Method and device for stripping an electrode tab
By combining microwave radiation treatment with an auxiliary separation medium, low-energy and environmentally friendly separation of lithium-ion battery electrodes is achieved, solving the problems of current collector damage and high energy consumption in existing technologies, and improving separation efficiency and product purity.
Patent Information
- Application Number
- CN202611433809.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-15
- Publication Date
- 2026-11-24
AI Technical Summary
In the current lithium-ion battery electrode recycling process, mechanical stripping causes damage to the current collector and contamination of the active material; high-temperature pyrolysis consumes a lot of energy and generates toxic gases; and chemical solvent methods are costly and difficult to recycle, making it difficult to achieve efficient and environmentally friendly electrode separation.
Microwave radiation treatment combined with an auxiliary separation medium is used. The electrode and the auxiliary separation medium are mixed in an inert atmosphere, and after microwave radiation treatment, solid-liquid separation and flexible peeling are performed to separate the current collector and the active material.
It achieves low-energy and environmentally friendly electrode separation, with high separation rate of current collector and active material, high product purity, energy consumption reduction of more than 80%, no toxic fumes, and recyclable medium, and is suitable for a variety of electrode systems.
Smart Images

Figure CN123162371A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of electrochemical technology, and in particular to a method and apparatus for stripping an electrode. Background Technology
[0002] Lithium-ion batteries, as the core of modern energy storage technology, are widely used in new energy vehicles, consumer electronics, and energy storage systems. With the rapid expansion of the global electric vehicle market and the upgrading of consumer electronics products, the volume of retired lithium-ion batteries is growing exponentially. Waste batteries contain high-value current collectors such as aluminum and copper foil, as well as active materials such as lithium iron phosphate, ternary materials, lithium cobalt oxide, and graphite. Their recycling is of great significance for alleviating resource shortages and reducing environmental pollution. However, in traditional recycling processes, the efficient stripping of the electrodes (composed of current collectors and active layers) remains a key bottleneck.
[0003] In existing technologies, mechanical stripping can easily lead to damage to the current collector and contamination of the active material; high-temperature pyrolysis requires a temperature of 400-700℃, which consumes a lot of energy and produces toxic gases; chemical solvent methods rely on a large amount of organic solvents, which are costly and difficult to recycle.
[0004] Therefore, there is an urgent need to develop a low-energy-consumption and environmentally friendly electrode stripping technology to meet the needs of large-scale recycling and promote the closed-loop recycling of lithium-ion battery materials. Summary of the Invention
[0005] This application provides a method and apparatus for peeling off an electrode sheet. This peeling method can separate the current collector and active material in the electrode sheet with low energy consumption and in an environmentally friendly manner, and is suitable for widespread application.
[0006] This application provides a method for peeling off an electrode, comprising:
[0007] After mixing the electrode with the auxiliary separation medium, microwave radiation treatment was carried out under an inert atmosphere to obtain a solid-liquid mixture.
[0008] The solid-liquid mixture is subjected to solid-liquid separation treatment to obtain a solid product;
[0009] The solid product is subjected to a flexible exfoliation process to obtain a current collector and an active material.
[0010] In the stripping method described above, the electrode is a positive electrode, the current collector is an aluminum foil, and the active material includes at least one of lithium iron phosphate, lithium cobalt oxide, and ternary positive electrode materials.
[0011] In the stripping method described above, the auxiliary separation medium includes an alkaline aqueous solution and a reducing agent, wherein the mass percentage of the reducing agent in the auxiliary separation medium is 2%-8%, and the reducing agent includes sodium sulfite and / or sodium dithionite;
[0012] The mass-to-volume ratio of the positive electrode to the auxiliary separation medium is 1:(10-30)g / mL;
[0013] And / or, in the microwave radiation treatment, the power is 400W-800W, the temperature is 180℃-260℃, and the time is 15min-40min.
[0014] In the stripping method described above, the electrode is a negative electrode, the current collector is copper foil, and the active material includes graphite.
[0015] In the stripping method described above, the auxiliary separation medium includes an organic solvent and an additive, wherein the additive has a mass percentage of 1%-5% in the auxiliary separation medium; the organic solvent includes N-methylpyrrolidone and / or dimethyl carbonate; and the additive includes lithium carbonate and / or lithium chloride.
[0016] The mass-to-volume ratio of the negative electrode to the auxiliary separation medium is 1:(15-40)g / mL;
[0017] And / or, in the microwave radiation treatment, the power is 300W-600W, the temperature is 120℃-200℃, and the time is 10min-30min.
[0018] The stripping method described above further includes drying the solid product after the solid-liquid separation process.
[0019] In the drying process, the temperature is 60℃-80℃ and the time is 2h-4h.
[0020] The peeling method described above, wherein the flexible peeling process includes impacting the solid product with an airflow of 15 m / s to 25 m / s; and / or,
[0021] The flow rate of the inert atmosphere is 0.5 L / min to 2 L / min.
[0022] The stripping method described above further includes a post-processing step after the flexible stripping treatment, which includes sieving and / or magnetic separation, wherein the sieving process has a mesh size of 100-200 mesh.
[0023] In the peeling method described above, the length of the first side of the electrode is 50mm-100mm, the length of the second side of the electrode is 50mm-100mm, and the first side and the second side are perpendicular to each other; and / or,
[0024] It also includes disassembling the battery after discharging it to a voltage of ≤1.5V to obtain the electrode sheet.
[0025] This application also provides an apparatus for implementing the electrode stripping method described above, comprising: an inert atmosphere channel, a microwave radiation unit, a solid-liquid separation unit, and a flexible stripping unit.
[0026] The inert atmosphere channel is connected to the inlet of the microwave radiation unit. The electrode and the auxiliary separation medium are located in the microwave radiation unit. The outlet of the microwave radiation unit is connected to the inlet of the solid-liquid separation unit. The solid outlet of the solid-liquid separation unit is connected to the inlet of the flexible stripping unit. The flexible stripping unit has a current collector outlet and an active material outlet.
[0027] This application involves mixing the electrode with an auxiliary separation medium and then subjecting it to microwave radiation treatment under an inert atmosphere. The resulting solid-liquid mixture is then subjected to solid-liquid separation treatment, followed by flexible peeling treatment of the solid product. This process promotes effective separation between the current collector and the active material in the electrode, reduces residue on the current collector surface, and improves the recovery purity of the active material. Consequently, it enhances the adaptability, separation efficiency, stability of the recovery process, and resource utilization of the electrode. Attached Figure Description
[0028] The accompanying drawings, which are incorporated in and form part of this specification, illustrate embodiments consistent with this application and, together with the description, serve to explain the principles of this application.
[0029] Figure 1 This is a process flow diagram of the stripping method in some embodiments of this application;
[0030] Figure 2 This is a process flow diagram of microwave radiation treatment in some embodiments of this application. Detailed Implementation
[0031] Exemplary embodiments will now be described in detail, examples of which are illustrated in the accompanying drawings. When the following description relates to the drawings, unless otherwise indicated, the same numbers in different drawings denote the same or similar elements. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with this application. Rather, they are merely examples of apparatuses and methods consistent with some aspects of this application as detailed in the appended claims.
[0032] Lithium-ion battery recycling falls under the field of battery resource regeneration technology, primarily targeting the separation and recycling of electrode sheets after the retirement of power batteries for new energy vehicles, consumer electronics batteries, and energy storage batteries. In this scenario, the objects to be processed are typically positive and negative electrode sheets with active layers, and the recycling process needs to balance the integrity of the current collector recovery with the reuse value of the active materials.
[0033] Existing electrode stripping methods typically employ mechanical separation, pyrolysis, and chemical solvent treatment. The basic idea is to weaken the bonding force between the active layer and the current collector, thus separating the active material from the metal foil. However, mechanical stripping easily leads to current collector breakage, active material contamination, and low separation rates. Pyrolysis requires temperatures of 400℃-700℃, resulting in high energy consumption and the generation of toxic fumes. Chemical solvent treatment consumes large amounts of organic solvents, leading to high costs and difficulties in recycling. Therefore, in actual recycling processes, existing stripping methods are prone to incomplete stripping, excessive residue on the current collector surface, and impurities trapped in the active material. Some methods also result in current collector damage, disturbance of the active material structure, excessive medium consumption, or high overall energy consumption, thus affecting the stability and economics of subsequent recycling. These shortcomings not only reduce the quality of recycled metal foil and active materials but also increase the burden of subsequent sorting, purification, and regeneration processes, making it difficult for large-scale recycling processes to simultaneously meet requirements for efficiency, purity, material protection, and resource utilization costs.
[0034] In view of this, how to balance separation efficiency, product purity, and material integrity during electrode recycling has become an urgent technical problem to be solved. To address this issue, an electrode stripping method is provided. This method is applicable to the stripping stage of the waste lithium-ion battery electrode recycling process. It revolves around the technical route of "mixing treatment, microwave action, solid-liquid separation, and flexible stripping," which helps reduce the risk of residue and damage during electrode separation and provides a foundation for subsequent material recycling and reuse.
[0035] Figure 1 This is a process flow diagram of the stripping method in some embodiments of this application; Figure 2 This is a process flow diagram of microwave radiation treatment in some embodiments of this application. For example... Figure 1 and Figure 2 As shown, some embodiments of this application provide a method for peeling off an electrode sheet, including:
[0036] After mixing the electrode with the auxiliary separation medium, microwave radiation treatment was carried out under an inert atmosphere to obtain a solid-liquid mixture.
[0037] Solid-liquid mixtures are subjected to solid-liquid separation treatment to obtain solid products;
[0038] The solid product is subjected to flexible exfoliation to obtain the current collector and the active material.
[0039] Specifically, the electrode to be recycled is mixed with an auxiliary separation medium and then subjected to microwave irradiation in an inert atmosphere. Microwave irradiation can be applied continuously or intermittently to reduce the risk of oxidation and thermal runaway during heating. The auxiliary separation medium, acting in conjunction with the electrode in the microwave field, can more evenly distribute microwave energy to the electrode surface and the interior of the active layer, weakening or loosening the bonding system, conductive agent network, and the bond between the active material and the current collector, thus forming a solid-liquid mixture containing both liquid and solid phases. After microwave treatment, the auxiliary separation medium enters the pores of the active layer and accelerates stress release at the interface, thereby promoting the active layer peeling process. The resulting solid-liquid mixture is then subjected to solid-liquid separation to separate the liquid and solid phases, yielding a solid product mainly composed of the current collector, residual active layer fragments, and some active material aggregates. Since the preceding microwave irradiation weakens the coating adhesion, solid-liquid separation can promptly remove detached fine particles, media, and dissolved components, reducing their re-adhesion in subsequent processing. Further, a flexible peeling process is applied to the solid product to separate the residual active material from the current collector under lower mechanical stress. This gently removes the residue from the surface of the current collector and yields both the current collector and the active material. Because the flexible peeling process is primarily low-damage, it can maintain the continuity of the metal foil while reducing the breakage of active material particles and the wrinkling and fracture of the current collector. Consequently, the separated current collector and active material are more suitable for subsequent recycling processes.
[0040] In this application, through a continuous process path of "microwave radiation pretreatment—solid-liquid separation—flexible peeling," the bonding state of the active layer of the electrode is first weakened by the auxiliary separation medium and the microwave field, then the liquid phase and detached components are removed through separation steps, and finally the residual peeling is completed in a low-mechanical-damage manner. This facilitates the separation of the electrode under relatively mild conditions and maintains a relatively stable level of current collector recovery integrity and active material separation purity. It should be understood that the above example is merely illustrative and not limiting.
[0041] In some embodiments, microwave radiation treatment may include placing electrodes and an auxiliary separation medium in a microwave resonant cavity, controlling the specific process parameters of the microwave radiation treatment such as temperature, power, and time of the microwave resonant cavity through a control system, and generating microwaves in the microwave resonant cavity through a generating system to achieve microwave radiation treatment. In some embodiments, the microwave resonant cavity also includes a stirring unit or a temperature measuring unit. In some embodiments, the microwave resonant cavity also includes a safety system, such as at least one of a door interlock, a leakage protection unit, a condensation reflux unit, and a pressure protection unit.
[0042] In some embodiments of this application, the auxiliary separation medium can be selected according to the electrode system, and the electrode can be differentially soaked using the auxiliary separation medium, followed by microwave radiation treatment. The two work synergistically to achieve efficient separation of the current collector and the active material.
[0043] In some embodiments of this application, the electrode is a positive electrode, the current collector is aluminum foil, and the active material includes at least one of lithium iron phosphate, lithium cobalt oxide, and ternary positive electrode materials.
[0044] During recycling, the positive electrode sheet is mixed with an auxiliary separation medium and placed in an inert atmosphere to receive microwave radiation. The microwave energy, combined with the dielectric and thermal response differences between the aluminum foil and the positive electrode active layer, rapidly weakens the adhesion between the positive electrode active layer and the aluminum foil interface, causing the positive electrode active material to detach from the aluminum foil surface, thus forming a solid-liquid mixture. The solid-liquid mixture is then subjected to solid-liquid separation to effectively distinguish the released positive electrode active material from the aluminum foil substrate. The resulting solid product is then subjected to flexible peeling to further remove the small amount of positive electrode active layer remaining on the aluminum foil surface, yielding the positive electrode current collector and the positive electrode active material. Because the positive electrode sheet, aluminum foil, and positive electrode active material system are limited to a highly compatible combination, the microwave action and flexible peeling can more stably and synergistically achieve interface dissociation, thereby reducing the probability of aluminum foil damage and residual positive electrode active material, and making the recycled product more suitable for subsequent recycling.
[0045] Furthermore, the auxiliary separation medium includes an alkaline aqueous solution and a reducing agent. The reducing agent in the auxiliary separation medium has a mass percentage of 2%-8%, and the reducing agent includes sodium sulfite and / or sodium dithionite.
[0046] The mass-to-volume ratio of the positive electrode to the auxiliary separation medium is 1:(10-30)g / mL.
[0047] The mass percentage of the reducing agent is controlled at 2%-8%, which can ensure that the reducing components maintain sufficient activity in the auxiliary separation medium, while avoiding insufficient effect due to too low concentration or excessive reaction of the system due to too high concentration. Sodium sulfite and / or sodium dithionite can provide effective reduction in this alkaline environment, and both can be used alone or in combination to adapt to different positive electrode systems.
[0048] The mass-to-volume ratio of the positive electrode to the auxiliary separation medium is 1:(10-30) g / mL. This means that the auxiliary separation medium per unit mass of positive electrode is sufficient to fully wet the positive electrode active layer and cover the surface of the positive electrode current collector, allowing the alkaline aqueous solution and reducing agent to uniformly contact all areas of the electrode, thereby reducing residues caused by insufficient local treatment. If the amount of auxiliary separation medium is too small, the interfacial reaction and heat and mass transfer will be limited; if the amount of auxiliary separation medium is too large, it will increase the burden on subsequent separation. Limiting this ratio within the above range can achieve a balance between the effectiveness of the auxiliary separation medium and the economic efficiency of treatment.
[0049] Furthermore, in the microwave radiation treatment, the power is 400W-800W, the temperature is 180℃-260℃, and the time is 15min-40min. Here, power characterizes the microwave input intensity, temperature reflects the system's thermal state, and time determines the duration of the interfacial interaction. By controlling the microwave radiation within this range, the polar components and reducing agents in the alkaline aqueous solution can rapidly absorb energy in the microwave field and generate a selective heating effect, causing the adhesive layer to soften, expand, and locally destabilize, thereby promoting the desorption of the positive electrode active material from the aluminum foil surface. The coordinated control of temperature and time avoids incomplete peeling or excessive thermal damage, thus making it easier to obtain a more complete positive electrode current collector and clearly separated positive electrode active material in subsequent solid-liquid separation and flexible peeling processes.
[0050] In some embodiments of this application, the electrode is a negative electrode, the current collector is copper foil, and the active material includes graphite.
[0051] In practice, the object to be processed is the negative electrode sheet from a spent lithium-ion battery, with copper foil as the current collector. The negative electrode active layer on the surface contains at least graphite and may be accompanied by a small amount of conductive carbon and binder. The bonding between the copper foil and the graphite system mainly depends on the interfacial adhesion formed by the binder. When the electrode sheet enters the auxiliary separation medium and is subjected to microwave radiation, the auxiliary separation medium wets and heats the bonding system, which can reduce the bonding force between the negative electrode active layer and the copper foil interface. At the same time, the peeling response of graphite particles on the copper foil substrate is relatively stable and is not prone to severe structural collapse. This makes it easier to perform flexible peeling treatment on the solid products after subsequent solid-liquid separation, resulting in relatively intact copper foil and graphite materials.
[0052] Furthermore, the auxiliary separation medium includes organic solvents and additives, wherein the mass percentage of the additives in the auxiliary separation medium is 1%-5%; the organic solvents include N-methylpyrrolidone and / or dimethyl carbonate; and the additives include lithium carbonate and / or lithium chloride.
[0053] The mass-to-volume ratio of the negative electrode to the auxiliary separation medium is 1:(15-40)g / mL.
[0054] N-methylpyrrolidone and / or dimethyl carbonate can wet and loosen the bonding system and active layer in the negative electrode sheet, while lithium carbonate and / or lithium chloride can weaken the bonding force between the negative electrode active material and the copper foil by adjusting the ionic strength and interfacial interaction of the auxiliary separation medium.
[0055] By controlling the mass percentage of the auxiliary agent at 1%-5%, it is possible to ensure that the auxiliary separation medium has an effective effect on the negative electrode while avoiding excessive auxiliary agent that could lead to increased solution viscosity or decreased system dispersibility. This allows the auxiliary separation medium to have both permeation efficiency and processing stability.
[0056] The mass-to-volume ratio of the negative electrode to the auxiliary separation medium is 1:(15-40) g / mL, indicating that a certain mass of negative electrode corresponds to a unit volume of auxiliary separation medium. This dosing ratio allows the auxiliary separation medium to fully wet the electrode surface and penetrate into the active layer of the negative electrode, resulting in a more uniform effect of the solvent and additives on the bonding interface. If the amount of auxiliary separation medium is too low, the stacked area of the negative electrode will not be able to fully contact the auxiliary separation medium; if the amount of auxiliary separation medium is too high, it will increase the consumption of the auxiliary separation medium and the burden on subsequent separation. Therefore, controlling this ratio within a certain range can achieve a balance between separation efficiency and process economy.
[0057] Furthermore, in the microwave radiation treatment, the power is 300W-600W, the temperature is 120℃-200℃, and the time is 10min-30min. Through the coupling effect of microwaves with the conductive components in the negative electrode and the auxiliary separation medium, the local interface is rapidly heated, inducing relaxation, pyrolysis, and desorption of the negative electrode active layer. By controlling the power, temperature, and time within this range, the effect of the auxiliary separation medium and the microwave thermal effect can work synergistically, effectively detaching the negative electrode active material from the negative electrode current collector while avoiding excessive heat load that could damage the copper foil structure or cause excessive disturbance to the surface of the negative electrode active material. This improves the integrity of the peeling and reduces residual impurities.
[0058] Because the negative electrode system and the positive electrode system differ in current collector material, active material composition, and interface bonding mode, this limitation makes the stripping conditions more closely match the characteristics of the negative electrode sheet, thereby reducing the probability of residual adhesion and metal foil damage, and ensuring that both the separated copper foil and graphite remain in a good recyclable state. In some embodiments, the stripping method of this application can efficiently separate the current collector and active material, with a separation rate ≥99.5%, and the residual active layer on the surface of the current collector ≤0.5%; the product has high purity: the purity of aluminum foil ≥99.2%, the purity of copper foil ≥99.5%, and the impurity content of the active material ≤0.3%, which can be directly regenerated; it is low-energy and environmentally friendly: the microwave time is shortened by more than 80%, energy consumption is reduced by 60%-70%, there is no toxic smoke, and the medium can be recycled. Moreover, the stripping method of this application has a wide range of applications and can be compatible with various electrode systems such as ternary positive electrode materials, lithium iron phosphate, lithium cobalt oxide, and graphite negative electrodes.
[0059] In some embodiments of this application, the solid product is further dried after the solid-liquid separation process.
[0060] During the drying process, the temperature is 60℃-80℃ and the time is 2h-4h.
[0061] In practice, the solid product after solid-liquid separation can be spread evenly in a heat-resistant container and placed in a constant-temperature drying device for heating treatment. The drying temperature is controlled at 60℃-80℃ and maintained for 2-4 hours. Limiting the temperature within this range allows the residual liquid to fully evaporate or be removed in a short time, while avoiding excessively high temperatures that could lead to oxidation of the current collector surface, disturbance of the active material structure, or further hardening of adhering residues, thus increasing the difficulty of subsequent separation. Controlling the drying time to 2-4 hours removes moisture and solvents while avoiding unnecessary energy consumption and material damage caused by overheating. Through the coordinated control of temperature and time, the liquid phase component in the solid product is effectively removed, reducing its liquid content and making the material state more stable. This facilitates subsequent flexible peeling treatment of the solid product and reduces the adverse effects of residual liquid on the purity of the current collector and the recovered active material.
[0062] The mechanism of this drying process is that after solid-liquid separation, a certain amount of liquid usually remains on the surface of the solid product. If it is directly introduced into subsequent processing, the residual liquid can easily cause material adhesion, poor dispersibility, and reduced separation efficiency. By using controlled drying conditions of 60℃-80℃ for 2h-4h, gentle dehydration can be achieved while ensuring the structural integrity of the solid product, thereby improving the stability of the subsequent recovery process and making the current collector and active material easier to separate and the recovery quality more consistent.
[0063] In some embodiments of this application, the flexible peeling process includes impacting the solid product with an airflow of 15 m / s to 25 m / s.
[0064] Solid products can be subjected to continuous airflow impact within a sealed peeling chamber, with the airflow velocity controlled between 15 m / s and 25 m / s. By limiting the airflow velocity within this range, the airflow can exert sufficient shearing and scouring action on the solid products, gradually loosening and separating the residues adhering to the surface of the current collector. This avoids incomplete peeling due to excessively low airflow velocity, or curling, breakage, and excessive pulverization of the current collector due to excessively high airflow velocity. This velocity range is determined by considering the particle state of the solid products, surface adhesion strength, and peeling integrity requirements, matching the airflow energy with the adhesion weakening process, thereby achieving a relatively stable flexible peeling process without introducing hard mechanical contact.
[0065] In some embodiments of this application, the flow rate of the inert atmosphere is 0.5 L / min to 2 L / min. By controlling the flow rate within this range, a stable inert protective environment can be maintained within the stripping chamber, reducing oxidation, moisture absorption, or secondary pollution caused by air ingress, while ensuring that the gas renewal rate is sufficient to remove fine dust and volatile residues generated during the stripping process. If the flow rate is too low, the inert replacement effect is insufficient, easily leading to environmental influences on the product surface; if the flow rate is too high, it may increase product scattering and local disturbances, which is not conducive to the stable execution of the flexible stripping process. Therefore, this flow rate range achieves a balance between inert protection and stripping disturbances, resulting in less residue on the surface of the current collector and higher integrity of the active material.
[0066] In some embodiments of this application, post-processing is included after the flexible peeling process. The post-processing includes sieving and / or magnetic separation, with the sieving process having a mesh size of 100-200 mesh.
[0067] Post-processing refers to the further purification and classification of the mixture of current collector and active material after the flexible stripping process. Sieving utilizes a sieve with a predetermined aperture size to separate particles of different sizes, further differentiating finer active material particles from larger metal foil fragments, agglomerates, and other impurities. The sieve mesh size is controlled between 100 and 200 mesh, indicating that the mesh size is suitable for separating the stripped mixture. This allows the active material to pass through the sieve more fully and separate from the current collector fragments without excessively entraining fine metal debris. This mesh size range matches the particle state after the flexible stripping process, avoiding incomplete separation due to an excessively low mesh size and sieving blockage and material loss due to an excessively high mesh size, thus resulting in a more stable product particle size distribution. Magnetic separation utilizes the potential differences in magnetic response within the current collector or inclusions to further remove residual metal impurities, thereby reducing the impact of non-target metals on the purity of the recovered product. Screening and magnetic separation can be carried out separately or in combination. Through the synergistic effect of particle size classification and magnetic separation, the separation of current collector and active material obtained after flexible stripping is more thorough, further reducing entrained impurities and cross-contamination, and improving the purity and consistency required for subsequent recycling.
[0068] In some embodiments of this application, the battery is discharged to a voltage ≤1.5V and then disassembled to obtain the electrode sheets.
[0069] Specifically, retired batteries can be discharged to a voltage no higher than 1.5V before being disassembled to obtain the electrodes. Discharging the battery to this voltage range can significantly reduce the risk of short circuits, thermal runaway, or localized heat release caused by residual energy, making the disassembly process safer and more stable. At the same time, the electrochemical activity inside the cell is weakened at a lower voltage, and the cooperation between the electrodes, separator, and casing is easier to break, thus facilitating the acquisition of structurally intact electrode materials.
[0070] In some embodiments of this application, the length of the first side of the electrode is 50mm-100mm, the length of the second side of the electrode is 50mm-100mm, and the first and second sides are perpendicular to each other. This can further unify the geometric dimensions of the object to be peeled off, making it more uniformly heated and reacting more consistently in subsequent microwave radiation and flexible peeling processes, ultimately improving the separation stability of the current collector and the active material, and reducing residues and damage.
[0071] This application also provides an apparatus for implementing the above-described electrode stripping method, comprising: an inert atmosphere channel, a microwave radiation unit, a solid-liquid separation unit, and a flexible stripping unit;
[0072] The inert atmosphere channel is connected to the inlet of the microwave radiation unit. The electrode and the auxiliary separation medium are located in the microwave radiation unit. The outlet of the microwave radiation unit is connected to the inlet of the solid-liquid separation unit. The solid outlet of the solid-liquid separation unit is connected to the inlet of the flexible stripping unit. The flexible stripping unit has a current collector outlet and an active material outlet.
[0073] Specifically, an inert atmosphere is continuously supplied to the inlet of the microwave radiation unit through an inert atmosphere channel. This suppresses oxidation and side reactions when the electrode and auxiliary separation medium are subjected to microwaves, thus weakening the bonding system and making it more stable. The microwave radiation unit and the solid-liquid separation unit are connected sequentially, allowing the processed solid-liquid mixture to be promptly discharged and separated, thereby reducing medium entrainment and material mixing. The solid product after solid-liquid separation continues to enter the flexible stripping unit, where the current collector and active material are separated under relatively mild stress conditions. This reduces damage to the current collector and structural disturbance of the active material, and the product is then discharged through the current collector outlet and the active material outlet, respectively. Therefore, this method is beneficial for improving the separation adaptability, product purity, and material integrity in the recovery process of different electrodes.
[0074] The present invention will be further described below with reference to specific embodiments.
[0075] Example 1
[0076] In the electrode stripping method of this embodiment, the electrode is a positive electrode, the current collector is aluminum foil, the active material includes lithium iron phosphate, and the stripping method includes:
[0077] 1) Pre-treatment: Discharge the waste lithium iron phosphate batteries to 1.2V, disassemble them to obtain the positive electrode sheet, and cut the positive electrode sheet to 80mm×80mm;
[0078] 2) Medium preparation: Prepare a 5% sodium sulfite aqueous solution, mix the cut positive electrode sheet with the sodium sulfite aqueous solution, and the solid-liquid ratio is 1:20 (g:mL).
[0079] 3) Microwave radiation treatment: The mixed positive electrode sheet and sodium sulfite aqueous solution were placed in a nitrogen-protected microwave reactor for microwave radiation treatment to obtain a solid-liquid mixture. During the microwave radiation treatment, the power was 600W, the temperature was raised to 220℃, and the treatment time was 25min.
[0080] 4) Separation and drying: After vacuum filtration of the solid-liquid mixture, a solid product is obtained, which is then dried at 70°C for 3 hours.
[0081] 5) Flexible peeling process: The dried solid product is impacted by a 20m / s airflow and then sieved through a 150-mesh sieve to obtain aluminum foil and lithium iron phosphate powder.
[0082] The obtained aluminum foil and lithium iron phosphate powder were tested, specifically including: the separation rate of aluminum foil and positive electrode active layer = mass of lithium iron phosphate powder after peeling treatment / (total mass of positive electrode sheet - total mass of aluminum foil of the same size); aluminum foil purity: the aluminum foil obtained from peeling off the positive electrode sheet was ultrasonically cleaned with NMP, washed with deionized water and ethanol, and vacuum dried at 60℃; a certain mass of aluminum foil sample was weighed, digested with hydrochloric acid-nitric acid mixed acid, and after being brought to a certain volume, it was analyzed by inductively coupled plasma atomic emission spectrometry (ICP-AES). The purity of aluminum foil is obtained by determining the mass fraction of aluminum.
[0083] Test of Al content by mass percentage in lithium iron phosphate powder: Lithium iron phosphate powder was dried in an oven at 105℃ for 2 hours. After cooling, 0.2000g of the dried lithium iron phosphate was weighed and placed in a polytetrafluoroethylene beaker. An appropriate amount of hydrochloric acid was added, and the mixture was heated at low temperature using a hot plate to dissolve the lithium iron phosphate. After adjusting the volume, inductively coupled plasma atomic emission spectrometry (ICP-AES) was used. The mass fraction of aluminum was determined to obtain the mass percentage of Al in lithium iron phosphate powder.
[0084] According to the test, the separation rate of aluminum foil and positive electrode active layer in this embodiment is 99.7%, the purity of the recovered aluminum foil is 99.3%, and the mass percentage of Al in the lithium iron phosphate powder is 0.2%.
[0085] Example 2
[0086] In the electrode stripping method of this embodiment, the electrode is a negative electrode, the current collector is copper foil, the active material includes graphite, and the stripping method includes:
[0087] 1) Pre-treatment: Discharge the waste graphite battery to 1V, disassemble it to obtain the negative electrode sheet, and cut the negative electrode sheet to 60mm×60mm;
[0088] 2) Medium preparation: Prepare a 3% lithium chloride NMP solution, mix the cut negative electrode sheet with the lithium chloride NMP solution, and the solid-liquid ratio is 1:25 (g:mL).
[0089] 3) Microwave radiation treatment: The mixed negative electrode sheet and lithium chloride NMP solution were placed in a nitrogen-protected microwave reactor for microwave radiation treatment to obtain a solid-liquid mixture. During the microwave radiation treatment, the power was 450W, the temperature was raised to 160℃, and the treatment time was 20min.
[0090] 4) Separation and drying: After vacuum filtration of the solid-liquid mixture, a solid product is obtained, which is then dried at 65°C for 3.5 hours.
[0091] 5) Flexible peeling process: The dried solid product is impacted by an airflow of 18 m / s, and then subjected to 200-mesh sieve and magnetic separation to obtain copper foil and graphite.
[0092] The obtained copper foil and graphite powder were tested, specifically including: the separation rate of copper foil and negative electrode active layer = mass of graphite powder after peeling treatment / (total mass of negative electrode sheet - total mass of copper foil of the same size); copper foil purity: the copper foil obtained from the negative electrode sheet was ultrasonically cleaned, washed with deionized water and ethanol, and vacuum dried at 60℃; a certain mass of copper foil sample was weighed, digested with hydrochloric acid-nitric acid mixed acid, and after being brought to a certain volume, it was analyzed by inductively coupled plasma atomic emission spectrometry (ICP-AES). The purity of the copper foil is obtained by determining the mass fraction of copper.
[0093] Test of the mass percentage of copper impurities in recycled graphite: Recycled graphite powder was dried in an oven at 105℃ for 2 hours. After cooling, a certain mass of sample was weighed and placed in a porcelain crucible. The crucible was placed in a muffle furnace and kept at 600℃ for 3 hours in air atmosphere to completely burn off the graphite matrix. After cooling, ash was obtained. A mixed acid of hydrochloric acid and nitric acid was added to the ash, and the ash was dissolved by low-temperature heating on a hot plate. After volume adjustment, inductively coupled plasma atomic emission spectrometry (ICP-AES) was used to analyze the ash content. The mass fraction of copper impurities in the test solution was determined to obtain the mass percentage of copper impurities in the recycled graphite. Testing showed that in this embodiment, the separation rate of copper foil and the negative electrode active layer was 99.6%, the purity of the recovered copper foil was 99.6%, and the mass percentage of copper impurities in the recycled graphite was 0.25%.
[0094] Comparative Example 1
[0095] In the electrode peeling method of this comparative example, the electrode is the same as that in Example 1. The difference is that the electrode to be tested is flattened and fixed, and the surface of the positive electrode active layer of the electrode is mechanically rubbed back and forth with a steel wool ball to separate the aluminum foil from the positive electrode active layer, thereby obtaining lithium iron phosphate powder and aluminum foil.
[0096] The obtained aluminum foil and lithium iron phosphate powder were tested, specifically including: aluminum foil breakage rate test: the aluminum foil peeled from the electrode was ultrasonically cleaned, washed with deionized water and ethanol, and vacuum dried at 60°C to constant weight; the dried aluminum foil samples were sieved, and aluminum foil with a longest side of 10 mm was defined as broken aluminum foil, and aluminum foil with a longest side of 10 mm or more was defined as intact aluminum foil; the mass of broken aluminum foil and the total mass of aluminum foil samples were weighed separately; aluminum foil breakage rate = mass of broken aluminum foil / total mass of aluminum foil × 100%.
[0097] Fe contamination content test of powder: Lithium iron phosphate powder was dried in an oven at 105℃ for 2 hours and then cooled; a certain mass of the dried lithium iron phosphate powder was weighed and placed in deionized water and stirred to disperse; a strong magnetic rod with a polyethylene protective film on its surface was inserted into the powder suspension and stirred thoroughly to adsorb the metallic ferromagnetic impurities in the powder; the magnetic rod was removed, and the lithium iron phosphate powder adhering to the surface of the magnetic rod was rinsed with deionized water, and then the metallic iron impurities adsorbed on the surface of the magnetic rod were washed off and collected; hydrochloric acid-nitric acid mixed acid was added to the collected iron impurities, and the mixture was digested by low-temperature heating on a hot plate; after volume adjustment, inductively coupled plasma atomic emission spectrometry (ICP-AES) was used. The concentration of iron ions in the test solution was determined, and the mass percentage of Fe contamination was calculated. (Due to the reciprocating mechanical friction of the positive electrode active layer surface by steel wool, during the separation of aluminum foil from the positive electrode active layer, the high-intensity friction wears down all contacted metal parts, such as clamps, screens, containers, and equipment, causing Fe particles to fall off, resulting in powdered Fe contamination in the recovered lithium iron phosphate.)
[0098] Tests showed that the separation rate of aluminum foil and positive electrode active layer in this comparative example was 92%, the aluminum foil breakage rate was 15%, and the Fe contamination content of the powder was 1.2%.
[0099] Comparative Example 2
[0100] In the electrode stripping method of this comparative example, the electrode is the same as that in Example 1, except that step 2) is not included, in which the cut positive electrode is directly placed in a microwave reactor for microwave radiation treatment.
[0101] The obtained aluminum foil and lithium iron phosphate powder were tested, specifically including: the mass percentage of residual active layer in the current collector; digestion with a mixed hydrochloric acid-nitric acid solution upon heating, followed by volume adjustment to obtain the test solution; and utilizing... The concentration of phosphorus in the test solution was determined, and the mass percentage of residual lithium iron phosphate was calculated.
[0102] Testing revealed that the separation rate between the aluminum foil and the positive electrode active layer in this comparative example was 94%, and the mass percentage of the residual active layer in the current collector was 3.5%. In summary, the electrode stripping method of this application embodiment can more efficiently separate the current collector from the active layer, and can obtain high-purity current collectors and active materials. Furthermore, this stripping method has low energy consumption, is environmentally friendly, and is suitable for widespread application.
[0103] Finally, it should be noted that other embodiments of the invention will readily occur to those skilled in the art upon consideration of the specification and practice of the invention disclosed herein. This invention is intended to cover any variations, uses, or adaptations of the invention that follow the general principles of the invention and include common knowledge or customary techniques in the art not disclosed herein, and is not limited to the precise structures described above and shown in the accompanying drawings, and various modifications and changes can be made without departing from its scope. The scope of the invention is limited only by the appended claims.
Claims
1. A method for peeling off an electrode sheet, characterized in that, include: After mixing the electrode with the auxiliary separation medium, microwave radiation treatment was carried out under an inert atmosphere to obtain a solid-liquid mixture. The solid-liquid mixture is subjected to solid-liquid separation treatment to obtain a solid product; The solid product is subjected to a flexible exfoliation process to obtain a current collector and an active material.
2. The peeling method according to claim 1, characterized in that, The electrode is a positive electrode, the current collector is aluminum foil, and the active material includes at least one of lithium iron phosphate, lithium cobalt oxide, and ternary positive electrode materials.
3. The peeling method according to claim 2, characterized in that, The auxiliary separation medium includes an alkaline aqueous solution and a reducing agent. The reducing agent has a mass percentage of 2%-8% and includes sodium sulfite and / or sodium dithionite. The mass-to-volume ratio of the positive electrode to the auxiliary separation medium is 1:(10-30)g / mL; And / or, in the microwave radiation treatment, the power is 400W-800W, the temperature is 180℃-260℃, and the time is 15min-40min.
4. The peeling method according to claim 1, characterized in that, The electrode is a negative electrode, the current collector is copper foil, and the active material includes graphite.
5. The peeling method according to claim 4, characterized in that, The auxiliary separation medium includes an organic solvent and an auxiliary agent, wherein the auxiliary agent has a mass percentage of 1%-5% in the auxiliary separation medium; the organic solvent includes N-methylpyrrolidone and / or dimethyl carbonate; and the auxiliary agent includes lithium carbonate and / or lithium chloride. The mass-to-volume ratio of the negative electrode to the auxiliary separation medium is 1:(15-40)g / mL; And / or, in the microwave radiation treatment, the power is 300W-600W, the temperature is 120℃-200℃, and the time is 10min-30min.
6. The peeling method according to any one of claims 1-5, characterized in that, The solid-liquid separation process further includes drying the solid product. In the drying process, the temperature is 60℃-80℃ and the time is 2h-4h.
7. The peeling method according to any one of claims 1-6, characterized in that, The flexible exfoliation process includes impacting the solid product with an airflow of 15 m / s to 25 m / s; and / or, The flow rate of the inert atmosphere is 0.5 L / min to 2 L / min.
8. The peeling method according to any one of claims 1-7, characterized in that, The process includes post-processing following the flexible peeling process, which includes sieving and / or magnetic separation, wherein the sieving process has a mesh size of 100-200 mesh.
9. The peeling method according to any one of claims 1-8, characterized in that, The length of the first side of the electrode is 50mm-100mm, the length of the second side of the electrode is 50mm-100mm, and the first side and the second side are perpendicular to each other; and / or, It also includes disassembling the battery after discharging it to a voltage of ≤1.5V to obtain the electrode sheet.
10. An apparatus for implementing the electrode stripping method according to any one of claims 1-9, characterized in that, include: Inert atmosphere channel, microwave radiation unit, solid-liquid separation unit, and flexible peeling unit; The inert atmosphere channel is connected to the inlet of the microwave radiation unit. The electrode and the auxiliary separation medium are located in the microwave radiation unit. The outlet of the microwave radiation unit is connected to the inlet of the solid-liquid separation unit. The solid outlet of the solid-liquid separation unit is connected to the inlet of the flexible stripping unit. The flexible stripping unit has a current collector outlet and an active material outlet.