Method for manufacturing mos capacitor structure for reducing failure of goi detection
By adding an annealing step before gate oxide growth, and using annealing treatment in a mixed atmosphere of H₂ and N₂, silicon wafer defects are eliminated, the problems of uneven oxide layer thickness and increased interface traps are solved, and the GOI inspection pass rate is significantly improved.
Patent Information
- Application Number
- CN202611329081.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-31
- Publication Date
- 2026-11-24
AI Technical Summary
In the fabrication of MOS capacitor structures, existing technologies suffer from silicon wafer defects that lead to uneven oxide layer thickness and increased interface traps, resulting in a decrease in the GOI (Gross Object Inspection) pass rate.
An annealing step is added before the gate oxide layer is grown. Annealing is performed using a mixed atmosphere of H₂ and N₂ to eliminate silicon wafer defects. Metal electrodes are then prepared by vapor deposition to avoid increasing the oxide layer thickness and interface trap density.
It significantly improved the GOI detection pass rate and enhanced the breakdown and interface characteristics of the gate oxide layer, increasing the GOI detection pass rate from 30% to 70%.
Smart Images

Figure CN123164785A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of semiconductor technology, specifically relating to a method for fabricating a MOS capacitor structure to reduce GOI detection failure. Background Technology
[0002] GOI, short for Gate Oxide Integrity, is a core structure in metal-oxide-semiconductor (MOS) devices, and its quality directly determines the device's electrical performance and long-term reliability. GOI is a key indicator of the gate oxide layer's resistance to electrical stress damage. By evaluating parameters such as its breakdown electric field and breakdown charge, the presence of harmful defects in the oxide layer can be effectively detected. With the continuous advancement of integrated circuit technology nodes and the continuous reduction in gate oxide layer thickness, its sensitivity to process defects has significantly increased, making GOI one of the main bottlenecks restricting device yield and reliability.
[0003] For example, the prior art with patent application number 202510293023.4 and invention title: Method for Forming Semiconductor Structure provides the following technical solution: a first oxidation treatment is performed on the substrate using a wet oxygen oxidation process to form a first oxide layer on the substrate surface. The first oxide layer has a first thickness. The first oxidation treatment of the substrate using the wet oxygen oxidation process includes an oxidation reaction stage. The oxidation reaction stage uses hydrogen and oxygen as reaction gases, and a first protective gas is introduced simultaneously with the hydrogen and oxygen to dilute the reaction gases. After the wet oxygen oxidation process, a second oxidation treatment is performed on the substrate using a dry oxygen oxidation process to form a second oxide layer between the substrate surface and the first oxide layer.
[0004] The above-mentioned technical methods combine wet oxidation and dry oxidation processes, taking advantage of the high density of the oxide layer formed by wet oxidation and the ability of dry oxidation to reduce interface defects between the oxide layer and the silicon substrate, thereby improving the performance of the fabricated MOS devices. However, the following technical problems still exist: neither wet oxidation nor dry oxidation processes alone can eliminate defects in the silicon wafer. These defects not only lead to uneven oxide layer thickness but also increase interface traps between the oxide layer and the silicon wafer, which in turn leads to a decrease in the GOI (Gross Detection Index) pass rate of the fabricated MOS devices. Summary of the Invention
[0005] In view of this, the present invention provides a method for fabricating a MOS capacitor structure to reduce GOI detection failure, thereby reducing the gate oxide interface trap density and improving the GOI detection pass rate by eliminating some defects in the silicon wafer.
[0006] The technical solution adopted by this invention to solve its technical problem is:
[0007] A method for fabricating a MOS capacitor structure to reduce GOI detection failure includes the following steps:
[0008] S1. Pre-treat the silicon wafer to remove surface particles, organic matter and metal impurities to obtain a pre-treated silicon wafer;
[0009] S2. The pretreated silicon wafer is kept at a predetermined temperature in a mixed atmosphere of H2 and N2 for a predetermined holding time. After the holding time is completed, it is cooled down at a predetermined cooling rate to complete the annealing process, so as to consume some defects of the pretreated silicon wafer and obtain the annealed silicon wafer.
[0010] S3. After annealing, the silicon wafer is grown under a dry oxygen atmosphere to generate a SiO2 layer of a predetermined thickness to obtain a silicon wafer with a gate oxide layer.
[0011] S4. Prepare metal electrodes on the gate oxide silicon wafer, deposit Al electrodes of predetermined specifications by vapor deposition, and form a MOS capacitor structure.
[0012] Preferably, the pretreatment in step S1 consists of sequential DSP polishing and RCA cleaning.
[0013] Preferably, the predetermined temperature in step S2 is 1100℃~1180℃.
[0014] Preferably, in step S2, the H2 content in the mixed atmosphere is 3% to 7%, and the N2 content is 97% to 93%.
[0015] Preferably, the predetermined heat preservation time in step S2 is 45 min to 75 min.
[0016] Preferably, the predetermined cooling rate in step S2 is 15℃ / min to 25℃ / min.
[0017] Preferably, the dry oxygen atmosphere in step S3 has a temperature of 850~950℃ and an oxygen flow rate of 1.8~2.2L / min.
[0018] Preferably, the SiO2 layer of predetermined thickness mentioned in step S3 has a thickness of 9~11 nm.
[0019] Preferably, the Al electrode with predetermined specifications mentioned in step S4 has an Al electrode diameter of 90~110μm and an Al electrode spacing of 180~220μm.
[0020] The present invention also provides a MOS capacitor structure prepared by the above-described method for preparing a MOS capacitor structure that reduces GOI detection failure.
[0021] The aforementioned method for fabricating a MOS capacitor structure to reduce GOI detection failure involves adding an annealing step before gate oxide growth. The heat generated by the annealing process drives Si atoms to migrate and rearrange in a directional manner, allowing silicon wafer defects to return from a high-energy unstable state to a low-energy stable state, thus eliminating some defects in the pre-treated silicon wafer. Using a mixed atmosphere of H2 and N2 as the annealing atmosphere effectively avoids the problem of increased gate oxide thickness caused by silicon wafer oxidation. Furthermore, H2 and N2 can passivate the silicon wafer surface, reducing the interface trap density and thereby improving the GOI detection pass rate. Attached Figure Description
[0022] Figure 1 This is a schematic flowchart of the method for fabricating a MOS capacitor structure to reduce GOI detection failure according to the present invention. Detailed Implementation
[0023] To more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0024] Please refer to Figure 1 A method for fabricating a MOS capacitor structure to reduce GOI detection failure includes the following steps:
[0025] S1. The silicon wafer is pretreated by DSP polishing and RCA cleaning in sequence to remove surface particles, organic matter and metal impurities to obtain a pretreated silicon wafer.
[0026] S2. The pretreated silicon wafer is held at 1100℃~1180℃ in a mixed atmosphere of H2 and N2 for 45min~75min. After the holding time, the temperature is reduced at 15℃ / min~25℃ / min to complete the annealing process, so as to eliminate some defects of the pretreated silicon wafer and obtain the annealed silicon wafer. The content of H2 in the mixed atmosphere is 3%~7%, and the content of N2 in the mixed atmosphere is 97%~93%.
[0027] S3. After annealing, the silicon wafer is subjected to gate oxide growth in a dry oxygen atmosphere at a temperature of 850~950℃ and an oxygen flow rate of 1.8~2.2L / min to generate a SiO2 layer of 9~11nm, thereby obtaining a gate oxide silicon wafer.
[0028] S4. Prepare metal electrodes on the gate oxide silicon wafer by evaporating Al electrodes with a diameter of 90~110μm and a spacing of 180~220μm to obtain a silicon wafer with a MOS capacitor structure.
[0029] For step S1, the silicon wafer is sequentially subjected to DSP polishing and RCA cleaning pretreatment to obtain a pretreated silicon wafer.
[0030] In this step, atomically flat mirror surfaces are achieved by DSP polishing of the silicon wafer to remove subsurface damage layers and residual stress left by previous processes. This provides a uniform thickness and flat surface for the processing of single-crystal silicon wafers. RCA cleaning removes impurities and contaminants from the polished silicon wafer surface, preventing the introduction of new contaminants from damaging the purity of the silicon wafer, affecting the growth of the gate oxide layer, and causing GOI detection failure.
[0031] For step S2, the pretreated silicon wafer is held at 1100℃~1180℃ in a mixed atmosphere of H2 and N2 for 45min~75min. After the holding period, the temperature is reduced at 15℃ / min~25℃ / min to complete the annealing process, so as to eliminate some defects of the pretreated silicon wafer and obtain the annealed silicon wafer. The content of H2 in the mixed atmosphere is 3%~7%, and the content of N2 in the mixed atmosphere is 97%~93%.
[0032] In this step, the pre-treated silicon wafer is annealed. The heat generated by annealing can bring the defective areas of the silicon wafer back from a high-energy unstable state to a low-energy stable state, eliminating some defects on the pre-treated silicon wafer. This avoids the problem of uneven gate oxide layer thickness caused by different oxidation rates between the defective areas and the silicon wafer surface, thus improving the GOI detection pass rate. A mixed atmosphere of H2 and N2 is used as the annealing atmosphere to protect the silicon wafer from oxidation. Furthermore, H2 and N2 passivate the silicon wafer surface, reducing the interface trap density and improving the GOI detection pass rate.
[0033] Specifically, the principle of H2 and N2 passivating the silicon wafer surface is as follows: Si atoms at the defects on the silicon wafer surface will form dangling bonds. H2 and N2 will diffuse to the defects during the annealing process and form stable Si-H bonds and Si-N bonds with the dangling bonds of Si atoms at the defects. After the dangling bonds are formed, they no longer provide energy levels that can trap charges, thereby neutralizing the electrical defects at the defects and reducing the interface trap density.
[0034] For step S3, the annealed silicon wafer is subjected to gate oxide growth in a dry oxygen atmosphere at a temperature of 850~950℃ and an oxygen flow rate of 1.8~2.2L / min to generate a SiO2 layer of 9~11nm, thereby obtaining a gate oxide silicon wafer.
[0035] In this step, the thickness of the gate oxide layer on the silicon wafer surface is controlled by precisely controlling the temperature and oxygen flow rate, so as to prepare a thin gate oxide layer.
[0036] For step S4, metal electrodes are prepared on the gate oxide silicon wafer by evaporating Al electrodes with a diameter of 90~110μm and a spacing of 180~220μm to obtain a MOS capacitor structure silicon wafer.
[0037] In this step, during the preparation of the metal electrode, vapor deposition is used instead of sputtering. Compared with sputtering, vapor deposition results in lower kinetic energy of high-energy particles during the preparation of the metal electrode, causing less damage to the gate oxide layer and resulting in a higher purity metal electrode.
[0038] The above-mentioned method for fabricating a MOS capacitor structure to reduce GOI detection failure involves annealing the pretreated silicon wafer before gate oxide layer growth to eliminate some defects. A mixed atmosphere of H2 and N2 is used as the annealing atmosphere. While avoiding oxidation of the silicon wafer, H2 and N2 passivate the silicon wafer. H2 and N2 form stable Si-H and Si-N bonds with the Si dangling bonds at the defects in the silicon wafer, reducing the interface trap density and improving the GOI detection pass rate.
[0039] Furthermore, the present invention also provides a MOS capacitor structure, which is prepared by the above-described method for preparing a MOS capacitor structure to reduce GOI detection failure.
[0040] To facilitate understanding of the technical concept and patentability of this application, the following embodiments are further provided:
[0041] Example 1
[0042] This embodiment provides a method for fabricating a MOS capacitor structure to reduce GOI detection failure. The specific steps are as follows:
[0043] S1. Perform DSP polishing and RCA cleaning pretreatment on the silicon wafer in sequence to remove surface particles, organic matter and metal impurities to obtain a pretreated silicon wafer.
[0044] S2. The pretreated silicon wafer is kept at 1050℃ in N2 atmosphere for 30 minutes. After the holding time is completed, the temperature is reduced at 5℃ / min to complete the annealing process and obtain the annealed silicon wafer.
[0045] S3. After annealing, the silicon wafer is subjected to gate oxide layer growth in a dry oxygen atmosphere at a temperature of 900℃ and an oxygen flow rate of 2L / min to generate a 10nm SiO2 layer, thereby obtaining a gate oxide layer silicon wafer.
[0046] S4. Prepare metal electrodes on the gate oxide silicon wafer by evaporating Al electrodes with a diameter of 100μm and a spacing of 200μm to obtain a MOS capacitor structure silicon wafer.
[0047] S5. Perform EBD testing on the silicon wafer with the MOS capacitor structure to test the GOI breakdown electric field of the silicon wafer with the MOS capacitor structure. The constant voltage ramp step is 0.1V / s. Breakdown is defined as when the leakage current >1μA. Calculate E. bd =V bd / d ;
[0048] S6. Use a laser scattering particle analyzer to scan the surface of the silicon wafer with MOS capacitor structure, test the COP density of the silicon wafer with MOS capacitor structure, and count the number of COPs.
[0049] S7. Perform high-frequency CV testing on the silicon wafer with the MOS capacitor structure and calculate the flat-band voltage offset ΔV. FB The calculation formula is: , where D it For interface trap density, ΔV FB For flat band voltage offset, C ox Let q be the total capacitance of the gate oxide layer, q be the fundamental charge constant, and A be the effective area of the MOS capacitor.
[0050] Example 2
[0051] The only difference between this embodiment 2 and embodiment 1 is the annealing process in step S2; the other steps are exactly the same.
[0052] Step S2 specifically involves: holding the pretreated silicon wafer at 1050℃ in a mixed atmosphere with 5% H2 content and 95% N2 content for 60 minutes, and then cooling it down at 20℃ / min after the holding period to complete the annealing process and obtain the annealed silicon wafer.
[0053] Example 3
[0054] The only difference between this embodiment 3 and embodiment 1 is the annealing process in step S2; the other steps are exactly the same.
[0055] Step S2 specifically involves: holding the pretreated silicon wafer at 1050℃ in an Ar atmosphere for 90 minutes, and then cooling it down at 50℃ / min after the holding period to complete the annealing process and obtain the annealed silicon wafer.
[0056] Example 4
[0057] The only difference between Example 4 and Example 1 is the annealing process in step S2; the other steps are exactly the same.
[0058] Step S2 specifically involves: holding the pretreated silicon wafer at 1100℃ in a mixed atmosphere with 5% H2 content and 95% N2 content for 30 minutes, and then cooling it down at 50℃ / min after the holding period to complete the annealing process and obtain the annealed silicon wafer.
[0059] Example 5
[0060] The only difference between Example 5 and Example 1 is the annealing process in step S2; the other steps are exactly the same.
[0061] Step S2 specifically involves: holding the pretreated silicon wafer at 1100℃ in an Ar atmosphere for 60 minutes, and then cooling it down at a rate of 5℃ / min after the holding period to complete the annealing process and obtain the annealed silicon wafer.
[0062] Example 6
[0063] The only difference between Example 6 and Example 1 is the annealing process in step S2; the other steps are exactly the same.
[0064] Step S2 specifically involves: holding the pretreated silicon wafer at 1100℃ in a pure N2 atmosphere for 90 minutes, and then cooling it down at a rate of 20℃ / min after the holding period to complete the annealing process and obtain the annealed silicon wafer.
[0065] Example 7
[0066] The only difference between Example 7 and Example 1 is the annealing process in step S2; the other steps are exactly the same.
[0067] Step S2 specifically involves: holding the pretreated silicon wafer at 1150℃ in an Ar atmosphere for 30 minutes, and then cooling it down at a rate of 20℃ / min after the holding period to complete the annealing process and obtain the annealed silicon wafer.
[0068] Example 8
[0069] The only difference between Example 8 and Example 1 is the annealing process in step S2; the other steps are exactly the same.
[0070] Step S2 specifically involves: holding the pretreated silicon wafer at 1150℃ in a N2 atmosphere for 60 minutes, and then cooling it down at 50℃ / min after the holding period to complete the annealing process and obtain the annealed silicon wafer.
[0071] Example 9
[0072] The only difference between Example 9 and Example 1 is the annealing process in step S2; the other steps are exactly the same.
[0073] Step S2 specifically involves: holding the pretreated silicon wafer at 1150℃ in a mixed atmosphere with 5% H2 content and 95% N2 content for 90 minutes, and then cooling it down at 5℃ / min after the holding period to complete the annealing process and obtain the annealed silicon wafer.
[0074]
[0075] As shown in Table 1, Example 9 exhibits the highest GOI breakdown electric field compared to Examples 1 to 8, indicating that the silicon wafer annealed using the annealing parameters of Example 9 has superior intrinsic quality of the gate oxide layer, resulting in higher reliability and longer lifespan. Furthermore, Example 9 shows a higher COP density D compared to Examples 1 to 8. cop The lowest value indicates that the silicon wafer annealed using the annealing parameters of Example 9 has fewer void-type defects, which is beneficial for the growth of the gate oxide layer; compared with Examples 1 to 8, Example 9 has a lower interface trap charge density D. it The lowest value indicates that the silicon wafer annealed using the annealing parameters of Example 9 has a more complete gate oxide layer and fewer interface defects, which is conducive to the movement of charge carriers and results in a semiconductor device with higher performance.
[0076] Use JMP or Minitab software to perform analysis of variance on the data in Table 1 to determine the degree of influence of each parameter condition on the test results.
[0077] As shown in Table 2, among the parameters mentioned above, annealing temperature, holding time, and annealing atmosphere are the core factors affecting the GOI performance of silicon wafers. Among them, the annealing atmosphere has the greatest impact on GOI performance, while the cooling rate has a relatively weak impact on the results.
[0078]
[0079] The main effects of the data in Table 2 were calculated using JMP or Minitab software to determine the priority of each parameter's impact on the silicon wafer's GOI performance.
[0080]
[0081] As shown in Table 3, the annealing atmosphere is related to the GOI breakdown electric field E. bd COP density D cop Interface trap charge D it The core influencing factor is that a mixed atmosphere of N2 and H2 is used as the annealing atmosphere, which can effectively improve the GOI detection pass rate.
[0082]
[0083] Based on the data in Tables 1 to 4, it can be seen that at 1150℃, E bd Compared to 1050℃, the performance improved by 23%, while the COP density decreased by 82%, with the greatest performance improvement observed in the 1150℃ temperature range. At a holding time of 60 minutes, the COP density decreased by 33% compared to a holding time of 30 minutes, but at a holding time of 90 minutes, the E... bd The efficiency is only increased by 3%, therefore, a holding time of 60 minutes is the optimal balance point for efficiency; compared to N2 atmosphere, E bd Increase by 10%, Dit A 56% reduction demonstrates that H atoms can effectively bind to dangling bonds on the silicon wafer surface, passivating trapped charges at the Si-SiO2 interface. Experiments have also verified that for every 1% increase in H2, D... it To reduce the concentration by 8%, a mixed atmosphere with 5% H2 and 95% N2 was chosen as the annealing atmosphere; although the cooling rate of 5℃ / min resulted in the lowest COP density, D... it The cooling rate is 27% higher than that of 20℃ / min, therefore, the optimal equilibrium point is a cooling rate of 20℃ / min.
[0084] The optimal annealing procedure is to anneal at 1150℃ in a mixed atmosphere with 5% H2 and 95% N2, hold for 60℃, and then cool down at a rate of 20℃ / min.
[0085]
[0086] As shown in Table 5, the MOS capacitor structure prepared by the method for reducing GOI detection failure provided by this invention has a breakdown electric field E bd The concentration reached 10.2±0.2MV / cm, a 24.4% improvement over the conventional method's 8.2±0.3MV / cm, demonstrating significantly better process consistency and stability than existing technologies; the COP density decreased to 9±1 particles / cm. 2 Compared to the conventional method, 45±5 cells / cm 2 The 80% reduction indicates that native vacancy defects in the silicon wafer have been effectively eliminated, fundamentally reducing the weak points for early failure of the gate oxide layer; interface trap density D it Reaching 1.1 ± 0.1 × 10 10 cm -2 eV -1 Compared to the conventional method, 3.2 ± 0.4 × 10 10 cm -2 eV -1 The reduction of 65.6% proves that the dangling bonds at the Si / SiO2 interface are sufficiently passivated.
[0087] In summary, the MOS capacitor structure fabrication method for reducing GOI detection failure provided by this invention adds an annealing step before the growth of the gate oxide layer, and performs synergistic optimization of the "temperature-time-atmosphere" of the annealing step, improves substrate defects and interface passivation effect, significantly improves the breakdown characteristics, interface characteristics and overall reliability of the gate oxide layer, and increases the GOI detection pass rate of MOS devices from 30% to 70%.
[0088] The above description discloses only preferred embodiments of the present invention and should not be construed as limiting the scope of the invention. Those skilled in the art will understand that all or part of the processes for implementing the above embodiments and equivalent variations made in accordance with the claims of the present invention are still within the scope of the invention.
Claims
1. A method for fabricating a MOS capacitor structure to reduce GOI detection failure, characterized in that, Includes the following steps: S1. Pre-treat the silicon wafer to remove surface particles, organic matter and metal impurities to obtain a pre-treated silicon wafer; S2. The pretreated silicon wafer is kept at a predetermined temperature in a mixed atmosphere of H2 and N2 for a predetermined holding time. After the holding time is completed, it is cooled down at a predetermined cooling rate to complete the annealing process, so as to eliminate some defects in the pretreated silicon wafer and obtain the annealed silicon wafer. S3. After annealing, the silicon wafer is grown under a dry oxygen atmosphere to generate a SiO2 layer of a predetermined thickness to obtain a silicon wafer with a gate oxide layer. S4. Prepare metal electrodes on the gate oxide silicon wafer, deposit Al electrodes of predetermined specifications by vapor deposition, and form a MOS capacitor structure.
2. The method for fabricating a MOS capacitor structure to reduce GOI detection failure according to claim 1, characterized in that, The preprocessing described in step S1 involves sequentially performing DSP polishing and RCA cleaning.
3. The method for fabricating a MOS capacitor structure to reduce GOI detection failure according to claim 1, characterized in that, The predetermined temperature mentioned in step S2 is 1100℃~1180℃.
4. The method for fabricating a MOS capacitor structure to reduce GOI detection failure according to claim 1, characterized in that, The H2 and N2 mixed atmosphere mentioned in step S2 has an H2 content of 3% to 7% and an N2 content of 97% to 93%.
5. The method for fabricating a MOS capacitor structure to reduce GOI detection failure according to claim 1, characterized in that, The predetermined heat preservation time mentioned in step S2 is 45 min to 75 min.
6. The method for fabricating a MOS capacitor structure to reduce GOI detection failure according to claim 1, characterized in that, The predetermined cooling rate in step S2 is 15℃ / min to 25℃ / min.
7. The method for fabricating a MOS capacitor structure to reduce GOI detection failure according to claim 1, characterized in that, The dry oxygen atmosphere described in step S3 is at a temperature of 850~950℃ and an oxygen flow rate of 1.8~2.2L / min.
8. The method for fabricating a MOS capacitor structure to reduce GOI detection failure according to claim 1, characterized in that, The SiO2 layer of predetermined thickness mentioned in step S3 has a thickness of 9~11 nm.
9. The method for fabricating a MOS capacitor structure to reduce GOI detection failure according to claim 1, characterized in that, The Al electrodes mentioned in step S4 have a diameter of 90~110μm and a spacing of 180~220μm.
10. A MOS capacitor structure, characterized in that, The MOS capacitor structure is prepared based on the method for preparing a MOS capacitor structure to reduce GOI detection failure as described in any one of claims 1 to 9.
Citation Information
Patent Citations
Formation method of semiconductor structure
CN120076390A