Composite shielding film, method for manufacturing the same, and display device

By introducing a composite shielding film consisting of an organic reinforcing layer and a self-adhesive buffer layer into the electromagnetic shielding structure, the problems of film marks and indentations caused by the easy deformation of metal foil were solved, improving the appearance and performance of electronic devices and increasing the yield rate.

CN123164731APending Publication Date: 2026-11-24HEFEI VISIONOX TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510661846.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-21
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

In existing electromagnetic shielding structures, the metal foil is prone to deformation, which leads to film marks and indentations on the screen, affecting the appearance quality and performance of electronic devices and reducing the product yield.

Method used

The composite shielding membrane structure includes a metal shielding layer and a deformation-resistant layer. The deformation-resistant layer consists of an organic reinforcement layer and a self-adhesive buffer layer. The tensile strength of the organic reinforcement layer is greater than that of the metal shielding layer, and the self-adhesive buffer layer provides adhesion and buffering, which together enhance the deformation resistance.

Benefits of technology

This effectively prevents deformation of the metal shielding layer from being transmitted to electronic devices, improves the appearance quality and performance of the display device, reduces the risk of defects, and increases the product yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123164731A_ABST
    Figure CN123164731A_ABST
Patent Text Reader

Abstract

This application provides a composite shielding film, its preparation method, and a display device. The composite shielding film includes a metal shielding layer stacked along a first direction and at least one deformation-resistant layer. The deformation-resistant layer includes an organic reinforcing layer and a self-adhesive buffer layer. The organic reinforcing layer is disposed between the metal shielding layer and the self-adhesive buffer layer, and the tensile strength of the organic reinforcing layer is greater than that of the metal shielding layer. The composite shielding film is bonded to the electronic device through the self-adhesive buffer layer. By providing an organic reinforcing layer and a self-adhesive buffer layer on one side of the metal shielding layer, the composite shielding film significantly improves its resistance to permanent deformation while providing shielding and grounding effects. This effectively avoids the problem of film marks and indentations caused by deformation of the metal shielding layer conducting to the electronic device, thus improving the appearance quality and performance of the display device, reducing the risk of defects caused by film marks and indentations in the subsequent manufacturing processes of the display device, and increasing the product yield.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of electromagnetic shielding technology, specifically relating to a composite shielding film and its preparation method, and a display device. Background Technology

[0002] In the manufacturing process of electronic devices, electromagnetic shielding materials are typically used to protect electronic components from electromagnetic interference. Currently, commonly used electromagnetic shielding structures employ metal foil, such as copper foil, as the shielding layer. However, these metal foils are relatively soft. During the application process, when rollers press over the protective film's edge, or when components on the back are pressed during assembly, the metal foil is prone to deformation and has poor resilience, making it difficult to return to its initial state. More seriously, the deformation of the metal foil is transmitted layer by layer to the screen body, leading to problems such as film marks and indentations on the front of the screen, affecting the appearance quality and performance of the electronic device, reducing product yield, and increasing production costs. Therefore, there is an urgent need for a deformation-resistant composite shielding film. Summary of the Invention

[0003] This application provides a composite shielding film and its preparation method, as well as a display device, to solve the problem that the metal foil in the existing electromagnetic shielding structure is easily deformed, resulting in film marks and indentations on the screen, thereby improving the appearance quality and performance of electronic devices and increasing the product yield.

[0004] In a first aspect, embodiments of this application provide a composite shielding film, comprising a metal shielding layer and at least one deformation-resistant layer stacked along a first direction. The deformation-resistant layer includes an organic reinforcement layer and a self-adhesive buffer layer. The at least one deformation-resistant layer has an organic reinforcement layer and a self-adhesive buffer layer at its two ends along the first direction, respectively. The metal shielding layer is used for electromagnetic shielding, the organic reinforcement layer is used to support the metal shielding layer, and the self-adhesive buffer layer is used for bonding and buffering. The organic reinforcement layer is disposed between the metal shielding layer and the self-adhesive buffer layer. The surface of the organic reinforcement layer at both ends facing away from the self-adhesive buffer layer is bonded to the metal shielding layer, and the surface of the organic reinforcement layer at both ends facing away from the metal shielding layer is bonded to the self-adhesive buffer layer. The composite shielding film is bonded to electronic devices through the self-adhesive buffer layers at both ends. The tensile strength of the organic reinforcement layer is greater than the tensile strength of the metal shielding layer.

[0005] According to an embodiment of the first aspect of this application, the tensile strength of the organic reinforcement layer is ≥350 MPa.

[0006] According to an embodiment of the first aspect of this application, in a first direction, the thickness of the organic reinforcement layer is greater than the thickness of the metal shielding layer.

[0007] According to an embodiment of the first aspect of this application, the thickness of the organic reinforcement layer in the first direction is 30-50 μm.

[0008] According to an embodiment of the first aspect of this application, the thickness of the metal shielding layer in the first direction is 5 to 10 μm.

[0009] According to an embodiment of the first aspect of this application, the density of the organic reinforcement layer is less than the density of the metal shielding layer.

[0010] According to an embodiment of the first aspect of this application, in a first direction, the thickness of the self-adhesive buffer layer is greater than the thickness of the organic reinforcement layer.

[0011] According to an embodiment of the first aspect of this application, the thickness of the self-adhesive buffer layer in the first direction is 80 μm to 150 μm.

[0012] According to an embodiment of the first aspect of this application, the storage modulus of the self-adhesive buffer layer is >150 kPa and the loss factor is >1.0; or, the storage modulus of the self-adhesive buffer layer is 60 to 150 kPa and the loss factor is 0.5 to 1.0.

[0013] According to an embodiment of the first aspect of this application, the material of the metal shielding layer includes one or more of copper, aluminum, iron-nickel alloy and steel; optionally, the metal shielding layer includes an aluminum layer and a nickel plating layer attached to the aluminum layer.

[0014] According to an embodiment of the first aspect of this application, the material of the organic reinforcement layer includes one or more of carbon fiber, polyetheretherketone, polyethylene terephthalate, and polyethylene naphthalate; preferably, the material of the organic reinforcement layer is polyetheretherketone modified with carbon fiber.

[0015] According to an embodiment of the first aspect of this application, the material of the self-adhesive buffer layer includes one or more of acrylic pressure-sensitive adhesive, silicone pressure-sensitive adhesive, and rubber-based pressure-sensitive adhesive.

[0016] According to an embodiment of the first aspect of this application, the metal shielding layer is attached to the side of the organic reinforcement layer away from the self-adhesive buffer layer by means of adhesive bonding or electroplating.

[0017] According to an embodiment of the first aspect of this application, an adhesive layer is provided between the metal shielding layer and the organic reinforcement layer, and the metal shielding layer and the organic reinforcement layer are bonded together by the adhesive layer.

[0018] According to an embodiment of the first aspect of this application, the thickness of the adhesive layer in the first direction is 5 to 10 μm.

[0019] According to an embodiment of the first aspect of this application, a self-adhesive buffer layer is coated or attached to the side of the organic reinforcement layer facing away from the metal shielding layer.

[0020] Secondly, embodiments of this application provide a method for preparing the above-mentioned composite shielding film, comprising: preparing at least one anti-deformation layer, the anti-deformation layer including an organic reinforcement layer and a self-adhesive buffer layer, wherein the two ends of the at least one anti-deformation layer along a first direction are an organic reinforcement layer and a self-adhesive buffer layer respectively; and forming a metal shielding layer on the side of the organic reinforcement layer away from the self-adhesive buffer layer at both ends.

[0021] Thirdly, embodiments of this application provide a display device, including: an OLED module and the aforementioned composite shielding film, wherein the composite shielding film is attached to one side surface of the OLED module.

[0022] The composite shielding film in this embodiment significantly improves its resistance to permanent deformation while providing shielding and grounding effects by setting an organic reinforcing layer and a self-adhesive buffer layer on one side of the metal shielding layer. This effectively avoids the problem of film marks and indentations caused by deformation of the metal shielding layer conducting to electronic devices, improving the appearance quality and performance of the display device, reducing the risk of defects caused by film marks and indentations in subsequent manufacturing processes, and increasing the product yield. It has good application prospects and economic benefits. Attached Figure Description

[0023] Figure 1 This is a schematic diagram of the structure of the composite shielding film provided in an embodiment of this application;

[0024] Figure 2 Another structural schematic diagram of the composite shielding film provided in the embodiments of this application;

[0025] Figure 3 A schematic diagram of yet another structure of the composite shielding film provided in the embodiments of this application;

[0026] Figure 4 A flowchart illustrating the preparation method of the composite shielding film provided in the embodiments of this application;

[0027] Figure 5 A schematic diagram of the structure of a display device provided in an embodiment of this application;

[0028] Figure 6 This is another schematic diagram of the structure of the display device provided in the embodiments of this application.

[0029] Figure label:

[0030] 100. Composite shielding film;

[0031] 110. Metallic shielding layer; 120. Deformation-resistant layer; 121. Organic reinforcement layer; 122. Self-adhesive buffer layer; 130. Adhesive layer;

[0032] 200, OLED module; X, first direction. Detailed Implementation

[0033] To make the purpose, technical solution, and beneficial technical effects of this application clearer, the following detailed description is provided in conjunction with embodiments. It should be understood that the embodiments described in this specification are merely for explaining this application and are not intended to limit it.

[0034] For simplicity, this application only explicitly discloses some numerical ranges. However, any lower limit can be combined with any upper limit to form a range not explicitly stated; and any lower limit can be combined with other lower limits to form a range not explicitly stated, just as any upper limit can be combined with any other upper limit to form a range not explicitly stated. Furthermore, although not explicitly stated, every point or individual value between the endpoints of the range is included within that range. Therefore, each point or individual value can be used as its own lower or upper limit and combined with any other point or individual value or with other lower or upper limits to form a range not explicitly stated.

[0035] In the description of this application, it should be noted that, unless otherwise stated, "above" and "below" include the stated number, and "multiple" in "one or more" means two or more.

[0036] As mentioned in the background technology, because the metal foil is too soft, easily deformed and has poor resilience, during the application process, the roller presses over the protective film step difference, and the back components are pressed during assembly, which will cause the metal foil to deform. The deformation of the metal foil will be transmitted to the screen body layer by layer, thus resulting in visible film marks and indentations on the front of the screen body.

[0037] In view of the above problems, this application provides a composite shielding film and its preparation method, as well as a display device, to solve the problem that the metal foil in the existing electromagnetic shielding structure is easily deformed, resulting in film marks and indentations on the screen, thereby improving the appearance quality and performance of electronic devices and increasing the product yield.

[0038] Please see Figure 1 and Figure 2In a first aspect, this application provides a composite shielding film 100, comprising a metal shielding layer 110 and at least one anti-deformation layer 120 stacked along a first direction X. The anti-deformation layer 120 includes an organic reinforcement layer 121 and a self-adhesive buffer layer 122. The at least one anti-deformation layer 120 has an organic reinforcement layer 121 and a self-adhesive buffer layer 122 at its two ends along the first direction X, respectively. The organic reinforcement layer 121 is disposed between the metal shielding layer 110 and the self-adhesive buffer layer 122. The surface of the organic reinforcement layer 121 at both ends facing away from the self-adhesive buffer layer 122 is bonded to the metal shielding layer 110, and the surface of the organic reinforcement layer 121 at both ends facing away from the metal shielding layer 110 is bonded to the self-adhesive buffer layer 122. The composite shielding film 100 is bonded to an electronic device through the self-adhesive buffer layer 122 at both ends. The tensile strength of the organic reinforcement layer 121 is greater than the tensile strength of the metal shielding layer 110.

[0039] In this embodiment, the metal shielding layer 110 is used for electromagnetic shielding and grounding, which can realize the electromagnetic shielding grounding function and block the influence of external electromagnetic interference on electronic devices.

[0040] For example, the electronic device in the embodiments of this application may be a screen including an OLED module.

[0041] The composite shielding film 100 in this application embodiment may include one anti-deformation layer 120, or multiple anti-deformation layers 120, such as two, three, four or more layers, and this application is not limited thereto.

[0042] When the composite shielding film 100 includes a deformation-resistant layer 120, the organic reinforcing layer 121 and the self-adhesive buffer layer 122 in the deformation-resistant layer 120 can be regarded as the organic reinforcing layer 121 and the self-adhesive buffer layer 122 on both ends.

[0043] In this embodiment, the organic reinforcing layer 121 is made of organic polymer material, which has high strength and rigidity. The organic reinforcing layer 121 is used to support the metal shielding layer 110, which can effectively improve the composite shielding film 100's resistance to permanent deformation and prevent deformation due to external forces during the attachment or assembly process.

[0044] Because the molecular chains of the organic reinforcing layer 121 have good orientation and crystalline structure, when subjected to extrusion or surface impact, the molecular chains can disperse the impact force throughout the entire material through internal intermolecular forces. For example, the organic reinforcing layer 121 is made of polyimide. When the organic reinforcing layer 121 is compressed, the hydrogen bonds and van der Waals forces between its molecular chains work synergistically to resist deformation caused by external forces, ensuring that the composite shielding film 100 maintains shape stability under large-area stress and preventing deformation of the metal shielding layer 110 due to extrusion or surface impact, which could then affect electronic devices.

[0045] In this embodiment, the tensile strength of the organic reinforcing layer 121 is greater than the tensile strength of the metal shielding layer 110.

[0046] In this embodiment, tensile strength refers to the maximum tensile stress that a material can withstand per unit cross-sectional area (usually mm² or m²) in a uniaxial tensile test, expressed in MPa (megapascals) or N / mm². The calculation formula is:

[0047] Tensile strength = Maximum tensile load (N) / Original cross-sectional area of ​​specimen (mm2)

[0048] For example, the tensile strength was measured at 23±2°C and 50±5% humidity according to ASTM D882.

[0049] In practical applications, electronic devices may be subjected to various tensile forces, such as during assembly and disassembly, or when the device is stretched by external forces, the structure will bear tensile stress. Since the tensile strength of the organic reinforcing layer 121 is greater than that of the metal shielding layer 110, when the composite shielding film 100 is subjected to tensile force, the organic reinforcing layer 121 can preferentially bear and disperse the tensile stress, preventing the metal shielding layer 110 from deforming or even tearing due to excessive tensile force.

[0050] High tensile strength can effectively resist plastic deformation caused by external forces such as roller pressing and pressure from back components, reducing deformation transmission to the screen body at the source. For example, if the composite shielding film 100 needs to be stretched to a certain extent during equipment assembly, the organic reinforcing layer 121, due to its higher tensile strength, will evenly distribute the tensile force, allowing the metal shielding layer 110 to maintain good integrity and functionality, ensuring that the electromagnetic shielding effect is not affected.

[0051] Meanwhile, the difference in tensile strength between the organic reinforcing layer 121 and the metal shielding layer 110 can also improve the overall stability of the composite shielding film 100. During long-term use, changes in environmental factors (such as temperature fluctuations and humidity changes) may cause slight deformation of the material, while the high tensile strength of the organic reinforcing layer 121 can effectively suppress the transmission and accumulation of such deformation. Even if the metal shielding layer 110 undergoes slight expansion and contraction due to environmental factors, the organic reinforcing layer 121 can limit its excessive deformation due to its own high strength, thereby maintaining the interlayer stability of the composite shielding film 100, ensuring tight adhesion between the layers, and avoiding the impact on electromagnetic shielding performance and impact resistance due to interlayer misalignment or separation.

[0052] Furthermore, when subjected to mechanical impact, the higher tensile strength of the organic reinforcing layer 121, combined with its structural characteristics, better enhances its resistance to compressive and surface impacts. When an impact force is applied to the composite shielding film 100, the organic reinforcing layer 121 not only disperses the impact force through intermolecular chain forces but also resists the tensile stress generated by the impact due to its high strength, preventing tensile failure of the structure during the impact. For example, in a surface impact scenario, the impact force over a large area may cause the structure to generate combined tensile and compressive stresses. Due to its high tensile strength and good toughness, the organic reinforcing layer 121 can effectively resist tensile deformation. At the same time, in conjunction with the self-adhesive buffer layer 122 to absorb impact energy, it further enhances the overall impact resistance of the composite shielding film 100, providing more comprehensive protection for electronic devices from damage.

[0053] In this embodiment, the self-adhesive buffer layer 122 is self-adhesive, which makes it easy to attach the composite shielding film 100 to the electronic device. At the same time, it can play a buffering role, reducing the impact of external pressure on the metal shielding layer 110 and the organic reinforcement layer 121.

[0054] The self-adhesive buffer layer 122 is made of a highly elastic and viscous material. When subjected to a falling ball impact or point impact, the high elasticity of this material allows it to deform rapidly and absorb impact energy. For example, in a falling ball impact scenario, the self-adhesive buffer layer 122 acts like a spring, compressing and deforming at the moment of impact, converting the ball's kinetic energy into its own elastic potential energy, thereby reducing the transmission of impact force to the electronic device. Simultaneously, its adhesiveness allows the buffer layer to adhere tightly to the electronic device, preventing relative displacement during impact and further enhancing the buffering effect, protecting the electronic device from impact damage.

[0055] When the composite shielding film 100 includes multiple deformation-resistant layers 120, each deformation-resistant layer 120 is bonded to the organic reinforcing layer 121 of another deformation-resistant layer 120 via its self-adhesive buffer layer 122. For example, please refer to... Figure 2 The composite shielding film 100 includes two anti-deformation layers 120.

[0056] When multiple anti-deformation layers 120 are provided in the composite shielding film 100, a more robust and comprehensive protection system is built for electronic devices through the synergistic effect between the layers.

[0057] In summary, the composite shielding film 100 in this embodiment, by providing an organic reinforcing layer 121 and a self-adhesive buffer layer 122 on one side of the metal shielding layer 110, significantly improves the resistance to permanent deformation while maintaining shielding and grounding effects. This effectively prevents deformation of the metal shielding layer 110 from being conducted to electronic devices, thus avoiding film marks and indentations. It improves the appearance quality and performance of the display device, reduces the risk of defects caused by film marks and indentations in subsequent manufacturing processes, and increases the product yield, demonstrating promising application prospects and economic benefits.

[0058] In some embodiments, the tensile strength of the organic reinforcing layer 121 is ≥350 MPa.

[0059] High tensile strength effectively resists plastic deformation caused by external forces such as roller pressing and pressure from back components, reducing deformation transmission to the screen body at the source. Metal foils have relatively low tensile strength; for example, copper foil has a tensile strength of approximately 200-300 MPa and is easily deformed under external forces. The organic reinforcing layer 121, with a tensile strength ≥350 MPa, can maintain its structural integrity under stress, thus maintaining the stability of each layer of the composite shielding film 100. This prevents problems such as interlayer misalignment and separation caused by deformation of a single layer, ensuring that the metal shielding layer 110 can properly perform its electromagnetic shielding function and continuously protect the internal electronic components of the display device from electromagnetic interference. Simultaneously, the high tensile strength of the organic reinforcing layer 121 prevents it from easily deforming under stress, avoiding the transmission of external forces to the screen body and preventing display defects such as image distortion and color spots. This ensures a clear and stable display image and improves the user's visual experience.

[0060] For example, the tensile strength of the organic reinforcement layer 121 is 350-500 MPa. Specifically, the tensile strength of the organic reinforcement layer 121 can be 350 MPa, 400 MPa, 450 MPa or 500 MPa.

[0061] In some embodiments, in the first direction X, the thickness of the organic reinforcement layer 121 is greater than the thickness of the metal shielding layer 110.

[0062] From the perspective of improving deformation resistance, a thicker organic reinforcing layer 121 means more material reserves to resist external deformation. During the production of display devices, such as when assembling the screen and the outer casing, the composite shielding film 100 may be subjected to significant compressive and tensile forces. Since the organic reinforcing layer 121 is thicker than the metal shielding layer 110, it can utilize more intermolecular forces to disperse and absorb external forces, greatly enhancing the overall structural deformation resistance. This can more effectively prevent the metal shielding layer 110 from deforming under stress, thereby preventing the deformation of the metal shielding layer 110 from being transmitted to the screen, ensuring the flatness of the screen during the production process, reducing display abnormalities caused by structural deformation, such as image distortion and local blurring, and improving the production quality of the display device.

[0063] Meanwhile, the organic reinforcement layer 121 is thicker than the metal shielding layer 110, allowing for a more reasonable stress distribution on the composite shielding film 100 when subjected to external forces. When the display device encounters an external impact or drop, the external force will first act on the composite shielding film 100. At this time, the thicker organic reinforcement layer 121 can act as the main stress-bearing layer, dispersing the impact force over a larger area and preventing stress concentration on the metal shielding layer 110 or direct transmission to the screen. This optimized stress distribution not only protects the electromagnetic shielding function of the metal shielding layer 110 from damage but also further reduces the risk of cracks and breakage of the screen due to stress concentration, effectively improving the reliability and stability of the display device in complex operating environments.

[0064] Furthermore, the organic reinforcing layer 121 typically uses relatively low-cost organic polymer materials, while the metal shielding layer 110 (such as copper foil, aluminum foil, etc.) is relatively expensive. While ensuring the composite shielding film 100 possesses good electromagnetic shielding and deformation resistance, appropriately increasing the thickness of the organic reinforcing layer 121 to be greater than that of the metal shielding layer 110 allows for full utilization of the mechanical performance advantages of the organic reinforcing layer 121 without significantly increasing costs. This satisfies the display device's requirements for electromagnetic shielding and deformation resistance, and through a reasonable material thickness configuration, achieves an optimized balance between performance and cost. This helps display device manufacturers control production costs while ensuring product quality, improving the product's price competitiveness in the market, and achieving better economic benefits.

[0065] In some embodiments, the thickness of the organic reinforcement layer 121 in the first direction X is 30–50 μm.

[0066] In some embodiments, the thickness of the metal shielding layer 110 in the first direction X is 5 to 10 μm.

[0067] In the scenario where the composite shielding film 100 is applied to a display device, when the thickness of the organic reinforcing layer 121 in the first direction X is 30-50 μm and the thickness of the metal shielding layer 110 in the first direction X is 5-10 μm, a balance between performance and cost can be achieved.

[0068] The organic reinforcing layer 121, with a thickness of 30-50µm, can fully utilize the synergistic effect of its internal molecular chains to disperse external forces throughout the entire structure. Compared to thicknesses less than 30µm, its resistance to deformation is significantly improved, effectively resisting tensile and compressive deformation caused by external forces, preventing deformation of the metal shielding layer 110, and thus avoiding display defects such as image distortion and uneven brightness caused by structural deformation of the screen. Simultaneously, the 5-10µm thickness of the metal shielding layer 110, while ensuring electromagnetic shielding effectiveness, is relatively thin and, under the protection of the organic reinforcing layer 121, is not easily deformed by external forces. The combination of these two elements improves the deformation resistance pass rate of the composite shielding film 100 during the production process.

[0069] When the display device is subjected to external impacts, such as drops or collisions, the 30-50µm organic reinforcement layer 121 acts as the primary stress buffer layer. Due to its greater thickness and material properties, it disperses the impact force over a wider area, preventing stress concentration on the metal shielding layer 110 and the screen body. Meanwhile, the 5-10µm metal shielding layer 110, protected by the organic reinforcement layer 121, only bears a smaller portion of the stress, maintaining good electromagnetic shielding functionality. This reasonable stress distribution reduces the probability of the screen body cracking or being damaged due to impact, effectively improving the reliability and stability of the display device in complex operating environments.

[0070] The organic reinforcement layer 121 uses relatively low-cost organic polymer materials, and its thickness of 30-50µm ensures excellent mechanical properties without significantly increasing material costs. The metal shielding layer 1105-10µm, while meeting electromagnetic shielding requirements, reduces the amount of precious metal materials used. The combination of these two materials, compared to other thickness configurations, reduces the material cost of a single display device without compromising product performance.

[0071] For example, in the first direction X, the thickness of the organic reinforcement layer 121 can be 30um, 35um, 40um, 45um or 50um.

[0072] For example, in the first direction X, the thickness of the metal shielding layer 110 can be 5um, 6um, 7um, 8um, 9um or 10um.

[0073] In some embodiments, the density of the organic reinforcement layer 121 is less than the density of the metal shielding layer 110.

[0074] Metallic materials typically have a high density. Simply increasing the thickness of the metal shielding layer 110 to enhance deformation resistance would significantly increase the weight of the entire composite shielding film 100. For example, when the thickness of the metal shielding layer 110 increases from 5-10 μm to 20-30 μm, the weight of the metal shielding layer 110 itself increases significantly. However, in this embodiment, a lower-density organic reinforcing layer 121 is selected, which requires a much smaller mass of material while achieving the same or even better deformation resistance.

[0075] Display devices, especially portable display devices such as tablets, laptops, and smartphones, have an increasingly urgent need for thinner and lighter designs. Because the organic reinforcement layer 121 has a low density, it ensures excellent deformation resistance without adding excessive weight to the composite shielding film 100. Compared to higher-density materials, the low-density organic reinforcement layer 121 can effectively reduce the overall weight of the composite shielding film 100 for the same volume.

[0076] The lower density of the organic reinforcing layer 121 results in a lighter overall weight of the composite shielding film 100. On automated production lines for display devices, this reduces the power required for robotic arms to grasp and handle the composite shielding film 100, allowing for more flexible operation and effectively reducing assembly errors and equipment wear caused by excessive weight. Simultaneously, the lighter weight facilitates manual assembly by workers, reducing labor intensity, increasing assembly efficiency, and lowering labor and time costs in the production process. Furthermore, the lower density of the organic reinforcing layer 121 reduces the load-bearing requirements of connecting components during assembly with other parts, allowing for the use of lighter and lower-cost connectors, further optimizing the overall structural design and production costs of the display device.

[0077] In some embodiments, in the first direction X, the thickness of the self-adhesive buffer layer 122 is greater than the thickness of the organic reinforcement layer 121.

[0078] A thicker self-adhesive buffer layer 122 provides better cushioning. When the display device is subjected to external impact or vibration, the self-adhesive buffer layer 122 can effectively absorb and disperse energy, reducing the impact of external forces on the internal structure and protecting fragile components such as the display screen from damage. For example, when a mobile phone is accidentally dropped or bumped, the thicker self-adhesive buffer layer 122 can greatly reduce the risk of screen breakage or loosening of internal circuit connections, extending the lifespan of the display device.

[0079] The self-adhesive buffer layer 122 is relatively thick, enabling it to form a stable transition and support between the organic reinforcing layer 121 and other components. It can fill the tiny gaps between components, making the entire composite shielding film 100 more compact and stable, reducing structural damage or performance degradation caused by relative displacement between components.

[0080] Meanwhile, the thicker self-adhesive buffer layer 122 provides a larger contact area with the organic reinforcing layer 121 and other adjacent layers, resulting in a stronger bond. This effectively prevents delamination or peeling during use, ensuring the integrity and functionality of the composite shielding film 100. Even in complex operating environments, such as high temperature, high humidity, or frequent vibration, the thicker self-adhesive buffer layer 122 maintains good adhesion, ensuring a tight connection between layers and improving the reliability and stability of the display device.

[0081] In addition, the thicker self-adhesive buffer layer 122 can provide better insulation, effectively preventing short circuits between conductive components such as the metal shielding layer 110 and other components, thus enhancing the electrical safety of the display device.

[0082] In some embodiments, the thickness of the self-adhesive buffer layer 122 in the first direction X is 80 μm to 150 μm.

[0083] In the first direction X, the thickness of the self-adhesive buffer layer 122 is 80um to 150um, allowing it to more effectively perform its buffering function. When the display device is subjected to external impact, such as a mobile phone falling from a table or being accidentally bumped, the thicker self-adhesive buffer layer 122 can effectively absorb a large amount of impact energy through its own elastic deformation, dispersing the impact force over a larger area. This significantly reduces the force transmitted to the display screen and other internal precision components, greatly reducing the risk of screen breakage, electronic component damage, and other risks, protecting the core components of the display device and extending its service life.

[0084] A thickness of 80µm-150µm ensures that the self-adhesive buffer layer 122 forms a strong connection between the organic reinforcing layer 121 and other adjacent layers. It can better fill the tiny gaps between the layers, effectively reducing the relative displacement between the layers even when the display device undergoes prolonged use or complex environmental conditions.

[0085] In terms of optics, the thicker self-adhesive buffer layer 122 can more effectively reduce light reflection and scattering between layers, further improving the contrast and brightness uniformity of the display screen, presenting users with clearer and more realistic images, and enhancing the visual experience. In terms of insulation, the increased thickness provides more reliable insulation protection, effectively isolating conductive components such as the metal shielding layer 110 from other components, reducing the risk of short circuits, and enhancing the safety and stability of the display device in various electrical environments.

[0086] For example, in the first direction X, the thickness of the self-adhesive buffer layer 122 can be 80um, 90um, 100um, 110um, 120um, 130um, 140um or 150um.

[0087] In some embodiments, the self-adhesive buffer layer 122 has a storage modulus ≥ 150 kPa and a loss factor ≥ 1.0; or, the self-adhesive buffer layer 122 has a storage modulus of 60 to 150 kPa and a loss factor of 0.5 to 1.0.

[0088] When the storage modulus of the self-adhesive buffer layer 122 is greater than 150 kPa and the loss factor is greater than 1.0, the high storage modulus gives the self-adhesive buffer layer 122 strong elasticity and stiffness, enabling it to store a large amount of energy when subjected to external forces. The loss factor greater than 1.0 allows the material to effectively convert the stored energy into heat during deformation and dissipate it. This allows the self-adhesive buffer layer 122 to withstand large external forces when impacted, relying on its high storage modulus, while also rapidly dissipating the impact energy through its high loss factor. This provides excellent buffer protection for the display device and effectively reduces damage to internal components from external forces. For example, when the display device suffers accidental collisions or vibrations, this self-adhesive buffer layer 122 can significantly reduce the risk of screen breakage or damage to internal circuit components.

[0089] The high storage modulus makes the self-adhesive buffer layer 122 less prone to excessive deformation under external forces, helping to maintain the structural stability of the display device. Even under long-term use or under significant external forces, it can maintain its shape and performance, ensuring the stability of the relative positions and structural relationships between the layers, thereby guaranteeing the reliability of electromagnetic shielding and other performance characteristics. At the same time, the high loss factor also helps the material quickly return to its initial state after a certain degree of deformation, reducing material fatigue and performance degradation caused by repeated deformation.

[0090] For example, the energy storage modulus of the self-adhesive buffer layer 122 can be 150 kPa, 155 kPa, 160 kPa, 165 kPa or 170 kPa, and the loss factor can be 1.0, 1.1, 1.2, 1.3, 1.4 or 1.5.

[0091] When the energy storage modulus is 60-150 kPa and the loss factor is 0.5-1.0, the energy storage modulus of 60-150 kPa gives the self-adhesive buffer layer 122 moderate elasticity and stiffness. This allows it to provide a certain degree of cushioning while maintaining good flexibility. When the display device is subjected to external force, this self-adhesive buffer layer 122 can deform appropriately according to the magnitude and frequency of the external force, absorbing a certain amount of energy without being too stiff and causing the external force to be directly transmitted to internal components, or too soft and losing its cushioning effect. In daily use, for some minor vibrations or impacts, such as slight shaking of the handheld device or accidental collisions, the self-adhesive buffer layer 122 can provide timely and effective cushioning protection.

[0092] With a loss factor ranging from 0.5 to 1.0, the self-adhesive buffer layer 122 exhibits excellent damping performance. During material deformation, it dissipates some energy as heat, effectively suppressing vibration and noise propagation. This is crucial for improving the user experience of display devices, especially in noise-sensitive environments such as conference rooms and libraries, reducing noise generated by vibrations of internal components. Furthermore, the optimized damping characteristics help reduce aftershocks after external forces, allowing the device to recover to a stable state more quickly, thus improving its stability and reliability.

[0093] If the energy storage modulus is too low, meaning the self-adhesive buffer layer 122 is too soft, although it can generate significant deformation to buffer energy when subjected to external impact, it may result in over-buffering. This means that it is difficult to quickly return to its initial state after buffering external force, failing to provide sufficient support for the display device. This can cause components such as the display screen to wobble or shift, affecting the display effect and the overall stability of the device. Setting the lower limit of the energy storage modulus to 60 kPa or higher can prevent the material from being too soft, ensuring that it has sufficient elastic recovery force after buffering external force, providing stable support for the display device.

[0094] Overly soft self-adhesive buffer layer 122 is prone to permanent deformation under its own weight or external pressure during long-term use, failing to maintain its initial thickness and shape. This not only leads to a decrease in buffering performance but may also worsen the adhesion between layers, affecting other properties such as electromagnetic shielding. A higher storage modulus can enhance the material's resistance to deformation, enabling it to maintain better shape stability during long-term use, ensuring tight adhesion between layers and structural stability.

[0095] An overly soft self-adhesive buffer layer 122 may also lead to poor adhesion between it and other adjacent layers such as the organic reinforcing layer 121. This is because overly soft materials are prone to creep or deformation under external forces or environmental influences, resulting in uneven stress distribution at the bonding interface. This reduces the bond's strength and increases the risk of delamination or peeling. An appropriate storage modulus helps maintain the material's shape and rigidity, allowing the bonding interface to bear stress evenly, ensuring good adhesion, and maintaining the integrity of the composite shielding film 100.

[0096] When the self-adhesive buffer layer 122 is too stiff, i.e., its energy storage modulus is too high (exceeding 150 kPa) and its loss factor is too low, the material's elastic deformation capacity will be limited. Under external impact, it cannot generate sufficient deformation to absorb energy, causing most of the impact force to be directly transmitted to the internal components of the display device, increasing the risk of screen breakage and damage to electronic components. Controlling the energy storage modulus within a certain range and ensuring a sufficiently high loss factor allows the material to possess good elastic deformation and energy absorption capabilities while maintaining a certain level of stiffness, thus effectively fulfilling its buffering function.

[0097] When the rigid self-adhesive buffer layer 122 is bonded to other layers, its poor deformability can easily lead to stress concentration at the interface. When the display device is subjected to external forces or changes in environmental factors (such as temperature changes), this stress concentration may cause cracks or delamination at the interface, thereby compromising the integrity and performance of the entire composite shielding film 100. In contrast, a suitable energy storage modulus and appropriate loss factor allow the material to distribute stress more evenly under load, reducing stress concentration and improving structural reliability.

[0098] An overly rigid self-adhesive buffer layer 122 may present difficulties during processing, such as challenges in coating and bonding, increasing the complexity and cost of the manufacturing process. During use, an overly rigid material can also reduce the flexibility of the display device, making it susceptible to damage from bending, twisting, and other external forces, thus reducing product durability and user experience. Controlling the energy storage modulus and loss factor within a reasonable range can improve the operability and adaptability of the self-adhesive buffer layer 122 during both processing and use.

[0099] The loss factor reflects a material's ability to convert mechanical energy into thermal energy. An excessively high loss factor means that energy is dissipated too quickly during deformation, potentially leading to excessive wear and tear on the material's internal structure, affecting its stability and lifespan. For example, during long-term use, excessive energy dissipation may cause premature fatigue and aging, reducing the performance of the self-adhesive buffer layer 122 and preventing it from continuously providing adequate protection for the display device.

[0100] An excessively high loss factor may also negatively impact other properties of the self-adhesive buffer layer 122, such as adhesion and elastic recovery. The self-adhesive buffer layer 122 needs to achieve a balance among various properties. An excessively high loss factor may disrupt this balance, preventing the material from returning to its initial state in a timely manner after buffering external forces, thus affecting its long-term protection of the display device and its ability to work collaboratively with other layers.

[0101] In some embodiments, the metal shielding layer 110 is made of one or more of copper, aluminum, iron-nickel alloy, and steel. Optionally, the metal shielding layer 110 includes an aluminum layer and a nickel plating layer attached to the aluminum layer.

[0102] Copper possesses excellent electrical conductivity and electromagnetic shielding properties, with an electrical conductivity as high as 5.96 × 10⁻⁶. 7 S / m effectively blocks electromagnetic interference and provides excellent shielding for high-frequency electromagnetic signals. The copper metal shielding layer 110 effectively protects the internal electronic components of the display device from external electromagnetic interference, ensuring the stability and accuracy of the displayed image. Furthermore, copper has good ductility, making it easy to process into shielding layers of various shapes.

[0103] Aluminum is a lightweight metal that offers significant advantages in meeting the lightweight design requirements of display devices, and is widely used in portable display devices such as laptops and tablets. A dense aluminum oxide film easily forms on the surface of aluminum, providing some corrosion resistance and protecting the metal shielding layer to a certain extent. Although aluminum's electrical conductivity is slightly lower than copper, approximately 3.5 × 10⁻⁶... 7 While it has a low S / m, it provides good shielding against low and medium frequency electromagnetic signals and is relatively inexpensive, making it cost-effective for large-scale production.

[0104] Iron-nickel alloys possess both excellent magnetic shielding properties and mechanical strength. For low-frequency magnetic field interference, iron-nickel alloys, due to their high magnetic permeability, can guide magnetic field lines to themselves, thereby achieving magnetic shielding protection for the internal components of the display device. In display devices located near strong magnetic field sources such as large motors and transformers, using a metal shielding layer 110 made of iron-nickel alloy can effectively reduce the impact of magnetic fields on the display image, avoiding problems such as image distortion and color abnormalities. Furthermore, the high strength and hardness of iron-nickel alloys can enhance the overall mechanical properties of the composite shielding film 100 and improve the display device's resistance to compression.

[0105] Steel possesses high strength and hardness, along with excellent mechanical properties, providing robust structural support for display devices and enhancing the deformation resistance of the composite shielding film 100. In applications requiring high structural strength, such as industrial control display equipment and large outdoor displays, the steel metal shielding layer 110 can effectively withstand external impacts and protect internal electronic components. However, steel has relatively weak electrical conductivity and electromagnetic shielding properties. To achieve better electromagnetic shielding, other highly conductive metals can be plated onto the steel surface.

[0106] When different materials are combined, synergistic performance enhancement can be achieved. For example, the combination of copper and aluminum combines the high conductivity of copper with the lightweight and low cost advantages of aluminum. While ensuring good electromagnetic shielding performance, it reduces the weight of the display device, making it suitable for consumer-grade display products that require both shielding performance and lightweight design.

[0107] Preferably, the metal shielding layer 110 includes an aluminum layer and a nickel plating layer attached to the aluminum layer. Nickel has good chemical stability and corrosion resistance; nickel plating on the aluminum layer surface can effectively protect the aluminum layer from environmental corrosion. In humid, acidic, or alkaline environments, the nickel plating layer can act as a robust barrier, preventing the aluminum layer from being oxidized or corroded, thus extending the service life of the metal shielding layer 110. Simultaneously, nickel has good electrical conductivity and strong adhesion to aluminum; therefore, nickel plating does not negatively affect the electromagnetic shielding performance of the aluminum layer. On the contrary, it can further improve the electromagnetic shielding effectiveness of the metal shielding layer 110 by optimizing surface smoothness and reducing electromagnetic signal reflection loss.

[0108] In some embodiments, the metal shielding layer 110 may be a copper foil layer, an aluminum foil layer, or a copper-aluminum composite foil layer, etc., to meet different electromagnetic shielding requirements.

[0109] In some embodiments, the organic reinforcing layer 121 is made of one or more of carbon fiber, polyetheretherketone, polyethylene terephthalate, and polyethylene naphthalate.

[0110] Preferably, the organic reinforcing layer 121 is made of polyetheretherketone modified with carbon fiber.

[0111] Carbon fiber boasts an exceptionally high strength-to-weight ratio; its strength is several times that of steel, while its density is far lower. In display devices, when subjected to external pressure or impact, the organic reinforcing layer 121 made of carbon fiber effectively disperses stress due to its excellent tensile strength, preventing deformation of the metal shielding layer 110 and the display screen body. Furthermore, carbon fiber exhibits excellent corrosion resistance, maintaining stable performance even in complex environments such as humidity and acid / alkali conditions, thus extending the lifespan of the display device.

[0112] Polyetheretherketone (PEEK) has excellent high-temperature resistance, maintaining stable physical and chemical properties even at high temperatures. It also possesses good chemical corrosion resistance, abrasion resistance, and mechanical properties, making it suitable for display devices with high environmental adaptability requirements.

[0113] Polyethylene terephthalate (PET) possesses excellent flexibility and processing properties, making it easy to fabricate organic reinforcing layers 121 of various shapes. PET boasts a light transmittance of over 89%, ensuring that its application as an organic reinforcing layer 121 in display devices does not significantly impact the display performance. Furthermore, PET exhibits a degree of impact resistance, acting as a buffer against minor external forces and reducing damage to internal components. Moreover, PET's relatively low cost allows for effective cost control in large-scale production, enhancing the product's market competitiveness.

[0114] Polyethylene naphthalate (PEN) possesses a high glass transition temperature (approximately 125°C) and superior mechanical properties, including higher tensile strength. In high-temperature environments, the organic reinforcement layer 121 of PEN maintains excellent dimensional stability, preventing structural deformation caused by temperature changes. Furthermore, PEN exhibits excellent chemical resistance and UV resistance, making it suitable for outdoor displays and other applications requiring high environmental adaptability. It effectively protects the internal structure of the display device, extending its lifespan in harsh environments.

[0115] When the organic reinforcing layer 121 uses a combination of two or more materials, synergistic optimization of performance can be achieved. Preferably, carbon fiber is composited with polyetheretherketone (PEEK), especially when carbon fiber-modified PEEK is used as the material of the organic reinforcing layer 121, the performance is further improved. The addition of carbon fiber significantly enhances the strength and modulus of PEEK. A strong interfacial bond is formed between the carbon fiber and the PEEK matrix. When the composite shielding film 100 is subjected to external forces, the carbon fiber can effectively bear and disperse the stress, which greatly improves the tensile strength, compressive strength, and flexural strength of the organic reinforcing layer 121. At the same time, the good toughness of PEEK itself also compensates for the relatively brittleness of carbon fiber to a certain extent, reduces the risk of structural fracture due to stress concentration, and improves the overall toughness and reliability of the composite shielding film.

[0116] In addition, the high temperature resistance of polyetheretherketone itself, combined with the high thermal stability of carbon fiber, can prevent it from softening and deforming due to high temperature, ensuring that the composite shielding film 100 can work stably for a long time in high temperature environments above 200℃, maintaining good deformation resistance and electromagnetic shielding performance.

[0117] In some embodiments, the material of the self-adhesive buffer layer 122 includes one or more of acrylic pressure-sensitive adhesive, silicone pressure-sensitive adhesive layer and rubber-based pressure-sensitive adhesive.

[0118] Acrylic pressure-sensitive adhesives possess moderate and durable tack, enabling them to adhere tightly to the organic reinforcing layer 121 and the surfaces of display device components. This ensures a stable bond between the layers of the composite shielding film 100, preventing delamination or peeling even during long-term use. Furthermore, acrylic pressure-sensitive adhesives exhibit excellent weather resistance, maintaining stable adhesion and physical properties even under complex environmental conditions such as high and low temperatures and humidity variations. For example, in the hot and humid southern regions or the cold and dry northern regions, display devices using acrylic pressure-sensitive adhesives as the self-adhesive buffer layer 122 can still maintain a tight bond between layers, ensuring normal electromagnetic shielding and deformation resistance. In addition, acrylic pressure-sensitive adhesives have good transparency, not significantly affecting the optical performance of the display device, thus helping to maintain the clarity and color accuracy of the screen display.

[0119] Silicone-based pressure-sensitive adhesives possess excellent high-temperature resistance, enabling long-term stable operation at temperatures up to 200°C or even higher without melting, flowing, or significant decrease in adhesion. This characteristic makes the self-adhesive buffer layer 122 using silicone-based pressure-sensitive adhesives particularly suitable for display devices with high heat dissipation requirements or operating environments with high temperatures, such as high-performance game console displays and industrial control monitors. During the operation of these devices, a large amount of heat is generated internally. The silicone-based pressure-sensitive adhesive can withstand high temperatures, maintaining the integrity and stability of the composite shielding film 100. Simultaneously, its excellent insulation properties provide additional electrical safety for the display device. Furthermore, silicone-based pressure-sensitive adhesives exhibit good adhesion to various material surfaces, including glass, metal, and plastics, enabling reliable connections with various components of the display device.

[0120] Rubber-type pressure-sensitive adhesive has high elasticity and excellent cushioning performance. When the display device is subjected to external impact or vibration, the rubber-type pressure-sensitive adhesive can quickly undergo elastic deformation, absorb a large amount of energy, and effectively reduce the impact of the impact on internal components.

[0121] The self-adhesive buffer layer 122 can be made of a single type of pressure-sensitive adhesive, or a combination of two or more pressure-sensitive adhesives. Combining two or more pressure-sensitive adhesives allows for complementary advantages, further enhancing the performance of the composite shielding film 100. For example, mixing acrylic pressure-sensitive adhesives with rubber-based pressure-sensitive adhesives can enhance the buffering performance of the self-adhesive buffer layer 122 while maintaining good adhesion and weather resistance; combining silicone pressure-sensitive adhesives with acrylic pressure-sensitive adhesives can significantly improve high-temperature resistance while maintaining high transparency and good optical performance. This diverse selection and combination of materials allows the self-adhesive buffer layer 122 to be flexibly configured according to the specific needs and usage scenarios of different display devices, providing higher quality and more reliable protection for display devices and improving the product's market competitiveness and adaptability.

[0122] When the composite shielding film 100 includes multiple anti-deformation layers 120, the organic reinforcing layers 121 in the multiple anti-deformation layers 120 can be made of the same or different materials. For example, the composite shielding film 100 includes two anti-deformation layers 120, wherein the outer organic reinforcing layer 121 is made of polyethylene naphthalate and the inner organic reinforcing layer 121 is made of polyetheretherketone; the self-adhesive buffer layers 122 in the multiple anti-deformation layers 120 can be made of the same or different materials.

[0123] In some embodiments, the metal shielding layer 110 is attached to the side of the organic reinforcing layer 121 opposite to the self-adhesive buffer layer 122 by means of adhesive bonding or electroplating.

[0124] The metal shielding layer 110 is attached to the side of the organic reinforcing layer 121 opposite to the self-adhesive buffer layer 122 using an adhesive method, which is simple to operate and highly flexible in process. This connection method can effectively fill the tiny gaps between the metal shielding layer 110 and the organic reinforcing layer 121, so that the two are tightly bonded and the integrity of the composite shielding film 100 is enhanced.

[0125] Please see Figure 3 In some embodiments, an adhesive layer 130 is provided between the metal shielding layer 110 and the organic reinforcement layer 121, and the metal shielding layer 110 and the organic reinforcement layer 121 are bonded together by the adhesive layer 130.

[0126] In actual production, suitable adhesives can be selected to form the bonding layer 130 based on the different material properties. For example, for the organic reinforcing layer 121 made of polyimide and the metal shielding layer 110 made of copper, a high-temperature resistant and highly adhesive epoxy resin adhesive can be used. Alternatively, one or more pressure-sensitive adhesives selected from acrylic pressure-sensitive adhesives, silicone pressure-sensitive adhesives, and rubber-based pressure-sensitive adhesives can be used to form the bonding layer 130. Because the adhesive itself has a certain degree of flexibility, it can act as a buffer when the display device is subjected to external impact or vibration, reducing stress concentration caused by differences in the coefficients of thermal expansion of the materials, and preventing delamination or detachment between the metal shielding layer 110 and the organic reinforcing layer 121. Furthermore, the bonding process has relatively low requirements for production equipment, reducing equipment investment costs for manufacturing enterprises. It is suitable for small and medium-sized enterprises and facilitates process adjustment and optimization to meet the personalized needs of different display devices.

[0127] In some embodiments, the thickness of the adhesive layer 130 in the first direction X is 5 to 10 μm.

[0128] For example, the thickness of the adhesive layer 130 in the first direction X can be 5um, 6um, 7um, 8um, 9um or 10um.

[0129] Electroplating can make the connection between the metal shielding layer 110 and the organic reinforcement layer 121 more robust and stable. Taking the metal shielding layer 110, which combines an aluminum layer and a nickel plating layer, as an example, the electroplating process can form a uniform and dense metal layer on the surface of the organic reinforcement layer 121, enabling molecular-level bonding between the metal shielding layer 110 and the organic reinforcement layer 121. This connection method significantly improves the mechanical strength and stability of the composite shielding film. During long-term use of the display device, even under significant external forces, the metal shielding layer 110 is less likely to shift or detach. Simultaneously, the electroplating layer can effectively improve the surface properties of the metal shielding layer 110, such as increasing surface flatness and smoothness, further enhancing electromagnetic shielding effectiveness. A smoother surface reduces electromagnetic signal reflection loss, resulting in better blocking of electromagnetic interference by the metal shielding layer 110.

[0130] In some embodiments, the self-adhesive buffer layer 122 is coated or attached to the side of the organic reinforcing layer 121 facing away from the metal shielding layer 110.

[0131] The self-adhesive buffer layer 122 can be coated onto the side of the organic reinforcing layer 121 facing away from the metal shielding layer 110, achieving uniform and continuous application of the self-adhesive buffer layer 122. During production, by precisely controlling coating process parameters such as coating speed and coating thickness, the thickness and performance of the self-adhesive buffer layer 122 can be flexibly adjusted according to the needs of different display devices. The coating process ensures full contact between the self-adhesive buffer layer 122 and the organic reinforcing layer 121, forming a tight bonding interface and ensuring good adhesive strength. This effectively prevents localized detachment or delamination of the self-adhesive buffer layer 122 during use, maintaining the integrity and stability of the composite shielding film 100. Simultaneously, the coating method also allows for efficient utilization of the self-adhesive buffer layer 122 material, reducing material waste and lowering production costs.

[0132] In this embodiment, the self-adhesive buffer layer 122 can also be attached to the side of the organic reinforcing layer 121 facing away from the metal shielding layer 110, offering advantages such as convenient operation and high production efficiency. In practical applications, the self-adhesive buffer layer 122 can be pre-processed into sheet materials of specific shapes and sizes, and then quickly bonded to the organic reinforcing layer 121 using automated attachment equipment, significantly shortening the production cycle and improving production efficiency. This method is particularly suitable for standardized production of display devices, ensuring consistent installation quality of the self-adhesive buffer layer 122 for each product and improving product yield. Moreover, the attachment method has relatively low requirements for the material of the self-adhesive buffer layer 122; some pressure-sensitive adhesive materials with good flexibility and adhesion can be used, further broadening the material selection range for the self-adhesive buffer layer 122. Simultaneously, during subsequent maintenance and replacement, the attached self-adhesive buffer layer 122 is easy to disassemble and reinstall, reducing the maintenance difficulty and cost of the display device.

[0133] Please refer to the following: Figures 1 to 4 Secondly, embodiments of this application provide a method for preparing the above-mentioned composite shielding film 100, comprising: preparing at least one anti-deformation layer 120, the anti-deformation layer 120 including an organic reinforcing layer 121 and a self-adhesive buffer layer 122, wherein the at least one anti-deformation layer 120 has an organic reinforcing layer 121 and a self-adhesive buffer layer 122 at its two ends along a first direction X, and forming a metal shielding layer 110 on the side of the organic reinforcing layer 121 facing away from the self-adhesive buffer layer 122 at both ends.

[0134] Depending on the performance requirements of different display devices, the organic reinforcement layer 121 can be made of one or more of the following materials: carbon fiber, polyetheretherketone, polyethylene terephthalate (PET), and polyethylene naphthalate (PEN).

[0135] In the step of forming a self-adhesive buffer layer 122 on one side of the organic reinforcement layer 121, the self-adhesive buffer layer 122 can be formed on one side of the organic reinforcement layer 121 by coating or attaching.

[0136] In the step of forming a metal shielding layer 110 on the side of the organic reinforcing layer 121 away from the self-adhesive buffer layer 122, the metal shielding layer 110 is formed on one side of the organic reinforcing layer 121 by means of bonding or electroplating.

[0137] Please see Figure 5 and Figure 6 Thirdly, embodiments of this application provide a display device, including: an OLED module 200 and the aforementioned composite shielding film 100, wherein the composite shielding film 100 is attached to one side surface of the OLED module 200.

[0138] The display device in this application includes the composite shielding film 100 in the first aspect of this application. By providing an organic reinforcing layer 121 and a self-adhesive buffer layer 122 on one side of the metal shielding layer 110, the composite shielding film 100 not only has a shielding grounding effect, but also significantly improves its resistance to permanent deformation. This effectively avoids the problem of film marks and indentations caused by the deformation of the metal shielding layer 110 being conducted to the screen body. This improves the appearance quality and performance of the display device, reduces the risk of defects caused by film marks and indentations in the subsequent manufacturing process of the display device, and improves the yield rate of the product. It has good application prospects and economic benefits.

[0139] Example

[0140] The following examples describe the disclosure of this invention in more detail. These examples are for illustrative purposes only, as various modifications and variations will be apparent to those skilled in the art within the scope of this disclosure. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are based on weight, and all reagents used in the examples are commercially available or synthesized by conventional methods and can be used directly without further processing, as are the instruments used in the examples.

[0141] Example 1

[0142] A composite shielding film includes a metal shielding layer, an organic reinforcing layer and a self-adhesive buffer layer stacked sequentially in a first direction;

[0143] The metal shielding layer is made of copper foil and has a thickness of 5µm in the first direction.

[0144] The organic reinforcement layer is made of carbon fiber modified polyetheretherketone, with a thickness of 30 μm in the first direction and a tensile strength of 350 MPa.

[0145] The metal shielding layer and the organic reinforcement layer are bonded together by an adhesive layer, the thickness of which is 5 μm in the first direction;

[0146] The self-adhesive buffer layer is made of acrylic pressure-sensitive adhesive, with a thickness of 80 μm in the first direction, a storage modulus of 160 MPa, and a loss factor of 1.2.

[0147] Example 2

[0148] A composite shielding film includes a metal shielding layer, an organic reinforcing layer and a self-adhesive buffer layer stacked sequentially in a first direction;

[0149] The metal shielding layer is made of copper foil and has a thickness of 5µm in the first direction.

[0150] The organic reinforcement layer is made of carbon fiber modified polyetheretherketone, with a thickness of 40 μm in the first direction and a tensile strength of 380 kPa.

[0151] The metal shielding layer and the organic reinforcement layer are bonded together by an adhesive layer, the thickness of which is 5 μm in the first direction;

[0152] The self-adhesive buffer layer is made of acrylic pressure-sensitive adhesive, with a thickness of 80 μm in the first direction, a storage modulus of 160 MPa, and a loss factor of 1.2.

[0153] Example 3

[0154] A composite shielding film includes a metal shielding layer, an organic reinforcing layer and a self-adhesive buffer layer stacked sequentially in a first direction;

[0155] The metal shielding layer is made of copper foil and has a thickness of 5µm in the first direction.

[0156] The organic reinforcement layer is made of carbon fiber modified polyetheretherketone, with a thickness of 50 μm in the first direction and a tensile strength of 380 kPa.

[0157] The metal shielding layer and the organic reinforcement layer are bonded together by an adhesive layer, the thickness of which is 5 μm in the first direction;

[0158] The self-adhesive buffer layer is made of acrylic pressure-sensitive adhesive, with a thickness of 80 μm in the first direction, a storage modulus of 160 MPa, and a loss factor of 1.2.

[0159] Example 4

[0160] A composite shielding film includes a metal shielding layer, an organic reinforcing layer and a self-adhesive buffer layer stacked sequentially in a first direction;

[0161] The metal shielding layer is made of copper foil and has a thickness of 5µm in the first direction.

[0162] The organic reinforcement layer is made of carbon fiber modified polyetheretherketone, with a thickness of 40 μm in the first direction and a tensile strength of 380 kPa.

[0163] The metal shielding layer and the organic reinforcement layer are bonded together by an adhesive layer, the thickness of which is 5 μm in the first direction;

[0164] The self-adhesive buffer layer is made of acrylic pressure-sensitive adhesive, with a thickness of 110 μm in the first direction, a storage modulus of 160 MPa, and a loss factor of 1.2.

[0165] Example 5

[0166] A composite shielding film includes a metal shielding layer, an organic reinforcing layer and a self-adhesive buffer layer stacked sequentially in a first direction;

[0167] The metal shielding layer is made of copper plating and has a thickness of 5µm in the first direction.

[0168] The organic reinforcement layer is made of carbon fiber modified polyetheretherketone, with a thickness of 40 μm in the first direction and a tensile strength of 380 kPa.

[0169] The self-adhesive buffer layer is made of acrylic pressure-sensitive adhesive, with a thickness of 110 μm in the first direction, a storage modulus of 160 MPa, and a loss factor of 1.2.

[0170] Example 6

[0171] A composite shielding film includes a metal shielding layer, an organic reinforcing layer and a self-adhesive buffer layer stacked sequentially in a first direction;

[0172] The metal shielding layer is made of copper plating and has a thickness of 5µm in the first direction.

[0173] The organic reinforcement layer is made of carbon fiber modified polyetheretherketone, with a thickness of 40 μm in the first direction and a tensile strength of 380 kPa.

[0174] The self-adhesive buffer layer is made of acrylic pressure-sensitive adhesive, with a thickness of 110 μm in the first direction, a storage modulus of 100 kPa, and a loss factor of 0.8.

[0175] Comparative Example 1

[0176] A composite shielding film includes a metal shielding layer and a self-adhesive buffer layer stacked sequentially in a first direction;

[0177] The metal shielding layer is made of copper plating and has a thickness of 5µm in the first direction.

[0178] The self-adhesive buffer layer is made of acrylic pressure-sensitive adhesive, with a thickness of 80 μm in the first direction, a storage modulus of 160 MPa, and a loss factor of 1.2.

[0179] Comparative Example 2

[0180] A composite shielding film includes a metal shielding layer, an organic reinforcing layer and a self-adhesive buffer layer stacked sequentially in a first direction;

[0181] The metal shielding layer is made of copper foil and has a thickness of 5µm in the first direction.

[0182] The organic reinforcement layer is made of carbon fiber modified polyetheretherketone, with a thickness of 40 μm in the first direction and a tensile strength of 300 MPa.

[0183] The metal shielding layer and the organic reinforcement layer are bonded together by an adhesive layer, the thickness of which is 5 μm in the first direction;

[0184] The self-adhesive buffer layer is made of acrylic pressure-sensitive adhesive, with a thickness of 80 μm in the first direction, a storage modulus of 160 MPa, and a loss factor of 1.2.

[0185] Comparative Example 3

[0186] A composite shielding film includes a metal shielding layer, an organic reinforcing layer and a self-adhesive buffer layer stacked sequentially in a first direction;

[0187] The metal shielding layer is made of copper foil and has a thickness of 5µm in the first direction.

[0188] The organic reinforcement layer is made of carbon fiber modified polyetheretherketone, with a thickness of 20 μm in the first direction and a tensile strength of 350 MPa.

[0189] The metal shielding layer and the organic reinforcement layer are bonded together by an adhesive layer, the thickness of which is 5 μm in the first direction;

[0190] The self-adhesive buffer layer is made of acrylic pressure-sensitive adhesive, with a thickness of 80 μm in the first direction, a storage modulus of 160 MPa, and a loss factor of 1.2.

[0191] Comparative Example 4

[0192] A composite shielding film includes a metal shielding layer, an organic reinforcing layer and a self-adhesive buffer layer stacked sequentially in a first direction;

[0193] The metal shielding layer is made of copper foil and has a thickness of 5µm in the first direction.

[0194] The organic reinforcement layer is made of carbon fiber modified polyetheretherketone, with a thickness of 40 μm in the first direction and a tensile strength of 380 MPa.

[0195] The metal shielding layer and the organic reinforcement layer are bonded together by an adhesive layer, the thickness of which is 5 μm in the first direction;

[0196] The self-adhesive buffer layer is made of acrylic pressure-sensitive adhesive, with a thickness of 80 μm in the first direction, a storage modulus of 180 MPa, and a loss factor of 0.8.

[0197] Comparative Example 5

[0198] A composite shielding film includes a metal shielding layer, an organic reinforcing layer and a self-adhesive buffer layer stacked sequentially in a first direction;

[0199] The metal shielding layer is made of copper foil and has a thickness of 5µm in the first direction.

[0200] The organic reinforcement layer is made of carbon fiber modified polyetheretherketone, with a thickness of 40 μm in the first direction and a tensile strength of 380 MPa.

[0201] The metal shielding layer and the organic reinforcement layer are bonded together by an adhesive layer, the thickness of which is 5 μm in the first direction;

[0202] The self-adhesive buffer layer is made of acrylic pressure-sensitive adhesive, with a thickness of 80 μm in the first direction, a storage modulus of 100 MPa, and a loss factor of 1.2.

[0203] Performance testing

[0204] The composite shielding films from Examples 1-6 and Comparative Examples 1-5 were adhered to one side of the OLED module for performance testing.

[0205] Impact resistance test: The OLED module was placed face down on a steel ball drop test device, with the side facing away from the composite shielding film facing down, and the four corners were secured with tape to prevent slippage. An 11.2g steel ball was dropped freely from different heights onto the side of the composite shielding film facing away from the OLED module, with five points tested at the same height. After the drop test, the module was turned on to check for any bright spots or dark spots. The height at which a bright spot or dark spot appears on the display module represents the impact resistance; that is, the higher the height, the stronger the impact resistance. The test results are shown in Table 1.

[0206] Table 1 Test Results

[0207] project Impact resistance Example 1 75mm Example 2 90mm Example 3 100mm Example 4 95mm Example 5 90mm Example 6 85mm Comparative Example 1 45mm Comparative Example 2 60mm Comparative Example 3 65mm Comparative Example 4 55mm Comparative Example 5 55mm

[0208] As shown in Table 1, the composite shielding film in this embodiment of the application significantly improves the resistance to permanent deformation while providing shielding and grounding effects by setting an organic reinforcing layer and a self-adhesive buffer layer on one side of the metal shielding layer.

[0209] The above are merely specific embodiments of this application, but the scope of protection of this application is not limited thereto. Any person skilled in the art can easily conceive of various equivalent modifications or substitutions within the technical scope disclosed in this application, and these modifications or substitutions should all be included within the scope of protection of this application. Therefore, the scope of protection of this application should be determined by the scope of the claims.

Claims

1. A composite shielding film, characterized in that, It includes a metal shielding layer stacked along a first direction and at least one deformation-resistant layer, wherein the deformation-resistant layer includes an organic reinforcement layer and a self-adhesive buffer layer, and the organic reinforcement layer and the self-adhesive buffer layer are respectively located at both ends of the at least one deformation-resistant layer along the first direction; The composite shielding film is attached to the electronic device via the self-adhesive buffer layer. The metal shielding layer provides electromagnetic shielding, the organic reinforcement layer supports the metal shielding layer, and the self-adhesive buffer layer provides adhesion and cushioning. The organic reinforcement layer is disposed between the metal shielding layer and the self-adhesive buffer layer. The surface of the organic reinforcement layer on both ends facing away from the self-adhesive buffer layer is bonded to the metal shielding layer, and the surface of the organic reinforcement layer on both ends facing away from the metal shielding layer is bonded to the self-adhesive buffer layer. The tensile strength of the organic reinforcement layer is greater than that of the metal shielding layer.

2. The composite shielding film according to claim 1, characterized in that, The tensile strength of the organic reinforcement layer is ≥350 MPa.

3. The composite shielding film according to claim 1, characterized in that, In the first direction, the thickness of the organic reinforcement layer is greater than the thickness of the metal shielding layer; Optionally, the thickness of the organic reinforcing layer in the first direction is 30–50 μm; Optionally, the thickness of the metal shielding layer in the first direction is 5 to 10 μm.

4. The composite shielding film according to any one of claims 1 to 3, characterized in that, The density of the organic reinforcement layer is less than the density of the metal shielding layer.

5. The composite shielding film according to any one of claims 1 to 3, characterized in that, In the first direction, the thickness of the self-adhesive buffer layer is greater than the thickness of the organic reinforcement layer; Optionally, the thickness of the self-adhesive buffer layer in the first direction is 80µm to 150µm.

6. The composite shielding film according to claim 5, characterized in that, The energy storage modulus of the self-adhesive buffer layer is >150 kPa, and the loss factor is >1.0; Alternatively, the energy storage modulus of the self-adhesive buffer layer is 60–150 kPa, and the loss factor is 0.5–1.

0.

7. The composite shielding film according to claim 1, characterized in that, The metal shielding layer is made of one or more of copper, aluminum, iron-nickel alloy, and steel; optionally, the metal shielding layer includes an aluminum layer and a nickel plating layer attached to the aluminum layer; and / or, The organic reinforcing layer is made of one or more of carbon fiber, polyetheretherketone, polyethylene terephthalate, and polyethylene naphthalate; preferably, the organic reinforcing layer is made of carbon fiber-modified polyetheretherketone; and / or, The material of the self-adhesive buffer layer includes one or more of acrylic pressure-sensitive adhesive, silicone pressure-sensitive adhesive, and rubber-based pressure-sensitive adhesive.

8. The composite shielding film according to claim 1, characterized in that, The metal shielding layer is attached to the side of the organic reinforcing layer away from the self-adhesive buffer layer by means of adhesive bonding or electroplating. Optionally, an adhesive layer is provided between the metal shielding layer and the organic reinforcement layer, and the metal shielding layer and the organic reinforcement layer are bonded together by the adhesive layer; Optionally, the thickness of the adhesive layer in the first direction is 5–10 μm; and / or, The self-adhesive buffer layer is coated or attached to the side of the organic reinforcing layer opposite to the metal shielding layer.

9. A method for preparing a composite shielding film as described in any one of claims 1 to 8, characterized in that, include: At least one anti-deformation layer is prepared, the anti-deformation layer comprising an organic reinforcement layer and a self-adhesive buffer layer, wherein the organic reinforcement layer and the self-adhesive buffer layer are respectively located at both ends along the first direction; A metal shielding layer is formed on the side of the organic reinforcing layer opposite to the self-adhesive buffer layer at both ends.

10. A display device, characterized in that, include: The OLED module and the composite shielding film according to any one of claims 1-8, wherein the composite shielding film is attached to one side surface of the OLED module.