A preparation process of a TOPCon cell based on double-sided laser isolation

By using double-sided laser isolation technology to perform double-sided laser processing on the pre-cut area of ​​photovoltaic cell modules, the problems of leakage and recombination loss at the cutting edge are solved, resulting in higher cell efficiency and module power output.

CN123164874APending Publication Date: 2026-11-24宜宾英发德耀科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611419483.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-14
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

During the laser cutting and slicing process of existing photovoltaic cell modules, the formation of an amorphous silicon layer at the cutting edge leads to carrier recombination centers, increasing leakage current and recombination losses. Existing technologies are unable to effectively block the leakage channels of the PN junction and passivate the cutting edge, resulting in efficiency loss.

Method used

By employing double-sided laser isolation technology, laser processing is performed on both the front and back sides of the silicon wafer to remove the borosilicate glass layer and the phosphosilicate glass layer. Simultaneously, an aluminum oxide passivation film and a silicon oxynitride passivation antireflection film are applied to the laser-processed area to form a good passivation protection.

Benefits of technology

It effectively blocks the migration of photogenerated carriers to the recombination region at the cutting edge, reduces edge recombination losses and leakage current, improves cell conversion efficiency and module output power, and avoids additional processes and cost increases.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123164874A_ABST
    Figure CN123164874A_ABST
Patent Text Reader

Abstract

This invention discloses a TOPCon cell fabrication process based on double-sided laser isolation, relating to the field of photovoltaic cell technology. The method includes: texturing, boron diffusion, and back-side polishing of a silicon wafer; fabricating a tunneling oxide layer and a doped amorphous silicon layer on the back side, followed by high-temperature annealing to crystallize into a doped polycrystalline silicon layer; performing double-sided laser treatment on the pre-cut area of ​​the silicon wafer to pre-remove the PN junction in that area; subsequently performing wet cleaning to simultaneously remove the surrounding coating, residual doped glass layer, and laser-damaged layer; then sequentially depositing aluminum oxide and silicon oxynitride passivation antireflection films on the front and back sides to simultaneously cover the pre-cut area; finally, fabricating electrodes, sintering, and slicing along the pre-cut area to obtain the target cell. This invention, by pre-removing the PN junction in the pre-cut area of ​​the module through double-sided laser isolation, effectively reduces efficiency loss caused by leakage and defect recombination in that area, significantly improving cell conversion efficiency and module output power.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of photovoltaic cell technology, and more specifically, to a TOPCon cell fabrication process based on double-sided laser isolation. Background Technology

[0002] Currently, half-cell and multi-cell packaging schemes are widely used in photovoltaic module manufacturing to improve module output power. However, during the laser cutting process, the instantaneous high temperature (local temperature >1500℃) causes the silicon lattice at the cutting edge to melt and recrystallize, forming an amorphous silicon layer. This layer becomes a carrier recombination center, where photogenerated carriers recombine rapidly in the edge region and cannot participate in conductivity. At the same time, the exposed silicon surface is prone to react with oxygen and moisture in the air to form an oxide layer. In addition, surface state traps formed by impurities and dust further aggravate recombination losses. Furthermore, the exposure of the edge PN junction during the cutting process leads to an increase in leakage current. Therefore, while half-cell and multi-cell technologies improve module power, they inevitably introduce efficiency losses due to edge leakage and defect recombination, partially offsetting the power gain brought by slicing and limiting further improvements in module power.

[0003] Based on this, existing technologies propose using single-sided laser isolation or half-cell passivation techniques. Single-sided laser isolation involves treating the cut area of ​​the module with a single laser after boron diffusion to remove the borosilicate glass layer in that area. However, treating only one side cannot effectively block the leakage path of the PN junction at the cut edge, and its effect on suppressing recombination loss and leakage current is limited. Similarly, half-cell passivation technology uses coating equipment to deposit a passivation film on the cut edge after cell cutting to reduce recombination. However, this approach requires an additional passivation coating process after slab separation, which is complex and increases manufacturing costs. Furthermore, cutting damage has already formed before coating, limiting the passivation effect.

[0004] In view of this, the present invention is proposed. Summary of the Invention

[0005] To address the aforementioned technical problems, the present invention aims to provide a TOPCon cell fabrication process based on double-sided laser isolation.

[0006] This invention is implemented as follows: In a first aspect, the present invention provides a TOPCon cell fabrication process based on double-sided laser isolation, comprising the following steps: A silicon wafer is provided, and the silicon wafer is sequentially subjected to texturing and boron diffusion treatments. The borosilicate glass layer on the back of the silicon wafer is removed, and the back of the silicon wafer is polished to form a silicon wafer with a polished morphology on the back. A tunneling oxide layer and a doped amorphous silicon layer are sequentially prepared on the back side of the silicon wafer, and the doped amorphous silicon layer is crystallized into a doped polycrystalline silicon layer by high-temperature annealing. Laser processing is performed on the front and back sides of the pre-cut area of ​​the silicon wafer to remove the borosilicate glass layer on the front side and the phosphosilicate glass layer on the back side of the area. The silicon wafer after laser treatment is placed with the back side facing up and subjected to wet post-cleaning treatment. The wet post-cleaning treatment simultaneously removes the polycrystalline silicon layer coated on the front side and the residual doped glass layer on the front and back sides, and polishes away the damaged layers in the laser-treated areas on the front and back sides of the silicon wafer. An aluminum oxide passivation film and a silicon oxynitride passivation antireflection film are sequentially deposited on the front and back sides of the silicon wafer, and the pre-cut area is simultaneously covered by the aluminum oxide passivation film and the silicon oxynitride passivation antireflection film; Electrodes are prepared on the front and back sides of the silicon wafer, and after sintering, a battery cell is obtained. The battery cell is then laser-cut along the pre-cut area to obtain the TOPCon battery.

[0007] In an optional embodiment, the thickness of the silicon wafer is 100-200 μm; And / or, the back-side polishing process creates a tower base with a size of 8 on the back side. Morphology of the polishing tower base at 15 μm.

[0008] In an optional embodiment, the thickness of the tunneling oxide layer is 1-2 nm, and the thickness of the doped amorphous silicon layer is 60-150 nm.

[0009] In an optional embodiment, the high-temperature annealing treatment is carried out in a tubular high-temperature diffusion furnace, with an annealing temperature of 900-940℃, an annealing time of 20-40 min, a furnace pressure of 850 mbar, and 5000-6000 sccm of nitrogen gas introduced during the annealing process.

[0010] In an optional embodiment, during the laser processing, a picosecond laser is used as the laser source, with a front laser power of 20-50W, a back laser power of 30-70W, a spot linewidth of 300-500μm, and a longitudinal overlap rate of 30%-50%. And / or, the pre-cut area divides the silicon wafer into a two-part, three-part, or four-part structure.

[0011] In an optional embodiment, the wet post-cleaning process includes: with the back side of the silicon wafer facing up, performing a first acid pickling to remove the phosphosilicate glass layer on the front side and the edges, an alkaline etching to remove the polycrystalline silicon layer around the front side, a second acid pickling to remove the phosphosilicate glass layer on the back side and the borosilicate glass layer on the front side, and finally a third acid pickling, water washing, slow lifting and drying process.

[0012] In an optional embodiment, the first and third pickling uses a hydrofluoric acid solution; the alkaline etching uses a potassium hydroxide solution or a sodium hydroxide solution; and the second pickling uses a mixed solution of hydrofluoric acid and hydrochloric acid.

[0013] In an optional embodiment, the alumina passivation film is prepared using a tubular ALD deposition furnace, during which TMA and water are alternately introduced, with a single TMA introduction time of 4-8 seconds, a single water introduction time of 4-8 seconds, a cycle number of 25-40 times, and a deposition temperature of 190-300℃. And / or, the thickness of the alumina passivation film is 3-10 nm.

[0014] In an optional embodiment, the silicon oxynitride passivation antireflection film is prepared using a PECVD tubular plasma thin film deposition furnace, with SiH4, NH3, and N2O as gas sources, a deposition temperature of 450-600℃, a deposition pressure of 700-2000 mtorr, and an RF power supply of 8000-20000 W. And / or, the thickness of the front silicon oxynitride passivation antireflective film is 65-75 nm and the refractive index is 2.0-2.2, and the thickness of the back silicon oxynitride passivation antireflective film is 60-80 nm and the refractive index is 2.1-2.2.

[0015] In an optional embodiment, the sintering temperature is 850-900℃, the sintering time is 60-80s, and after sintering, light injection and laser-induced sintering are performed.

[0016] The present invention has the following beneficial effects: This application employs double-sided laser treatment on the pre-cut area of ​​the module after boron diffusion and POLY fabrication to pre-remove the PN junction in this area, eliminating minority carrier drift channels at the source and effectively blocking the migration of photogenerated carriers to the recombination region at the cutting edge. This significantly reduces edge recombination losses and leakage current, avoiding the inherent efficiency losses of half-cell and multi-cell technologies. Simultaneously, the laser-treated area is covered with alumina and silicon oxynitride passivation films during subsequent coating processes, achieving good passivation of the cut area without additional steps and preventing edge oxidation and surface state trap formation after cutting. Through these synergistic effects, this invention effectively reduces efficiency losses caused by module cutting and significantly improves cell conversion efficiency and module output power. Attached Figure Description

[0017] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.

[0018] Figure 1 This is a schematic diagram of the two-segment laser processing areas in an embodiment of this application. Detailed Implementation

[0019] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.

[0020] The following is a detailed description of a TOPCon battery fabrication process based on double-sided laser isolation provided by the present invention.

[0021] This invention provides a TOPCon cell fabrication process based on double-sided laser isolation, comprising the following steps: S1. Provide a silicon wafer and perform texturing and boron diffusion treatments on the silicon wafer in sequence; In some preferred embodiments, the thickness of the silicon wafer is 100-200 μm, for example, it can be at least one of 100 μm, 120 μm, 140 μm, 160 μm, 180 μm or 200 μm or any range of two of these values. S2. Remove the borosilicate glass layer (BSG) on the back of the silicon wafer and polish the back of the silicon wafer to form a silicon wafer with a polished morphology on the back. Specifically, the boron-diffused silicon wafer is placed in a chain cleaning device with the front side facing up, and the BSG on the back and edges is removed with hydrofluoric acid (HF) solution. Then, the silicon wafer is transferred to a tank alkaline polishing device and immersed in an alkaline solution containing polishing additives for back polishing. Preferably, the polishing solution temperature is controlled at 65-80℃ and the processing time is 60-300s, so that the back of the silicon wafer forms a flat and smooth polished morphology. After polishing, it is washed with water, acid-washed and neutralized, slowly lifted and dried to obtain a silicon wafer with a polished morphology on the back.

[0022] In some preferred embodiments, the back-side polishing process creates a tower base with a size of 8 on the back side. The morphology of the polishing tower base is 15 μm; as an example, the tower base size can be 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm or 15 μm, etc.

[0023] S3. A tunneling oxide layer and a doped amorphous silicon layer are sequentially prepared on the back side of the silicon wafer, and the doped amorphous silicon layer is crystallized into a doped polycrystalline silicon layer by high-temperature annealing. In some embodiments, the silicon wafer obtained in step S2 is inserted into a graphite boat and placed in a PECVD tubular plasma thin film deposition furnace. First, using N2O or O2 as the oxygen source, a tunneling oxide layer (SiO2) is deposited on the back side of the silicon wafer under the conditions of RF power of 8000-20000W, deposition temperature of 400-600℃, and reaction pressure of 700-2000mtorr. Then, the gas source is switched to a mixed gas of SiH4, PH3, and H2, and under the same temperature and pressure conditions, PH3 is used as the doping source for in-situ doping to deposit a phosphorus-doped amorphous silicon layer on the surface of the tunneling oxide layer.

[0024] Preferably, the thickness of the tunneling oxide layer is 1-2 nm, for example, it can be 1 nm, 1.5 nm or 2 nm, etc.; the thickness of the doped amorphous silicon layer is 60-150 nm, for example, it can be 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 110 nm, 120 nm, 130 nm, 140 nm or 150 nm, etc.

[0025] Furthermore, the high-temperature annealing treatment is carried out in a tubular high-temperature diffusion furnace, with an annealing temperature of 900-940℃, an annealing time of 20-40 min, a furnace pressure of 850 mbar, and 5000-6000 sccm of nitrogen gas introduced during the annealing process to complete the activation of phosphorus doping and the crystallization of amorphous silicon.

[0026] For example, the annealing temperature can be 900℃, 910℃, 920℃, 930℃ or 940℃, etc.; the annealing time can be 20min, 30min or 40min, etc.; the nitrogen flow rate is 5000sccm, 5500sccm or 6000sccm, etc.

[0027] S4. Laser processing is performed on the front and back sides of the pre-cut area of ​​the silicon wafer to remove the borosilicate glass layer on the front side and the phosphosilicate glass layer on the back side of the area. In this process, the silicon wafer obtained in step S3 is placed on the worktable of the laser processing equipment. According to the preset component cutting area, the silicon wafer can be divided into two, three, or four pieces. A picosecond laser is used to perform laser scanning on the front and back of the pre-cut area to remove the borosilicate glass layer (BSG) on the front and the phosphosilicate glass layer (PSG) on the back of the area.

[0028] In some preferred embodiments, during laser processing, the spot linewidth is controlled to be 300-500μm, for example, 300μm, 350μm, 400μm, 450μm or 500μm, and the longitudinal overlap rate is controlled to be 30%-50%, for example, 30%, 40% or 50%.

[0029] Preferably, the front laser power is set to 20-50W, such as 20W, 30W, 40W, or 50W; the back laser power is set to 30-70W, such as 30W, 40W, 50W, 60W, or 70W. Since the back laser power is higher than the front laser power, it effectively compensates for the energy attenuation of the back laser after it passes through the silicon wafer, ensuring consistency in the laser processing effect between the front and back sides, while avoiding thermal damage to the silicon wafer caused by excessively high laser power. By using a picosecond laser and the above-mentioned optimized power parameters, the laser action time is extremely short, the heat-affected zone is small, which can effectively reduce the thermal damage caused by the laser and avoid microcracks and thermal stress at the edges of the silicon wafer.

[0030] S5. Place the silicon wafer, after laser treatment in step S4, with the back side facing up, into a chain cleaning machine for wet post-cleaning. Since a phosphosilicate glass (PSG) layer and a polycrystalline silicon layer were formed on the front side of the silicon wafer in the aforementioned steps, and a layer of PSG also remains on the back surface, the wet post-cleaning process simultaneously removes the polycrystalline silicon layer on the front side and the residual doped glass layers on both sides, and polishes away the damaged layers in the laser-treated areas on both the front and back sides of the silicon wafer. The specific cleaning process is as follows: (1) First pickling: The silicon wafer is placed with the back side facing up into the first pickling tank, and the PSG layer on the front side and edge of the silicon wafer is removed with hydrofluoric acid (HF) solution. The mass concentration of HF solution is preferably 5%-15%, and the processing time is 60-180s. (2) Alkaline etching: The silicon wafer is transferred into an alkaline etching tank and etched with potassium hydroxide (KOH) solution or sodium hydroxide (NaOH) to remove the polycrystalline silicon layer coated on the front side. The KOH solution mass concentration is preferably 5%-15%, the temperature is controlled at 50-80℃, the processing time is 60-300s, and the etching depth is controlled at 0.5-3μm to ensure that the polycrystalline silicon layer coated on the front side is completely removed without damaging the silicon wafer substrate. (3) Second pickling: The silicon wafer is transferred into the second pickling tank and pickled with a mixed solution of hydrofluoric acid and hydrochloric acid (HF+HCl) to remove the PSG layer remaining on the back side and the borosilicate glass layer (BSG) remaining on the front side in step S1. The mass concentration of HF in the mixed acid solution is 5%-15% and the mass concentration of HCl is 5%-15%. (4) Third acid washing and drying: The silicon wafer is sequentially cleaned with HF solution, washed with deionized water, slowly pulled and dried to complete the cleaning process.

[0031] After the above wet cleaning process, the polycrystalline silicon layer on the front side and the residual doped glass layer on the front and back sides are removed simultaneously. At the same time, the damaged layer in the laser-treated area is polished and removed under the corrosive action of acid and alkali solutions, the cutting edges are corroded and smoothed, and the surface defect recombination center is significantly reduced.

[0032] S6. Insert the cleaned and dried silicon wafer from step S5 into an aluminum boat and load it into a tubular ALD (Atomic Layer Deposition) furnace to prepare aluminum oxide passivation films on both sides of the silicon wafer. During the deposition process, trimethylaluminum (TMA) and deionized water (H2O) are used as precursor sources. TMA and H2O are alternately pulsed through the silicon wafer to grow aluminum oxide (Al2O3) films layer by layer on the silicon wafer surface using their self-limiting chemical reaction. The time for a single TMA introduction is 4-8 seconds, for example, 4s, 5s, 6s, 7s, or 8s; the time for a single H2O introduction is 4-8 seconds, for example, 4s, 5s, 6s, 7s, or 8s; the number of cycles is 25-40, for example, 25, 28, 30, 32, 35, 38, or 40; and the deposition temperature is controlled at 190-300℃, for example, 190℃, 200℃, 220℃, 250℃, 280℃, or 300℃. After the above deposition, an alumina film with a thickness of 3-10nm is formed on both sides of the silicon wafer. This alumina film is rich in fixed negative charges, which can provide excellent field-effect passivation effect on the P-type silicon surface and effectively reduce the surface recombination rate. As an example, the thickness of the alumina film can be 3nm, 4nm, 5nm, 6nm, 7nm, 8nm, 9nm or 10nm, preferably 4.5nm.

[0033] Furthermore, the silicon wafer after alumina deposition is inserted into a graphite boat and placed in a PECVD tubular plasma thin film deposition furnace to continue depositing a silicon oxynitride (SiON) passivation antireflection film on the alumina film surface. Deposition is carried out with the aid of plasma generated by an RF power supply, using silane (SiH4), ammonia (NH3), and nitrous oxide (N2O) as the reaction gas source.

[0034] The deposition temperature is controlled between 450-600℃, for example, 450℃, 480℃, 500℃, 520℃, 550℃, 580℃ or 600℃, etc. The deposition pressure is controlled between 700-2000 mtorr, for example, 700 mtorr, 800 mtorr, 1000 mtorr, 1200 mtorr, 1500 mtorr, 1800 mtorr or 2000 mtorr, etc. The RF power supply is 8000-20000W, for example, 8000W, 10000W, 12000W, 15000W, 18000W or 20000W, etc.

[0035] By adjusting the deposition process parameters, the thickness of the front-side silicon oxynitride film is controlled at 65-75 nm, for example, 65 nm, 68 nm, 70 nm, 72 nm, or 75 nm, and the refractive index is controlled at 2.0-2.2, for example, 2.0, 2.05, 2.1, 2.15, or 2.2; the thickness of the back-side silicon oxynitride film is controlled at 60-80 nm, for example, 60 nm, 65 nm, 70 nm, 75 nm, or 80 nm, and the refractive index is controlled at 2.1-2.2, for example, 2.1, 2.12, 2.15, 2.18, or 2.2.

[0036] After laser isolation treatment, the pre-cut area was simultaneously covered with alumina and silicon oxynitride films along with other areas of the silicon wafer, ensuring that the cut area also received good chemical passivation and field-effect passivation protection. Therefore, during subsequent laser slitting, the cut edges are pre-covered with passivation films, effectively preventing recombination losses caused by exposed silicon dangling bonds in the air after cutting, further reducing the edge recombination rate and improving battery efficiency.

[0037] S7. Electrodes are prepared on the front and back sides of the silicon wafer, and after sintering, a battery cell is obtained. The battery cell is then laser-cut along the pre-cut area to obtain the TOPCon battery.

[0038] In this process, the silicon wafer obtained in step S6 is placed in a screen printing machine, and silver gate line electrodes are printed on the front and back sides of the silicon wafer using screen printing technology. Specifically, silver gate lines are printed on the front side and the back side to form a complete electrode pattern.

[0039] The silicon wafer with printed electrodes is then placed in a sintering furnace for high-temperature sintering at temperatures ranging from 850-900℃ (e.g., 850℃, 860℃, 870℃, 880℃, 890℃, or 900℃) for 60-80 seconds (e.g., 60s, 65s, 70s, 75s, or 80s). During sintering, the silver particles in the silver grid lines form good ohmic contact with the silicon wafer surface, while the glassy phase in the silver paste is etched through the passivation film, creating a conductive path between the silver and the silicon substrate. After sintering, the silicon wafer undergoes photoinjection, where high-intensity light is irradiated to inject photons. These photogenerated carriers activate hydrogen atoms in the passivation film, causing them to diffuse to the silicon wafer interface, further passivating interface defects and improving minority carrier lifetime.

[0040] Subsequently, the sintered and light-injected solar cells are subjected to laser-induced contact optimization (LECO) treatment. By utilizing the synergistic effect of local laser heating and applied bias voltage, the contact performance of the silver-silicon contact interface is selectively improved, the contact resistance is reduced, and the fill factor and cell conversion efficiency are further enhanced.

[0041] Furthermore, since the PN junction has been removed from the pre-cut area in the aforementioned steps and the alumina and silicon oxynitride passivation films have been simultaneously applied, the cut edges after slicing have good passivation protection, effectively avoiding edge recombination losses and increased leakage current caused by cutting exposure. The sliced ​​cells are then encapsulated through busbar welding, lamination, framing, and junction box installation to produce N-type TOPCon battery modules.

[0042] The above embodiments only use TOPCon cells as an example to describe the present invention in detail, but the application scope of the present invention is not limited thereto. PERC cells, BC cells, and heterojunction cells also suffer from edge recombination loss and increased leakage current during the laser slicing process. Therefore, the double-sided laser isolation scheme of the present invention can also be used. In the corresponding process (such as after back passivation of PERC cells, before metallization of BC cells, etc.), the pre-cut area is subjected to double-sided laser treatment and simultaneously covered by subsequent coating to reduce cutting loss and improve module power.

[0043] The features and performance of the present invention will be further described in detail below with reference to embodiments.

[0044] Example 1 This embodiment provides a TOPCon cell fabrication process based on double-sided laser isolation, specifically including the following steps: (1) Provide an N-type single crystal silicon wafer with a thickness of 120 μm, perform texturing on the silicon wafer to form a pyramid textured surface, and then perform boron diffusion treatment to form a boron diffusion layer.

[0045] (2) Remove the BSG on the back of the silicon wafer and polish the back of the silicon wafer using a tank-type alkaline polishing equipment to form a polished morphology with a base size of 8μm.

[0046] (3) A tunneling oxide layer with a thickness of 1 nm and a doped amorphous silicon layer with a thickness of 110 nm were sequentially prepared on the back side of the silicon wafer by PECVD. Then, a high-temperature annealing treatment was carried out in a tube-type high-temperature diffusion furnace. The annealing temperature was 910℃ and the annealing time was 30 min, so that the doped amorphous silicon layer crystallized into a doped polycrystalline silicon layer.

[0047] (4) A picosecond laser is used to perform double-sided laser processing on the pre-defined cutting area (division) of the silicon wafer, such as... Figure 1As shown, the laser power on the front side is 20W, the laser power on the back side is 30W, the laser spot linewidth is 300μm, and the longitudinal overlap rate is 50%. The BSG layer on the front side and the PSG on the back side of this region are removed.

[0048] (5) After laser treatment, the back side of the silicon wafer is facing up and wet cleaning is performed: the PSG layer on the front side and the edge is removed by HF solution, the polysilicon layer on the front side is removed by KOH solution, the PSG layer on the back side and the BSG layer on the front side are removed by HF+HCl mixed acid solution, and finally the wafer is cleaned with HF solution, washed with water, slowly pulled up and dried.

[0049] (6) Alumina passivation films with a thickness of 4.5 nm were deposited on the front and back sides of the silicon wafer using a tubular ALD deposition furnace; then, silicon oxynitride passivation antireflection films were deposited on the surface of the alumina films using PECVD, with a front film thickness of 70 nm and a refractive index of 2.02, and a back film thickness of 80 nm and a refractive index of 2.15.

[0050] (7) Silver grid lines are printed on the front and back of the silicon wafer by screen printing, sintered at 860°C for 60s, and after light injection and LECO treatment, laser slicing is performed along the pre-cut area to obtain N-type TOPCon cells.

[0051] Comparative Example 1 This comparative example provides a TOPCon battery fabrication process. The remaining steps and parameters are the same as in Example 1, except that the laser treatment of the pre-cut area after annealing is not performed.

[0052] Experimental Example 1 The battery cells prepared in Example 1 and Comparative Example 1 were subjected to electrical performance tests under the following conditions: temperature: 25±1℃, spectrum: AM1.5G, irradiance: 1000 / m². 2 The results are shown in Table 1.

[0053] Table 1. Electrical performance test results

[0054] As shown in Table 1, the Pmax of Example 1 is 583.2 W, which is 3.9 W higher than that of Comparative Example 1 (579.3 W). The Isc of Example 1 is 13.920 A, which is approximately 0.141 A higher than that of Comparative Example 1 (13.779 A). Simultaneously, the Voc increases from 52.68 V to 52.74 V. These results demonstrate that the present invention, by performing double-sided laser treatment on the pre-cut region after boron diffusion and POLY fabrication, effectively eliminates minority carrier drift channels, reduces recombination losses and leakage current at the cutting edge, and improves the collection efficiency of photogenerated carriers. Furthermore, the laser-treated region simultaneously forms a passivation layer during subsequent coating processes, preventing edge oxidation and surface state trap formation after cutting, thus significantly improving the output power of the battery module.

[0055] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A fabrication process for TOPCon cells based on double-sided laser isolation, characterized in that, Includes the following steps: A silicon wafer is provided, and the silicon wafer is sequentially subjected to texturing and boron diffusion treatments. The borosilicate glass layer on the back of the silicon wafer is removed, and the back of the silicon wafer is polished to form a silicon wafer with a polished morphology on the back. A tunneling oxide layer and a doped amorphous silicon layer are sequentially prepared on the back side of the silicon wafer, and the doped amorphous silicon layer is crystallized into a doped polycrystalline silicon layer by high-temperature annealing. Laser processing is performed on the front and back sides of the pre-cut area of ​​the silicon wafer to remove the borosilicate glass layer on the front side and the phosphosilicate glass layer on the back side of the area. The silicon wafer after laser treatment is placed with the back side facing up and subjected to wet post-cleaning treatment. The wet post-cleaning treatment simultaneously removes the polycrystalline silicon layer coated on the front side and the residual doped glass layer on the front and back sides, and polishes away the damaged layers in the laser-treated areas on the front and back sides of the silicon wafer. An aluminum oxide passivation film and a silicon oxynitride passivation antireflection film are sequentially deposited on the front and back sides of the silicon wafer, and the pre-cut area is simultaneously covered by the aluminum oxide passivation film and the silicon oxynitride passivation antireflection film; Electrodes are prepared on the front and back sides of the silicon wafer, and after sintering, a battery cell is obtained. The battery cell is then laser-cut along the pre-cut area to obtain the TOPCon battery.

2. The preparation process according to claim 1, characterized in that, The thickness of the silicon wafer is 100-200 μm; And / or, the back-side polishing process creates a tower base with a size of 8 on the back side. Morphology of the polishing tower base at 15 μm.

3. The preparation process according to claim 1, characterized in that, The thickness of the tunneling oxide layer is 1-2 nm, and the thickness of the doped amorphous silicon layer is 60-150 nm.

4. The preparation process according to claim 1, characterized in that, The high-temperature annealing process is carried out in a tubular high-temperature diffusion furnace at a temperature of 900-940℃ for 20-40 minutes, with a furnace pressure of 850 mbar and 5000-6000 sccm of nitrogen gas introduced during the annealing process.

5. The preparation process according to claim 1, characterized in that, During the laser processing, a picosecond laser is used as the laser source, with a front laser power of 20-50W, a back laser power of 30-70W, a spot linewidth of 300-500μm, and a longitudinal overlap rate of 30%-50%. And / or, the pre-cut area divides the silicon wafer into a two-part, three-part, or four-part structure.

6. The preparation process according to claim 1, characterized in that, The wet post-cleaning process includes: with the back side of the silicon wafer facing up, performing a first acid pickling to remove the phosphosilicate glass layer on the front side and edges, an alkaline etching to remove the polycrystalline silicon layer around the front side, a second acid pickling to remove the phosphosilicate glass layer on the back side and the borosilicate glass layer on the front side, and finally a third acid pickling, water washing, slow lifting and drying process.

7. The preparation process according to claim 6, characterized in that, The first and third acid pickling uses hydrofluoric acid solution; the alkaline etching uses potassium hydroxide solution or sodium hydroxide solution; and the second acid pickling uses a mixed solution of hydrofluoric acid and hydrochloric acid.

8. The preparation process according to claim 1, characterized in that, The alumina passivation film was prepared using a tubular ALD deposition furnace. During the deposition process, TMA and water were alternately introduced. The time for each TMA introduction was 4-8 seconds, the time for each water introduction was 4-8 seconds, the number of cycles was 25-40, and the deposition temperature was 190-300℃. And / or, the thickness of the alumina passivation film is 3-10 nm.

9. The preparation process according to claim 1, characterized in that, The silicon oxynitride passivated antireflective film was prepared using a PECVD tubular plasma thin film deposition furnace with SiH4, NH3, and N2O as gas sources, a deposition temperature of 450-600℃, a deposition pressure of 700-2000 mtorr, and an RF power supply of 8000-20000 W. And / or, the thickness of the front silicon oxynitride passivation antireflective film is 65-75 nm and the refractive index is 2.0-2.2, and the thickness of the back silicon oxynitride passivation antireflective film is 60-80 nm and the refractive index is 2.1-2.

2.

10. The preparation process according to claim 1, characterized in that, The sintering temperature is 850-900℃, the sintering time is 60-80s, and after sintering, light injection and laser-induced sintering are performed.