Electromagnetic shield film and circuit board

By setting insulating and shielding layers with different gloss levels in the electromagnetic shielding film, and utilizing the high-gloss surface to reflect laser energy, the problem of insulation layer breakdown caused by laser drilling is solved, and the reliability of the insulation layer and grounding conductivity are synergistically optimized.

CN123164645APending Publication Date: 2026-11-24GUANGZHOU FANGBANG ELECTRONICS +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611246103.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-17
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing electromagnetic shielding films are prone to insulation layer breakdown during laser drilling, resulting in poor insulation performance and affecting the reliability of the electromagnetic shielding film.

Method used

By setting an insulating layer with different gloss levels on the shielding layer, the high-gloss insulating layer surface reflects laser energy, reducing the laser energy absorption rate of the insulating layer and avoiding breakdown. At the same time, a suitable microstructure is formed on the insulating layer to ensure subsequent grounding conduction.

Benefits of technology

This improved the insulation reliability and grounding performance of the electromagnetic shielding film, reduced the risk of insulation breakdown during laser drilling, and improved the manufacturing yield and electromagnetic shielding effect of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123164645A_ABST
    Figure CN123164645A_ABST
Patent Text Reader

Abstract

This application relates to an electromagnetic shielding film and a circuit board. The electromagnetic shielding film includes a shielding layer and an insulating layer stacked together; the shielding layer has a plurality of through holes extending through it in the thickness direction; the shielding layer has a first surface facing away from the insulating layer, and the insulating layer has a second surface facing the shielding layer; the gloss level A of the first surface at a test angle of 60 degrees is less than the gloss level B of the second surface at a test angle of 60 degrees. This application can reduce the risk of the insulating layer being broken down and improve the insulation reliability of the electromagnetic shielding film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of electronic technology, and in particular to electromagnetic shielding films and circuit boards. Background Technology

[0002] With the rapid development of 5G communication and millimeter-wave radar technology, electromagnetic shielding films are widely used to cover electronic components and circuit boards to reduce electromagnetic interference. Electromagnetic shielding films consist of an insulating layer, a shielding layer, and an adhesive film layer. The surface of the shielding layer is roughened to create raised bumps, which are used to pierce the adhesive film layer during hot pressing, thereby making contact with the grounding pads of the circuit board to form a conductive path. During the hot pressing process, air can easily be trapped between the film layers, and thermal expansion often leads to defects such as board bursting or delamination. Related technologies typically use lasers to process a perforated array of micropores through the shielding layer, allowing volatiles and residual gases to escape, thus mitigating the risk of board bursting.

[0003] However, during laser drilling, due to the thinness of the shielding layer, excess energy can easily be generated during drilling, leading to the breakdown of the insulation layer. This results in a significant reduction in the surface insulation resistance of the electromagnetic shielding film and poor insulation performance. Summary of the Invention

[0004] Based on this, this application provides an electromagnetic shielding film and a circuit board, which can reduce the risk of insulation layer breakdown and improve the insulation reliability of the electromagnetic shielding film.

[0005] In a first aspect, this application provides an electromagnetic shielding film, comprising a shielding layer and an insulating layer stacked together; the shielding layer has a plurality of through holes disposed in the thickness direction; the shielding layer has a first surface facing away from the insulating layer, and the insulating layer has a second surface facing the shielding layer; the gloss A of the first surface at a test angle of 60 degrees is less than the gloss B of the second surface at a test angle of 60 degrees.

[0006] In one embodiment, the difference between glossiness A and glossiness B satisfies: 5GU≤BA≤15GU.

[0007] In one embodiment, the gloss level A is not less than 5 GU and not more than 8 GU, and the gloss level B is not less than 13 GU and not more than 20 GU.

[0008] In one embodiment, the kurtosis Sku of the second surface satisfies: 2≤Sku≤3.

[0009] In one embodiment, in a sliced ​​state along the thickness direction, the height difference H between the highest point of the protrusion and the lowest point of the depression on the second surface is: 2μm≤H≤5μm.

[0010] In one embodiment, the diameter of the through hole is not less than 10 μm and not more than 30 μm.

[0011] In one embodiment, the spacing between two adjacent through holes is not less than 30 μm and not more than 100 μm.

[0012] In one embodiment, the adhesive film layer is further stacked on the first surface, and the first surface is provided with a plurality of protrusion structures.

[0013] In one embodiment, in the thickness direction of the electromagnetic shielding film, the height of the protrusion structure is not less than 2 μm and not more than 20 μm, and the thickness of the adhesive film layer is not less than 2 μm and not more than 20 μm.

[0014] Secondly, this application also provides a circuit board, including a circuit board body and an electromagnetic shielding film as described above; the electromagnetic shielding film is pressed onto the circuit board body, and the shielding layer is electrically connected to the grounding layer of the circuit board body.

[0015] Based on the electromagnetic shielding film of this application, since the gloss A of the first surface is less than the gloss B of the second surface, meaning the second surface is smoother and has higher reflectivity than the first surface, when laser drilling is performed from one side of the shielding layer, the higher surface gloss B means that the reflectivity of the second surface to the laser is significantly improved, thereby greatly reducing the absorption rate of laser energy by the insulating layer. This ensures that after the laser energy penetrates the shielding layer, the remaining energy is insufficient to damage the molecular structure of the insulating layer, avoiding the risk of the insulating layer being broken down, and thus improving the insulation reliability of the electromagnetic shielding film. Attached Figure Description

[0016] Figure 1 This is a schematic diagram of the structure of the electromagnetic shielding film in some embodiments of this application.

[0017] Figure 2 This is an exploded view of the electromagnetic shielding film in some embodiments of this application.

[0018] Figure 3 This is a schematic diagram of the structure of the electromagnetic shielding film in some embodiments of this application.

[0019] Explanation of reference numerals in the attached figures:

[0020] 1. Electromagnetic shielding film; 10. Insulating layer; 11. Second surface; 20. Shielding layer; 21. Through hole; 22. First surface; 23. Raised structure; 30. Adhesive film layer; 40. Protective layer; 50. Carrier layer. Detailed Implementation

[0021] To make the above-mentioned objectives, features, and advantages of this application more apparent and understandable, the specific embodiments of this application are described in detail below with reference to the accompanying drawings. Many specific details are set forth in the following description to provide a thorough understanding of this application. However, this application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar modifications without departing from the spirit of this application. Therefore, this application is not limited to the specific embodiments disclosed below.

[0022] In the description of this application, it should be understood that if terms such as "center", "longitudinal", "lateral", "length", "width", "thickness", "upper", "lower", "front", "rear", "left", "right", "vertical", "horizontal", "top", "bottom", "inner", "outer", "clockwise", "counterclockwise", "axial", "radial", "circumferential" appear, these terms indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, and are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this application.

[0023] Furthermore, where the terms "first" and "second" appear, these terms are for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined with "first" or "second" may explicitly or implicitly include at least one of that feature. In the description of this application, where the term "multiple" appears, "multiple" means at least two, such as two, three, etc., unless otherwise explicitly specified.

[0024] In this application, unless otherwise expressly specified and limited, the terms "installation," "connection," "joining," and "fixing," etc., should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral part; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; they can refer to the internal communication of two components or the interaction between two components, unless otherwise expressly limited. Those skilled in the art can understand the specific meaning of the above terms in this application based on the specific circumstances.

[0025] In this application, unless otherwise expressly specified and limited, the use of descriptions such as "above" or "below" the second feature indicates that the first and second features are in direct contact or indirect contact via an intermediate medium. Furthermore, "above," "on top of," and "over" the second feature can mean that the first feature is directly above or diagonally above the second feature, or simply that the first feature is at a higher horizontal level than the second feature. Similarly, "below," "below," and "under" the second feature can mean that the first feature is directly below or diagonally below the second feature, or simply that the first feature is at a lower horizontal level than the second feature.

[0026] It should be noted that if an element is referred to as being "fixed to" or "set on" another element, it can be directly on the other element or there may be an intervening element. If an element is considered to be "connected to" another element, it can be directly connected to the other element or there may be an intervening element. If so, the terms "vertical," "horizontal," "upper," "lower," "left," "right," and similar expressions used in this application are for illustrative purposes only and do not represent the only possible implementation.

[0027] With the rapid development of 5G communication and millimeter-wave radar technology, electromagnetic shielding films are widely used to cover electronic components and circuit boards to reduce electromagnetic interference. These electromagnetic shielding films typically include a laminated insulating layer, a shielding layer, and an adhesive film layer. The surface of the shielding layer is roughened to create raised protrusions, designed to pierce the adhesive film layer during the hot-pressing process, thereby making contact with the grounding pads of the circuit board and achieving reliable grounding.

[0028] However, in actual hot-press bonding processes, air is easily trapped between film layers, and volatiles in the adhesive film layer will escape after heating. If these gases cannot be discharged in time, they will cause serious defects such as board bursting or interlayer delamination due to thermal expansion. To address this, related technologies typically use lasers to process a perforated array of micropores through the shielding layer, aiming to use this micropore array as an exhaust channel to mitigate the risk of board bursting.

[0029] However, the aforementioned laser drilling solution has significant limitations in practical applications: the shielding layer is extremely thin (typically on the micrometer scale), and the energy window for laser processing is very narrow. Power control during the laser process is extremely difficult; when the laser energy is too high, the beam carries residual energy after penetrating the shielding layer, easily continuing to penetrate the insulating layer. Once the insulating layer is breached, the surface insulation resistance of the finished electromagnetic shielding film will decrease significantly, leading to insulation failure and a substantial reduction in product quality. In practice, even with repeated adjustments to various power parameters, it is still difficult to completely avoid this breakdown phenomenon, resulting in poor process stability.

[0030] Based on this, see Figure 1This application provides an electromagnetic shielding film 1, including a shielding layer 20 and an insulating layer 10 stacked together; the shielding layer 20 has a plurality of through holes 21 extending through the thickness direction; please refer to the following reference. Figure 2 The shielding layer 20 has a first surface 22 facing away from the insulating layer 10, and the insulating layer 10 has a second surface 11 facing the shielding layer 20; the gloss A of the first surface 22 at a test angle of 60 degrees is less than the gloss B of the second surface 11 at a test angle of 60 degrees.

[0031] Specifically, gloss level reflects the reflectivity of a surface to incident light; higher gloss indicates higher reflectivity and lower absorption of laser energy. This application achieves this by making the gloss level B of the second surface 11 of the insulating layer 10 facing the shielding layer 20 higher than the gloss level A of the first surface 22 on the perforated side of the shielding layer 20. This improves the absorption rate of the first surface 22 to the incident laser, allowing reliable melting penetration of the shielding layer 20 and formation of the through-hole 21 at lower laser energy. Furthermore, because the second surface 11 of the insulating layer 10 has higher gloss, even if some laser energy remains after penetrating the shielding layer 20, it will be largely reflected upon reaching the surface of the insulating layer 10 due to its high reflectivity, effectively reducing the actual absorption of residual laser energy by the insulating layer 10 and preventing a sudden temperature rise and burn-through.

[0032] Based on the electromagnetic shielding film 1 of this application embodiment, the gloss level A of the first surface 22 is lower than the gloss level B of the second surface 11. When laser drilling is performed on the shielding layer 20 side, the shielding layer 20 has a higher absorption rate for the laser due to its lower gloss level A, which is beneficial for achieving melt penetration and forming a through hole 21. At the same time, the second surface 11 on the insulating layer 10 side has a higher reflectivity for the residual laser after penetrating the shielding layer 20 due to its higher gloss level B, which can reduce the actual absorption of this part of the energy by the insulating layer 10, thereby reducing the risk of it being broken down. Therefore, the electromagnetic shielding film 1 of this application can effectively improve insulation reliability by differentiating the gloss levels of the first surface 22 and the second surface 11, while retaining the laser-perforated ventilation structure and solving the problem of pressure-bonded plate bursting.

[0033] In some embodiments, the difference between glossiness A and glossiness B further satisfies: 5 GU ≤ B − A ≤ 15 GU. It is understood that the magnitude of the glossiness difference not only affects the absorption distribution of laser energy but also has a related impact on the surface morphology of the shielding layer 20. By limiting the difference between glossiness A and glossiness B to the above range, this application achieves the following beneficial effects:

[0034] When the gloss difference is not less than 5 GU, the gloss B of the second surface 11 has a sufficient margin of difference compared to the gloss A of the first surface 22. Under this condition, the second surface 11 has a sufficiently high reflectivity, which can effectively reflect the remaining laser energy after penetrating the shielding layer 20, reduce the absorption rate of this part of the energy by the insulating layer 10, and thus effectively reduce the probability of the insulating layer 10 being accidentally broken through during laser drilling.

[0035] A gloss difference of no more than 15 GU can prevent the gloss level B of the second surface 11 from being too high. Since the shielding layer 20 is formed on the second surface 11 of the insulating layer 10 by electroplating or chemical deposition, the higher the gloss level of the second surface 11, the smoother the surface of the shielding layer 20 will be, and the lower the roughness will be. If the surface roughness of the shielding layer 20 is too low, it will be difficult to form a large-roughness protrusion structure 23 in the subsequent roughening process. This protrusion structure 23 is used to pierce the adhesive film layer 30 and connect with the ground layer of the circuit board during the pressing process to establish a conductive path and reduce contact resistance. Therefore, controlling the gloss difference within the above range is beneficial for the laser to effectively penetrate the shielding layer 20 for drilling, and also allows the second surface 11 to have a suitable roughness after restoration, which is conducive to the formation of an effective protrusion structure 23 in the subsequent roughening process, thereby improving the grounding conductivity of the electromagnetic shielding film 1.

[0036] In some embodiments, the gloss level A is not less than 5 GU and not greater than 8 GU, and the gloss level B is not less than 13 GU and not greater than 20 GU. Specifically, the gloss level A of the first surface 22 is controlled within the range of 5 GU to 8 GU. On the one hand, this allows the first surface 22 to have a good absorption rate for the incident laser, which is beneficial for forming the through hole 21. On the other hand, the surface roughness corresponding to this gloss level A range is moderate, which is beneficial for subsequent roughening processes to form a raised structure 23 with a larger roughness. This is beneficial for the electromagnetic shielding film 1 to reliably pierce the adhesive film layer 30 and achieve good conductivity with the ground layer of the circuit board during the hot pressing process.

[0037] For the second surface 11 of the insulating layer 10, the gloss of a conventional insulating layer 10 at a 60° gloss test angle is typically only 6 GU to 9 GU, and its absorption rate of 355nm ultraviolet laser is as high as 50% to 70%. Therefore, the insulating layer 10 in related technologies is easily broken down by the remaining laser energy. However, this application sets the gloss B of the second surface 11 to 13 GU to 20 GU. Within this gloss range, the reflectivity of the second surface 11 to ultraviolet laser can be improved, and the actual absorption rate can be reduced to below 20%. This effectively reflects the remaining laser energy after penetrating the shielding layer 20, ensuring that the energy absorbed by the insulating layer 10 is insufficient to cause its temperature to rise sharply to the damage threshold, thus helping to avoid the risk of the insulating layer 10 being broken down.

[0038] In summary, this application achieves synergistic optimization between drilling efficiency, insulation performance of insulating layer 10, and grounding reliability of shielding layer 20 by controlling gloss A to 5 GU to 8 GU and gloss B to 13 GU to 20 GU, and ensuring that both satisfy 5 GU≤BA≤15 GU. This ensures that the venting holes 21 of electromagnetic shielding film 1 are formed smoothly and that grounding performance is reliable, while improving the insulation performance and manufacturing yield of electromagnetic shielding film 1.

[0039] In some embodiments, the kurtosis Sku of the second surface 11 of the insulating layer 10 facing the shielding layer 20 satisfies: 2 ≤ Sku ≤ 3. It should be noted that kurtosis (Sku) is a dimensionless parameter used to characterize the microscopic profile distribution of a surface, reflecting the steepness of the surface height distribution. In surface morphology, kurtosis values ​​can quantitatively describe the sharpness or flatness of surface peaks and valleys: when Sku = 3, the surface height distribution follows a normal distribution; when Sku > 3, it indicates a relatively steep surface distribution with many sharp peaks or deep valleys; when Sku < 3, it indicates a relatively flat surface distribution with relatively rounded peaks and valleys.

[0040] Based on the above definition, this application limits the kurtosis Sku of the second surface 11 of the insulating layer 10 to between 2 and 3, meaning that the roughness height of the second surface 11 has a moderate dispersion, and there are no extreme peaks or valleys on the surface. Under this microscopic profile, the incident light is mainly reflected once, the scattering path of the light is relatively regular, and the diffuse reflection component is low, thereby keeping the total hemispherical reflectivity at a high level, effectively reducing the surface absorption rate of laser energy, and further suppressing the risk of laser penetration of the insulating layer 10.

[0041] In some embodiments, in a sliced ​​state along the thickness direction, the height difference H between the highest point of the protrusion and the lowest point of the depression on the second surface 11 is: 2μm≤H≤5μm.

[0042] It should be noted that the height difference H is the maximum peak-valley height of the microscopic profile of the second surface 11 of the insulating layer 10, which characterizes the degree of undulation of the surface in the vertical direction.

[0043] Specifically, since the shielding layer 20 is typically formed on the second surface 11 of the insulating layer 10 through electroplating or chemical deposition, the microscopic profile of the second surface 11 is transferred to the first surface 22 of the shielding layer 20. If the height difference H of the second surface 11 is less than 2 μm, the surface of the insulating layer 10 is too flat, and the first surface 22 formed by subsequent electroplating lacks sufficient microscopic undulations. This makes it difficult to form a sufficiently high and sharp protrusion structure 23 during subsequent roughening, which can easily affect the reliability of the protrusion structure 23 piercing the adhesive film layer 30 and contacting the ground plane of the circuit board. Setting the height difference H of the second surface 11 to be no less than 2 μm ensures that the first surface 22 of the shielding layer 20 after reshaping has a suitable initial roughness, providing a structural basis for subsequent roughening, thereby forming a protrusion structure 23 with sufficient piercing capability.

[0044] During laser drilling, if the height difference H is greater than 5 μm, the second surface 11 will have drastically undulating protrusions and depressions. In this case, the incident residual laser will undergo multiple diffuse reflections at these steep microstructures, making the light scattering path more complex. This leads to a decrease in the total hemispherical reflectivity and an increase in the actual laser energy absorbed by the surface, thereby weakening the expected effect of reducing laser absorption by improving gloss. At the same time, excessive peaks and valleys can also easily cause uneven thickness distribution of the shielding layer 20 during electroplating, affecting the structural uniformity and conductivity reliability of the shielding layer 20.

[0045] Based on the above embodiments, this application controls the height difference H between the highest point of the protrusion and the lowest point of the depression on the second surface 11 within the range of 2μm to 5μm. This ensures that the second surface 11 has sufficient microscopic undulations to facilitate the roughening of the first surface 22 after its reconstruction to form an effective protrusion structure 23. At the same time, within this range, the second surface 11 does not have extreme peaks or valleys. When the laser irradiates the second surface 11, it is mainly reflected by a single reflection, and the total hemispherical reflectivity remains at a high level, thereby effectively reducing the absorption rate of laser energy by the surface of the insulating layer 10.

[0046] It is worth noting that, in order to avoid the insulation layer 10 being punctured, in addition to the aforementioned gloss and surface morphology factors, the laser processing energy itself is also one of the key influencing parameters. When the laser drills holes in the shielding layer 20, the total volume of the via 21 also affects the required total laser energy input. Specifically, the larger the total volume of the via 21, the more material needs to be removed, the higher the corresponding laser energy requirement, and the higher the risk of the insulation layer 10 being damaged due to the absorption of residual energy. Based on this, the geometric parameters of the via 21 have been further optimized in this embodiment.

[0047] In some embodiments, the aperture D of the through-hole 21 is not less than 10 μm and not more than 30 μm. Specifically, the aperture of the through-hole 21 can be 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, etc. It is understood that if the aperture of the through-hole 21 is less than 10 μm, the exhaust cross-section of a single through-hole 21 is insufficient, and gas cannot pass smoothly during the hot pressing process. This can easily lead to micropore blockage or exhaust delay due to poor exhaust, weakening its actual effect in mitigating the risk of board explosion. If the aperture of the through-hole 21 is greater than 30 μm, the amount of material removed from a single through-hole 21 increases significantly, which means that the laser energy required for single-hole forming increases, and the heat conducted from the shielding layer 20 to the insulating layer 10 increases accordingly, thus increasing the risk of breakdown.

[0048] In some embodiments, the spacing between two adjacent through holes 21 is not less than 30 μm and not more than 100 μm. It should be noted that the spacing between two adjacent through holes 21 refers to the shortest distance between the edges of the two through holes 21. Specifically, this spacing can be 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, or 100 μm. Specifically, if the spacing between two adjacent through holes 21 is less than 30 μm, the bridging area of ​​the shielding material between adjacent through holes 21 is too narrow, resulting in too many through holes 21 per unit area. During the drilling process, the laser heat-affected zones are prone to overlap, generating a heat accumulation effect, leading to a significant increase in local temperature and increasing the risk of the insulation layer 10 being burned through. Simultaneously, the excessively narrow material bridging area weakens the local mechanical strength of the shielding layer 20, making it prone to cracks or even breakage during subsequent bending or hot pressing, affecting the structural reliability of the product. If the spacing between two adjacent through holes 21 is greater than 100 μm, the through holes 21 are sparsely distributed, reducing exhaust efficiency.

[0049] Based on the above embodiments, by limiting the aperture D of the through hole 21 to 10μm to 30μm and the edge spacing of adjacent through holes 21 to 30μm to 100μm, it is possible to reduce the total laser energy input required for drilling while ensuring the exhaust effect and meeting the requirements of the explosion-proof plate, thereby mitigating the thermal impact of the drilling process on the insulating layer 10 from the source.

[0050] In some embodiments, the electromagnetic shielding film 1 further includes an adhesive film layer 30 stacked on the first surface 22 of the shielding layer 20. The material used for the adhesive film layer 30 is selected from at least one of the following groups: modified epoxy resin, acrylic resin, modified rubber, and modified thermoplastic polyimide. The above material system has slight tackiness at room temperature, facilitating the bonding between the electromagnetic shielding film 1 and the circuit board. Simultaneously, this type of material can soften under hot pressing conditions and exhibit viscous flow, fully wetting the microstructure of the circuit board surface, and forming a strong adhesive interface after curing, ensuring the long-term reliability of the bond between the shielding film and the circuit board.

[0051] In some embodiments, the height of the raised structure 23 is not less than 2 μm and not more than 20 μm in the thickness direction of the electromagnetic shielding film 1, and the thickness of the adhesive film layer 30 is not less than 2 μm and not more than 20 μm. Specifically, if the thickness of the adhesive film layer 30 is less than 2 μm, it is easy to lead to insufficient bonding strength and difficulty in providing reliable interfacial bonding force; if the thickness of the adhesive film layer 30 is greater than 20 μm, it increases the thickness of the adhesive film layer 30 that the raised structure 23 needs to penetrate, and may not be able to effectively contact the grounding pad due to insufficient piercing stroke. At the same time, the height of the raised structure 23 needs to be adapted to the thickness of the adhesive film layer 30 to ensure that the raised structure 23 can completely penetrate the adhesive film layer 30 and form reliable contact with the grounding pad of the circuit board during the hot pressing process.

[0052] Please see Figure 3 Furthermore, in some embodiments, the electromagnetic shielding film 1 further includes a protective layer 40, which is disposed on the surface of the adhesive film layer 30 away from the shielding layer 20. The protective layer 40 is used to protect the adhesive film layer 30 during the winding and transportation of the electromagnetic shielding film 1, preventing the adhesive film layer 30 from being contaminated or damaged. In use, after peeling off the protective layer 40, the electromagnetic shielding film 1 is pressed onto the surface of the circuit board.

[0053] As an example, this application provides a method for preparing the electromagnetic shielding film 1 described above, which specifically includes the following steps:

[0054] S1: Provides a carrier layer of 50;

[0055] The carrier layer 50 can be a release film. Specifically, the release film is a polyester film (PET) or polypropylene film (PP) treated with silicone oil or fluorine, used to carry the functional layers in subsequent processes and to be easily peeled off when the finished product is used.

[0056] S2: Prepare insulating layer 10;

[0057] An insulating layer 10 is formed on a release film through a coating process. An insulating adhesive is prepared by blending insulating substrates such as polyethylene terephthalate (PET) and polyimide (PI) with black ink, and then uniformly coated onto the surface of the carrier layer 50. After drying and curing, the insulating layer 10 is formed. The thickness of the insulating layer 10 is controlled between 3 μm and 10 μm, and the gloss B of the second surface 11 of the insulating layer 10 is controlled between 13 GU and 20 GU.

[0058] S3: Prepare shielding layer 20;

[0059] A shielding layer 20 is prepared on the surface of the insulating layer 10 away from the carrier layer 50. Specifically, a conductive seed layer is deposited on the surface of the insulating layer 10 by physical vapor deposition (PVD) sputtering. The seed layer is made of copper or a copper-nickel alloy and serves to provide a conductive substrate for subsequent electroplating. Then, a deposited metal layer is thickened on the seed layer by electroplating. The electroplating material is copper or a copper alloy containing one or more alloying elements selected from nickel, tin, and chromium. After electroplating, the thickness of the shielding layer 20 is controlled between 1 μm and 6 μm. In other embodiments, rolled copper foil or electrolytic copper foil can also be directly adhered to the surface of the insulating layer 10 by hot pressing or bonding to form the shielding layer 20.

[0060] Subsequently, the exposed surface of the shielding layer 20 is subjected to a micro-roughening treatment to form a grounding protrusion structure 23. Specifically, the protrusion structure 23 is formed on the first surface 22 by chemical etching, mechanical polishing, electroplating nodules or laser etching. The protrusion structure 23 can be a micro-protrusion, a ridge-like line or a pointed cone-shaped protrusion, and its height is between 2μm and 20μm.

[0061] S4: Machining through hole 21;

[0062] Multiple through holes 21 are fabricated on the shielding layer 20 using ultraviolet or infrared lasers. Specifically, a 355nm ultraviolet nanosecond laser can be used to drill holes in the shielding layer 20. The diameter D of the through holes 21 is controlled between 10μm and 30μm, and the spacing between the edges of two adjacent through holes 21 is controlled between 30μm and 100μm.

[0063] S5: Prepare adhesive film layer 30;

[0064] An adhesive is applied to the surface of the perforated shielding layer 20, and then pre-cured to form an adhesive film layer 30. The adhesive can be a modified epoxy resin, acrylic resin, modified rubber resin, or modified thermoplastic polyimide resin.

[0065] S6: Post-baking curing and slitting;

[0066] The finished product is then baked and cured to achieve the required degree of cross-linking of the adhesive film layer (30%). Finally, it is cut into specified widths to obtain the finished electromagnetic shielding film 1.

[0067] To verify the grounding reliability of the electromagnetic shielding film 1 provided in the above embodiments of this application, the following experimental data are also provided. It should be noted that the following experimental data are merely exemplary verification results of various embodiments of this application and are not intended to limit the scope of protection of this application in any way.

[0068] Multiple samples of the same batch of coated wafers were drilled under uniform laser energy parameters. After drilling, the samples were sliced, and the cross-sectional morphology of the slices was observed using a scanning electron microscope.

[0069] Evaluation criteria: Observe and record whether there are signs of damage such as breakdown, carbonization or cracking at the corresponding holes on the 10 sides of the insulation layer.

[0070] The laser-drilled sheet is further coated with an adhesive film layer 30 to form the finished electromagnetic shielding film 1; then the finished film is pressed onto the FPC grounding pad with the following pressing parameters: temperature 180℃, pressure 3MPa, and time 60s.

[0071] The samples after lamination were subjected to thermal shock testing. The test conditions were as follows: the samples were placed in a tin bath at 260℃ for tin immersion test, each immersion lasted 10 seconds, and the immersion was repeated 3 times.

[0072] Evaluation index: Measure the grounding resistance of the samples before and after thermal shock, and calculate the rate of change of grounding resistance using the following formula:

[0073] Grounding resistance change rate = (resistance after test - initial resistance) / initial resistance × 100%.

[0074]

[0075] In Comparative Example 1, the gloss level B of the second surface 11 is 8, and the difference between the gloss level B of the second surface 11 and the gloss level A of the first surface 22 is 2; in Comparative Example 2, the gloss level B of the second surface 11 is 25, and the difference between the gloss level B of the second surface 11 and the gloss level A of the first surface 22 is 18; in Examples 1 to 3, the difference between the gloss level B of the second surface 11 and the gloss level A of the first surface 22 all satisfy 5 GU≤B−A≤15 GU, and the gloss level B all satisfy 13 GU≤B≤20 GU.

[0076] The data in the table above shows that:

[0077] In Comparative Example 1, the gloss level B of the second surface 11 of the insulating layer 10 is less than 13 GU, and the difference in gloss level between it and the first surface 22 of the shielding layer 20 is less than 5 GU. After laser drilling, the cross-section was observed by electron microscopy and the hole breakdown was statistically analyzed. Under these conditions, the breakdown rate of the insulating layer 10 was relatively high, reaching over 86%. However, due to its low gloss level B, the surface roughness of the shielding layer 20 formed by subsequent electroplating was relatively large. The raised structure 23 formed after roughening treatment had a better grounding effect. After the finished product underwent tin-bleaching test, the grounding resistance change rate was 13%, indicating good grounding performance.

[0078] In Comparative Example 2, the gloss level B of the second surface 11 of the insulating layer 10 is higher than 20 GU, and the difference in gloss level between it and the first surface 22 of the shielding layer 20 is greater than 15 GU. After laser drilling, the breakdown rate of the insulating layer 10 is low, less than 15%. However, due to its excessively high gloss level B, the surface roughness of the shielding layer 20 formed by subsequent electroplating is small. The grounding effect of the raised structure 23 formed after roughening treatment is poor. After the finished product is tested for tinning, the grounding resistance change rate is as high as 116%, indicating poor grounding performance.

[0079] In Examples 1-3, the gloss level B of the second surface 11 of the insulating layer 10 is in the range of 13 GU to 20 GU, and the difference in gloss level between the second surface 11 and the first surface 22 of the shielding layer 20 is in the range of 5 GU to 15 GU. After laser drilling, the breakdown rate of the insulating layer 10 in each example is low, not exceeding 20%. At the same time, because its gloss level B is moderate, the surface of the shielding layer 20 formed by subsequent electroplating has a suitable roughness. The raised structure 23 formed after roughening treatment can effectively pierce the adhesive film layer 30 to achieve grounding conductivity. After the finished product is tested by tinning, the grounding resistance change rate is less than 30%, and the grounding performance is good.

[0080] In summary, this application controls the gloss level B of the second surface 11 of the insulating layer 10 within the range of 13 GU to 20 GU, and controls the difference between it and the gloss level A of the first surface 22 of the shielding layer 20 within the range of 5 GU to 15 GU. This effectively reduces the absorption of residual laser energy by the insulating layer 10 after penetrating the shielding layer 20 during laser drilling, preventing the insulating layer 10 from being broken down and ensuring the insulation performance of the shielding film. At the same time, this gloss level range is conducive to the subsequent electroplating to form a shielding layer 20 surface with suitable roughness. The protruding structure 23 formed after roughening treatment can effectively pierce the adhesive film layer 30 to achieve grounding conduction, ensuring that the grounding resistance change rate is at a low level after thermal shock, thereby achieving a good balance between laser drilling safety and grounding reliability.

[0081] Secondly, this application also provides a circuit board, including a circuit board body and an electromagnetic shielding film 1 as described in any of the above embodiments. The circuit board body includes a substrate layer, a ground layer, and a cover layer. The substrate layer includes a carrier layer and a circuit structure disposed on the surface of the carrier layer. The carrier layer provides mechanical support, and the circuit structure enables the transmission and connection of electrical signals. The ground layer is disposed on one side surface of the substrate layer and electrically connected to the grounding line in the circuit structure, providing a grounding potential. The cover layer covers the ground layer and the surface of the substrate layer, and the cover layer has a window to at least partially expose the ground layer, allowing the protrusion structure 23 of the shielding layer 20 to penetrate and form an electrical connection with the ground layer. Because the circuit board is provided with the electromagnetic shielding film 1 described above, it has at least the aforementioned beneficial effects, which will not be elaborated further here.

[0082] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0083] The embodiments described above are merely illustrative of several implementation methods of this application, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the patent application. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the protection scope of this application. Therefore, the protection scope of this patent application should be determined by the appended claims.

Claims

1. An electromagnetic shielding film, characterized in that, This includes a layered shielding layer and an insulating layer; The shielding layer has multiple through holes that extend through the thickness direction; The shielding layer has a first surface facing away from the insulating layer, and the insulating layer has a second surface facing the shielding layer; The gloss A of the first surface at a test angle of 60 degrees is less than the gloss B of the second surface at a test angle of 60 degrees.

2. The electromagnetic shielding film according to claim 1, characterized in that, The difference between glossiness A and glossiness B satisfies: 5GU≤BA≤15GU.

3. The electromagnetic shielding film according to claim 1, characterized in that, The gloss level A is not less than 5 GU and not more than 8 GU, and the gloss level B is not less than 13 GU and not more than 20 GU.

4. The electromagnetic shielding film according to claim 1, characterized in that, The kurtosis Sku of the second surface satisfies: 2≤Sku≤3.

5. The electromagnetic shielding film according to claim 1, characterized in that, In the sliced ​​state along the thickness direction, the height difference H between the highest point of the protrusion and the lowest point of the depression on the second surface is: 2μm≤H≤5μm.

6. The electromagnetic shielding film according to claim 1, characterized in that, The diameter of the through hole is not less than 10 μm and not more than 30 μm.

7. The electromagnetic shielding film according to claim 1, characterized in that, The distance between two adjacent through holes shall be no less than 30 μm and no more than 100 μm.

8. The electromagnetic shielding film according to claim 1, characterized in that, It also includes a film layer stacked on the first surface, and the first surface is provided with a plurality of protrusion structures.

9. The electromagnetic shielding film according to claim 8, characterized in that, In the thickness direction of the electromagnetic shielding film, the height of the raised structure is not less than 2μm and not more than 20μm, and the thickness of the adhesive film layer is not less than 2μm and not more than 20μm.

10. A circuit board, characterized in that, include: Circuit board body; as well as The electromagnetic shielding film as described in any one of claims 1 to 9; The electromagnetic shielding film is pressed onto the circuit board body, and the shielding layer is electrically connected to the grounding layer of the circuit board body.