A mesa glass passivation chip and a laser processing method thereof
By combining laser pattern transfer and in-situ selective oxidation technology with electrophoretic glass passivation, the manufacturing process of mesa glass passivated chips has been simplified, solving the problems of long production cycle and high cost, and achieving a reduction in production cycle and cost.
Patent Information
- Application Number
- CN202610998836.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-06
- Publication Date
- 2026-11-24
AI Technical Summary
Traditional tabletop glass passivation chip production has a long cycle and high cost, high requirements for cleanliness, lengthy processes, and high equipment and time costs.
Laser pattern transfer technology is used to etch trenches and stepped structures, combined with laser in-situ selective oxidation and electrophoretic glass passivation, which simplifies the production process and reduces photolithography and wet etching steps.
The production cycle has been shortened from 9.5 days to 5.5-6.5 days, and the actual production cycle has been shortened from 19 days to 11-12.5 days, reducing manufacturing costs and improving production efficiency and product reliability.
Smart Images

Figure CN123164787A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor manufacturing technology, specifically to a mesa glass passivation chip and its laser processing method. Background Technology
[0002] Traditional TVS chip manufacturing mainly involves over 40 steps, including RCA cleaning, phosphorus pre-expansion, push-up main expansion, oxidation annealing, HMDS baking, double-sided coating, exposure, development, hardening, BOE etching, trench etching, glass coating, glass sintering, LTO deposition, multiple nickel plating, testing, and dicing. The theoretical production cycle is approximately 9.5 days, but in actual production, due to factors such as material standby, transfer, and repeated testing, the cycle often extends to over 19 days, severely impacting delivery efficiency and capacity. Furthermore, the photolithography + wet etching grooving process requires high photolithography cleanliness and is complex, leading to lengthy processes. When scraping glass, to ensure complete glass coverage, two glass coatings, two pre-firings, two sinterings, and two glass cleanings are required, further lengthening the process. Photolithography processes such as LTO deposition, HMDS baking, double-sided coating, exposure, and development are time-consuming and costly. High-temperature thermal oxidation or PECVD deposition of the silicon dioxide protective layer increases equipment and time costs.
[0003] Therefore, how to shorten the production cycle of the passivated chip on the tabletop glass and reduce the manufacturing cost is an urgent problem to be solved. Summary of the Invention
[0004] The main technical problem solved by this invention is to shorten the production cycle of the passivated glass chip and reduce the manufacturing cost.
[0005] According to a first aspect, one embodiment provides a laser processing method for a mesa glass passivation chip, the method comprising: A first laser baffle is placed on the surface of a wafer, where multiple chip regions of the wafer have formed PN junctions. The first laser baffle has a first light-transmitting pattern corresponding to the chip trenches. A laser for etching is emitted to the first laser baffle, and the laser etches the wafer after passing through the first light-transmitting pattern, thereby etching trenches between the chip regions of the wafer. A second laser baffle is placed on the wafer surface, and the second laser baffle has a second light-transmitting pattern corresponding to the stepped structure. A laser for etching is emitted into the second laser baffle, and the laser passes through the second light-transmitting pattern to etch the wafer, thereby etching a stepped structure on the side of the chip region near the trench. The stepped structure is a transition structure between the mesa of the chip region and the trench. The linewidth of the second laser baffle is smaller than the linewidth of the first laser baffle.
[0006] In one embodiment, the front and back sides of multiple chip regions of the wafer are coated with a water-soluble laser protective liquid to capture slag and spatter generated by laser etching; the water-soluble laser protective liquid is obtained by mixing a variety of water-soluble polymers, surfactants, defoamers and deionized water.
[0007] In one embodiment, in-situ selective scanning oxidation is performed on the trench, the stepped structure, and the mesa of the chip region to obtain an oxide layer.
[0008] In one embodiment, the oxide layer includes a first oxide layer and a second oxide layer; the thickness of the first oxide layer is greater than the thickness of the second oxide layer. In-situ selective scanning oxidation is performed on the trenches, the stepped structure, and the mesa of the chip region to obtain an oxide layer, including: Selective laser scanning oxidation is performed on the bottom region of the trench, the region between the edge of the platform and the stepped structure, so that the first oxide layer is generated in situ in the bottom region of the trench, the region between the edge of the platform and the stepped structure. Laser scanning oxidation is performed on the welding window area of the table surface to generate the second oxide layer in the welding window area of the table surface.
[0009] In one embodiment, the atmosphere for in-situ selective scanning oxidation includes pure oxygen or dry compressed air.
[0010] In one embodiment, the method further includes: After obtaining the oxide layer, an electrophoretic solution is deposited in the unoxidized area of the wafer to obtain a glass passivation layer; The wafer is subjected to surface metallization treatment to obtain a chip bonding metal layer.
[0011] In one embodiment, the deposition of electrophoretic solution in the unoxidized region of the wafer to obtain a glass passivation layer includes: The wafer is placed in the electrophoretic solution, which is then deposited on the non-oxidized regions of the chip stepped structure and the chip trenches, respectively. The electrophoretic solution is obtained by mixing glass paste, silica nanoparticles, and deionized water. The silica nanoparticles have a particle size between 10 nm and 50 nm. The wafer after electrophoretic deposition is subjected to glass sintering to obtain the glass passivation layer.
[0012] In one embodiment, the method further includes: The wafer is placed in a dilute hydrofluoric acid solution to remove the second oxide layer in the welding window area of the mesa.
[0013] In one embodiment, the surface metallization treatment of the wafer to obtain a chip bonding metal layer includes: The welding window of the mesa on the wafer is subjected to surface metallization treatment to obtain the chip welding metal layer.
[0014] According to a second aspect, one embodiment provides a mesa glass passivation chip, comprising: Substrate; A first type semiconductor layer is stacked on the substrate; A heavily doped type II semiconductor layer is stacked on the lower layer of the substrate; The first type of semiconductor layer has a trench on its side, and a stepped structure is provided at the junction of the first type of semiconductor layer and the trench; wherein the trench and the stepped structure are processed by the laser processing method described above; Both the first type semiconductor layer and the heavily doped second type semiconductor layer are covered with a metallization layer.
[0015] According to the above embodiment of a mesa glass passivation chip and its laser processing method, since the first light-transmitting pattern on the first laser baffle corresponds exactly to the area where the chip trench is located; after placing the first laser baffle and the wafer in a laser etching machine, the laser etching machine emits a laser for etching towards the first light-transmitting pattern on the first laser baffle. The laser passes through the first light-transmitting pattern and completes etching between the chip areas of the wafer, thereby forming trenches; since the second light-transmitting pattern on the second laser baffle corresponds exactly to the area where the chip stepped structure is located; after placing the second laser baffle... After the wafer with etched trenches is placed in a laser etching machine, the laser etching machine emits a laser for etching onto a second transparent pattern on a second laser baffle. The laser passes through the second transparent pattern and completes the etching on the side of the chip area near the trench, thereby forming a stepped structure. The trenches and stepped structure are achieved through laser baffle pattern transfer and laser grooving processes, reducing the steps of photolithography and wet trench etching, and effectively shortening the chip manufacturing process. In addition, the laser etching process of this invention does not require a photolithography cleanroom, reducing consumables such as photolithography cleanrooms, photoresist, and developer. Attached Figure Description
[0016] Figure 1 A flowchart illustrating a laser processing method for a passivated glass chip on a mesa, according to one embodiment; Figure 2 This is a schematic diagram of a first laser baffle according to one embodiment; Figure 3 This is a schematic diagram of the trench structure of a mesa glass passivation chip according to one embodiment; Figure 4 This is a schematic diagram of a stepped structure of a mesa glass passivation chip according to one embodiment; Figure 5 This is a schematic diagram of the first oxide layer of a mesa glass passivation chip according to one embodiment. Figure 6 for Figure 5 A magnified view of the first oxide layer in the area between the edge of the central platform and the stepped structure; Figure 7 for Figure 5 A magnified view of the first oxide layer in the bottom region of the central trench; Figure 8 This is a schematic diagram of the second oxide layer of a mesa glass passivation chip according to one embodiment. Figure 9 This is a schematic diagram of a laser baffle for a welding window according to one embodiment; Figure 10 This is a schematic diagram of the glass passivation layer of a mesa glass passivation chip according to one embodiment; Figure 11 This is a schematic diagram of the structure of a mesa glass passivation chip according to one embodiment. Detailed Implementation
[0017] The present invention will now be described in further detail with reference to specific embodiments and accompanying drawings. Similar elements in different embodiments are referred to by associated similar element reference numerals. In the following embodiments, many details are described to facilitate a better understanding of the invention. However, those skilled in the art will readily recognize that some features may be omitted in different situations, or may be replaced by other elements, materials, or methods. In some cases, certain operations related to the present invention are not shown or described in the specification. This is to avoid obscuring the core parts of the invention with excessive description. For those skilled in the art, detailed description of these related operations is not necessary; they can fully understand the related operations based on the description in the specification and general technical knowledge in the art.
[0018] Furthermore, the features, operations, or characteristics described in the specification can be combined in any suitable manner to form various embodiments. At the same time, the steps or actions in the method description can be rearranged or adjusted in a manner obvious to those skilled in the art. Therefore, the various orders in the specification and drawings are only for the clear description of a particular embodiment and do not imply a necessary order, unless otherwise stated that a particular order must be followed.
[0019] The serial numbers assigned to components in this article, such as "first" and "second", are used only to distinguish the objects being described and have no sequential or technical meaning.
[0020] Traditional TVS chip manufacturing mainly involves over 40 steps, including RCA cleaning, phosphorus pre-expansion, push-up main expansion, oxidation annealing, HMDS baking, double-sided coating, exposure, development, hardening, BOE etching, trench etching, glass coating, glass sintering, LTO deposition, multiple nickel plating, testing, and dicing. The theoretical production cycle is approximately 9.5 days, but in actual production, due to factors such as material standby, transfer, and repeated testing, the cycle often extends to over 19 days, severely impacting delivery efficiency and capacity. Furthermore, the photolithography + wet etching grooving process requires high photolithography cleanliness and is complex, leading to lengthy processes. When scraping glass, to ensure complete glass coverage, two glass coatings, two pre-firings, two sinterings, and two glass cleanings are required, further lengthening the process. Photolithography processes such as LTO deposition, HMDS baking, double-sided coating, exposure, and development are time-consuming and costly. High-temperature thermal oxidation or PECVD deposition of the silicon dioxide protective layer increases equipment and time costs.
[0021] Based on this, this invention addresses the pain points of existing TVS chip manufacturing processes, such as lengthy processes, long cycles, high costs, and high dependence on photolithography cleanliness. It proposes a solution involving laser pattern transfer (no photoresist, no photolithography chamber, no development / etching), laser grooving, laser in-situ oxidation, electrophoretic glass passivation, and functional modification of the passivation layer. This systematically simplifies the chip manufacturing process, shortens the chip production cycle, and reduces chip manufacturing costs. Furthermore, the laser processing method for mesa glass passivated chips in this invention is applicable to large-scale production scenarios of GPP glass passivated TVS chips.
[0022] Please refer to Figure 1 , Figure 1 This is a flowchart of a laser processing method for a passivated glass chip on a mesa, one embodiment of which includes steps S101 and S102: S101. A first laser baffle is placed on the surface of a wafer. Multiple chip regions of the wafer have formed PN junctions. A first light-transmitting pattern corresponding to the chip trench is provided on the first laser baffle. A laser for etching is emitted to the first laser baffle. After passing through the first light-transmitting pattern, the laser etches the wafer, thereby etching trenches between the chip regions of the wafer.
[0023] It should be noted that the first laser baffle can be fabricated by forming a metallic chromium pattern on a quartz substrate. Specifically, a metallic chromium pattern is fabricated on an ultraviolet fused silica substrate as a mask, closely attached to the wafer surface, and patterned etching is achieved under laser scanning. The entire process eliminates the need for consumables such as photoresist cleanrooms, photoresist, and developer. It should also be noted that the first laser can be an ultraviolet laser, a picosecond laser, or a femtosecond laser, which can further reduce thermal damage and debris. Of course, other lasers capable of etching trenches can also be used.
[0024] In practical applications, after the first laser baffle is placed on the wafer surface, it can be automatically positioned and clamped together in a vacuum environment. At this time, the first transparent pattern on the first laser baffle corresponds exactly to the area where the chip trench is located. After the first laser baffle and the wafer are placed in a surface standard ultraviolet laser etching machine, the machine emits a laser for etching towards the first transparent pattern on the first laser baffle. This laser passes through the first transparent pattern and completes the etching between the chip areas of the wafer, thereby forming trenches. Figure 3 As shown.
[0025] It should be noted that the parameters of the etching trench of the standard ultraviolet laser etching machine include: linewidth of 20μm; line spacing of 4.064mm, which is the same as the chip edge length; depth between 50μm and 60μm; wavelength of 355nm; pulse width between 10ns and 30ns; repetition frequency between 50kHz and 200kHz; average power between 5W and 20W; single pulse energy between 10μJ and 50μJ; scanning speed between 100mm / s and 500mm / s; and a field lens of 120mm×120mm, which can cover the 5-inch wafer area.
[0026] It should be noted that the atmosphere used for etching the trenches is nitrogen or SF6 atmosphere; of course, the trenches can also be etched indoors or in a closed vacuum environment.
[0027] like Figure 2 As shown, the black lines on the first laser baffle are chromium-covered areas that cannot transmit laser light, while the white areas are transparent areas that can transmit laser light.
[0028] It should be noted that the present invention uses trenches to divide multiple chips on the wafer; that is, the trenches are the boundaries between the chips.
[0029] S102. A second laser baffle is placed on the wafer surface. The second laser baffle has a second light-transmitting pattern corresponding to the stepped structure. A laser for etching is emitted to the second laser baffle. After passing through the second light-transmitting pattern, the laser etches the wafer, thereby etching a stepped structure on the side of the chip area near the trench. The stepped structure is a transition structure between the mesa and the trench in the chip area. The linewidth of the second laser baffle is smaller than the linewidth of the first laser baffle.
[0030] It should be noted that the second laser baffle can be fabricated by forming a metallic chromium pattern on a quartz substrate. Specifically, a metallic chromium pattern is fabricated on an ultraviolet fused quartz substrate as a mask, closely attached to the wafer surface, and patterned etching is achieved under laser scanning. The entire process does not require consumables such as a photolithography cleanroom, photoresist, or developer. It should also be noted that the second laser can be an ultraviolet laser, or other lasers capable of etching stepped structures (shallow grooves).
[0031] In practical applications, after placing the second laser baffle on the surface of the etched trenched wafer, the second laser baffle and the wafer can be automatically positioned and clamped together in a vacuum environment. At this time, the second transparent pattern on the second laser baffle corresponds exactly to the area where the chip's stepped structure is located. After placing the second laser baffle and the etched trenched wafer into a surface standard ultraviolet laser etching machine, the surface standard ultraviolet laser etching machine emits a laser for etching onto the second transparent pattern on the second laser baffle. This laser passes through the second transparent pattern and completes the etching on the side of the chip area near the trench, thus forming a stepped structure, that is, forming a transition structure between the mesa and the trench in the chip area, such as... Figure 4 As shown.
[0032] It should be noted that the parameters of the etching stepped structure of the standard ultraviolet laser etching machine include: linewidth of 30μm; line spacing of 4.064mm, which is the same as the chip edge length; depth between 5μm and 10μm; laser wavelength of 355nm; pulse width between 10ns and 30ns; repetition frequency between 50kHz and 200kHz; average power between 5W and 20W; single pulse energy between 10μJ and 50μJ; scanning speed between 100mm / s and 500mm / s; and a field lens of 120mm×120mm, which can cover the 5-inch wafer area.
[0033] It should be noted that the atmosphere used when etching the stepped structure is nitrogen or SF6; of course, the stepped structure can also be etched indoors or in a closed vacuum environment.
[0034] It should be noted that the black lines on the second laser baffle are chromium-covered areas that are not transparent to laser light, while the white areas are transparent areas that are transparent to laser light.
[0035] It should be noted that the stepped structure includes a single-step structure or a multi-step structure; the depth of the stepped structure is between 5μm and 10μm, and the width is between 3μm and 10μm. That is, the depth of the stepped structure can be any value between 5μm and 10μm, for example, the depth can be 5μm, 8μm, or 10μm. The width of the stepped structure can be any value between 3μm and 10μm, for example, the width can be 3μm, 6μm, 8μm, or 10μm. This application does not impose any limitations on this.
[0036] It should be noted that this stepped structure can also be formed by directly ablating the trench edges with laser equipment. This involves fixing the wafer with the etched trenches onto a high-precision laser processing platform, setting a laser scanning path on the inner or outer side of the trench edge, aligning an optical microscope or coaxial vision system with the trench edge, setting the laser ablation parameters, and then starting the scanning ablation process to form a stepped structure on the side of the wafer.
[0037] It should be noted that this stepped structure can be continuous or discontinuous. Since this stepped structure is not part of the chip's PN junction effective region, minor damage such as glass gaps, incomplete glass filling, or minor impact damage at the interface between the chip's mesa and trench will not harm the chip's PN junction effective region. This improves the reliability of mesa-passivated chips.
[0038] It should be noted that the glass passivation layer subsequently grown using electrophoresis is relatively thick, especially at the corners of the chip mesa and trench, where the thicker glass extends beyond the plane of the chip mesa's soldering window. If the metal solder joint touches this glass passivation layer or multiple chips are stacked and connected in series, excessive stress will occur at the glass passivation layer, leading to packaging stress risks in the product. Therefore, to solve this problem, this invention proposes etching a stepped structure between the trench and the chip mesa. Since the plane of this stepped structure is lower than the plane of the chip mesa's soldering window, even if a passivation glass layer is applied to this stepped structure, it can be ensured that the glass passivation layer on the stepped structure will not be higher than the plane of the soldering window. In this way, the drawback of the thick glass layer deposited by electrophoresis is overcome.
[0039] In some embodiments, before trench etching, a water-soluble laser protective solution is applied to both the front and back sides of multiple chip areas of the wafer to capture slag and spatter generated by laser etching. The water-soluble laser protective solution is obtained by mixing water-soluble polymers, surfactants, defoamers, and various components in deionized water.
[0040] It should be noted that the water-soluble laser protective liquid of the present invention can be a water-based temporary protective coating, comprising: a water-soluble polymer, a surfactant, a defoamer, and deionized water; the water-soluble polymer is 5-15 parts by weight, the surfactant is 0.1-1 parts by weight, the defoamer is 0.01-0.1 parts by weight, and the deionized water is 60-90 parts by weight.
[0041] It should be noted that the water-soluble polymer can be polyvinyl alcohol (PVA), polyethylene glycol (PEG), or polyvinylpyrrolidone (PVP), primarily used to form a continuous film that can be dissolved in water. The surfactant can be a polyoxyethylene ether or sodium dodecyl sulfate, primarily used to reduce the surface tension of the water-soluble laser protective solution, thereby enabling the solution to be uniformly coated on the chip surface. The defoamer can be tributyl phosphate, primarily used to prevent the formation of bubbles during the coating process that could affect the protective effect.
[0042] It should be noted that the specific ratio of the water-soluble laser protective solution can be optimized and adjusted according to factors such as laser energy and chip size. After the water-soluble laser protective solution is coated on the front and back of the chip area at room temperature, it needs to be baked at 80℃-100℃ for 1-2 minutes to dry and form a film. After completing the two laser etching processes, it can be removed by rinsing with deionized water without affecting the chip's performance.
[0043] In some embodiments, after obtaining the stepped structure, the wafer is then subjected to mixed acid rinsing and RCA cleaning in sequence, and then the trenches, stepped structure and mesa of the chip area are subjected to in-situ selective scanning oxidation to obtain an oxide layer.
[0044] It should be noted that the RCA cleaning process is an existing cleaning process and will not be described in detail here. The mixed acid can be obtained by mixing hydrofluoric acid, nitric acid, and glacial acetic acid in a ratio of 5:3:3, or it can be obtained by mixing in other ratios.
[0045] In some embodiments, in-situ selective scanning oxidation is performed on the trenches, stepped structures, and mesas of the chip region to obtain an oxide layer, including: Selective laser scanning oxidation is performed on the bottom area of the trench, the area between the edge of the platform and the stepped structure, so that the first oxide layer is generated in situ in the bottom area of the trench, the area between the edge of the platform and the stepped structure. Laser scanning oxidation is performed on the welding window area of the worktable to generate a second oxide layer in the welding window area of the worktable.
[0046] It should be noted that the laser used for selective laser scanning oxidation can be a CO2 laser or a semiconductor-pumped solid-state laser.
[0047] In practical applications, the bottom area of the trench, the area between the edge of the platform and the stepped structure (such as...) Figure 5 The selective laser scanning oxidation process (in the green area) includes: First, the wafer after the stepped structure etching is subjected to RCA cleaning to obtain a clean wafer; then, the atmosphere in the ultraviolet laser equipment is switched to pure oxygen or dry compressed air, and the laser scanning parameters are set. The clean wafer is placed in the ultraviolet laser equipment, and selective scanning oxidation is performed on the bottom area of the trench and the area requiring a long oxide layer at the mesa edge (i.e., the area between the mesa edge and the stepped structure). This allows the first oxide layer to be generated in situ in the bottom area of the trench and the area between the mesa edge and the stepped structure. Figure 6 , 7 As shown. This first oxide layer has higher density and no pinhole defects compared to oxide layers prepared by traditional high-temperature furnace thermal oxidation processes.
[0048] In practical applications, laser scanning oxidation is performed on the welding window area of the worktable to make the welding window area (such as...) Figure 8 The process of generating the second oxide layer (in the red-lined area in the image) includes: placing a welding window laser baffle on a clean wafer and then placing it in an ultraviolet laser device. Since the welding window laser baffle has a third light-transmitting pattern corresponding to the chip welding window, the laser emitted by the ultraviolet laser device can pass through the third light-transmitting pattern to scan and oxidize the welding window area of the chip mesa, thereby forming the second oxide layer.
[0049] It should be noted that, as Figure 9 As shown, the black lines on the laser baffle of the welding window represent the chromium-covered area, which is impenetrable to the laser, while the white areas are transparent and allow the laser to pass through.
[0050] It should be noted that the thickness of the first oxide layer is greater than the thickness of the second oxide layer. In practical applications, the thickness of the first oxide layer is between 200nm and 1000nm, meaning it can be 200nm, 500nm, 700nm, 850nm, or 1000nm; the thickness of the second oxide layer is between 10nm and 100nm, meaning it can be 10nm, 60nm, 85nm, or 100nm. It should be noted that the first oxide layer is used for passivation protection, so it needs to have a certain thickness to achieve this passivation effect; the second oxide layer is used as a solder barrier, so its thickness only needs to serve as a solder resisting element and does not need to be too thick.
[0051] It should be noted that the parameters for selective laser scanning oxidation and laser scanning oxidation are the same, including: oxygen flow rate between 0.5 L / min and 3 L / min; chamber pressure can be between 0.1 MPa and 0.11 MPa to 0.15 MPa; laser scanning speed between 200 mm / s and 800 mm / s; and the number of scans between 1 and 5.
[0052] Traditional methods involve thermal oxidation of the entire silicon wafer surface followed by photolithography and selective wet etching to create the chip oxide layer. This process is complex and has a long production cycle. In contrast, this invention uses in-situ laser selective oxidation to automate the processing of the wafer oxide layer, eliminating the need for subsequent photolithography and selective wet etching steps, thereby reducing production time and costs.
[0053] In some embodiments, after obtaining the oxide layer, an electrophoretic solution is deposited in the unoxidized area of the wafer to obtain a glass passivation layer; the wafer is then subjected to surface metallization treatment to obtain a chip bonding metal layer.
[0054] In some embodiments, the process of depositing electrophoretic solution in the unoxidized regions of the wafer includes: placing the wafer in the electrophoretic solution, so that the electrophoretic solution is deposited on the unoxidized regions of the chip ladder structure and the unoxidized regions of the chip trenches (e.g., Figure 10 (The gray area shown) is used to perform glass sintering on the electrophoretically deposited wafer to obtain a glass passivation layer.
[0055] It should be noted that the electrophoresis solution is obtained by mixing glass slurry, silica nanoparticles, and deionized water; specifically, the electrophoresis solution is prepared by mixing glass slurry, silica nanoparticles, and deionized water in a weight ratio of 100:(0.5-5):(100-300). Of course, deionized water can be replaced with ethanol or isopropanol. The silica nanoparticles have a particle size between 10nm and 50nm, meaning the particle size can be 10nm, 20nm, 40nm, or 50nm. The glass slurry contains glass powder with a solid content between 5wt% and 15wt%, meaning the solid content of the glass powder can be 5wt%, 10wt%, or 15wt%.
[0056] In practical applications, a basket of wafers with pre-formed PN junctions is immersed in an electrophoresis bath. A DC voltage (20V-100V) is applied at 20℃-30℃, causing charged glass paste particles to selectively deposit on the exposed silicon surface (conductive region) requiring passivation, driven by the potential, without depositing on the laser-generated in-situ silicon dioxide insulating region. The electrophoresis time is 10s-60s. The electrophoretically deposited wafer is then removed and baked to obtain the glass passivation layer. It should be noted that this glass passivation layer is a dense SiO2 layer, eliminating the need for LTO deposition or additional PECVD deposition. This electrophoretic deposition process is simple, requiring no manual scraping or photolithography steps, eliminating organic residue issues, and facilitating mass production and automation with good consistency. Most importantly, this electrophoretic deposition method can save chip manufacturing time and shorten the chip production cycle.
[0057] This invention achieves glass passivation by depositing electrophoretic flux in the unoxidized regions of trenches and the unoxidized regions of a stepped structure. In other words, this invention can achieve highly efficient passivation with electrophoretic flux using very few process steps. Furthermore, the glass passivation layer formed after passivation by the electrophoretic flux of this invention is lower than the chip mesa, thus not affecting the flatness of the chip soldering window or the chip soldering quality. In addition, the glass layer within the trench is fully filled, preventing the formation of weak areas and ensuring that the chip will not be damaged during subsequent processes or packaging, thereby improving the chip packaging quality.
[0058] In some embodiments, the process of surface metallizing a wafer includes: surface metallizing the bonding windows of the wafer's mesa to obtain a chip bonding metal layer.
[0059] It should be noted that electroless nickel plating mainly involves the reduction and deposition of nickel ions through an autocatalytic reaction to form a nickel-phosphorus alloy coating. After nickel plating is completed, the deposited nickel powder can be instantly heated to a molten state using a laser and shaped, thereby achieving nickel sintering. After nickel sintering, hot nitric acid can be used to remove the nickel oxide produced during the sintering process, thus cleaning up impurities on the chip.
[0060] In practical applications, the surface metallization process for wafers includes: surface metallization using chemical plating and nickel sintering. Specifically, nickel plating (plating temperature between 90℃ and 100℃, plating time between 20s and 40s) is performed sequentially on both the front and back sides of the wafer. This is followed by nickel sintering (sintering temperature between 520℃ and 535℃, sintering time between 20min and 60min), nickel oxide removal (nickel oxide removal time is 10mins), and nickel plating (plating temperature between 90℃ and 100℃, nickel plating time between 20s and 40s), ultimately forming the chip bonding metal layer.
[0061] It should be noted that the thickness of the chip bonding metal layer is between 0.35μm and 0.65μm. That is to say, the thickness of the chip bonding metal layer can be 0.35μm, 0.50μm, 0.58μm or 0.65μm.
[0062] In some embodiments, before surface metallization, the wafer with the glass passivation layer is immersed in a dilute hydrofluoric acid solution for 1 minute to remove the second oxide layer in the welding window area of the mesa.
[0063] In practical applications, the dilute hydrofluoric acid solution is prepared by mixing hydrofluoric acid and deionized water at a volume ratio of 1:10. It is primarily used to remove the second oxide layer from the surface of the welding window on the mezzanine, while the first oxide layer remains in the bottom area of the trench and between the mezzanine edge and the stepped structure. Since the welding window area of the mezzanine only undergoes one laser scanning oxidation to form the second oxide layer, when the welding window needs to be exposed, only the second oxide layer needs to be removed; no additional secondary photolithography is required to form the welding window.
[0064] Table 1 shows the comparison results between traditional chip processing methods and the laser processing method of this invention:
[0065]
[0066]
[0067] Table 1 shows steps 1-4 of the laser processing method of the present invention, which are existing processing steps and will not be repeated here. As can be seen from Table 1, the laser processing method of the present invention reduces the main processes to only 17 steps, achieving a reduction in production steps and a shorter cycle time compared to traditional processing methods.
[0068] This invention provides a laser processing method for a mesa glass passivated chip. The method includes: placing a first laser baffle on the surface of a wafer, wherein multiple chip regions of the wafer have formed PN junctions, and the first laser baffle has a first light-transmitting pattern corresponding to chip trenches; emitting an etching laser onto the first laser baffle, the laser passing through the first light-transmitting pattern and etching the wafer to form trenches between the chip regions of the wafer; placing a second laser baffle on the surface of the wafer, the second laser baffle having a second light-transmitting pattern corresponding to a stepped structure; emitting an etching laser onto the second laser baffle, the laser passing through the second light-transmitting pattern and etching the wafer to form a stepped structure on the side of the chip region near the trench; the stepped structure is a transition structure between the mesa and the trench of the chip region; wherein the linewidth of the second laser baffle is smaller than the linewidth of the first laser baffle. This invention employs laser baffle pattern transfer and laser grooving to replace traditional photolithography and wet etching, eliminating the need for a yellow light cleanroom and resolving the reliance on yellow light areas. It uses a water-soluble laser protective solution to capture slag and spatter generated during laser etching, protecting the mask and chip surface and solving the problem of laser processing debris contaminating the chip. It utilizes an in-situ selective oxidation laser scheme, generating SiO2 in situ in areas requiring a long oxide layer after grooving, eliminating the need for additional LTO or PECVD equipment. It achieves one-time glass passivation layer formation via electrophoretic deposition, resolving the redundancy issue of multiple glass sintering processes. It uses a dilute hydrofluoric acid solution to etch away the oxide layer in the mesa welding window area, eliminating the need for secondary photolithography. The stepped structure ensures that the height of the electrophoretically grown glass passivation layer does not exceed the horizontal plane of the mesa where the chip welding window is located, avoiding welding stress issues caused by solder joints contacting the glass during welding. This is packaging-friendly, resulting in higher product reliability. Furthermore, the chip of this invention is more suitable for large solder joint wire bonding. This invention achieves a reduction in production steps and a shorter cycle by using laser baffle pattern transfer, laser grooving, laser in-situ oxidation, electrophoretic one-time glass passivation, and glass slurry doped with nano-SiO2 to form a glass passivation layer. Specifically, by reducing the photolithography and wet trench etching steps, the main processes are reduced to only 17 steps, the theoretical cycle is shortened from 9.5 days to 5.5-6.5 days, and the actual production cycle is shortened from 19 days to 11-12.5 days.
[0069] Please refer to Figure 11 , Figure 11 This is a schematic diagram of the structure of a mesa glass passivation chip according to one embodiment, as shown below. Figure 11 As shown, the passivated glass chip includes: Substrate; A first type semiconductor layer is stacked on the substrate; A heavily doped type II semiconductor layer is stacked on the lower layer of the substrate; The first type of semiconductor layer has trenches on its side, and a stepped structure is provided at the junction of the first type of semiconductor layer and the trenches; wherein the trenches and the stepped structure are obtained by laser processing method as described above; Both the first type semiconductor layer and the heavily doped second type semiconductor layer are covered with a metallization layer.
[0070] This invention provides a mesa glass passivation chip, comprising: a substrate; a first type semiconductor layer stacked on the upper layer of the substrate; a heavily doped second type semiconductor layer stacked on the lower layer of the substrate; trenches are provided on the sides of the first type semiconductor layer, and a stepped structure is provided at the junction of the first type semiconductor layer and the trenches; wherein the trenches and the stepped structure are processed by the laser processing method described above; both the first type semiconductor layer and the heavily doped second type semiconductor layer are covered with a metallization layer.
[0071] This document describes various exemplary embodiments with reference to them. However, those skilled in the art will recognize that changes and modifications can be made to the exemplary embodiments without departing from the scope of this document. For example, various operational steps and components for performing operational steps can be implemented in different ways depending on the specific application or considering any number of cost functions associated with the operation of the system (e.g., one or more steps can be deleted, modified, or combined with other steps).
[0072] While the principles herein have been illustrated in various embodiments, numerous modifications to the structures, arrangements, proportions, elements, materials, and components, particularly suited to specific environments and operational requirements, may be used without departing from the principles and scope of this disclosure. These modifications and other alterations or alterations will be included within the scope of this document. Those skilled in the art will recognize that many changes can be made to the details of the above embodiments without departing from the fundamental principles of the invention.
Claims
1. A method of laser processing of a mesa glass passivated chip, characterized in that, The method includes: A first laser baffle is placed on the surface of a wafer, where multiple chip regions of the wafer have formed PN junctions. The first laser baffle has a first light-transmitting pattern corresponding to the chip trenches. A laser for etching is emitted to the first laser baffle, and the laser etches the wafer after passing through the first light-transmitting pattern, thereby etching trenches between the chip regions of the wafer. A second laser baffle is placed on the wafer surface, and the second laser baffle has a second light-transmitting pattern corresponding to the stepped structure. A laser for etching is emitted into the second laser baffle, and the laser passes through the second light-transmitting pattern to etch the wafer, thereby etching a stepped structure on the side of the chip region near the trench. The stepped structure is a transition structure between the mesa of the chip region and the trench. The linewidth of the second laser baffle is smaller than the linewidth of the first laser baffle.
2. The method of claim 1, wherein, The front and back sides of multiple chip areas of the wafer are coated with a water-soluble laser protective liquid to capture slag and spatter generated by laser etching; the water-soluble laser protective liquid is obtained by mixing water-soluble polymers, surfactants, defoamers and various components of deionized water.
3. The method of claim 1, wherein, The method further includes: In-situ selective scanning oxidation is performed on the trenches, the stepped structure, and the mesa of the chip region to obtain an oxide layer.
4. The method of claim 3, wherein, The oxide layer includes a first oxide layer and a second oxide layer; the thickness of the first oxide layer is greater than the thickness of the second oxide layer. In-situ selective scanning oxidation is performed on the trenches, the stepped structure, and the mesa of the chip region to obtain an oxide layer, including: Selective laser scanning oxidation is performed on the bottom region of the trench, the region between the edge of the platform and the stepped structure, so that the first oxide layer is generated in situ in the bottom region of the trench, the region between the edge of the platform and the stepped structure. Laser scanning oxidation is performed on the welding window area of the table surface to generate the second oxide layer in the welding window area of the table surface.
5. The method of claim 4, wherein, The atmosphere used for in-situ selective scanning oxidation includes pure oxygen or dry compressed air.
6. The method of claim 3, wherein, The method further includes: After obtaining the oxide layer, an electrophoretic solution is deposited in the unoxidized area of the wafer to obtain a glass passivation layer; The wafer is subjected to surface metallization treatment to obtain a chip bonding metal layer.
7. The method of claim 6, wherein, The deposition of an electrophoretic solution in the unoxidized region of the wafer to obtain a glass passivation layer includes: The wafer is placed in the electrophoretic solution, which is then deposited on the non-oxidized regions of the chip stepped structure and the chip trenches, respectively. The electrophoretic solution is obtained by mixing glass paste, silica nanoparticles, and deionized water. The silica nanoparticles have a particle size between 10 nm and 50 nm. The wafer after electrophoretic deposition is subjected to glass sintering to obtain the glass passivation layer.
8. The method of claim 4 or 5, wherein, The method further includes: The wafer is placed in a dilute hydrofluoric acid solution to remove the second oxide layer in the welding window area of the mesa.
9. The method of claim 6, wherein, The process of performing surface metallization on the wafer to obtain a chip bonding metal layer includes: The welding window of the mesa on the wafer is subjected to surface metallization treatment to obtain the chip welding metal layer.
10. A mesa glass passivated chip, characterized by, include: Substrate; A first type semiconductor layer is stacked on the substrate; A heavily doped type II semiconductor layer is stacked on the lower layer of the substrate; The first type of semiconductor layer has a trench on its side, and a stepped structure is provided at the junction of the first type of semiconductor layer and the trench; wherein the trench and the stepped structure are processed by the laser processing method as described in claim 1. Both the first type semiconductor layer and the heavily doped second type semiconductor layer are covered with a metallization layer.