A semiconductor device and a semiconductor wafer
By employing a silicon carbide substrate and a 4° off-axis growth technique in trench gate MOSFETs, trench sidewalls with (2-1-10) or (-2110) crystal planes are formed, solving the problem of low carrier mobility and achieving a reduction in on-resistance and an improvement in device performance.
Patent Information
- Application Number
- CN202510681300.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-23
- Publication Date
- 2026-11-24
AI Technical Summary
The carrier mobility of existing trench gate MOSFETs still needs to be improved, resulting in high on-resistance, which makes it difficult to meet the miniaturization and high efficiency requirements of modern electronic devices.
Using a silicon carbide substrate and introducing a 4° off-axis growth technique, the trench sidewalls of the epitaxial layer are formed as (2-1-10) or (-2110) crystal planes. Combined with an optimized gate structure, the carrier mobility is improved.
It significantly improves carrier mobility, reduces the on-resistance of semiconductor devices, and enhances device performance and power density, making it suitable for high-frequency and high-power applications.
Smart Images

Figure CN123164801A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the semiconductor field, and in particular to a semiconductor device and a semiconductor wafer. Background Technology
[0002] To further expand the application scenarios of semiconductor devices, reducing the on-resistance of semiconductor devices has become a research hotspot.
[0003] Taking MOSFET (silicon carbide metal-oxide-semiconductor field-effect transistor) as an example, the MOSFET structure generally includes planar gate MOSFET and trench gate MOSFET. Among them, trench gate MOSFET (or trench gate MOSFET) has advantages such as high cell density and junctionless field-effect region (JFET), which can effectively reduce the on-resistance and become an ideal structural choice.
[0004] In MOSFET design, improving carrier mobility is one of the key ways to reduce device on-resistance and improve device performance. However, the mobility of existing trench gate MOSFETs still needs to be improved. Summary of the Invention
[0005] To address the aforementioned issues, this application provides a semiconductor device and a semiconductor wafer that can effectively improve carrier mobility, thereby mitigating the problem of high on-resistance in existing semiconductor devices.
[0006] To address the aforementioned problems, the first technical solution provided in this application is: to provide a semiconductor device, the semiconductor device comprising a plurality of cells, each cell comprising:
[0007] Substrate;
[0008] An epitaxial layer is disposed on the epitaxial surface of the substrate, the epitaxial layer having a trench extending from the surface of the epitaxial layer away from the substrate toward the substrate; wherein, one sidewall of the trench is a (2-1-10) crystal plane or a (-2110) crystal plane;
[0009] A gate structure is disposed within the trench.
[0010] To address the aforementioned issues, the second technical solution provided in this application is: to provide a semiconductor wafer having a main positioning flat edge, comprising: a plurality of semiconductor devices; wherein the semiconductor devices have trenches;
[0011] The angle between the extension direction of the groove and the positioning flat edge is 25-35 degrees.
[0012] The beneficial effect of this application is that, unlike the prior art, the semiconductor device provided in this application includes a plurality of cells, each cell including a substrate, an epitaxial layer, and a gate structure. The epitaxial layer is disposed on one surface of the substrate and has trenches extending from the surface of the epitaxial layer away from the substrate towards the substrate. One sidewall of the trench is a (2-1-10) crystal plane or a (-2110) crystal plane. The gate structure is disposed within the trench. Specifically, the semiconductor device provided in this application is a trench gate semiconductor device, which has a higher carrier mobility, thereby further reducing the on-resistance of the semiconductor device. Attached Figure Description
[0013] To more clearly illustrate the technical solutions in the embodiments of this application, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort, wherein:
[0014] Figure 1 This is a schematic diagram of the cell structure of a semiconductor device provided in an embodiment of this application;
[0015] Figure 2 A schematic diagram of the crystal axis of a wafer at different rotation angles;
[0016] Figure 3 The diagram shows the corresponding relationship between the transconductance of the trench sidewalls under different crystal planes when VGS is 18V.
[0017] Figure 4 Electron micrograph of the gate dielectric layer under the (2-1-10) crystal plane of the sidewall surface of the trench provided in an embodiment of this application;
[0018] Figure 5 Electron micrograph of the gate dielectric layer under the (11-20) crystal plane of the sidewall surface of the trench provided in an embodiment of this application;
[0019] Figure 6 A diagram showing the positional relationship between a trench with a (2-1-10) crystal plane and an ideal crystal plane, fabricated on a substrate with a 4° off-axis angle, provided as an embodiment of this application;
[0020] Figure 7 The diagram shows the positional relationship between the trench with (11-20) crystal planes and the ideal crystal planes prepared on a substrate with a 4° off-axis angle.
[0021] Figure 8 This is a schematic diagram of the structure of a semiconductor wafer provided in an embodiment of this application.
[0022] Label Explanation:
[0023] Semiconductor wafers - 10000; Semiconductor devices - 1000; Cells - 100;
[0024] Substrate-10; Epitaxial layer-20; Gate structure-30; Gate dielectric layer-31; Gate electrode-32; Doped region-40; First doped region-41; Second doped region-42; Third doped region-43; Source structure-50; Drain structure-60; Insulating layer-70;
[0025] Groove - G; Main positioning flat edge - L1; Second positioning flat edge - L2. Detailed Implementation
[0026] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of this application, and not all of the embodiments. Based on the embodiments of this application, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of this application.
[0027] The terms "first," "second," and "third" in this application are for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Therefore, a feature defined as "first," "second," or "third" may explicitly or implicitly include at least one of that feature. In the description of this application, "multiple" means at least two, such as two, three, etc., unless otherwise explicitly specified. All directional indications (such as up, down, left, right, front, back, etc.) in the embodiments of this application are only used to explain the relative positional relationships and movements between components in a specific orientation (as shown in the figures). If the specific orientation changes, the directional indications also change accordingly. Furthermore, the terms "comprising" and "having," and any variations thereof, are intended to cover non-exclusive inclusion. For example, a process, method, system, product, or device that includes a series of steps or units is not limited to the listed steps or units, but may optionally include steps or units not listed, or may optionally include other steps or units inherent to these processes, methods, products, or devices.
[0028] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.
[0029] In the description of the embodiments in this application, the term "and / or" is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, and B existing alone. Additionally, the character " / " in this document generally indicates that the preceding and following related objects have an "or" relationship.
[0030] In the description of the embodiments of this application, the term "multiple" refers to two or more (including two).
[0031] As a type of semiconductor device, MOSFETs generally include planar gate MOSFETs and trench gate MOSFETs.
[0032] From a structural perspective, in a planar gate MOSFET, the gate is located on the surface of the epitaxial layer, with its source, drain, and gate on the same plane, and the conductive channels are distributed laterally along the surface of the epitaxial layer. In contrast, a trench gate MOSFET uses photolithography and etching processes to etch deep trenches perpendicular to the surface of the epitaxial layer, placing the gate within the trench. This makes the conductive channels vertical, significantly shortening the carrier transport path. This vertical structural design allows for the integration of more cells within a unit chip area, achieving high cell density. The parallel connection of more cells effectively distributes current, further reducing on-resistance and improving the device's current carrying capacity.
[0033] Regarding on-resistance, planar gate MOSFETs have a junction field-effect region (JFET) between their source and drain, which generates additional resistance and increases conduction losses. In contrast, trench gate MOSFETs, with their unique vertical channel design, fundamentally eliminate the JFET region, reducing parasitic resistance and allowing for smoother current conduction, resulting in a significant reduction in on-resistance. Experimental data shows that, under the same voltage and current conditions, the on-resistance of trench gate MOSFETs can be reduced by 30%-50% compared to planar gate MOSFETs, significantly improving power conversion efficiency.
[0034] Extending its performance advantages, trench gate MOSFETs not only reduce on-resistance, but their structural optimization also brings other performance improvements. For example, due to the reduction of parasitic capacitance (Cgd) between the gate and drain, the switching speed of the device is improved and the switching loss is reduced, making it suitable for high-frequency operating scenarios. At the same time, the high cell density and vertical structure also help to improve the power density of the device, enabling the chip to achieve higher power handling capabilities in a smaller volume, meeting the miniaturization and high efficiency requirements of modern electronic devices.
[0035] These characteristics make trench gate MOSFETs a highly favored device structure in fields with stringent requirements for power efficiency and space layout, such as switching power supplies, motor drives, and new energy vehicles.
[0036] Given the advantages of trench gate MOSFETs mentioned above, this application takes a trench gate MOSFET as an example of a semiconductor device.
[0037] In related technologies, trench gate MOSFETs often use (11-20) or (1-100) crystal planes as trench sidewalls (or channel planes). Although the mobility of these trench sidewalls is about 30% higher than that of the (0001) plane, their physical limits have not yet been broken. Furthermore, although the channel crystal plane characteristics of trench gate MOSFETs have a significant impact on their performance, research on the correlation mechanism between crystal planes and mobility is still limited in existing technologies. On the one hand, research on the correlation mechanism between crystal planes and mobility requires combining multiple disciplines such as crystal growth, material characterization, and device simulation, which is technically challenging and costly. On the other hand, traditional R&D focuses primarily on device structure optimization and process improvement, with insufficient attention paid to the intrinsic characteristics of crystal planes, resulting in slow progress in exploring different crystal plane-mobility correlation mechanisms to improve device mobility.
[0038] To further improve the carrier mobility of trench gate MOSFETs and reduce the on-resistance of the device, this application provides a semiconductor device comprising a plurality of cells 100, see [link to relevant documentation]. Figure 1 , Figure 1 This is a schematic diagram of the structure of a cell of a semiconductor device provided in an embodiment of this application. Each cell 100 includes a substrate 10, an epitaxial layer 20, a gate structure 30, a source structure 50, and a drain structure 60.
[0039] The substrate 10 is made of materials including, but not limited to, silicon, silicon carbide, or sapphire.
[0040] Compared to silicon or sapphire substrates, silicon carbide substrates have wide bandgap characteristics, high thermal conductivity, and high carrier saturation velocity, which gives them advantages such as reducing device on-resistance, adapting to high-temperature and high-power scenarios, improving switching speed, and reducing high-frequency losses.
[0041] Therefore, in this embodiment, the substrate 10 is a silicon carbide substrate, and the crystal plane of the substrate 10 is a standard SiC(0001) crystal plane.
[0042] See Figure 2 , Figure 2 This is a schematic diagram of the crystal axis of a wafer at different rotation angles, where the arrows point in the direction of the crystal axis, and the extension direction of the trench G is perpendicular to the direction of the crystal axis.
[0043] In one embodiment, the substrate 10 has a main positioning flat edge L1 and a second positioning flat edge L2, the main positioning flat edge L1 being formed along the [11-20] crystal orientation and the second positioning flat edge L2 being formed along the [1-100] crystal orientation.
[0044] In this context, a crystal plane is a plane in a crystal composed of atoms, consisting of a set of parallel and equidistant atomic layers. In this application, crystal planes are indicated by parentheses.
[0045] Crystal orientation is the direction in which atoms in a crystal are arranged, determined by the line connecting any two atoms in the crystal lattice, reflecting the periodicity and symmetry of the crystal in that direction. In this application, crystal orientation is indicated by square brackets. In a cubic crystal system, the crystal orientation is perpendicular to the crystal plane.
[0046] The epitaxial layer 20 is disposed on the epitaxial surface of the substrate 10 and is formed by epitaxial growth of the substrate 10.
[0047] In one embodiment, silicon carbide homoepitaxial growth is performed on substrate 10 with the
[0001] crystal axis tilted at 4° towards the [-1-120] crystal orientation, introducing a 4° off-axis pointing towards the [11-20] crystal orientation. That is, the epitaxial layer 20 is a SiC epitaxial layer with a
[0001] crystal axis and has a 4° off-axis angle. The main purpose of introducing the 4° off-axis growth is to improve the quality of the epitaxial layer 20.
[0048] Specifically, when the substrate 10 is tilted along the [-1-120] crystal orientation, periodic atomic steps are formed on the surface, with the step direction aligned with the tilted crystal orientation. During vapor phase epitaxy (such as CVD), Si / C atoms preferentially adsorb at the step edges and grow layer by layer along the step direction (rather than random nucleation), thereby reducing microtubes and helical dislocations and improving surface smoothness. Furthermore, the higher surface energy at the step edges of the tilted substrate 10 is beneficial for dopant adsorption and diffusion.
[0049] In the epitaxial growth of silicon carbide, precise control of the growth direction can reduce the generation of defects. Furthermore, 4° off-axis growth helps to control the deposition pattern of atoms, resulting in a more uniform and stable epitaxial layer 20 in terms of crystal structure and electrical properties.
[0050] Furthermore, the epitaxial layer 20 has a trench G that extends from the surface of the epitaxial layer 20 away from the substrate 10 toward the substrate 10. A gate structure 30 is disposed in the trench G and includes a gate dielectric layer 31 and a gate electrode 32, thereby forming a trench gate MOSFET.
[0051] The trench G has a sidewall surface. In this embodiment, one sidewall surface of the trench G is a (2-1-10) crystal plane or a (-2110) crystal plane.
[0052] In a test fabrication, this application fabricates multiple epitaxial wafers by performing homoepitaxial growth of silicon carbide on a substrate 10 with a 4° offset, using the (1-100) plane as a reference. After ion doping, the multiple epitaxial wafers are sequentially rotated counterclockwise at 30° intervals to etch trench G, resulting in multiple epitaxial wafers with different channel crystal planes (see [link to relevant documentation]). Figure 2 Then, the gate structure 30, source structure 50 and drain structure 60 are fabricated to precisely construct trench gate MOSFETs with different channel crystal planes.
[0053] A voltage of 0-30V is applied to the gate structure 30 of each trench gate MOSFET, and a voltage of 0.1V is applied to the source structure 50 and the drain structure 60 to generate source-drain current (IDS). See [link to relevant documentation]. Figure 3 , Figure 3 This is a graph showing the transconductance of the trench sidewalls under different crystal planes at a VGS of 18V. Transconductance g M It is extracted from the IDS-VGS curve of the test device, and the specific calculation formula is as follows: Depend on Figure 3 It can be seen that trench gate MOSFETs located on the (2-1-10) and (-2110) crystal planes have the highest g M .
[0054] According to the mobility calculation formula:
[0055] μ FE =(L * g M (V G )) / (C ox *W*V DS (1)
[0056] Where, μ FE Let L be the mobility, L be the channel length, and g be the channel length. M For transconductance, C ox The capacitance per unit area of the gate dielectric layer, W is the channel width, and V is the capacitance per unit area of the gate dielectric layer. DS This is the source-drain voltage.
[0057] Based on the above formula (1), the trench gate MOSFET located on the (2-1-10) crystal plane and the (-2110) crystal plane has the highest mobility. FE It is approximately 65 cm²V⁻¹s⁻¹, which is about 14% higher than the mobility of trench gate MOSFETs with (11-20) crystal planes.
[0058] The anisotropy of mobility in trench gate MOSFETs is mainly due to two factors:
[0059] First, the thickness of the gate dielectric layer 31 on the sidewalls of trench G is different, see [reference]. Figure 4 and Figure 5 , Figure 4 Electron micrograph of the gate dielectric layer under the (2-1-10) crystal plane of the sidewall surface of the trench provided in an embodiment of this application; Figure 5 The image shows an electron microscope (EM) image of the gate dielectric layer on the (11-20) crystal plane of the sidewall of the trench provided in an embodiment of this application. The thickness of the gate dielectric layer 31 grown on the two crystal planes perpendicular to the C-axis was measured by scanning electron microscopy (SEM). Therefore, it can be concluded that the sidewall of the trench G in this application is a (2-1-10) crystal plane or a (-2110) crystal plane. The reason for the higher carrier mobility is not due to the different thickness of the gate dielectric layer 31.
[0060] Second, the tilt angle of the sidewalls of trench G causes a difference from the ideal crystal plane. See also Figure 6 and Figure 7 , Figure 6 A diagram showing the positional relationship between a trench with a (2-1-10) crystal plane and an ideal crystal plane, fabricated on a substrate with a 4° off-axis angle, provided as an embodiment of this application; Figure 7 The diagram shows the positional relationship between a trench with a (11-20) crystal plane fabricated on a substrate with a 4° off-axis angle and the ideal crystal plane. Since the actual device is fabricated on a substrate 10 with a 4° off-axis angle, the angle of the trench G fabricated by the process is approximately 87°. It can be observed that the (-1-120) crystal plane has the greatest difference from the ideal crystal plane, resulting in a decrease in mobility at this plane. This application adjusts the etching angle of the trench G to minimize the difference between the (2-1-10) crystal plane and the ideal crystal plane. This allows the carriers on this crystal plane to have a smaller effective mass, thus achieving a higher mobility.
[0061] As can be seen from the above, the semiconductor device provided in this application is a trench gate semiconductor device, and further, one sidewall of the trench G is configured as a (2-1-10) crystal plane or a (-2110) crystal plane. Compared with the existing sidewall crystal planes of the trench G, the (2-1-10) crystal plane and the (-2110) crystal plane have higher carrier mobility, thereby further reducing the on-resistance of the semiconductor device.
[0062] In one embodiment, the trench G has two opposing sidewalls, and the two sidewalls of the trench G are symmetrically arranged. Therefore, if one sidewall of the trench G is a (2-1-10) crystal plane, the other sidewall is a (-2110) crystal plane. Alternatively, if one sidewall of the trench G is a (-2110) crystal plane, the other sidewall is a (2-1-10) crystal plane.
[0063] Thus, both opposite sidewalls of trench G have higher carrier mobility, thereby further reducing the on-resistance of semiconductor devices.
[0064] See Figure 1 In some embodiments, the included angle α1 between the sidewall of the trench G and the surface of the substrate 10 ranges from 86° to 90°. For example, the included angle α1 between the sidewall of the trench G and the surface of the substrate 10 is 86°; or, the included angle α1 between the sidewall of the trench G and the surface of the substrate 10 is 87°; or, the included angle α1 between the sidewall of the trench G and the surface of the substrate 10 is 90°; no limitation is made here.
[0065] Specifically, the near-vertical (86°-90°) sidewalls of the G-groove significantly simplify the orientation control in the etching process, avoiding complex ion beam angle adjustments and multiple etching corrections required due to excessive sidewall tilt, thereby reducing equipment setup costs and process complexity. Simultaneously, this angle range provides ample tolerance for process fluctuations, avoiding cost losses due to rework caused by exceeding tolerances, and providing reliable process margins for large-scale production.
[0066] Please continue reading Figure 1 In some embodiments, the width W of the bottom wall surface of the trench G ranges from 0.3 to 0.6 μm. For example, the width W of the bottom wall surface of the trench G ranges from 0.3 μm; or, the width W of the bottom wall surface of the trench G ranges from 0.4 μm; or, the width W of the bottom wall surface of the trench G ranges from 0.6 μm. No limitation is made here.
[0067] In some embodiments, the depth H of the trench G ranges from 0.6 to 2.0 μm. For example, the depth H of the trench G ranges from 0.6 μm; or, the depth H of the trench G ranges from 1.0 μm; or, the depth H of the trench G ranges from 1.5 μm; or, the depth H of the trench G ranges from 2.0 μm. No limitation is made here.
[0068] Specifically, the width W of the bottom wall of the trench G and the depth H of the trench G are key parameters affecting device performance. If the width W is too narrow (≤0.3μm), the channel cross-sectional area decreases, the on-resistance increases significantly, leading to increased device heating, which may cause thermal failure, especially in high-current scenarios. If the width W is too wide (≥0.6μm), the cell density per unit area decreases, requiring an increase in chip area to maintain current carrying capacity, resulting in increased cost; at the same time, a wide trench G may introduce edge electric field concentration, reducing breakdown voltage.
[0069] If the depth H is insufficient (≤0.6μm), the trench G cannot penetrate the doped region 40 in the epitaxial layer 20, resulting in an excessively short PN junction spacing between the drain structure 60 and the source structure 50, which easily leads to breakdown. If the depth H is too large (≥2.0μm), the increased etching depth will cause the sidewall damage layer to thicken, the interface trap density to increase, and the channel mobility to decrease; at the same time, the parasitic capacitance (Cgd) will increase, and the switching loss will increase.
[0070] The gate dielectric layer 31 is disposed on the trench wall (including the bottom wall and the side wall) of the trench G, and the gate dielectric layer 31 forms a receiving groove; the gate electrode 32 is disposed in the receiving groove.
[0071] The material of the gate dielectric layer 31 includes, but is not limited to, silicon dioxide, and the material of the gate electrode 32 includes, but is not limited to, polysilicon, conductive metal, etc.
[0072] Specifically, the gate dielectric layer 31 is used to prevent the gate electrode 32 from directly contacting the epitaxial layer 20 (or semiconductor channel) and causing a short circuit, and the accommodating trench defines the position of the gate electrode 32 to avoid channel inhomogeneity caused by electrode offset.
[0073] In one embodiment, the thickness of the gate dielectric layer 31 between the gate electrode 32 and the trench wall of the trench G ranges from 35 to 70 nm. For example, the thickness of the gate dielectric layer 31 between the gate electrode 32 and the trench wall of the trench G is 35 nm; or, the thickness of the gate dielectric layer 31 between the gate electrode 32 and the trench wall of the trench G is 45 nm; or, the thickness of the gate dielectric layer 31 between the gate electrode 32 and the trench wall of the trench G is 55 nm; or, the thickness of the gate dielectric layer 31 between the gate electrode 32 and the trench wall of the trench G is 75 nm. No limitation is made here.
[0074] Specifically, if the thickness of the gate dielectric layer 31 is insufficient (≤35nm), it is prone to breakdown, affecting the reliability of the device; if the thickness of the gate dielectric layer 31 is too large (≥70nm), the gate capacitance decreases significantly, requiring a higher gate voltage to open the channel and increase the driving power; at the same time, the channel control capability is weakened and the on-resistance increases.
[0075] Please continue reading Figure 1 Furthermore, each cell 100 also includes a doped region 40, which extends from the surface of the epitaxial layer 20 away from the substrate 10 toward the substrate 10, and the depth of the doped region 40 is less than or equal to the depth of the trench G.
[0076] The doped region 40 includes a first doped region 41, a second doped region 42, and a third doped region 43. The first doped region 41 extends from the surface of the epitaxial layer 20 away from the substrate 10 toward the substrate 10, and one side of the first doped region 41 contacts the gate structure 30. The first doped region 41 has the same conductivity type as the epitaxial layer 20, for example, N-type. The second doped region 42 extends from the surface of the epitaxial layer 20 away from the substrate 10 toward the substrate 10, and the second doped region 42 contacts the side of the first doped region 41 away from the gate structure 30. The second doped region 42 has a different conductivity type than the epitaxial layer 20, for example, P-type. The third doped region 43 is located below and in contact with the first doped region 41 and the second doped region 42. The third doped region 43 has a different conductivity type than the epitaxial layer 20, for example, P-type, and the ion doping concentration of the third doped region 43 is lower than that of the second doped region 42. The device channel is formed in the region of the third doped region 43 near the gate structure 30.
[0077] In one embodiment, the ion doping concentration of the first doped region 41 is less than 1E15cm. -2 The implantation depth is 0.2-0.3 μm. The ion doping concentration of the second doped region 42 is lower than 1E15cm. -2 The implantation depth is 0.2-0.3 μm. The ion doping concentration in the third doped region 43 is lower than 5E14cm. -2 The injection depth is 0.4-0.7μm.
[0078] Please continue reading Figure 1 The drain structure 60 is formed on the surface of the substrate 10 away from the epitaxial layer 20, and the source structure 50 is formed on the first doped region 41 and the second doped region 42. The source structure 50 is electrically connected to the first doped region 41 and the second doped region 42 through an ohmic contact metal. An insulating layer 70 is also covered on the gate structure 30, which is used to insulate the gate structure 30 from the source structure 50.
[0079] Specifically, the semiconductor device provided in this application is a trench gate semiconductor device, and one sidewall of the trench G is further configured as a (2-1-10) crystal plane or a (-2110) crystal plane. Compared with the existing sidewall crystal planes of the trench G, the (2-1-10) crystal plane and the (-2110) crystal plane have higher carrier mobility, thereby further reducing the on-resistance of the semiconductor device.
[0080] See Figure 8 , Figure 8 This is a schematic diagram of the structure of a semiconductor wafer provided in an embodiment of this application.
[0081] This application also provides a semiconductor wafer 10000, including a plurality of semiconductor devices 1000; each semiconductor device 1000 has a trench G. The semiconductor device 1000 can be any of the semiconductor devices provided in the above embodiments.
[0082] In one embodiment, the semiconductor wafer 10000 is a SiC (0001) wafer, wherein a SiC (0001) wafer refers to a wafer of silicon carbide material with a (0001) crystal plane orientation, where the (0001) crystal plane orientation indicates that the atomic arrangement direction of the crystal plane is consistent with the c-axis direction of the crystal. The outermost surface of 4H-SiC, which is completely covered by Si atoms, is called the (0001) crystal plane. The epitaxial layer 20 in the semiconductor wafer 10000 is formed by epitaxial growth of the (0001) crystal plane of the substrate.
[0083] The semiconductor wafer has several positioning flat edges, including at least a main positioning flat edge L1 formed along the [11-20] crystal orientation. The angle α2 between the extension direction X of the trench G and the main positioning flat edge L1 is 25-35 degrees. For example, the angle α2 between the extension direction X of the trench G and the main positioning flat edge L1 is 25, 30, or 35 degrees, etc., and is not limited here.
[0084] Specifically, by setting the angle α2 between the extension direction X of the trench G and the main positioning flat edge L1 to 25-35 degrees, the two sidewalls of the trench G are respectively the (2-1-10) crystal plane and the (-2110) crystal plane. As can be seen from the above, the (2-1-10) crystal plane and the (-2110) crystal plane have higher carrier mobility than the existing sidewall crystal planes of the trench G, thereby further reducing the on-resistance of the semiconductor device.
[0085] In one embodiment, a plurality of semiconductor devices 1000 are arranged in an array, with the row direction parallel to the extension direction of the trench G.
[0086] Specifically, the above layout method can increase the density of semiconductor devices per unit area and facilitate standardized production.
[0087] The above are merely embodiments of this application and do not limit the scope of this patent application. Any equivalent structural or procedural changes made using the content of this application's specification and drawings, or direct or indirect applications in other related technical fields, are similarly included within the scope of patent protection of this application.
Claims
1. A semiconductor device, characterized by, The semiconductor device includes a plurality of cells, each cell comprising: Substrate; An epitaxial layer is disposed on the epitaxial surface of the substrate, the epitaxial layer having a trench extending from the surface of the epitaxial layer away from the substrate toward the substrate; wherein, one sidewall of the trench is a (2-1-10) crystal plane or a (-2110) crystal plane; A gate structure is disposed within the trench.
2. The semiconductor device according to claim 1, wherein The angle between the sidewall of the trench and the epitaxial surface of the substrate ranges from 86° to 90°.
3. The semiconductor device of claim 2, wherein, The width of the bottom wall of the trench ranges from 0.3 to 0.6 μm; and / or, The depth of the trench ranges from 0.6 to 2.0 μm.
4. The semiconductor device of claim 1, wherein The epitaxial layer has an off-axis angle of 4°.
5. The semiconductor device of claim 1, wherein The gate structure includes: A gate dielectric layer is disposed on the trench wall, and the gate dielectric layer forms a receiving groove; The gate electrode is disposed within the receiving groove; The thickness of the gate dielectric layer between the gate electrode and the trench wall ranges from 35 to 70 nm.
6. The semiconductor device of claim 1, wherein Each cell further includes a doped region extending from the surface of the epitaxial layer away from the substrate toward the substrate, and the depth of the doped region is less than or equal to the depth of the trench; The doped region includes: A first doped region extends from the surface of the epitaxial layer away from the substrate toward the substrate, and one side of the first doped region is in contact with the gate structure; the first doped region has the same conductivity type as the epitaxial layer. The second doped region extends from the surface of the epitaxial layer away from the substrate toward the substrate, and the second doped region is in contact with the side of the first doped region away from the gate structure; the second doped region has a different conductivity type than the epitaxial layer. The third doped region is located below and in contact with the first and second doped regions; the third doped region has a different conductivity type than the epitaxial layer.
7. The semiconductor device according to any one of claims 1-6, characterized in that, The epitaxial layer is a SiC epitaxial layer with crystal axis [0001], and one sidewall of the trench is a (2-1-10) crystal plane and the other sidewall is a (-2110) crystal plane.
8. A semiconductor wafer having a main locating flat edge, characterized in that include: Multiple semiconductor devices; The semiconductor device has trenches; The angle between the extension direction of the groove and the main positioning flat edge is 25-35 degrees.
9. The semiconductor wafer according to claim 8, characterized in that, Multiple semiconductor devices are arranged in an array, with the row direction parallel to the extension direction of the trench.
10. The semiconductor wafer according to claim 8, characterized in that, The semiconductor wafer is a SiC(0001) wafer; The sidewall of the trench is a (2-1-10) crystal plane or a (-2110) crystal plane, and the main positioning flat edge is formed along the [11-20] crystal direction.