A method of making a stable phase radio frequency cable

By forming a microtexture on the surface of the inner conductor of the RF cable and covering it with a temperature-compensated dielectric layer and a multilayer foamed polytetrafluoroethylene insulation layer, the dielectric constant and axial linear expansion coefficient of the dielectric structure are adjusted, thus solving the phase drift problem of the RF cable in a wide temperature range and improving the phase stability and interface bonding strength of the cable.

CN123162500APending Publication Date: 2026-11-24嘉兴翼波电子有限公司
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611666354.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-27
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing technologies struggle to achieve near-zero electrical length phase temperature coefficients in RF cables across a wide temperature range, and the interface between the dielectric layer and the inner conductor is unstable, leading to phase drift.

Method used

A microtexture is formed on the surface of the inner conductor, and a temperature-compensated dielectric layer and a foamed polytetrafluoroethylene insulating layer are wrapped around it. By adjusting the temperature coefficient of dielectric constant and the coefficient of axial linear expansion of the dielectric structure, and combining mechanical interlocking to improve the interfacial bonding force, a four-layer structure of inner dense layer, transition layer, high foaming layer and outer dense layer is formed.

Benefits of technology

It improves the phase temperature stability of RF cables over a wide temperature range and their stability under long-term temperature cycling, reduces the phase temperature coefficient of electrical length, and enhances the interfacial bonding strength between the dielectric layer and the inner conductor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123162500A_ABST
    Figure CN123162500A_ABST
Patent Text Reader

Abstract

This invention relates to the field of radio frequency (RF) cable manufacturing technology, and more particularly to a method for manufacturing a phase-stable RF cable, comprising: forming a microtexture on the outer surface of an inner conductor; covering the inner conductor with the microtexture with a temperature-compensated dielectric layer and determining the measured temperature coefficient of the dielectric constant of the temperature-compensated dielectric layer; determining a target equivalent temperature coefficient of dielectric constant based on the target electrical length phase temperature coefficient and the axial linear expansion coefficient of the RF cable, thereby determining the target temperature coefficient of dielectric constant of the foamed polytetrafluoroethylene (PTFE) insulation layer; determining the target crystallinity of the foamed PTFE insulation layer based on the target temperature coefficient of dielectric constant; preparing the foamed PTFE insulation layer based on the target crystallinity, thereby adjusting the annealing temperature of the foamed PTFE insulation layer and the production line transmission speed; and sequentially covering the outer side of the foamed PTFE insulation layer with an outer conductor layer, a shielding layer, and an outer sheath layer to obtain the RF cable. This invention achieves a phase-stable target with the electrical length phase temperature coefficient approaching zero.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of radio frequency cable manufacturing technology, and in particular to a method for manufacturing a phase-stable radio frequency cable. Background Technology

[0002] Radio frequency (RF) coaxial cables are key transmission components in phase-sensitive electronic systems such as phased array radars, electronic countermeasures equipment, and satellite and missile telemetry and control. Their performance directly determines the phase consistency of the entire system. The core indicator of a stable RF cable is the electrical length-phase temperature coefficient, which is the change in phase per unit length of the cable caused by temperature within a specified operating temperature range. The smaller the value, the better the phase stability of the cable. The electrical length-phase of a cable consists of two parts: the physical length of the cable and the equivalent dielectric constant of the medium between the inner and outer conductors. When the temperature rises, the cable expands axially, increasing its physical length, while the equivalent dielectric constant of the medium decreases, shortening its electrical length. These two changes occur in opposite directions, theoretically providing some natural cancellation. However, the actual axial linear expansion coefficient of the cable is constrained by the inner conductor, each dielectric layer, and the outer conductor, and its value is much greater than the compensation caused by the change in the dielectric constant of the medium with temperature. Therefore, untreated cables still exhibit significant phase drift over a wide temperature range.

[0003] To reduce phase drift, existing technologies primarily focus on the dielectric structure, employing methods such as wrapping with microporous PTFE films, stretch extruded foam insulation, spiral tubular dielectrics, or porous dielectric structures to introduce air and lower the equivalent dielectric constant, thereby reducing the absolute magnitude of the dielectric constant change with temperature. These methods can improve temperature-dependent phase performance to some extent, for example, reducing the phase change in the -55℃ to +85℃ range from over 800ppm to around 400ppm. However, their effectiveness is limited by the temperature characteristics of the dielectric material itself, making further reduction difficult. Furthermore, PTFE undergoes a crystal transformation around 19℃, causing a sudden volume change and resulting in an inflection point in the phase curve at that temperature, further deteriorating phase stability.

[0004] Another existing technology adjusts the dielectric constant by filling the dielectric with high-dielectric-constant ceramic powder, such as doping barium strontium titanate with barium strontium niobate to obtain the desired temperature coefficient of dielectric constant. This type of method is often used in components such as capacitors, phase shifters, and microwave tuners, with the design goal of bringing the material's temperature coefficient of dielectric constant close to zero, thus eliminating the effect of temperature changes on the dielectric constant. However, directly applying this goal to radio frequency (RF) cables does not achieve phase stability: the phase stability of the cable depends on the overall change in electrical length. When the equivalent temperature coefficient of dielectric constant is adjusted to zero, the phase drift of the cable is entirely determined by axial linear expansion, and its value is actually greater than the result of the negative temperature coefficient of dielectric constant partially offsetting axial expansion when no treatment is done. In other words, for the specific application of RF cables, simply pursuing a near-zero temperature coefficient of dielectric constant is counterproductive.

[0005] In addition, existing phase-stable cables mainly rely on interface bonding or adhesive bonding to achieve the bonding between the dielectric layer and the inner conductor. Under repeated temperature cycles, due to the large difference in the thermal expansion coefficients between the metal conductor and the fluoropolymer dielectric, micro gaps are easily generated at the interface, which leads to a change in the local equivalent dielectric constant and causes irreversible phase drift.

[0006] Chinese Patent Application Publication No. CN110380175A discloses an anti-interference phase-stable radio frequency cable and its manufacturing method. The anti-interference phase-stable radio frequency cable includes, from the inside out, a conductor, an insulation layer, a first outer conductor layer, a second outer conductor layer, and a sheath layer. The conductor is a silver-plated copper-clad aluminum alloy copper wire; the insulation layer is wrapped with an expanded polytetrafluoroethylene (PTFE) film; the first outer conductor layer is wrapped with a silver-plated flat copper strip; the second outer conductor layer is wrapped with a silver-plated carbon nanofiber film; and the sheath layer is a soluble PTFE layer. This anti-interference phase-stable radio frequency cable has the advantages of being lightweight, having electromagnetic shielding properties, and exhibiting good temperature and mechanical phase stability. Furthermore, the manufacturing method is simple and easy to implement.

[0007] The existing technology still has the following problems: reducing the magnitude of the change of dielectric constant with temperature by only using foamed dielectric structure, or simply pursuing the dielectric constant temperature coefficient of the dielectric to approach zero, does not take the axial linear expansion of the cable and the equivalent dielectric constant temperature coefficient of the dielectric as a whole. Furthermore, it lacks effective control over the interface stability between the dielectric layer and the inner conductor, the 19℃ phase transition inflection point of polytetrafluoroethylene, and the crystallinity of the foamed insulation layer. Therefore, it is difficult to achieve the stable phase target of the electrical length phase temperature coefficient approaching zero in a wide temperature range. Summary of the Invention

[0008] Therefore, the present invention provides a method for preparing a phase-stable radio frequency cable to overcome the problem in the prior art that it is difficult to achieve a phase-stable target with the electrical length phase temperature coefficient approaching zero over a wide temperature range.

[0009] To achieve the above objectives, the present invention provides a method for preparing a phase-stable radio frequency cable, comprising: An inner conductor of a radio frequency cable is prepared and a microtexture is formed on the outer surface of the inner conductor to enhance the mechanical bonding force with adjacent layers; A temperature-compensated dielectric layer is coated on the inner conductor having the microtexture and the measured temperature coefficient of the dielectric constant of the temperature-compensated dielectric layer is determined. The temperature-compensated dielectric layer is a thin film layer composed of barium strontium titanate powder and polytetrafluoroethylene propylene resin with a thickness of 80-150 μm. Based on the target electrical length phase temperature coefficient of the radio frequency cable and the pre-calibrated axial linear expansion coefficient of the radio frequency cable, the target equivalent dielectric constant temperature coefficient of the dielectric structure composed of the temperature-compensated dielectric layer and the foamed polytetrafluoroethylene insulation layer is determined, and the target dielectric constant temperature coefficient of the foamed polytetrafluoroethylene insulation layer is determined based on the target equivalent dielectric constant temperature coefficient and the measured dielectric constant temperature coefficient. The target crystallinity of the foamed polytetrafluoroethylene insulation layer is determined based on the target dielectric constant temperature coefficient. The foamed polytetrafluoroethylene insulation layer is prepared based on the target crystallinity, and the annealing temperature and production line transfer speed of the foamed polytetrafluoroethylene insulation layer are adjusted based on the measured crystallinity of the foamed polytetrafluoroethylene insulation layer. An outer conductor layer, a shielding layer, and an outer sheath layer are sequentially wrapped around the outside of the foamed polytetrafluoroethylene insulation layer to obtain a radio frequency cable.

[0010] Furthermore, the depth of the microtexture is 1–5 μm and not greater than 1% of the radius of the inner conductor, with a coverage of 30%–70%; the inner conductor also has a silver plating layer on the surface of the microtexture, the thickness of the silver plating layer being 0.5–2.5 μm and less than the depth of the microtexture.

[0011] Furthermore, the axial linear expansion coefficient is determined based on the electrical length phase temperature coefficient and the equivalent dielectric constant temperature coefficient of the reference cable.

[0012] Furthermore, the preparation process of the temperature-compensated dielectric layer includes: Based on the target negative permittivity temperature coefficient of the temperature-compensated dielectric layer, the mole fraction of strontium in barium strontium titanate and the thickness of the temperature-compensated dielectric layer are determined. Strontium barium titanate powder was prepared and calcined at 800–1200°C for 1–6 h, followed by ball milling and sieving. Dissolve 0.5% to 3% of the coupling agent by weight of barium strontium titanate powder in a mixed ethanol solution, add barium strontium titanate powder, ultrasonically disperse for 10 to 60 minutes, and then dry at 60 to 120°C to obtain modified barium strontium titanate powder. The modified barium strontium titanate powder was mixed with polytetrafluoroethylene propylene resin, solvent, and dispersant, and then ball-milled to prepare a uniform and stable slurry. The slurry is applied evenly to a flat substrate through a slit coating head. After drying and curing in an oven, it is peeled off from the substrate to obtain a composite film. The composite film is coated onto the surface of the inner conductor with a microtexture to obtain the temperature-compensated dielectric layer.

[0013] Furthermore, the chemical formula of the barium strontium titanate is Ba. 1-x Sr x TiO3, wherein the molar fraction x of strontium is 0.52 to 0.70, and the Curie temperature of the barium strontium titanate is below -80°C.

[0014] Furthermore, the target dielectric constant temperature coefficient of the foamed polytetrafluoroethylene insulation layer is determined based on the measured dielectric constant temperature coefficient of the temperature-compensated dielectric layer and the axial linear expansion coefficient of the RF cable, as well as the contribution weights of the temperature-compensated dielectric layer and the foamed polytetrafluoroethylene insulation layer.

[0015] Furthermore, the foamed polytetrafluoroethylene insulation layer has an inner dense layer 3a, a transition layer, a high-foaming layer, and an outer dense layer with different porosities arranged sequentially from the inside to the outside. The thickness of the inner dense layer 3a accounts for 8% to 15% of the total wall thickness of the foamed polytetrafluoroethylene insulation layer, the thickness of the transition layer accounts for 12% to 20% of the total wall thickness of the foamed polytetrafluoroethylene insulation layer, the thickness of the high-foaming layer accounts for 50% to 65% of the total wall thickness of the foamed polytetrafluoroethylene insulation layer, and the thickness of the outer dense layer accounts for 10% to 18% of the total wall thickness of the foamed polytetrafluoroethylene insulation layer.

[0016] Furthermore, the process of adjusting the annealing temperature of the foamed polytetrafluoroethylene insulation layer and the production line conveyor speed includes: Compare the measured crystallinity with the target crystallinity; If the measured crystallinity is less than the target crystallinity, then increase the annealing temperature or decrease the production line transfer speed; If the measured crystallinity is greater than the target crystallinity, then reduce the annealing temperature or increase the production line transfer speed.

[0017] Furthermore, the outer conductor is made of silver-plated copper flat strip wrapped around it, and the shielding layer is made of silver-plated copper wire braided together.

[0018] Furthermore, the outer sheath is a polytetrafluoroethylene propylene (PTFE) outer sheath, wherein the PTFE outer sheath has a tensile strength of not less than 20 MPa, an elongation at break of not less than 250%, a dielectric strength of not less than 20 kV / mm, and a volume resistivity of not less than 1 × 10⁻⁶. 16 Ω·m.

[0019] Compared with the prior art, the beneficial effects of the present invention are as follows: The present invention prepares a reference cable with the same structure as the cable to be prepared, except that the temperature compensation dielectric layer is replaced with a pure polytetrafluoroethylene propylene layer of equal thickness, and measures its electrical length phase temperature coefficient to determine the axial linear expansion coefficient of the radio frequency cable; the constraint state contained in the reference cable is completely consistent with that of the formal cable, and the thickness of the temperature compensation dielectric layer is no more than 25% of the thickness of the foamed insulation layer, and the resin matrix is ​​the same as that of the pure polytetrafluoroethylene propylene layer. Therefore, the difference in the axial linear expansion coefficient between the two is no more than 2%. The measured calibration value is used instead of the theoretical estimate as the design input, so that the target equivalent dielectric constant temperature coefficient obtained by subsequent inversion matches the actual requirements of the cable, avoiding systematic undercompensation or overcompensation caused by input distortion, thereby improving the target matching accuracy of phase compensation design.

[0020] Furthermore, barium strontium titanate is in the paraelectric phase above its Curie temperature, and its dielectric constant monotonically decreases with increasing temperature, exhibiting a negative temperature coefficient much larger than that of fluoropolymers. In this invention, it is combined with perfluoroethylene propylene to form a temperature-compensated dielectric layer, which is placed between the inner conductor and the foamed polytetrafluoroethylene insulation layer. It participates in the overall equivalent dielectric constant according to radial series contribution weight, and the Curie temperature is set below the lower limit of the stable phase operating temperature range. This ensures that the negative temperature coefficient remains monotonically, continuously, and predictably throughout the entire operating temperature range, preventing abrupt changes in the dielectric constant and a change in the sign of the temperature coefficient due to the phase transition point falling into the temperature range. Its negative temperature coefficient offsets the positive phase drift term introduced by axial linear expansion, so that the equivalent dielectric constant temperature coefficient of the dielectric is actively pushed towards the direction that makes the electrical length phase temperature coefficient approach zero, rather than passively approaching zero, thereby improving the phase temperature stability of the cable in a wide temperature range.

[0021] Furthermore, the difference in axial and radial thermal expansion between the copper inner conductor and the fluoropolymer dielectric during temperature cycling will generate periodic shear stress at the interface. If the interface is only physically bonded, the shear will gradually cause the interface to separate and form a micron-level gap. The dielectric constant of this gap is different from that of the dielectric layer, thus changing the local equivalent dielectric constant and causing irreversible phase drift. In this invention, after rolling a microtexture on the outer surface of the inner conductor, a temperature-compensated dielectric layer is coated on it. The polytetrafluoroethylene propylene resin melts and flows, embedding into the valley of the microtexture. After curing, a mechanical interlock is formed. The failure mode at the interface changes from interface debonding to the cohesive failure of the dielectric layer itself. The energy required for failure increases by an order of magnitude. At the same time, the thickness of the silver plating layer is limited to less than the depth of the microtexture, so that the texture still retains no less than 50% of the residual depth after silver plating. This avoids the plating layer filling the texture and causing the interlock structure to fail. As a result, the interface remains tightly bonded under repeated temperature cycling, thereby improving the stability of the cable phase under long-term temperature cycling.

[0022] Furthermore, the axial elongation of the high-foaming layer under heat increases the overall axial linear expansion coefficient of the dielectric layer. The abrupt changes in modulus and thermal expansion coefficient between layers cause stress concentration at the interface, which accumulates as localized plastic deformation during temperature cycling. This invention constructs a four-layer radial gradient structure for the foamed polytetrafluoroethylene insulation layer: an inner dense layer 3a, a transition layer, a high-foaming layer, and an outer dense layer. The inner dense layer 3a, adjacent to the temperature-compensated dielectric layer, provides high-strength interfacial bonding and electrical resistance, and together with the outer dense layer, forms a radial constriction around the high-foaming layer, suppressing its axial free movement. The elongation reduces the overall axial linear expansion coefficient of the dielectric layer to approximately 47 ppm / ℃. A transition layer smoothly and gradually changes the porosity from the inside to the outside, eliminating abrupt changes between layers. The high porosity of the foamed layer introduces air to lower the overall dielectric constant and attenuation. An outer dense layer blocks the intrusion of external moisture, preventing moisture from replacing the air in the foam cells and causing dielectric constant drift. Each of the four layers performs its function and works together to ensure that the dielectric structure maintains a low dielectric constant while achieving a defined axial constraint. This improves the structural consistency of the cable phase temperature coefficient across multiple batches and operating conditions. Attached Figure Description

[0023] Figure 1 This is a schematic diagram of the structure of a phase-stable radio frequency cable according to an embodiment of the present invention; Figure 2 This is a flowchart illustrating the preparation method of a phase-stable radio frequency cable according to an embodiment of the present invention; Figure 3 This is a flowchart illustrating the preparation of the temperature-compensated dielectric layer according to an embodiment of the present invention; Figure 4 This is a flowchart illustrating the adjustment of the annealing temperature and production line transmission speed of the foamed polytetrafluoroethylene insulation layer according to an embodiment of the present invention. In the diagram: 1-Inner conductor, 2-Temperature-compensated dielectric layer, 3-Foamed polytetrafluoroethylene insulation layer, 3a-Inner dense layer, 3b-Transition layer, 3c-High foaming layer, 3d-Outer dense layer, 4-Outer conductor layer, 5-Shielding layer, 6-Outer sheath layer. Detailed Implementation

[0024] To make the objectives and advantages of the present invention clearer, the present invention will be further described below with reference to embodiments; it should be understood that the specific embodiments described herein are merely for explaining the present invention and are not intended to limit the present invention.

[0025] Preferred embodiments of the present invention will now be described with reference to the accompanying drawings. Those skilled in the art should understand that these embodiments are merely illustrative of the technical principles of the present invention and are not intended to limit the scope of protection of the present invention.

[0026] Please see Figure 1 The diagram shown is a structural schematic of a phase-stable radio frequency cable according to an embodiment of the present invention. The phase-stable radio frequency cable according to an embodiment of the present invention includes: The radio frequency cable is coaxially arranged from the inside to the outside as follows: inner conductor 1, temperature compensation dielectric layer 2, foamed polytetrafluoroethylene insulation layer 3, outer conductor layer 4, shielding layer 5, and outer sheath layer 6. In this embodiment, the nominal characteristic impedance of the radio frequency cable is 50Ω±1.5Ω, and the stable operating temperature range is -55 to +125℃; the diameter of the inner conductor 1 is 1.0mm, the thickness of the temperature-compensated dielectric layer 2 is 80 to 150μm, the single-sided thickness of the foamed polytetrafluoroethylene insulation layer 3 is 0.71 to 0.78mm, the outer diameter of the foamed polytetrafluoroethylene insulation layer 3 is 2.72mm, and the thickness of the temperature-compensated dielectric layer 2 is 10% to 25% of the thickness of the foamed polytetrafluoroethylene insulation layer 3.

[0027] Please see Figure 2 The diagram shows a flowchart of a method for preparing a phase-stable radio frequency cable according to an embodiment of the present invention. The method includes: Step S1: Prepare the inner conductor 1 of the radio frequency cable and form a microtexture on the outer surface of the inner conductor 1 to enhance the mechanical bonding force with the adjacent layers; Step S2: A temperature-compensated dielectric layer 2 is coated on the inner conductor 1 with the microtexture and the measured temperature coefficient of the dielectric constant of the temperature-compensated dielectric layer 2 is determined. The temperature-compensated dielectric layer 2 is a thin film layer composed of barium strontium titanate powder and polytetrafluoroethylene propylene resin with a thickness of 80-150 μm. Step S3: Based on the target electrical length phase temperature coefficient of the RF cable and the pre-calibrated axial linear expansion coefficient of the RF cable, determine the target equivalent dielectric constant temperature coefficient of the dielectric structure composed of the temperature-compensated dielectric layer 2 and the foamed polytetrafluoroethylene insulation layer 3, and determine the target dielectric constant temperature coefficient of the foamed polytetrafluoroethylene insulation layer 3 based on the target equivalent dielectric constant temperature coefficient and the measured dielectric constant temperature coefficient. Step S4: Determine the target crystallinity of the foamed polytetrafluoroethylene insulating layer 3 based on the target dielectric constant temperature coefficient. Step S5: Prepare the foamed polytetrafluoroethylene insulation layer 3 based on the target crystallinity, and adjust the annealing temperature and production line transfer speed of the foamed polytetrafluoroethylene insulation layer 3 based on the measured crystallinity of the foamed polytetrafluoroethylene insulation layer 3. Step S6: On the outside of the foamed polytetrafluoroethylene insulation layer 3, the outer conductor layer 4, the shielding layer 5, and the outer sheath layer 6 are sequentially wrapped to obtain the radio frequency cable.

[0028] In this embodiment, the inner conductor 1 is drawn from an oxygen-free copper rod with a purity of 99.995%.

[0029] In this embodiment, the process of forming the microtexture includes: A rolling roller with raised texture is used to press the inner conductor 1 surface with a preset pressure. The rolling roller moves synchronously with the inner conductor 1 to press a microtexture onto the surface of the inner conductor 1.

[0030] In this embodiment, 3 to 6 rolling rollers are evenly arranged along the circumference of the inner conductor 1. The raised texture is at least one of rhombus, hexagon, cross spiral or dot matrix. The raised height is 2 to 20 μm, the raised spacing is 50 to 200 μm, and the ratio of raised height to raised spacing is not greater than 0.4.

[0031] In this embodiment, before rolling, the inner conductor 1 is preheated to 40-150°C, the preset pressure is 50-150N, the depth of the microtexture is 1-5μm, the coverage is 30%-70%, and the ratio of the microtexture depth to the radius of the inner conductor 1 is not greater than 1%. After rolling, the microtexture is cleaned and deburred, and a silver plating layer with a thickness of 0.5-2.5μm is electroplated on the surface of the microtexture, so that the residual depth of the microtexture after silver plating is not less than 50% of the depth before silver plating, and the residual coverage is not less than 80% of the coverage before silver plating, thereby preserving the outline of the microtexture.

[0032] In this embodiment, the linear speed of the rolling roller is synchronized with the traction speed of the inner conductor 1 and the speed ratio is 0.98 to 1.02.

[0033] In this embodiment, the axial linear expansion coefficient of the radio frequency cable is calibrated using a reference cable.

[0034] In this embodiment, the reference cable and the radio frequency cable to be prepared have the same inner conductor 1, and the inner conductor 1 has the same microtexture and the same thickness of silver plating layer, the same foamed polytetrafluoroethylene insulation layer 3 structure and the same radial gradient distribution of porosity, the same outer conductor layer 4 and shielding layer 5, and the same outer sheath layer 6. The only difference is that the temperature compensation dielectric layer 2 is replaced with a pure perfluoroethylene propylene layer of equal thickness, and the pure perfluoroethylene propylene layer does not contain barium strontium titanate.

[0035] In this embodiment, the reference cable is subjected to temperature cycling pretreatment, which involves cycling 3 to 5 times at a rate of not less than 5°C / min within the range of -55°C to +125°C, while maintaining a constant temperature at both ends for not less than 20 minutes, in order to release the residual stress generated by wrapping and extrusion.

[0036] In this embodiment, the electrical length phase temperature coefficient of the reference cable is measured. The phase of the reference cable is measured with temperature in the frequency range of 1GHz to 18GHz. The phase value at 6GHz is used to perform a linear regression on the temperature. The slope obtained is divided by the electrical length to obtain the electrical length phase temperature coefficient of the reference cable.

[0037] In this embodiment, determining the equivalent dielectric constant temperature coefficient of the reference cable includes: measuring the dielectric constants of the pure polytetrafluoroethylene propylene layer and the foamed polytetrafluoroethylene insulation layer 3 at 1 GHz and their temperature-dependent relationship to obtain their dielectric constant temperature coefficients; then weighting and summing them according to their radial series contribution weights, wherein the series contribution factor of each layer is the quotient obtained by dividing the natural logarithm of the ratio of the outer radius to the inner radius of the layer by the dielectric constant of the layer, and the contribution weight of the layer is the proportion of the series contribution factor of the layer to the sum of the series contribution factors of the two layers.

[0038] In this embodiment, the difference between the electrical length phase temperature coefficient of the reference cable and half of the equivalent dielectric constant temperature coefficient of the reference cable is the axial linear expansion coefficient of the radio frequency cable.

[0039] In this embodiment, since the thickness of the temperature compensation dielectric layer 2 is no more than 25% of the thickness of the foamed polytetrafluoroethylene insulation layer 3, and its resin matrix is ​​the same as that of the pure perfluoroethylene propylene layer, the axial linear expansion coefficients of the reference cable and the radio frequency cable to be prepared differ by no more than 2%, and the two are considered to be equal.

[0040] In this embodiment, the electrical length phase temperature coefficient of the radio frequency cable is the sum of half of the axial linear expansion coefficient of the radio frequency cable and the equivalent dielectric constant temperature coefficient, so that the electrical length phase temperature coefficient approaches zero, thus obtaining the target electrical length phase temperature coefficient of the radio frequency cable.

[0041] In this embodiment, the target electrical length phase temperature coefficient of the radio frequency cable is close to zero, that is, the target equivalent dielectric constant temperature coefficient is negative two times the axial linear expansion coefficient of the radio frequency cable.

[0042] Please see Figure 3 As shown, this is a flowchart illustrating the preparation of the temperature-compensated dielectric layer 2 according to an embodiment of the present invention. In this embodiment, the preparation process of the temperature-compensated dielectric layer 2 includes: Based on the target negative permittivity temperature coefficient of the temperature-compensated dielectric layer 2, the mole fraction of strontium in barium strontium titanate and the thickness of the temperature-compensated dielectric layer 2 are determined. Strontium barium titanate powder is prepared and calcined at 800-1200℃ for 1-6 hours, followed by ball milling and sieving. The preferred particle size of the powder is 0.1-2 μm. Dissolve 0.5% to 3% of the coupling agent by weight of barium strontium titanate powder in a mixed ethanol solution, add barium strontium titanate powder, ultrasonically disperse for 10 to 60 minutes, and then dry at 60 to 120°C to obtain modified barium strontium titanate powder. The modified barium strontium titanate powder was mixed with polytetrafluoroethylene propylene resin, solvent, and dispersant, and then ball-milled to prepare a uniform and stable slurry. The slurry is applied evenly to a flat substrate through a slit coating head. After drying and curing in an oven, it is peeled off from the substrate to obtain a composite film. The composite film is coated onto the surface of the inner conductor 1, which has a microtextured structure, to obtain the temperature compensation dielectric layer 2.

[0043] In this embodiment, the barium strontium titanate is a ferroelectric ceramic material with a perovskite structure, which exhibits a drastic change in dielectric constant near the Curie temperature and has a negative temperature coefficient.

[0044] In this embodiment, the chemical formula of the barium strontium titanate is Ba. 1-x Sr x TiO3 is a perovskite-type composite oxide composed of barium, strontium, titanium and oxygen. The mole fraction x of strontium (Sr) is the ratio of the number of moles of strontium to the sum of the number of moles of barium (Ba) and Sr.

[0045] In this embodiment, the Curie temperature of barium strontium titanate decreases with the increase of the mole fraction of strontium. The Curie temperature of barium strontium titanate is linearly related to the mole fraction of strontium. When the mole fraction of Sr is 0.52 to 0.70, the Curie temperature of barium strontium titanate is -83°C to -153°C.

[0046] In this embodiment, the Curie temperature of the barium strontium titanate is below -80°C, preferably -90°C to -150°C, so that the barium strontium titanate is always in the paraelectric phase within the stable phase operating temperature range, thereby providing a monotonic, continuous, and predictable negative temperature coefficient throughout the entire stable phase operating temperature range of the cable.

[0047] In this embodiment, the thickness of the temperature compensation dielectric layer 2 is 80–150 μm.

[0048] In this embodiment, barium strontium titanate powder is prepared using any one of the following methods: solid-phase method, sol-gel method, hydrothermal method, or co-precipitation method.

[0049] In this embodiment, the mass ratio of barium strontium titanate powder to polytetrafluoroethylene propylene resin is 40-58:40-58, and 0.1-2 parts of dispersant and 0.1-1 parts of antioxidant are added, with the total of all components being 100 parts.

[0050] In this embodiment, the temperature-compensated dielectric layer 2 prepared according to the above ratio has a dielectric constant of 55 to 75 at 1 GHz and a dielectric constant temperature coefficient of -6000 to -9000 ppm / ℃ in the range of -55℃ to +125℃.

[0051] In this embodiment, the composite material can be made into a film by any one of the following processes: extrusion casting, hot pressing or blow molding, and the film thickness is 80-150 μm.

[0052] In this embodiment, when the temperature compensation dielectric layer 2 is wrapped around the inner conductor 1, it is wrapped around the outer surface of the inner conductor 1 in a wrapping manner, with an overlap rate of 15% to 35% and a wrapping layer of 1 to 2 layers. After wrapping, it is heat-treated at 260 to 320°C for 5 to 30 minutes to allow the polytetrafluoroethylene propylene resin to melt, flow, and level and embed into the microtexture on the surface of the inner conductor 1, forming a mechanical interlock with the microtexture. Then, it is cooled at a rate of 5 to 20°C / min to ensure that the temperature compensation dielectric layer 2 is tightly wrapped around the inner conductor 1.

[0053] In this embodiment, the dielectric constant temperature coefficient of the temperature-compensated dielectric layer 2 is obtained by measuring the dielectric constant of the temperature-compensated dielectric layer 2 and its relationship with temperature within a stable operating temperature range of -55℃ to +125℃ and a frequency range of 1MHz to 40GHz using a dielectric spectrometer, impedance analyzer, or network analyzer.

[0054] In this embodiment, the target dielectric constant temperature coefficient of the foamed polytetrafluoroethylene insulation layer 3 is determined based on the measured dielectric constant temperature coefficient of the temperature-compensated dielectric layer 2 and the axial linear expansion coefficient of the radio frequency cable, as well as the contribution weights of the temperature-compensated dielectric layer 2 and the foamed polytetrafluoroethylene insulation layer 3.

[0055] In this embodiment, the electrical length phase temperature coefficient of the radio frequency cable is the sum of half of the axial linear expansion coefficient of the radio frequency cable and the equivalent dielectric constant temperature coefficient, so that the target electrical length phase temperature coefficient of the radio frequency cable approaches zero.

[0056] In this embodiment, the equivalent dielectric constant temperature coefficient is the sum of the measured dielectric constant temperature coefficient of the temperature-compensated dielectric layer 2 after being weighted according to its contribution and the dielectric constant temperature coefficient of the foamed polytetrafluoroethylene insulating layer 3 after being weighted according to its contribution. Based on this, the target dielectric constant temperature coefficient of the foamed polytetrafluoroethylene insulating layer 3 is determined, which is obtained by subtracting the measured dielectric constant temperature coefficient of the temperature-compensated dielectric layer 2 after being weighted according to its contribution from the target equivalent dielectric constant temperature coefficient, and then dividing by the contribution weight of the foamed polytetrafluoroethylene insulating layer 3.

[0057] In this embodiment, the negative dielectric constant temperature coefficient of the temperature-compensated dielectric layer 2 is used to offset the positive phase drift introduced by the axial linear expansion coefficient of the radio frequency cable, and the dielectric constant temperature coefficient of the foamed polytetrafluoroethylene insulation layer 3 is always negative. The two are superimposed with the same sign and cannot cancel each other out.

[0058] In this embodiment, the contribution weights of the temperature-compensated dielectric layer 2 and the foamed polytetrafluoroethylene insulation layer 3 are determined according to the design requirements of the radio frequency cable. The dielectric structure between the inner conductor 1 and the outer conductor is considered as the temperature-compensated dielectric layer 2 and the foamed polytetrafluoroethylene insulation layer 3 connected in series. Based on the series capacitance relationship per unit length of the coaxial cable, the contribution of each layer to the overall equivalent dielectric constant temperature coefficient is jointly determined by the radial geometric factor and dielectric constant of each layer.

[0059] In this embodiment, at a reference temperature, the series contribution factors of the temperature-compensated dielectric layer 2 and the foamed polytetrafluoroethylene insulating layer 3 are calculated respectively. The series contribution factor of the temperature-compensated dielectric layer 2 is its radial geometric factor divided by its dielectric constant, wherein the radial geometric factor is the natural logarithm of the ratio of the outer radius of the temperature-compensated dielectric layer 2 to the outer radius of the inner conductor 1; the series contribution factor of the foamed polytetrafluoroethylene insulating layer 3 is its radial geometric factor divided by its dielectric constant, wherein the radial geometric factor is the natural logarithm of the ratio of the outer radius of the foamed polytetrafluoroethylene insulating layer 3 to the outer radius of the temperature-compensated dielectric layer 2.

[0060] In this embodiment, the contribution weight of the temperature-compensated dielectric layer 2 is the ratio of the series contribution factor of the temperature-compensated dielectric layer 2 to the sum of the series contribution factors of the temperature-compensated dielectric layer 2 and the series contribution factors of the foamed polytetrafluoroethylene insulation layer 3; the contribution weight of the foamed polytetrafluoroethylene insulation layer 3 is the ratio of the series contribution factor of the foamed polytetrafluoroethylene insulation layer 3 to the sum of the series contribution factors of the temperature-compensated dielectric layer 2 and the series contribution factors of the foamed polytetrafluoroethylene insulation layer 3.

[0061] In this embodiment, the thickness of the temperature compensation dielectric layer 2 is 80-150 μm, so that the contribution weight of the temperature compensation dielectric layer 2 is 0.38%-0.76%, thereby reducing the electrical length phase temperature coefficient of the RF cable from 21.0 ppm / ℃ when the temperature compensation dielectric layer 2 is not provided to below 8 ppm / ℃.

[0062] In this embodiment, a pre-established correspondence between the crystallinity of the foamed polytetrafluoroethylene insulation layer 3 and its dielectric constant temperature coefficient is established. Specifically, the same foaming agent system and foaming process as the radio frequency cable to be prepared are used, i.e., a bimodal pore size foaming agent system composed of 1,1,1,3,3-pentafluoropropane (HFC-245fa) and supercritical CO2 is used. Under the condition of maintaining the same radial gradient distribution of porosity, bimodal pore size structure, closed-cell ratio, foaming ratio, and temperature compensation dielectric layer 2 parameters, a set of foamed polytetrafluoroethylene samples are prepared, with no fewer than 5 samples. By adjusting process parameters such as heat treatment temperature, holding time, heating and cooling rates, and cooling rates, the crystallinity of each sample is made to fall within the range of 60% to 75%, and the crystallinity interval between adjacent samples is no more than 3 percentage points. For each sample, the crystallinity was determined using differential scanning calorimetry (DSC). DSC was preferably performed under a nitrogen atmosphere at a heating rate of 10 °C / min. The crystallinity was calculated based on the ratio of the enthalpy of fusion to the enthalpy of fusion of fully crystalline PTFE, where the enthalpy of fusion of fully crystalline PTFE was taken as 82 J / g. Then, within the stable operating temperature range of the RF cable, at least five temperature points were selected, and the dielectric constant of each sample was measured as a function of temperature using an impedance analyzer or network analyzer in the frequency range of 1 GHz to 18 GHz. The temperature coefficient of dielectric constant for each sample was calculated. A one-to-one correspondence between the crystallinity of each sample and its corresponding temperature coefficient of dielectric constant was established to form a fitting curve showing the relationship between the crystallinity and the temperature coefficient of dielectric constant of the foamed PTFE insulation layer 3.

[0063] In this embodiment, when using differential scanning calorimetry (DSC) to determine crystallinity, the melting behavior of crystalline and amorphous regions is difficult to completely separate; when using X-ray diffraction (XRD) to determine crystallinity, only the diffraction intensity of the crystalline phase is considered. The measured values ​​from the two methods cannot be directly compared. Therefore, the crystallinity of the same group of samples is pre-determined using both DSC and XRD. A linear correspondence is established between the DSC measurement as the baseline and the XRD measurement as the independent variable. That is, the crystallinity measured by DSC is equal to the crystallinity measured by XRD multiplied by a calibration coefficient plus a calibration constant. The calibration coefficient and calibration constant are obtained by fitting the two sets of measured values ​​from the same group of samples. After determining the calibration coefficient and calibration constant, the measured crystallinity of the foamed polytetrafluoroethylene insulation layer 3 is determined using XRD. The measured value of XRD is substituted into the above linear correspondence to calculate the equivalent crystallinity of the DSC, which is then compared with the target crystallinity.

[0064] In this embodiment, the crystallinity of the foamed polytetrafluoroethylene insulating layer 3 is negatively correlated with the temperature coefficient of dielectric constant. That is, when the crystallinity increases, the proportion of crystalline regions increases, the thermal motion of molecular chain segments is restricted, and the density change caused by thermal expansion decreases. Consequently, the absolute value of the temperature coefficient of dielectric constant of the foamed polytetrafluoroethylene insulating layer 3 decreases and its value tends to be positive.

[0065] In this embodiment, the foamed polytetrafluoroethylene insulation layer 3 is prepared in one step by a multi-layer co-extrusion mold, forming a four-layer structure consisting of an inner dense layer 3a, a transition layer 3b, a high-foaming layer 3c, and an outer dense layer 3d arranged sequentially from the inside out. The inner dense layer 3a has the lowest porosity, ranging from 5% to 15%, and is adjacent to the temperature-compensated dielectric layer 2, providing high interfacial bonding strength and excellent dielectric strength. The transition layer 3b has a porosity between the inner dense layer 3a and the high-foaming layer 3c, ranging from 20% to 35%, achieving a smooth and gradual change in porosity, effectively alleviating stress concentration that may be caused by abrupt structural changes. The high-foaming layer 3c is the main body of the foamed polytetrafluoroethylene insulation layer 3, with the highest porosity, ranging from 60% to 70%, to maximize the introduction of air with a low dielectric constant, thereby reducing the overall dielectric constant of the cable. The outer dense 3d layer also has a low porosity of 10% to 20%, which is used to enhance the bonding force with the outer conductor and to act as a physical barrier to prevent the intrusion of external moisture.

[0066] In this embodiment, the thickness of each layer accounts for the proportion of the total wall thickness of the foamed polytetrafluoroethylene insulation layer 3 as follows: inner dense layer 3a 8%–15%, transition layer 3b 12%–20%, high foaming layer 3c 50%–65%, and outer dense layer 3d 0%–18%.

[0067] In this embodiment, the target content of HFC-245fa and supercritical CO2 in each layer of premix is ​​set according to porosity: in the high foaming layer 3c, HFC-245fa accounts for 5% of the resin mass and supercritical CO2 accounts for 3% of the resin mass; in the inner dense layer 3a, HFC-245fa accounts for 1% of the resin mass and supercritical CO2 accounts for 0.5% of the resin mass; and the transition layer 3b and the outer dense layer 3d are selected between the two target porosities. A nucleating agent accounting for 0.5% to 2% of the resin mass is added to each layer of premix. The nucleating agent is polytetrafluoroethylene ultrafine powder or boron nitride with a particle size of 50 to 200 nm. Each layer of premix is ​​placed in a sealed container, and HFC-245fa and supercritical CO2 are introduced for saturated impregnation for 12 to 48 hours at 20 to 40°C and 2 to 6 MPa to allow the foaming agent to reach dissolution equilibrium in the resin.

[0068] In this embodiment, four groups of saturated impregnated premixes are mixed with an extrusion aid comprising 18% to 25% of the resin mass. The extrusion aid is an isoparaffin. The mixture is then extruded as a paste through a four-channel multi-layer co-extrusion die at 30–60°C and a pressure of 10–18 MPa, sequentially forming a concentric structure of four layers: an inner dense layer 3a, a transition layer 3b, a high-foaming layer 3c, and an outer dense layer 3d. When the melt exits through the gradient die, the pressure drops sharply, triggering uniform nucleation and foaming of the foaming agent.

[0069] In this embodiment, the billet obtained by paste extrusion is first treated in a drying furnace at 120-200°C for 10-40 minutes to allow the extrusion aid to fully volatilize and be removed, and then enters a controlled atmosphere gradient sintering furnace for sintering.

[0070] In this embodiment, the foamed billet is immediately placed into a controlled atmosphere gradient sintering furnace for sintering at a temperature of 360–380°C for 10–40 minutes. Pure nitrogen gas is circulated throughout the furnace, with a flow rate of 8 L / min at the inlet, 12 L / min in the middle section, and 8 L / min at the outlet. The oxygen content is no more than 10 ppm. The pure nitrogen gas is used to suppress oxidation of polytetrafluoroethylene at the sintering temperature, preventing the formation of polar groups such as carbonyl and carboxyl groups at the chain ends, which would increase the dielectric loss tangent. After sintering, the billet is placed in an annealing furnace for isothermal annealing at 300°C for 3 hours.

[0071] Please see Figure 4 The diagram shows a flowchart illustrating the adjustment of the annealing temperature and production line transport speed of the foamed polytetrafluoroethylene (PTFE) insulation layer 3 according to an embodiment of the present invention. In this embodiment, an online X-ray diffraction system with a 40W micro-focusing X-ray source and an area array detector is used at the outlet of the middle section of the annealing furnace to collect the crystal diffraction peaks of PTFE in real time in transmission mode. The measured crystallinity of the foamed PTFE insulation layer 3 is determined in real time using the Rietveld refinement method. The measured crystallinity is converted into the equivalent crystallinity of differential scanning calorimetry according to the above calibration relationship and compared with the target crystallinity. When the measured crystallinity is less than the target crystallinity, the annealing temperature is increased or the production line transport speed is decreased; when the measured crystallinity is greater than the target crystallinity, the annealing temperature is decreased or the production line transport speed is increased, so that the deviation between the measured crystallinity and the target crystallinity is controlled within the allowable deviation range.

[0072] In this embodiment, after annealing, the temperature of the foamed polytetrafluoroethylene insulation layer 3 is cooled from the annealing temperature to below 100°C at a cooling rate of 12°C / min, and then naturally cooled to room temperature.

[0073] In this embodiment, after the preparation of the foamed polytetrafluoroethylene insulation layer 3 is completed, the silver-plated copper flat strip is obliquely wrapped around the outer conductor layer 4. A high-precision constant tension winding machine is used to tightly and obliquely wind a 0.08mm × 2.5mm silver-plated copper flat strip around the outer surface of the foamed polytetrafluoroethylene insulation layer 3 at a 35° helix angle and an 18% overlap rate under a constant tension of 5N, forming the outer conductor layer 4. The silver-plated copper flat strip is obliquely wound along the axial direction of the RF cable, so that adjacent turns overlap each other without gaps, thereby simultaneously providing conductivity and shielding, and applying radial constraint to the foamed polytetrafluoroethylene insulation layer 3 and the temperature-compensated dielectric layer 2 along the circumference of the RF cable.

[0074] In this embodiment, a shielding layer 5 with a braiding density of 92% is woven from silver-plated copper wire with a diameter of 0.12 mm on the outside of the outer conductor layer 4.

[0075] In this embodiment, a 0.4 mm thick polytetrafluoroethylene propylene outer sheath layer 6 is extruded using a single-screw extruder at a temperature of 280°C. The polytetrafluoroethylene propylene outer sheath layer 6 has a tensile strength of not less than 20 MPa, an elongation at break of not less than 250%, a dielectric strength of not less than 20 kV / mm, and a volume resistivity of not less than 1 × 10⁻⁶. 16 Ω·m, to complete the overall fabrication of the radio frequency cable.

[0076] In this embodiment, after the radio frequency cable is prepared, it is subjected to temperature cycling pretreatment at a rate of not less than 5℃ / min within the range of -55℃ to +125℃ for 3 to 5 times, and the two ends are kept at a constant temperature for not less than 20 minutes to release the residual stress generated by wrapping and extrusion, and to avoid irreversible phase drift of the radio frequency cable during the first temperature cycle.

[0077] Example 1 The inner conductor 1 is drawn from an oxygen-free copper rod with a diameter of 1.0 mm. After preheating to 90°C, it is rolled with four rolling rollers with diamond-shaped raised patterns on the surface under a pressure of 100 N to form a microtexture with a depth of 3 μm and a coverage of 50%. After rolling, it is cleaned to remove burrs and then electroplated with a silver plating layer with a thickness of 1.5 μm. The residual depth of the microtexture is 1.8 μm and the residual coverage is 45%. The temperature compensation dielectric layer 2 is formed by wrapping a composite film of barium strontium titanate and perfluoroethylene propylene. The chemical formula of barium strontium titanate is Ba. 0.4 Sr 0.6TiO3, Curie temperature -114℃, powder particle size 0.5~1μm, barium strontium titanate powder was surface modified with 1.5% silane coupling agent by mass and mixed with polytetrafluoroethylene propylene resin at 50% solid mass each. The composite film thickness was 110μm. After being wrapped in a single layer with an overlap rate of 25%, it was heat-treated at 300℃ for 15min and cooled at 10℃ / min. The outer radius of the temperature compensation dielectric layer 2 was 0.61mm. The measured dielectric constant at 25℃ and 1GHz was 65. The measured temperature coefficient of dielectric constant in the range of -55℃~+125℃ was -7194ppm / ℃. The foamed polytetrafluoroethylene insulation layer 3 adopts a four-layer radial gradient structure: the inner dense layer 3a has a porosity of 10%, the transition layer 3b has a porosity of 28%, the high foaming layer 3c has a porosity of 65%, and the outer dense layer 3d has a porosity of 15%. The thicknesses of the four layers account for 12%, 16%, 56%, and 16% of the total wall thickness, respectively. Each layer of premixed material is mixed with 1% polytetrafluoroethylene ultrafine powder nucleating agent with a particle size of 100nm, and is saturated with HFC-245fa and supercritical CO2 for 24h at 30℃ and 4MPa. After being mixed with isoparaffinic extrusion aid accounting for 20% of the resin mass, it is co-extruded in four channels at 45℃ and 14MPa. The extrusion aid is removed at 160℃ for 25min, sintered at 370℃ for 25min, and annealed at 300℃ for 3h. The annealing temperature and production line transfer speed are adjusted based on the crystallinity measured by online X-ray diffraction. The thickness on one side is 0.75 mm, the outer radius is 1.36 mm, and the measured dielectric constant at 25℃ and 1GHz is 1.45. The outer conductor layer 4 is made of 0.08mm×2.5mm silver-plated copper flat strip with a 35° helix angle, 18% overlap rate, and 5N tension, and is obliquely wrapped. The shielding layer 5 is made of 0.12mm diameter silver-plated copper wire in a single layer braid with a braiding density of 92%. The outer sheath layer 6 is made of polytetrafluoroethylene propylene extruded at 280℃ with a thickness of 0.4mm.

[0078] The difference between the reference cable and the RF cable to be prepared is that the temperature-compensated dielectric layer 2 is replaced with a pure polytetrafluoroethylene propylene layer with a thickness of 110μm and without barium strontium titanate. After the reference cable is cyclically run at 5℃ / min for 4 times in the range of -55℃ to +125℃ and kept at constant temperature at both ends for 30min, the measured phase temperature coefficient of the electrical length is 21.0ppm / ℃. The equivalent dielectric constant temperature coefficient, which is obtained by weighting and summing the series contribution factors of each layer, is -52.0ppm / ℃. After deducting half of this value, the axial linear expansion coefficient of the RF cable is 47.0ppm / ℃.

[0079] The target electrical length phase temperature coefficient is taken to be close to zero, therefore the target equivalent dielectric constant temperature coefficient is -94.0 ppm / ℃. The series contribution factor of the temperature-compensated dielectric layer 2 is the ratio of the natural logarithm of the ratio of its inner and outer radii to its dielectric constant. The series contribution factor of the foamed polytetrafluoroethylene insulation layer 3 is obtained in the same way. After normalization, the contribution weight of the temperature-compensated dielectric layer 2 is 0.55%, and the contribution weight of the foamed polytetrafluoroethylene insulation layer 3 is 99.45%. The dielectric constant temperature coefficient of the temperature-compensated dielectric layer 2 is converted according to its contribution weight to -39.6 ppm / ℃. After deducting this converted value from the target equivalent dielectric constant temperature coefficient, the final value is... Dividing by the contribution weight of the expanded polytetrafluoroethylene insulation layer 3, the target dielectric constant temperature coefficient of the expanded polytetrafluoroethylene insulation layer 3 is -54.7 ppm / ℃; according to the pre-established fitting curve of crystallinity and dielectric constant temperature coefficient, the target crystallinity is 67.5%; the crystallinity measured by online X-ray diffraction is converted into the equivalent crystallinity of differential scanning calorimetry of 66.8% according to the linear calibration relationship, which is 0.7% different from the target crystallinity. Therefore, the annealing temperature of 300℃ and the production line transfer speed are kept unchanged; after annealing, it is cooled to below 100℃ at 12℃ / min and then naturally cooled to room temperature.

[0080] After the finished cable underwent temperature cycling pretreatment within the range of -55℃ to +125℃, cycling at 5℃ / min for 4 times and maintaining constant temperature at both ends for 30 minutes, the following measurements were taken: electrical length phase temperature coefficient 1.9ppm / ℃, phase-temperature nonlinearity 12ppm, phase drift 42ppm after 20 temperature cycles, 180° peel strength between temperature-compensated dielectric layer 2 and inner conductor 1.85N / mm, characteristic impedance 50.2Ω, and 18GHz attenuation 1.62dB / m.

[0081] Example 2 The materials for each layer are the same as in Example 1. The thickness of the temperature compensation dielectric layer 2 is changed to 140 μm, and the chemical formula of barium strontium titanate is changed to Ba. 0.35 S r0.65 TiO3 was calcined at 1120℃ for 3.5 hours and held at that temperature for 3 hours. The Curie temperature was -133.5℃. After wrapping, the outer radius of the temperature-compensated dielectric layer 2 was 0.64mm, and the thickness of the foamed polytetrafluoroethylene insulation layer 3 on one side was changed to 0.72mm. The measured dielectric constant of the temperature-compensated dielectric layer 2 at 25℃ and 1GHz was 68, and the temperature coefficient of the dielectric constant in the range of -55℃ to +125℃ was -6309ppm / ℃. The dielectric constant of the foamed polytetrafluoroethylene insulation layer 3 was 1.43. The temperature-compensated dielectric layer 2 contributes 0.68% and the expanded polytetrafluoroethylene insulation layer 3 contributes 99.32%. The temperature coefficient of dielectric constant of the temperature-compensated dielectric layer 2 is -43.1 ppm / ℃, and the target temperature coefficient of dielectric constant of the expanded polytetrafluoroethylene insulation layer 3 is -51.3 ppm / ℃. The target crystallinity is found to be 62%, and the equivalent crystallinity measured by differential scanning calorimetry is 61.3%, with a deviation of 0.7%. The annealing temperature and production line transfer speed are kept constant.

[0082] The electrical length phase temperature coefficient is -1.4ppm / ℃, the phase-temperature nonlinearity is 15ppm, the phase drift after 20 temperature cycles is 48ppm, the 180° peel strength is 1.92N / mm, the characteristic impedance is 50.0Ω, and the 18GHz attenuation is 1.68dB / m.

[0083] Example 3 The materials for each layer are the same as in Example 1. The thickness of the temperature compensation dielectric layer 2 is changed to 80 μm, and the chemical formula of barium strontium titanate is changed to Ba. 0.45 Sr 0.55 TiO3, calcined at 1080℃ and held for 2.5h, Curie temperature -94.5℃, outer radius of the temperature compensation dielectric layer 2 after wrapping is 0.58mm, and the thickness of the foamed polytetrafluoroethylene insulation layer 3 on one side is changed to 0.78mm. The measured dielectric constant of the temperature-compensated dielectric layer 2 at 25℃ and 1GHz is 62, and the dielectric constant temperature coefficient within the range of -55℃ to +125℃ is -8368ppm / ℃. The dielectric constant of the foamed PTFE insulation layer 3 is 1.47. The contribution weight of the temperature-compensated dielectric layer 2 is 0.41%, and the contribution weight of the foamed PTFE insulation layer 3 is 99.59%. The converted value of the dielectric constant temperature coefficient of the temperature-compensated dielectric layer 2 is -34.4ppm / ℃, and the target dielectric constant temperature coefficient of the foamed PTFE insulation layer 3 is -59.9ppm / ℃. The target crystallinity obtained by reverse lookup is 73.0%, and the equivalent crystallinity measured by differential scanning calorimetry is 72.4%, with a deviation of 0.6%, while keeping the annealing temperature and production line transmission speed constant.

[0084] The electrical length phase temperature coefficient is 2.7 ppm / ℃, the phase-temperature nonlinearity is 21 ppm, the phase drift after 20 temperature cycles is 68 ppm, the 180° peel strength is 1.71 N / mm, the characteristic impedance is 50.4 Ω, and the 18 GHz attenuation is 1.58 dB / m.

[0085] Example 4 The temperature-compensated dielectric layer 2 was modified by directly coating the slurry onto the surface of the inner conductor 1, which has a microtextured structure, through a slit coating head. After drying and curing, it was heat-treated at 300℃ for 15 minutes to melt and level the polytetrafluoroethylene propylene resin and embed it into the microtextured structure to form a mechanical interlock. No film wrapping was performed, and the thickness of the temperature-compensated dielectric layer 2 remained at 110 μm. The materials and specifications of the remaining layers were the same as in Example 1. The measured dielectric constant of the temperature-compensated dielectric layer 2 at 25℃ and 1GHz was 70, and its dielectric constant temperature coefficient within the range of -55℃ to +125℃ was -7194 ppm / ℃, contributing 0.51% of the total dielectric constant. The converted value of the dielectric constant temperature coefficient was -36.8 ppm / ℃. The target dielectric constant temperature coefficient of the foamed polytetrafluoroethylene insulation layer 3 was -57.5 ppm / ℃. The target crystallinity was found to be 70.5%, and the measured equivalent crystallinity by differential scanning calorimetry was 69.8%, with a deviation of 0.7%.

[0086] The electrical length phase temperature coefficient is 2.2 ppm / ℃, the phase-temperature nonlinearity is 13 ppm, the phase drift after 20 temperature cycles is 40 ppm, the 180° peel strength is 2.05 N / mm, the characteristic impedance is 50.1 Ω, and the 18 GHz attenuation is 1.61 dB / m. This confirms that the present invention is also applicable to the directly coated temperature-compensated dielectric layer 2, and the interface between the coating layer and the inner conductor 1 has no overlapping seam, further improving the peel strength compared to Example 1.

[0087] Example 5 The radial gradient of the expanded polytetrafluoroethylene (PTFE) insulation layer 3 was changed from four layers to three layers: an inner dense layer 3a with a porosity of 12%, a highly foamed layer 3c with a porosity of 63%, and an outer dense layer 3d with a porosity of 18%. The thicknesses of the three layers account for 15%, 60%, and 25% of the total wall thickness, respectively, and the transition layer 3b was eliminated. The materials and specifications of the remaining layers are the same as in Example 1. The axial linear expansion coefficient of the reference cable was calibrated to be 47.5 ppm / ℃, and the target equivalent dielectric constant temperature coefficient was -95.0 ppm / ℃. The target dielectric constant temperature coefficient of the expanded polytetrafluoroethylene insulation layer 3 was -55.7 ppm / ℃. The target crystallinity was found to be 68.5%, and the measured equivalent crystallinity by differential scanning calorimetry was 67.9%, with a deviation of 0.6%.

[0088] The electrical length phase temperature coefficient is -0.8 ppm / ℃, the phase-temperature nonlinearity is 18 ppm, the phase drift after 20 temperature cycles is 52 ppm, the 180° peel strength is 1.74 N / mm, the characteristic impedance is 50.3 Ω, and the attenuation at 18 GHz is 1.65 dB / m. This confirms that the proposed solution is also applicable to three-layer radial gradient structures.

[0089] Comparative Example 1 The materials and specifications of each layer are the same as in Example 1, but no microtexture is formed on the outer surface of the inner conductor 1, that is, the rolling step is omitted, and a silver plating layer with a thickness of 1.5 μm is directly electroplated on the smooth surface of the inner conductor 1. The measured peel strength between the temperature compensated dielectric layer 2 and the inner conductor 1 at 80° is only 0.42 N / mm, and the interface slips during temperature cycling, with the electrical length phase temperature coefficient rising to 6.8 ppm / ℃.

[0090] The electrical length phase temperature coefficient is 6.8 ppm / ℃, the phase-temperature nonlinearity is 38 ppm, the phase drift after 20 temperature cycles is 104 ppm, the 180° peel strength is 0.42 N / mm, the characteristic impedance is 50.3 Ω, and the 18 GHz attenuation is 1.53 dB / m.

[0091] Comparative Example 2 The materials and specifications of each layer are the same as in Example 1, but the temperature-compensated dielectric layer 2 is replaced with a pure perfluoroethylene propylene layer with a thickness of 110 μm that does not contain barium strontium titanate. This comparative example is the reference cable used in Example 1. The temperature coefficient of the equivalent dielectric constant is -52.0 ppm / ℃, which is superimposed in the same direction as the axial linear expansion coefficient of 47.0 ppm / ℃, and the positive phase drift is not compensated.

[0092] The electrical length phase temperature coefficient is 21.0 ppm / ℃, the phase-temperature nonlinearity is 96 ppm, the phase drift after 20 temperature cycles is 188 ppm, the 180° peel strength is 1.24 N / mm, the characteristic impedance is 49.0 Ω, and the 18 GHz attenuation is 1.60 dB / m.

[0093] Comparative Example 3 The materials and specifications of each layer are the same as in Example 1, but the molar fraction of strontium in barium strontium titanate is 0.25, and the chemical formula is Ba. 0.75 Sr 0.25 TiO3, with a Curie temperature of 22.5℃, falls within the stable operating temperature range of -55℃ to +125℃. The measured dielectric constant of the temperature-compensated dielectric layer 2 first increases and then decreases within the operating temperature range, peaking near 22.5℃. Its average dielectric constant within the operating temperature range reaches 274, significantly higher than the 65 of Example 1. Consequently, the series contribution factor decreases, with the contribution weight dropping from 0.55% to 0.13%, indicating that the temperature compensation effect is almost ineffective.

[0094] The electrical length phase temperature coefficient is 15.3 ppm / ℃, the phase-temperature nonlinearity is 142 ppm, the phase drift after 20 temperature cycles is 265 ppm, the 180° peel strength is 1.58 N / mm, the characteristic impedance is 50.1 Ω, and the 18 GHz attenuation is 1.61 dB / m.

[0095] Comparative Example 4 The materials and specifications of each layer are the same as in Example 1, but the thickness of the temperature compensation dielectric layer 2 is 20 μm, the outer radius of the temperature compensation dielectric layer 2 after wrapping is 0.52 mm, and the thickness of the foamed polytetrafluoroethylene insulation layer 3 on one side is 0.84 mm. The measured contribution weight of the temperature compensation dielectric layer 2 is only 0.09%, and the converted value of the dielectric constant temperature coefficient is less than -6.5 ppm / ℃, indicating a serious deficiency in compensation.

[0096] The electrical length phase temperature coefficient is 16.4 ppm / ℃, the phase-temperature nonlinearity is 64 ppm, the phase drift after 20 temperature cycles is 152 ppm, the 180° peel strength is 1.35 N / mm, the characteristic impedance is 50.6 Ω, and the 18 GHz attenuation is 1.59 dB / m.

[0097] Comparative Example 5 The materials and specifications of each layer are the same as in Example 1, but the annealing temperature and production line transfer speed are not adjusted according to the measured crystallinity. The annealing temperature is fixed at 270℃ and the holding time is fixed at 2h. The online X-ray diffraction system is not used. The measured equivalent crystallinity by differential scanning calorimetry is 48.0%, which is lower than the target crystallinity of 67.5%. The temperature coefficient of dielectric constant of the foamed polytetrafluoroethylene insulation layer 3 is only -40.2ppm / ℃, which is 14.5ppm / ℃ lower than the target value of -54.7ppm / ℃.

[0098] The electrical length phase temperature coefficient is 7.2 ppm / ℃, the phase-temperature nonlinearity is 47 ppm, the phase drift after 20 temperature cycles is 118 ppm, the 180° peel strength is 1.62 N / mm, the characteristic impedance is 50.5 Ω, and the 18 GHz attenuation is 1.57 dB / m.

[0099] Comparative Example 6 The materials and specifications of each layer are the same as in Example 1, but the foamed polytetrafluoroethylene insulation layer 3 has a uniform porosity structure without radial gradient, and the porosity of the entire wall thickness is 45%. It does not have an inner dense layer 3a, a transition layer 3b, or an outer dense layer 3d, and the thickness on one side remains 0.75 mm. Because of the lack of radial confinement of the high-foaming layer 3c by the inner dense layer 3a and the outer dense layer 3d, the foamed polytetrafluoroethylene insulation layer 3 can freely elongate axially when heated. The axial linear expansion coefficient obtained from the reference cable calibration increases to 58.0 ppm / ℃, higher than the 47.0 ppm / ℃ of Example 1.

[0100] Electrical length phase temperature coefficient 11.0ppm / ℃, phase-temperature nonlinearity 31ppm, phase drift after 20 temperature cycles 96ppm, 180° peel strength 1.55N / mm, characteristic impedance 50.2Ω, 18GHz attenuation 1.64dB / m.

[0101] As can be seen from the above embodiments and comparative examples, the absolute value of the electrical length phase temperature coefficient of Embodiments 1 to 5 is not greater than 2.7 ppm / ℃, the phase-temperature nonlinearity is not greater than 21 ppm, the phase drift after 20 temperature cycles is not greater than 68 ppm, and the 180° peel strength between the temperature-compensated dielectric layer 2 and the inner conductor 1 is not less than 1.71 N / mm. In Comparative Examples 1 to 6, the minimum absolute value of the electrical length phase temperature coefficient was 6.8 ppm / ℃, the minimum phase-temperature nonlinearity was 31 ppm, the minimum phase drift after temperature cycling was 96 ppm, and the maximum peel strength was 1.62 N / mm. The best values ​​of all four indicators were worse than the worst values ​​of the examples. Among them, Comparative Example 2, compared with Example 1, only omitted the addition of barium strontium titanate and replaced the temperature-compensated dielectric layer 2 with a pure perfluoroethylene propylene layer of equal thickness. The electrical length phase temperature coefficient increased from 1.9 ppm / ℃ to 21.0 ppm / ℃, indicating that the barium strontium titanate temperature-compensated dielectric layer 2 has a substantial compensating effect on the positive phase drift caused by axial linear expansion.

[0102] Compared with Example 1, Comparative Example 3 only changed the mole fraction of strontium from 0.60 to 0.25, increased the Curie temperature from -114℃ to 22.5℃, thus falling into the stable operating temperature range, changed the electric length phase temperature coefficient from 1.9ppm / ℃ to 15.3ppm / ℃, and increased the phase-temperature nonlinearity from 12ppm to 142ppm. This shows that the Curie temperature being below the lower limit of the stable operating temperature range is a necessary condition for temperature compensation to remain monotonous, continuous, and predictable. Compared with Example 1, Comparative Example 4 only reduced the thickness of the temperature compensation dielectric layer 2 from 110μm to 20μm, and reduced the contribution weight from 0.55% to 0.09%. This shows that the thickness of the temperature compensation dielectric layer 2 must be sufficient to allow the compensation amount to enter the effective range.

[0103] The technical solution of the present invention has been described above with reference to the preferred embodiments shown in the accompanying drawings. However, it will be readily understood by those skilled in the art that the scope of protection of the present invention is obviously not limited to these specific embodiments. Without departing from the principles of the present invention, those skilled in the art can make equivalent changes or substitutions to the relevant technical features, and the technical solutions after these changes or substitutions will all fall within the scope of protection of the present invention.

Claims

1. A method for preparing a phase-stable radio frequency cable, characterized in that, include: An inner conductor of a radio frequency cable is prepared and a microtexture is formed on the outer surface of the inner conductor to enhance the mechanical bonding force with adjacent layers; A temperature-compensated dielectric layer is coated on the inner conductor having the microtexture and the measured temperature coefficient of the dielectric constant of the temperature-compensated dielectric layer is determined. The temperature-compensated dielectric layer is a thin film layer composed of barium strontium titanate powder and polytetrafluoroethylene propylene resin with a thickness of 80-150 μm. Based on the target electrical length phase temperature coefficient of the radio frequency cable and the pre-calibrated axial linear expansion coefficient of the radio frequency cable, the target equivalent dielectric constant temperature coefficient of the dielectric structure composed of the temperature-compensated dielectric layer and the foamed polytetrafluoroethylene insulation layer is determined, and the target dielectric constant temperature coefficient of the foamed polytetrafluoroethylene insulation layer is determined based on the target equivalent dielectric constant temperature coefficient and the measured dielectric constant temperature coefficient. The target crystallinity of the foamed polytetrafluoroethylene insulating layer is determined based on the target dielectric constant temperature coefficient. The foamed polytetrafluoroethylene insulation layer is prepared based on the target crystallinity, and the annealing temperature and production line transfer speed of the foamed polytetrafluoroethylene insulation layer are adjusted based on the measured crystallinity of the foamed polytetrafluoroethylene insulation layer. An outer conductor layer, a shielding layer, and an outer sheath layer are sequentially wrapped around the outside of the foamed polytetrafluoroethylene insulation layer to obtain a radio frequency cable.

2. The method for preparing a phase-stable radio frequency cable according to claim 1, characterized in that, The depth of the microtexture is 1–5 μm and not greater than 1% of the radius of the inner conductor, with a coverage of 30%–70%. The inner conductor also has a silver plating layer on the surface of the microtexture, the thickness of which is 0.5–2.5 μm and less than the depth of the microtexture.

3. The method for preparing a phase-stable radio frequency cable according to claim 1, characterized in that, The axial linear expansion coefficient is determined based on the electrical length phase temperature coefficient and the equivalent dielectric constant temperature coefficient of the reference cable.

4. The method for preparing a phase-stable radio frequency cable according to claim 1, characterized in that, The preparation process of the temperature compensation dielectric layer includes: Based on the target negative permittivity temperature coefficient of the temperature-compensated dielectric layer, the mole fraction of strontium in barium strontium titanate and the thickness of the temperature-compensated dielectric layer are determined. Strontium barium titanate powder was prepared and calcined at 800–1200°C for 1–6 h, followed by ball milling and sieving. Dissolve 0.5% to 3% of the coupling agent by weight of barium strontium titanate powder in a mixed ethanol solution, add barium strontium titanate powder, ultrasonically disperse for 10 to 60 minutes, and then dry at 60 to 120°C to obtain modified barium strontium titanate powder. The modified barium strontium titanate powder was mixed with polytetrafluoroethylene propylene resin, solvent, and dispersant, and then ball-milled to prepare a uniform and stable slurry. The slurry is applied evenly to a flat substrate through a slit coating head. After drying and curing in an oven, it is peeled off from the substrate to obtain a composite film. The composite film is coated onto the surface of the inner conductor with a microtexture to obtain the temperature-compensated dielectric layer.

5. The method for preparing a phase-stable radio frequency cable according to claim 4, characterized in that, The chemical formula of the barium strontium titanate is Ba. 1-x Sr x TiO3, wherein the molar fraction x of strontium is 0.52 to 0.70, and the Curie temperature of the barium strontium titanate is below -80°C.

6. The method for preparing a phase-stable radio frequency cable according to claim 1, characterized in that, The target dielectric constant temperature coefficient of the foamed polytetrafluoroethylene insulation layer is determined based on the measured dielectric constant temperature coefficient of the temperature-compensated dielectric layer and the axial linear expansion coefficient of the RF cable, as well as the contribution weights of the temperature-compensated dielectric layer and the foamed polytetrafluoroethylene insulation layer.

7. The method for preparing a phase-stable radio frequency cable according to claim 1, characterized in that, The foamed polytetrafluoroethylene insulation layer has an inner dense layer 3a, a transition layer, a high-foaming layer, and an outer dense layer with different porosities arranged sequentially from the inside to the outside. The thickness of the inner dense layer 3a accounts for 8% to 15% of the total wall thickness of the foamed polytetrafluoroethylene insulation layer, the thickness of the transition layer accounts for 12% to 20% of the total wall thickness of the foamed polytetrafluoroethylene insulation layer, the thickness of the high-foaming layer accounts for 50% to 65% of the total wall thickness of the foamed polytetrafluoroethylene insulation layer, and the thickness of the outer dense layer accounts for 10% to 18% of the total wall thickness of the foamed polytetrafluoroethylene insulation layer.

8. The method for preparing a phase-stable radio frequency cable according to claim 1, characterized in that, The process of adjusting the annealing temperature and production line conveyor speed of the foamed polytetrafluoroethylene insulation layer includes: Compare the measured crystallinity with the target crystallinity; If the measured crystallinity is less than the target crystallinity, then increase the annealing temperature or decrease the production line transfer speed; If the measured crystallinity is greater than the target crystallinity, then reduce the annealing temperature or increase the production line transfer speed.

9. The method for preparing a phase-stable radio frequency cable according to claim 1, characterized in that, The outer conductor is made of silver-plated copper flat strip wrapped around it, and the shielding layer is made of silver-plated copper wire braided together.

10. The method for preparing a phase-stable radio frequency cable according to claim 1, characterized in that, The outer sheath is a polytetrafluoroethylene propylene (PTFE) outer sheath, wherein the PTFE outer sheath has a tensile strength of not less than 20 MPa, an elongation at break of not less than 250%, a dielectric strength of not less than 20 kV / mm, and a volume resistivity of not less than 1 × 10⁻⁶. 16 Ω·m.

Citation Information

Patent Citations

  • Anti-interference phase-stable radio frequency cable and preparation method thereof

    CN110380175A