A functional separator of zinc ion-coordinated tannic acid and bacterial cellulose and a preparation method and application thereof

By introducing tannic acid and zinc ions into the bacterial cellulose membrane to form a zinc ion coordination structure and construct a functional membrane, the problems of zinc ion transport and iodine species migration in aqueous zinc-iodine batteries are solved, thereby improving the performance and lifespan of the battery.

CN123162471APending Publication Date: 2026-11-24TANGSHAN COLLEGE
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611392731.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-09
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Aqueous zinc-iodine batteries suffer from irreversible loss of iodine species on the positive electrode side, zinc anode corrosion, and zinc dendrite growth during charging and discharging. Traditional separators cannot effectively regulate zinc ion transport and polyiodide migration, leading to decreased battery efficiency and shortened lifespan.

Method used

A functional membrane that coordinates zinc ions with tannic acid and bacterial cellulose is used. By introducing tannic acid and zinc ions into the bacterial cellulose network, hydrogen bonds and coordination structures are formed, and a three-dimensional nanofiber network is constructed. This provides zinc-loving transport and polyiodide adsorption functions. Combined with an activated carbon iodine-supported cathode and a bromine-containing composite electrolyte, the migration of zinc ions and iodine species is synergistically regulated.

Benefits of technology

It improves the battery's specific capacity, rate performance, and cycle life, reduces electrochemical polarization, enhances the uniformity of zinc ion transport, suppresses zinc dendrites and hydrogen evolution corrosion, and improves the battery's coulombic efficiency and long-term stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123162471A_ABST
    Figure CN123162471A_ABST
Patent Text Reader

Abstract

This invention relates to a functional membrane composed of zinc ion-coordinated tannic acid and bacterial cellulose, its preparation method, and its application, belonging to the technical fields of aqueous zinc-based secondary batteries, biomass nanofiber materials, and electrochemical functional membranes. The technical solution involves mixing a bacterial cellulose dispersion with tannic acid, adding a soluble zinc salt to coordinate zinc ions with the oxygen-containing groups of tannic acid, followed by alcohol-induced flocculation, vacuum filtration, compaction, and drying to obtain a self-supporting membrane with a three-dimensional nanofiber network and zinc ion coordination sites. Bacterial cellulose provides electrolyte wetting and ion transport channels, tannic acid forms hydrogen bonds with bacterial cellulose, and the zinc ion coordination sites facilitate the regulation of Zn... 2+ This invention improves battery specific capacity, rate performance, coulombic efficiency, and cycle life through the synergistic effect of membrane structure regulation, activated carbon-supported iodine cathode, and optional bromine-containing composite electrolyte. It also transfers and homogenizes ion flux at the negative electrode interface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a functional membrane composed of zinc ion-coordinated tannic acid and bacterial cellulose, its preparation method and application, belonging to the technical fields of aqueous zinc-based secondary batteries, biomass nanofiber materials and electrochemical functional membranes. Background Technology

[0002] With the rapid growth of renewable energy utilization and the demand for large-scale energy storage, aqueous zinc-based batteries, which combine safety, low cost, and environmental friendliness, have attracted widespread attention. Aqueous zinc-iodine batteries typically use metallic zinc as the negative electrode and iodine species as the positive electrode active material. They have advantages such as abundant raw material reserves, high theoretical capacity, moderate operating voltage, and intrinsic safety of aqueous electrolytes, making them promising for application in stationary energy storage and distributed energy systems.

[0003] However, aqueous zinc-iodine batteries still face several bottlenecks during charge and discharge. On one hand, iodine species on the positive electrode side readily react with iodine ions in the electrolyte to form I3+. - I5 - Soluble polyiodides migrate through conventional porous membranes towards the negative electrode under the drive of concentration gradients, leading to irreversible loss of active iodine, increased self-discharge, and decreased coulombic efficiency. Furthermore, the polyiodides migrating to the negative electrode can corrode metallic zinc and induce interface passivation. On the other hand, zinc negative electrodes in aqueous electrolytes exhibit uneven zinc deposition / stripping, dendrite growth, hydrogen evolution reaction, and corrosion side reactions, which may cause battery short circuits, capacity decay, and reduced cycle life.

[0004] As a key functional layer between the positive and negative electrodes, the separator not only needs to isolate the electrodes and prevent short circuits, but also needs to provide rapid and uniform Zn absorption. 2+ Transmission Channel. Although commonly used glass fiber membranes have certain mechanical strength and liquid absorption capacity, they are relatively thick, have uneven pore size distribution, and lack the ability to actively regulate zinc ion migration and polyiodide shuttle, making it difficult to simultaneously solve the problems of zinc anode dendrite formation, polyiodide shuttle, and slow reaction kinetics.

[0005] Bacterial nanocellulose possesses a three-dimensional nanonetwork structure, high hydrophilicity, good flexibility, renewability, and biodegradability, making it an ideal matrix for constructing green battery separators. For example, Chinese patent CN202110573180.2 discloses "A method for preparing a bacterial cellulose-based aqueous zinc-ion battery separator material," and Chinese patent application CN202411488731.5 discloses "An aqueous zinc-ion bacterial cellulose separator, its preparation method, and its application." However, single bacterial nanocellulose separators have limited surface functional sites, limiting their effectiveness against Zn. 2+The solvation structure, electric field distribution, and polyiodide immobilization effects are still insufficient. Therefore, a functional membrane that is simple to process, low in cost, scalable, and capable of synergistically regulating zinc ion transport and iodine species migration is needed. Summary of the Invention

[0006] The purpose of this invention is to provide a functional membrane for coordinating zinc ions with tannic acid and bacterial cellulose, as well as its preparation method and application. Tannic acid and zinc ions are introduced together into the bacterial cellulose network to construct a green membrane that combines structural enhancement, zinc-loving transport, and polyiodide adsorption functions. Through the synergistic effect of membrane structure regulation, activated carbon iodine-supported cathode, and optional bromine-containing composite electrolyte, the specific capacity, rate performance, coulombic efficiency, and cycle life of the battery are improved, thus solving the aforementioned technical problems existing in the background art.

[0007] The technical solution of this invention is: A method for preparing a functional membrane composed of zinc ion-coordinated tannic acid and bacterial cellulose involves mixing a bacterial cellulose dispersion with tannic acid, adding a soluble zinc salt to coordinate zinc ions with the oxygen-containing groups of tannic acid, followed by alcohol-induced flocculation, vacuum filtration, compaction, and drying to obtain a self-supporting membrane with a three-dimensional nanofiber network and zinc ion coordination sites. Bacterial cellulose provides electrolyte wetting and ion transport channels, tannic acid forms hydrogen bonds with bacterial cellulose, and the zinc ion coordination sites facilitate the regulation of Zn. 2+ This method transports and homogenizes the ion flux at the negative electrode interface. The preparation process is mild, and the raw materials are widely available. The prepared separator is suitable for aqueous zinc-iodine batteries, which exhibit low electrochemical polarization, high rate performance, and good cycle stability.

[0008] This invention includes the following steps: (1) Mix the bacterial cellulose dispersion with tannic acid and stir, so that the tannic acid is bound to the surface of the bacterial cellulose nanofiber through hydrogen bonding and physical adsorption, to obtain a mixed dispersion of tannic acid and bacterial cellulose. (2) Add soluble zinc salt to the mixed dispersion and stir to coordinate zinc ions with the phenolic hydroxyl group and the ortho-oxy group of tannic acid to form a dispersion of tannic acid and bacterial cellulose containing zinc ion coordination sites. (3) Add an alcohol precipitant to the dispersion obtained in step (2) to flocculate the solid components, and then perform vacuum filtration to form a film; (4) Compact and dry the obtained wet film to obtain a zinc ion coordinated tannic acid / bacterial cellulose functional membrane.

[0009] The bacterial cellulose dispersion has a solid content of 0.1–2.0 wt% and a mass ratio of tannic acid to bacterial cellulose dry basis of 0.8–1.2:1.

[0010] The soluble zinc salt is selected from one or more of zinc sulfate, zinc chloride, zinc acetate and zinc nitrate; the zinc salt is added in the form of an aqueous solution with a zinc ion concentration of 0.1 to 3.0 mol / L; the alcohol precipitant is ethanol, isopropanol or a mixture thereof, and the volume ratio of the alcohol precipitant to the dispersion in step (2) is 1:10 to 3:1, and the mixture is stirred for 5 to 60 min after addition.

[0011] The stirring time in step (1) is 1 to 6 hours, the stirring time in step (2) is 2 to 8 hours, and the stirring temperature is 15 to 35 ℃.

[0012] In step (3), vacuum filtration uses nylon membrane, polytetrafluoroethylene membrane or cellulose filter membrane as the support membrane; the wet membrane is dried at 40-90 ℃ for 6-24 h to obtain a self-supporting diaphragm with a thickness of 10-100 μm.

[0013] A functional membrane for zinc ion-coordinated tannic acid and bacterial cellulose prepared by the above method comprises a three-dimensional interconnected framework of bacterial cellulose nanofibers, tannic acid bound to the surface of the framework, and zinc ions coordinated with the oxygen-containing groups of the tannic acid; the membrane has interconnected channels and zinc ion coordination sites distributed on the channels and the fiber surface.

[0014] The mass ratio of tannic acid to bacterial cellulose in the diaphragm is 0.8–1.2, and the diaphragm thickness is 10–100 μm.

[0015] An application of the above-mentioned functional separator in the preparation of an aqueous zinc-iodine battery, the aqueous zinc-iodine battery comprising a zinc negative electrode, an iodine-based positive electrode, an aqueous electrolyte, and a separator disposed between the zinc negative electrode and the iodine-based positive electrode, the separator being the above-mentioned functional separator.

[0016] The iodine-based cathode comprises a conductive carbon material and an iodine-active substance, wherein the iodine-active substance is supported on the conductive carbon material by an aqueous solution containing I2 and an iodide; the iodide is selected from one or more of LiI, KI, NaI, and ZnI2; the aqueous electrolyte comprises 0.5–3.0 mol / L of a zinc salt; the zinc salt is selected from one or more of ZnSO4, ZnCl2, Zn(CF3SO3)2, and Zn(CH3COO)2; the aqueous electrolyte further comprises 0.1–2.0 mol / L of ZnBr2 to form an iodine / bromine synergistic multi-electron halogen redox system. This is used to improve Zn... 2+ One or more of the following: migration number, homogenization of zinc ion flux, promotion of uniform zinc deposition, inhibition of zinc dendrite formation, hydrogen evolution, and corrosion side reactions.

[0017] The aqueous zinc-based battery is an aqueous zinc-iodine battery, a zinc-bromine battery, a zinc-ion battery, or a zinc-air battery.

[0018] The beneficial effects of this invention are: This invention uses bacterial nanocellulose as a green and renewable matrix. The raw materials are widely available, and the process includes blending, coordination, filtration and drying. The conditions are mild and suitable for large-scale preparation.

[0019] The phenolic hydroxyl and carbonyl groups introduced by tannic acid can enhance the hydrophilicity of the membrane and provide multiple adsorption sites. Zn 2+ It forms a coordination network with tannic acid, which can construct a zinc-loving interface and enhance Zn content. 2+ Transferability.

[0020] (3) The dense and uniform three-dimensional nanofiber network of the modified membrane can shorten and homogenize the ion transport path, thereby improving the electric field on the electrode surface and the Zn 2+ The flux is more uniform, thereby inducing uniform zinc deposition and suppressing zinc dendrites, hydrogen evolution and corrosion side reactions.

[0021] (4) Compared with the unmodified BC membrane, the zinc-iodine battery using the modified membrane of this invention exhibits lower charge transfer resistance, smaller redox peak potential difference, better rate performance, and longer cycle stability. In bromine-containing composite electrolytes, the multi-electron conversion capacity can be further improved. Attached Figure Description

[0022] Figure 1 This is a scanning electron microscope image of the ZnTA50-BC diaphragm cross section in Embodiment 3 of the present invention; Figure 2 This is a scanning electron microscope image of the ZnTA50-BC diaphragm surface in Example 3 of the present invention; Figure 3 This is a Zn element distribution diagram on the surface of the ZnTA50-BC membrane in Embodiment 3 of the present invention; Figure 4 This is a scanning electron microscope image of the ZnTA50-BC-Cl diaphragm in Example 8 of the present invention; Figure 5 This is a Zn elemental distribution diagram of the ZnTA50-BC-Cl separator in Example 8 of the present invention; Figure 6 Images showing the flexibility of the ZnTA50-BC diaphragm in Example 3 of this invention; Figure 7 XRD characterization images of the BC membrane of Comparative Example 1 (Example 1) and the ZnTA50-BC membrane prepared in Example 3; Figure 8 This is a high-resolution Zn 2p spectrum of the ZnTA50-BC membrane prepared in Example 3; Figure 9 High-resolution O 1s spectra of the BC membrane prepared in Comparative Example 1 and the ZnTA50-BC membrane prepared in Example 3; Figure 10 This is a scanning electron microscope image of the BC-AC@I positive electrode in Embodiment 5 of the present invention; Figure 11 This is a diagram showing the I element distribution of the BC-AC@I cathode in Embodiment 5 of the present invention; Figure 12 Zn||Zn cycling was performed using the BC diaphragm prepared in Comparative Example 1 and the ZnTA50-BC diaphragm prepared in Example 3. Figure 13 The cyclic voltammetry curves of an aqueous zinc-iodine battery assembled with the BC separator in Comparative Example 1 and the ZnTA50-BC separator in Example 3 are shown in Example 6 of this invention. Figure 14 The electrochemical impedance spectroscopy of an aqueous zinc-iodine battery assembled with the BC separator in Comparative Example 1 and the ZnTA50-BC separator in Example 3 in Example 6 is shown. Figure 15 In Example 6 of this invention, the constant current charge-discharge curves of an aqueous zinc-iodine battery assembled with the BC separator in Comparative Example 1 and the ZnTA50-BC separator in Example 3 are shown. Figure 16 This is a rate performance diagram of an aqueous zinc-iodine battery assembled with the BC separator in Comparative Example 1 and the ZnTA50-BC separator in Example 3 in Example 6 of the present invention. Figure 17 The diagram shows the long-cycle performance of aqueous zinc-iodine batteries using different separators according to the present invention. In Example 6, the long-cycle performance of aqueous zinc-iodine batteries assembled with the BC separator in Comparative Example 1, the ZnTA40-BC separator in Example 2, the ZnTA50-BC separator in Example 3, the ZnTA60-BC separator in Example 4, and the BC-AC positive electrode separator in Example 5 is shown at a rate of 2.50 C. Figure 18 The present invention provides high-capacity cycling performance in a ZnBr2 electrolyte; in Example 7, the long-cycle performance of an aqueous zinc-iodine battery assembled with the BC membrane in Comparative Example 1 and the ZnTA50-BC membrane in Example 3 is demonstrated in a bromine-containing composite electrolyte. Figure 19 This is a physical demonstration diagram of the aqueous zinc-iodine battery-driven electronic device according to an embodiment of the present invention. Detailed Implementation

[0023] The present invention will be further described below with reference to embodiments. It should be understood that the following embodiments are for illustrative purposes only and do not constitute a limitation on the scope of protection of the present invention. Without departing from the concept of the present invention, those skilled in the art can make appropriate adjustments to the types and proportions of raw materials, stirring conditions, film formation methods, and battery structures.

[0024] In the examples, all reagents used were of analytical grade, and all operations were performed at 25±2 °C unless otherwise specified. The bacterial cellulose dispersion had a solid content of 5 mg / g, tannic acid was of analytical grade, zinc salt was ZnSO4·7H2O, and ethanol was 95 vol%.

[0025] In the preparation method of this invention, vacuum filtration allows for the control of membrane thickness by adjusting the concentration of the suspension, enabling efficient and uniform membrane preparation. Iodine-active material is loaded into the porous positive electrode using an impregnation method.

[0026] The embodiment provides a method using bacterial cellulose as the backbone, tannic acid as the functional component, and Zn as the functional component. 2+ A composite membrane with coordination centers. The preparation steps are as follows: Tannic acid was mixed with bacterial cellulose dispersion with a solid content of 0.1–2.0 wt% at a dry basis mass ratio of 0.8–1.2:1 and stirred at 15–35 °C for 1–6 h; 0.1–3.0 mol / L soluble zinc salt aqueous solution was added and stirred for 2–8 h; ethanol or isopropanol was added and stirred for 5–60 min; the mixture was vacuum filtered to form a membrane, which was then compacted and dried at 40–90 °C for 6–24 h to obtain a self-supporting membrane with a thickness of 10–100 μm.

[0027] Take 10 g of bacterial cellulose dispersion with a solid content of 5 mg / g, add 40–60 mg of tannic acid, and stir at room temperature for 3 h; add 2 mL of 2.0 mol / L ZnSO4 solution, and continue stirring for 4 h; add approximately 20 mL of 95 vol% ethanol, and stir for 30 min; filter using a nylon-66 supported membrane, and dry at 60 ℃ for 12 h to obtain a composite membrane. Hydrogen bonds form between tannic acid and bacterial cellulose, and Zn... 2+ It forms a coordination structure with phenolic oxygen groups and is dispersed in an interconnected nanofiber network.

[0028] The aqueous zinc-iodine battery of the present invention comprises a zinc negative electrode, an iodine-based positive electrode, an aqueous electrolyte, and the aforementioned separator. The iodine-based positive electrode is preferably a bacterial cellulose / activated carbon self-supporting membrane, supported by an aqueous solution containing 0.05–0.5 mol / L I₂ and 0.5–3.0 mol / L LiI. The base electrolyte is preferably 2.0 mol / L ZnSO₄, but 0.1–2.0 mol / L ZnBr₂ can also be added to form an iodine / bromine synergistic multi-electron reaction system.

[0029] Comparative Example 1 (Example 1)

[0030] Take 10 g of bacterial cellulose dispersion (containing 50 mg of bacterial cellulose dry basis), without adding tannic acid and ZnSO4 solution; add 20 mL of ethanol and stir for 30 min, then filter under vacuum. Press the wet film onto a plate, dry at 60 ℃ for 12 h, and peel off to obtain the BC diaphragm. Example 2

[0031] Take 10 g of bacterial cellulose dispersion (containing 50 mg of bacterial cellulose dry basis), add 40 mg of tannic acid, and stir at 300 r / min for 3 h; add 2 mL of 2.0 mol / L ZnSO4 solution, and continue stirring for 4 h; add 20 mL of ethanol and stir for 30 min; vacuum filter, compact and dry at 60 ℃ for 12 h to obtain ZnTA40-BC membrane. Example 3

[0032] Take 10 g of bacterial cellulose dispersion (containing 50 mg of bacterial cellulose dry basis), add 50 mg of tannic acid, and stir for 3 h; add 2 mL of 2.0 mol / L ZnSO4 solution and stir for 4 h; add 20 mL of 95 vol% ethanol and stir for 30 min. Filter the slurry onto a nylon-66 membrane, compact the wet membrane, and dry it at 60 ℃ for 12 h to obtain a ZnTA50-BC membrane with a thickness of approximately 40 μm. Example 4

[0033] Following the procedure in Example 3, the amount of tannic acid was changed to 60 mg, while the other conditions remained unchanged, to obtain a ZnTA60-BC membrane. Example 5

[0034] Bacterial cellulose and activated carbon (AC) were dispersed in water at a mass ratio of 1:4, totaling 100 mg. After stirring, the mixture was vacuum filtered and dried to form a membrane. Subsequently, an aqueous solution containing 2 M LiI and 0.2 M I2 was used as the positive electrode electrolyte, with a concentration of 5 mg I / cm. 2 The theoretical loading amount was added dropwise to the positive electrode membrane, and the membrane was sealed and left to stand for 12 h to obtain the iodine-loaded positive electrode (labeled as BC-AC@I positive electrode). Example 6

[0035] Using zinc foil as the negative electrode, and employing the BC separator from Comparative Example 1, the ZnTA40-BC separator from Example 2, the ZnTA50-BC separator from Example 3, and the ZnTA60-BC separator from Example 4, respectively, and the iodine-loaded positive electrode prepared in Example 5 as the positive electrode, and using a 2.0 mol / L ZnSO4 aqueous solution as the electrolyte, CR2025 coin-type aqueous zinc-iodine batteries were assembled. The zinc foil and separator diameters were both 16 mm, the iodine-loaded positive electrode diameter was 12 mm, and 30 μL of electrolyte was added to each battery. Example 7

[0036] Using zinc foil as the negative electrode, batteries were assembled using the BC separator from Comparative Example 1 and the ZnTA50-BC separator from Example 3, respectively, and the iodine-loaded positive electrode from Example 5. The electrolytes were changed to 2.0 mol / L ZnSO4 and 1.0 mol / L ZnBr2.- It participates in halogen conversion and stabilizes high-valent iodine species, thus extending the iodine reaction from a conventional two-electron process to a multi-electron process. Example 8

[0037] Following the procedure in Example 3, the ZnSO4 solution was replaced with 1.0 mol / L ZnCl2, while other conditions remained unchanged, to obtain the corresponding coordination membrane, which was labeled as ZnTA50-BC-Cl membrane.

[0038] Figure 1 and Figure 2 Cross-sectional and surface scanning electron microscope (SEM) images of the ZnTA50-BC diaphragm prepared in Example 3; Figure 3 The elemental mapping diagram of the energy dispersive X-ray spectroscopy (EDS) of the ZnTA50-BC membrane.

[0039] Depend on Figure 1 It can be seen that the ZnTA50-BC membrane has a continuous membrane structure with a cross-sectional thickness of approximately 40 μm. Figure 2 It is evident that the membrane retains the interwoven nanofiber network structure characteristic of bacterial cellulose, with the fibers entangled and forming numerous interconnected pores, which facilitates electrolyte wetting and ion transport. Simultaneously, the relatively tight contact between the fibers helps improve the structural integrity of the membrane and, to some extent, reduces the possibility of localized zinc deposits penetrating the membrane. Figure 3 It can be seen that zinc is evenly distributed in the tested area, and no obvious zinc-rich agglomeration areas were observed, indicating that zinc species can be relatively evenly dispersed in the tannic acid-modified bacterial cellulose network.

[0040] Figure 4 and Figure 5 The images show the surface SEM image and zinc element EDS mapping image of the ZnTA50-BC-Cl membrane prepared in Example 8.

[0041] Depend on Figure 4 It can be seen that after replacing the ZnSO4 solution with a 1.0 mol / L ZnCl2 solution, the resulting membrane still maintains the porous network structure formed by the interwoven bacterial cellulose nanofibers, without obvious fiber collapse or large-area pore blockage. Figure 5 It can be seen that the zinc element is relatively evenly distributed in the observation area, and no obvious zinc-rich agglomeration phenomenon is observed. This indicates that when ZnCl2 is used as the zinc source, the zinc element can also be relatively evenly dispersed in the tannic acid / bacterial cellulose network.

[0042] Figure 6 This is a digital photograph of the electrode membrane of the ZnTA50-BC separator prepared in Example 3. The ZnTA50-BC separator can be bent without obvious cracks or breaks, indicating that it possesses the flexibility required for battery assembly.

[0043] Figure 7 X-ray diffraction (XRD) of the BC membrane prepared in Comparative Example 1 and the ZnTA50-BC membrane prepared in Example 3.

[0044] As shown in Figure 7, the BC membrane exhibits distinct diffraction peaks at approximately 14.3°, 16.9°, and 22.9°, corresponding to the (1-10), (110), and (200) crystal planes of cellulose type I crystals, respectively, indicating that the BC framework possesses a typical cellulose type I crystal structure. The introduction of tannic acid and Zn... 2+ After coordination, the ZnTA50-BC membrane retained the characteristic diffraction peaks of cellulose and no new sharp diffraction peaks appeared, indicating that no detectable crystalline zinc-containing secondary phase was formed in the membrane. Compared with the BC membrane, the cellulose diffraction peak intensity of the ZnTA50-BC membrane decreased and showed a certain degree of peak broadening. This may be due to the introduction of amorphous tannic acid components and the interaction between tannic acid and Zn. 2+ This is due to hydrogen bonds and coordination interactions formed between the bacterial cellulose nanofibers and cellulose. The above results indicate that the functionalization treatment of this invention mainly alters the chemical environment and intermolecular interactions on the surface of bacterial cellulose nanofibers, without destroying their basic cellulose type I crystal framework.

[0045] Figure 8 This is a high-resolution Zn 2p spectrum of the ZnTA50-BC membrane prepared in Example 3; Figure 9 High-resolution O 1s spectra of the BC membrane prepared in Comparative Example 1 and the ZnTA50-BC membrane prepared in Example 3.

[0046] XPS was further used to analyze the surface elemental composition and chemical state of the membrane. Figure 8 In the high-resolution Zn 2p spectrum shown, two characteristic peaks appear at approximately 1020.6 eV and 1043.7 eV, corresponding to Zn 2p, respectively. 3 / 2 and Zn2p 1 / 2 This indicates the presence of Zn in the ZnTA50-BC membrane. 2+ Species. For example... Figure 9 As shown, the O 1s spectrum of the BC membrane is mainly composed of a component at approximately 532.1 eV, which can be attributed to CO and C-OH groups in cellulose. This was achieved through tannic acid modification and the introduction of Zn. 2+ Subsequently, the O 1s peak of the ZnTA50-BC membrane broadened and could be decomposed into a CO / C-OH component at approximately 532.1 eV and a low binding energy component at approximately 531.5 eV. The low binding energy component can be attributed to the Zn... 2+ Coordinated oxygen species.

[0047] Figure 10 and Figure 11 The images show the surface SEM image and iodine element EDS mapping of the iodine-loaded cathode (BC-AC@I cathode) in Example 5.

[0048] As shown in the figure, the interwoven BC nanofibers provide a mechanically integrated framework, while the dispersed AC particles provide conductive surfaces and porous spaces for iodine containment. The corresponding elemental distribution map shows that the iodine signal is relatively uniform within the observation area, indicating that iodine is not confined to isolated macroscopic regions.

[0049] Figure 12 Cycling curves of a Zn||Zn symmetric battery assembled from the BC separator prepared in Comparative Example 1 and the ZnTA50-BC separator prepared in Example 3 were obtained. The test current density was 1 mA / cm². 2 The deposition / stripping surface capacity is 1 mAh / cm². 2 .

[0050] The symmetric cell using the ZnTA50-BC separator maintained small and relatively stable voltage polarization throughout the 1000-hour test, without significant voltage spikes or short circuits, indicating high reversibility of the zinc deposition and stripping process. In contrast, the symmetric cell using the BC separator showed gradually increasing polarization during cycling, accompanied by significant voltage fluctuations, and its stability decreased significantly after approximately 500 hours, indicating that its zinc / electrolyte interface gradually deteriorated during repeated deposition and stripping.

[0051] The above results indicate that the oxygen-containing functional groups and Zn in the ZnTA50-BC membrane... 2+ Coordination sites can improve Zn 2+ The migration behavior within the membrane results in a more uniform ion flux reaching the zinc anode surface. This more uniform Zn... 2+ Flux can alleviate local ion depletion and concentration polarization on the negative electrode surface, reduce ion aggregation in high electric field regions, thereby inhibiting preferential nucleation and local growth of zinc at surface protrusions and reducing dendrite formation caused by this.

[0052] Figure 13 , Figure 14 , Figure 15 and Figure 16 Cyclic voltammetry, electrochemical impedance spectroscopy, constant current charge-discharge curves, and rate performance of an aqueous zinc-iodine battery assembled with the BC separator from Comparative Example 1 and the ZnTA50-BC separator from Example 3 are presented in Example 6.

[0053] Depend on Figure 13It was found that at a scan rate of 0.6 mV / s, both batteries using different separators exhibited oxidation and reduction peaks related to the reversible redox reaction of iodine species, indicating that both batteries are capable of electrochemical conversion of iodine species. Compared with the battery using the BC separator, the battery using the ZnTA50-BC separator exhibited higher oxidation and reduction peak currents, and the redox peak spacing decreased from approximately 0.31 V to approximately 0.21 V. This suggests that the use of the ZnTA50-BC separator reduced the electrochemical polarization of the battery, improving the reversibility and reaction kinetics of the iodine species conversion reaction.

[0054] Depend on Figure 14 It can be seen that the charge transfer resistance of the battery using the ZnTA50-BC separator is significantly lower than that of the battery using the BC separator. The fitted charge transfer resistance is approximately 104.1 Ω, while the charge transfer resistance of the battery using the BC separator is approximately 249.2 Ω. These results indicate that the ZnTA50-BC separator can reduce the charge transfer resistance at the electrode / electrolyte interface and promote Zn... 2+ Migration and iodine species transformation.

[0055] Depend on Figure 15 It can be seen that at a 2.50 C rate, the battery using the ZnTA50-BC separator has a more stable charge and discharge plateau with a smaller voltage gap between the charging and discharging plateaus. In contrast, the battery using the BC separator has a larger charge and discharge plateau gap and exhibits more pronounced polarization. This result indicates that the ZnTA50-BC separator can improve ion transport and interfacial reaction processes within the battery, thereby reducing voltage loss during charge and discharge.

[0056] Depend on Figure 16 It can be seen that at rates of 2.50 C, 3.75 C, 5.00 C, 6.25 C, and 7.50 C, the specific discharge capacities of the batteries using the ZnTA50-BC separator are approximately 237.9, 231.2, 223.8, 213.7, and 198.9 mAh / g, respectively. Even at the high rate of 7.50 C, the battery still maintains a high discharge capacity. In contrast, the battery using the BC separator exhibits more significant capacity decay with increasing rate, and its discharge capacity at 7.50 C decreases significantly. During the rate testing, the coulombic efficiency of the battery using the ZnTA50-BC separator is close to 100% overall, indicating that its charge-discharge reaction has high reversibility.

[0057] Figure 17Example 6 was used to assess the long-cycle performance of an aqueous zinc-iodine battery assembled with the BC separator from Comparative Example 1, the ZnTA40-BC separator from Example 2, the ZnTA50-BC separator from Example 3, the ZnTA60-BC separator from Example 4, and the BC-AC positive electrode separator from Example 5, at a rate of 2.50 C. The BC, ZnTA40-BC, ZnTA50-BC, and ZnTA60-BC separators corresponded to tannin addition amounts of 0 mg, 40 mg, 50 mg, and 60 mg, respectively.

[0058] Depend on Figure 17 It can be seen that the initial discharge specific capacity of the aqueous zinc-iodine battery using the BC separator is approximately 218 mAh / g. With increasing cycle number, its discharge specific capacity continuously decreases, dropping to approximately 185 mAh / g after about 600 cycles, indicating that tannic acid and Zn were not introduced. 2+ BC membranes with coordination structures are difficult to effectively regulate Zn² during long-term cycling. + The zinc anode interface is transported and stabilized. In contrast, batteries using ZnTA40-BC, ZnTA50-BC, and ZnTA60-BC separators all exhibited significantly improved cycle stability. After 3000 cycles at 2.50 C rate, the three types of batteries still maintained discharge specific capacities of approximately 228.9, 235.0, and 231.5 mAh / g, respectively, corresponding to capacity retention rates of approximately 97.7%, 98.7%, and 97.8%. These results indicate that the introduction of tannic acid into the bacterial cellulose separator and the formation of Zn... 2+ The coordination structure can effectively slow down battery capacity decay and significantly improve the long-term cycle stability of aqueous zinc-iodine batteries.

[0059] Among the three tannic acid addition levels, the battery using the ZnTA50-BC separator exhibited relatively high discharge specific capacity and capacity retention, indicating that when the bacterial cellulose dry basis dosage is 50 mg, a tannic acid addition of 50 mg can achieve a good balance between the number of functional sites and ion transport channels. When the tannic acid addition is 40 mg, the oxygen-containing functional groups in the separator and Zn... 2+ There are relatively few coordination sites for Zn 2+ The modulatory effects on flux and electrode interface are relatively limited. When the amount of tannic acid added is increased to 60 mg, although more oxygen-containing functional groups and coordination sites can be provided, excessive tannic acid may cover part of the fiber surface or occupy part of the pores, thus increasing the resistance to ion transport.

[0060] Therefore, 40–60 mg of tannic acid can improve the function of bacterial cellulose membranes, with 50 mg being the optimal addition amount. This result indicates that the present invention, by adjusting the amount of tannic acid added, can improve the Zn content in the membrane. 2+The number of coordination sites, pore structure, and ion transport performance are optimized to improve the capacity retention and cycle life of aqueous zinc-iodine batteries.

[0061] Figure 18 Example 7 demonstrates the long-cycle performance of an aqueous zinc-iodine battery assembled with the BC separator from Comparative Example 1 and the ZnTA50-BC separator from Example 3 in a bromine-containing composite electrolyte. The composite electrolyte consists of ZnSO4 and ZnBr2, and the test rate is 2.50 C.

[0062] Depend on Figure 18 It is known that the battery using the BC separator has a certain discharge capacity in the early stage of cycling, but the battery capacity gradually decreases with cycling and shows significant failure after about 300 cycles, indicating that the unmodified BC separator is difficult to effectively suppress polyiodide shuttle and side reactions at the zinc anode interface. In contrast, the battery using the ZnTA50-BC separator has a discharge specific capacity of about 407.8 mAh / g at 2.50 C, and the capacity remains relatively stable during 2000 cycles, with a capacity retention of about 99% after cycling. Therefore, there is a synergistic effect between the bromine-containing composite electrolyte and the ZnTA50-BC functional separator: the former is beneficial to improving the multi-electron reaction capacity and reaction reversibility of the iodine cathode, while the latter is beneficial to stabilizing the zinc anode deposition / stripping process. Together, they improve the capacity, coulombic efficiency, and long-cycle stability of aqueous zinc-iodine batteries. The above results indicate that the ZnTA50-BC functional separator of the present invention is suitable for bromine-containing aqueous zinc-iodine batteries and other halogen synergistic redox energy storage systems.

[0063] Figure 19 This is a schematic diagram of an aqueous zinc-iodine battery using the ZnTA50-BC functional separator of this invention to drive electronic devices. The aqueous zinc-iodine battery assembled with the ZnTA50-BC separator is connected to an electronic clock via wires, with the positive and negative terminals of the battery connected to the corresponding terminals of the electronic clock. Figure 19 As can be seen, the electronic clock can display the time normally, indicating that the aqueous zinc-iodine battery prepared in this invention can output stable electrical energy and drive external electronic devices.

[0064] The physical test further demonstrates that the ZnTA50-BC functional separator can maintain good electrolyte wettability, ion transport capability, and interface stability in actual battery structures, and the assembled battery has actual discharge and power supply capabilities. Compared with coin cells used only for electrochemical testing, the battery of this invention can connect to and drive low-power electronic devices, indicating its application potential in the fields of miniaturized energy storage and low-power power supply.

[0065] The above description represents the preferred embodiments of the present invention. It should be noted that those skilled in the art can make various improvements and modifications without departing from the principles of the present invention, and these improvements and modifications are also considered to be within the scope of protection of the present invention.

Claims

1. A method for the preparation of a functional separator of zinc ion-coordinated tannic acid and bacterial cellulose, characterized by: The bacterial cellulose dispersion liquid is mixed with tannic acid, a soluble zinc salt is added to coordinate zinc ions with oxygen-containing groups of the tannic acid, and then alcohol is induced to flocculate, vacuum suction filtration, compaction and drying are performed to obtain a self-supporting diaphragm with a three-dimensional nanofiber network and zinc ion coordination sites; the bacterial cellulose provides electrolyte infiltration and ion transmission channels, the tannic acid forms hydrogen bonds with the bacterial cellulose, and the zinc ion coordination sites are conducive to regulating Zn 2+ transport and uniformizing negative electrode interface ion flux.

2. The method of claim 1, wherein the functional separator is prepared by the steps of: (a) mixing zinc ion-coordinated tannic acid and bacterial cellulose; (b) adding a cross-linking agent to the mixture; (c) drying the mixture; and (d) washing the dried mixture with water. Includes the following steps: (1) Mix the bacterial cellulose dispersion with tannic acid and stir, so that the tannic acid is bound to the surface of the bacterial cellulose nanofiber through hydrogen bonding and physical adsorption, to obtain a mixed dispersion of tannic acid and bacterial cellulose. (2) Add soluble zinc salt to the mixed dispersion and stir to coordinate zinc ions with the phenolic hydroxyl group and the ortho-oxy group of tannic acid to form a dispersion of tannic acid and bacterial cellulose containing zinc ion coordination sites. (3) Add an alcohol precipitant to the dispersion obtained in step (2) to flocculate the solid components, and then perform vacuum filtration to form a film; (4) Compact and dry the obtained wet film to obtain a zinc ion coordinated tannic acid / bacterial cellulose functional membrane.

3. The method for preparing a functional membrane of zinc ion-coordinated tannic acid and bacterial cellulose according to claim 2, characterized in that: The bacterial cellulose dispersion has a solid content of 0.1–2.0 wt% and a mass ratio of tannic acid to bacterial cellulose dry basis of 0.8–1.2:

1.

4. The method for preparing a functional membrane of zinc ion-coordinated tannic acid and bacterial cellulose according to claim 2 or 3, characterized in that: The soluble zinc salt is selected from one or more of zinc sulfate, zinc chloride, zinc acetate and zinc nitrate; the zinc salt is added in the form of an aqueous solution with a zinc ion concentration of 0.1 to 3.0 mol / L; the alcohol precipitant is ethanol, isopropanol or a mixture thereof, and the volume ratio of the alcohol precipitant to the dispersion in step (2) is 1:10 to 3:1, and the mixture is stirred for 5 to 60 min after addition.

5. The method for preparing a functional membrane of zinc ion-coordinated tannic acid and bacterial cellulose according to claim 2 or 3, characterized in that: The stirring time in step (1) is 1 to 6 hours, the stirring time in step (2) is 2 to 8 hours, and the stirring temperature is 15 to 35 ℃.

6. The method for preparing a functional membrane of zinc ion-coordinated tannic acid and bacterial cellulose according to claim 2 or 3, characterized in that: In step (3), vacuum filtration uses nylon membrane, polytetrafluoroethylene membrane or cellulose filter membrane as the support membrane; the wet membrane is dried at 40-90 ℃ for 6-24 h to obtain a self-supporting diaphragm with a thickness of 10-100 μm.

7. A functional membrane prepared using the method of any one of claims 1-6, comprising zinc ion-coordinated tannic acid and bacterial cellulose, characterized in that: The membrane comprises a three-dimensional interconnected framework of bacterial cellulose nanofibers, tannic acid bound to the surface of the framework, and zinc ions coordinated with the oxygen-containing groups of the tannic acid; the membrane has interconnected channels and zinc ion coordination sites distributed on the channels and the fiber surface.

8. The functional membrane for zinc ion-coordinated tannic acid and bacterial cellulose according to claim 7, characterized in that: The mass ratio of tannic acid to bacterial cellulose in the diaphragm is 0.8–1.2, and the diaphragm thickness is 10–100 μm.

9. An application of the functional separator described in any one of claims 7-8 in the preparation of an aqueous zinc-iodine battery, characterized in that: The aqueous zinc-iodine battery includes a zinc negative electrode, an iodine-based positive electrode, an aqueous electrolyte, and a separator disposed between the zinc negative electrode and the iodine-based positive electrode, wherein the separator is the functional separator as described in any one of claims 7-8.

10. The application of the functional separator according to claim 9 in the preparation of aqueous zinc-iodine batteries, characterized in that: The iodine-based cathode comprises a conductive carbon material and an iodine-active substance, wherein the iodine-active substance is supported on the conductive carbon material by an aqueous solution containing I2 and an iodide; the iodide is selected from one or more of LiI, KI, NaI, and ZnI2; the aqueous electrolyte comprises 0.5–3.0 mol / L of a zinc salt; the zinc salt is selected from one or more of ZnSO4, ZnCl2, Zn(CF3SO3)2, and Zn(CH3COO)2; the aqueous electrolyte further comprises 0.1–2.0 mol / L of ZnBr2 to form an iodine / bromine synergistic multi-electron halogen redox system.

Citation Information

Patent Citations

  • Preparation method of bacterial cellulose-based aqueous zinc ion battery diaphragm material

    CN113270686A

  • Aqueous zinc ion bacterial cellulose diaphragm, preparation method and application

    CN119361965A