Secondary battery and electric device
By introducing a gas-generating layer into the positive electrode of a secondary battery, and utilizing the gas-generating agent to decompose at high temperature to generate a gas separation active material layer, the safety problems caused by thermal runaway and overcharging of secondary batteries are solved, achieving higher safety and stability.
Patent Information
- Application Number
- CN202510676718.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-23
- Publication Date
- 2026-11-24
AI Technical Summary
Secondary batteries are prone to thermal runaway under extreme conditions, leading to fire or explosion, especially large-capacity energy storage batteries which have insufficient safety performance.
A gas-generating layer containing a gas-generating agent is introduced into the positive electrode sheet. When a first temperature is reached, gas is generated to separate the positive electrode active material layer from the current collector, interrupt the charging current, reduce heat accumulation, and terminate overcharging and thermal runaway.
It improves the safety performance of secondary batteries, enabling them to reliably pass thermal runaway and overcharge tests, reducing the risk of fire and explosion, and maintaining normal battery operation.
Smart Images

Figure CN123162489A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of secondary battery technology, and in particular to a secondary battery and an electrical device. Background Technology
[0002] In recent years, rechargeable batteries have been widely used in energy storage systems for hydropower, thermal power, wind power, and solar power plants, as well as in power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace, and many other fields. With the increasing prevalence of rechargeable batteries, higher requirements have been placed on their safety performance. During use, extreme external temperatures or internal short circuits can cause a rapid rise in the internal temperature of a rechargeable battery, easily leading to the decomposition of the solid electrolyte interphase (SEI) film and the chain reaction of the electrolyte. This further accumulates heat, potentially causing thermal runaway. After thermal runaway, the battery may catch fire or even explode, seriously threatening battery safety. For large-capacity energy storage batteries that generate a lot of heat and dissipate it slowly, safety performance is an even more crucial consideration.
[0003] Therefore, there is an urgent need for a secondary battery with higher safety performance, which can reliably pass thermal runaway and overcharge tests and effectively prevent potential safety risks. Summary of the Invention
[0004] To address the aforementioned issues, this application provides a secondary battery in which the positive electrode includes a gas-generating layer. When the internal temperature of the secondary battery reaches a first temperature, the gas-generating layer decomposes to generate gas and causes the positive electrode active material layer to separate from the current collector, thereby terminating overcharging. At the same time, it reduces the amount of positive electrode active material involved in heat generation and the accumulation of battery heat, thereby reducing the risk of battery fire and explosion and improving battery safety.
[0005] A first aspect of this application provides a secondary battery, including a positive electrode, a separator, and a negative electrode, wherein the separator is disposed between the positive electrode and the negative electrode; the positive electrode includes a current collector, a gas-generating layer, and a positive active material layer, wherein the gas-generating layer is disposed between the current collector and the positive active material layer; the gas-generating layer includes a gas-generating agent, and the gas-generating layer generates gas when the positive electrode reaches a first temperature.
[0006] The secondary battery provided in this application has a gas-generating layer between the positive electrode active material layer and the current collector. The gas-generating agent in the gas-generating layer generates gas when the positive electrode reaches a first temperature. The gas accumulates between the positive electrode active material layer and the current collector, increasing the pressure between the positive electrode active material layer and the current collector. This causes part or all of the positive electrode active material layer to peel off and separate from the current collector, interrupting the charging current, increasing the polarization of the battery, and enabling the battery to quickly reach the charging cutoff voltage. At the same time, it reduces the amount of positive electrode active material involved in heat generation, reduces the degree of battery temperature rise, terminates overcharging and thermal runaway behavior, reduces the risk of battery explosion, and improves safety performance.
[0007] In any embodiment, the first temperature is at least 5°C higher than the upper limit of the operating temperature of the secondary battery. In any embodiment, the first temperature is 5°C to 100°C higher than the upper limit of the operating temperature of the secondary battery.
[0008] If the first temperature is greater than the upper limit of the operating temperature of the secondary battery within the above range, the safety performance of the battery can be improved without affecting the normal operation of the secondary battery, and the risk of battery fire and explosion can be reduced.
[0009] In any embodiment, the heat generated by the positive electrode in the differential scanning calorimetry (DSC) test does not exceed 2000 J / g. In any embodiment, the heat generated by the positive electrode in the DSC test does not exceed 50 J / g-1900 J / g.
[0010] The heat generated by the positive electrode sheet during DSC testing was within the above range, indicating that the positive electrode active material possesses high thermal and structural stability. This stability makes the active material less prone to structural collapse or violent chemical reactions under battery thermal runaway and overcharge conditions, reducing the risk of fire and explosion and improving battery safety performance.
[0011] In any embodiment, the cell capacity of the secondary battery is greater than or equal to 250Ah. In any embodiment, the cell capacity of the secondary battery is between 250Ah and 800Ah.
[0012] Rechargeable batteries with larger cell capacity can store more energy and provide a longer lifespan. Controlling the cell capacity of rechargeable batteries within the aforementioned range helps optimize charge and discharge rates, reduce internal chemical reaction losses, and extend the battery's cycle life.
[0013] In any embodiment, the secondary battery satisfies either condition 1) or 2):
[0014] 1) The secondary battery is a lithium secondary battery, and the positive electrode active material layer includes at least one of the positive electrode active material represented by Formula 1 and the positive electrode active material represented by Formula 2:
[0015] Li x1 A y1 Me a1 M b1 P 1-c1 X c1 Y z1 Formula 1
[0016] Wherein, 0.5≤x1≤1.3, 0≤y1≤1.3, and 0.7≤x1+y1≤1.3; 0.9≤a1≤1.5, 0≤b1≤0.5, and 0.9≤a1+b1≤1.5; 0≤c1≤0.5; 3≤z1≤5; A includes one or more of Na, K, and Mg; Me includes one or more of Mn, Fe, Co, and Ni; M includes one or more of B, Mg, Al, Si, P, S, Ca, Sc, Ti, V, Cr, Cu, Zn, Sr, Y, Zr, Nb, Mo, Cd, Sn, Sb, Te, Ba, Ta, W, Yb, La, and Ce; X includes one or more of S, Si, Cl, B, C, and N; Y includes one or more of O and F.
[0017] Li x2 Ni y2 Co z2 M' a2 Me' b2 O c2 A' d2 Formula 2
[0018] Wherein, 0.85≤x²≤1.15, 0≤y²<1, 0≤z²≤1, 0≤a²<1, 0≤b²≤0.1, 1.8≤c²≤2.2, 0≤d²≤1, d²+c²≤2, y²+z²+a²+b²=1, M' includes Al, Me' is selected from one or more of Mn, Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, Sr, Sb, Y, W, Nb, and A' is selected from one or more of N, F, S, Cl; or
[0019] 2) The secondary battery is a sodium secondary battery, and the positive electrode active material layer includes at least one of the following positive electrode active materials: layered metal oxide, Prussian compound, and polyanionic compound.
[0020] The aforementioned positive electrode active materials possess high energy density, good cycle life, thermal stability, and structural stability, which help reduce the risk of fire and explosion and improve battery safety performance under overcharge or overheating conditions.
[0021] In any embodiment, the gas-generating agent includes at least one selected from alkali metal bicarbonate, alkaline earth metal bicarbonate, ammonium carbonate, aluminum hydroxide, and nitrogen-containing compounds.
[0022] In any embodiment, the alkali metal bicarbonate includes at least one of potassium bicarbonate and sodium bicarbonate; the alkaline earth metal bicarbonate includes magnesium bicarbonate; and the nitrogen-containing compound includes at least one of urea, nitrosamine, and sodium azide.
[0023] The aforementioned gas-generating agents can decompose under set temperature conditions, releasing harmless gases such as carbon dioxide or ammonia. Because these gases are relatively stable and unlikely to trigger violent reactions, the batteries possess high safety and environmental friendliness. Furthermore, these gas-generating agents also exhibit extremely high stability under the operating temperature conditions of secondary batteries, beginning to decompose when the temperature reaches a set threshold, which helps improve the long-term storage stability of batteries using such gas-generating agents.
[0024] In any embodiment, 1) the secondary battery is a lithium secondary battery, and satisfies one of the following conditions a) to d).
[0025] a) The positive electrode active material includes the positive electrode active material represented by the following formula 1-1.
[0026] Li x1 Fe a1 M b1 P 1-c1 X c1 O z1 Equation 1-1
[0027] Wherein, 0.5≤x1≤1.3; 0.9≤a1≤1.5, 0≤b1≤0.5, and 0.9≤a1+b1≤1.5; 0≤c1≤0.5; 3≤z1≤5; M includes one or more of B, Mg, Al, Si, P, S, Ca, Sc, Ti, V, Cr, Cu, Zn, Sr, Y, Zr, Nb, Mo, Cd, Sn, Sb, Te, Ba, Ta, W, Yb, La, Ce; X includes one or more of S, Si, Cl, B, C, N;
[0028] b) The positive electrode active material includes the positive electrode active material represented by the following formula 1-2.
[0029] Li x1 Me a1 M b1 P 1-c1 X c1 O z1 Formula 1-2
[0030] wherein 0.5≤x1≤1.3; 0.9≤a1≤1.5, 0≤b1≤0.5, and 0.9≤a1+b1≤1.5; 0≤c1≤0.5; 3≤z1≤5; Me includes Mn and Fe; M includes one or more of B, Mg, Al, Si, P, S, Ca, Sc, Ti, V, Cr, Cu, Zn, Sr, Y, Zr, Nb, Mo, Cd, Sn, Sb, Te, Ba, Ta, W, Yb, La, and Ce; X includes one or more of S, Si, Cl, B, C, and N;
[0031] c) the positive electrode active material includes a positive electrode active material represented by Formula 2-1,
[0032] Li x2 Ni y2 Co z2 Al a2 Me' b2 O c2 A' d2 Formula 2-1
[0033] wherein 0.85≤x2≤1.15, 0≤y2<1, 0<z2≤1, 0≤a2<1, 0≤b2≤0.1, 1.8≤c2≤2.2, 0≤d2≤1, d2+c2≤2, y2+z2+a2+b2=1, Me' is selected from one or more of Mn, Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, Sr, Sb, Y, W, and Nb, and A' is selected from one or more of N, F, S, and Cl,
[0034] d) the positive electrode active material includes a positive electrode active material represented by Formula 2-2,
[0035] Li x2 Ni y2 Me' b2 O c2 A' d2 Formula 2-2
[0036] wherein 0.85≤x2≤1.15, 0<y2<1, 0≤b2≤0.1, 1.8≤c2≤2.2, 0≤d2≤1, d2+c2≤2, y2+b2=1, Me' is selected from one or more of Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, Sr, Sb, Y, W, and Nb, and A' is selected from one or more of N, F, S, and Cl; or
[0037] 2) the secondary battery is a sodium secondary battery, and satisfies one of the following conditions e) to h),
[0038] e) the positive electrode active material includes a positive electrode active material represented by Formula 3,
[0039] Na x3 M1 y3 Ni z3 Fe a3 Mn b3 O 2±δ Formula 3
[0040] wherein M1 is a metal cation different from Ni, Fe and Mn and comprises at least one selected from the group consisting of Li + , Cu 2+ , Zn 2+ , Co 2+ , Ti 4+ ; 0.67<x3<1.1; 0<y3<0.25, preferably 0.05<y3<0.15; 0<z3<0.3, preferably 0.05<z3<0.25; 0<y3+z3<0.55; 0.45<a3+b3<1; and y3+z3+a3+b3=1; 0≤δ≤0.1;
[0041] f) the positive electrode active material includes a positive electrode active material represented by the following Formula 4,
[0042] Na x4 M2[M1′(CN)6] y4 ·z4H2O Formula 4
[0043] wherein M2 is a transition metal, M1′ is a transition metal, 0<x4≤2, 0.8≤y4<1, and 0<z4≤20;
[0044] g) the positive electrode active material includes a positive electrode active material represented by the following Formula 5,
[0045] Na x5 Fe 1-y5 B1 y5 (SO4) z5 Formula 5
[0046] wherein 1.1≤x5≤1.7, 0≤y5≤0.1; and B1 includes at least one selected from the group consisting of Mn 2+ , Ni 2+ , Co 2+ , Cu 2+ , Ca 2+ , Mg 2+ , Ba 2+ , and Zn 2+ ,
[0047] h) the positive electrode active material includes a positive electrode active material represented by the following Formula 6,
[0048] Na x6 M3 y6 X1 z6(PO4) m P2O7 formula 6
[0049] Wherein, M3 includes at least one of Fe, Co, Ni, and Mn, X1 includes at least one of Al and Ti, and 1≤x6≤4, 1≤y6≤4, 0≤z6≤0.1, and 1≤m≤2.
[0050] The positive electrode active material has a stable structure, which helps to reduce the risk of fire and explosion and improve battery safety performance.
[0051] In any embodiment, the mass content of the gas-generating agent is 40%-80% based on the total mass of the gas-generating layer; optionally, the mass content of the gas-generating agent is 55%-80% based on the total mass of the gas-generating layer.
[0052] For high-capacity rechargeable batteries, the content of the gas-generating agent in the gas-generating layer within the aforementioned range is beneficial for the battery to pass thermal runaway and overcharge tests. Insufficient gas-generating agent content leads to insufficient gas generation, delaying or hindering the separation of the positive electrode active material layer and the current collector, failing to effectively prevent overcharging, and affecting battery safety. Excessive content increases the proportion of inactive materials inside the battery, reducing battery capacity or increasing manufacturing difficulty. A suitable gas-generating agent content can adequately generate gas to prevent thermal runaway and overcharging without significantly affecting battery capacity and manufacturing process.
[0053] In any embodiment, the volumetric particle size distribution Dv50 of the gas-generating agent is 0.2 μm-6 μm. In any embodiment, the volumetric particle size distribution Dv50 of the gas-generating agent is 0.2 μm-5 μm.
[0054] The volume particle size distribution Dv50 of the gas-generating agent is within the above range, which helps to reduce the coating difficulty, improve the uniformity and consistency of the gas-generating layer, and make the gas generation effect of the gas-generating agent more uniform. This allows the positive electrode active material layer to be better peeled off and separated from the current collector when the battery is overcharged or thermally runaway, thereby enhancing the battery safety performance.
[0055] In any embodiment, the thickness ratio of the gas-generating layer to the positive electrode active material layer is 1:(15-150). In any embodiment, the thickness ratio of the gas-generating layer to the positive electrode active material layer is 1:(24-150).
[0056] The ratio of the thickness of the gas-generating layer to the thickness of the positive electrode active material layer is within the above range, which is beneficial to balance the gas generation effect and the battery capacity. The battery can reliably pass the thermal runaway and overcharge tests while maintaining the overall performance of the battery.
[0057] In any embodiment, the thickness of the gas-producing layer is 0.5 μm-10 μm. In any embodiment, the thickness of the gas-producing layer is 0.5 μm-5 μm.
[0058] Within the aforementioned range, a gas-generating layer thickness is beneficial for the battery to pass thermal runaway and overcharge tests. An excessively thick gas-generating layer occupies too much battery space, reducing battery capacity; a layer that is too thin results in insufficient gas generation, failing to effectively prevent thermal runaway and overcharge. An appropriate thickness allows the battery to balance safety and capacity.
[0059] In any embodiment, the gas-generating layer includes a binder, the binder having a mass content of 5%-40% based on the total mass of the gas-generating layer.
[0060] In any embodiment, the mass ratio of the binder to the gas-generating agent in the gas-generating layer is 1:(1-20). In any embodiment, the mass ratio of the binder to the gas-generating agent in the gas-generating layer may be 1:(1-16).
[0061] An appropriate amount of binder or the ratio of binder to gas-generating agent in the gas-generating layer can enhance the adhesion between the gas-generating layer and the current collector and positive electrode material, and reduce demolding during coating or rolling.
[0062] In any embodiment, the gas-generating layer includes a conductive agent, and the mass content of the conductive agent is 10%-25% based on the total mass of the gas-generating layer. In any embodiment, the mass content of the conductive agent is 15%-25% based on the total mass of the gas-generating layer.
[0063] In any embodiment, the mass ratio of the conductive agent to the gas-generating agent in the gas-generating layer is 1:(2-10). In any embodiment, the mass ratio of the conductive agent to the gas-generating agent in the gas-generating layer is 1:(2-6).
[0064] When the mass ratio of conductive agent to gas-generating agent is within the above range, it can provide conductivity to the gas-generating layer, enabling the battery to have good electrochemical performance.
[0065] In any embodiment, the length of the secondary battery is L, the height is H, the thickness is T, and the dimensions of the secondary battery cell satisfy: 200mm≤L≤550mm, 150mm≤H≤250mm, 60mm≤T≤80mm, and 0.5≤L / H≤3, 2≤H / T≤4.
[0066] Optionally, the dimensions of the secondary battery cell satisfy the following: 160mm≤L≤300mm, 180mm≤H≤220mm, 65mm≤T≤75mm.
[0067] The size of a secondary battery cell within the above range can balance battery capacity and industrial manufacturability.
[0068] In any embodiment, based on the total mass of the gas-generating layer, the gas-generating layer comprises a positive electrode active material with a mass content of less than or equal to 5%. In any embodiment, based on the total mass of the gas-generating layer, the gas-generating layer comprises a positive electrode active material with a mass content of 0%-1%.
[0069] The trace amounts of positive electrode active material contained in the gas-generating layer are usually unavoidable in industrial preparation. They have little impact on the amount of gas-generating agent and / or conductive agent in the gas-generating layer, allowing the gas-generating layer to function normally.
[0070] In any embodiment, the positive electrode active material in the gas-generating layer is the same as the positive electrode active material in the positive electrode active material layer.
[0071] In any embodiment, the separator of the secondary battery includes a ceramic coating, which comprises inorganic ceramic particles. In any embodiment, the inorganic ceramic particles include one or more of boehmite and alumina. The separator can reduce the risk of the exposed current collector coming into contact with the negative electrode after partial or complete detachment of the positive electrode active material layer, further improving the safety of the battery after overcharging.
[0072] A second aspect of this application provides an electrical device including a secondary battery selected from the first aspect of this application. Attached Figure Description
[0073] Figure 1 This is a schematic diagram of a secondary battery according to one embodiment of this application.
[0074] Figure 2 yes Figure 1 An exploded view of a secondary battery according to one embodiment of this application is shown.
[0075] Figure 3 This is a schematic diagram of a battery module according to one embodiment of this application.
[0076] Figure 4 This is a schematic diagram of a battery pack according to one embodiment of this application.
[0077] Figure 5 yes Figure 4 An exploded view of a battery pack according to one embodiment of this application is shown.
[0078] Figure 6 This is a schematic diagram of an electrical device that uses a secondary battery as a power source according to one embodiment of this application.
[0079] Explanation of reference numerals in the attached figures:
[0080] 1 Battery pack; 2 Upper housing; 3 Lower housing; 4 Battery module; 5 Secondary battery; 51 Casing; 52 Electrode assembly; 53 Cover plate. Detailed Implementation
[0081] The embodiments of the secondary battery and power-consuming device of this application are hereby disclosed in detail with appropriate reference to the accompanying drawings. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of actually identical structures may be omitted. This is to avoid making the following description unnecessarily lengthy and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided to enable those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.
[0082] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values of 1 and 2 are listed, and if maximum range values of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0083] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.
[0084] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.
[0085] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.
[0086] Unless otherwise specified, the terms "comprising" and "including" as used in this application can be open-ended or closed-ended. For example, "comprising" and "including" can mean that other components not listed may also be included, or that only the listed components may be included.
[0087] In recent years, rechargeable batteries have been widely used in energy storage power systems such as hydropower, thermal power, wind power, and solar power plants, as well as in power tools, electric bicycles, electric motorcycles, electric cars, military equipment, aerospace, and many other fields. With the increasing prevalence of rechargeable batteries, higher requirements have been placed on their safety performance. During use, extreme external high temperatures or internal short circuits can cause a rapid rise in the internal temperature of a rechargeable battery, easily leading to the decomposition of the SEI film and the chain reaction of electrolyte breakdown. This further accumulates heat, potentially causing thermal runaway. After thermal runaway, the battery may catch fire or even explode, seriously threatening battery safety. For large-capacity energy storage batteries that generate a lot of heat and dissipate it slowly, safety performance is an even more crucial consideration.
[0088] Based on this, the first aspect of this application provides a secondary battery, including a positive electrode, a separator, and a negative electrode, wherein the separator is disposed between the positive and negative electrode. During the charging and discharging process of the battery, active ions repeatedly insert and extract between the positive and negative electrode, and the electrolyte plays a role in conducting ions between the positive and negative electrode. The separator, disposed between the positive and negative electrode, mainly serves to prevent short circuits between the positive and negative electrodes, while allowing ions to pass through.
[0089] This application provides a secondary battery in which the positive electrode includes a current collector, a gas-generating layer, and a positive electrode active material layer, wherein the gas-generating layer is disposed between the current collector and the positive electrode active material layer; the gas-generating layer includes a gas-generating agent, and the gas-generating layer generates gas when the positive electrode reaches a first temperature.
[0090] In this application, the term "first temperature" refers to the temperature at which the gas-generating agent in the gas-generating layer begins to decompose. This temperature characterizes the minimum critical value at which the electrochemical decomposition reaction occurs in the gas-generating layer.
[0091] The secondary battery provided in this application has a gas-generating layer containing a gas-generating agent between the positive electrode active material layer and the current collector. This gas-generating layer generates gas when the secondary battery reaches a first temperature. The gas accumulates between the positive electrode active material layer and the current collector, increasing the pressure between them. This causes part or all of the positive electrode active material layer to peel off from the current collector, interrupting the charging current, increasing battery polarization, and enabling the battery to quickly reach the charging cutoff voltage. Simultaneously, it reduces the amount of positive electrode active material involved in heat generation, decreasing battery heat accumulation and terminating overcharging and thermal runaway behavior, thus reducing the risk of battery fire and explosion. The secondary battery provided in this application has excellent safety performance and can reliably pass thermal runaway and overcharge tests.
[0092] In this application, the term "thermal runaway" refers to a phenomenon where the heat generated by internal chemical reactions in a battery exceeds the battery's heat dissipation capacity, causing a rapid rise in battery temperature and triggering a series of irreversible chemical reactions. As the temperature rises, these reactions accelerate, generating even more heat, creating a vicious cycle that may ultimately lead to battery fire or explosion.
[0093] In this application, the term "overcharge" refers to the act of continuing to charge a battery after the individual battery cell has reached its charging cutoff voltage. Overcharging can lead to chemical reactions and physical changes inside the battery, causing increased internal pressure, heat generation, battery deformation, and other issues, which can significantly reduce and damage battery performance.
[0094] In this application, the term "charging cut-off voltage" refers to the highest voltage a battery is allowed to reach during the charging process of a secondary battery. Exceeding this voltage may lead to overcharging, affecting the battery's safety and lifespan. Within the range below the charging cut-off voltage, a secondary battery can be considered to be in a normal operating state. Those skilled in the art can determine the "normal operating state" of a battery based on knowledge widely known in the industry. The charging cut-off voltage may differ for secondary batteries composed of different active materials or electrolytes. For commercially available secondary batteries, the charging cut-off voltage can be determined from the product instructions.
[0095] The charging cut-off voltage of a secondary battery can be measured using any method known in the art. For example, the upper limit of the charging voltage specified by the battery manufacturer can be referenced; alternatively, a freshly prepared secondary battery, a charging / discharging device, and a pressure data sampling system can be connected, and the battery can be charged at a constant current (Irc) to the rated voltage at a temperature of 20±5°C. Afterward, the voltage is increased by 0.05V-0.1V each time for constant voltage charging, and the battery status is continuously observed until the battery begins to exhibit abnormal behavior. Charging is then stopped and the device disconnected, and the charging voltage at this point is recorded as the charging cut-off voltage of the secondary battery.
[0096] In some embodiments, the first temperature is at least 5°C higher than the upper limit of the operating temperature of the secondary battery. In some embodiments, the first temperature is 5°C-100°C, 5°C-90°C, 10°C-100°C, 20°C-100°C, 30°C-100°C, 20°C-90°C, 30°C-90°C, 30°C-60°C, 5°C-60°C, 60°C-90°C, or 10°C-60°C higher than the upper limit of the operating temperature of the secondary battery.
[0097] In some embodiments, the first temperature is at least 5°C, 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, or 100°C, or it can be any value in the range of 5°C to 100°C.
[0098] In this application, the term "operating temperature of a secondary battery" refers to the temperature of the positive electrode plate inside the battery when it is charged within its normal operating voltage range. The operating temperature of a secondary battery is -20°C to 60°C. In this application, the term "upper limit of operating temperature of a secondary battery" is 60°C.
[0099] In this application, the term "normal operating voltage" refers to the voltage range exhibited by the battery during normal charging, which is typically greater than or equal to the discharge cutoff voltage and less than or equal to the charge cutoff voltage. For example, the operating voltage range of a lithium-ion battery is 3.0V to 4.2V. The operating voltage range of a sodium-ion battery is 2.0V to 4.7V.
[0100] The operating temperature of a secondary battery can be tested using any method known in the art. For example, under environmental conditions of relative humidity <60% and atmospheric pressure of 86kPa-106kPa, the secondary battery is connected to a charging / discharging device and a temperature data sampling system, and temperature sensors are arranged at multiple different locations on the positive electrode inside the battery; the rated charging current (I0) is used. rc Constant current charging is applied, with the charging cutoff voltage as the charging cutoff condition. The temperature changes of each secondary battery cell are recorded, and the temperature rise curve of each secondary battery cell is plotted. By analyzing the temperature rise curve during the charging process, the maximum temperature on the curve is recorded as the charging temperature of the secondary battery at the operating voltage.
[0101] If the first temperature is greater than the upper limit of the operating temperature of the secondary battery within the above range, the safety performance of the battery can be improved without affecting the normal operation of the secondary battery, and the risk of battery fire and explosion can be reduced.
[0102] In some embodiments, the heat generated by the positive electrode during DSC testing does not exceed 2000 J / g. In some embodiments, the heat generated by the positive electrode during DSC testing does not exceed 50 J / g-1900 J / g, 60 J / g-1900 J / g, 70 J / g-1900 J / g, or 80 J / g-1900 J / g.
[0103] In some embodiments, the heat generated by the positive electrode in the DSC test does not exceed 50 J / g, 100 J / g, 200 J / g, 400 J / g, 600 J / g, 800 J / g, 1000 J / g, 1200 J / g, 1400 J / g, 1600 J / g, 1800 J / g, or 1900 J / g, and may also be any value within the range of 50 J / g to 1900 J / g.
[0104] In this application, the term "DSC test" refers to Differential Scanning Calorimetry, a thermal analysis technique. DSC testing analyzes the thermal properties of materials by measuring the heat difference between a sample and a reference material.
[0105] In this application, the steps for DSC testing of the positive electrode sheet include: taking the positive electrode sheet and cutting it into pieces with an area greater than or equal to 15 cm². 2 For electrodes with dimensions of 3cm x 5cm or greater, differential scanning calorimetry (DSC) was used to analyze their thermal stability.
[0106] The heat generated by the positive electrode in DSC testing reflects its potential to release energy under thermal runaway conditions. Higher heat values indicate poorer thermal stability of the positive electrode active material and a greater safety risk. If the heat generated by the positive electrode in DSC testing falls within the aforementioned range, it indicates that the positive electrode active material possesses high thermal and structural stability. This stability makes it less prone to structural collapse or violent chemical reactions under battery thermal runaway and overcharge conditions, thereby reducing the risk of fire and explosion and improving battery safety performance.
[0107] In some embodiments, the cell capacity of the secondary battery is greater than or equal to 250Ah. In some embodiments, the cell capacity of the secondary battery is 250Ah-800Ah, 250Ah-600Ah, 250Ah-500Ah, or 250Ah-400Ah.
[0108] In some embodiments, the cell capacity of the secondary battery is 250Ah, 300Ah, 350Ah, 400Ah, 450Ah, 500Ah, 550Ah, 600Ah, 650Ah, 700Ah, 750Ah, or 800Ah, or any value within the range of 250Ah to 800Ah.
[0109] In this application, the term "cell capacity" refers to the maximum amount of charge that a single battery cell can store.
[0110] The cell capacity can be tested using equipment and methods known in the art. For example, at 25°C, a secondary battery with lithium iron phosphate as the active material is charged at a charging current of 0.5C until the upper limit voltage is 3.65V, and then discharged at a constant current of 0.2C until the final voltage is 2.0V. This is one charge-discharge process, and the capacity of the first discharge is the capacity of the secondary battery.
[0111] Rechargeable batteries with larger cell capacity can store more energy and provide a longer lifespan. Controlling the cell capacity of rechargeable batteries within the aforementioned range helps optimize charge and discharge rates, reduce internal chemical reaction losses, and extend the battery's cycle life.
[0112] In some embodiments, the secondary battery satisfies the following condition 1): the secondary battery is a lithium-ion battery, and the positive electrode active material includes the positive electrode active material shown in Formula 1.
[0113] Li x1 A y1 Me a1 M b1 P 1-c1 X c1 Y z1 Formula 1
[0114] Wherein, 0.5≤x1≤1.3, 0≤y1≤1.3, and 0.7≤x1+y1≤1.3; 0.9≤a1≤1.5, 0≤b1≤0.5, and 0.9≤a1+b1≤1.5; 0≤c1≤0.5; 3≤z1≤5; A includes one or more of Na, K, and Mg; Me includes one or more of Mn, Fe, Co, and Ni; M includes one or more of B, Mg, Al, Si, P, S, Ca, Sc, Ti, V, Cr, Cu, Zn, Sr, Y, Zr, Nb, Mo, Cd, Sn, Sb, Te, Ba, Ta, W, Yb, La, and Ce; X includes one or more of S, Si, Cl, B, C, and N; Y includes one or more of O and F.
[0115] In some embodiments, in the positive electrode active material shown in Formula 1, x1 is a value range of 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, or any two of these values; y1 can be selected from a value range of 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, or any two of these values; x1+y1 can be selected from a value range of 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, or any two of these values; and a1 can be selected from a value range of 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, or any two of these values. The numerical ranges are as follows: b1 can be 0, 0.1, 0.2, 0.3, 0.4, 0.5, or any two of these values; a1+b1 can be 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, or any two of these values; c1 can be 0, 0.1, 0.2, 0.3, 0.4, 0.5, or any two of these values; and z1 can be 3, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5, or any two of these values.
[0116] In some embodiments, the secondary battery is a lithium secondary battery, and the positive electrode active material includes the positive electrode active material represented by Formula 1-1.
[0117] Li x1 Fe a1 M b1 P 1-c1 X c1 O z1 Equation 1-1
[0118] Wherein, 0.5≤x1≤1.3; 0.9≤a1≤1.5, 0≤b1≤0.5, and 0.9≤a1+b1≤1.5; 0≤c1≤0.5; 3≤z1≤5; M includes one or more of B, Mg, Al, Si, P, S, Ca, Sc, Ti, V, Cr, Cu, Zn, Sr, Y, Zr, Nb, Mo, Cd, Sn, Sb, Te, Ba, Ta, W, Yb, La, Ce; X includes one or more of S, Si, Cl, B, C, N.
[0119] In some embodiments, the secondary battery is a lithium secondary battery, and the positive electrode active material includes the positive electrode active material represented by formula 1-2 below.
[0120] Li x1 Me a1 M b1 P 1-c1 X c1O z1 Formula 1-2
[0121] Wherein, 0.5≤x1≤1.3; 0.9≤a1≤1.5, 0≤b1≤0.5, and 0.9≤a1+b1≤1.5; 0≤c1≤0.5; 3≤z1≤5; Me includes Mn and Fe; M includes one or more of B, Mg, Al, Si, P, S, Ca, Sc, Ti, V, Cr, Cu, Zn, Sr, Y, Zr, Nb, Mo, Cd, Sn, Sb, Te, Ba, Ta, W, Yb, La, Ce; X includes one or more of S, Si, Cl, B, C, N.
[0122] In some embodiments, the positive electrode active material shown in Formula 1 includes, but is not limited to, one or more of lithium iron phosphate, lithium manganese phosphate, lithium manganese iron phosphate, and their respective doped modified materials, coated modified materials, and composite modified materials.
[0123] In some embodiments, the secondary battery satisfies the following condition 1): the secondary battery is a lithium-ion battery, and the positive electrode active material includes the positive electrode active material shown in Formula 2.
[0124] Li x2 Ni y2 Co z2 M' a2 Me' b2 O c2 A' d2 Formula 2
[0125] Wherein, 0.85≤x2≤1.15, 0≤y2<1, 0≤z2≤1, 0≤a2<1, 0≤b2≤0.1, 1.8≤c2≤2.2, 0≤d2≤1, d2+c2≤2, y2+z2+a2+b2=1, M' includes Al, Me' is selected from one or more of Mn, Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, Sr, Sb, Y, W, Nb, and A' is selected from one or more of N, F, S, Cl.
[0126] In some embodiments, in the positive electrode active material represented by Formula 2, x2 may be 0.85, 0.9, 1, 1.1, 1.15 or a range between any two of them, y2 may be 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1 or a range between any two of them, z2 may be 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1 or a range between any two of them, a2 may be 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9 or a range between any two of them, b2 may be 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1 or a range between any two of them, c2 may be 1.8, 1.9, 2.0, 2.1, 2.2 or a range between any two of them, d2 may be 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1 or a range between any two of them, and d2+c2 may be 1.8, 1.9, 2 or a range between any two of them.
[0127] In some embodiments, the secondary battery is a lithium secondary battery, and the positive electrode active material includes a positive electrode active material represented by the following Formula 2-1:
[0128] Li x2 Ni y2 Co z2 Al a2 Me' b2 O c2 A' d2 Formula 2-1
[0129] where 0.85≤x2≤1.15, 0≤y2<1, 0<z2≤1, 0≤a2<1, 0≤b2≤0.1, 1.8≤c2≤2.2, 0≤d2≤1, d2+c2≤2, and y2+z2+a2+b2=1; Me' is selected from one or more of Mn, Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, Sr, Sb, Y, W, and Nb; and A' is selected from one or more of N, F, S, and Cl.
[0130] In some embodiments, the positive electrode active material includes a positive electrode active material represented by the following Formula 2-2:
[0131] Li x2 Ni y2 Me' b2 O c2 A' d2 Formula 2-2
[0132] wherein 0.85≤x2≤1.15, 0<y2<1, 0≤b2≤0.1, 1.8≤c2≤2.2, 0≤d2≤1, d2+c2≤2, y2+b2=1, Me' is selected from one or more of Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, Sr, Sb, Y, W and Nb, and A' is selected from one or more of N, F, S and Cl.
[0133] In some embodiments, the positive active material represented by Formula 2 includes but is not limited to at least one of lithium cobalt oxide (LiCoO2), lithium nickel oxide (e.g., LiNiO2), lithium manganese oxide (LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel manganese cobalt oxide (LiNi 0.85 Mn 0.1 Co 0.05 O2, LiNi 0.5 Mn 0.2 Co 0.3 O2), lithium nickel cobalt aluminum oxide (LiNi 0.85 Co 0.15 Al 0.05 O2) and modified compounds thereof.
[0134] In some embodiments, the secondary battery satisfies the following condition 2): the secondary battery is a sodium-ion battery, and the positive active material includes at least one of layered metal oxides, Prussian blue analogues, and polyanionic compounds.
[0135] In some embodiments, the secondary battery is a sodium secondary battery, and the positive active material includes a positive active material represented by the following Formula 3:
[0136] Na x3 M1 y3 Ni z3 Fe a3 Mn b3 O 2±δ Formula 3
[0137] wherein M1 is a metal cation different from Ni, Fe and Mn, and includes at least one selected from Li + , Cu 2+ , Zn 2+ , Co 2+ , Ti 4+ ; 0.67<x3<1.1; 0<y3<0.25, optionally 0.05<y3<0.15; 0<z3<0.3, optionally 0.05<z3<0.25; 0<y3+z3<0.55; 0.45<a3+b3<1; and y3+z3+a3+b3=1; 0≤δ≤0.1.
[0138] In some embodiments, the secondary battery is a sodium secondary battery, and the positive electrode active material includes the positive electrode active material represented by Formula 4 below.
[0139] Na x4 M2[M1′(CN)6] y4 ·z4H2O formula 4
[0140] Where M2 is a transition metal, M1′ is a transition metal, and 0 <x4≤2,0.8≤y4<1,0<z4≤20。
[0141] In some embodiments, the secondary battery is a sodium secondary battery, and the positive electrode active material includes the positive electrode active material represented by Formula 5 below.
[0142] Na x5 Fe 1-y5 B1 y5 (SO4) z5 Formula 5
[0143] Wherein, 1.1≤x5≤1.7, 0≤y5≤0.1; B1 includes those selected from Mn 2+ Ni 2+ Co 2+ Cu 2+ Ca 2+ Mg 2+ Ba 2+ and Zn 2+ At least one of them.
[0144] In some embodiments, the secondary battery is a sodium secondary battery, and the positive electrode active material includes the positive electrode active material represented by Formula 6 below.
[0145] Na x6 M3 y6 X1 z6 (PO4) m P2O7 formula 6
[0146] Wherein, M3 includes at least one of Fe, Co, Ni, and Mn, X1 includes at least one of Al and Ti, and 1≤x6≤4, 1≤y6≤4, 0≤z6≤0.1, and 1≤m≤2.
[0147] In the aforementioned secondary battery, the positive electrode active material has a stable structure and high thermal stability, which helps to further improve the safety of the secondary battery.
[0148] In some embodiments, the gas-generating agent comprises at least one selected from alkali metal bicarbonates, alkaline earth metal bicarbonates, ammonium carbonate, aluminum hydroxide, and nitrogen-containing compounds. In some embodiments, the alkali metal bicarbonate comprises at least one selected from potassium bicarbonate and sodium bicarbonate. In some embodiments, the alkaline earth metal bicarbonate comprises magnesium bicarbonate. In some embodiments, the nitrogen-containing compound comprises at least one selected from urea, nitrosamine, and sodium azide.
[0149] In this application, nitrogen-containing compounds refer to organic or inorganic compounds whose molecules contain nitrogen.
[0150] The aforementioned gas-generating agents can decompose under set temperature conditions, releasing harmless gases such as carbon dioxide or ammonia. Because these gases are relatively stable and unlikely to trigger violent reactions, the batteries possess high safety and environmental friendliness. Furthermore, these gas-generating agents also exhibit extremely high stability at room temperature, beginning to decompose when the temperature reaches a set threshold, which helps improve the long-term storage stability of batteries containing such gas-generating agents.
[0151] In some embodiments, the mass content of the gas-generating agent is 40%-80% based on the total mass of the gas-generating layer.
[0152] In some embodiments, the mass content of the gas-generating agent is 50%-80%, 55%-80%, 50%-70%, or 55%-65% based on the total mass of the gas-generating layer.
[0153] In some embodiments, the mass content of the gas-generating agent is 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, or 80% based on the total mass of the gas-generating layer, and it can also be any value in the range of 40%-80%.
[0154] For rechargeable batteries, especially high-capacity batteries, if the mass content of the gas-generating agent in the gas-generating layer is too low, it may lead to insufficient gas generation, delaying or making it difficult for the positive electrode active material layer and the current collector to separate, thus failing to prevent overcharging. If the mass content of the gas-generating agent in the gas-generating layer is too high, it may increase the proportion of inactive materials inside the battery, reducing the battery capacity or increasing the difficulty of battery manufacturing. A mass content of the gas-generating agent within the aforementioned range can balance battery capacity and safety.
[0155] In some embodiments, the volumetric particle size distribution Dv50 of the gas-generating agent is 0.2 μm-6 μm. In some embodiments, the volumetric particle size distribution Dv50 of the gas-generating agent is 0.2 μm-5.5 μm, 0.2 μm-5 μm, 0.2 μm-4.5 μm, 0.2 μm-3.5 μm, 0.5 μm-4 μm, 1 μm-5 μm, or 2 μm-5 μm.
[0156] In some embodiments, the volumetric particle size distribution Dv50 of the gas-generating agent is 0.2 μm, 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, 5.5 μm, or 6 μm, or it can be any value in the range of 0.2 μm to 6 μm.
[0157] The volumetric particle size distribution Dv50 of the gas-generating agent is within the above range, which helps to maintain the rheological properties of the slurry, reduce the gelation phenomenon caused by excessive particle aggregation during the preparation of the gas-generating layer slurry, reduce the coating difficulty, improve the uniformity and consistency of the gas-generating layer, and make the gas generation effect of the gas-generating agent more uniform. Thus, in the event of battery overcharging or thermal runaway, the active material layer can be better peeled off and separated from the current collector, thereby enhancing the battery safety performance.
[0158] The volumetric particle size distribution (Dv50) of the gas-generating agent in the secondary battery gas-generating layer has a meaning known in the art and can be tested using methods known in the art, such as a Malvern laser particle size analyzer. As an example, the Dv50 of the particles can be tested using a Mastersizer 2000E laser particle size analyzer according to the test standard GB / T19077-2016.
[0159] In some implementations, the gas-generating agent in the gas-generating layer of the secondary battery can be processed by: disassembling the battery, removing the positive electrode and cutting it open to expose the gas-generating layer, measuring the particle size of the gas-generating agent particles using a scanning electron microscope (SEM), and performing statistical calculations.
[0160] In some embodiments, the thickness ratio of the gas-generating layer to the positive electrode active material layer is 1:(15-150). In some embodiments, the thickness ratio of the gas-generating layer to the positive electrode active material layer is 1:(15-30), 1:(15-90), 1:(25-150), 1:(20-30), 1:(15-100), 1:(20-50), or 1:(15-50).
[0161] In some embodiments, the thickness ratio of the gas-generating layer to the positive electrode active material layer is 1:15, 1:20, 1:25, 1:30, 1:40, 1:50, 1:60, 1:70, 1:80, 1:90, 1:100, 1:110, 1:120, 1:130, 1:140, 1:150, or any value range between the two.
[0162] The ratio of the thickness of the gas-generating layer to the thickness of the positive electrode active material layer is within the above range, which is beneficial to balance the gas generation effect and the battery capacity. This allows the battery to reliably pass thermal runaway and overcharge tests while maintaining the overall performance of the battery.
[0163] In some embodiments, the thickness of the gas-generating layer is 0.5 μm-10 μm. In some embodiments, the thickness of the gas-generating layer is 1 μm-10 μm, 2 μm-10 μm, 5 μm-10 μm, 2 μm-8 μm, 2 μm-6 μm, 0.5 μm-1 μm, or 0.5 μm-5 μm.
[0164] In some embodiments, the thickness of the gas-generating layer is 0.5μm, 1μm, 1.5μm, 2μm, 2.5μm, 3μm, 3.5μm, 4μm, 4.5μm, 5μm, 5.5μm, 6μm, 6.5μm, 7μm, 7.5μm, 8μm, 8.5μm, 9μm, 9.5μm, or 10μm, or it can be any value within the range of 0.5μm to 10μm.
[0165] Excessive thickness of the gas-generating layer may cause inactive materials to occupy too much space inside the battery, affecting battery capacity and potentially impacting the cell winding process during battery manufacturing. Conversely, insufficient gas generation may prevent the active material layer from separating from the current collector, failing to stop overcharging. A gas-generating layer thickness within the specified range can improve the gas generation effect of the gas-generating agent without significantly affecting battery capacity. This promotes the separation of the active material layer from the current collector, interrupts the charging current, increases battery polarization, and allows the battery to quickly reach the charging cutoff voltage. Simultaneously, it reduces the amount of positive electrode active material involved in heat generation and the accumulation of battery heat, thus stopping overcharging and thermal runaway.
[0166] The thickness of the gas-generating layer in a secondary battery can be determined by methods known in the art. As an example, the battery is disassembled, the positive electrode is removed, the electrode is cut to expose the gas-generating layer and the active material layer, and the thickness of the gas-generating layer and the positive electrode active material layer in the positive electrode is measured using a scanning electron microscope (SEM).
[0167] In some embodiments, the gas-generating layer includes a binder, and the binder content is 5%-40% by mass based on the total mass of the gas-generating layer. In some embodiments, the gas-generating layer includes a binder, and the binder content is 5%-35%, 5%-30%, 5%-25%, 5%-20%, 15%-30%, or 15%-25% by mass based on the total mass of the gas-generating layer.
[0168] In some embodiments, the gas-generating layer includes a binder, the mass content of which is 5%, 10%, 15%, 20%, 25%, 30%, 35%, or 40% based on the total mass of the gas-generating layer, or any value within the range of 5% to 40%.
[0169] When the mass content of the binder in the gas-generating layer is within the above range, it helps to improve the adhesion between the gas-generating layer and the current collector, as well as the adhesion between the gas-generating layer and the positive electrode active material layer, and reduces the demolding phenomenon of the gas-generating layer during coating or electrode rolling.
[0170] In some embodiments, the ratio of the binder to the gas-generating agent in the gas-generating layer is 1:(1-20). In some embodiments, the ratio of the binder to the gas-generating agent in the gas-generating layer is 1:(1-16), 1:(2-16), 1:(2.5-16), 1:(1-15), or 1:(2-15).
[0171] In some embodiments, the ratio of the binder to the gas-generating agent in the gas-generating layer is 1:1, 1:1.5, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, 1:16, or any range between the two.
[0172] The ratio of binder to gas-generating agent in the gas-generating layer within the above range is beneficial to enhance the adhesion between the gas-generating layer and the current collector and the positive electrode active material, and prevent demolding during coating or rolling.
[0173] In some embodiments, the gas-generating layer includes a conductive agent, and the conductive agent has a mass content of 10%-25% based on the total mass of the gas-generating layer. In some embodiments, the gas-generating layer includes a conductive agent, and the conductive agent has a mass content of 15%-25% or 15%-20% based on the total mass of the gas-generating layer.
[0174] In some embodiments, the gas-generating layer includes a conductive agent, and the mass content of the conductive agent is 10%, 15%, 20%, or 25% based on the total mass of the gas-generating layer, or it can be any value in the range of 10% to 25%.
[0175] In the gas-generating layer, by controlling the mass content of the conductive agent within the above range, the conductivity of the gas-generating layer can be improved. This allows the gas-generating agent to generate gas sufficiently while ensuring good electrical performance of the battery, thereby improving the battery's safety performance.
[0176] In some embodiments, the ratio of the conductive agent to the gas-generating agent in the gas-generating layer is 1:(2-10). In some embodiments, the ratio of the conductive agent to the gas-generating agent in the gas-generating layer is 1:(2-6), 1:(2.2-6), or 1:(2-5.5).
[0177] In some embodiments, the ratio of the gas-generating agent to the conductive agent in the gas-generating layer is 2:1, 2.5:1, 3:1, 3.5:1, 4:1, 4.5:1, 5:1, 5.5:1, 6:1, 6.5:1, 7:1, 7.5:1, 8:1, 8.5:1, 9:1, 9.5:1, or 10:1, or any numerical range between the two aforementioned ratios.
[0178] When the ratio of the conductive agent to the gas-generating agent in the gas-generating layer is within the above range, the conductivity of the gas-generating layer can be improved, and the gas-generating agent can fully generate gas while the battery has good electrochemical performance, thereby improving the safety performance of the battery.
[0179] The mass content of gas-generating agent, conductive agent, or binder in the gas-generating layer of a secondary battery can be determined using methods known in the art. For example, the mass content of gas-generating agent, conductive agent, or binder in the gas-generating layer can be determined by disassembling the battery, removing the positive electrode, and using thermogravimetric-mass spectrometry (TG-MS).
[0180] In some embodiments, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0181] In some embodiments, the adhesive includes at least one selected from polyacrylate, polyacrylonitrile, polyvinylidene fluoride, and polytetrafluoroethylene.
[0182] In some embodiments, the secondary battery has a length of L, a height of H, and a thickness of T. The dimensions of the secondary battery cell satisfy the following: 150mm≤L≤550mm, 150mm≤H≤250mm, 60mm≤T≤80mm, and 0.5≤L / H≤3, 2≤H / T≤4.
[0183] In some embodiments, the secondary battery has a length of L, a height of H, and a thickness of T, and the dimensions of the secondary battery cell satisfy the following: 160mm≤L≤300mm, 180mm≤H≤220mm, and 65mm≤T≤75mm.
[0184] In some embodiments, the length L of the secondary battery is 150mm, 175mm, 200mm, 225mm, 250mm, 275mm, 300mm, 325mm, 350mm, 375mm, 400mm, 425mm, 450mm, 475mm, 500mm, 525mm, or 550mm, or any value within the range of 150mm-550mm.
[0185] In some embodiments, the height H of the secondary battery is 150mm, 175mm, 200mm, 225mm or 250mm, or any value within the range of 150mm-250mm.
[0186] In some embodiments, the thickness T of the secondary battery is 60mm, 65mm, 70mm, 75mm or 80mm, or any value within the range of 60mm-80mm.
[0187] In some implementations, L / H is 0.5, 1, 1.5, 2, 2.5 or 3, or any value between 0.5 and 3.
[0188] In some implementations, H / T is 2, 2.5, 3, 3.5 or 4, or it can be any value between 2 and 4.
[0189] The size of a secondary battery cell within the above range can balance battery capacity and industrial manufacturability.
[0190] In some embodiments, based on the total mass of the gas-generating layer, the gas-generating layer includes a positive electrode active material with a mass content of less than or equal to 5%. In some embodiments, the gas-generating layer includes a positive electrode active material with a mass content of 0%-1%. In some embodiments, the positive electrode active material in the gas-generating layer and the positive electrode active material layer is the same.
[0191] The trace amounts of positive electrode active material contained in the gas-generating layer are usually unavoidable in industrial preparation. They have little impact on the amount of gas-generating agent and / or conductive agent in the gas-generating layer, and can enable the gas-generating layer to play its normal role in improving the safety of secondary batteries.
[0192] In some embodiments, the gas-generating layer does not contain positive electrode active material, or contains trace amounts of positive electrode active material that are unavoidably introduced during production.
[0193] In some embodiments, the current collector has two surfaces opposite each other in its own thickness direction, and the gas generation layer is only disposed on one surface of the current collector close to the positive electrode active material layer.
[0194] In some embodiments, the current collector has two surfaces opposite each other in its own thickness direction, and the gas generation layer is disposed on the two opposite surfaces of the current collector.
[0195] In some embodiments, the current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0196] In some embodiments, the positive electrode sheet can be prepared by: dispersing the components used to prepare the gas-generating layer of the positive electrode sheet, such as gas-generating agent, conductive agent, binder and any other components, in a solvent (e.g., N-methylpyrrolidone) to form a gas-generating layer slurry; coating the gas-generating layer slurry onto the positive electrode current collector, and obtaining the gas-generating layer after drying and other processes; then dispersing the components used to prepare the positive electrode active material layer, such as positive electrode active material, conductive agent, binder and any other components, in a solvent (e.g., N-methylpyrrolidone) to form a positive electrode slurry; coating the positive electrode slurry onto the gas-generating layer, and obtaining the positive electrode sheet after drying, cold pressing and other processes.
[0197] [Negative electrode plate]
[0198] The negative electrode sheet includes a negative current collector and a negative electrode film layer disposed on at least one surface of the negative current collector, the negative electrode film layer including a negative electrode active material.
[0199] As an example, the negative electrode current collector has two surfaces opposite each other in its own thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.
[0200] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0201] In some embodiments, the negative electrode active material may be a negative electrode active material known in the art for use in batteries. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxide compounds, and tin alloys. However, this application is not limited to these materials, and other conventional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0202] In some embodiments, the negative electrode film layer may optionally include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).
[0203] In some embodiments, the negative electrode film may optionally include a conductive agent. The conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0204] In some embodiments, the negative electrode film may optionally include other additives, such as thickeners (e.g., sodium carboxymethyl cellulose (CMC-Na)).
[0205] In some embodiments, the negative electrode sheet can be prepared by dispersing the components used to prepare the negative electrode sheet, such as the negative electrode active material, conductive agent, binder and any other components, in a solvent (e.g., deionized water) to form a negative electrode slurry; coating the negative electrode slurry onto the negative electrode current collector, and then obtaining the negative electrode sheet after drying, cold pressing and other processes.
[0206] [Electrolytes]
[0207] The electrolyte acts as a conductor of ions between the positive and negative electrodes. This application does not impose specific restrictions on the type of electrolyte; it can be selected according to requirements. For example, the electrolyte can be liquid, gel, or entirely solid.
[0208] In some embodiments, the electrolyte is an electrolyte solution. The electrolyte solution includes an electrolyte salt and a solvent.
[0209] In some embodiments, the secondary battery is a lithium secondary battery, and the electrolyte salt is selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalate borate, lithium dioxalate borate, lithium difluorodioxalate phosphate, and lithium tetrafluorooxalate phosphate; the solvent is selected from at least one of ethylene carbonate, propylene carbonate, methyl ethyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butyl carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, sulfolane, dimethyl sulfone, methyl ethyl sulfone, and diethyl sulfone.
[0210] In some embodiments, the secondary battery is a sodium secondary battery, and the electrolyte salt can be selected from NaNO3, NaPF6, NaBF4, or NaClO4. - The solvent is at least one of NaBOB, NaDFOB, NaSbF6, NaAsF6, NaN(SO2CF3)2, NaN(SO2C2F5)2, NaC(SO2CF3)3, and NaN(SO2F)2; the solvent is a non-aqueous solvent or an ether solvent. In some embodiments, the ether solvent is selected from one or more of ethylene glycol dimethyl ether, ethylene glycol diethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, diethylene glycol diethyl ether, 1,3-dioxolane, tetrahydrofuran, methyltetrahydrofuran, diphenyl ether, and crown ether. In some embodiments, the non-aqueous solvent may be selected from at least one of ethylene carbonate, propylene carbonate, methyl ethyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butyl carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, sulfolane, dimethyl sulfone, methyl ethyl sulfone, and diethyl sulfone.
[0211] In some embodiments, the electrolyte may optionally include additives. For example, additives may include negative electrode film-forming additives, positive electrode film-forming additives, and may also include additives that can improve certain battery performance, such as additives that improve battery overcharge performance, additives that improve battery high-temperature or low-temperature performance, etc.
[0212] [Isolation Component]
[0213] In some embodiments, the secondary battery also includes a separator. This application does not impose any particular limitation on the type of separator; any known porous separator with good chemical and mechanical stability can be selected.
[0214] In some embodiments, the material of the separator can be selected from at least one of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0215] In some embodiments, the separator includes a ceramic coating comprising inorganic ceramic particles.
[0216] In some embodiments, the inorganic ceramic particles include one or more of boehmite and alumina.
[0217] The aforementioned inorganic materials all possess excellent thermal stability, which helps reduce the thermal shrinkage rate of the separator, lowers the risk of the exposed current collector coming into contact with the negative electrode after partial or complete detachment of the positive electrode active material layer, and further improves the safety risk after battery overcharging. In some embodiments, the positive electrode, negative electrode, and separator can be fabricated into an electrode assembly using a winding or stacking process.
[0218] In some embodiments, the secondary battery may include an outer packaging. This outer packaging may be used to encapsulate the electrode assembly and electrolyte described above.
[0219] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. The outer packaging of the secondary battery can also be a soft pack, such as a pouch. The material of the soft pack can be plastic; examples of plastics include polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0220] This application does not impose any particular limitation on the shape of the secondary battery; it can be cylindrical, square, or any other arbitrary shape. For example, Figure 5 This is an example of a square-structured secondary battery 5.
[0221] In some implementations, refer to Figure 2 The outer packaging may include a housing 51 and a cover plate 53. The housing 51 may include a base plate and side plates connected to the base plate, the base plate and side plates forming a receiving cavity. The housing 51 has an opening communicating with the receiving cavity, and the cover plate 53 can be placed over the opening to close the receiving cavity. Positive electrode sheets, negative electrode sheets, and separators may be formed into electrode assemblies 52 through a winding process or a stacking process. The electrode assembly 52 is encapsulated within the receiving cavity. Electrolyte is immersed in the electrode assembly 52. The secondary battery 5 may contain one or more electrode assemblies 52, which can be selected by those skilled in the art according to specific practical needs.
[0222] In some implementations, the secondary batteries can be assembled into a battery module, and the number of secondary batteries contained in the battery module can be one or more, the specific number of which can be selected by those skilled in the art according to the application and capacity of the battery module.
[0223] Figure 3 This is battery module 4, used as an example. (See reference...) Figure 3 In battery module 4, multiple secondary batteries 5 can be arranged sequentially along the length of battery module 4. Of course, they can also be arranged in any other manner. Furthermore, these multiple secondary batteries 5 can be fixed in place using fasteners.
[0224] Optionally, the battery module 4 may also include a housing with a receiving space in which a plurality of secondary batteries 5 are received.
[0225] In some embodiments, the battery modules described above can also be assembled into a battery pack, and the number of battery modules contained in the battery pack can be one or more, the specific number of which can be selected by those skilled in the art according to the application and capacity of the battery pack.
[0226] Figure 4 and Figure 5 This is battery pack 1 as an example. (See reference...) Figure 4 and Figure 5 The battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box includes an upper body 2 and a lower body 3, with the upper body 2 covering the lower body 3 to form a closed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.
[0227] The secondary battery provided in this application can also be applied in the field of energy storage, including scenarios such as generation-side energy storage, transmission and distribution-side energy storage, and user energy storage. Specifically, it can be used as, for example, an energy storage cabinet for backup power or a charging cabinet for charging electrical devices. In addition, this application also provides an electrical device, which includes at least one of the secondary battery, battery module, or battery pack provided in this application. The secondary battery, battery module, or battery pack can be used as a power source for the electrical device or as an energy storage unit for the electrical device. The electrical device can include mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but is not limited to these.
[0228] As the electrical device, a secondary battery, battery module, or battery pack can be selected according to its usage requirements.
[0229] Figure 6This is an example of an electrical device. The device could be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the secondary battery for this device, a battery pack or battery module can be used.
[0230] Another example device could be a mobile phone, tablet, or laptop. These devices typically require a slim and lightweight design and can use a rechargeable battery as their power source.
[0231] Example
[0232] The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.
[0233] Preparation and performance characterization of primary and secondary batteries
[0234] Example 1
[0235] 1) Preparation of positive electrode sheet
[0236] Preparation of the gas-generating layer: Urea (volume particle size distribution Dv50 of 3.02 μm), conductive carbon black (SP), and polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 55:25:20. N-methylpyrrolidone was added as a solvent, and the mixture was stirred until homogeneous to obtain a gas-generating layer slurry with a viscosity of 1500 mPa·s. The gas-generating layer slurry was then coated onto both surfaces of the positive electrode current collector aluminum foil using an extrusion coating method, with a single-sided coating amount of 0.15 mg / cm². 2 The gas-producing layer was then dried at 80°C for 2 minutes, and the thickness of one side of the gas-producing layer was 5 μm.
[0237] Preparation of the positive electrode active material layer: The positive electrode active material LiNi... 0.5 Mn 0.2 Co 0.3 O2, conductive agent SP, and binder PVDF are mixed in a mass ratio of 97:1:2, and N-methylpyrrolidone solvent is added. The mixture is stirred until homogeneous to obtain a positive electrode active material slurry with a solid content of 65%. The positive electrode active material slurry is then uniformly coated onto the surface of the gas-generating layer, with a single-sided coating amount of 20 mg / cm². 2 After drying at 85℃, the material is cold-pressed, slit, and cut into sheets, with a thickness of 130μm for the positive electrode active material layer.
[0238] 2) Preparation of negative electrode sheet
[0239] The negative electrode active material graphite, conductive agent SP, binder styrene-butadiene rubber, and thickener sodium carboxymethyl cellulose were mixed evenly in a weight percentage of 95:1.0:2.0:2.0, and deionized water was added. After stirring and dispersing, a negative electrode slurry with a solid content of 50% was obtained. The negative electrode slurry was uniformly coated on both surfaces of the negative electrode current collector copper foil, with a single-sided coating amount of 10 mg / cm². 2 After drying, cold pressing, slitting, and sheet preparation, negative electrode sheets are obtained.
[0240] 3) Isolation components
[0241] The base membrane of the separator is a 9μm thick polyethylene microporous membrane, and the surface of the base membrane is coated with a 4μm thick ceramic coating. The preparation method of the ceramic coating includes: mixing inorganic ceramic particles boehmite, sodium carboxymethyl cellulose, styrene-butadiene rubber and polyvinylpyrrolidone in a mass ratio of 80:8:10:2, adding deionized water and stirring evenly to form a coating slurry, uniformly coating the obtained inorganic coating slurry onto both surfaces of the base membrane using a microgravure coating method, and obtaining the ceramic coating after drying.
[0242] 4) Preparation of electrolyte
[0243] In an argon atmosphere glove box (H2O < 0.1 ppm, O2 < 0.1 ppm), the organic solvents ethylene carbonate and dimethyl carbonate are mixed evenly at a volume ratio of 4 / 6. Lithium salt LiPF6 with a mass content of 12.5% is added and dissolved in the organic solvent and stirred evenly to obtain the electrolyte.
[0244] 5) Preparation of secondary batteries
[0245] The positive electrode, separator, and negative electrode are stacked in sequence, with the separator positioned between the positive and negative electrodes to provide isolation. The resulting battery cell is then wound to obtain a bare cell. This bare cell is placed in an outer aluminum casing, electrolyte is injected, and the battery undergoes vacuum sealing, settling, formation, and shaping processes to obtain a secondary battery. The length, height, and thickness of the outer aluminum casing for the secondary battery are 175mm, 205mm, and 70mm, respectively. The upper limit of the operating temperature for the secondary battery is 60℃.
[0246] Examples 2-11 and Comparative Example 1
[0247] The preparation methods of Examples 2-4 and 6-11 are basically the same as those of Example 1, but the material and thickness of the positive electrode active material layer and the material and thickness of the gas-generating layer are adjusted. Examples 6-8 adjust the cell capacity by adjusting the effective area of the battery positive electrode active material layer slurry coating. The preparation method of Comparative Example 1 is similar to that of the examples, but a gas-generating layer is not provided.
[0248] The preparation method of Example 5 is basically the same as that of Example 1, except that the type of positive electrode active material is adjusted to Na4Fe3(PO4)2P2O7. The electrolyte is adjusted as follows: in an argon atmosphere glove box (H2O < 0.1 ppm, O2 < 0.1 ppm), sodium hexafluorophosphate (NaPF6) is dissolved in the organic solvent dimethyl ethylene glycol (DME), with a sodium salt mass content of 12.5%, and stirred evenly to obtain the electrolyte.
[0249] The preparation parameters for Examples 1-11 and Comparative Example 1 are shown in Table 1.
[0250] Table 1. Preparation parameters of Examples 1-11 and Comparative Example 1
[0251]
[0252] The mass content of binder in the gas-generating layer = 100% - mass content of gas-generating agent - mass content of conductive agent.
[0253] The performance of the secondary batteries prepared in the above embodiments and comparative examples was tested according to the following test methods.
[0254] 1. First temperature test of the gas-producing layer
[0255] Thermogravimetric analysis (TGA) of the gas-generating agent is performed, and its initial temperature of weight loss is the first temperature at which the gas-generating layer begins to produce gas. Alternatively, the electrode containing the gas-generating agent can be heated and tested. The state of the electrode can be observed, and the temperature at which the delamination begins can be recorded as the first temperature of the gas-generating layer.
[0256] 2. Secondary battery capacity test
[0257] The positive electrode active material is LiNi 0.5 Mn 0.2 Co 0.3 O2 or LiNi 0.85 Mn 0.1 Co 0.05 O2 secondary battery: At 25°C, the prepared secondary battery is charged at a charging current of 0.5C until the upper limit voltage is 4.2V. Then, it is discharged at a constant current of 0.2C until the final voltage is 3.0V. This is one charge-discharge process. The capacity of the first discharge is the capacity of the secondary battery.
[0258] The secondary battery with Na4Fe3(PO4)2P2O7 as the positive electrode active material has a maximum charging voltage of 3.8V and a final discharging voltage of 2.0V. Other steps are the same as those with LiNi as the positive electrode active material. 0.5 Mn 0.2 Co 0.3 The testing process for O2 secondary batteries is the same.
[0259] For secondary batteries with LiFePO4 or LiCoO2 as the positive electrode active material: the prepared secondary battery is charged at 25°C with a charging current of 0.5C until the upper limit voltage is 3.65V, and then discharged at a constant current of 0.2C until the final voltage is 2.0V. This is one charge-discharge process. The capacity of the first discharge is the capacity of the secondary battery.
[0260] 3. Secondary battery thermal runaway test
[0261] Referring to GB / T 36276-2023, thermal runaway testing of secondary battery cells is conducted, specifically including the following steps: The battery cell that has completed initial charging is placed in a thermal runaway test apparatus; heating components and temperature sensors are selected and arranged on the surface of the secondary battery cell; a temperature sampling period of 1 second is set; the criteria for determining thermal runaway are that three consecutive temperature rise rates ≥3℃ / s, or fire or explosion; the secondary battery cell is connected to the charging / discharging device and its voltage data sampling line; and I = P rc / U nom Constant current charging is initiated, heating is started, and time, voltage, current, temperature, and temperature rise rate are recorded. Experimental phenomena are also recorded, including expansion, leakage, smoke, fire, explosion, casing rupture, and rupture location. Charging and heating are stopped when the thermal runaway criteria are triggered, the temperature reaches 300℃, or the test time reaches 4 hours. Observation is performed for 1 hour, recording time, voltage, temperature, and temperature rise rate, and experimental phenomena, including expansion, leakage, smoke, fire, explosion, casing rupture, and rupture location. The connection between the secondary battery cell and the charging / discharging device is disconnected, the heating element and data sampling line are removed, and the secondary battery cell is taken out. Here, Prc represents the rated charging power, and Unom represents the nominal voltage.
[0262] 4. Overcharge test of secondary battery
[0263] According to GB / T 36276-2023, the overcharge test of a secondary battery cell is conducted, specifically including the following steps: Connect the battery cell that has completed initial charging to the voltage and temperature data sampling lines of the charging and discharging device. Charge at a constant current of I = Prc / Unom until the voltage reaches 1.5 times the charging cutoff voltage of the battery cell or the charging time reaches 1 hour. Observe for 1 hour and record the time when the battery reaches the cutoff voltage, the highest temperature of the battery, and the test phenomena (test phenomena include expansion, leakage, smoke, fire, explosion, shell cracking and crack location). Disconnect the test sample from the charging and discharging device, remove the data sampling lines, and take out the test sample. Where Prc represents the rated charging power and Unom represents the nominal voltage.
[0264] 5. State of the positive electrode after thermal runaway test
[0265] After disassembling the secondary battery following the thermal runaway test, remove the positive electrode sheet and observe the peeling of the gas-generating layer of the positive active material layer in a single fold (for wound structures) or a single sheet (for stacked structures). Record the percentage of the area of the gas-generating layer of the positive active material layer peeling off to the total area of the electrode sheet as A. The peeling level is shown in Table 2 below.
[0266] Table 2. Peeling Grades of Positive Electrode Sheets
[0267] Percentage of detached area A% Classification <10% + 10%≤A<50% ++ 50%≤A≤100% +++
[0268] The performance parameters of the secondary battery are shown in Table 3 below.
[0269] Table 3 Performance parameters of each embodiment and comparative example
[0270]
[0271] As shown in Examples 1-11 and Comparative Example 1, the positive electrode of the secondary battery is provided with a gas-generating layer containing a gas-generating agent. This gas-generating layer generates gas under the influence of a first temperature, which is beneficial for improving the battery's safety performance and reliably passing thermal runaway and overcharge tests. This may be because the gas-generating agent can decompose to generate gas when the internal temperature of the secondary battery reaches the first temperature, and accumulates between the positive electrode active material layer and the current collector in a short time, increasing the pressure between them. This causes the positive electrode active material layer to separate from the current collector, interrupting the charging current, increasing the battery's polarization, and allowing the battery to quickly reach the charging cutoff voltage, thereby terminating overcharge and thermal runaway behavior.
[0272] As can be seen from Examples 1-5, urea, ammonium carbonate, magnesium bicarbonate, potassium bicarbonate and sodium bicarbonate are used as gas-generating agents and combined with different positive electrode active materials. The batteries of different systems improve safety while operating normally. The secondary batteries provided in this application have a wide range of applications.
[0273] As shown in Examples 1 and 6-8, when the particle size of the gas-generating agent is in the range of 0.2 μm to 6 μm, the gas-generating agent can generate sufficient gas to promote the separation of the positive electrode active material layer from the current collector, interrupt the charging current, improve battery polarization, and effectively prevent battery overcharging. Furthermore, a particle size of 0.2 μm to 3.5 μm can further improve the gas-generating effect. Reducing the particle size of the gas-generating agent can easily lead to agglomeration during the preparation of the gas-generating layer slurry, resulting in poor stability of the slurry. A particle size of 0.2 μm to 6 μm for the gas-generating agent combines excellent gas-generating performance with good industrial preparation performance.
[0274] As can be seen from Examples 1 and 6-8, the thickness of the gas-generating layer is in the range of 0.5μm-10μm, which can effectively prevent battery overcharging without significantly affecting battery capacity.
[0275] As shown in Examples 1 and 9-11, when the mass content of the gas-generating agent in the gas-generating layer is in the range of 40%-80%, it can rapidly decompose to generate gas when the internal temperature of the secondary battery reaches the first temperature. This promotes the separation of the positive electrode active material layer from the current collector, interrupts the charging current, and improves the polarization of the battery, thereby terminating overcharging. Furthermore, the higher the mass content of the gas-generating agent, the better the separation effect between the positive electrode active material layer and the current collector, and the better the battery safety. Excessive gas-generating agent content can increase the difficulty of preparing the gas-generating layer slurry and also degrade the battery's electrical performance. When the mass content of the gas-generating agent is in the range of 55%-80%, the battery can possess good electrical performance, superior safety performance, and industrial manufacturing performance.
[0276] Examples 12-13
[0277] The preparation method of Example 12 is basically the same as that of Example 1, but the material and thickness of the positive electrode active material layer and the material and thickness of the gas-generating layer are adjusted. The preparation method of Example 13 is basically the same as that of Example 1, but the amount of gas-generating agent and conductive agent in the gas-generating layer is adjusted. Specific preparation parameters are shown in Table 4.
[0278] Table 4 Preparation parameters of Examples 12-13
[0279]
[0280] The mass content of binder in the gas-generating layer = 100% - mass content of gas-generating agent - mass content of conductive agent.
[0281] In Example 12, due to the increase in the particle size of the gas-generating agent, the thickness of the gas-generating layer is correspondingly increased to achieve the preparation of the gas-generating layer; at the same time, in order to achieve the predetermined battery capacity, the effective coating area of the positive electrode active material layer is adjusted, which leads to an increase in the total thickness of the electrode film layer. After the cell is wound, it affects the consistency and reliability of battery performance, which is not conducive to the preparation of the battery.
[0282] In Example 13, the excessive amount of gas-generating agent caused agglomeration of the gas-generating layer slurry, making it impossible to prepare a secondary battery with consistent and reliable performance.
[0283] Further analysis was conducted on the thermal stability of the electrodes in the secondary batteries prepared in Examples 1, 2, and 5. The heat generated by the positive electrode was tested using DSC, specifically as follows: The prepared positive electrode was taken and cut into pieces with an area greater than or equal to 15 cm². 2 Alternatively, the size of the electrode (length × width) is greater than or equal to 3cm × 5cm, and its thermal stability is analyzed.
[0284] The results are shown in Table 5.
[0285] Table 5. Parameters for Thermal Stability Analysis of Electrodes
[0286]
[0287] The positive electrode sheet of the secondary battery prepared in the above embodiments generates no more than 2000 J / g of heat in DSC testing, indicating that the positive electrode active material used has high thermal and structural stability. It remains relatively stable under thermal runaway and overcharge conditions, and is not prone to structural collapse or violent chemical reactions, thereby reducing heat accumulation during overcharge and the risk of battery fire and explosion. The rational combination of the above-mentioned positive electrode active material and gas-generating agent helps improve the safety performance of the battery.
[0288] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.
Claims
1. A secondary battery, characterized in that, It includes a positive electrode, a separator, and a negative electrode, wherein the separator is disposed between the positive electrode and the negative electrode; the positive electrode includes a current collector, a gas generation layer, and a positive active material layer, wherein the gas generation layer is disposed between the current collector and the positive active material layer; The gas-generating layer includes a gas-generating agent, and the gas-generating layer generates gas when the positive electrode reaches a first temperature.
2. The secondary battery according to claim 1, characterized in that, The first temperature is at least 5°C higher than the upper limit of the operating temperature of the secondary battery. Optionally, the first temperature is 5°C to 100°C higher than the upper limit of the operating temperature of the secondary battery.
3. The secondary battery according to claim 1 or 2, characterized in that, The heat generated by the positive electrode in the DSC test does not exceed 2000 J / g. Optionally, the heat generated by the positive electrode in the DSC test does not exceed 50 J / g-1900 J / g.
4. The secondary battery according to any one of claims 1 to 3, characterized in that, The secondary battery cell capacity is greater than or equal to 250Ah, and optionally, the secondary battery cell capacity is 250Ah-800Ah.
5. The secondary battery according to any one of claims 1 to 4, characterized in that, The secondary battery satisfies either condition 1) or 2): 1) The secondary battery is a lithium secondary battery, and the positive electrode active material layer includes at least one of the positive electrode active material represented by Formula 1 and the positive electrode active material represented by Formula 2: Li x1 A y1 Me a1 M b1 P 1-c1 X c1 Y z1 Formula 1 Wherein, 0.5≤x1≤1.3, 0≤y1≤1.3, and 0.7≤x1+y1≤1.3; 0.9≤a1≤1.5, 0≤b1≤0.5, and 0.9≤a1+b1≤1.5; 0≤c1≤0.5; 3≤z1≤5; A includes one or more of Na, K, and Mg; Me includes one or more of Mn, Fe, Co, and Ni; M includes one or more of B, Mg, Al, Si, P, S, Ca, Sc, Ti, V, Cr, Cu, Zn, Sr, Y, Zr, Nb, Mo, Cd, Sn, Sb, Te, Ba, Ta, W, Yb, La, and Ce; X includes one or more of S, Si, Cl, B, C, and N; Y includes one or more of O and F. Li x2 Ni y2 Co z2 M' a2 Me' b2 O c2 A' d2 Formula 2 Wherein, 0.85≤x²≤1.15, 0≤y²<1, 0≤z²≤1, 0≤a²<1, 0≤b²≤0.1, 1.8≤c²≤2.2, 0≤d²≤1, d²+c²≤2, y²+z²+a²+b²=1, M' includes Al, Me' is selected from one or more of Mn, Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, Sr, Sb, Y, W, Nb, and A' is selected from one or more of N, F, S, Cl; or 2) The secondary battery is a sodium secondary battery, and the positive electrode active material layer includes at least one of the following positive electrode active materials: layered metal oxide, Prussian compound, and polyanionic compound.
6. The secondary battery according to any one of claims 1 to 5, characterized in that, The gas-generating agent includes at least one of alkali metal bicarbonate, alkaline earth metal bicarbonate, ammonium carbonate, aluminum hydroxide, and nitrogen-containing compounds.
7. The secondary battery according to any one of claims 1 to 6, characterized in that, 1) The secondary battery is a lithium secondary battery and satisfies one of the following conditions a) to d). a) The positive electrode active material includes the positive electrode active material represented by the following formula 1-1. Li x1 Fe a1 M b1 P 1-c1 X c1 O z1 Formula 1-1 wherein, 0.5≤x1≤1.3; 0.9≤a1≤1.5, 0≤b1≤0.5, and 0.9≤a1+b1≤1.5; 0≤c1≤0.5; 3≤z1≤5; M includes one or more of B, Mg, Al, Si, P, S, Ca, Sc, Ti, V, Cr, Cu, Zn, Sr, Y, Zr, Nb, Mo, Cd, Sn, Sb, Te, Ba, Ta, W, Yb, La, and Ce; X includes one or more of S, Si, Cl, B, C, and N; b) the positive active material includes a positive active material represented by the following Formula 1-2, Li x1 Me a1 M b1 P 1-c1 X c1 O z1 Formula 1-2 wherein, 0.5≤x1≤1.3; 0.9≤a1≤1.5, 0≤b1≤0.5, and 0.9≤a1+b1≤1.5; 0≤c1≤0.5; 3≤z1≤5; Me includes Mn and Fe; M includes one or more of B, Mg, Al, Si, P, S, Ca, Sc, Ti, V, Cr, Cu, Zn, Sr, Y, Zr, Nb, Mo, Cd, Sn, Sb, Te, Ba, Ta, W, Yb, La, and Ce; X includes one or more of S, Si, Cl, B, C, and N; c) the positive active material includes a positive active material represented by the following Formula 2-1, Li x2 Ni y2 Co z2 Al a2 Me' b2 O c2 A' d2 Formula 2-1 wherein, 0.85≤x2≤1.15, 0≤y2<1, 0<z2≤1, 0≤a2<1, 0≤b2≤0.1, 1.8≤c2≤2.2, 0≤d2≤1, d2+c2≤2, y2+z2+a2+b2=1, Me' is selected from one or more of Mn, Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, Sr, Sb, Y, W, and Nb, and A' is selected from one or more of N, F, S, and Cl, d) the positive active material includes a positive active material represented by the following Formula 2-2, Li x2 Ni y2 Me' b2 O c2 A' d2 Formula 2-2 wherein, 0.85≤x2≤1.15, 0<y2<1, 0≤b2≤0.1, 1.8≤c2≤2.2, 0≤d2≤1, d2+c2≤2, y2+b2=1, Me' is selected from one or more of Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, Sr, Sb, Y, W, and Nb, and A' is selected from one or more of N, F, S, and Cl; or 2) the secondary battery is a sodium secondary battery and satisfies one of the following conditions e) to h), e) the positive active material includes a positive active material represented by the following Formula 3 and Na x3 M1 y3 Ni z3 Fe a3 Mn b3 O 2±δ formula 3 wherein M1 is a metal cation different from Ni, Fe and Mn, and includes at least one selected from the group consisting of Li + , Cu 2+ , Zn 2+ , Co 2+ , Ti 4+ ; 0.67<x3<1.1; 0<y3<0.25, preferably 0.05<y3<0.15; 0<z3<0.3, preferably 0.05<z3<0.25; 0<y3+z3<0.55; 0.45<a3+b3<1; and y3+z3+a3+b3=1; 0≤δ≤0.1; f) the positive active material includes a positive active material represented by the following Formula 4, Na x4 M2[M1′(CN)6] y4 ·z4H2O Formula 4 wherein, M2 is a transition metal, M1' is a transition metal, 0<x4≤2, 0.8≤y4<1, and 0<z4≤20; g) the positive active material includes a positive active material represented by the following Formula 5, Na x5 Fe 1-y5 B1 y5 (SO4) z5 formula 5 Wherein, 1.1≤x5≤1.7, 0≤y5≤0.1; B1 includes those selected from Mn 2+ Ni 2+ Co 2+ Cu 2+ Ca 2+ Mg 2+ Ba 2+ and Zn 2+ At least one of them, h) the positive active material includes a positive active material represented by the following Formula 6, Na x6 M3 y6 X1 z6 (PO4) m P2O7 formula 6 wherein, M3 includes at least one of Fe, Co, Ni, and Mn, X1 includes at least one of Al and Ti, and 1≤x6≤4, 1≤y6≤4, 0≤z6≤0.1, and 1≤m≤2.
8. The secondary battery according to any one of claims 1 to 7, characterized in that, The gas-generating agent has a mass content of 40%-80% based on the total mass of the gas-producing layer; alternatively, the gas-generating agent has a mass content of 55%-80% based on the total mass of the gas-producing layer.
9. The secondary battery according to any one of claims 1 to 8, characterized in that, The gas-generating agent has a volumetric particle size distribution Dv50 of 0.2 μm-6 μm; optionally, the gas-generating agent has a volumetric particle size distribution Dv50 of 0.2 μm-5 μm.
10. The secondary battery according to any one of claims 1 to 9, characterized in that, The thickness ratio of the gas-generating layer to the positive electrode active material layer is 1:(15-150); optionally, the thickness ratio of the gas-generating layer to the positive electrode active material layer is 1:(24-150).
11. The secondary battery according to any one of claims 1 to 10, characterized in that, The thickness of the gas-producing layer is 0.5μm-10μm, and can be selected as 0.5μm-5μm.
12. The secondary battery according to any one of claims 1 to 11, characterized in that, The gas-producing layer includes a binder, and the binder content is 5%-40% by mass based on the total mass of the gas-producing layer.
13. The secondary battery according to claim 12, characterized in that, Based on the total mass of the gas-producing layer, the mass ratio of the binder to the gas-producing agent in the gas-producing layer is 1:(1-20), or optionally 1:(1-16).
14. The secondary battery according to any one of claims 1 to 13, characterized in that, The gas-producing layer includes a conductive agent, and the mass content of the conductive agent is 10%-25% based on the total mass of the gas-producing layer, optionally 15%-25%.
15. The secondary battery according to claim 14, characterized in that, The mass ratio of the conductive agent to the gas-generating agent in the gas-generating layer is 1:(2-10), and can be optionally 1:(2-6).
16. The secondary battery according to any one of claims 1 to 15, characterized in that, The alkali metal bicarbonate includes at least one of potassium bicarbonate and sodium bicarbonate. The alkaline earth metal bicarbonates include magnesium bicarbonate. The nitrogen-containing compound includes at least one of urea, nitrosamine, and sodium azide.
17. The secondary battery according to any one of claims 1 to 16, characterized in that, The secondary battery has a length of L, a height of H, and a thickness of T. The dimensions of the secondary battery cell satisfy the following: 200mm≤L≤550mm, 150mm≤H≤250mm, 60mm≤T≤80mm, and 0.5≤L / H≤3, 2≤H / T≤4. Optionally, the dimensions of the secondary battery cell satisfy the following: 160mm≤L≤300mm, 180mm≤H≤220mm, 65mm≤T≤75mm.
18. The secondary battery according to any one of claims 1 to 17, characterized in that, Based on the total mass of the gas-generating layer, the gas-generating layer includes positive electrode active material with a mass content of less than or equal to 5%, optionally, the gas-generating layer includes positive electrode active material with a mass content of 0%-1%; and / or, the positive electrode active material in the gas-generating layer is the same as the positive electrode active material in the positive electrode active material layer.
19. The secondary battery according to any one of claims 1 to 18, characterized in that, The separator includes a ceramic coating comprising inorganic ceramic particles; optionally, the inorganic ceramic particles comprise one or more of boehmite and alumina.
20. An electrical device, characterized in that, The secondary battery includes any one of claims 1 to 19.