A method for preparing a sodium battery positive electrode by solid-phase modification of waste ternary lithium transition metal oxide
By using organic acid wet ball milling and high-temperature sintering to build coherent coating interfaces, waste ternary lithium battery cathode materials are regenerated into high-performance sodium-ion battery cathode materials. This solves the problem of weak interfacial bonding and improves cycle stability and rate performance.
Patent Information
- Application Number
- CN202611517978.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-29
- Publication Date
- 2026-11-24
AI Technical Summary
Existing technologies make it difficult to efficiently regenerate waste ternary lithium battery cathode materials into sodium-ion battery cathode materials, and traditional coating modification methods have weak interfacial bonding, resulting in poor cycle stability.
A coherent coating interface was constructed by wet ball milling with organic acids and high-temperature sintering, combining waste ternary lithium battery cathode materials with Na₃Zr₂Si₂PO₁₂ coating layers to form a lattice-matched coherent coating layer, thereby enhancing the interfacial bonding force.
It significantly improves the cycle stability and rate performance of recycled materials, inhibits the dissolution of transition metals and the erosion of electrolyte, and realizes the preparation of high-performance sodium-ion battery cathode materials.
Smart Images

Figure CN123162373A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of waste lithium-ion battery recycling technology, specifically involving a method for solid-phase modification and regeneration of waste ternary lithium battery cathode materials into high-performance sodium-ion battery cathode materials by achieving coherent coating of high-valence elements through organic acid surface activation. Background Technology
[0002] With the advancement of the "dual-carbon" strategy, lithium-ion batteries are being used on a large scale in new energy vehicles, energy storage power stations, and other fields, resulting in a rapid increase in the number of waste lithium-ion batteries. Waste ternary lithium batteries contain a large number of valuable metals and toxic compounds. Improper disposal will not only waste resources but also pose serious environmental risks. Therefore, the efficient recycling and high-value utilization of retired lithium batteries has become an important development direction for the new energy industry.
[0003] Sodium-ion batteries are considered an important technology in the energy storage field due to the abundance and low cost of sodium resources and their similar working principle to lithium-ion batteries. Directly regenerating spent ternary lithium battery cathode materials into sodium-ion battery cathode materials through elemental regulation can eliminate the complex processes of acid leaching, extraction, and separation required in traditional wet recycling, achieving a short-process, high-value conversion of retired lithium batteries, thus combining economic and environmental benefits.
[0004] However, existing direct regeneration technologies still have significant shortcomings: on the one hand, after lithium extraction, the surface atoms of waste ternary materials are densely packed with numerous lattice defects, making it difficult for dopant elements to effectively penetrate the surface lattice during regeneration, thus limiting the modification effect; on the other hand, traditional coating modification is mostly physical deposition coating, resulting in poor lattice matching between the coating layer and the substrate, weak interfacial bonding, and easy peeling due to material volume expansion during long cycles. This also fails to continuously suppress transition metal dissolution and electrolyte side reactions, leading to poor cycle stability of the regenerated material. Therefore, developing a direct regeneration method for waste ternary cathodes that can achieve coherent bonding between the coating layer and the substrate and a stable interfacial structure is of significant practical importance.
[0005] In summary, constructing a coherent coating interface through organic acid surface activation to directly regenerate waste ternary lithium-ion battery cathode materials into high-performance sodium-ion battery cathode materials has broad development prospects and application value. Summary of the Invention
[0006] To address the shortcomings of existing technologies, this invention provides a method for preparing sodium-ion cathodes by solid-phase modification of waste ternary lithium-ion battery transition metal oxides.
[0007] The objective of this invention is achieved through the following technical solution, including the following steps:
[0008] (1) The waste ternary lithium battery positive electrode powder and ammonium sulfate are mechanically ball-milled and then mixed evenly;
[0009] (2) The mixture was calcined at high temperature in a tube furnace, and after cooling, lithium salt was extracted by ultrasonic water leaching, filtered and dried to obtain transition metal oxide precursors;
[0010] (3) The above transition metal oxide precursor is mixed with an organic acid solution and subjected to wet ball milling to loosen the surface atomic arrangement;
[0011] (4) The wet ball milled slurry is washed with water and filtered to collect the filter cake and placed in an oven to dry, so as to obtain the activated precursor powder.
[0012] (5) The activated precursor powder, sodium salt and Na3Zr2Si2PO doped with high-valence elements are combined. 12 The materials are mixed in proportion and then uniformly compounded by mechanical ball milling.
[0013] (6) The uniformly mixed powder is placed in a muffle furnace for high-temperature solid-state sintering to obtain a coherent coated sodium cathode material doped with high-valence elements.
[0014] Preferably, in step (1), the mass ratio of waste ternary lithium battery cathode powder to ammonium sulfate is 1:0.5 to 1:0.9; the ball milling time is 0.5 to 6 hours; and the ball milling speed is 100 to 800 rpm.
[0015] Preferably, in step (2), the high-temperature calcination atmosphere in the tubular furnace is Ar or N2 or Ar / N2 mixture, the calcination temperature is 400~1000℃, the heating rate is 1~10℃ / min, and the calcination time is 1~10 h.
[0016] Preferably, in step (3), the organic acid is one or more of citric acid, malic acid, and oxalic acid in any proportion; the concentration of the organic acid solution is 0.1~2.0 mol / L, the solid-liquid ratio of the precursor powder to the organic acid solution is 1:5~1:20 g / mL; the wet ball milling time is 1~8h, and the ball milling speed is 200~600 rpm.
[0017] Preferably, in step (4), the drying temperature is 60~120℃ and the drying time is 6~12 h.
[0018] Preferably, in step (5), the sodium salt is sodium carbonate or sodium hydroxide, and the molar ratio of the activation precursor to the sodium salt is 1:0.8 to 1:1.2; Na3Zr2Si2PO 12 The high-valence elements doped in Na3Zr2Si2PO are any one or more of Ti, Nb, W, Ta, and Mo. 12 The amount of transition metal is 2% to 10% of the total molar amount; the ball milling time is 1 to 12 hours, and the ball milling speed is 200 to 800 rpm.
[0019] Preferably, in step (6), the sintering temperature is 700~1000℃, the heating rate is 1~10℃ / min, and the sintering time is 8~24h.
[0020] Preferably, in step (6), the resulting regenerated sodium-ion ternary cathode material has the following composition: Na x Li y (Ni z Co m Mn n ) 1− a TM a O2@Na3Zr 2-b TM b Si2PO 12 , where 0.8≤x≤1.2, 0.01≤y≤0.1, z+m+n=1, 0.01≤a≤0.05, 0.1≤b≤0.2, and TM is one or more tetravalent or higher valence elements among Ti, Nb, W, Ta, and Mo.
[0021] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0022] (1) The present invention uses organic acid wet ball milling to activate the surface of the lithium-extracted precursor. Through the synergistic effect of acid etching and mechanical force, the atomic arrangement of the material surface layer is loosened and the surface energy is increased, providing sufficient active sites for subsequent element diffusion and crystal growth.
[0023] (2) During the high-temperature sintering process, the high-valence elements doped in the coating layer play an anchoring role at the interface, diffuse in situ into the surface lattice of the matrix, bond the coating layer and the matrix lattice, stabilize the layered crystal structure, form a coherent coating interface with lattice matching and tight bonding, suppress lattice distortion and phase transformation during the cycling process, and fundamentally solve the problem of easy peeling of traditional physical coating layers.
[0024] (3) Na3Zr2Si2PO 12 The coating layer can provide a rapid three-dimensional transport channel for sodium ions and reduce interfacial impedance, while also effectively isolating the active material from the corrosion of the electrolyte, inhibiting the dissolution of transition metals, and significantly improving the cycle stability and rate performance of the recycled material. Attached Figure Description
[0025] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0026] Figure 1 This is a graph showing the electrochemical performance test results of the recycled material obtained through solid-phase modification in Example 1 of this invention.
[0027] Figure 2 This is a graph showing the electrochemical performance test results of the recycled material obtained without solid-phase modification in Comparative Example 1 of this invention.
[0028] Figure 3 Na3Zr2Si2PO in Comparative Example 2 of this invention 12 Electrochemical performance test diagram of recycled materials obtained without high-valence elements in the coating layer.
[0029] Figure 4 This is the XRD pattern of the recycled material obtained by solid-phase modification in Example 1 of the present invention.
[0030] Figure 5 This is a SEM image of the recycled material obtained through solid-phase modification in Embodiment 1 of the present invention. Detailed Implementation
[0031] To facilitate understanding of the present invention, the present invention will be described more fully and in detail below with reference to the embodiments, but the scope of protection of the present invention is not limited to the following specific embodiments.
[0032] Unless otherwise defined, all technical terms used herein have the same meaning as commonly understood by those skilled in the art. The technical terms used herein are for the purpose of describing particular embodiments only and are not intended to limit the scope of the invention.
[0033] Unless otherwise specified, all raw materials, reagents, instruments and equipment used in this invention can be purchased from the market or prepared by existing methods.
[0034] Example 1:
[0035] This embodiment provides a method for preparing sodium-ion cathodes by solid-phase modification of waste ternary lithium-ion battery transition metal oxides. The material composition is Na. 1.05 Li 0.02 (Ni) 0.55 Co 0.15 Mn 0.30 ) 0.98 Ti 0.02 O2@ Na3Zr 1.9 Ti 0.1 Si2PO 12 This includes the following steps:
[0036] (1) Take 5 g of waste ternary cathode powder and 3.5 g of ammonium sulfate and add them to a ball mill jar. Ball mill at 400 r / min for 6 h to obtain a uniformly mixed powder.
[0037] (2) Place the powder in a porcelain boat, put it in the middle of a tube furnace, and calcine it at 700°C at 5°C / min under an Ar atmosphere for 2.5 h.
[0038] (3) After cooling, take out the material, add 500 mL of deionized water, soak in ultrasonic water for 20 min, filter and dry the filter cake in an oven at 80℃ for 12 h to obtain the transition metal oxide precursor.
[0039] (4) Take the above precursor and add it to a citric acid solution with a concentration of 1 mol / L, with a solid-liquid ratio of 1:10 g / mL. Transfer it to a ball mill jar for wet ball milling at a speed of 600 r / min for 3 h to complete surface activation.
[0040] (5) The activated slurry was repeatedly washed and filtered with deionized water, and the filter cake was dried at 80°C for 12 h to obtain activated precursor powder.
[0041] (6) Based on the total molar amount of transition metals, the activated precursor and sodium carbonate are mixed at a molar ratio of 1:1.05, and Ti-doped Na3Zr2Si2PO4, accounting for 2% of the total molar amount of transition metals, is added simultaneously. 12 The mixture was transferred into a ball mill jar and ball-milled at 400 r / min for 10 h to obtain a uniformly mixed powder.
[0042] (7) The mixed powder was placed in a ceramic boat, placed in a muffle furnace, heated to 900°C at 3°C / min, sintered for 12 h, and cooled with the furnace to obtain the target cathode material Na. 1.05 Li 0.02 (Ni) 0.55 Co 0.15 Mn 0.30 ) 0.98 Ti 0.02 O2@ Na3Zr 1.9 Ti 0.1 Si2PO 12 .
[0043] (8) Electrochemical performance was tested at room temperature. The results showed that the initial discharge specific capacity was 133.76 mAh / g, and the specific capacity retention rate after 40 cycles at 1C was 100.75%, demonstrating excellent specific capacity and cycle stability.
[0044] Example 2:
[0045] This embodiment provides a method for preparing sodium-ion cathodes by solid-phase modification of waste ternary lithium-ion battery transition metal oxides. The resulting material has a Na composition. 1.03 Li 0.02 (Ni) 0.55 Co 0.15Mn 0.30 ) 0.98 Nb 0.02 O2@ Na3Zr 1.9 Nb 0.1 Si2PO 12 This includes the following steps:
[0046] (1) Take 5 g of waste ternary cathode powder and 4 g of ammonium sulfate and add them to a ball mill jar. Ball mill at 600 r / min for 3 h to obtain a uniformly mixed powder.
[0047] (2) Place the powder in a porcelain boat, put it in the middle of a tube furnace, and calcine it to 800°C at 10°C / min under an Ar atmosphere for 2.5 h.
[0048] (3) After cooling, take out the material, add 500 mL of deionized water, ultrasonically soak for 25 min, filter and dry the filter cake in an oven at 100℃ for 10 h to obtain the transition metal oxide precursor.
[0049] (4) Take the above precursor and add it to a citric acid solution with a concentration of 1.5 mol / L, with a solid-liquid ratio of 1:8 g / mL. Transfer it to a ball mill jar for wet ball milling at a speed of 400 r / min for 6 h to complete surface activation.
[0050] (5) The activated slurry was repeatedly washed and filtered with deionized water, and the filter cake was dried at 100°C for 10 h to obtain activated precursor powder.
[0051] (6) Based on the total molar amount of transition metals, the activated precursor and sodium carbonate are mixed at a molar ratio of 1:1.03, and Nb-doped Na3Zr2Si2PO4, accounting for 2% of the total molar amount of transition metals, is added simultaneously. 12 The mixture was transferred into a ball mill jar and ball-milled at 600 r / min for 8 h to obtain a uniformly mixed powder.
[0052] (7) The mixed powder was placed in a ceramic boat, placed in a muffle furnace, heated to 850°C at 5°C / min, sintered for 12 h, and cooled with the furnace to obtain the target cathode material Na. 1.03 Li 0.02 (Ni) 0.55 Co 0.15 Mn 0.30 ) 0.98 Nb 0.02 O2@ Na3Zr 1.9 Nb 0.1 Si2PO 12 .
[0053] Comparative Example 1:
[0054] This comparative example provides a method for preparing sodium-ion cathodes by solid-phase modification of transition metal oxides from waste ternary lithium-ion batteries. Except for the transition metal oxide precursor not undergoing organic acid wet ball milling, the method is identical to that in Example 1. The resulting cathode material has the composition Na. 1.05 Li 0.02 (Ni) 0.55 Co 0.15 Mn 0.30 ) 0.98 Ti 0.02 O2@ Na3Zr 1.9 Ti 0.1 Si2PO 12 Electrochemical performance tests showed that the initial discharge specific capacity was 107.56 mAh / g, and the specific capacity retention rate after 100 cycles at 1C was 84.74%. The specific capacity and cycling performance were significantly worse than those of Example 1, demonstrating that organic acid activation plays a key role in improving interfacial bonding and cycling stability.
[0055] Comparative Example 2:
[0056] This comparative example provides a method for preparing sodium-ion cathodes by solid-phase modification of waste ternary lithium-ion battery transition metal oxides, in addition to the Na3Zr coating layer. 1.9 Ti 0.1 Si2PO 12 Without doping with high-valence elements, and otherwise identical to Example 1, the resulting cathode material has the composition of Na. 1.05 Li 0.02 Ni 0.55 Co 0.15 Mn 0.30 O2@Na3Zr2Si2PO 12 Electrochemical performance tests showed that the initial discharge specific capacity was 117.93 mAh / g, and the specific capacity retention rate after 100 cycles at 1C was 92.50%. The specific capacity and cycling performance were significantly worse than those of Example 1, demonstrating that coherent coating with high-valence elements can effectively improve the specific capacity and structural stability of the material.
Claims
1. A method for preparing sodium-ion cathodes by solid-phase modification of waste ternary lithium-ion battery transition metal oxides, characterized in that, Includes the following steps: (1) The waste ternary lithium battery positive electrode powder and ammonium sulfate are mechanically ball-milled and then mixed evenly; (2) The mixture was calcined at high temperature in a tube furnace, and after cooling, lithium salt was extracted by ultrasonic water leaching, filtered and dried to obtain transition metal oxide precursors; (3) The above transition metal oxide precursor is mixed with an organic acid solution and subjected to wet ball milling to loosen the surface atomic arrangement; (4) The wet ball milled slurry is washed with water and filtered to collect the filter cake and placed in an oven to dry, so as to obtain the activated precursor powder. (5) The activated precursor powder, sodium salt and Na3Zr2Si2PO doped with high-valence elements are combined. 12 The materials are mixed in proportion and then uniformly compounded by mechanical ball milling. (6) The uniformly mixed powder is placed in a muffle furnace for high-temperature solid-state sintering to obtain a coherent coated sodium cathode material doped with high-valence elements.
2. The method for preparing sodium-ion cathodes by solid-phase modification of waste ternary lithium-ion battery transition metal oxides as described in claim 1, characterized in that, In step (1), the mass ratio of waste ternary lithium battery cathode powder to ammonium sulfate is 1:0.5 to 1:0.9; the ball milling time is 0.5 to 6 h and the ball milling speed is 100 to 800 rpm.
3. The method for preparing sodium-ion cathodes by solid-phase modification of waste ternary lithium-ion battery transition metal oxides as described in claims 1-2, characterized in that, In step (2), the high-temperature calcination atmosphere in the tubular furnace is Ar or N2 or Ar / N2 mixture, the calcination temperature is 400~1000℃, the heating rate is 1~10℃ / min, and the calcination time is 1~10 h.
4. The method for preparing sodium-ion cathodes by solid-phase modification of waste ternary lithium-ion battery transition metal oxides as described in claims 1-3, characterized in that, In step (3), the organic acid is one or more of citric acid, malic acid, and oxalic acid in any proportion; the concentration of the organic acid solution is 0.1~2.0 mol / L, the solid-liquid ratio of the precursor powder to the organic acid solution is 1:5~1:20 g / mL; the wet ball milling time is 1~8 h, and the ball milling speed is 200~600 rpm.
5. The method for preparing sodium-ion cathodes by solid-phase modification of waste ternary lithium-ion battery transition metal oxides as described in claims 1-4, characterized in that, In step (4), the drying temperature is 60~120℃ and the drying time is 6~12 h.
6. The method for preparing sodium-ion cathode by solid-phase modification of waste ternary lithium-ion battery transition metal oxides as described in claims 1-5, characterized in that, In step (5), the sodium salt is sodium carbonate or sodium hydroxide, and the molar ratio of the activation precursor to the sodium salt is 1:0.8~1:1.2; Na3Zr2Si2PO 12 The high-valence elements doped in Na3Zr2Si2PO are any one or more of Ti, Nb, W, Ta, and Mo. 12 The amount of transition metal is 2% to 10% of the total molar amount; the ball milling time is 1 to 12 hours, and the ball milling speed is 200 to 800 rpm.
7. The method for preparing sodium-ion cathode by solid-phase modification of waste ternary lithium-ion battery transition metal oxides as described in claims 1-6, characterized in that, In step (6), the sintering temperature is 700~1000℃, the heating rate is 1~10℃ / min, and the sintering time is 8~24 h.
8. The method for preparing sodium-ion cathode by solid-phase modification of waste ternary lithium-ion battery transition metal oxides as described in claims 1-7, characterized in that, In step (6), the resulting regenerated sodium-ion ternary cathode material has the following composition: Na x Li y (Ni z Co m Mn n ) 1− a TM a O2@Na3Zr 2-b TM b Si2PO 12 , where 0.8≤x≤1.2, 0.01≤y≤0.1, z+m+n=1, 0.01≤a≤0.05, 0.1≤b≤0.2, and TM is one or more tetravalent or higher valence elements among Ti, Nb, W, Ta, and Mo.