A method for manufacturing a solar cell and a solar cell
By forming a silicon thin film layer on the outside of the borosilicate glass layer and oxidizing it into a first silicon oxide layer, the oxygen diffusion rate is controlled, which solves the problems of poor doping and sheet resistance uniformity of the boron diffusion layer, and achieves uniform oxidation source absorption treatment and improved doping uniformity of the boron diffusion layer.
Patent Information
- Application Number
- CN202611452409.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-17
- Publication Date
- 2026-11-24
AI Technical Summary
The difference in thermal field uniformity in the tube furnace results in a low doping concentration at the edge of the boron diffusion layer and a high doping concentration in the middle region, leading to poor doping uniformity and sheet resistance uniformity of the boron diffusion layer.
A silicon thin film layer is formed on the outside of the borosilicate glass layer and oxidized into a first silicon oxide layer in an oxygen atmosphere. The oxygen diffusion rate is controlled to make the oxygen distribution uniform at the interface between the boron diffusion layer and the borosilicate glass layer. The uniformity of doping and sheet resistance is improved by adjusting the oxidation source absorption treatment.
Uniform oxidation source absorption treatment was achieved at all locations of the boron diffusion layer, which improved the uniformity of doped boron atoms and the sheet resistance uniformity of the boron diffusion layer, and improved the doping uniformity and sheet resistance uniformity of the boron diffusion layer in the same batch of crystalline silicon substrates.
Smart Images

Figure CN123164875A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a method for preparing a solar cell and the solar cell itself. Background Technology
[0002] For solar cells containing a boron diffusion layer, the boron diffusion layer is generally formed within a diffusion furnace tube by sequentially advancing and oxidizing the boron source layer formed on the surface of the crystalline silicon substrate in an oxygen-free manner. Due to the influence of thermal field uniformity within the diffusion furnace tube (the temperature near the tube wall is higher than the central area of the diffusion furnace), and the longer oxidation absorption time, the oxidation absorption capacity of the edge region of the crystalline silicon substrate near the tube wall is stronger than that of the central region. This means that more boron atoms are deposited in the edge region of the boron diffusion layer, resulting in a significant difference in doping concentration between the edge and central regions (lower doping concentration in the edge region and higher doping concentration in the central region). This leads to the problem of uneven sheet resistance of the boron diffusion layer. Summary of the Invention
[0003] In view of this, the present invention provides a method for preparing a solar cell and a solar cell. The method involves forming a silicon thin film layer on the outside of a borosilicate glass layer and oxidizing the silicon thin film layer into a first silicon oxide layer. The first silicon oxide layer, in conjunction with an oxidation absorption source, enables the oxygen reaching the interface between the boron diffusion layer and the borosilicate glass layer to be uniformly distributed. This allows for uniform oxidation absorption at various locations in the boron diffusion layer, improving both the uniformity of boron atom doping in the final boron diffusion layer and the uniformity of sheet resistance of the boron diffusion layer.
[0004] Specifically, the present invention provides the following technical solutions: In a first aspect, the present invention provides a method for preparing a solar cell, comprising: Step S201: Provide a crystalline silicon substrate; Step S202: A boron diffusion layer and a borosilicate glass layer are formed from the inside to the outside on the first main surface of the crystalline silicon substrate; Step S203: Form a silicon thin film layer on the outside of the borosilicate glass layer; Step S204-1: In an oxygen atmosphere, the silicon thin film layer is oxidized into a first silicon oxide layer, and the boron diffusion layer is subjected to an oxidation source absorption treatment to adjust the boron diffusion layer and thicken the borosilicate glass layer. The first silicon oxide layer is used to regulate the diffusion rate of oxygen so that the oxygen reaching the interface between the boron diffusion layer and the borosilicate glass layer is uniformly distributed. Step S205: Remove the first silicon oxide layer and the thickened borosilicate glass layer.
[0005] Secondly, embodiments of the present invention provide a solar cell, which is prepared based on the preparation method provided in the first aspect embodiments described above.
[0006] The technical solution of the first aspect of the above invention has the following advantages or beneficial effects: The preparation method provided in this invention involves forming a boron diffusion layer and a borosilicate glass layer stacked from the inside to the outside on the first main surface of a crystalline silicon substrate, and forming a silicon thin film layer on the borosilicate glass layer. Because the temperature is high near the furnace wall and decreases towards the center in the diffusion furnace, the silicon thin film layer on the borosilicate glass layer is first oxidized into a first silicon oxide layer under an oxygen atmosphere. The thickness and density of the first silicon oxide layer also decrease from the edge to the center. During the oxidation source absorption process, the high temperature near the furnace wall allows oxygen to enter the interface more actively, while the high thickness and density at the edge of the first silicon oxide layer hinder oxygen from entering the interface. The temperature in the middle region of the diffusion furnace is lower than that near the furnace wall. The intermediate region allows oxygen to have lower activity, while the low thickness and low density of the intermediate region of the first silica layer corresponding to the intermediate region of the diffusion furnace are conducive to oxygen entering the interface. This allows the first silica layer to regulate the oxygen distribution at the interface between the boron diffusion layer and the borosilicate glass layer. That is, the more active oxygen is combined with the edge region of the first silica layer with higher thickness and higher density, and the less active oxygen is combined with the edge region of the first silica layer with lower thickness and lower density. This makes the oxygen distribution at the interface between the boron diffusion layer and the borosilicate glass layer more uniform, so that all positions of the boron diffusion layer can obtain uniform oxidation source treatment, improving the uniformity of boron atoms doped in the final boron diffusion layer and the sheet resistance uniformity of the boron diffusion layer. Attached Figure Description
[0007] Figure 1 This is a schematic diagram illustrating the relative relationship between the crystalline silicon substrate and the boron diffusion layer in existing technology; Figure 2 This is a schematic diagram of the main process of the method for preparing a solar cell provided in an embodiment of the present invention; Figure 3 This is a schematic diagram showing some structural changes in the TOPCon battery prepared by the preparation method provided in this embodiment of the invention; Figure 4 This is a schematic diagram showing partial structural changes in the preparation of the first type of back-contact solar cell using the preparation method provided in this embodiment of the invention. Figure 5 This is a schematic diagram showing partial structural changes in the preparation of a second type of back-contact solar cell using the preparation method provided in this embodiment of the invention. Figure 6 This is a partial cross-sectional structural schematic diagram of a back-contact solar cell provided in an embodiment of the present invention; Figure 7 These are doping concentration curves at different depths in the central and edge regions of the boron diffusion layers prepared in Examples 1, 2, and Comparative Example 1.
[0008] The attached figures are labeled as follows: 10 - Crystalline silicon substrate; 11 - P-type conductive region; 12 - N-type conductive region; 13 - Isolation region; 20 - Boron diffusion layer; 30 - Borosilicate glass layer; 40 - First silicon oxide layer; 40' - Silicon thin film layer; 50 - Tunneling passivation layer; 60 - N-type doped polycrystalline silicon layer; 70 - N-type doped silicon glass layer. Detailed Implementation
[0009] In existing technologies, a boron diffusion layer 20 is typically formed on the surface of a crystalline silicon substrate 10 using thermal diffusion in a tube furnace. Specifically, existing technologies first form a high-concentration boron source layer on the surface of the crystalline silicon substrate 10, then advance boron atoms from the boron source layer to a certain depth in the crystalline silicon substrate 10, and subsequently further heat the substrate to form the boron diffusion layer 20 through oxidation absorption. The doping uniformity, sheet resistance, and uniformity of the boron diffusion layer 20 are affected by the amount of boron atoms doped in the boron diffusion layer 20. This boron doping amount is influenced by the amount of boron source at different locations in the boron source layer, the advancement amount, the advancement depth, and the amount of oxygen absorbed by the oxidation absorption. Research has found that because the temperature is higher near the furnace wall in a tube furnace, and the temperature increases further closer to the furnace wall, there is a significant doping difference between the edge region and the middle region of the final boron diffusion layer 20. Further research revealed that, due to the relatively short temperature and time required for boron source layer deposition and boron atom propulsion, the doping concentration difference between the edge region and the middle region of the boron diffusion layer 20 before oxidation source absorption was not significant after the boron source layer deposition and boron atom propulsion processes. This suggests that, compared to the shorter temperature and time combination of boron source layer deposition and boron atom propulsion, the oxidation source absorption process requires a higher temperature and a longer duration. This results in a greater temperature difference between the region near and away from the furnace wall during oxidation source absorption, leading to a significantly higher concentration and activity of oxygen atoms in the edge region compared to other regions (i.e., regions away from the furnace wall). Consequently, more oxygen atoms participate in oxidation source absorption in the edge region, causing more boron atoms to be absorbed from the boron diffusion layer 20, thus achieving the desired effect. Figure 1 The doping concentration of the edge region 21 of the boron diffusion layer 20 is significantly lower than that of other regions 22 (i.e., regions outside the edge region 21 in the boron diffusion layer 20). Specifically, after oxidation source absorption, in addition to causing excessively low doping concentration in the edge region 21, the boron diffusion layer 20 also exhibits a tendency for the doping concentration to increase from the edge towards the center. Figure 1As shown, the boron diffusion layer 20 increases from the left edge along the K1 direction to the center region, from the right edge along the K3 direction to the center region, from the front edge along the K2 direction to the center region, and from the rear edge along the K3 direction to the center region, resulting in poor doping uniformity and sheet resistance uniformity of the boron diffusion layer 20.
[0010] Generally speaking, in a tube furnace, a batch of silicon substrates 10 is deposited with a boron diffusion layer 20 at a time. The existing process also results in poor doping uniformity and sheet resistance uniformity of the boron diffusion layer 20 deposited on silicon substrates 10 located at different positions in the same batch of tube furnace.
[0011] To address the aforementioned problems of poor doping uniformity and sheet resistance uniformity in the preparation of boron diffusion layers using tube furnaces, this invention provides a method for preparing a solar cell and a solar cell. Specifically, the technical solution provided by this invention mainly improves the preparation process of the boron diffusion layer 20 to obtain a more uniformly doped boron diffusion layer 20.
[0012] Furthermore, the terms "first" and "second" in the embodiments of the present invention are not limitations on the number or order, but are used to distinguish different functional regions, different types of atoms, or different film layers produced by different processing processes or steps. For example, the first silicon oxide layer 40 is a silicon oxide layer formed on the outside of the borosilicate glass layer 30, and the second silicon oxide layer 21 is a silicon oxide layer used to form part of the borosilicate glass layer 30.
[0013] The edge region and the middle region of the tubular furnace involved in the embodiments of the present invention are generally defined as the region near the furnace wall in the radial direction of the tubular furnace as the edge region, and the other regions inside the tubular furnace other than the edge region as the middle region.
[0014] In the embodiments of the present invention, a film layer located on another film layer or a film layer formed on another film layer generally refers to a film layer located on the side of another film layer away from the crystalline silicon substrate 10 or a film layer formed on the side of another film layer away from the crystalline silicon substrate 10.
[0015] In the embodiments of the present invention, "from inside to outside" generally refers to the position in the thickness direction of the solar cell, from the position close to the crystalline silicon substrate 10 to the position away from the crystalline silicon substrate 10.
[0016] Specifically, such as Figure 2 As shown, a method for preparing a solar cell according to an embodiment of the present invention may include the following steps: Step S201: Provide a crystalline silicon substrate 10.
[0017] The silicon substrate 10 can be an N-type silicon substrate or a P-type silicon substrate. Preferably, the silicon substrate 10 is an N-type silicon substrate.
[0018] Step S202: A boron diffusion layer 20 and a borosilicate glass layer 30 are formed on the first main surface of the crystalline silicon substrate 10, stacked from the inside to the outside.
[0019] The formation of the boron diffusion layer 20 and the borosilicate glass layer 30 can be accomplished using existing technologies or using the technical solutions provided in the embodiments of the present invention. The specific implementation schemes for step S202 provided in the embodiments of the present invention will be described in detail later.
[0020] This step is typically performed in a tube furnace, so step S202 can be implemented using existing equipment for solar cell processes without introducing new equipment.
[0021] Step S203: Form a silicon thin film layer 40' on the outside of the borosilicate glass layer 30.
[0022] The step S203, forming the silicon thin film layer 40', can also be completed in a tube furnace. The silicon thin film layer 40' can be one of a polycrystalline silicon layer, a microcrystalline silicon layer, an amorphous silicon layer, or a monocrystalline silicon layer. During the formation of the silicon thin film layer 40' in step S203, hydrogen (H) atoms can also be introduced into the silicon thin film layer 40'. These H atoms can passivate defects in the boron diffusion layer 20.
[0023] It should be noted that the temperature used in step S203 to form the silicon thin film layer 40' is generally relatively low. At a relatively low temperature (generally not higher than 620°C), the uniformity of the formed silicon thin film layer 40' can be guaranteed as much as possible in a tube furnace.
[0024] Step S204-1: Under an oxygen atmosphere, the silicon thin film layer 40' is oxidized into a first silicon oxide layer 40, and the boron diffusion layer 20 is subjected to an oxidation source absorption treatment to adjust the boron diffusion layer 20 and thicken the borosilicate glass layer 30. The first silicon oxide layer 40 is used to control the diffusion rate of oxygen so that the oxygen reaching the interface between the boron diffusion layer 20 and the borosilicate glass layer 30 is uniformly distributed.
[0025] In step S204-1, oxygen atoms first contact the silicon thin film layer 40', oxidizing the silicon thin film layer 40'. After forming the first silicon oxide layer 40, oxygen further enters the interface between the boron diffusion layer 20 and the borosilicate glass layer 30 to complete the oxidation source absorption. Oxidizing the silicon thin film layer 40' into the first silicon oxide layer 40 generally means that oxygen reacts with some of the silicon in the silicon thin film layer 40' to form silicon oxide, thereby converting the silicon thin film layer 40' into the first silicon oxide layer 40.
[0026] It is worth noting that step S204-1 uses a relatively high temperature (generally not lower than 950℃). At this relatively high temperature, there is a relatively high temperature difference between the edge region of the tube furnace (i.e., the region near the furnace wall) and the middle region of the tube furnace (the other regions in the tube furnace excluding the edge region). This high temperature difference causes more oxygen to be distributed in the region near the furnace wall, and the oxygen in the region near the furnace wall has a higher activity level and is more likely to combine with the silicon thin film layer 40'. Therefore, the density and thickness of the edge region of the first silicon oxide layer 40 formed in step S204 are greater than the density and thickness of the middle region of the first silicon oxide layer 40. Compared to the central region of a tube furnace, oxygen is more concentrated in the edge region (near the furnace wall). Furthermore, the oxygen in the edge region is more reactive. This higher reactive oxygen, combined with the higher density and greater thickness of the edge region of the first silica layer 40, reduces the rate at which highly reactive oxygen enters the interface between the boron diffusion layer 20 and the borosilicate glass layer 30 (i.e., the edge region of the first silica layer 40 further reduces the rate at which highly reactive oxygen enters the interface between the boron diffusion layer 20 and the borosilicate glass layer 30). The lower density and thinner thickness of the central region of the first silica layer 40, combined with the lower oxygen content and activity in the central region, has a smaller impact on the rate at which oxygen enters the interface between the boron diffusion layer 20 and the borosilicate glass layer 30. This results in a more balanced rate of oxygen entering the interface between the boron diffusion layer 20 and the borosilicate glass layer 30, allowing for more uniform oxidation source absorption at each location.
[0027] Understandably, the "higher or higher" in the context of the higher or higher oxygen activity in the edge region of a tube furnace is relative to the "lower or lower" in the context of the lower or lower oxygen activity in the middle region of a tube furnace. That is, the oxygen activity in the edge region of a tube furnace is higher or higher than the oxygen activity in the middle region of the tube furnace; correspondingly, the oxygen activity in the middle region of a tube furnace is lower or lower than the oxygen activity in the edge region of the tube furnace.
[0028] Step S205: Remove the first silicon oxide layer 40 and the thickened borosilicate glass layer 30.
[0029] In step S205, the first silicon oxide layer 40 and the thickened borosilicate glass layer 30 can be removed by cleaning with a 20% HF solution for 240 seconds.
[0030] The embodiments of the present invention provide Figure 2The fabrication method shown involves forming a boron diffusion layer 20 and a borosilicate glass layer 30 stacked from the inside to the outside on the first main surface of a crystalline silicon substrate 10, and forming a silicon thin film layer 40' on the borosilicate glass layer 30. Because the temperature is high near the furnace wall and decreases towards the center in the diffusion furnace, the silicon thin film layer 40' on the borosilicate glass layer 30 is first oxidized into a first silicon oxide layer 40 under an oxygen atmosphere. Furthermore, the thickness and density of the first silicon oxide layer 40 decrease from the edge to the center. During the oxidation source absorption process, the high temperature near the furnace wall allows oxygen to have a higher activity at the entry interface, while the high thickness and density at the edge of the first silicon oxide layer 40 block oxygen. When gas enters the interface, the temperature in the middle region of the diffusion furnace is lower. Compared to the region near the furnace wall, the middle region of the diffusion furnace has a lower oxygen activity. The low thickness and low density of the middle region of the first silicon oxide layer 40 corresponding to the middle region of the diffusion furnace are conducive to oxygen entering the interface. This allows the first silicon oxide layer 40 to regulate the oxygen distribution at the interface between the boron diffusion layer 20 and the borosilicate glass layer 30, making the oxygen distribution at the interface between the boron diffusion layer 20 and the borosilicate glass layer 30 more uniform. This results in uniform oxidation source treatment at all positions of the boron diffusion layer 20, improving the uniformity of boron atoms doped in the final boron diffusion layer 20 and the sheet resistance uniformity of the boron diffusion layer 20.
[0031] In addition, the technical solution provided by the embodiments of the present invention can also effectively improve the doping uniformity and sheet resistance uniformity of boron diffusion layers 20 deposited on different silicon substrates 10 in the same batch.
[0032] The preparation method provided in this invention can be used to prepare TOPCon cells or back-contact solar cells.
[0033] For TOPCon cells, after step S204-1 and before step S205, the above-mentioned fabrication method may further include: Step S204-2: sequentially stacking a tunneling passivation layer 50, an N-type doped polycrystalline silicon layer 60, and an N-type doped silicon glass layer 70 on the second main surface of the crystalline silicon substrate 10. Correspondingly, step S205 may also simultaneously remove the N-type doped silicon glass layer 70, thereby forming a boron diffusion layer 20 on the first main surface of the crystalline silicon substrate 10, and forming a tunneling passivation layer 50 and an N-type doped polycrystalline silicon layer 60 stacked from the inside to the outside on the second main surface of the crystalline silicon substrate 10. Understandably, for the TOPCon cell fabrication method, after step S205, a passivation antireflection layer and a metal electrode that burns through the passivation antireflection layer may be further formed on the outer side of the N-type doped polycrystalline silicon layer 60 and the outer side of the boron diffusion layer 20, respectively. The passivation antireflection layer and the metal electrode can be implemented using existing processes, which will not be elaborated here.
[0034] For TOPCon batteries, the structural changes corresponding to each step provided in the embodiments of the present invention are as follows: Figure 3 As shown.
[0035] For a back-contact solar cell, the first main surface of the crystalline silicon substrate 10 is used to form alternating P-type conductive regions 11 and N-type conductive regions 12, and an isolation region 13 located between the P-type conductive regions 11 and N-type conductive regions 12. It is understood that the P-type conductive regions 11, N-type conductive regions 12, and isolation region 13 are formed based on various film layers formed on the first main surface of the crystalline silicon substrate 10; the first main surface of the crystalline silicon substrate 10 itself does not exist. In this embodiment of the invention, there are two fabrication schemes for the back-contact solar cell. In addition to steps S201 to S203, S204-1, and S205 described above, for the first scheme of fabricating the back-contact solar cell, after step S204-1 and before step S205, steps S204-2'1 and S204-2'2 may also be included. For the second scheme of preparing a back contact solar cell, after step S204-1 and before step S205, steps S204-2''1 and S204-2''2 may also be included.
[0036] Specifically, the first method for fabricating a back-contact solar cell includes steps S204-2'1 and S204-2'2: Step S204-2'1: Remove the first silicon oxide layer 40, the thickened borosilicate glass layer 30, and the boron diffusion layer 20 corresponding to the N-type conductive region.
[0037] Specifically, in step S204-2'1, a laser is first used to remove the first silicon oxide layer 40 and the thickened borosilicate glass layer 30 corresponding to the N-type conductive region 12, and then an alkaline solution is used to clean and remove the boron diffusion layer 20 corresponding to the N-type conductive region. It is worth noting that the laser parameters, alkaline solution mass fraction, and cleaning temperature selected in step S204-2'1 can be adjusted according to the thickness, density, and doping concentration of the first silicon oxide layer 40, the thickened borosilicate glass layer 30, and the boron diffusion layer 20; therefore, the laser parameters, alkaline solution mass fraction, and cleaning temperature are not limited here.
[0038] Additionally, in this step, the first silicon oxide layer 40, the thickened borosilicate glass layer 30, and the boron diffusion layer 20 in a localized area along the extension direction of the isolation region 13 can also be removed.
[0039] Step S204-2'2: A tunneling passivation layer 50, an N-type doped polysilicon layer 60, and an N-type doped silicon glass layer 70 are sequentially stacked in the N-type conductive region 12 and the isolation region 13.
[0040] More specifically, the specific implementation of step S204-2'2 may include: sequentially stacking a tunneling passivation layer 50, an N-type doped polysilicon layer 60, and an N-type doped silicon glass layer 70 on the exposed crystalline silicon substrate 10 of the N-type conductive region 12 and on the outside of the remaining first silicon oxide layer 40; removing the N-type doped silicon glass layer 70 located in the P-type conductive region 11 using a laser, and removing the N-type doped polysilicon layer 60 located in the P-type conductive region 11 using an alkaline solution.
[0041] The structural changes corresponding to steps S204-2'1 and S204-2'2 above are as follows: Figure 4 As shown.
[0042] Additionally, in step S204-2'2, a tunneling passivation layer 50, an N-type doped polysilicon layer 60, and an N-type doped silicon glass layer 70 can be formed in a localized region along the extension direction of the isolation region 13. For example, the tunneling passivation layer 50, the N-type doped polysilicon layer 60, and the N-type doped silicon glass layer 70 can be formed on a region in the extension direction of the isolation region 13 where a first silicon oxide layer 40 is locally disposed.
[0043] The structure formed by the above steps S204-2'1 and S204-2'2 can generate weak leakage current or local leakage current in the isolation region 13 to reduce the risk of hot spots on the back contact solar cell.
[0044] Based on steps S204-2'1 and S204-2'2 above, the implementation of step S205 may include: using an HF solution to remove the N-type doped silicon glass layer 70 corresponding to the N-type conductive region 12 and each film layer corresponding to the P-type conductive region 11 and located outside the boron diffusion layer 20, thereby exposing the boron diffusion layer 20 of the P-type conductive region. Based on steps S204-2'1 and S204-2'2 above, the structural change corresponding to step S205 is as follows: Figure 4 As shown.
[0045] from Figure 4 As can be seen, in the back contact solar cell prepared by the first scheme, the isolation region 13 can realize the electrically isolated boron diffusion layer 20 and the N-type doped polycrystalline silicon layer 60 through the tunneling passivation layer 50, the first silicon oxide layer 40 and the thickened borosilicate glass layer 30 located in the isolation region 13, without the need to prepare an additional electrically isolated layer for the back contact solar cell, thus simplifying the preparation process.
[0046] In addition, the second method for fabricating back-contact solar cells includes steps S204-2''1 and S204-2''2: Step S204-2''1: Remove the first silicon oxide layer 40, the thickened borosilicate glass layer 30, and the boron diffusion layer 20 corresponding to the N-type conductive region 12 and the isolation region 13.
[0047] Specifically, in step S204-2''1, a laser is first used to remove the first silicon oxide layer 40 and the thickened borosilicate glass layer 30 corresponding to the N-type conductive region 12 and the isolation region 13. Then, an alkaline solution is used to clean and remove the boron diffusion layer 20 corresponding to the N-type conductive region 12 and the isolation region 13. It is worth noting that the laser parameters, alkaline solution mass fraction, and cleaning temperature selected in step S204-2''1 can be adjusted according to the thickness, density, and doping concentration of the first silicon oxide layer 40, the thickened borosilicate glass layer 30, and the boron diffusion layer 20. Here, the laser parameters, alkaline solution mass fraction, and cleaning temperature are not limited.
[0048] Step S204-2''2: A tunneling passivation layer 50, an N-type doped polysilicon layer 60, and an N-type doped silicon glass layer 70 are sequentially stacked in the N-type conductive region 12.
[0049] More specifically, the specific implementation of step 204-2''2 may include: sequentially stacking a tunneling passivation layer 50, an N-type doped polysilicon layer 60, and an N-type doped silicon glass layer 70 on the outer side of the first main surface of the exposed crystalline silicon substrate 10 in the N-type conductive region 12 and the isolation region 13 and the remaining first silicon oxide layer 40 in the P-type conductive region 11; using a laser to remove the N-type doped silicon glass layer 70 corresponding to the P-type conductive region 11 and the isolation region 13, and using an alkaline solution to remove the N-type doped polysilicon layer 60 corresponding to the P-type conductive region 11 and the isolation region 13.
[0050] The structural changes corresponding to steps S204-2''1 and S204-2''2 above are as follows: Figure 5 As shown.
[0051] Based on steps S204-2''1 and S204-2''2 above, the implementation of step S205 may include: using an HF solution to remove the remaining N-type doped silicon glass layer 70 and the remaining film layers corresponding to the P-type conductive region 11 and located outside the boron diffusion layer 20, as well as the remaining film layers of the isolation region 13, to expose the crystalline silicon substrate of the boron diffusion layer 20 and the isolation region 13. The film layers corresponding to the P-type conductive region 11 and located outside the boron diffusion layer 20 include a first silicon oxide layer 40 and a thickened borosilicate glass layer 30. The remaining film layer of the isolation region 13 is a tunneling passivation layer 50 corresponding to the isolation region 13.
[0052] from Figure 5 As can be seen, in the back-contact solar cell prepared by the second scheme, the isolation region 13 exposes the crystalline silicon substrate 10, realizing the electrically isolated boron diffusion layer 20 and the N-type doped polycrystalline silicon layer 60.
[0053] It should be noted that, regardless of whether the back contact solar cell is prepared using the first or the second method, after step S205, the method may further include: forming a passivation antireflection layer in the P-type conductive region 11, the N-type conductive region 12 and the isolation region 13, and then preparing a metal electrode that is burned through the passivation antireflection layer and electrically connected to the boron diffusion layer 20 of the P-type conductive region 11 and the N-type doped polycrystalline silicon layer 60 of the N-type conductive region 12, respectively.
[0054] It is worth noting that the aforementioned N-type doped polycrystalline silicon layer 60 is generally formed by doping N-type doping atoms (such as phosphorus atoms, arsenic atoms, etc.) into the polycrystalline silicon layer.
[0055] Furthermore, regardless of the type of solar cell (TOPCon or back contact structure) being prepared, the specific implementation schemes for steps S202, S203, and S204-1 are basically the same. The specific implementation schemes for steps S202, S203, and S204-1 are described in detail below.
[0056] Specifically, in the embodiments of the present invention, the specific implementation of the above step S202 may include: step S2021 and step S2022.
[0057] Step S2021: A second silicon oxide layer 21 and a boron source layer 22 are sequentially stacked on the first main surface of the crystalline silicon substrate 10.
[0058] More specifically, the specific implementation of step S2021 may include steps S20211 and S20212: Step S20211: Under the conditions of oxygen flow rate of 5000 sccm to 15000 sccm and temperature of 810℃ to 850℃, a second silicon oxide layer 21 is formed on the first main surface of the crystalline silicon substrate 10.
[0059] For example, the oxygen flow rate for forming the second silicon oxide layer 21 can be 5000 sccm, 8000 sccm, 10000 sccm, or 15000 sccm, etc.; the temperature for forming the second silicon oxide layer 21 can be 810℃, 820℃, 840℃, or 850℃, etc.; and the duration for forming the second silicon oxide layer 21 can be 2 min to 5 min, for example, the duration for forming the second silicon oxide layer 21 can be 2 min, 3 min, 4 min, or 5 min, etc. By coordinating the oxygen flow rate, temperature, and duration, the uniformity of the second silicon oxide layer 21 formed at various locations on the first main surface of the crystalline silicon substrate 10 can be ensured, that is, the thickness and density of the second silicon oxide layer 21 formed at various locations can be kept as consistent as possible, reducing the impact of the temperature difference between the edge region near the furnace wall and the middle region inside the furnace on the deposited second silicon oxide layer 21.
[0060] Step S20212: The boron source layer 22 is formed by sequentially passing through three source treatments.
[0061] More specifically, the conditions for the first source treatment in step S20212 include: an oxygen flow rate of 300 sccm to 600 sccm, a boron source flow rate of 250 sccm to 450 sccm, a nitrogen flow rate carrying the boron source of 3500 sccm to 5500 sccm, a temperature of 810℃ to 850℃, a pressure of 100 to 300 mbar, and a duration of 1 min to 3 min; the conditions for the second source treatment include: an oxygen flow rate of 300 sccm to 600 sccm, a boron source flow rate of 250 sccm to 450 sccm, a nitrogen flow rate carrying the boron source of 3500 sccm to 5500 sccm, a temperature of 830℃ to 850℃, a pressure of 100 to 300 mbar, and a duration of 2 min to 4 min. The conditions for the third source treatment included: an oxygen flow rate of 300 sccm to 600 sccm, a boron source flow rate of 250 sccm to 450 sccm, a nitrogen flow rate carrying the boron source of 3500 sccm to 5500 sccm, a temperature of 830℃ to 880℃, a pressure of 100 to 300 mbar, and a duration of 2 min to 4 min.
[0062] For example, the oxygen flow rate for the first source treatment can be 300 sccm, 400 sccm, 500 sccm, or 600 sccm, etc.; the flow rate of the boron source (such as BCl3, B2H6, or BBr3) can be 250 sccm, 300 sccm, 350 sccm, 400 sccm, or 450 sccm, etc.; the flow rate of the nitrogen carrying the boron source can be 3500 sccm, 4000 sccm, 4500 sccm, 5000 sccm, or 5500 sccm, etc.; the temperature can be 810℃, 820℃, 830℃, 840℃, or 850℃, etc.; the pressure can be 100 mbar, 150 mbar, 200 mbar, 250 mbar, or 300 mbar, etc.; and the duration can be 1 min, 1.5 min, 2 min, 2.5 min, or 3 min, etc. Based on the formation of the second silicon oxide layer 21 in step S20211 above, the temperature of each area in the furnace can be kept basically consistent during the first power supply process. The uniformity of deposition can be ensured by adjusting the temperature, oxygen flow rate, boron source flow rate, nitrogen flow rate carrying the boron source, pressure and duration.
[0063] The oxygen flow rate for the second source treatment can be 300 sccm, 400 sccm, 500 sccm, or 600 sccm, etc.; the flow rate of the boron source (such as BCl3, B2H6, or BBr3) can be 250 sccm, 300 sccm, 350 sccm, 400 sccm, or 450 sccm, etc.; the nitrogen flow rate carrying the boron source can be 3500 sccm, 4000 sccm, 4500 sccm, 5000 sccm, or 5500 sccm, etc.; the temperature can be 830℃, 840℃, or 850℃, etc.; the pressure can be 100 mbar, 150 mbar, 200 mbar, 250 mbar, or 300 mbar, etc.; and the duration can be 1 min, 1.5 min, 2 min, 2.5 min, or 3 min, etc. By further increasing the temperature for the second source treatment based on the first, the temperature of each area within the furnace can be kept as consistent as possible, thus ensuring the uniformity of the deposition. Preferably, based on the first source treatment, only the temperature and duration can be adjusted to enter the second source treatment stage, so as to keep the reaction environment in the furnace as uniform as possible and improve the deposition uniformity of the second source treatment.
[0064] The oxygen flow rate for the third source treatment can be 300 sccm, 400 sccm, 500 sccm, or 600 sccm, etc.; the flow rate of the boron source (such as BCl3, B2H6, or BBr3) can be 250 sccm, 300 sccm, 350 sccm, 400 sccm, or 450 sccm, etc.; the flow rate of the nitrogen carrying the boron source can be 3500 sccm, 4000 sccm, 4500 sccm, 5000 sccm, or 5500 sccm, etc.; the temperature can be 830℃, 840℃, 850℃, 860℃, 870℃, or 880℃, etc.; the pressure can be 100 mbar, 150 mbar, 200 mbar, 250 mbar, or 300 mbar, etc.; and the duration can be 2 min, 2.5 min, 3 min, 3.5 min, or 4 min, etc. Based on the second source treatment described above, a third source treatment is performed with further heating. This can keep the temperature in different areas of the furnace as consistent as possible, thus ensuring the uniformity of the deposition. Preferably, based on the second source treatment, only the temperature and duration are adjusted to enter the third source treatment stage, thereby maintaining a relatively uniform change in the reaction environment inside the furnace, improving the deposition uniformity of the third source treatment, and ensuring the uniformity of the final boron source layer 22.
[0065] Step S2022: Under oxygen-free conditions, boron atoms in the boron source layer 22 are promoted oxygen-free in the first temperature stage, and then the temperature is lowered to the second temperature stage to further promote boron atoms in the boron source layer 22 oxygen-free. The boron atoms enter the crystalline silicon substrate 10 to form a boron diffusion layer 20. The second silicon oxide layer 21 with boron atoms and the boron source layer 22 with reduced boron atoms together constitute the borosilicate glass layer 30.
[0066] Understandably, during the oxygen-free propulsion process, as boron atoms enter the crystalline silicon substrate 10, they pass through the second silicon oxide layer 21. Some boron atoms remain in the second silicon oxide layer 21 and react with it to form borosilicate glass. The boron source layer 22, which is essentially boron-rich borosilicate glass, loses some of its boron atoms after migrating to the crystalline silicon substrate 10 and the second silicon oxide layer 21. This reduces the number of boron atoms in the boron source layer 22, making it part of the borosilicate glass layer 30. Understandably, due to the migration of boron atoms, there is no clear interface between the second silicon oxide layer 21 containing boron atoms and the boron source layer 22 with reduced boron atoms.
[0067] It is worth noting that the oxygen-free conditions can be achieved by replacing the various gases delivered in step S2021 with inert gases, thus creating an oxygen-free environment inside the furnace.
[0068] The conditions for the first temperature stage of oxygen-free propulsion in step S2022 include: a temperature of 880℃~920℃, an inert gas flow rate of 3000sccm~5000sccm, a pressure of 100mbar~300mbar, and a duration of boron atoms in the boron source layer for 5min~15min.
[0069] For example, the temperature for the oxygen-free propulsion control in the first temperature stage can be 880℃, 890℃, 900℃, 910℃, or 920℃, etc.; the inert gas flow rate can be 3000 sccm, 3500 sccm, 4000 sccm, 4500 sccm, or 5000 sccm, etc.; the pressure can be 100 mbar, 150 mbar, 200 mbar, 250 mbar, or 300 mbar, etc.; and the duration can be 5 min, 7 min, 9 min, 10 min, 12 min, or 15 min, etc. That is, based on the third source treatment, increasing the temperature of the oxygen-free propulsion in the first temperature stage can ensure temperature uniformity in various areas of the furnace, so that the amount of boron atoms propagated at each position remains balanced after the first temperature stage of oxygen-free propulsion.
[0070] The conditions for the second temperature stage of oxygen-free propulsion in step S2022 include: the temperature is reduced to 780℃~800℃, the inert gas flow rate is 20000sccm~30000sccm, the pressure is restored to atmospheric pressure, and the duration of boron atoms in the boron source layer during oxygen-free propulsion is 10min~15min.
[0071] For example, the temperature of the oxygen-free propulsion in the second temperature stage can be reduced to 780℃, 790℃, or 800℃. The inert gas flow rate of the oxygen-free propulsion in the second temperature stage can be 20000 sccm, 22000 sccm, 25000 sccm, 28000 sccm, or 30000 sccm, etc., and the duration of boron atom propulsion in the boron source layer can be 10 min, 12 min, 13 min, 14 min, or 15 min, etc. From the first temperature stage to the second temperature stage, the temperature of each region in the furnace can be effectively controlled evenly, and the amount of boron atom propulsion can be effectively controlled within the duration. This, in conjunction with subsequent steps S203 and S204-1, ensures the uniformity of the doped boron diffusion layer 20 and the uniformity of its sheet resistance.
[0072] Further, in this embodiment of the invention, the specific implementation of step S203 may include: depositing a silicon thin film layer using low-temperature plasma chemical vapor deposition under deposition conditions of 570℃~620℃, 180mTorr~260mTorr, silane flow rate of 360sccm~750sccm, nitrogen flow rate of 1000sccm~2000sccm, and deposition time of 2min~6min; optionally, in step S203, the crystalline silicon substrate 10 is continuously heated from room temperature to 570℃~620℃.
[0073] For example, the temperature for depositing the silicon thin film can be 570℃, 580℃, 600℃, 610℃ or 620℃, the pressure can be 180mTorr, 200mTorr, 220mTorr, 240mTorr or 260mTorr, the silane flow rate can be 360sccm, 400sccm, 450sccm, 500sccm, 600sccm, 700sccm or 750sccm, the nitrogen flow rate can be 1000sccm, 1300sccm, 1500sccm, 1800sccm or 2000sccm, and the deposition time can be 2min, 3min, 4min, 5min or 6min.
[0074] By using low-temperature plasma chemical vapor deposition and the above deposition parameters, the uniformity of the deposited silicon thin film layer 40' can be guaranteed.
[0075] More specifically, the thickness of the deposited silicon thin film layer 40' is 20nm to 50nm. For example, the thickness of the silicon thin film layer 40' can be 20nm, 25nm, 30nm, 35nm, 40nm, 45nm, or 50nm, etc. By coordinating the thickness of the silicon thin film layer 40' with step S204-1, it is possible to ensure that the thickness and density of the edge region of the formed first silicon oxide layer 40 are relatively large, and to ensure that the oxygen at the interface between the boron diffusion layer 20 and the borosilicate glass layer 30 is uniformly distributed. In particular, while ensuring the uniform thickness of the deposited silicon thin film layer 40' in step S203, the temperature and oxygen flow rate parameters in step S204-1 can enable more oxygen atoms to recombine in the edge region of the silicon thin film layer 40', thereby increasing the thickness and density of the edge region of the first silicon oxide layer 40. Preferably, the silicon thin film layer 40' deposited by low-temperature plasma chemical vapor deposition is a polycrystalline silicon layer.
[0076] Furthermore, in the embodiments of the present invention, the specific implementation of step S204-1 may include: first oxidizing the silicon thin film layer 40' to form a first silicon oxide layer 40, and then performing an oxidation source absorption treatment on the boron diffusion layer 20.
[0077] Furthermore, in this embodiment of the invention, step S204-1 may further include a stage of heating the silicon thin film layer 40'. This stage of heating the silicon thin film layer 40' occurs before the silicon oxide thin film layer 40'. It can be understood that this stage of heating the silicon thin film layer 40' can simultaneously heat the crystalline silicon substrate 10, the boron diffusion layer 20 formed in step S202, and the borosilicate glass layer 30. Specifically, the conditions for the stage of heating the silicon thin film layer 40' include: the temperature of the reaction environment continuously increasing to 950°C to 1050°C, the pressure of the reaction environment being 100 mbar to 200 mbar, the nitrogen flow rate supplied to the reaction environment being 2000 sccm to 3000 sccm, and the reaction time for forming the first silicon oxide layer being 5 min to 8 min. This process is carried out in a tube furnace. By selecting a tube furnace and continuously raising the temperature to a high level (950℃~1050℃), an environment with a significant temperature difference from the edge to the center is created for the silicon thin film layer 40'. For example, the temperature of this reaction environment can be raised to 950℃, 980℃, 1000℃ or 1050℃, the pressure of the reaction environment can be 100mbar, 120mbar, 150mbar, 180mbar or 200mbar, the nitrogen flow rate can be 2000sccm, 2300sccm, 2500sccm, 2800sccm or 3000sccm, and the reaction time can be 5min, 6min, 7min or 8min. In addition, the above-mentioned heating stage can also create a significant temperature difference between the furnace tube inlet area, the middle section area of the furnace tube, and the tail area of the furnace tube. This allows for the formation of a first silicon oxide layer 40 with higher density and thickness in the edge area in step S204-1. Furthermore, there are certain differences in the first silicon oxide layer 40 formed on the crystalline silicon substrate 10 in different areas of the furnace tube. The differences in the first silicon oxide layer 40 formed on the crystalline silicon substrate 10 in different areas of the furnace tube match the oxygen distribution in the furnace tube. This can reduce the difference in the oxidation absorption source of the boron diffusion layer 20 on the crystalline silicon substrate 10 in different areas of the furnace tube, reduce the difference between the boron diffusion layers 20 on different crystalline silicon substrates 10 of the same batch produced in the same furnace tube, and thus improve the uniformity of the boron diffusion layers 20 of the same batch produced in the same furnace tube.
[0078] In an optional embodiment, the reaction conditions in step S204-1 include: an oxygen flow rate of 18000 sccm to 26000 sccm supplied to the reaction environment, an oxidation temperature of 1000℃ to 1050℃, a reaction environment pressure of 600 mbar to 850 mbar, and a duration of 60 min to 100 min; optionally, the temperature rise rate of the heating source is 10℃ / min to 20℃ / min. For example, the oxygen flow rate can be 18000 sccm, 20000 sccm, 22000 sccm, 25000 sccm, or 26000 sccm, etc.; the oxidation temperature can be 1000℃, 1020℃, or 1050℃, etc.; the pressure can be 600 mbar, 650 mbar, 700 mbar, 750 mbar, 800 mbar, or 850 mbar, etc.; the duration can be 60 min, 70 min, 80 min, 90 min, or 100 min, etc.; and the heating rate can be 10℃ / min, 12℃ / min, 15℃ / min, 1... The reaction conditions, such as 8℃ / min or 20℃ / min, can be combined to first convert the silicon thin film layer 40' into the first silicon oxide layer 40, and can make the edge region of the first silicon oxide layer 40 more dense and thicker. After the first silicon oxide layer 40 is formed, oxidation source absorption (the oxidation source absorption is a heated source absorption) is performed. Through the formed first silicon oxide layer 40, it can be ensured that the oxygen at the interface between the boron diffusion layer 20 and the borosilicate glass layer 30 is uniformly distributed, effectively reducing the doping concentration difference between the edge region and the middle region of the formed boron diffusion layer 20, thereby improving the doping uniformity and sheet resistance uniformity of the boron diffusion layer 20.
[0079] In addition, the oxidation source absorption treatment in step S204-1 can also involve first heating up to absorb the source, and then cooling down to absorb the source. That is, step S204-1 also includes a cooling source absorption stage.
[0080] Specifically, after the aforementioned heating and absorption phase, a cooling and absorption phase begins. The conditions for this cooling and absorption phase in step S204-1 include: the reaction environment cooling to 790℃~800℃, the reaction environment pressure returning to atmospheric pressure, and the duration of the cooling and absorption phase being 40min~50min. Furthermore, the oxygen flow rate during this cooling and absorption phase can be 10000sccm~20000sccm. For example, the temperature can be lowered to 790℃ or 800℃, the duration of the cooling and absorption phase can be 40min, 45min, or 50min, and the oxygen flow rate can be 10000sccm, 12000sccm, 15000sccm, 18000sccm, or 20000sccm, etc. As the temperature decreases from a higher temperature to a lower temperature, the first silicon oxide layer 40 can further balance the differences in oxygen distribution and oxygen activity caused by the temperature difference between the edge region and the middle region, so that the oxygen reaching the interface between the boron diffusion layer 20 and the borosilicate glass layer 30 is evenly distributed, thereby further improving the doping uniformity and sheet resistance uniformity of the formed boron diffusion layer 20, improving the contact uniformity between the metal electrode and the boron diffusion layer 20, and improving the fill factor, open circuit voltage and conversion efficiency of the battery.
[0081] Furthermore, in this embodiment of the invention, after the heating and absorption of the source in step S204-1, the process can directly proceed to the cooling and unloading stage. Specifically, the conditions for the cooling and unloading stage include: the ambient temperature dropping to 790℃~800℃, the pressure returning to atmospheric pressure, and the cooling duration being 40min~50min. Additionally, the nitrogen flow rate during this cooling stage can be 10000sccm~20000sccm. For example, the temperature can be lowered to 790℃ or 800℃, the cooling duration can be 40min, 45min, or 50min, and the nitrogen flow rate can be 10000sccm, 12000sccm, 15000sccm, 18000sccm, or 20000sccm, etc.
[0082] In addition, the solution for improving the doping uniformity and sheet resistance uniformity of the boron diffusion layer 20 provided by the embodiments of the present invention is simple and easy to industrialize.
[0083] It is worth noting that the process of thickening the borosilicate glass layer 30 in step S204-1 is as follows: after oxygen atoms enter the interface between the boron diffusion layer 20 and the borosilicate glass layer 30, the oxygen atoms recombine with the outer part of the boron diffusion layer 20 to form borosilicate glass, while simultaneously drawing out some boron atoms from the inner part of the boron diffusion layer 20.
[0084] Furthermore, embodiments of the present invention provide a solar cell. This solar cell is prepared based on the preparation method provided in any of the above embodiments.
[0085] More specifically, the solar cell can be a TOPCon cell. The TOPCon cell may include: a crystalline silicon substrate 10, a boron diffusion layer 20 disposed on a first main surface of the crystalline silicon substrate 10, and a tunneling passivation layer 50 and an N-type doped polycrystalline silicon layer 60 stacked from the inside to the outside on a second main surface of the crystalline silicon substrate 10. Additionally, the TOPCon cell may further include: passivation and antireflection layers disposed outside the boron diffusion layer 20 and outside the N-type doped polycrystalline silicon layer 60, respectively, and metal electrodes penetrating the passivation and antireflection layers in the thickness direction and electrically connected to the boron diffusion layer 20 and the N-type doped polycrystalline silicon layer 60, respectively.
[0086] This solar cell can also be a back-contact solar cell. There are two possible structures for back-contact solar cells.
[0087] Specifically, such as Figure 6 As shown, the first type of back-contact solar cell may include: a crystalline silicon substrate 10, wherein a first main surface of the crystalline silicon substrate 10 is alternately arranged with P-type conductive regions 11 and N-type conductive regions 12, and an isolation region 13 disposed between adjacent P-type conductive regions 11 and N-type conductive regions 12. The P-type conductive region 11 is provided with a boron diffusion layer 20, and the N-type conductive region 12 is provided with a tunneling passivation layer 50 and an N-type doped polycrystalline silicon layer 60 stacked from the inside to the outside. The boron diffusion layer 20 extends to the isolation region 13, and the tunneling passivation layer 50 and the N-type doped polycrystalline silicon layer 60 extend to the isolation region 13. The tunneling passivation layer 50 and the N-type doped polycrystalline silicon layer 60 are located outside the boron diffusion layer 20. In the isolation region 13, between the tunneling passivation layer 50 and the boron diffusion layer 20, there is also a borosilicate glass layer 30 and a first silicon oxide layer 40 stacked from the inside to the outside. This structure can form a weak leakage current in the isolation region 13 to reduce the risk of hot spots in the back contact solar cell. The boron diffusion layer 20 extending to the isolation region 13, as well as the tunneling passivation layer 50 and the N-type doped polycrystalline silicon layer 60 extending to the isolation region 13, can exist only in a portion of the isolation region 13, so that a localized weak leakage current is formed between the boron diffusion layer 20 extending to the isolation region 13 and the N-type doped polycrystalline silicon layer 60 in the N-type conductive region 12, thereby reducing the risk of hot spots on the back contact solar cell.
[0088] The second type of back-contact solar cell may include: a crystalline silicon substrate 10, wherein a first main surface of the crystalline silicon substrate 10 is alternately arranged with P-type conductive regions 11 and N-type conductive regions 12, and an isolation region 13 disposed between adjacent P-type conductive regions 11 and N-type conductive regions 12. The P-type conductive regions 11 are provided with a boron diffusion layer 20, and the N-type conductive regions 12 are provided with a tunneling passivation layer 50 and an N-type doped polycrystalline silicon layer 60 stacked from the inside to the outside, wherein the boron diffusion layer 20, the tunneling passivation layer 50 and the N-type doped polycrystalline silicon layer 60 do not cover the isolation region 13.
[0089] Furthermore, for the two back-contact solar cells described above, it may also include: a passivation and antireflection layer disposed in the P-type conductive region 11, the N-type conductive region 12 and the isolation region 13, and a metal electrode that penetrates the passivation and antireflection layer in the thickness direction and is electrically connected to the outer side of the boron diffusion layer 20 and the N-type doped polycrystalline silicon layer 60, respectively.
[0090] The technical solutions provided by the embodiments of the present invention are described in detail below with test results from multiple examples and two comparative examples.
[0091] Example 1: Step A1, Preparation Stage: The temperature inside the tube of the tubular furnace is set at 820℃, and the flow rate of nitrogen is 2000 scm.
[0092] Step B1: Boat loading. The quartz boat carrying the silicon wafer is placed into the furnace tube. The running time is 6 minutes, and the temperature inside the furnace tube is set to 820℃.
[0093] Step C1: Vacuuming. The furnace tubes are evacuated to the set vacuum level by a vacuum pump, and the pressure inside the furnace is 180 mbar.
[0094] Step D1, pre-oxidation: The temperature inside the furnace tube is maintained at 820℃, the oxygen flow rate is 5000 sccm, and the oxidation duration is 3.5 min, forming a second silicon oxide layer on the two main surfaces of the silicon wafer.
[0095] Step E1: Initial power supply. The temperature inside the furnace tubes is 820℃, the oxygen flow rate is 420 sccm, the boron source flow rate is 250 sccm, and the nitrogen carrying the boron source has a flow rate of 5000 sccm for 2 minutes. After power supply, the furnace tubes are purged with purging nitrogen at a flow rate of 300 sccm and furnace door nitrogen at a flow rate of 1000 sccm for 5 minutes, maintaining the tube pressure at 180 mbar.
[0096] F1. Second power supply: The temperature inside the furnace tube is 835℃, the oxygen flow rate is 510 sccm, the boron source flow rate is 280 sccm, and the nitrogen carrying the boron source has a flow rate of 5500 sccm for 2 minutes. After power supply, the furnace tube is purged with purging nitrogen at a flow rate of 300 sccm and furnace door nitrogen at a flow rate of 1000 sccm for 5 minutes.
[0097] G1. Third power supply: The temperature inside the furnace tube is 845℃, the oxygen flow rate is 510 sccm, the boron source flow rate is 280 sccm, and the nitrogen carrying the boron source has a flow rate of 5500 sccm for 2 minutes. After power supply, the furnace tube is purged with purging nitrogen at a flow rate of 300 sccm for 5 minutes, forming a boron source layer on the outer side of the second silicon oxide layer on both main surfaces of the silicon wafer.
[0098] H1. Heating is promoted, and the furnace tube temperature is increased from 845℃ to 890℃ for 10 minutes to form the initial boron diffusion layer. The second silicon oxide layer is converted into a borosilicate glass layer.
[0099] I1. The furnace tube is cooled down and the boat is removed. The furnace tube temperature drops to 780℃, the nitrogen flow rate is 20000sccm, the furnace tube pressure is restored to atmospheric pressure, the furnace door is opened, and the quartz boat is pulled out of the furnace tube, thus ending the boron expansion process.
[0100] J1. In the preparation stage of depositing polycrystalline silicon layer (i.e. silicon thin film layer) using low-temperature plasma chemical vapor deposition (LPCVD), after the silicon wafer is cooled to near room temperature, it is reintroduced into the LPCVD furnace tube. After the furnace tube is evacuated and leak-tested, the pressure reaches 220 mtorr, the temperature rises to 600℃, the nitrogen flow rate is 2000 sccm, and the heating duration is 5 min.
[0101] K1. Polycrystalline silicon layer (i.e. silicon thin film layer) deposition: silane flow rate is 480 sccm, nitrogen flow rate is 1000 sccm, deposition temperature is 600℃, pressure inside furnace tube is 220 mtorr, deposition time is 3 min. Polycrystalline silicon layer is deposited on the outside of borosilicate glass layer on the two main surfaces of silicon wafer, and the thickness of the deposited polycrystalline silicon layer is 20 nm.
[0102] L1, cooling, unloading: The furnace tube temperature of LPCVD is reduced to 550℃, the nitrogen flow rate is 10000 sccm, the pressure inside the furnace tube is restored to 1060 mtorr, and the duration is 10 minutes. After unloading, the silicon wafer temperature is reduced to close to room temperature.
[0103] M1, Inlet, Vacuuming, Heating: When the silicon wafer is cooled to near room temperature, it is reintroduced into the tube furnace. After the tube is evacuated and leak-tested, the pressure reaches 200 mbar. Subsequently, the temperature inside the tube is raised to 950°C, the nitrogen flow rate is 2000 sccm, and the heating duration is 5 minutes.
[0104] N1, oxidation source: Under the condition of oxygen flow rate of 20000 sccm, the furnace tube temperature is raised and maintained at 1045℃, the pressure inside the furnace tube is increased to 800 mbar, the polycrystalline silicon layer is converted into the first silicon oxide layer, and oxidation source is continued at constant temperature. The entire oxidation source duration is 85 min, thickening the borosilicate glass layer.
[0105] O1. Cooling and pressure return: The furnace tube temperature drops to 790℃, and 20000sccm of nitrogen is introduced. The pressure inside the furnace tube is restored to atmospheric pressure, and the quartz boat is pushed out of the furnace tube.
[0106] P1. Use a 7% HF solution to remove the first silicon oxide layer and the thickened borosilicate glass layer from the first and second main surfaces of the silicon wafer, and use a 10% NaOH solution to remove the boron diffusion layer from the second main surface of the silicon wafer, so that only the boron diffusion layer exists on the first main surface of the silicon wafer, and the second main surface of the silicon wafer is exposed.
[0107] Example 2: The difference from Example 1 is that the temperature in step J1 is increased to 605°C, the silane flow rate in step K1 is 500 sccm, the deposition temperature is 610°C, the pressure inside the furnace tube is 220 mtorr, the deposition time is 4 min, and the thickness of the deposited polycrystalline silicon layer is 35 nm.
[0108] Example 3: The difference from Example 1 is that the nitrogen in O1 is replaced with oxygen.
[0109] Example 4: The difference from Example 2 is that nitrogen in O1 is replaced with oxygen.
[0110] Example 5: The difference from Example 1 is that P1 is omitted, and Q1, R1 and S1 are executed sequentially after O1.
[0111] Q1. A tunneling passivation layer, a phosphorus-doped polycrystalline silicon layer, and a phosphorus-silicon glass layer are sequentially stacked on the second main surface of a silicon wafer and the outer side of the first silicon oxide layer on the first main surface of the silicon wafer using low-temperature chemical vapor deposition.
[0112] R1. The phosphorus silicate glass layer on the first main surface of the silicon wafer is removed using a 7% HF solution, and the phosphorus-doped polysilicon layer on the first main surface of the silicon wafer is removed using a 10% NaOH solution. Then, the tunneling passivation layer, the first silicon oxide layer, and the thickened borosilicate glass layer on the first main surface of the silicon wafer, as well as the phosphorus silicate glass layer on the second main surface of the silicon wafer, are removed using a 7% HF solution.
[0113] S1. Low-temperature chemical vapor deposition is used to deposit an aluminum oxide passivation layer on the outer side of the phosphorus-doped polycrystalline silicon layer on the second main surface of the silicon wafer and on the outer side of the boron diffusion layer on the first main surface of the silicon wafer. A silver paste is then printed and sintered to form a silver metal electrode in contact with the phosphorus-doped polycrystalline silicon layer and a silver metal electrode in contact with the boron diffusion layer.
[0114] The processing parameters used in steps Q1, R1, and S1 above are all conventional parameters in the prior art.
[0115] Example 6
[0116] The difference from Example 5 is that the temperature in step J1 is increased to 605°C, the silane flow rate in step K1 is 500 sccm, the deposition temperature is 610°C, the pressure inside the furnace tube is 220 mtorr, the deposition time is 4 min, and the thickness of the deposited polycrystalline silicon layer is 35 nm. That is, Example 6 is based on Example 2, where a passivation layer is deposited and a metal electrode is prepared.
[0117] Comparative Example 1: The difference from Example 1 is that steps J1 to L1 are omitted.
[0118] Comparative Example 2: The difference from Example 5 is that steps J1 to L1 are omitted.
[0119] The sheet resistance of Examples 1, 2, 3, and 4 was tested using a four-probe sheet resistance tester. The specific testing process was as follows: The furnace tube was divided into three temperature zones: the furnace mouth temperature zone (zone 1 in Table 1), the furnace middle section temperature zone (zone 3 in Table 1), and the furnace tail section temperature zone (zone 5 in Table 1). Three products were randomly selected from each temperature zone, and the sheet resistance of the middle region and the four edge regions of these three randomly selected products were measured using the four-probe sheet resistance tester. The sheet resistance of the four edge regions and the middle region, the mean sheet resistance within the sheet, the quantified uniformity of the sheet resistance within the sheet, the mean sheet resistance within the tube, and the quantified uniformity of the sheet resistance within the tube were calculated using the sheet resistance of the three randomly selected products within the same temperature zone.
[0120] Specifically, the sheet resistance of the middle area and the edge area of products in different temperature zones is calculated using the following formula (1).
[0121] (1)
[0122] in, Indicates the temperature range Product area The obstruction; Indicates temperature zone Temperature zone The values are taken as follows: furnace mouth temperature zone (i.e., temperature zone 1 in Table 1 below), furnace middle section temperature zone (i.e., temperature zone 3 in Table 1 below), and furnace tail section temperature zone (i.e., temperature zone 5 in Table 1 below). Indicates different areas of the product. The values are: center (center in Table 1 below), edge region 1 (edge1 in Table 1 below), edge region 2 (edge2 in Table 1 below), edge region 3 (edge3 in Table 1 below), and edge region 4 (edge4 in Table 1 below). In the temperature range The sequential number of the randomly selected products. For example, if 3 products are selected, their sequential numbers are 1, 2 and 3.
[0123] Furthermore, the average sheet resistance of products in different temperature zones is calculated using the following formula (2).
[0124] (2)
[0125] in, Indicates the temperature range The average sheet resistance of the products within the product range; Indicates temperature zone Temperature zone The values are taken as follows: furnace mouth temperature zone (i.e., temperature zone 1 in Table 1 below), furnace middle section temperature zone (i.e., temperature zone 3 in Table 1 below), and furnace tail section temperature zone (i.e., temperature zone 5 in Table 1 below). Indicates different areas of the product. The values are: center (center in Table 1 below), edge region 1 (edge1 in Table 1 below), edge region 2 (edge2 in Table 1 below), edge region 3 (edge3 in Table 1 below), and edge region 4 (edge4 in Table 1 below).
[0126] The quantification value of the uniformity of sheet resistance within the chip of products in different temperature zones is calculated using the following formula (3).
[0127] (3)
[0128] in, Indicates the temperature range Quantitative value of the uniformity of sheet resistance within the product; Indicates the temperature range The average sheet resistance of the products within the product range; Indicates the temperature range Various areas of the products within The maximum value in the square resistance; Indicates the temperature range Various areas of the products within The minimum value of the square resistance.
[0129] The average sheet resistance inside the tube is calculated using the following formula (4).
[0130] (4)
[0131] in, This represents the average sheet resistance inside the tube.
[0132] The quantification value of the uniformity of sheet resistance inside the tube is calculated using the following formula (5).
[0133] (5)
[0134] in, This represents the quantified value of the uniformity of sheet resistance within the tube. This represents the average sheet resistance inside the tube; Indicates the various temperature zones Various areas of the products within The maximum value in the square resistance; Indicates the various temperature zones Various areas of the products within The minimum value of the square resistance.
[0135] Based on the calculation formula (1) above, the middle region (center in Table 1 below), edge region 1 (edge1 in Table 1 below), edge region 2 (edge2 in Table 1 below), edge region 3 (edge3 in Table 1 below), and edge region 4 (edge4 in Table 1 below) of the products in different temperature zones of Examples 1 to 4 were calculated. The comparison results show that the results of Example 1 and Example 3 are similar, and the results of Example 2 and Example 4 are similar. Therefore, whether or not cooling is performed after heating to absorb the source has no significant impact on the sheet resistance. For easier comparison, Table 1 only shows the sheet resistance calculation results of Example 1, Example 2, and Comparative Example 1.
[0136] Table 1
[0137] The larger the sheet resistance uniformity quantification value, the worse the sheet resistance uniformity of the boron diffusion layer, resulting in a smaller contact matching window between the Ag paste and the boron emitter after metallization, and thus poorer contact performance. Comparing the calculation results of Examples 1 and 2 in Table 1, it can be seen that increasing the thickness of the silicon thin film layer is beneficial for improving both on-wafer and in-tube uniformity. Comparing the calculation results of Examples 1 and 2 with those of Comparative Example 1, the boron diffusion layer obtained by the method provided in this invention exhibits better sheet resistance uniformity in both on-wafer and in-tube applications.
[0138] Furthermore, the doping concentration at different depths (depths from the surface of the boron diffusion layer) of the central and edge regions of multiple products randomly selected from Examples 1, 2, and Comparative Example 1 were detected. Using the doping concentration at the same depth in the central region of the multiple products of Example 1, the average doping concentration at one depth in the central region of Example 1 was calculated. Similarly, using the doping concentration at the same depth in each edge region of the multiple products of Example 1, the average doping concentration at one depth in the edge region of Example 1 was calculated. Likewise, using the doping concentration at the same depth in the central region of the multiple products of Example 2, the average doping concentration at one depth in the central region of Example 2 was calculated. Similarly, using the doping concentration at the same depth in each edge region of the multiple products of Example 2, the average doping concentration at one depth in the edge region of Example 2 was calculated. Using the doping concentration at the same depth in the central region of the multiple products of Comparative Example 1, the average doping concentration at one depth in the central region of Comparative Example 1 was calculated. Using the doping concentration at the same depth in each edge region of the multiple products of Comparative Example 1, the average doping concentration at one depth in the edge region of Comparative Example 1 was calculated. Based on the calculated average doping concentration, doping concentration curves at different depths were plotted for Examples 1, 2, and Comparative Example 1, as shown below. Figure 7 As shown. From Figure 7 It can be seen that the surface doping concentration of the edge region of Comparative Example 1 is significantly lower than that of the middle region. Even at shallower depths (especially less than 0.3 μm), the doping concentration of the edge region of Comparative Example 1 is also significantly lower than that of the middle region. In contrast, the surface doping concentrations of the edge regions and the middle regions of the products in Examples 1 and 2 are similar, indicating that the technical solution provided by the embodiments of the present invention can effectively improve the doping uniformity of the boron diffusion layer surface in both the edge and middle regions.
[0139] Furthermore, for the products prepared in Examples 5, 6, and Comparative Example 2, three products were randomly selected from each of the three temperature zones (furnace mouth zone, furnace middle section zone, and furnace tail zone), resulting in nine products. The contact resistivity between the boron diffusion layer and the Ag metal electrode was measured using the Transfer Length Method (TLM). The mean contact resistivity of Examples 5, 6, and Comparative Example 2 was calculated using the following formula (6), and the standard deviation of the contact resistivity of Examples 5, 6, and Comparative Example 2 was calculated using the following formula (7).
[0140] (6)
[0141] in, Indicates group The average contact resistivity of this group; These are Example 5, Example 6, and Comparative Example 2, respectively. Indicates the detected group The selected number Contact resistivity between the boron diffusion layer and the Ag metal electrode of each product; By group The nine selected products were numbered sequentially.
[0142] (7)
[0143] in, Indicates group The standard deviation of contact resistivity; Indicates group The average contact resistivity of this group; These are Example 5, Example 6, and Comparative Example 2, respectively. Indicates the detected group The selected number Contact resistivity between the boron diffusion layer and the Ag metal electrode of each product; By group The nine selected products were numbered sequentially.
[0144] The mean and standard deviation of contact resistivity for Examples 5, 6 and Comparative Example 2 are shown in Table 2 below.
[0145] Table 2
[0146] Contact resistivity represents the contact resistance per unit area between the boron diffusion layer and the Ag metal electrode, which directly affects the conductivity of the contact point. A lower contact resistivity indicates better contact performance between the boron diffusion layer and the Ag metal electrode. Table 2 shows that the boron diffusion layer obtained by the method provided in this embodiment has a more uniform sheet resistance, resulting in a lower contact resistivity and better convergence. In particular, the calculation results of Example 6 are better than those of Example 5, indicating that increasing the thickness of the silicon thin film layer is beneficial for improving the sheet resistance uniformity of the boron diffusion layer, thereby improving the contact performance between the boron diffusion layer and the Ag metal electrode.
[0147] Furthermore, for the products prepared in Examples 5, 6, and Comparative Example 2, three products were randomly selected from each of the three temperature zones (furnace mouth zone, furnace middle section zone, and furnace tail zone), resulting in nine products. The performance of each product was tested using Current-Voltage Measurement (IV) to obtain the open-circuit voltage (Voc), fill factor (FF), photoelectric conversion efficiency (Eta), and parallel resistance (Rsh) for each product. The mean values of each performance characteristic of Example 5 were calculated using the test results of the nine products in Example 5; the mean values of each performance characteristic of Example 6 were calculated using the test results of the nine products in Example 6; and the mean values of each performance characteristic of Comparative Example 2 were calculated using the test results of the nine products in Comparative Example 2. The results are shown in Table 3.
[0148] Table 3
[0149] As can be seen from Table 3, compared with Comparative Example 2, the open-circuit voltage, fill factor, photoelectric conversion efficiency and parallel resistance of Examples 5 and 6 are significantly better, indicating that the technical solution provided by the embodiments of the present invention can improve the open-circuit voltage, fill factor, photoelectric conversion efficiency and parallel resistance while improving the uniformity of the boron diffusion layer.
[0150] The above steps are provided only to help understand the method, structure, and core ideas of this invention. Those skilled in the art can make various improvements and modifications to this invention without departing from its principles, and these improvements and modifications also fall within the scope of protection of the claims.
Claims
1. A method for preparing a solar cell, characterized in that, include: Step S201: Provide a crystalline silicon substrate (10); Step S202: A boron diffusion layer (20) and a borosilicate glass layer (30) are formed from the inside to the outside on the first main surface of the crystalline silicon substrate (10). Step S203: Form a silicon thin film layer (40') on the outside of the borosilicate glass layer (30); Step S204-1: In an oxygen atmosphere, the silicon thin film layer (40') is oxidized into a first silicon oxide layer (40), and the boron diffusion layer (20) is subjected to an oxidation source absorption treatment to adjust the boron diffusion layer (20) and thicken the borosilicate glass layer (30). The first silicon oxide layer (40) is used to regulate the diffusion rate of oxygen so that the oxygen reaching the interface between the boron diffusion layer (20) and the borosilicate glass layer (30) is uniformly distributed. Step S205: Remove the first silicon oxide layer (40) and the thickened borosilicate glass layer (30).
2. The preparation method according to claim 1, characterized in that, After step S204-1 and before step S205, the method further includes: step S204-2, in which a tunneling passivation layer (50), an N-type doped polycrystalline silicon layer (60) and an N-type doped silicon glass layer (70) are sequentially stacked on the second main surface of the crystalline silicon substrate (10).
3. The preparation method according to claim 1, characterized in that, The first main surface of the crystalline silicon substrate (10) is used to provide alternating P-type conductive regions (11) and N-type conductive regions (12) and an isolation region (13) located between the P-type conductive regions (11) and the N-type conductive regions (12). After step S204-1 and before step 5, the following is also included: Step S204-2'1: Remove the first silicon oxide layer (40), the thickened borosilicate glass layer (30), and the boron diffusion layer (20) corresponding to the N-type conductive region (12). Step S204-2'2: A tunneling passivation layer (50), an N-type doped polysilicon layer (60), and an N-type doped silicon glass layer (70) are sequentially stacked in the N-type conductive region (12) and the isolation region (13). Optionally, step S204-2'2 includes: sequentially stacking a tunneling passivation layer (50), an N-type doped polysilicon layer (60), and an N-type doped silicon glass layer (70) on the exposed crystalline silicon substrate (10) of the N-type conductive region (12) and on the outside of the remaining first silicon oxide layer (40); removing the N-type doped silicon glass layer (70) located in the P-type conductive region (11) using a laser, and removing the N-type doped polysilicon layer (60) located in the P-type conductive region (11) using an alkaline solution; Step S205 includes: using an HF solution to remove the N-type doped silicon glass layer (70) corresponding to the N-type conductive region (12) and each film layer corresponding to the P-type conductive region (11) and located outside the boron diffusion layer (20), so as to expose the boron diffusion layer (20) of the P-type conductive region.
4. The preparation method according to claim 1, characterized in that, The first main surface of the crystalline silicon substrate (10) is used to provide alternating P-type conductive regions (11) and N-type conductive regions (12) and an isolation region (13) located between the P-type conductive regions (11) and the N-type conductive regions (12). After step S204-1 and before step S205, the method further includes: Step S204-2''1: Remove the first silicon oxide layer (40), the thickened borosilicate glass layer (30), and the boron diffusion layer (20) corresponding to the N-type conductive region (12) and the isolation region (13). Step S204-2''2: A tunneling passivation layer (50), an N-type doped polysilicon layer (60), and an N-type doped silicon glass layer (70) are sequentially stacked in the N-type conductive region (12); Optionally, step S204-2''2 includes: a tunneling passivation layer (50), an N-type doped polysilicon layer (60), and an N-type doped silicon glass layer (70) are sequentially stacked on the first main surface of the exposed crystalline silicon substrate (10) in the N-type conductive region (12) and the isolation region (13) and on the outside of the remaining first silicon oxide layer (40) in the P-type conductive region (11); the N-type doped silicon glass layer (70) corresponding to the P-type conductive region (11) and the isolation region (13) is removed by laser, and the N-type doped polysilicon layer (60) corresponding to the P-type conductive region (11) and the isolation region (13) is removed by alkaline solution; Step S205 includes: using an HF solution to remove the remaining N-type doped silicon glass layer (70) and each film layer corresponding to the P-type conductive region (11) and located outside the boron diffusion layer (20) and the remaining film layer of the isolation region (13), so as to expose the crystalline silicon substrate of the boron diffusion layer (20) of the P-type conductive region and the isolation region (13).
5. The preparation method according to any one of claims 1 to 4, characterized in that, Step S203 includes: depositing the silicon thin film layer (40') using low-temperature plasma chemical vapor deposition under deposition conditions of 570℃~620℃, 180mTorr~260mTorr, silane flow rate of 360sccm~750sccm, nitrogen flow rate of 1000sccm~2000sccm, and deposition time of 2min~6min; Optionally, in step S203, the crystalline silicon substrate (10) is continuously heated from room temperature to 570℃~620℃; And / or, The thickness of the silicon thin film layer (40') is 20nm~50nm; And / or, The silicon thin film layer (40') is one of a polycrystalline silicon layer, a microcrystalline silicon layer, an amorphous silicon layer, and a monocrystalline silicon layer.
6. The preparation method according to any one of claims 1 to 4, characterized in that, Step S204-1 includes: first oxidizing the silicon thin film layer (40') into a first silicon oxide layer (40), and then performing an oxidation source absorption treatment on the boron diffusion layer (20); Optionally, step S204-1 further includes a stage of heating the silicon thin film layer (40'), wherein the conditions for heating the silicon thin film layer (40') include: the temperature continuously rising to 950°C to 1050°C, the pressure being 100 mbar to 200 mbar, the nitrogen flow rate being 2000 sccm to 3000 sccm, and the heating time being 5 min to 8 min; Optionally, the reaction conditions in step S204-1 include: an oxygen flow rate of 18000 sccm to 26000 sccm in the reaction environment, an oxidation temperature of 1000℃ to 1050℃, a pressure of 600 mbar to 850 mbar in the reaction environment, and a duration of 60 min to 100 min; optionally, the heating rate of the oxidation temperature is 10℃ / min to 20℃ / min. Optionally, step S204-1 may also include a cooling and absorption phase, the conditions of which include: the reaction environment is cooled to 790°C to 800°C, the pressure of the reaction environment is restored to atmospheric pressure, and the duration of cooling and absorption is 40 min to 50 min.
7. The preparation method according to any one of claims 1 to 4, characterized in that, Step S202 includes: Step S2021: A second silicon oxide layer (21) and a boron source layer (22) are sequentially stacked on the first main surface of the crystalline silicon substrate (10). Step S2022: Under oxygen-free conditions, the boron atoms in the boron source layer (22) are promoted oxygen-free in the first temperature stage, and the temperature is lowered to the second temperature stage to further promote the boron atoms in the boron source layer (22) oxygen-free. The boron atoms enter the crystalline silicon substrate (10) to form the boron diffusion layer (20). The second silicon oxide layer (21) with boron atoms and the boron source layer (22) with reduced boron atoms together constitute the borosilicate glass layer (30).
8. The preparation method according to claim 7, characterized in that, The conditions for the first temperature stage of step S2022 for oxygen-free propulsion include: a temperature of 880℃~920℃, an inert gas flow rate of 3000sccm~5000sccm, a pressure of 100mbar~300mbar, and a duration of 5min~15min for oxygen-free propulsion of boron atoms in the boron source layer. And / or, the conditions for the second temperature stage of anaerobic propulsion in step S2022 include: the temperature is reduced to 780°C to 800°C, the inert gas flow rate is 20,000 sccm to 30,000 sccm, the pressure is restored to atmospheric pressure, and the duration of anaerobic propulsion of boron atoms in the boron source layer is 10 min to 15 min.
9. The preparation method according to claim 7, characterized in that, Step S2021 includes: Step S20211, under the conditions of oxygen flow rate of 5000 sccm to 15000 sccm and temperature of 810℃ to 850℃, forming a second silicon oxide layer (21) on the first main surface of the crystalline silicon substrate (10) for a deposition time of 2 min to 5 min; Optionally, step S2021 further includes: step S20212, forming a boron source layer (22) through three sequential source processing steps. Optionally, the conditions for the first source treatment include: oxygen flow rate of 300 sccm to 600 sccm, boron source flow rate of 250 sccm to 450 sccm, nitrogen carrying boron source flow rate of 3500 sccm to 5500 sccm, temperature of 810℃ to 850℃, pressure of 100 mbar to 300 mbar, and duration of 1 min to 3 min. The conditions for the second source treatment included: oxygen flow rate of 300 sccm to 600 sccm, boron source flow rate of 250 sccm to 450 sccm, nitrogen carrying boron source flow rate of 3500 sccm to 5500 sccm, temperature of 830℃ to 850℃, pressure of 100 mbar to 300 mbar, and duration of 2 min to 4 min. The conditions for the third source treatment included: an oxygen flow rate of 300 sccm to 600 sccm, a boron source flow rate of 250 sccm to 450 sccm, a nitrogen flow rate carrying the boron source of 3500 sccm to 5500 sccm, a temperature of 830℃ to 880℃, a pressure of 100 mbar to 300 mbar, and a duration of 2 min to 4 min.
10. A solar cell, characterized in that, The solar cell is prepared according to the preparation method described in any one of claims 1 to 9.