A secondary texturing rounding method and a textured silicon wafer for N-type TOPCon cells

By performing secondary alkaline texturing and rounding of the tower tip during the texturing process of crystalline silicon solar cells, the problem of appearance and process matching caused by reduced reflectivity in the existing technology is solved, the effect of boron diffusion and passivation coating is improved, and the conversion efficiency of the solar cells is increased.

CN123164873APending Publication Date: 2026-11-24HUAIAN JIETAI NEW ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611406564.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-10
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing texturing methods for crystalline silicon solar cells, while reducing reflectivity, may lead to appearance issues and difficulties in matching subsequent processes. Furthermore, the uneven state of the pyramidal structure apex in a single texturing process can affect boron diffusion and passivation coating.

Method used

After forming the pyramid structure using a single texturing process, a second alkaline texturing process is performed before the boron diffusion process to corrode and round the apex of the pyramid structure, forming a smooth transition surface.

Benefits of technology

It improves the optical performance and appearance quality of the textured surface, enhances the uniformity of subsequent boron diffusion and passivation coating processes, and comprehensively improves the conversion efficiency of the solar cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123164873A_ABST
    Figure CN123164873A_ABST
Patent Text Reader

Abstract

This invention relates to the field of crystalline silicon solar cell manufacturing technology, and discloses a secondary texturing method for rounding the textured surface and a textured silicon wafer for N-type TOPCon cells. The method involves first texturing the original silicon wafer with a primary texturing solution, forming a textured surface with multiple pyramidal structures. A secondary texturing solution is then used to perform a secondary texturing process on the silicon wafer after the primary texturing, causing the apexes of the pyramidal structures to be etched and rounded. Both the primary and secondary texturing solutions are alkaline. The rounded transition surface formed at the apexes of the pyramidal structures after the secondary texturing improves the textured surface morphology before boron diffusion, providing a good foundation for subsequent boron diffusion, film coating, and passivation treatment, and is beneficial for improving the open-circuit voltage, fill factor, and conversion efficiency of the solar cell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of crystalline silicon solar cell manufacturing technology, and more particularly to a secondary texturing and rounding textured surface method that involves forming a pyramid structure through a primary texturing process before the boron diffusion process, followed by a secondary alkaline texturing process to etch and round the pyramid structure apex, and a textured silicon wafer for N-type TOPCon cells prepared using this method. Background Technology

[0002] Solar cells typically utilize light wavelengths ranging from 300 nm to 1100 nm, with the visible light band being approximately 380 nm to 780 nm. The main absorption range for crystalline silicon cells is approximately 320 nm to 1100 nm. To increase the multiple reflections and absorption of incident light on the silicon wafer surface, the manufacturing process of crystalline silicon cells usually involves alkaline texturing to create a pyramidal textured surface on the wafer. The aim is to reduce the reflectivity of the textured wafer to achieve current gain.

[0003] Existing production lines typically control the reflectivity of texturing to between 8.5% and 9.0%. However, continuously pursuing texturing with lower reflectivity and smaller base sizes may lead to problems such as a hazy appearance, basket welts, airflow marks, or uneven cell patterns, increasing the burden on subsequent cleaning and process matching. During the subsequent film formation process, color anomalies such as reddish film and rework issues may also occur. Although reducing reflectivity can bring some current gain, the open-circuit voltage, fill factor, reliability, and final conversion efficiency of the solar cell may not necessarily improve simultaneously.

[0004] For N-type TOPCon cells, the texturized silicon wafer still needs to undergo boron diffusion and subsequent passivation coating processes. The pyramid structure formed by texturing in one step usually has relatively sharp apexes, and the size and apex condition of the pyramid structure vary at different locations. If the apex condition is not effectively controlled before the boron diffusion process, the subsequent high-temperature boron diffusion and film formation processes may be affected by the texturing morphology.

[0005] Therefore, a new texturing method is needed to controllably modify the pyramid tip before the boron diffusion process while preserving the overall pyramid textured surface structure, so as to balance the optical performance, appearance quality, and subsequent boron diffusion and passivation coating process requirements of the textured surface. Summary of the Invention

[0006] The purpose of this invention is to provide a secondary texturing and rounding method for textured surfaces and a textured silicon wafer for N-type TOPCon batteries. The method involves forming a pyramid structure through a primary texturing process, and then using a secondary alkaline texturing process to etch and round the tips of the pyramid structure before the boron diffusion process. This improves the textured surface morphology before boron diffusion and provides a good textured surface foundation for subsequent boron diffusion and passivation coating.

[0007] To achieve the above objectives, the present invention provides a method for secondary pile forming and rounding pile surface, comprising the following steps: The original silicon wafer is texturized once using a texturing solution, so that the surface of the original silicon wafer forms a textured surface with multiple pyramid structures; Before the boron diffusion process, a secondary texturing solution is used to perform a secondary texturing on the silicon wafer after the primary texturing, so that the apex of the pyramid structure is etched and rounded. Both the primary and secondary texturing solutions are alkaline texturing solutions.

[0008] In some embodiments, the alkaline solution may be an aqueous solution of sodium hydroxide, an aqueous solution of potassium hydroxide, or other alkaline aqueous solutions that can be used for alkaline texturing of silicon wafers.

[0009] The first texturing process is used to form multiple pyramid structures on the surface of the original silicon wafer. The second texturing process, while preserving the overall shape of the pyramid structure, further etches the sharp tips and edges of at least some of the pyramid structures to reduce the sharpness of the tips and form a rounded transition surface.

[0010] In some embodiments, the secondary texturing and rounding texturing method sequentially includes pre-cleaning, first water washing, first texturing, second water washing, second texturing, third water washing, post-cleaning, fourth water washing, acid washing, fifth water washing, slow lifting and drying steps, and after drying, a texturing silicon wafer for boron diffusion process is obtained.

[0011] In some embodiments, the time for one flocking process is 230–290 s, and the temperature is 77–87°C. Preferably, the time for one flocking process is 260 s, and the temperature is 82°C.

[0012] In some embodiments, the secondary texturing time is 80–140 seconds, and the temperature is 55–65°C. Preferably, the secondary texturing time is 110 seconds, and the temperature is 55°C.

[0013] In some embodiments, the primary texturing solution includes water, an alkaline solution, and a first additive, wherein the alkaline solution is an aqueous sodium hydroxide solution. When initially preparing the primary texturing solution, the volume ratio of water, alkaline solution, and the first additive is 100:(1.17–1.18):(0.32–0.33); when replenishing the solution during the primary texturing process, the volume ratio of water, alkaline solution, and the first additive is 100:(3.78–3.79):(0.71–0.72). After each batch of primary texturing is completed, the primary texturing tank is replenished, and this replenishment is completed before the next row of silicon wafers is fed.

[0014] In some embodiments, the secondary texturing solution includes water, an alkaline solution, and a second additive, wherein the alkaline solution is an aqueous sodium hydroxide solution. When initially preparing the secondary texturing solution, the volume ratio of water, alkaline solution, and the second additive is 100:(0.26–0.27):(0.36–0.37); when replenishing the solution during the secondary texturing process, the volume ratio of the added water, alkaline solution, and second additive is 100:0.60:0.50. After each batch of secondary texturing is completed, the secondary texturing tank is replenished, and this replenishment is completed before the next row of silicon wafers is fed.

[0015] In some embodiments, the first additive comprises 1% to 2% sodium benzoate, 3% to 4% surfactant, 7% to 10% sodium polystyrene sulfonate, and 84% to 89% deionized water, based on the total mass of the first additive.

[0016] In some embodiments, the second additive comprises, based on the total mass of the second additive, 0.5% to 4% of a polyhydroxy organic acid salt, 1% to 2.5% of sodium benzoate, 7% to 9% of sodium polystyrene sulfonate, and 84.5% to 91.5% of deionized water.

[0017] In some embodiments, the polyhydroxy organic acid salt is an environmentally friendly additive for texturing N-type TOPCon silicon wafers, used to improve the wettability of the silicon surface, regulate pyramid nucleation, and improve the uniformity of pyramid morphology; the polyhydroxy organic acid salt can remain stable in a strongly alkaline bath of sodium hydroxide or potassium hydroxide at 75-85°C and is not easily volatilized.

[0018] In some embodiments, the reflectivity of the pile surface after secondary pile forming is 10.0%–11.0%, the width of the pyramid structure is 1.7–1.8 μm, the height is 1.0–1.15 μm, and the number of nuclei is 185,000–220,000 / mm. 2 The ratio is 1.2 to 1.38.

[0019] The present invention also provides a textured silicon wafer for N-type TOPCon batteries, which is prepared by the above-described secondary texturing and rounding texturing method. The surface of the textured silicon wafer has multiple pyramid structures, and the apex of the pyramid structure has a rounded transition surface formed by secondary texturing.

[0020] Compared with the prior art, the present invention has at least the following beneficial effects: This invention performs a second alkaline texturing process after the pyramid structure is formed in the first texturing stage, before the boron diffusion process. This process can further etch the sharp tips and edges of the pyramid without changing the overall structure of the pyramid texturing surface, so that the tips form a smoother, rounded transition surface.

[0021] Rounding the apex of the pyramid structure before the boron diffusion process improves the textured surface for subsequent boron diffusion and film coating, and also enhances the uniformity of the subsequent passivation process.

[0022] This invention does not take the lowest texturing reflectivity as the sole process objective. Instead, it achieves a comprehensive improvement in conversion efficiency by utilizing the gains in open-circuit voltage and fill factor, while allowing for a moderate increase in texturing reflectivity and a possible slight decrease in current.

[0023] In addition, this method can also help alleviate the appearance problems of velluming material cutting, such as gray haze, basket print, airflow print or mottled pattern, that may be caused by excessive reduction of velluming reflectivity. Attached Figure Description

[0024] Figure 1 This is a flowchart of the secondary pile forming and rounding pile surface method of the present invention; Figure 2 This is a schematic diagram comparing the napped surface after one napping process with the rounded napped surface after two napping processes. Figure 3 SEM image of the pile surface before secondary pile forming and rounding; Figure 4 This is a SEM image of the pile surface after secondary pile forming and rounding.

[0025] Figure labeling: 1. Silicon wafer substrate; 2. Pyramid structure; 21. Sharp pyramid tip; 22. Rounded transition surface. Detailed Implementation

[0026] The technical solutions of this application will now be clearly and completely described with reference to the accompanying drawings. Obviously, the described embodiments are merely some embodiments of this application, and not all embodiments. The components of this application described and shown in the accompanying drawings can generally be arranged and designed in various different configurations. Therefore, the following detailed description of the embodiments of this application provided in the accompanying drawings is not intended to limit the scope of the claimed application, but merely to illustrate selected embodiments of this application. All other embodiments obtained by those skilled in the art based on the embodiments of this application without inventive effort are within the scope of protection of this application.

[0027] The present invention will be further described below with reference to the accompanying drawings and embodiments. The described embodiments are only for explaining the present invention and are not intended to limit the scope of protection of the present invention.

[0028] The term "original silicon wafer" as used in this article refers to a silicon wafer that has not yet formed the pyramidal textured surface before entering this secondary texturing and rounding process. The term "primary texturing" as used in this article refers to the process of nucleating and forming multiple pyramidal structures on the surface of the original silicon wafer; the term "secondary texturing" or "pyramid tip rounding" as used in this article refers to the process of continuing alkaline etching on the pyramidal textured surface formed by primary texturing, so that at least some of the sharp pyramid tips form a rounded transition surface. The rounded transition surface can manifest as a reduction in the sharpness of the pyramidal edges and apex, and the formation of continuous arcs or multiple smooth transition morphologies near the apex.

[0029] The term "large pile surface" or "large pyramid base" used in this article describes a pile surface morphology with a larger pyramid width or height compared to existing low-reflectivity small-pyramid pile surfaces. The term "reflectivity enhancement" used in this article refers to an increase in the reflectivity of the pile surface after secondary pile forming and rounding compared to the control process or the pile surface after primary pile forming; this increase can be expressed as an absolute percentage change or a relative increase in reflectivity.

[0030] In this specification, sheet resistance is measured in Ω, film thickness in nm, refractive index is dimensionless, and reflectivity is expressed as a percentage (%). Pyramid width and height are measured in μm, and nucleation count is measured in nuclei per mm. 2 The ratio is the ratio of the surface area of ​​a velvet surface to the surface area of ​​a flat surface, and it is a dimensionless number.

[0031] Example 1: Secondary pile forming and rounding pile surface process In this embodiment, the original silicon wafer is first texturized with a primary texturing solution to form a textured surface with multiple pyramid structures 2. Then, before the boron diffusion process, the silicon wafer after the primary texturing is texturized with a secondary texturing solution to further etch the sharp tips 21 of the pyramid structures 2 and form a rounded transition surface 22.

[0032] In this embodiment, both the primary and secondary texturing solutions are alkaline. The primary texturing is mainly used to form the pyramid structure 2, while the secondary texturing is mainly used to modify the already formed pyramid structure 2 and round off the sharp tips 21.

[0033] As a specific complete process, such as Figure 1 As shown, the following steps are performed sequentially in this embodiment.

[0034] Step A, Pre-cleaning. The original silicon wafer is an N-type silicon wafer used to fabricate N-type TOPCon cells, with dimensions of 210mm × 210mm, resistivity of 0.9–1.6 Ω·cm, crystal orientation of <100>, and an initial smooth silicon surface. A pre-cleaning solution composed of water, alkaline solution, hydrogen peroxide, and cleaning agent is used to pre-clean the silicon wafer at a temperature of 70℃ for 130–150 seconds to remove metallic impurities from the wafer surface.

[0035] Step B, First water rinse. The silicon wafer after the previous cleaning is rinsed with water to reduce the amount of cleaning solution carried over into the texturing solution.

[0036] Step C, primary texturing. An alkaline primary texturing solution is used to texture the silicon wafer after the first water wash, causing nucleation and growth of multiple pyramid structures 2 on the wafer surface. The primary texturing time is 230–290 s, and the temperature is 77–87 °C; in this embodiment, 260 s and 82 °C are used. The textured surface formed by primary texturing has relatively large pyramid bases and relatively sharp pyramid tips 21, such as… Figure 2 Left side and Figure 3 As shown.

[0037] When initially preparing the texturing solution, the volume ratio of water, sodium hydroxide aqueous solution, and the first additive is 100:(1.17-1.18):(0.32-0.33). Taking 680L of water as an example, the amount of sodium hydroxide aqueous solution added is 8L, and the amount of the first additive added is 2.2L, which translates to a volume ratio of approximately 100:1.176:0.324. When replenishing the solution during the first texturing process, the volume ratio of water, sodium hydroxide aqueous solution, and the first additive added is 100:(3.78-3.79):(0.71-0.72); the corresponding replenishment amounts are 14000mL of water, 530mL of sodium hydroxide aqueous solution, and 100mL of the first additive, which translates to a volume ratio of approximately 100:3.786:0.714. The replenishment is performed on the first texturing tank after each batch of texturing is completed and before the next row of silicon wafers is fed.

[0038] The sodium hydroxide aqueous solution used in this embodiment can be an industrial sodium hydroxide stock solution with a mass concentration of 48% to 50%; when using sodium hydroxide aqueous solutions of other concentrations, the amount added can be converted to an equivalent amount according to the effective sodium hydroxide content.

[0039] Based on the total mass of the first additive, the first additive comprises 1%–2% sodium benzoate, 3%–4% surfactant, 7%–10% sodium polystyrene sulfonate, and 84%–89% deionized water. The first additive can be used in conjunction with an aqueous sodium hydroxide solution to control nucleation, growth, and pyramidal morphology in the primary texturing stage.

[0040] The surfactant can be a nonionic surfactant suitable for strongly alkaline silicon wafer texturing systems, such as alkyl glycosides.

[0041] Step D, second water wash. The silicon wafer after the first texturing is washed with water to reduce the amount of the first texturing solution carried over into the second texturing solution, so that the subsequent second texturing can be carried out under the preset solution conditions.

[0042] Step E, Secondary texturing. The silicon wafer after the second water wash is texturized using an alkaline secondary texturing solution. The secondary texturing solution continues to etch the sharp tips 21 of the pyramid structure 2 obtained from the first texturing, causing the sharp tips 21 to form a rounded transition surface 22, such as... Figure 2 right side and Figure 4 As shown. The rounding of the tower tip occurs before the boron diffusion process and is achieved by a secondary texturing weak alkali treatment, not by subsequent acid washing.

[0043] The secondary texturing time is 80–140 seconds, and the temperature is 55–65°C; this embodiment uses 110 seconds and 55°C. When initially preparing the secondary texturing solution, the volume ratio of water, sodium hydroxide aqueous solution, and the second additive is 100:(0.26–0.27):(0.36–0.37). Taking 680L of water as an example, the amount of sodium hydroxide aqueous solution added is 1.8L, and the amount of the second additive added is 2.5L, which translates to a volume ratio of approximately 100:0.265:0.368. When replenishing the solution during the secondary texturing process, the volume ratio of water, sodium hydroxide aqueous solution, and the second additive is 100:0.60:0.50; the corresponding replenishment amounts are 10000mL of water, 60mL of sodium hydroxide aqueous solution, and 50mL of the second additive. This replenishment is performed on the secondary texturing tank after each batch of secondary texturing is completed, and is finished before the next row of silicon wafers is fed.

[0044] Based on the total mass of the second additive, the second additive comprises 0.5%–4% polyhydroxy organic acid salt, 1%–2.5% sodium benzoate, 7%–9% sodium polystyrene sulfonate, and 84.5%–91.5% deionized water. The second additive, in combination with an aqueous sodium hydroxide solution, allows for secondary texturing at a lower temperature and shorter time to modify the existing pyramid structure and control the rounding degree of the pyramid apex. The polyhydroxy organic acid salt is an environmentally friendly additive for alkaline texturing of N-type TOPCon silicon wafers, which improves the wettability of the silicon surface, regulates pyramid nucleation during the texturing process, and enhances pyramid uniformity. This polyhydroxy organic acid salt is resistant to strongly alkaline sodium hydroxide or potassium hydroxide baths at 75–85°C and is not easily volatile, thus maintaining stability under the secondary texturing conditions of this embodiment.

[0045] When the alkali solution is an aqueous solution of sodium hydroxide, the polyhydroxy organic acid salt can be sodium gluconate; when the alkali solution is an aqueous solution of potassium hydroxide, the polyhydroxy organic acid salt can be potassium gluconate.

[0046] It should be noted that this embodiment uses sodium hydroxide aqueous solution as the alkali solution for illustration, but this does not mean that the alkali solution is limited to sodium hydroxide aqueous solution. In other embodiments, potassium hydroxide aqueous solution or other alkaline aqueous solutions that can be used for alkaline texturing of silicon wafers can be used; when using different types or concentrations of alkali solutions, the amount added can be adjusted according to their corrosion ability on silicon wafers to achieve single-stage texturing to form a tower or two-stage texturing to round the tower tip.

[0047] In one process control method, the degree of pyramid tip rounding can be controlled by adjusting one or more of the following: the amount of alkali solution used in the secondary texturing process, the amount of the second additive, the temperature, the time, and the power of the circulating pump. The circulating pump power setting ratio for the primary texturing process is 90%–95%, and the circulating pump power setting ratio for the secondary texturing process is 80%–95%. This causes the primary texturing process to favor pyramid nucleation and growth, while the secondary texturing process tends to favor slight corrosion modification of the existing pyramid tip.

[0048] Step F, third water wash. The silicon wafer after the second texturing is washed with water to reduce the introduction of the second texturing solution and its reaction residues into subsequent cleaning processes.

[0049] Step G, post-cleaning. The silicon wafer after the third water wash is post-cleaned using a post-cleaning solution composed of water, alkaline solution, hydrogen peroxide and cleaning agent. The post-cleaning temperature is 65-70℃ and the time is 100-150s to remove additives, organic matter or other reaction residues left on the texturing surface during the texturing process.

[0050] Step H, fourth water rinse. The silicon wafer is rinsed with water after the post-cleaning process to reduce the amount of post-cleaning solution carried over to the acid pickling process.

[0051] Step I, pickling. A pickling solution is prepared using room temperature deionized water. The pickling solution includes hydrofluoric acid, with a volume concentration of 0.5%–1.5%. The temperature of the pickling tank is 20–25°C. The silicon wafers after the fourth water rinse are pickled for 100–130 seconds to remove alkaline residues or residues formed during texturing and cleaning that can be removed by pickling. The pickling tank does not perform the function of rounding the pyramid tip.

[0052] Step J, fifth water rinse. Rinse the acid-washed silicon wafer with water to reduce the residue of acid washing solution on the textured surface.

[0053] Step K, slow lifting. Begin by lifting the basket loaded with silicon wafers from a state where it is completely submerged in the fifth water washing tank, and continue lifting until the basket is completely removed from the tank. The lifting process takes 10 seconds to reduce uneven residue of droplets or water marks on the textured surface.

[0054] Step L, Drying. The silicon wafer after slow pulling is placed in a drying tank and dried at 95°C for 700 seconds to obtain a textured silicon wafer for the boron diffusion process. The dried textured silicon wafer has multiple pyramid structures 2, and at least some of the pyramid structures 2 have rounded transition surfaces 22 at their apex.

[0055] It should be noted that the pre-washing, each water wash, post-washing, pickling, slow lifting, and drying are the process connections and cleaning and drying steps adopted in this embodiment according to the corresponding production line settings. The core process of this invention is the formation of the pyramid structure 2 through a single flocking process and the rounding of the pyramid tip through a secondary alkaline flocking process before the boron diffusion process.

[0056] Example 2: Reflectivity and Textured Surface In a set of process results, the reflectance of the textured surface after one texturing step was 10.40%, and the reflectance after two texturing steps and rounding was 10.73%, an absolute increase of 0.33 percentage points. The relative increase, calculated based on 10.40%, was approximately 3.17%. By adjusting the parameters of the second texturing step, the relative increase in reflectance could be adjusted within the range of 0.5% to 10%. Reflectance was measured using a D8 reflectance meter in the 250–1100 nm wavelength range, with a sample size of 48 silicon wafers. Nine points were measured on each wafer, and the arithmetic mean was taken. This process does not aim to further reduce reflectance, but rather to moderately increase reflectance in exchange for comprehensive benefits in terms of peak rounding, appearance, and subsequent boron diffusion and passivation matching.

[0057] The test results for the two sets of suede surfaces are shown in the table below: Figure 3 and Figure 4 SEM images were taken at magnifications ranging from 1000 to 3000x, with samples taken from the center of the silicon wafer. Texture morphology data were continuously monitored across six batches of samples. Pyramid width, height, nucleus count, and specific gravity were measured using a ZeTA-20 instrument. For each silicon wafer, three points were selected along the diagonal: the upper left, middle, and lower right, and the arithmetic mean of these three points was calculated. Figure 3 and Figure 4 As can be seen, the apex and edges of the pyramid before rounding are relatively sharp, while a smoother transition area is formed at the top of the pyramid after the second rounding process. By changing the intensity of the second rounding process, the apex of the pyramid at different locations can be rounded to varying degrees without destroying the overall pyramid surface already formed by the first rounding process.

[0058] Example 3: SPC Results of Related Processes The SPC summary data for the texturing, boron diffusion, and positive film related processes are as follows: In the table, "Production Line Data" refers to mass production data, and "Experimental Data" refers to the data from this rounded texturing process. The boron-expanded sheet resistance and positive film data are the Statistical Process Control (SPC) data for the corresponding processes. The texturing process has two tanks for each primary texturing step. The two parallel values ​​for texturing reflectance in the table correspond to the two primary texturing tanks, with three silicon wafers sampled from each tank and the average value taken. The boron-expanded sheet resistance is the average of test data from every six silicon wafers. The two parallel values ​​for positive film reflectance, refractive index, and film thickness correspond to two sets of small boats, with each value being the average of test data from the furnace opening, furnace middle, and furnace tail of the corresponding set of small boats. The above data indicates that the reflectance of the experimental texturing surface is higher than that of the production line texturing surface, the average boron-expanded sheet resistance is similar, and there are corresponding variations in the positive film reflectance, refractive index, and film thickness.

[0059] Example 4: Electrical Performance Comparison The summary data of the four sets of electrical performance and yield are as follows.

[0060] In the table, “Quantity” refers to the sample size of each group; Eta and FF are in %, Voc is in mV, Isc and IRev2 are in A, Rsh is in Ω, Rser is in mΩ, and Tcell is in ℃; each electrical performance index is the arithmetic mean of all samples in the corresponding group, and EL yield and PL yield are expressed as %.

[0061] In the table, group SY represents the secondary pile forming and rounding pile process data of this invention, while groups before, BL, and after the experiment represent the conventional pile forming process data of the production line. Using group before the experiment as a control, the conversion efficiency of group SY increased from 26.91684% to 26.98182%, an absolute increase of approximately 0.065 percentage points; Voc increased by approximately 2.999 mV; FF increased by approximately 0.325 percentage points; and Isc decreased by approximately 0.100. This trend aligns with the technical logic that "increased reflectivity slightly reduces current, but the gains in Voc and FF result in a net increase in final efficiency."

[0062] The data above also shows that the yields of Rsh, Rser, IRev2, EL, and PL in the SY group have changed compared to the data before the experiment. The appearance, leakage current, and mass production stability of the secondary texturing and rounding process can be further evaluated by combining specific process groups, test calibers, and statistical methods.

[0063] Process mechanism and adjustable method Primary texturing is used to form a pyramid structure on the surface of the original silicon wafer, ensuring a large base and a high degree of texturing. Secondary texturing, while retaining the overall pyramid structure, involves slight etching of the pyramid tips and edges. Since secondary texturing occurs before boron diffusion, the pyramid tips are transformed into a smoother, rounded transition surface before entering the high-temperature boron diffusion process. This reduces the degree of morphological abrupt changes of sharp pyramid tips during subsequent high-temperature and film formation processes, and facilitates continuous coverage of the subsequent film layer on the textured surface.

[0064] Without altering the core technical principle of "primary texturing to form the tower, secondary alkaline texturing to round the tower tip, with rounding occurring before boron diffusion," the time, temperature, alkali addition ratio, second additive addition ratio, replenishment ratio, and circulation conditions of the secondary texturing process can be adjusted according to the target texturing surface morphology. During adjustment, the texturing surface reflectance, SEM morphology, pyramid width and height, nucleation number, and specific surface area can be comprehensively observed to determine the endpoint of the secondary texturing process.

[0065] The endpoint of the secondary texturing process can be determined by observing, through SEM, that at least some sharp pyramidal apexes have formed a continuously rounded transition surface, and then verifying this conclusion in conjunction with reflectivity and surface morphology. After secondary texturing, the surface reflectivity should be controlled at 10.0%–11.0%, the width of the pyramidal structure at 1.7–1.8 μm, the height at 1.0–1.15 μm, and the nucleus count at 185,000–220,000 nuclei / mm. 2 The ratio of the diametrical index should be controlled between 1.2 and 1.38.

[0066] Primary and secondary texturing can be completed sequentially in different tanks of an existing texturing machine without altering the basic order of subsequent boron diffusion and passivation coating processes. For N-type silicon wafers of different sizes, resistivity, or initial surface conditions, the processing conditions can be adjusted within the specified parameter range to ensure that the pyramid structure formed by primary texturing meets the requirements for pyramid formation and that the pyramid apex after secondary texturing achieves the desired degree of roundness.

[0067] The above description is merely an embodiment of this application and is not intended to limit the scope of protection of this application. Various modifications and variations can be made to this application by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the scope of protection of this application.

Claims

1. A method for secondary pile forming and rounding pile surface, characterized in that, Includes the following steps: The original silicon wafer is texturized once using a texturing solution, so that the surface of the original silicon wafer forms a textured surface with multiple pyramidal structures. A secondary texturing solution is used to perform a secondary texturing process on the silicon wafer after the primary texturing, so that the apex of the pyramid structure is etched and rounded. Both the primary and secondary texturing solutions are alkaline texturing solutions.

2. The method for secondary pile forming and rounding pile surface according to claim 1, characterized in that, The time for one pass of the flocking process is 230–290 seconds, and the temperature is 77–87℃.

3. The method for secondary pile forming and rounding pile surface according to claim 1, characterized in that, The secondary texturing process takes 80–140 seconds and is carried out at a temperature of 55–65°C.

4. The method for secondary pile forming and rounding pile surface according to claim 2, characterized in that, The fabrication process takes 260 seconds and the temperature is 82℃.

5. The method for secondary pile forming and rounding pile surface according to claim 3, characterized in that, The secondary texturing process takes 110 seconds and is carried out at a temperature of 55°C.

6. The method for secondary pile forming and rounding pile surface according to claim 1, characterized in that, The primary texturing solution includes water, alkali solution, and a first additive. When initially preparing the primary texturing solution, the volume ratio of water, alkali solution, and the first additive is 100:(1.17-1.18):(0.32-0.33). When replenishing the solution during the primary texturing process, the volume ratio of the added water, alkali solution, and the first additive is 100:(3.78-3.79):(0.71-0.72).

7. The method for secondary pile forming and rounding pile surface according to claim 1, characterized in that, The secondary texturing solution includes water, alkali solution, and a second additive. When initially preparing the secondary texturing solution, the volume ratio of water, alkali solution, and the second additive is 100:(0.26-0.27):(0.36-0.37). When replenishing the solution during the secondary texturing process, the volume ratio of the added water, alkali solution, and the second additive is 100:0.60:0.

50.

8. The method for secondary pile forming and rounding pile surface according to claim 6, characterized in that, The alkaline solution is an aqueous sodium hydroxide solution; when initially preparing the primary texturing solution, the amounts of water, aqueous sodium hydroxide solution, and the first additive added are 680L, 8L, and 2.2L, respectively; when replenishing the solution during the primary texturing process, the amounts of water, aqueous sodium hydroxide solution, and the first additive added are 14000mL, 530mL, and 100mL, respectively.

9. The method for secondary pile forming and rounding pile surface according to claim 7, characterized in that, The alkaline solution is an aqueous sodium hydroxide solution; when initially preparing the secondary texturing solution, the amounts of water, aqueous sodium hydroxide solution, and the second additive added are 680L, 1.8L, and 2.5L, respectively; when replenishing the solution during the secondary texturing process, the amounts of water, aqueous sodium hydroxide solution, and the second additive added are 10000mL, 60mL, and 50mL, respectively.

10. The method for secondary pile forming and rounding pile surface according to claim 6, characterized in that, Based on the total mass of the first additive, the first additive comprises 1% to 2% sodium benzoate, 3% to 4% surfactant, 7% to 10% sodium polystyrene sulfonate and 84% to 89% deionized water.

11. The method for secondary pile forming and rounding pile surface according to claim 7, characterized in that, Based on the total mass of the second additive, the second additive comprises 0.5% to 4% of polyhydroxy organic acid salts, 1% to 2.5% of sodium benzoate, 7% to 9% of sodium polystyrene sulfonate, and 84.5% to 91.5% of deionized water.

12. The method for secondary pile forming and rounding pile surface according to claim 1, characterized in that, The reflectivity of the pile surface after secondary pile forming is 10.0%–11.0%. The width of the pyramid structure is 1.7–1.8 μm, the height is 1.0–1.15 μm, and the number of nuclei is 185,000–220,000 / mm. 2 The ratio is 1.2 to 1.

38.

13. A textured silicon wafer for N-type TOPCon batteries, characterized in that, The textured silicon wafer is prepared by the secondary texturing and rounding texturing method according to any one of claims 1 to 12. The surface of the textured silicon wafer has multiple pyramid structures, and the apex of the pyramid structure has a rounded transition surface formed by secondary texturing.