 1.5 mol / L.
6. The modified electrolyte according to claim 1, characterized in that, The modified electrolyte also includes at least one of a second, third, or fourth additive, which is different from the first additive. The second additive is a high-voltage antioxidant, the third additive is a low-impedance additive, and the fourth additive is a film-forming additive.
7. The modified electrolyte according to claim 6, characterized in that, The second additive includes at least one of 1,3-propanesulfonate lactone, vinyl sulfate, or adiponitrile; And / or, the third additive includes lithium difluorophosphate and / or lithium tetrafluoroborate; And / or, the fourth additive includes fluoroethylene carbonate and / or vinylene carbonate.
8. The modified electrolyte according to claim 6 or 7, characterized in that, Based on a total mass of 100 wt% for the non-aqueous solvent, the lithium salt, and the first additive, the mass of the second additive added is 0.1 wt% to 3 wt%. And / or, based on a total mass of 100 wt% for the non-aqueous solvent, the lithium salt, and the first additive, the added mass of the third additive is 0.1 wt% to 2 wt%; And / or, based on a total mass of 100wt% of the non-aqueous solvent, the lithium salt, and the first additive, the mass of the fourth additive is 0.5wt% to 8wt%.
9. A battery, characterized in that, The battery comprises the modified electrolyte as described in any one of claims 1-8.
10. An electrical device, characterized in that, The electrical device includes the battery as described in claim 9.