battery
By setting a bonding layer between the positive electrode layer and the porous substrate and controlling its thickness and surface roughness ratio, the problem of poor bonding caused by the carbon-coated positive electrode active material particles on the surface is solved, thereby achieving the suppression of battery resistance and the improvement of adhesion.
Patent Information
- Application Number
- CN202610655059.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2025-05-22
- Filing Date
- 2026-05-13
- Publication Date
- 2026-11-24
AI Technical Summary
When using positive electrode active material particles with a carbon coating on the surface, the poor bonding between the positive electrode and the separator leads to an increase in battery resistance.
A porous bonding layer is provided between the positive electrode layer and the porous substrate. The ratio of the thickness t of the bonding layer to the average surface roughness Sa of the positive electrode layer, Sa/t, is controlled to be less than 4.0. A composite positive electrode active material containing lithium iron phosphate or lithium manganese iron phosphate with an olivine structure is used, and vinylidene fluoride resin is used as the main component in the bonding layer.
It improves the bonding between the positive electrode layer and the separator, suppresses the increase in battery resistance, and enhances the adhesion of the battery.
Smart Images

Figure CN123162479A_ABST
Abstract
Description
Technical Field
[0001] This disclosure relates to batteries. Background Technology
[0002] Various technologies have been proposed regarding the battery disclosed in Patent Document 1.
[0003] Existing technical documents
[0004] Patent Document 1: Japanese Patent Application Publication No. 2021-197279 Summary of the Invention
[0005] A known battery comprises a positive electrode having a positive current collector and a positive electrode layer, an electrolyte layer containing a separator and an electrolyte, and a negative electrode. The positive electrode layer is a layer containing at least a positive electrode active material. Previously, techniques aimed at ensuring the bonding between the electrode and the separator have been proposed. This is because if the bonding between the electrode and the separator is poor, delamination between the electrode and the electrolyte layer can occur due to gas generation inside the battery, leading to an increase in battery resistance.
[0006] Especially when using positive electrode active material particles with a carbon coating on their surface, the adhesion between the positive electrode and the separator decreases significantly. Because carbon has a very large specific surface area, the contact between the positive electrode active material particle surface and the separator becomes a point contact due to the presence of a carbon coating on the surface of the positive electrode active material particles.
[0007] However, when using materials lacking electronic conductivity as positive electrode active materials, at least a portion of the surface of the positive electrode active material particles needs to be coated with carbon to supplement electronic conductivity. Therefore, even when using positive electrode active material particles with a carbon coating on their surface, it is desirable to ensure the bonding between the positive electrode and the separator.
[0008] This disclosure was made in view of the above-mentioned circumstances, and its main objective is to provide a battery in which the bonding between the positive electrode and the separator is excellent even when using positive electrode active material particles with a carbon coating on their surface.
[0009] <1> A battery comprises, in sequence, a positive electrode, an electrolyte layer, and a negative electrode, wherein the electrolyte layer comprises a separator and an electrolyte solution.
[0010] The positive electrode has a positive electrode layer and a positive electrode current collector.
[0011] The diaphragm has a porous substrate and a porous bonding layer located on at least one side of the porous substrate.
[0012] The bonding layer is disposed at least between the positive electrode layer and the porous substrate.
[0013] The positive electrode layer contains a composite positive electrode active material.
[0014] The composite positive electrode active material has positive electrode active material particles as positive electrode active material and carbon located on at least a portion of the surface of the positive electrode active material.
[0015] The ratio of the average surface roughness Sa on the bonding layer side of the positive electrode layer to the thickness t of the bonding layer, Sa / t, is less than 4.0.
[0016] <2> according to <1> In the battery, the positive electrode active material is at least one of lithium iron phosphate (LFP) having an olivine structure and lithium manganese iron phosphate (LMFP) having an olivine structure.
[0017] <3> according to <1> or <2> The battery, wherein the bonding layer contains vinylidene fluoride resin as the main component.
[0018] <4> according to <1> ~ <3> In any one of the battery types, the average surface roughness Sa is 1.0 μm or more and 1.5 μm or less, and the thickness t is 0.3 μm or more and 0.5 μm or less.
[0019] <5> according to <1> ~ <4> In any one of the batteries, the electrolyte is a non-aqueous electrolyte.
[0020] According to this disclosure, a battery can be provided in which the bonding between the positive electrode and the separator is excellent even when using positive electrode active material particles with a carbon coating on their surface. Attached Figure Description
[0021] Figure 1 This is a cross-sectional schematic diagram illustrating an example of the structure of the battery disclosed herein.
[0022] Explanation of reference numerals in the attached figures
[0023] 10… Positive current collector, 20… Positive electrode layer, 30… Electrolyte layer, 31… Porous substrate, 32A… Positive electrode side bonding layer, 32B… Negative electrode side bonding layer, 33… Separator, 40… Negative electrode layer, 50… Negative current collector, 100… Battery Detailed Implementation
[0024] In this disclosure, unless otherwise specified, the average particle size is the particle size at which the cumulative value of the particle size distribution of the volume reference obtained by laser diffraction-scattering particle size distribution is 50%, i.e., the median particle size (D50).
[0025] In this disclosure, a battery is provided, which sequentially comprises a positive electrode, an electrolyte layer, and a negative electrode. The electrolyte layer comprises a separator and an electrolyte solution. The positive electrode has a positive electrode layer and a positive electrode current collector. The separator has a porous substrate and a porous bonding layer located on at least one side of the porous substrate. The bonding layer is disposed at least between the positive electrode layer and the porous substrate. The positive electrode layer comprises a composite positive electrode active material. The composite positive electrode active material has positive electrode active material particles as positive electrode active material and carbon located on at least a portion of the surface of the positive electrode active material particles. The average surface roughness Sa of the bonding layer side of the positive electrode layer is less than 4.0 in the ratio Sa / t to the thickness t of the bonding layer.
[0026] This disclosure is based on the following novel insight: In a battery where a bonding layer is present on the side of the separator constituting the electrolyte layer opposite to the positive electrode layer, the bonding strength between the positive electrode layer and the electrolyte layer is improved by making the aforementioned ratio Sa / t less than 4.0. By reducing the average surface roughness Sa of the positive electrode layer and controlling the thickness t of the bonding layer, the contact area between the bonding layer and the positive electrode layer can be increased. As a result, the adhesion between the bonding layer and the positive electrode layer can be improved. Therefore, according to this disclosure, even when using positive electrode active material particles with a carbon coating on their surface, the bonding strength between the positive electrode layer and the bonding layer can be improved, thereby suppressing the increase in battery resistance. The aforementioned ratio Sa / t only needs to be less than 4.0, but can also be 2.0 or more and 3.7 or less.
[0027] Figure 1 This is a cross-sectional schematic diagram illustrating an example of the structure of the battery disclosed herein. For example... Figure 1 As shown, the battery 100 sequentially comprises a positive current collector 10, a positive electrode layer 20, an electrolyte layer 30, a negative electrode layer 40, and a negative current collector 50. The electrolyte layer 30 includes a separator 33 and an electrolyte (not shown).
[0028] In the battery 100 of this disclosure, the separator 33 has a structure in which porous bonding layers 32A and 32B are disposed on the surface of a porous substrate 31. The bonding layer 32A disposed between the positive electrode layer 20 and the porous substrate 31 has a thickness t. The thickness t and the average surface roughness Sa of the bonding layer 32A side of the positive electrode layer 20 satisfy the following formula (1).
[0029] Equation (1): Sa / t < 4.0
[0030] The positive electrode has a positive electrode layer and a positive current collector sequentially from the electrolyte layer side. The positive electrode layer can be disposed on one surface of the positive current collector or on both surfaces of the positive current collector.
[0031] The positive electrode layer contains a composite positive electrode active material, and may also contain at least one of an electrolyte, a conductive material, and a binder, depending on the requirements.
[0032] In this disclosure, the composite positive electrode active material contained in the positive electrode layer comprises: positive electrode active material particles as the positive electrode active material, and carbon located on at least a portion of the surface of the positive electrode active material particles. Here, having carbon on at least a portion of the surface means that carbon material is present on at least a portion of the surface of the positive electrode active material particles, including a state where a portion or the entire surface of the positive electrode active material particles is covered by a film (carbon coating) of carbon material. The carbon material can be either amorphous or crystalline, as long as it can improve the conductivity of the positive electrode active material particles. The coverage rate of the positive electrode active material particles based on the carbon coating is not particularly limited; for example, it can be 30% or more, or 50% or more, of the surface area of the positive electrode active material particles.
[0033] There are no particular limitations on the method of introducing carbon onto the surface of positive electrode active material particles, and known methods can be used. For example, one method is to cover the positive electrode active material particles with a predetermined organic compound, and then calcine the positive electrode active material particles covered with the organic compound in an inactive atmosphere, thereby carbonizing the organic compound.
[0034] The average particle size of the positive electrode active material can be, for example, greater than 0.5 μm or greater than 1.0 μm. The average particle size of the positive electrode active material can be less than 100 μm or less than 30 μm.
[0035] As positive electrode active materials, at least one of lithium iron phosphate (LFP) with an olivine structure and lithium manganese iron phosphate (LMFP) with an olivine structure can be used, for example. Here, having an olivine structure means having an olivine-type crystal structure. LFP and LMFP lack electronic conductivity, but can be used as excellent active materials by coating at least part of their surface with carbon.
[0036] The ratio of Mn to the total Mn and Fe in lithium manganese iron phosphate (LMFP), Mn / (Mn+Fe), can have a lower limit of 50 mol% or more and an upper limit of 90 mol% or less or 75 mol% or less.
[0037] In the battery disclosed herein, other positive electrode active materials may be used as positive electrode active materials, in addition to composite positive electrode active materials having carbon on at least a portion of the surface of the positive electrode active material particles.
[0038] The proportion of composite positive electrode active material in the positive electrode layer can be, for example, more than 20% by mass, less than 95% by mass, or less than 70% by mass.
[0039] As electrolytes, examples include solid electrolytes. Solid electrolytes can be inorganic solid electrolytes such as sulfide solid electrolytes, halide solid electrolytes, oxide solid electrolytes, and complex hydride solid electrolytes, or organic solid electrolytes such as gel electrolytes.
[0040] From an operational point of view, the solid electrolyte can be in particle form. The average particle size of the solid electrolyte is not particularly limited and can range from 1 nm to 100 μm. The proportion of solid electrolyte in the positive electrode layer can be, for example, more than 1% by mass or less than 60% by mass.
[0041] Examples of conductive materials include carbon-based conductive materials, metal particles, and conductive polymers. Examples of carbon-based conductive materials include particulate materials such as acetylene black (AB) and Ketjen black (KB), and fibrous materials such as vapor-phase carbon fiber (VGCF), carbon nanotubes (CNTs), and carbon nanofibers (CNFs). The proportion of conductive material in the positive electrode layer can be, for example, 0.1% by mass or more, or 5% by mass or less.
[0042] The positive electrode layer may contain an adhesive. Examples of adhesives include styrene-butadiene rubber (SBR), polyimide (PI), polyacrylic acid (PAA), acrylonitrile-butadiene rubber (NBR), butadiene rubber (BR), polyvinylidene fluoride (PVdF), and polytetrafluoroethylene (PTFE). The proportion of adhesive in the positive electrode layer may be, for example, 0.5% by mass or more, or 15% by mass or less.
[0043] The thickness of the positive electrode layer can be, for example, greater than 1 μm or less than 1000 μm.
[0044] The manufacturing method of the positive electrode layer is not particularly limited; for example, the following methods can be used. First, a composite positive electrode active material is mixed with a conductive material, a binder, and a solvent to prepare a slurry for the positive electrode layer. Then, by applying the slurry to a positive electrode current collector and drying it, a positive electrode layer can be formed on the positive electrode current collector. After the slurry for the positive electrode layer has dried, a pressing process can be performed to press the positive electrode layer in the thickness direction. Examples of pressing processes include rolling and flat pressing. Examples of solvents include water, N-methylpyrrolidone (NMP), butyl butyrate, and toluene.
[0045] In the battery disclosed herein, the bonding layer side surface of the positive electrode layer has an average surface roughness Sa that satisfies the above formula (1). The average surface roughness Sa is a parameter representing the average value of the absolute values of the height differences between points relative to the average surface of the surface. The value of the average surface roughness Sa on the bonding layer side of the positive electrode layer is not particularly limited as long as it satisfies the above formula (1), for example, it can be 0.8 μm or more, 1.0 μm or more, 2.0 μm or less, or 1.5 μm or less. The average surface roughness Sa can also be 1.0 μm or more and 1.5 μm or less.
[0046] The average surface roughness Sa of the positive electrode layer can be measured, for example, using a KEYENCE VHX-7000 digital microscope. Specifically, firstly, 3D images (1000x magnification) are obtained at five locations on the bonding layer side surface of the positive electrode layer, and the arithmetic mean height is calculated from each image. Next, the average value of the arithmetic mean heights at the five locations is calculated, and this value is taken as the average surface roughness Sa of the positive electrode layer. Furthermore, in the above method, the average value at the five locations on the bonding layer side surface of the positive electrode layer is set as Sa, but the number of samples used to calculate the average value is not limited to five.
[0047] The average surface roughness Sa of the positive electrode layer can be controlled, for example, by the pressing process in the above-described positive electrode layer manufacturing method. By pressing, the surface unevenness of the positive electrode layer can be reduced by increasing its density. Specific pressing conditions are not particularly limited; appropriate settings for temperature, pressure, etc., are sufficient.
[0048] Materials used as positive current collectors include, for example, SUS, Cr, Au, Pt, Zn, aluminum, copper, nickel, iron, titanium, and carbon. The thickness of the positive current collector is, for example, 0.1 μm or more and 100 μm or less. The shape of the positive current collector can be foil or plate, etc.
[0049] The negative electrode has a negative electrode layer and, if necessary, a negative electrode current collector.
[0050] The negative electrode layer is a layer containing at least a negative electrode active material. Additionally, the negative electrode layer may, as needed, contain at least one of an electrolyte, a conductive material, and a binder.
[0051] The negative electrode active material can be in the form of particles or sheets. The average particle size of the negative electrode active material can be, for example, greater than 1 μm or less than 30 μm.
[0052] The negative electrode active material may include at least one selected from carbon-based active materials, Li-based active materials, Si-based active materials, Si-C composite materials, and lithium titanate.
[0053] Carbon-based active materials may include at least one selected from graphite, soft carbon, and hard carbon. "Graphite" is a general term for both natural and artificial graphite. Li-based active materials may include, for example, Li, lithium silicates, and Li alloys. Si-based active materials may include, for example, Si, SiO, and Si alloys. Si-C composite materials refer to composite materials of carbon-based active materials (such as graphite) and Si-based active materials (such as Si).
[0054] Regarding the electrolyte, conductive material, and binder used in the negative electrode layer, the same substances as those described in the positive electrode layer can be listed.
[0055] The negative electrode layer may also contain a thickener as needed. Examples of thickeners include carboxymethyl cellulose (CMC).
[0056] Materials used as negative electrode current collectors include, for example, SUS, aluminum, copper, nickel, iron, titanium, and carbon. The thickness of the negative electrode current collector can range from, for example, 1 μm to 50 μm. The shape of the negative electrode current collector can be foil or plate, etc.
[0057] The electrolyte layer is a layer containing the membrane and electrolyte, formed between the positive electrode layer and the negative electrode layer.
[0058] The separator is impregnated with electrolyte and prevents contact between the positive and negative electrode layers. In the battery of this disclosure, the separator has a porous substrate and a porous bonding layer located on at least one side of the porous substrate. The bonding layer is disposed at least between the positive electrode layer and the porous substrate, which helps to improve the adhesion between the positive electrode layer and the electrolyte layer.
[0059] The material used as the porous substrate is not particularly limited as long as it is a porous membrane. Examples include resins such as polyethylene (PE), polypropylene (PP), polyester, polyvinyl alcohol, cellulose, and polyamide, among which polyethylene and polypropylene are also possible. Furthermore, the aforementioned membrane can be a single-layer structure or a multi-layer structure. Examples of multi-layer membranes include a two-layer PE / PP structure, or a three-layer PP / PE / PP or PE / PP / PE structure. The membrane can be made of non-woven fabrics such as resin non-woven fabric and glass fiber non-woven fabric.
[0060] The thickness of the porous substrate is not particularly limited; for example, it can be above 0.1 μm, below 1000 μm, below 500 μm, or below 100 μm.
[0061] The bonding layer may be disposed on at least one side of the porous substrate, at least between the positive electrode layer and the porous substrate. Alternatively, the bonding layer may be disposed on both sides of the porous substrate, between the positive electrode layer and the porous substrate, and between the negative electrode layer and the porous substrate (see reference). Figure 1 ).
[0062] The bonding layer has a porous structure and, like the porous substrate, can be impregnated with electrolyte. Furthermore, the bonding layer is the layer that bonds the porous substrate and the positive electrode layer. Examples of materials for the bonding layer include vinylidene fluoride-based resins. The vinylidene fluoride-based resin can also be a homopolymer of vinylidene fluoride (polyvinylidene fluoride). Alternatively, it can be a copolymer composed of vinylidene fluoride and at least one selected from tetrafluoroethylene, hexafluoropropylene, and ethylene. The molecular weight of the vinylidene fluoride-based resin is not particularly limited, but the weight-average molecular weight can be, for example, 130,000 to 500,000.
[0063] The bonding layer may also contain vinylidene fluoride-based resin as a main component. Here, "containing vinylidene fluoride-based resin as a main component" means that, when the entire bonding layer is set to 100% by mass, it contains 50% by mass or more of vinylidene fluoride-based resin. The bonding layer may contain 70% by mass or more of vinylidene fluoride-based resin, and 100% by mass of the bonding layer may also be vinylidene fluoride-based resin.
[0064] Examples of methods for forming a bonding layer with vinylidene fluoride resin as the main component include the following: First, a solution of vinylidene fluoride resin dissolved in a good solvent is coated onto the surface of a porous substrate. Then, the coated porous substrate is immersed in a coagulating solution of the vinylidene fluoride resin, allowing the resin to solidify on the surface of the porous substrate. The coating method is not particularly limited and can include spraying, dip coating, roller coating, doctor blade coating, gravure coating, and screen printing. Examples of good solvents for dissolving the vinylidene fluoride resin include N-methyl-2-pyrrolidone (NMP), N,N-dimethylacetamide, dimethyl sulfoxide, and cyclohexanone. Examples of unsuitable solvents for the coagulating solution of the vinylidene fluoride resin include those that are not suitable for the resin. Examples of unsuitable solvents include methanol, 1-hexanol and other alcohol-based solvents; ethylene glycol, tripropylene glycol and other glycol-based solvents; methyl cellosolve, ethyl cellosolve and other ether-based solvents; propylene carbonate, dimethyl carbonate and other carbonate-based solvents; decane, dodecane and other hydrocarbon-based solvents; and water. A good solvent and an unsuitable solvent can each be only one type, or a combination of two or more. Furthermore, the coagulating liquid may contain a good solvent in addition to an unsuitable solvent.
[0065] The thickness t of the bonding layer can be determined, for example, using scanning electron microscopy (SEM) images of the membrane cross-section. Specifically, in the SEM image of the membrane cross-section, the distance from the interface between the porous substrate and the bonding layer to the interface between the bonding layer and the positive or negative electrode layer (the surface of the bonding layer) is measured at multiple locations (e.g., more than 5 locations), and the calculated average value is taken as the thickness (t).
[0066] The thickness t of the bonding layer is not particularly limited as long as it satisfies the above formula (1). For example, it can be above 0.2μm, above 0.3μm, below 0.6μm, or below 0.5μm.
[0067] Non-aqueous electrolytes can be used as electrolytes. Typically, non-aqueous electrolytes containing lithium salts and non-aqueous solvents are used.
[0068] Examples of lithium salts include inorganic lithium salts such as LiPF6, LiBF4, LiClO4, and LiAsF6; and organic lithium salts such as LiCF3SO3, LiN(SO2CF3)2(Li-TFSI), LiN(SO2C2F5)2, and LiC(SO2CF3)3.
[0069] Examples of non-aqueous solvents include ethylene carbonate (EC), propylene carbonate (PC), butyl carbonate (BC), dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (EMC), γ-butyrolactone, sulfolane, acetonitrile (AcN), dimethoxymethane, 1,2-dimethoxyethane (DME), 1,3-dimethoxypropane, diethyl ether, tetraethylene glycol dimethyl ether (TEGDME), tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide (DMSO), and mixtures thereof. From the viewpoint of ensuring high dielectric constant and low viscosity, it can be a mixture of cyclic carbonate compounds such as EC, PC, and BC, which have high dielectric constant and high viscosity, and chain carbonate compounds such as DMC, DEC, and EMC, which have low dielectric constant and low viscosity; or it can be a mixture of EC and DEC.
[0070] The concentration of lithium salt in non-aqueous electrolytes can be, for example, 0.3~5M.
[0071] Non-aqueous electrolytes may contain ionic liquids. Ionic liquids may include, for example, sulfonium salts, ammonium salts, and pyridine. Salt, piperidine Salt, pyrrolidine Salt, Morpholine Salt, Salt, imidazole At least one of salts and their derivatives.
[0072] The positive electrode, electrolyte layer, and negative electrode can also be bonded by hot pressing or other heat-pressing processes as needed. For example, these layers can be bonded by performing hot pressing or other heat-pressing processes after laminating the positive electrode, electrolyte layer, and negative electrode. Specific conditions for heat pressing are not particularly limited; for example, a temperature of 50–80°C, a pressure of 1 MPa, and a heat pressing time of 90–180 seconds are also acceptable. Heat pressing can also be performed after sealing the positive electrode, electrolyte layer, negative electrode, and electrolyte solution into the laminated outer casing.
[0073] The battery disclosed herein may further include a constraint clamp that applies constraint pressure to the positive electrode layer, the electrolyte layer, and the negative electrode layer along the thickness direction. The constraint pressure may be, for example, 0.1 MPa or more, 1 MPa or more, or 5 MPa or more. Alternatively, the constraint pressure may be, for example, 100 MPa or less, 50 MPa or less, or 20 MPa or less.
[0074] The type of battery disclosed herein is not particularly limited, but is typically a lithium-ion battery. Furthermore, the battery disclosed herein can be a primary battery or a secondary battery, with a secondary battery being preferred. This is because it can be repeatedly charged and discharged, making it useful, for example, as a vehicle battery.
[0075] There are no particular limitations on the shape of the battery; for example, it can be coin-shaped, cylindrical, square, sheet-shaped, button-shaped, flat, or stacked.
[0076] In the case of a battery stack with multiple batteries stacked together, the battery stack can be either unipolar or bipolar.
[0077] Batteries are used in various applications, including as power sources for vehicles such as hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), battery electric vehicles (BEVs), gasoline vehicles, and diesel vehicles. In particular, they can be used as a power source for driving hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), or battery electric vehicles (BEVs). Furthermore, batteries can be used as a power source for mobile bodies other than vehicles (such as trains, ships, and aircraft), and also as a power source for electronic devices such as information processing equipment.
[0078] [Example]
[0079] (Example 1)
[0080] [The production of the positive electrode]
[0081] As a composite positive electrode active material, olivine-type LFP particles (average particle size 9 μm) with a carbon coating on the surface were prepared. A slurry for the positive electrode layer was prepared using the aforementioned LFP particles, CNTs (conductive materials), and PVDF (binder). The mass ratio of LFP particles:CNTs:PVDF in the positive electrode layer slurry was 94.5:1.5:4.0. The positive electrode layer slurry was coated onto an Al foil (positive electrode current collector) using a doctor blade and dried at 120°C for 10 minutes, thereby fabricating a positive electrode with a positive electrode layer on the positive electrode current collector. Subsequently, the density of the positive electrode layer and the average surface roughness Sa on the bonding layer side were adjusted by roll forming.
[0082] Using a KEYENCE VHX-7000 digital microscope, 3D images (1000x magnification) were obtained at five locations on the bonding layer side surface of the aforementioned positive electrode. The arithmetic mean height was calculated from each image. The average of the arithmetic mean heights at the five locations was calculated as the average surface roughness Sa of the bonding layer side of the positive electrode layer. The results are shown in Table 1.
[0083] [Making the negative electrode]
[0084] Artificial graphite (average particle size 22 μm) was prepared as the negative electrode active material. A slurry for the negative electrode layer was prepared using artificial graphite, SBR (binder), and CMC (thickener). The mass ratio of artificial graphite:SBR:CMC in the negative electrode layer slurry was 96:3:1. The negative electrode layer slurry was coated onto a Cu foil (negative electrode current collector) using a doctor blade and dried at 100°C for 10 minutes, thereby fabricating a negative electrode with a negative electrode layer on the negative electrode current collector. The coating amount of the negative electrode layer slurry was set to a ratio of negative electrode capacity to positive electrode capacity (negative electrode capacity / positive electrode capacity) of 1.2. Subsequently, the density of the negative electrode layer was set to 1.25 g / cm³. 3 Suppress it in this way.
[0085] [Septum fabrication]
[0086] First, polyvinylidene fluoride (PVDF) resin (weight average molecular weight 400,000) and N-methyl-2-pyrrolidone (NMP) with a solid content ratio of 7% by mass were weighed out at a ratio of 95.5% by mass and 4.5% by mass. The PVDF resin and NMP were stirred at room temperature until the PVDF resin was uniformly dissolved, thereby preparing a PVDF resin slurry.
[0087] Next, a slurry of the aforementioned polyvinylidene fluoride resin was blown onto both sides of a porous substrate (a three-layer structure of PP / PE / PP, 16 μm thick). The membrane was then impregnated in a coagulation solution (40°C) with a water / dimethylacetamide / tripropylene glycol mass ratio of 55 / 30 / 15, thereby curing the polyvinylidene fluoride resin. Subsequently, it was dried at 60°C to produce a membrane with bonding layers on both sides of the porous substrate.
[0088] The thickness of the bonding layer at five locations was measured in the SEM image of the diaphragm cross section, and the average value was taken as the bonding layer thickness (t). The results are shown in Table 1.
[0089] [Battery Manufacturing]
[0090] A battery (laminated cell) is fabricated by stacking the positive electrode, separator, and negative electrode. A 1.1M LiPF6 solution is prepared as the electrolyte and injected into the laminate. The electrolyte uses a solvent containing ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC). The volume ratio of EC:DMC:EMC in the solvent is 30:40:30. After injection, hot pressing is performed at 80°C and 1 MPa for 3 minutes to bond the separator and electrodes. The battery's constraint pressure is set to 0.5 MPa.
[0091] [Activation and Characterization Evaluation]
[0092] The activation and characteristic evaluation of each unit produced above are carried out as follows.
[0093] <Activation>
[0094] The initial charge is performed using a constant current-constant voltage method, charging at a constant current of 0.1C until 3.75V, followed by constant voltage charging for 3 hours. Afterwards, the battery is discharged at a constant current of 0.1C until 2.5V to activate the battery.
[0095] <sa t>
[0096] Sa / t was calculated based on the average surface roughness Sa of the positive electrode layer and the thickness t of the bonding layer of the separator. The results are shown in Table 1.
[0097] <Rate of resistance rise>
[0098] After activation treatment, the cells are charged at a constant current of 0.1C until the state of charge (SOC) reaches 60%. Subsequently, the 10-second IV resistance is calculated based on the cell voltage after discharging at a current of 1.5C for 10 seconds, and this value is used as the initial resistance.
[0099] The evaluation temperature was set to 40°C, and 200 cycles of 0.3C charging and 0.5C discharging were performed within a SOC range of 10%-90%. Subsequently, the 10-second IV resistance was calculated using the same method as described above and used as the resistance after the cycle test.
[0100] The rate of increase in resistance is calculated using the following formula. The results are shown in Table 1.
[0101] Resistance rise rate = (resistance after cyclic testing) / initial resistance × 100%
[0102] <Wet Adhesion Evaluation>
[0103] First, the prepared positive electrode is cut into pieces 20mm wide and 70mm long, and the prepared separator is cut into pieces 25mm wide and 80mm long. They are then overlapped with the positive electrode layer and separator bonding layer facing each other, allowing the electrolyte to penetrate. Subsequently, they are sealed with an aluminum laminate and hot-pressed at 80°C and 1MPa for 90 seconds.
[0104] For the positive electrode and separator laminate removed from the aluminum laminate, a 30mm wide × 100mm long adhesive tape (3M Scotch 600) was applied to the separator. Using a 90-degree peel strength tester (IMADA IP-5N), the force required to peel the positive electrode from the separator at a speed of 50mm / min was measured. The obtained peel strength value was taken as the wet adhesive force between the positive electrode and the separator. The results are shown in Table 1.
[0105] (Example 2)
[0106] In the above-described [cathode fabrication], the rolling conditions were changed, the average surface roughness Sa of the cathode layer was changed, and in the above-described [separator fabrication], the blowing rate of the polyvinylidene fluoride resin slurry was adjusted, and the bonding layer thickness t was changed. Otherwise, the battery was fabricated in the same manner as in Example 1, and the above-described [activation and characteristic evaluation] was performed. The results are shown in Table 1.
[0107] (Example 3)
[0108] In the above-described [cathode fabrication], the rolling conditions and the average surface roughness Sa of the cathode layer were changed. Otherwise, the battery was fabricated in the same manner as in Example 1, and the above-described [activation and characteristic evaluation] was performed. The results are shown in Table 1.
[0109] (Example 4)
[0110] In the above [cathode fabrication], as the composite cathode active material, olivine-type LMFP (average particle size 10 μm) with a carbon coating on the surface was used instead of olivine-type LFP with a carbon coating on the surface, and the rolling conditions were changed to change the average surface roughness Sa of the cathode layer. Otherwise, the battery was fabricated in the same manner as in Example 2.
[0111] In the above-described activation process, a constant current charge of 0.1C was applied during the initial charge until 4.3V was reached. Otherwise, the activation and characteristic evaluation were performed in the same manner as in Example 1. The results are shown in Table 1.
[0112] (Comparative Example 1)
[0113] In the above-described [cathode fabrication], the rolling conditions and the average surface roughness Sa of the cathode layer were changed. Otherwise, the battery was fabricated in the same manner as in Example 1, and the above-described [activation and characteristic evaluation] was performed. The results are shown in Table 1.
[0114] (Comparative Example 2)
[0115] In the above-described [cathode fabrication], the rolling conditions and the average surface roughness Sa of the cathode layer were changed. Otherwise, the battery was fabricated in the same manner as in Example 4, and the above-described [activation and characteristic evaluation] was performed. The results are shown in Table 1.
[0116] (Comparative Example 3)
[0117] In the above-described [cathode fabrication], the rolling conditions and the average surface roughness Sa of the cathode layer were changed. Otherwise, the battery was fabricated in the same manner as in Example 4, and the above-described [activation and characteristic evaluation] was performed. The results are shown in Table 1.
[0118] Table 1
[0119]
[0120] Examples 1-3 and Comparative Example 1, which used the same composite positive electrode active material (LFP with a carbon coating), were compared. The results from Examples 1-3 confirmed that even when using LFP with a carbon coating as the composite positive electrode active material, sufficient adhesion was achieved by keeping Sa / t less than 4.0, resulting in a wet adhesion force of 17-30 N / m between the positive electrode layer and the separator. In contrast, in Comparative Example 1, where Sa / t was 4.0 or higher, the wet adhesion force was only 2 N / m, a significant decrease. Furthermore, regarding the rate of increase in resistance, Examples 1-3 showed a significant improvement of 128-129% compared to 170% in Comparative Example 1.
[0121] Example 4 and Comparative Examples 2-3, which used the same composite positive electrode active material (LMFP with a carbon coating), were compared. The wet adhesion strength of Comparative Examples 2-3, with a Sa / t of 4.0 or higher, was 3-7 N / m, while that of Example 4, with a Sa / t of less than 4.0, was 18 N / m, confirming an improvement in adhesion strength. Furthermore, regarding the rate of increase in resistance, Example 4 showed a significant improvement at 145%, compared to 199-221% for Comparative Examples 2-3.
[0122] Furthermore, the average surface roughness Sa of Examples 1 to 4 is 1.0 μm or more and 1.5 μm or less, and the thickness t is 0.3 μm or more and 0.5 μm or less.< / sa>
Claims
1. A battery comprising, in sequence, a positive electrode, an electrolyte layer, and a negative electrode, wherein the electrolyte layer comprises a separator and an electrolyte solution. The positive electrode has a positive electrode layer and a positive electrode current collector. The diaphragm has a porous substrate and a porous bonding layer located on at least one side of the porous substrate. The bonding layer is disposed at least between the positive electrode layer and the porous substrate. The positive electrode layer contains a composite positive electrode active material. The composite positive electrode active material has positive electrode active material particles as positive electrode active material and carbon located on at least a portion of the surface of the positive electrode active material particles. The ratio of the average surface roughness Sa on the bonding layer side of the positive electrode layer to the thickness t of the bonding layer, Sa / t, is less than 4.
0.
2. The battery according to claim 1, wherein the positive electrode active material is at least one of lithium iron phosphate (LFP) having an olivine structure and lithium manganese iron phosphate (LMFP) having an olivine structure.
3. The battery according to claim 1, wherein the bonding layer contains a vinylidene fluoride-based resin as the main component.
4. The battery according to claim 1, wherein the average surface roughness Sa is 1.0 μm or more and 1.5 μm or less, and the thickness t is 0.3 μm or more and 0.5 μm or less.
5. The battery according to claim 1, wherein the electrolyte is a non-aqueous electrolyte.
Citation Information
Patent Citations
Power storage cell and power storage device
JP2021197279A