Semiconductor structure and method of forming the same, memory

By using anisotropic etching to form a passivation material layer during the semiconductor structure formation process, the problems of complex processes and high costs in existing technologies are solved, achieving the effects of simplifying the process flow and reducing costs.

CN123164777APending Publication Date: 2026-11-24SHENZHEN ZHANGGE INSTR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511863668.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-12-10
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing semiconductor structure formation methods involve complex processes and high technical difficulty, making it difficult to reduce costs. In particular, there are risks of inhomogeneity and reliability issues during the deposition and removal of the etched protective layer.

Method used

An anisotropic etching process is used to form a passivation material layer. The passivation material layer on the bottom surface of the protective material layer is removed, while the passivation material layer on the sidewall is retained as a stop layer, which simplifies the process and reduces costs.

Benefits of technology

By simplifying the process flow, the manufacturing difficulty and cost of semiconductor structures are reduced, while electrical connection performance and reliability are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123164777A_ABST
    Figure CN123164777A_ABST
Patent Text Reader

Abstract

A semiconductor structure and its formation method, and a memory, wherein the semiconductor structure formation method involves forming a protective material layer covering the top, sidewalls, and bottom of the stacked structure, and performing an anisotropic etching process. The anisotropic etching process performs surface passivation treatment on the protective material layer to form a passivation material layer. The anisotropic etching process also removes the passivation material layer located on the bottom surface of the protective material layer, while retaining the passivation material layer located on the sidewalls of the protective material layer as a passivation layer. This allows the passivation layer to serve as a stop layer, enabling the removal of the exposed portion of the first protective layer along each first trench without the need for an additional process to form a stop layer, thereby simplifying the process and reducing costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor manufacturing, and more particularly to a semiconductor structure and a method for forming the same, and a memory. Background Technology

[0002] A 3D (Three Dimensional) memory structure consists of multiple conductive plates and dielectric layers stacked in a cross pattern, with numerous conductive pillars that are wider at the top and narrower at the bottom. The opposing surfaces of the conductive plates and pillars are the upper and lower electrodes, respectively. The memory cell includes a capacitor, which comprises an upper electrode, a lower electrode, and a dielectric material located between the upper and lower electrodes. 3D memory uses a plate-last process, where the conductive pillar structure is first completed, then wet etching is used to create trenches near the conductive pillars to contact the protective material layers at the corresponding positions of each conductive plate. The protective material layers are then removed, and finally, the conductive plate material is filled in to form the conductive plates. Summary of the Invention

[0003] The problem solved by the embodiments of the present invention is to provide a semiconductor structure and its formation method, and a memory, which can simplify the process and reduce costs.

[0004] To address the above problems, embodiments of the present invention provide a method for forming a semiconductor structure, comprising: A substrate is provided on which a stacked structure is formed, the stacked structure comprising dielectric layers and sacrificial layers stacked alternately from bottom to top in a longitudinal direction; Forming through-holes that penetrate the stacked structure; A protective material layer is formed covering the top, sidewalls, and bottom of the stacked structure, wherein the material of the protective material layer includes a conductive material; An anisotropic etching process is performed to passivate the protective material layer on the sidewall and bottom surface of the via, forming a passivation material layer. The anisotropic etching process removes the passivation material layer on the bottom surface of the protective material layer on the bottom surface of the via, while retaining the passivation material layer on the sidewall of the protective material layer on the sidewall of the via. A conductive pillar structure is formed to fill the through-hole; Remove the protective material layer on top of the stacked structure, retain the protective material layer on the sidewall and bottom of the through hole as the first protective layer, and the remaining passivation material layer as the passivation layer, which is located on the sidewall of the first protective layer; The sacrificial layer in the stacked structure is removed to form a plurality of first trenches arranged at intervals along the longitudinal direction, the first trenches being surrounded by longitudinally adjacent dielectric layers; Using the passivation layer as a stop layer, the exposed portion of the first protective layer is removed along each of the first trenches to form a second trench. The second trench is connected to the first trench to form a third trench, and the remaining first protective layer is formed as the second protective layer. A dielectric layer is formed covering each side and bottom surface of the third trench; A conductive plate structure is formed to fill the third trench, and the conductive plate structure covers the dielectric layer.

[0005] Accordingly, embodiments of the present invention also provide a semiconductor structure prepared using the formation method described in any of the preceding claims.

[0006] Accordingly, embodiments of the present invention also provide a semiconductor structure, comprising: Base; A stacked layer, located on the substrate, the stacked layer comprising dielectric layers and conductive plate structures alternately stacked longitudinally from bottom to top; Multiple conductive pillar structures penetrate the stacked layers; A passivation layer is continuously disposed along the sidewall of the conductive pillar structure; A second protective layer is provided along the entire surface of the conductive pillar structure that does not deviate from the substrate. The second protective layer is interrupted by the conductive plate structure to form a discontinuous layer. The second protective layer contacts the passivation layer on the surface that deviates from the conductive pillar structure. A dielectric layer is formed on the surface of the conductive plate structure opposite to the second protective layer and the dielectric layer; The passivation layer and the second protective layer have at least one of the same elements.

[0007] Compared with the prior art, the technical solution of the embodiments of the present invention has the following advantages: In the semiconductor structure formation method provided by the embodiments of the present invention, a protective material layer is formed covering the top of the stacked structure, the sidewalls of the vias, and the bottom surface. An anisotropic etching process is then performed. The anisotropic etching process passivates the surface of the protective material layer to form a passivation material layer. The anisotropic etching process also removes the passivation material layer located on the bottom surface of the protective material layer, while retaining the passivation material layer located on the sidewalls of the protective material layer as a passivation layer. This allows the passivation layer to serve as a stop layer, enabling the removal of the exposed portion of the first protective layer along each first trench without the need for an additional process to form a stop layer. This simplifies the process and reduces costs. Attached Figure Description

[0008] Figures 1 to 9 This is a schematic diagram of the structure corresponding to each step in one embodiment of the method for forming a semiconductor structure of the present invention; Figure 10 This is a schematic diagram of a semiconductor structure according to one embodiment of the present invention. Detailed Implementation

[0009] As the background technology shows, current semiconductor structure formation methods typically require the deposition of an etch-protected layer on the outer wall of the conductive pillar structure (i.e., the sidewall of the via containing the conductive pillar structure) to protect the conductive pillar structure during the etching removal of the sacrificial material layer. After forming the conductive pillar structure, the sacrificial material layer is removed using the deposited etch-protected layer as a stop layer. Due to the large depth-to-width ratio of the vias containing the conductive pillar structure, the deposition process of the etch-protected layer is difficult and uniform. Insufficient etch-protected layer thickness fails to protect the conductive pillar structure, while excessive thickness occupies space within the via and affects the fabrication and electrical properties of the conductive pillar structure. Particularly concerning are the thicker portions caused by uneven etch-protected layer thickness, especially when the etch-protected layer uses an insulating material. This necessitates removing the etch-protected layer at the bottom of the via to allow the conductive pillar structure to electrically connect with the conductive structure at the bottom of the via. After removing the sacrificial material layer, the exposed etch-protected layer must also be etched away, and etching the unevenly thick etch-protected layer further increases reliability risks. In summary, current methods for forming semiconductor structures suffer from complex processes and high technological difficulty, which hinders efforts to reduce the cost of semiconductor structures.

[0010] To address the aforementioned technical problems, the present invention provides a method for forming a semiconductor structure, comprising: providing a substrate, on which a stacked structure is formed, the stacked structure including a dielectric layer and a sacrificial layer alternately stacked longitudinally from bottom to top; forming a via through the stacked structure; forming a protective material layer covering the top, sidewalls, and bottom of the stacked structure, the material of the protective material layer including a conductive material; performing an anisotropic etching process, wherein the anisotropic etching process performs surface passivation treatment on the protective material layer on the sidewalls and bottom of the via to form a passivation material layer, and the anisotropic etching process further removes the passivation material layer on the surface of the protective material layer located on the bottom surface of the via, while retaining the passivation material layer on the surface of the protective material layer located on the sidewalls of the via; forming A conductive pillar structure filling through-holes; removing the protective material layer at the top of the stacked structure, retaining the protective material layers on the sidewalls and bottom of the through-holes as the first protective layer, and the remaining passivation material layer as the passivation layer, the passivation layer being located on the sidewalls of the first protective layer; removing the sacrificial layer in the stacked structure to form multiple first trenches arranged longitudinally at intervals, the first trenches being surrounded by longitudinally adjacent dielectric layers; using the passivation layer as a stop layer, removing the exposed portion of the first protective layer along each first trench to form a second trench, the second trench being connected to the first trench to form a third trench, the remaining first protective layer forming the second protective layer; forming a dielectric layer covering each side and bottom of the third trench; forming a conductive plate structure filling the third trench, the conductive plate structure covering the dielectric layer.

[0011] In the semiconductor structure formation method provided by the embodiments of the present invention, a protective material layer covering the top, via sidewalls and bottom surface of the stacked structure is formed, and an anisotropic etching process is performed. The anisotropic etching process performs surface passivation treatment on the protective material layer to form a passivation material layer. The anisotropic etching process also removes the passivation material layer located on the bottom surface of the protective material layer, while retaining the passivation material layer located on the sidewall of the protective material layer as a passivation layer. Thus, the passivation layer can be used as a stop layer. The exposed portion of the first protective layer is removed along each first trench without the need for an additional process to form a stop layer, which helps to simplify the process and reduce costs.

[0012] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings.

[0013] Please refer to the reference. Figure 1 A substrate 100 is provided, on which a laminated structure 120 is formed, the laminated structure 120 including longitudinal (e.g., Figure 9 The dielectric layer 121 and the sacrificial layer 122 are stacked alternately from bottom to top in the Z direction (perpendicular or approximately perpendicular to the substrate 100). Exemplarily, the dielectric layer 121 closest to the substrate 100 is such that the substrate 100 is spaced apart from the sacrificial layer 122.

[0014] The substrate 100 provides the process basis for the formation process of the semiconductor structure of the present invention.

[0015] In this embodiment, the substrate 100 is a semiconductor substrate or an insulating substrate. Exemplarily, the substrate 100 may include other semiconductor devices or conductive components, and the surface of the substrate 100 in contact with the stacked structure 120 is an insulating surface. For example, the substrate 100 includes a semiconductor substrate and an insulating film layer located between the semiconductor substrate and the stacked structure 120. The material of the insulating film layer includes, for example, silicon oxide or silicon nitride. As an example, the material of the insulating film layer in the substrate 100 in contact with the stacked structure 120 is silicon oxide.

[0016] The stacked structure 120 is used to provide a foundation for the subsequent formation of conductive pillar structures and conductive plate structures therein.

[0017] It should be noted that in this embodiment, the bottom layer and the top layer of the stacked structure 120 are both dielectric layers 121.

[0018] Specifically, the sacrificial layer 122 is used to occupy space for the subsequent formation of the conductive plate structure.

[0019] In this embodiment, the material of the sacrificial layer 122 includes silicon nitride.

[0020] The thickness of the sacrificial layer 122 can be set by those skilled in the art according to actual needs. Specifically, the thickness of the sacrificial layer 122 is sufficient to provide enough space for the subsequent formation of the conductive plate structure, and ensures that the longitudinal dimension of the formed semiconductor structure is not too large. The conductivity of the conductive plate structure meets the process requirements. When the semiconductor structure is used in a memory, the area of ​​the capacitor serving as the memory cell meets the design requirements, thereby improving the integration of the formed semiconductor structure and meeting the application requirements of the semiconductor structure. The structure of the capacitor will be described later.

[0021] The dielectric layer 121 is used to achieve electrical isolation between adjacent conductive plate structures in the longitudinal direction.

[0022] In this embodiment, the material of the dielectric layer 121 includes silicon oxide.

[0023] The sacrificial layer 122 is made of silicon nitride, and the dielectric layer 121 is made of silicon oxide. By making the two materials different, there is an etching selectivity between the sacrificial layer 122 and the dielectric layer 121 during the subsequent wet etching process to remove the sacrificial layer 122. This results in less or almost no damage to the dielectric layer 121 by the etching solution, which is beneficial to improving the performance of the formed semiconductor structure. However, it is not limited to this; it is sufficient that the sacrificial layer 122 and the dielectric layer 121 are made of different materials and have etching selectivity.

[0024] The thickness of the dielectric layer 121 is configured to ensure that the electrical isolation effect of the dielectric layer 121 meets the requirements, and to ensure that the space occupied by the semiconductor structure is not too large, thereby helping to improve the integration of the formed semiconductor structure.

[0025] In this embodiment, during the step of providing the substrate 100, a conductive structure 110 is formed in the substrate 100, and the conductive structure 110 is exposed on the top surface of the substrate 100.

[0026] The conductive structure 110 is used to make an electrical connection with the subsequently formed conductive pillar structure.

[0027] For example, the conductive structure 110 may include conductive contacts, pads, or conductive lines, etc., and this application does not make any specific limitations.

[0028] For example, the conductive structure 110 does not contact the sacrificial layer 122, and the dielectric layer 121 is located between the sacrificial layer 122 and the conductive structure 110.

[0029] Please refer to the reference. Figure 2 This forms a through-hole 125 that penetrates the stacked structure 120.

[0030] The through hole 125 is used to provide space for the subsequent formation of the conductive pillar structure.

[0031] In this embodiment, a dry etching process is used to form a through-hole 125 that penetrates the stacked structure 120.

[0032] For example, in the step of forming the through hole 125 through the stacked structure 120, the through hole 125 is formed with a shape that is wider at the top and narrower at the bottom, that is, the sidewall has an inclined angle. For example, at the opening position of the through hole 125, the angle between the sidewall of the through hole 125 and the horizontal direction is 80° to 90°.

[0033] In this embodiment, during the step of forming the through-hole 125 through the stacked structure 120 using a dry etching process, the through-hole 125 exposes the conductive structure 110, allowing the second protective layer subsequently formed in the through-hole 125 to contact the conductive structure 110. This enables the subsequently formed conductive pillar structure to achieve electrical connection with the conductive structure 110 through the second protective layer. The second protective layer is prepared from a protective material layer, which includes a conductive material and is conductive. The second protective layer also includes a conductive material and is conductive.

[0034] Through hole 125 is used to form a conductive post structure, and the opening size of through hole 125 can be set according to requirements.

[0035] Please refer to the reference. Figure 3 A protective material layer 130' is formed covering the top of the laminated structure 120, the sidewalls of the through-hole 125, and the bottom surface. The material of the protective material layer 130' includes a conductive material.

[0036] The protective material layer 130' is used for the subsequent formation of the first protective layer, and the first protective layer is used for the subsequent formation of the second protective layer.

[0037] Please refer to the reference. Figure 4 An anisotropic etching process is performed to passivate the protective material layer 130' on the sidewall and bottom surface of the via 125, forming a passivation material layer (not shown). The anisotropic etching process also removes the passivation material layer on the bottom surface of the protective material layer 130' located on the bottom surface of the via 125, while retaining the passivation material layer on the surface of the protective material layer 130' located on the sidewall of the via 125. The passivation material layer includes the passivation layer 135.

[0038] Exemplarily, the passivation material layer also includes a portion located above the stacked structure 120 (i.e. Figure 4 The portion extending from the passivation material layer 135 above the dashed line), but this portion is removed in subsequent steps (i.e., the passivation layer 135 does not include this portion). Figure 4 (The portion above the dashed line). However, it is not limited to this. In some embodiments not shown, the passivation layer 135 does not completely cover the protective material layer 130' on the sidewall of the through hole 125. The passivation layer 135 can cover the portion of the protective material layer 130' in the stacked structure 120 corresponding to the sacrificial layer 122.

[0039] It should be noted that passivation here refers to a change in the material of the film layer, without specifying whether or not the conductivity of the film layer is changed, or in what way.

[0040] Anisotropic etching involves high-energy particles that can react with the material on the surface of the protective material layer 130', thereby passivating the surface of the protective material layer 130' and forming passivation material layers on the bottom and sidewalls of the protective material layer 130'. Simultaneously, the anisotropic etching process possesses anisotropic etching characteristics; by controlling its bias power, it is possible to remove the passivation material layer on the bottom surface of the protective material layer 130' along the longitudinal direction, while retaining the passivation material layer on the sidewalls of the protective material layer 130'.

[0041] Specifically, etching removes the passivation material layer located on the bottom surface of the protective material layer 130' to avoid the passivation material layer affecting the electrical connection performance between the subsequently formed conductive pillar structure and the conductive structure; the passivation material layer located on the sidewall of the protective material layer 130' is retained to form a passivation layer on the sidewall of the protective material layer 130', which serves as a stop layer in the subsequent removal of part of the first protective layer.

[0042] The passivation material layer on the surface of the protective material layer 130' located on the sidewall of the via 125 is retained to effectively protect the conductive pillar structure when the first protective layer is subsequently removed and the second protective layer is formed, thereby helping to improve the performance of the formed semiconductor structure. The passivation material layer on the surface of the protective material layer 130' located at the bottom of the via 125 is etched away to avoid affecting the electrical connection performance between the subsequently formed conductive pillar structure and the conductive structure 110. Thus, the subsequent passivation layer can be formed and the bottom of the passivation material layer can be removed in one step, facilitating the subsequent electrical connection between the conductive pillar structure and the underlying structure.

[0043] Accordingly, the thickness of the passivation layer 135 on the surface of the protective material layer 130' located on the sidewall of the via 125 can be configured by controlling the process parameters of the anisotropic etching process to meet the etching protection requirements when removing part of the first protective layer. In this embodiment, the thickness of the passivation layer 135 on the surface of the protective material layer 130' located on the sidewall of the via 125 is 1~3nm, which can meet the etching protection requirements when removing part of the first protective layer.

[0044] In this embodiment, in the step of forming a protective material layer 130' covering the top of the stacked structure 120, the sidewalls of the through-hole 125, and the bottom surface, the process for preparing the protective material layer 130' ensures that the step coverage of the protective material layer 130' satisfies the requirement that the inner diameter of the protective material layer 130' is uniform in the longitudinal direction after its formation. That is, the inner sidewall of the protective material layer 130' is perpendicular or approximately perpendicular to the substrate 100. For example, the angle between the inner wall surface of the protective material layer 130' and the substrate is 90-91°. The passivation material layer is formed by passivating the surface portion of the protective material layer 130'. That is, the passivation material layer is conformal to the surface of the protective material layer 130'. Thus, it is possible to achieve that the perimeter of the multiple third trenches subsequently formed corresponding to the same conductive pillar structure is consistent around the conductive pillar structure and the passivation layer, and is not affected by the top-wide and bottom-narrow morphology of the through-hole 125. Therefore, the thickness of the sacrificial layer 122 can be easily controlled, thereby controlling the area of ​​the capacitor formed subsequently, without having to consider the morphology of the via 125. This helps to reduce the process difficulty of semiconductor structure manufacturing and improve the performance of the formed semiconductor structure. Specifically, a deposition process with a corresponding step coverage can be selected to form the protective material layer 130' based on the difference between the top and bottom opening dimensions of the through-hole 125. That is, the parameters of the fabrication process for the protective material layer 130' can be adjusted based on the etching result of the through-hole 125, i.e., the sidewall tilt angle of the through-hole 125, thereby adjusting the step coverage of the protective material layer 130' to meet the inner sidewall tilt angle requirements. This improves process flexibility and reduces the difficulty of the through-hole etching and deposition processes. For example, the deposition process may include chemical vapor deposition (CVD).

[0045] In this embodiment, the material of the protective material layer 130' includes tantalum nitride (TaN). Tantalum nitride is conductive, ensuring contact between the conductive pillar structure and the conductive structure 110.

[0046] Furthermore, the material of the protective layer 130' includes amorphous tantalum nitride. Accordingly, the preparation process of amorphous tantalum nitride is simple and the step coverage is easy to adjust, and it also has good protective capabilities for conductive pillar structures.

[0047] Correspondingly, after a passivation layer is formed on the surface of the protective material layer 130' on the sidewall of the through hole 125, and the protective material layer 130' eventually forms a second protective layer, the structure formed by the second protective layer and the passivation layer on its surface together with the subsequently formed conductive pillar structure has good conductivity. Removing the passivation material layer formed by the surface passivation of the protective material layer 130' on the bottom surface of the through hole 125 also helps to reduce the connection resistance between the subsequently formed conductive pillar structure and the conductive structure 110.

[0048] In other embodiments, the protective material layer can also be made of doped or undoped polysilicon prepared using a low-pressure chemical vapor deposition (LPCVD) process. The doped or undoped polysilicon is conductive. In other words, the protective material layer is formed using an LPCVD process. The LPCVD process ensures that the inner diameter of the protective material layer 130' is uniform in the longitudinal direction after its formation, simplifying the process. Furthermore, the doped or undoped polysilicon undergoes a passivation process to form a passivation layer, such as a silicon oxide layer. Since the passivation layer at the bottom of the via 125 has been removed, the conductive connection between the conductive pillar structure and the conductive structure 110 is not affected.

[0049] It should be noted that in this application, the material of the protective material layer includes conductive material, which means that the material of the protective material layer includes conductive material, and conductive material can be conductive material or semiconductor material.

[0050] Please refer to the reference. Figure 4 An anisotropic etching process is performed to passivate the protective material layer 130' on the sidewalls and bottom surface of the via 125, forming a passivation material layer. The anisotropic etching process also removes the passivation material layer on the bottom surface of the protective material layer 130' of the via 125, while retaining the passivation material layer on the surface of the protective material layer 130' on the sidewalls of the via 125. This passivation material layer forms a passivation layer, which serves as a stop layer for subsequent partial removal of the first protective layer and formation of the second protective layer.

[0051] In some embodiments, the anisotropic etching process includes a plasma-assisted etching process. For example, a reactive gas is introduced into a reaction chamber and ionized to form plasma. The plasma acts on the surface of the protective material layer 130', causing a passivation reaction on a portion of the surface of the protective material layer 130', thereby generating a passivation material layer. Simultaneously, based on the characteristics of anisotropic etching, the passivation material layer on the surface of the protective material layer 130' located on the bottom surface of the via 125 is etched away, while the passivation material layer on the surface of the protective material layer 130' located on the sidewall of the via 125 is retained.

[0052] In some embodiments, anisotropic etching processes, such as plasma-assisted etching, can also remove a portion of the thickness of the passivation material layer on the sidewalls of the via 125. However, due to the anisotropic etching characteristics, the thickness of the passivation material layer removed from the portion on the sidewalls of the via 125 is negligible compared to the thickness removed from the portion at the bottom of the via 125. Specifically, the anisotropic etching process is a vapor-phase process, which has good consistency, i.e., the passivation material layer is generated at a consistent rate throughout. However, the anisotropic etching process can make its etching characteristics directional by adjusting the bias power, resulting in different removal rates from the sidewalls and bottom of the via 125. Therefore, in this embodiment, the passivation material layer on the surface of the protective material layer 130' on the sidewalls of the via 125 is retained, while the passivation material layer on the surface of the protective material layer 130' at the bottom of the via 125 is removed.

[0053] In this embodiment, the steps of the anisotropic etching process include: depositing a protective layer 140, the protective layer 140 including a portion located at the top of the stacked structure 120; performing a plasma-assisted etching process to perform surface passivation treatment, passivate the surface of the protective material layer 130', and remove the passivation material layer on the surface of the protective material layer 130' located at the bottom surface of the via 125.

[0054] In this embodiment, the protective layer 140 is used to protect the protective material layer 130' on top of the stacked structure 120 in the subsequent plasma-assisted etching process, so as to avoid damage to the protective material layer 130' on top of the stacked structure 120, thereby avoiding damage to the stacked structure 120 caused by the plasma-assisted etching process.

[0055] In this embodiment, the material of the protective layer 140 includes a polymer. Accordingly, the protective layer 140 is prepared by a plasma-assisted deposition process. The plasma-assisted deposition process employs a deposition process with poor step coverage, such as chemical vapor deposition (CVD), to avoid the protective layer 140 covering the bottom surface of the via 125 and to cover less of the sidewalls of the via 125.

[0056] Accordingly, in this embodiment, the process gas for plasma-assisted deposition includes a carbon-containing gas, which includes one or more selected from carbon hexafluoride, carbon difluoride, methane, and fluoromethane.

[0057] In other embodiments, the protective layer includes a portion extending to a certain depth of the through-hole to cover the sidewalls of the protective material layer, thereby protecting the sidewalls of the protective material layer from damage.

[0058] In this embodiment, depending on the thickness of the passivation layer to be formed subsequently, the anisotropic etching process may include repeatedly performing the deposition of a protective layer and the plasma-assisted etching process once or multiple times. That is, the deposition-etching combination steps can be performed cyclically, so that the passivation material layer on the surface of the protective material layer 130' on the bottom of the via 125 is etched, and the morphology of the top portion of the protective material layer 130' on the sidewall of the via 125 is not destroyed by the etching steps.

[0059] The process parameters of the plasma-assisted etching process can be set according to the need to perform surface passivation treatment on the protective material layer 130', remove the passivation material layer located on the bottom surface of the protective material layer 130', and retain the passivation material layer located on the sidewall of the protective material layer 130'.

[0060] Accordingly, the process parameters of the plasma-assisted deposition process are set according to the etching degree of the plasma-assisted etching process and the protection requirements of the protective material layer 130'.

[0061] In this embodiment, the material of the protective material layer 130' is TaN. Accordingly, the process gas of the plasma-assisted etching process includes fluorine-containing and / or chlorine-containing process gases to perform surface passivation treatment on the protective material layer 130'.

[0062] For example, the fluorine-based gas is selected from one or more of fluorocarbon gas, sulfur hexafluoride gas, and nitrogen trifluoride gas. Accordingly, the material of the passivation layer includes one or both of tantalum fluoride (TaF) and tantalum fluoride nitride (TaFN).

[0063] For example, the chlorine-based gas is selected from one or more of chlorine gas and boron chloride gas. Accordingly, the material of the passivation layer includes one or both of tantalum chloride (TaCl) and tantalum nitride (TaClN).

[0064] It should be noted that during the plasma-assisted etching process, a bias power is applied to the surface of the substrate 100 to drive high-energy plasma toward the substrate 100, giving the plasma a high velocity and energy, thereby etching the passivation material layer on the surface of the protective material layer 130' at the bottom of the via 125. Therefore, the bias power of the plasma-assisted etching process should not be too high. If the bias power is too high, resulting in excessively high plasma velocity and energy, it can easily cause plasma damage and may also etch away the protective material layer 130' at the bottom of the via 125, potentially damaging the substrate 100 and hindering subsequent processes. In some embodiments, it may also impede the electrical connection between the conductive pillar structure and the conductive structure 110. Furthermore, the bias power of the plasma-assisted etching process should not be too low. If the bias power is too low, resulting in a low plasma velocity and energy, the passivation material layer on the protective material layer 130' at the bottom of the via 125 will not be completely etched, which is detrimental to subsequent processes. In some embodiments, it is also detrimental to the electrical connection between the conductive pillar structure 145 and the conductive structure 110. Therefore, in this embodiment, the bias power of the plasma-assisted etching process is 400W to 800W.

[0065] In other embodiments, the material of the protective layer can also be doped or undoped polycrystalline silicon prepared using a low-pressure chemical vapor deposition (LPCVD) process. Accordingly, the process gas for the plasma-assisted etching process includes an oxygen-containing process gas to passivate the surface of the protective layer.

[0066] For example, the oxygen-containing process gas includes one or more selected from oxygen and ozone. Accordingly, the material of the passivation layer includes silicon oxide.

[0067] In other embodiments, the passivation material layer comprises one or more selected from tantalum chloride, tantalum oxychloride, tantalum fluoride, tantalum fluoride oxychloride, and silicon oxide. These materials are commonly used in the art, have simple preparation processes, and can exhibit etching selectivity with other commonly used materials, thus they can be used as passivation material layers and further formed in subsequent steps. Exemplarily, the protective material layer comprises tantalum nitride, and the passivation material layer comprises one or more selected from tantalum chloride, tantalum oxychloride, tantalum fluoride, and tantalum fluoride oxychloride; exemplarily, the protective material layer comprises doped or undoped polycrystalline silicon, and the passivation material layer comprises silicon oxide; exemplarily, the protective material layer comprises doped or undoped polycrystalline silicon and tantalum nitride, and the passivation material layer comprises one or more selected from tantalum chloride, tantalum oxychloride, tantalum fluoride, and tantalum fluoride oxychloride, and silicon oxide.

[0068] Please refer to the reference. Figures 5 to 6 A conductive pillar structure 145 is formed to fill the through hole 125, and the conductive pillar structure 145 covers the passivation material layer on the surface of the protective material layer 130' on the sidewall of the through hole 125.

[0069] The conductive pillar structure 145 is used as a conductive pillar in a 3D memory.

[0070] In this embodiment, in the step of forming a conductive pillar structure 145 that fills the through hole 125 and covers the surface of the protective material layer 130' on the sidewall of the through hole 125, the conductive pillar structure 145 contacts the protective material layer 130' located on the bottom surface of the through hole 125 to be electrically connected, thereby realizing the electrical connection between the conductive pillar structure 145 and the conductive structure 110 through the protective material layer 130'.

[0071] This application does not impose specific limitations on the materials and manufacturing processes of the conductive pillar structure; these can be set according to actual needs.

[0072] Please refer to the reference. Figures 5 to 6 The protective material layer 130' above the stacked structure 120 is removed, and the protective material layer 130' on the sidewall of the through hole 125 is retained as the first protective layer 130. The remaining passivation material layer is used as the passivation layer 135, which is located on the sidewall of the first protective layer 130. Correspondingly, the protective layer 140 above the stacked structure 120 is also removed.

[0073] The first protective layer 130 is used to protect the sidewalls of the conductive pillar structure 145 during the subsequent removal of the sacrificial layer 122. Moreover, in order to completely remove the sacrificial layer 122, it is usually necessary to increase the etching time, so the first protective layer 130 can play a better protective role for the conductive pillar structure during this etching process.

[0074] In this embodiment, the conductive pillar structure 145 and the first protective layer 130 are formed in the same process step.

[0075] Specifically, the steps of forming the conductive pillar structure 145 and the first protective layer 130 include: combining with a reference Figure 5 A conductive pillar material layer 145' is formed on the protective material layer 130', and the conductive pillar material layer 145' also fills the through-hole 125; in conjunction with the reference Figure 6 Remove the conductive pillar material layer 145' and protective material layer 130' above the top of the stacked structure 120, and the remaining protective material layer 130' and conductive pillar material layer 145' form the first protective layer 130 and the conductive pillar structure 145, respectively.

[0076] In this embodiment, a chemical mechanical polishing (CMP) process is used to remove the conductive pillar material layer 145' and the protective material layer 130' that extend above the top of the stacked structure 120. The CMP process not only effectively removes the conductive pillar material layer 145' and the protective material layer 130' that extend above the top of the stacked structure 120, but also, by precisely controlling the material removal rate (MRR), ensures that the top of the stacked structure 120 after removing these layers achieves a certain surface morphology.

[0077] In this embodiment, during the step of removing the conductive pillar material layer 145' and the protective material layer 130' above the top of the stacked structure 120, a protective layer 140 is also formed between the protective material layer 130' and the conductive pillar material layer 145' at the top of the stacked structure 120. Correspondingly, during the step of removing the conductive pillar material layer 145' and the protective material layer 130' above the top of the stacked structure 120, the protective layer 140 located between the protective material layer 130' and the conductive pillar material layer 145' at the top of the stacked structure 120 is also removed. If a passivation material layer is partially formed above the stacked structure 120, the passivation material layer above the stacked structure 120 is also removed.

[0078] It should be noted that if there are other film layers on the protective material layer 130' at the top of the stacked structure 120, these other film layers are also removed during the step of removing the conductive pillar material layer 145' and the protective material layer 130' above the top of the stacked structure 120.

[0079] The passivation layer 135 is used as a stop layer when a portion of the first protective layer 130 is subsequently removed.

[0080] Please refer to the reference. Figure 7 The sacrificial layer 122 in the stacked structure 120 is removed to form a plurality of first trenches 123 arranged longitudinally at intervals. The first trenches 123 are surrounded by longitudinally adjacent dielectric layers 121.

[0081] The first groove 123 is used to provide space for the subsequent formation of the conductive plate structure.

[0082] In this embodiment, a wet etching process is used to remove all sacrificial layers 122 in the stacked structure 120. It should be understood that the wet etching process is used to remove the sacrificial layers 122, and before the wet etching process, at least one opening (not shown) penetrating the stacked structure 120 is formed, with the sidewalls of the opening exposing the sacrificial layers 122, allowing the etching solution to etch and remove the sacrificial layers 122 through this opening.

[0083] Wet etching has isotropic etching characteristics, which is beneficial for completely removing all sacrificial layers 122 in the stacked structure 120. Furthermore, wet etching easily achieves a large etching selectivity, thereby reducing damage to other film layers when removing the sacrificial layer 122. However, it is not limited to this; other etching processes with etching selectivity relative to the dielectric layer 121 and the first protective layer 130 can be used to remove the sacrificial layer 122.

[0084] In this embodiment, the sacrificial layer 122 is made of silicon nitride (SiN). Accordingly, the etching solution used to remove all sacrificial layers 122 in the stacked structure 120 includes a hot phosphoric acid solution. The process parameters of the hot phosphoric acid solution can be set according to the requirements of etching rate of sacrificial layer 122, process stability and controllability, and avoiding etching loss of other film layers, and are not limited here.

[0085] Please refer to the reference. Figure 8 Using the passivation layer 135 as a stop layer, the exposed portion of the first protective layer 130 is removed along each first trench 123 to form a second trench 124. The second trench 124 is connected to the first trench 123 to form a third trench 126, and the remaining first protective layer 130 is formed as a second protective layer 170.

[0086] A passivation layer 135 is used as a stop layer for removing the exposed portion of the first protective layer 130 along each first trench 123. Correspondingly, the passivation layer 135 exists as an etching stop layer between the conductive pillar structure 145 and the first protective layer 130, avoiding damage to the conductive pillar structure 145 when removing part of the first protective layer 130, which is beneficial to improving the performance of the formed semiconductor structure.

[0087] In this embodiment, using the passivation layer 135 as a stop layer, a wet etching process is employed to remove the exposed portion of the first protective layer 130 along each first trench 123, forming a second trench 124 exposing the portion of the passivation layer 135. However, this is not a limitation; other etching processes with etching selectivity relative to the dielectric layer 121 and the passivation layer 135 can be used to remove the exposed portion of the first protective layer 130.

[0088] The passivation layer 135 is obtained by performing surface passivation treatment on the protective material layer 130'. Since the two materials are different, a large etching selectivity ratio between the passivation layer 135 and the first protective layer 130 can be achieved by controlling the etching process. Correspondingly, removing the exposed portion of the first protective layer 130 along each first trench 123 can stop the passivation layer 135 on the sidewall of the first protective layer 130. Even if the passivation layer 135 is partially damaged during the removal of the exposed portion of the first protective layer 130, the conductive pillar structure 145 is protected from damage, and the passivation layer 135 between the conductive pillar structure 145 and the conductive structure 110 is partially retained, thus the electrical performance of the semiconductor structure is unaffected.

[0089] The wet etching process can easily achieve a large etching selectivity, thereby reducing damage to other film layers when removing part of the first protective layer 130.

[0090] In this embodiment, the material of the first protective layer 130 includes tantalum nitride, and the passivation layer 135 includes one or more of tantalum chloride, tantalum oxychloride, tantalum fluoride, and tantalum oxyfluoride. Accordingly, the etching solution for the wet etching process uses Standard Clean 1 (SC1). SC1 solution is a mixed solution including ammonia, hydrogen peroxide, and water.

[0091] In other embodiments, the material of the first protective layer is tantalum nitride, and the passivation layer includes one or more of tantalum chloride, tantalum oxychloride, tantalum fluoride, and tantalum oxyfluoride. Accordingly, in the step of removing the exposed portion of the first protective layer along each first trench with the passivation layer as the stop layer, a portion of the first protective layer can also be removed by etching with a hot phosphoric acid solution. Accordingly, by increasing the etching time of the wet etching process used in the step of removing the sacrificial layer in the stacked structure, the operation of removing the sacrificial layer in the stacked structure and removing the exposed portion of the first protective layer along the first trench and stopping at the passivation layer can be achieved in the same process step, which helps to simplify the process.

[0092] Please refer to the reference. Figure 9 A dielectric layer 150 is formed covering each side and bottom surface of the third trench 126; a conductive plate structure 160 is formed filling the third trench 126, and the conductive plate structure 160 covers the dielectric layer 150. It can be understood that the side surface of the third trench 126 refers to the surface of the third trench 126 opposite each other in the vertical direction, and the bottom surface of the third trench 126 refers to the surface of the third trench 126 near the conductive post structure 145.

[0093] Dielectric layer 150 is used as a storage capacitor material in the memory.

[0094] In this embodiment, the dielectric layer 150 includes a ferroelectric material layer. The ferroelectric material layer has spontaneous polarization characteristics and can form two different stable residual polarization states under the action of an external electric field. By utilizing the above-mentioned polarization characteristics of the ferroelectric material layer to store data "0" or "1", it is possible to achieve benefits such as high-speed read and write, high durability and low power consumption, and is suitable for various application scenarios with high-performance storage requirements.

[0095] However, it is not limited to this. The dielectric layer 150 may include other dielectric material layers for storage, such as phase change material layers or magnetic tunnel junction storage material layers, so that the semiconductor structure can be used to form the corresponding type of memory. This application does not make specific limitations.

[0096] In this embodiment, after the passivation layer 135 is formed, the angle between the substrate 100 and the passivation layer 135 is 90°~91°. Correspondingly, after the dielectric layer 150 covering each side and bottom surface of the third trench 126 is formed, the portion of the dielectric layer 150 in contact with the passivation layer 135 is used to form the capacitor dielectric layer of the capacitor. As mentioned above, this reduces the difficulty of controlling the capacitor area.

[0097] The dielectric layer 150, including a ferroelectric material layer, serves as a storage medium layer in the portion of the dielectric layer 150 located between the opposing surfaces of the electrode plate structure and the conductive pillar structure 145. It can be polarized according to the direction and magnitude of an external electric field, and retains partial polarization (residual polarization) even after the external electric field is removed. This residual polarization creates a potential difference, causing the capacitor electrodes on both sides of the dielectric layer 150—that is, the surfaces of the dielectric layer 150 closest to the conductive pillar structure 145 and the conductive plate structure 160, respectively—to induce charges of opposite polarities. Different polarization directions induce different charges, thereby enabling the storage of logic "0" and logic "1". In other words, a semiconductor structure can be used for ferroelectric memory.

[0098] When the dielectric layer 150 includes a ferroelectric material layer, enabling the semiconductor structure to be used in a ferroelectric memory, the area of ​​the capacitor depends on the relative areas of the conductive plate structure 160 and the conductive pillar structure 145. The area of ​​the capacitor is related to the reading of the memory cell in the ferroelectric memory, and a controllable capacitor area helps reduce the read / write control difficulty of the ferroelectric memory. By controlling the angle between the substrate 100 and the passivation layer 135 to 90°~91°, the horizontal perimeter of the bottom surface of the third trench corresponding to the same conductive pillar structure 145 is made consistent. Furthermore, the step coverage of the protective material layer deposition can be adjusted according to the via etching results to improve the stability of the consistent horizontal perimeter of the bottom surface of the third trench 126 corresponding to the same conductive pillar structure 145. Thus, by controlling the uniformity of the thickness of the sacrificial layer 122, it is possible to achieve uniform area among multiple capacitors corresponding to the same conductive pillar structure. Capacitors with consistent areas can induce an equal amount of charge during data reading, thereby improving the accuracy of data reading and improving the performance of the formed semiconductor structure while reducing the difficulty of the process. However, this is not the only one. In some embodiments, the thickness of the sacrificial layer 122 can be controlled to vary according to actual needs, thereby achieving a consistent ratio between the area of ​​multiple capacitors corresponding to the same conductive pillar structure and the thickness of the corresponding sacrificial layer 122, which is beneficial for achieving differentiated control between different capacitors.

[0099] The conductive plate structure 160 is used as a conductive plate in a 3D memory.

[0100] In this embodiment, the surfaces of the conductive plate structure 160 and the conductive pillar structure 145 facing each other are the upper electrode and the lower electrode, respectively. The conductive plate structure 160 includes an upper electrode covering the dielectric layer 150 and an upper conductor filling the third trench 126 and covering the upper electrode. The conductive pillar structure 145 includes a lower conductor and a plurality of lower electrodes. The capacitor includes an upper electrode, a lower electrode and a dielectric layer 150 located between the upper electrode and the lower electrode.

[0101] This invention also provides a semiconductor structure formed using the semiconductor structure formation method described in any of the foregoing embodiments.

[0102] Accordingly, embodiments of the present invention also provide a semiconductor structure.

[0103] Figure 10 A schematic diagram of a semiconductor structure provided by the technical solution of the present invention is shown. (Referring to the reference...) Figure 10 A semiconductor structure includes: a substrate 100; and a stacked layer 120' located on the substrate 100, the stacked layer 120' comprising elements along a longitudinal direction (e.g., ...). Figure 9 The dielectric layer 121 and conductive plate structure 160 are alternately stacked from bottom to top in the Z direction (in the Z direction); a plurality of conductive pillar structures 145 penetrate the stacked layers 120'; a passivation layer 135 is continuously disposed along the sidewall of the conductive pillar structure 145; a second protective layer 170 is disposed along the entire surface of the conductive pillar structure 145 without facing away from the substrate 100, the second protective layer 170 is truncated by the conductive plate structure 160 to form a discontinuous layer, and the second protective layer 170 contacts the surface of the passivation layer 135 facing away from the conductive pillar structure 145; a dielectric layer 150 is formed on the surface of the conductive plate structure 160 opposite to the second protective layer 170, the passivation layer 135 and the dielectric layer 121; wherein, the passivation layer 135 and the second protective layer 170 have at least one identical element.

[0104] The substrate 100 provides the process basis for the formation process of the semiconductor structure of the present invention.

[0105] In this embodiment, the substrate 100 is a semiconductor substrate or an insulating substrate. The substrate 100 is the same as described above and will not be repeated here.

[0106] The stacked layers 120' are used to form a longitudinally spaced multiple conductive plate structure 160.

[0107] The conductive plate structure 160 is used as a conductive plate in a 3D memory.

[0108] In this embodiment, the conductive plate structure 160 includes an upper electrode covering the dielectric layer 150 and an upper conductive line filling the spaces between longitudinally adjacent dielectric layers 121 and covering the upper electrode. The upper electrode and upper conductive line are the same as described above and will not be repeated here.

[0109] The dielectric layer 121 is used to achieve electrical isolation between adjacent conductive plate structures 160 in the longitudinal direction.

[0110] In this embodiment, the material of the dielectric layer 121 includes silicon oxide.

[0111] In this embodiment, the thickness of the dielectric layer 121 can be specifically set according to actual needs to ensure that the dielectric layer 121 has a good electrical isolation effect and that the space occupied by the semiconductor structure is not too large, which helps to improve the integration of the formed semiconductor structure.

[0112] In this embodiment, a conductive structure 110 is formed in the substrate 100, and the conductive structure 110 is exposed on the top surface of the substrate 100.

[0113] The conductive structure 110 is used for electrical connection with the conductive post structure 160.

[0114] The conductive pillar structure 145 is used as a conductive pillar in a 3D memory.

[0115] In this embodiment, the conductive pillar structure 145 includes a lower conductor and a plurality of lower electrodes, wherein the lower conductor and lower electrodes are the same as described above and will not be repeated here.

[0116] The passivation layer 135 is used as a stop layer in the semiconductor manufacturing process to remove part of the first protective layer 130 and prepare the second protective layer 170.

[0117] A passivation layer 135 is used as a stop layer in the semiconductor manufacturing process to remove a portion of the first protective layer 130, thus preventing damage to the conductive pillar structure 145 during the removal of the first protective layer 130 and improving the performance of the formed semiconductor structure. The first protective layer 130 serves as an etching protection layer during the removal of the sacrificial layer to fabricate the conductive plate structure 160, protecting the conductive pillar structure 145.

[0118] The passivation layer 135 is formed by passivating the surface of the protective material layer. The shape of the passivation layer 135 can be controlled by controlling the shape of the protective material layer facing the conductive pillar structure 145. As mentioned above, the first protective layer 130 is formed by depositing the protective material layer on the sidewall and bottom of the via. The via usually has a structure that is wider at the top and narrower at the bottom, while the deposited protective material layer has a structure that is thicker at the top and thinner at the bottom. Moreover, the coverage of the deposited step is easy to adjust. As a result, it is easy to make the inner diameter of the protective material layer uniform, thereby making the horizontal dimension of the passivation layer 135 consistent in the vertical direction. When the semiconductor structure is used to form a memory, the difficulty of controlling the area of ​​the capacitor is reduced.

[0119] In this embodiment, the passivation layer 135 is formed by passivating the surface of the protective material layer, and the remaining part of the protective material layer after the etching process forms the second protective layer 170. Therefore, the passivation layer 135 and the second protective layer 170 have at least one of the same elements.

[0120] Accordingly, in semiconductor manufacturing processes, the thickness of the passivation layer 135 on the surface of the protective material layer 130' located on the sidewall of the via can be configured to avoid over-etching during subsequent removal of the first protective layer. In this embodiment, the thickness of the passivation layer 135 is 1 nm to 3 nm.

[0121] In the semiconductor manufacturing process, during the step of forming a protective material layer covering the top, sidewalls, and bottom of the stacked structure, the step coverage of the protective material layer satisfies a condition that ensures the inner diameter of the protective material layer is uniform in the longitudinal direction after its formation. Correspondingly, after forming the passivation layer 135, the angle between the passivation layer 135 and the substrate 100 is 90° to 91°. Here, the angle between the passivation layer and the substrate 100 refers to the angle between the passivation layer 135 and the surface of the substrate 100 facing the stacked layers.

[0122] In semiconductor manufacturing, a stacked structure of alternating dielectric layer 121 and sacrificial layer is first formed, and then a via is formed through the stacked structure. A protective material layer for forming a first protective layer is deposited on the top of the stacked structure and on the sidewalls and bottom of the via. The step coverage of the protective material layer satisfies the requirement that the inner diameter of the first protective layer formed on the sidewall of the via is uniform in the longitudinal direction. For example, the angle between the passivation layer 135 and the substrate 100 is 90°~91°. Thus, the relative area of ​​the electrode plate structure 160 and the conductive pillar structure 145 can be controlled by controlling the thickness of the sacrificial layer 122, without being affected by the inclination of the sidewall of the via. This reduces the difficulty of controlling the etching process and the difficulty of controlling the capacitor area. The via is formed by an etching process and has a shape that is wider at the top and narrower at the bottom. The step coverage of the protective material layer is sufficient to ensure that the inner diameter of the first protective layer formed on the sidewall of the via is uniform in the longitudinal direction. Therefore, the thickness of the protective material layer on the sidewall of the via gradually increases in the direction away from the substrate. The thickness of the second protective material layer formed subsequently on the part of the passivation layer away from the conductive pillar structure gradually increases in the direction from the substrate to the stacked layer.

[0123] In this embodiment, the material of the second protective layer 170 is TaN. Correspondingly, the material of the passivation layer 135 includes one or two of tantalum chloride (TaCl), tantalum oxychloride (TaClN), tantalum fluoride (TaF), and tantalum fluoride nitride (TaFN).

[0124] In other embodiments, the material of the second protective layer includes polycrystalline silicon. Exemplarily, the polycrystalline silicon may be doped or undoped polycrystalline silicon. Accordingly, the material of the passivation layer includes silicon oxide.

[0125] The second protective layer 170 is used to provide better protection for the conductive pillar structure 145 during semiconductor manufacturing.

[0126] In this embodiment, a second protective layer 170 is also formed between the conductive pillar structure 145 and the conductive structure 110, thereby achieving an electrical connection between the conductive pillar structure 145 and the conductive structure 110 through the second protective layer 170. Accordingly, the second protective layer 170 includes a conductive material.

[0127] In this embodiment, a conductive structure 110 is formed in the substrate 100. The conductive structure 110 is located on the side of the second protective layer 170 away from the conductive pillar structure 145. The conductive structure 110 is located between the bottom surface of the conductive pillar structure 145 and the substrate 100.

[0128] The conductive structure 110 includes conductive contacts, pads, or conductive lines, etc., which are not specifically limited in this application.

[0129] The conductive structure 110 is used to electrically connect with the conductive pillar structure 145 to realize the electrical function of the conductive pillar structure 145. For example, one end of the conductive structure 110 is electrically connected to the conductive pillar structure 145, and the other end is used to electrically connect to the selection unit.

[0130] In this embodiment, the material of the second protective layer 170 includes amorphous tantalum nitride (TaN). The second protective layer 170 (a part of the protective material layer) comprises an amorphous material, which allows for more effective protection of the conductive pillar structure 145 during the removal of the sacrificial layer 122, and the deposition process of the amorphous material is simple. Correspondingly, both the second protective layer 170 and the conductive pillar structure 145 have good conductivity, resulting in a lower connection resistance between the conductive pillar structure 145 and the conductive structure 110.

[0131] Dielectric layer 150 is used as the dielectric material for storage capacitors in the memory.

[0132] In this embodiment, the dielectric layer 150 includes a ferroelectric material layer. The ferroelectric material layer has spontaneous polarization characteristics and can form two different stable residual polarization states under the action of an external electric field. By utilizing the above-mentioned polarization characteristics of the ferroelectric material layer to store data "0" or "1", it is possible to achieve benefits such as high-speed read and write, high durability and low power consumption, and is suitable for various application scenarios with high-performance storage requirements.

[0133] In this embodiment, as explained above, the capacitor area is easy to control.

[0134] The dielectric layer 150, including a ferroelectric material layer as a storage medium, can be polarized according to the direction and magnitude of an external electric field. Even after the external electric field is removed, it retains partial polarization, i.e., residual polarization. This residual polarization has a potential difference, causing the capacitor electrodes on both sides of the dielectric layer 150—that is, the surfaces of the conductive pillar structure 145 and the conductive plate structure 160 near the dielectric layer 150—to induce charges of opposite polarities. Different polarization directions induce different charges, thus enabling the storage of logic "0" and logic "1". The area of ​​the dielectric layer 150, including the ferroelectric material layer, in contact with the passivation layer 135 is easier to control, allowing for uniform capacitor area while reducing fabrication complexity. This enables the capacitor electrodes on both sides of the dielectric layer 150 to release equal amounts of charge during data reading, thereby improving data reading accuracy, reducing the difficulty of memory read / write control, and consequently improving the performance of the formed semiconductor structure when applied to ferroelectric memory.

[0135] Specifically, the opposing surfaces of the conductive plate structure 160 and the conductive pillar structure 145 are the upper electrode and the lower electrode, respectively. The capacitor includes the upper electrode, the lower electrode, and a dielectric layer located between them. The upper electrode is connected to the upper conductor in the conductive plate structure 160, and the lower electrode is connected to the lower conductor in the conductive pillar structure 145.

[0136] Accordingly, embodiments of the present invention also provide a memory, including a semiconductor structure and a selection unit provided in the embodiments of the present invention, wherein the selection unit is connected to a conductive pillar structure in a one-to-one correspondence. For details regarding the semiconductor structure provided in the embodiments of the present invention, please refer to the foregoing section; further details will not be repeated here.

[0137] The memory is a three-dimensional memory, with multiple capacitors distributed in a three-dimensional array within the semiconductor structure. Each column vertically includes multiple capacitors. In each capacitor, a lower electrode is electrically connected to a lower wire in the conductive pillar structure, and an upper electrode is connected to an upper wire in the electrode plate structure. Multiple capacitors in the same layer are electrically connected to each other via upper wires. The selection unit is connected one-to-one with the conductive pillar structure in the semiconductor structure provided in this embodiment, thereby applying voltage to the conductive pillar structure through the selection unit to achieve the memory read operation.

[0138] While the present invention has been disclosed above, it is not limited thereto. Any person skilled in the art can make various modifications and alterations without departing from the spirit and scope of the invention; therefore, the scope of protection of the present invention should be determined by the scope defined in the claims.

Claims

1. A method of forming a semiconductor structure, characterized by, include: A substrate is provided on which a stacked structure is formed, the stacked structure comprising dielectric layers and sacrificial layers stacked alternately from bottom to top in a longitudinal direction; Forming through-holes that penetrate the stacked structure; A protective material layer is formed covering the top, sidewalls, and bottom of the stacked structure, wherein the material of the protective material layer includes a conductive material; An anisotropic etching process is performed to passivate the protective material layer on the sidewall and bottom surface of the via, forming a passivation material layer. The anisotropic etching process also removes the passivation material layer on the surface of the protective material layer on the bottom surface of the via, while retaining the passivation material layer on the surface of the protective material layer on the sidewall of the via. A conductive pillar structure is formed to fill the through-hole; Remove the protective material layer on top of the stacked structure, retain the protective material layer on the sidewall and bottom of the through hole as the first protective layer, and the remaining passivation material layer as the passivation layer, which is located on the sidewall of the first protective layer; The sacrificial layer in the stacked structure is removed to form a plurality of first trenches arranged at intervals along the longitudinal direction, the first trenches being surrounded by longitudinally adjacent dielectric layers; Using the passivation layer as a stop layer, the exposed portion of the first protective layer is removed along each of the first trenches to form a second trench. The second trench is connected to the first trench to form a third trench, and the remaining first protective layer is formed as the second protective layer. A dielectric layer is formed covering each side and bottom surface of the third trench; A conductive plate structure is formed to fill the third trench, and the conductive plate structure covers the dielectric layer.

2. The formation process of claim 1 wherein, The anisotropic etching process includes plasma-assisted etching.

3. The formation method of claim 2, wherein, The protective material layer includes tantalum nitride, and the process gas for the plasma-assisted etching process includes fluorine-containing and / or chlorine-containing process gases.

4. The formation method of claim 3, wherein, The bias power of the plasma-assisted etching process is 400W to 800W.

5. The formation method of claim 2, wherein, The protective material layer comprises doped or undoped polycrystalline silicon prepared by LPCVD process, and the process gas of the plasma-assisted etching process comprises an oxygen-containing process gas.

6. The formation method of claim 2, wherein, The anisotropic etching process includes: A protective layer is deposited, the protective layer including a portion located at the top of the stacked structure; Perform the plasma-assisted etching process to perform the surface passivation treatment, passivate the surface of the protective material layer, and remove the passivation material layer located on the surface of the protective material layer on the bottom surface of the via.

7. The formation method of claim 6, wherein, In the step of depositing the protective layer, the protective layer further includes a portion extending to a certain depth of the through-hole to cover a portion of the sidewall of the protective material layer.

8. The formation method of claim 6, wherein, In the step of depositing the protective layer, the protective layer comprises a polymer, and the protective layer is prepared by a plasma-assisted deposition process, wherein the process gas of the plasma-assisted deposition process comprises a carbon-containing gas.

9. The formation method of claim 6, wherein, The anisotropic etching process includes: The steps of depositing the protective layer and performing the plasma-assisted etching process are repeated multiple times.

10. The formation process of claim 1 wherein, The passivation material layer is made of one or more selected from tantalum chloride, tantalum oxychloride, tantalum fluoride, tantalum oxyfluoride, and silicon oxide.

11. The formation process of claim 1 wherein, The thickness of the passivation layer is 1 nm to 3 nm.

12. The formation process of claim 1 wherein, In the step of forming a protective material layer covering the top, sidewalls and bottom of the stacked structure, the process of preparing the protective material layer is such that the step coverage of the protective material layer satisfies the requirement that the inner diameter of the protective material layer is uniform in the longitudinal direction after its formation.

13. The formation process of claim 1 wherein, The material of the protective layer includes amorphous tantalum nitride.

14. The formation process of claim 1 wherein, In the step of providing the substrate, a conductive structure is formed in the substrate; In the step of forming a through-hole through the stacked structure, the bottom of the through-hole exposes the conductive structure.

15. A semiconductor structure, characterized by Prepared using the formation method described in any one of claims 1 to 14.

16. A semiconductor structure, characterized by include: Base; A stacked layer, located on the substrate, the stacked layer comprising dielectric layers and conductive plate structures alternately stacked longitudinally from bottom to top; Multiple conductive pillar structures penetrate the stacked layers; A passivation layer is continuously disposed along the sidewall of the conductive pillar structure; A second protective layer is provided along the entire surface of the conductive pillar structure that does not deviate from the substrate. The second protective layer is interrupted by the conductive plate structure to form a discontinuous layer. The second protective layer contacts the passivation layer on the surface that deviates from the conductive pillar structure. A dielectric layer is formed on the surface of the conductive plate structure opposite to the second protective layer, the passivation layer, and the dielectric layer; The passivation layer and the second protective layer have at least one of the same elements.

17. The semiconductor structure of claim 16, wherein, The thickness of the passivation layer is 1 nm to 3 nm.

18. The semiconductor structure of claim 16, wherein, The angle between the passivation layer and the substrate is 90°~91°.

19. The semiconductor structure of claim 16, wherein, The thickness of the second protective layer on the portion of the passivation layer away from the conductive pillar structure gradually increases in the direction from the substrate toward the stacked layer.

20. The semiconductor structure of claim 16, wherein, The second protective layer includes tantalum nitride, and the passivation layer material includes one or more selected from tantalum chloride, tantalum oxychloride, tantalum fluoride, and tantalum oxyfluoride; or The second protective layer comprises polycrystalline silicon, and the passivation layer comprises silicon oxide.

21. The semiconductor structure of claim 16, wherein, The second protective layer comprises amorphous tantalum nitride.

22. The semiconductor structure of claim 16, wherein, A conductive structure is formed in the substrate, the conductive structure being located on the side of the second protective layer away from the conductive pillar structure, and the conductive structure being located on the side of the conductive pillar facing the substrate.

23. A memory, comprising: include: The semiconductor structure as claimed in any one of claims 15 to 22; The selection unit is connected one-to-one with the conductive pillar structure in the semiconductor structure.