A cadmium telluride thin film solar cell and a preparation method and application thereof
By using As(SCN)₃ and NaSCN composite thin films as the back contact layer, combined with magnetron sputtering and solution spin coating technologies, the problems of high interfacial contact resistance and high preparation cost of the back contact layer of cadmium telluride thin film solar cells have been solved, and the carrier transport efficiency has been improved and mass production adaptability has been achieved.
Patent Information
- Application Number
- CN202611424805.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-15
- Publication Date
- 2026-11-24
AI Technical Summary
Existing cadmium telluride thin-film solar cells have problems with high interfacial contact resistance, high interfacial state density, complex fabrication process and high cost, making it difficult to meet the demand for large-scale low-cost mass production.
A dense and uniform back contact layer was prepared by using As(SCN)₃ and NaSCN composite thin film as the back contact layer and combining magnetron sputtering and solution spin coating techniques. The energy level structure and conductivity of the composite thin film were controlled by doping agents to optimize carrier transport.
It significantly reduces interfacial contact resistance, improves carrier transport efficiency, reduces manufacturing costs, is suitable for large-scale mass production, and has good material stability, adapts to different back electrode materials, and broadens application scenarios.
Smart Images

Figure CN123164879A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of solar cell technology, and particularly relates to a cadmium telluride thin-film solar cell, its preparation method, and its application. Background Technology
[0002] Cadmium telluride (CdTe) thin-film solar cells have become one of the most competitive technologies for commercial application in the field of thin-film solar cells due to their suitable bandgap (approximately 1.5 eV), high light absorption coefficient, low manufacturing cost, and great potential for mass production. To date, the highest laboratory conversion efficiency of CdTe thin-film solar cells has approached 25%, and the efficiency of mass-produced modules has gradually exceeded 22%. However, further performance improvements are still limited by the interfacial characteristics of the back contact layer.
[0003] As a key functional layer between the cadmium telluride absorber layer and the back electrode, the back contact layer plays a crucial role in reducing interfacial contact resistance, suppressing carrier recombination, and optimizing hole transport efficiency. Its material selection and structural design directly determine the battery's open-circuit voltage (Voc), fill factor (FF), and final conversion efficiency. In existing technologies, back contact layer materials are mainly divided into metallic and non-metallic back contact materials. While traditional metallic back contact materials, such as metal compounds (e.g., ZnTe, Sb₂Te₃, MoN), can reduce contact resistance to some extent, they suffer from large lattice mismatches, high interfacial state densities, complex fabrication processes, and high costs, making it difficult to meet the demands of large-scale, low-cost mass production. Furthermore, existing back contact layer fabrication methods (e.g., magnetron sputtering, vacuum evaporation) often involve large equipment investments, high energy consumption, and poor film thickness uniformity. While solution methods (e.g., spin coating, spray coating) offer advantages such as low cost and ease of scalability, the quality of solution-formed films from single materials is often poor, prone to pinholes and cracks, affecting interfacial contact characteristics.
[0004] Therefore, how to provide a method for preparing the back contact layer of a composite system, and achieve uniform film formation and performance control of the composite back contact layer, is a technical problem that urgently needs to be solved by those skilled in the art. Summary of the Invention
[0005] To address the aforementioned technical problems, this invention proposes a cadmium telluride thin-film solar cell, its preparation method, and its application.
[0006] To achieve the above objectives, the present invention provides the following technical solution: A cadmium telluride thin-film solar cell includes a substrate layer, a window layer, a cadmium telluride absorber layer, a back contact layer, and a back electrode layer stacked sequentially. The back contact layer is an As(SCN)3 and NaSCN composite film with a thickness of 10-150 nm.
[0007] Beneficial Effects: This invention uses a composite film of As(SCN)3 and NaSCN as the back contact layer, located between the cadmium telluride absorber layer and the back electrode layer. This reduces interfacial contact resistance and optimizes hole transport. The energy level structure of As(SCN)3 has a high degree of matching with the p-type CdTe absorber layer, effectively controlling the interfacial electronic states and reducing the interfacial state density. NaSCN has excellent ionic conductivity, promoting hole migration. The synergistic effect of these two materials reduces the interfacial contact resistance between the back contact layer and the CdTe absorber layer, significantly optimizing carrier transport efficiency and improving the battery's fill factor and open-circuit voltage. Furthermore, As(SCN)3 exhibits good stability, and NaSCN is chemically stable with excellent temperature and humidity resistance. The resulting composite film is dense and uniform, without obvious pinholes or cracks, effectively preventing impurities such as oxygen and moisture from penetrating the CdTe absorber layer and inhibiting interfacial oxidation and carrier recombination. Simultaneously, the composite film exhibits strong interfacial bonding with the CdTe absorber layer and the back electrode layer, making it less prone to peeling and degradation, significantly superior to existing single thiocyanate or metal compound back contact layers.
[0008] More preferably, the back contact layer further includes a dopant with a mass fraction of 0.5%-5%, wherein the dopant is selected from one or more of CuCl2, SbCl3, and InCl3.
[0009] Beneficial effects: The above dopants can further modulate the energy level structure and conductivity of the composite thin film, optimizing carrier transport efficiency. This invention, by adding dopants such as CuCl2, SbCl3, and InCl3, can further modulate the energy level structure and conductivity of the composite back contact layer, optimizing carrier transport efficiency and improving the conversion efficiency of cadmium telluride thin-film solar cells by 1%-3%, providing a new approach for the subsequent development of high-performance cadmium telluride batteries.
[0010] Preferably, the substrate layer is FTO conductive glass with a thickness of 1.1-3.2 mm, used to support each functional layer.
[0011] The transparent conductive film layer of the substrate is fluorine-doped tin oxide (FTO), with a thickness of 80nm-200nm, a sheet resistance ≤15Ω, and a visible light transmittance ≥85%, used for collecting and transmitting electrons.
[0012] Beneficial Effects: This invention uses 1.1-3.2 mm thick FTO conductive glass as the substrate. The glass substrate has high mechanical strength and excellent thermal stability, providing a flat and rigid physical support for subsequent functional thin films such as CdS and CdTe. It can withstand the high-temperature 400-450℃ cadmium chloride activation annealing process during cadmium telluride battery fabrication, is less prone to warping and deformation, ensures the continuous film formation quality of multilayer films, and reduces the risk of device cracking and film delamination. Compared to flexible substrates, the rigid glass substrate can effectively suppress the degradation of the conductive layer morphology under high-temperature treatment, which is beneficial for obtaining uniform and dense window and absorption layer films, improving batch consistency of devices. Furthermore, its 80-200nm thick FTO (SnO2:F) transparent conductive film combines high visible light transmittance with low sheet resistance. FTO is a wide-bandgap n-type semiconductor with a bandgap greater than 3.8eV and visible light transmittance ≥85%, which can minimize the optical loss of incident light in the electrode layer, allowing more photons to reach the CdTe light absorption layer, which is beneficial to improving the short-circuit current density of the device. The sheet resistance is controlled at ≤15Ω, which can reduce ohmic losses in the carrier transport process, efficiently collect and transport photogenerated electrons, improve the battery fill factor FF, and reduce the performance loss caused by series resistance. This parameter range matches the performance requirements of CdTe cells for the front electrode TCO.
[0013] The FTO thin film used in this invention exhibits superior high-temperature chemical stability compared to ITO. It is less prone to conductivity degradation under high-temperature processes such as CdCl2 annealing and cadmium-based thin film deposition, and it avoids indium diffusion contamination of the PN junction region due to high temperatures, reducing the formation of interfacial recombination centers. This helps maintain the open-circuit voltage of the device and improves its thermal processing tolerance and yield. Simultaneously, the FTO thin film has good lattice compatibility with the CdS window layer and excellent interfacial contact ohmic characteristics, facilitating the cross-interface transport of photogenerated carriers and reducing the probability of carrier recombination at the interface. The FTO conductive glass in this invention can be fabricated over large areas with controllable material costs, meeting the needs of large-scale production of cadmium telluride thin-film battery modules. The glass substrate is resistant to environmental corrosion, and the FTO film layer has good chemical stability, which can improve the long-term operating environment stability of the battery module and has a positive effect on the reliability of the device during long-term outdoor service. Preferably, the window layer is a composite window layer of cadmium sulfide and cadmium selenide, with a thickness of 80-200 nm; The cadmium sulfide and cadmium selenide composite window layer includes a cadmium sulfide layer and a cadmium selenide layer sequentially stacked on the surface of the substrate layer. The thickness ratio of the cadmium sulfide layer to the cadmium selenide layer is 5:3.
[0014] Beneficial effects: The cadmium sulfide and cadmium selenide composite window layer is an n-type semiconductor, which forms a pn heterojunction with the p-type cadmium telluride absorption layer to reduce photogenerated carrier recombination.
[0015] Preferably, the thickness of the cadmium telluride absorber layer is 1-5 μm.
[0016] The cadmium telluride absorber layer is a p-type semiconductor with a bandgap of 1.45 eV-1.55 eV and an absorption coefficient ≥10. 5 cm -1 (Visible light band), used to absorb sunlight and generate photogenerated carriers; Beneficial effects: This invention limits the thickness of the CdTe absorption layer to 1-5 μm, balancing light absorption and carrier transport performance. The visible light absorption coefficient of CdTe can reach 10. 5 cm -1 At a thickness of 1 μm or more, over 93% absorption of visible light with energies greater than the bandgap can be achieved. However, with a thickness less than 1 μm, insufficient absorption of long-wavelength photons leads to a significant decrease in short-circuit current density. Beyond 5 μm, light absorption tends to saturate, but the increased transport distance of photogenerated carriers significantly raises bulk recombination losses, reducing the fill factor (FF) and increasing tellurium consumption and manufacturing costs. A thickness range of 1-5 μm ensures sufficient photogenerated carrier generation while controlling carrier bulk recombination. This range is suitable for high-temperature recrystallization annealing of CdCl2, facilitating the formation of large-grain polycrystalline thin films, reducing grain boundary defect density, and is also suitable for large-scale module production, balancing device performance and material costs. Preferably, the back electrode layer is a gold thin film with a thickness of 50-100 nm.
[0017] Beneficial effects: Gold films have a high work function and a relatively low hole barrier, which is beneficial for hole extraction. They can consume the native CdTeO3 oxide layer on the CdTe surface, improve interfacial contact, form a complete and continuous gold film, have low film surface resistance, and good lateral conductivity, which meets the current collection requirements of laboratory devices.
[0018] A method for preparing a cadmium telluride thin-film solar cell includes the following steps: (1) A window layer was prepared on the substrate by magnetron sputtering, and a CdTe thin film was deposited on the surface of the window layer by near-space sublimation to obtain a cadmium telluride absorption layer. (2) After post-treatment of the cadmium telluride absorption layer, a mixed solution of As(SCN)3 and NaSCN is spin-coated onto the surface of the cadmium telluride absorption layer, and then subjected to segmented annealing to obtain the back contact layer. (3) A back electrode layer is deposited on the back contact layer by magnetron sputtering to obtain the cadmium telluride thin film solar cell.
[0019] Preferably, in step (2), the total concentration of As(SCN)3 and NaSCN in the mixed solution of As(SCN)3 and NaSCN is 0.05-0.5 mol / L, and the mass ratio of As(SCN)3 to NaSCN is 7:3-3:7; More preferably, the solvent of the mixed solution of As(SCN)3 and NaSCN is DMF.
[0020] More preferably, the mixed solution of As(SCN)3 and NaSCN also includes a dopant.
[0021] More preferably, the As(SCN)3 powder has a purity of 99.5% and a particle size of 50-100 mesh; The NaSCN powder has a purity of 99.8% and a particle size of 100-200 mesh.
[0022] Beneficial effects: The SCN in this invention - Thiocyanate ions achieve mild chemical modification of the CdTe back surface, removing the original insulating oxide layer CdTeO. x This reduces the hole transport barrier. As(SCN)3 provides a Group V arsenic source, enabling in-situ p-type doping of the CdTe back surface and increasing the surface hole carrier concentration. DMF, as a solvent, does not corrode the CdTe matrix, is suitable for spin coating processes, and produces films with good uniformity. Furthermore, the use of high-purity raw materials in this invention reduces the introduction of impurities and prevents the formation of recombination centers. Appropriate powder particle size facilitates rapid and complete dissolution, reduces insoluble particles, prevents particle defects and pinholes during spin coating, and ensures batch-to-batch process repeatability. Further addition of dopants to the mixed solution can synergistically regulate p-type conductivity, further reducing interfacial contact resistance and adapting to CdTe absorber layers of different thicknesses and grain qualities. The all-solution method for preparing the back contact modified layer is simple, requires no high-vacuum equipment, and is less expensive than vapor-deposited ZnTe:As back buffer layers, facilitating scale-up from research to pilot production and further industrial-scale application.
[0023] Preferably, the segmented annealing process in step (2) includes the following steps: under an inert atmosphere, the temperature is raised to 80℃-120℃ at a heating rate of 5-10℃ / min, held for 10min-20min, and then raised to 200℃-280℃ at a heating rate of 5-10℃ / min, held for 10min-30min.
[0024] Beneficial effects: The first stage of annealing effectively removes dissolution from the film. Subsequent heating to 200℃-280℃ and holding at that temperature for 10-30 minutes promotes the crystallization and fusion of As(SCN)3 and NaSCN, optimizing film density and interfacial adhesion. The heating rate is 5℃ / min-10℃ / min to avoid excessively rapid heating that could cause cracks, peeling, or other defects that would affect film performance and interfacial adhesion.
[0025] Preferably, the spin coating speed in step (2) is 2000-5000 r / min and the time is 30-60 s.
[0026] Beneficial effects: This invention sets the spin coating speed to 2000-5000 r / min and the spin coating time to 30-60 s. On the one hand, centrifugation allows the DMF mixed solution of As(SCN)3 and NaSCN to be fully spread on the surface of the cadmium telluride absorber layer, forming a salt precursor film of moderate thickness and complete coverage. This avoids the problems of excessively thick film and solute agglomeration caused by excessively low speed and short time, while preventing excessively thin film, local exposure of the substrate, and insufficient supply of dopant source caused by excessively high speed and long time. On the other hand, it adapts to the volatility characteristics of DMF solvent, achieving moderate pre-evaporation during spin coating, suppressing the premature precipitation of large salt particles and the violent boiling and foaming of solvent in the subsequent annealing stage, reducing film defects such as pinholes and streaks, and ensuring that the precursor film composition is uniform and controllable. This parameter window can stably control the salt loading per unit area, ensuring that the As doping dose diffused into the cadmium telluride surface during subsequent annealing is within a reasonable range. This achieves effective p-type modification of the back surface, avoids the aggregation of residual impurity phases which introduces recombination defects, improves the device open-circuit voltage and fill factor, and also has good process tolerance and improves sample batch repeatability.
[0027] Preferably, the magnetron sputtering method used in step (1) to prepare the window layer on the substrate includes sputtering a CdS thin film using magnetron sputtering and sputtering a CdSe thin film using magnetron sputtering.
[0028] Beneficial Effects: This invention employs magnetron sputtering to sequentially sputter CdS and CdSe films to prepare a window layer. Firstly, the thickness of the CdS and CdSe films can be precisely controlled by adjusting the sputtering power and time. During subsequent annealing, CdS and CdSe interdiffusion forms a CdSeS solid solution transition layer, optimizing the bandgap matching between the window layer and the cadmium telluride absorption layer, broadening the short-wavelength spectral response of the device, and increasing the short-circuit current density. The CdS and CdSe films obtained by magnetron sputtering have high density and few pinhole defects, effectively suppressing device leakage and reducing reverse leakage current. Secondly, CdS and CdSe can be deposited within the same magnetron sputtering vacuum chamber by switching targets, eliminating the need for atmospheric exposure and ensuring clean interlayer interfaces. This avoids problems such as chemical bath processes involving waste liquids, water vapor adsorption, and residual hydrogen and oxygen impurities. The films exhibit good thickness and compositional uniformity, providing a foundation for scaling up to large-area substrates. Meanwhile, the CdSe layer can buffer the intense interdiffusion between CdS and CdTe under high-temperature annealing, prevent the CdS window layer from being excessively consumed, reduce non-radiative recombination at the interface, and improve the open-circuit voltage of the device and the repeatability of the process batches.
[0029] More preferably, the parameters for sputtering CdS thin films using magnetron sputtering are: vacuum degree 5 × 10⁻⁶. -4 The sputtering conditions were: Pa, sputtering power 100W, sputtering atmosphere 99.999% argon, gas flow rate 40 SCCM, substrate temperature 150℃, chamber pressure 1.3Pa, and sputtering time 9min.
[0030] More preferably, the parameters for sputtering CdSe thin films using magnetron sputtering are: vacuum degree 5 × 10⁻⁶. -4 The sputtering conditions were: Pa, sputtering power 80W, sputtering atmosphere 99.999% argon, gas flow rate 40 SCCM, substrate temperature 120℃, chamber pressure 1.3Pa, and sputtering time 5min.
[0031] Beneficial effects: The background vacuum during CdS thin film sputtering in this invention is 5×10⁻⁶. -4Pa effectively reduces residual impurities such as oxygen and water vapor in the cavity, minimizing oxidation defects in CdS and CdSe films. High-purity argon, a gas flow rate of 40 SCCM, and a chamber pressure of 1.3 Pa maintain a stable plasma discharge environment, ensuring moderate energy of deposited particles and obtaining a dense window layer film with few pinholes. For CdS, a sputtering power of 100 W, a substrate temperature of 150 °C, and a sputtering time of 9 min yields a CdS underlayer with good crystal quality and appropriate thickness, avoiding both excessively thick films that cause short-wavelength photon loss and excessively thin films that lead to device leakage. For CdSe, a relatively lower sputtering power of 80 W, a substrate temperature of 120 °C, and a sputtering time of 5 min reduces the bombardment damage of high-energy particles to the lower CdS film, resulting in a thin and continuous CdSe upper layer. The close deposition temperatures of the two layers reduce interlayer thermal stress and improve film adhesion. Subsequent activation annealing allows for full interdiffusion between CdS and CdSe to form a CdSeS alloy transition layer, optimizing bandgap matching and broadening the short-wavelength spectral response. The entire process parameters are controllable, the thin film quality has good batch consistency, and it is easy to expand to large-area device processes.
[0032] Preferably, the parameters of the near-space sublimation method in step (1) are: substrate temperature 550℃, source temperature 680℃, distance between source and substrate 2cm, and deposition for 400s under a pressure of 10 torr.
[0033] Beneficial Effects: This invention employs a near-space sublimation method to deposit a cadmium telluride absorber layer. A source temperature of 680℃ ensures stable sublimation of the cadmium telluride source to generate gaseous precursors, while a substrate temperature of 550℃ provides sufficient surface migration capability for deposited atoms. This facilitates the formation of polycrystalline CdTe films with large grains and low grain boundary density, reducing non-radiative recombination losses at grain boundaries. A near-space distance of 2cm between the source and substrate shortens the vapor transport path, reduces segregation of gaseous Cd and Te components, ensures a balanced stoichiometric ratio in the film, achieves a high deposition rate, and avoids thermal radiation interference with substrate temperature caused by excessively small spacing. A chamber pressure of 10 torr regulates the mean free path of gaseous molecules, resulting in moderate energy of deposited particles, suppressing defects introduced by high-energy bombardment, and inhibiting excessive re-evaporation of the CdTe film. A deposition time of 400s precisely controls the absorber layer thickness, ensuring sufficient absorption of incident visible light to obtain a high short-circuit current while avoiding excessively thick film layers that increase carrier transport losses. The CdTe thin film obtained under these process conditions has high density and low stress, and is well matched with the CdS / CdSe window layer prepared by magnetron sputtering. It can be adapted to subsequent CdCl2 activation annealing treatment. The film is not prone to cracking or peeling, the process window is stable, and it has the potential to be extended to large-area devices.
[0034] Preferably, the post-treatment in step (2) is performed using a saturated cadmium chloride methanol solution, specifically including the following steps: A saturated CdCl2 methanol solution was spin-coated onto the surface of a cadmium telluride absorber layer at room temperature and a spin speed of 2000 r / min for 60 s, forming a uniform CdCl2 film on the surface of the cadmium telluride absorber layer. The film was then annealed at 450 °C for 30 minutes, and the surface of the film was rinsed with pure water to remove excess cadmium chloride. This was the final treatment.
[0035] Beneficial effects: The methanol solvent used in the post-processing of this invention can dissolve high concentrations of CdCl2 without corroding the cadmium telluride substrate. Spin coating at 2000 r / min for 60 s can form a moderately thick and uniformly distributed CdCl2 salt precursor film on the CdTe surface, avoiding localized excessive salt thickness or insufficient activation source. Annealing at 450℃ for 30 min allows CdCl2 to act as an activating flux, promoting cadmium telluride grain growth and grain boundary recrystallization, repairing film defects introduced by near-space sublimation deposition, and reducing non-radiative recrystallization at grain boundaries. Simultaneously, it promotes the interdiffusion of S, Se, and Te elements between the window layer and the cadmium telluride absorber layer, forming an alloy transition layer, optimizing interface bandgap matching, and improving open-circuit voltage and short-circuit current. After annealing, rinsing with pure water removes unreacted free CdCl2 residues from the surface, preventing moisture-absorbing salts from causing device leakage and performance degradation, while also eliminating interference from residual salts in subsequent back contact layer fabrication processes. This post-processing technology does not require a vacuum environment, is easy to operate, has good batch consistency, and is highly compatible with the preceding window layer and absorption layer preparation processes.
[0036] Preferably, the parameters for the magnetron sputtering method in step (3) are: vacuum degree 5×10 -4 The sputtering parameters were: Pa, 99.999% argon gas, sputtering power 150W, sputtering pressure 1.3Pa, gas flow rate 30SCCM, sputtering time 20min.
[0037] Compared with the prior art, the present invention has the following advantages and technical effects: The solar cell provided by this invention uses a composite of As(SCN)3 and NaSCN to form the back contact layer, exhibiting excellent interface characteristics, significantly reduced contact resistance, and stable performance with a low degradation rate. Furthermore, the raw materials As(SCN)3 and NaSCN used in this invention are inexpensive and widely available, reducing raw material costs by 30%-50% compared to traditional back contact materials such as ZnTe and Sb2Te3, resulting in low manufacturing costs and easy mass production. In addition, the preparation method of this invention employs a solution spin-coating-annealing process, eliminating the need for expensive magnetron sputtering and vacuum evaporation equipment, resulting in low equipment investment, low energy consumption, and simple, convenient process steps, making it suitable for large-scale continuous production and significantly reducing the mass production cost of cadmium telluride thin-film solar cells. This invention further optimizes the precursor solution concentration, spin-coating parameters, and segmented annealing process to prepare a dense, uniform, pinhole-free, and crack-free composite film with a film thickness that can be flexibly adjusted within the range of 10nm-150nm. At the same time, the back contact layer can be adapted to different types of back electrode materials (such as IWO, ITO, Ag, etc.), and can be used for single-sided cadmium telluride batteries as well as for bi-sided power generation with transparent back electrodes, thus broadening the application scenarios. Attached Figure Description
[0038] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. In the drawings: Figure 1 This is a schematic diagram of the structure of the cadmium telluride thin-film solar cell obtained in Example 1 of the present invention. Detailed Implementation
[0039] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0040] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, the present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments.
[0041] Unless otherwise specified, all raw materials used in the embodiments of this invention were purchased through commercial channels; The FTO conductive glass with tin oxide layer was purchased from Shangyang Technology, with specifications of 15mm×15mm×3.2mm.
[0042] Unless otherwise specified, room temperature or normal temperature in the embodiments of the present invention refers to 25±3℃.
[0043] Example 1 A method for preparing a cadmium telluride thin-film solar cell includes the following steps: (1) Cleaning of FTO conductive glass: The FTO conductive glass with a tin oxide layer was placed in a glass cleaning solution and ultrasonically cleaned for 30 minutes. Then, it was ultrasonically cleaned with ultrapure water in an ultrasonic cleaning device for 30 minutes until the surface of the FTO conductive glass was cleaned with ultrapure water. Finally, it was ultrasonically cleaned with alcohol for 10 minutes. After cleaning, it was placed in a drying oven to dry, and the cleaned FTO conductive glass substrate was obtained.
[0044] (2) Preparation of CdS window layer and CdSe composite window layer: A 100 nm thick CdS thin film was sputtered using magnetron sputtering equipment. The magnetron sputtering parameters were: vacuum degree 5 × 10⁻⁶. -4 The sputtering parameters were: Pa, sputtering power 100 W, sputtering atmosphere 99.999% argon, gas flow rate 40 SCCM, substrate temperature 150℃, chamber pressure 1.3 Pa, and sputtering time 9 min. A CdSe window layer was then prepared, and a 60 nm thick CdSe thin film was sputtered using magnetron sputtering. The magnetron sputtering parameters were: vacuum degree 5 × 10⁻⁶ Pa. -4 The sputtering conditions were: Pa, sputtering power 80W, sputtering atmosphere 99.999% argon, gas flow rate 40 SCCM, substrate temperature 120℃, chamber pressure 1.3Pa, and sputtering time 5min. The resulting deposited FTO conductive glass was obtained.
[0045] (3) Deposition of CdTe thin film using CSS equipment The FTO conductive glass obtained in step (2) was placed in a CSS device for heating. The substrate was heated to 550°C, the source temperature was 680°C, the distance between the source and the substrate was 2cm, and the pressure was 10 torr for 400s to obtain a CdTe thin film with a thickness of 3μm.
[0046] (4) Post-treatment using a saturated cadmium chloride methanol solution. By spin coating, a saturated CdCl2 methanol solution was spin-coated on the surface of the CdTe thin film obtained in step (3) at room temperature at a spin coating speed of 2000 r / min for 60 s, so that a CdCl2 thin film was uniformly covered on the surface of the CdTe thin film. Then, it was annealed at 450℃ for 30 minutes, and then the surface of the film was rinsed with pure water to remove excess cadmium chloride, so as to obtain the post-treated FTO conductive glass.
[0047] (5) Select As(SCN)3 powder with a purity of 99.5% and a particle size of 50-100 mesh, and NaSCN powder with a purity of 99.8% and a particle size of 100-200 mesh, and add them to DMF solvent at a mass ratio of 5:5. Stir for 30 min until completely dissolved to obtain a mixed solution with a total concentration of 0.2 mol / L of As(SCN)3 and NaSCN. Place the mixed solution in a 150W ultrasonic instrument for ultrasonic dispersion for 20 min to remove bubbles and impurities. Then, spin coat the mixed solution onto the cadmium telluride film surface of the post-treated FTO conductive glass using a spin coater. The spin coater speed is 2000 r / min and the spin coater time is 60 min. The spin-coating environment was room temperature. The spin-coated substrate was placed in an annealing furnace and annealed using a segmented annealing process under the protection of an inert gas (nitrogen or argon) at a flow rate of 80 sccm: First, the temperature was increased to 120℃ at a heating rate of 10℃ / min and held for 20 min to remove the solvent from the film; then, the temperature was increased to 280℃ at a heating rate of 10℃ / min and held for 20 min to promote the crystallization and fusion of As(SCN)3 and NaSCN, and to optimize the film density and interfacial adhesion; finally, the film was naturally cooled to room temperature to obtain a dense and uniform As(SCN)3 and NaSCN composite back contact layer with a thickness of 30 nm. (6) An Au electrode layer was deposited on the surface of the As(SCN)3 and NaSCN composite back contact layer using magnetron sputtering. The magnetron sputtering parameters were: vacuum degree 5×10 -4 Using 99.999% argon gas, sputtering power of 150 W, sputtering pressure of 1.3 Pa, gas flow rate of 30 SCCM, and sputtering time of 20 min, an Au electrode layer with a thickness of 100 nm was obtained, thus completing the fabrication of cadmium telluride thin-film solar cells.
[0048] Example 2 A method for preparing a cadmium telluride thin-film solar cell includes the following steps: (1) Cleaning of FTO conductive glass: The FTO conductive glass with a tin oxide layer was placed in a glass cleaning solution and ultrasonically cleaned for 30 minutes. Then, it was ultrasonically cleaned with ultrapure water in an ultrasonic cleaning device for 30 minutes until the surface of the FTO conductive glass was cleaned with ultrapure water. Finally, it was ultrasonically cleaned with alcohol for 10 minutes. After cleaning, it was placed in a drying oven to dry, and the cleaned FTO conductive glass substrate was obtained.
[0049] (2) Preparation of CdS window layer and CdSe composite window layer: A 100 nm thick CdS thin film was sputtered using magnetron sputtering equipment. The magnetron sputtering parameters were: vacuum degree 5 × 10⁻⁶. -4The sputtering parameters were: Pa, sputtering power 100 W, sputtering atmosphere 99.999% argon, gas flow rate 40 SCCM, substrate temperature 150℃, chamber pressure 1.3 Pa, and sputtering time 9 min. A CdSe window layer was then prepared, and a 60 nm thick CdSe thin film was sputtered using magnetron sputtering. The magnetron sputtering parameters were: vacuum degree 5 × 10⁻⁶ Pa. -4 The sputtering conditions were: Pa, sputtering power 80W, sputtering atmosphere 99.999% argon, gas flow rate 40 SCCM, substrate temperature 120℃, chamber pressure 1.3Pa, and sputtering time 5min. The resulting deposited FTO conductive glass was obtained.
[0050] (3) Deposition of CdTe thin film using CSS equipment The FTO conductive glass obtained in step (2) was placed in a CSS device for heating. The substrate was heated to 550°C, the source temperature was 680°C, the distance between the source and the substrate was 2cm, and the pressure was 10 torr for 400s to obtain a CdTe thin film with a thickness of 3μm.
[0051] (4) Post-treatment using a saturated cadmium chloride methanol solution. By spin coating, a saturated CdCl2 methanol solution was spin-coated on the surface of the CdTe thin film obtained in step (3) at room temperature at a spin coating speed of 2000 r / min for 60 s, so that a CdCl2 thin film was uniformly covered on the surface of the CdTe thin film. Then, it was annealed at 450℃ for 30 minutes, and then the surface of the film was rinsed with pure water to remove excess cadmium chloride, so as to obtain the post-treated FTO conductive glass.
[0052] (5) Select As(SCN)3 powder with a purity of 99.5% and a particle size of 50-100 mesh, and NaSCN powder with a purity of 99.8% and a particle size of 100-200 mesh, add them to DMF solvent at a mass ratio of 3:7, stir for 40 min until completely dissolved, then add CuCl2 dopant with a mass fraction of 2%, and continue stirring for 20 min until completely dissolved to obtain a mixed solution with a total concentration of 0.1 mol / L of As(SCN)3 and NaSCN. The mixed solution was ultrasonically dispersed in a 100W ultrasonic instrument for 30 minutes to remove bubbles and impurities. Then, the mixed solution was spin-coated onto the cadmium telluride film surface of the post-treated FTO conductive glass using a spin coater at a speed of 2000 r / min and a spin-coating time of 60 s at room temperature. The spin-coated substrate was then placed in an annealing furnace and annealed using a segmented annealing process under the protection of an inert gas (nitrogen or argon) at a flow rate of 80 sccm: first, the temperature was increased to 120℃ at a heating rate of 10℃ / min and held for 20 minutes to remove the solvent from the film; then, the temperature was increased to 280℃ at a heating rate of 10℃ / min and held for 20 minutes to promote the crystallization and fusion of As(SCN)3 and NaSCN, optimizing the film density and interfacial adhesion; finally, the film was naturally cooled to room temperature to obtain a dense and uniform As(SCN)3 and NaSCN composite back contact layer with a thickness of 30 nm. (6) An Au electrode layer was deposited on the surface of the As(SCN)3 and NaSCN composite back contact layer using magnetron sputtering. The magnetron sputtering parameters were: vacuum degree 5×10 -4 Using 99.999% argon gas, sputtering power of 150 W, sputtering pressure of 1.3 Pa, gas flow rate of 30 SCCM, and sputtering time of 20 min, an Au electrode layer with a thickness of 100 nm was obtained, thus completing the fabrication of cadmium telluride thin-film solar cells.
[0053] Example 3 A method for preparing a cadmium telluride thin-film solar cell includes the following steps: (1) Cleaning of FTO conductive glass: The FTO conductive glass with a tin oxide layer was placed in a glass cleaning solution and ultrasonically cleaned for 30 minutes. Then, it was ultrasonically cleaned with ultrapure water in an ultrasonic cleaning device for 30 minutes until the surface of the FTO conductive glass was cleaned with ultrapure water. Finally, it was ultrasonically cleaned with alcohol for 10 minutes. After cleaning, it was placed in a drying oven to dry, and the cleaned FTO conductive glass substrate was obtained.
[0054] (2) Preparation of CdS window layer and CdSe composite window layer: A 100 nm thick CdS thin film was sputtered using magnetron sputtering equipment. The magnetron sputtering parameters were: vacuum degree 5 × 10⁻⁶. -4The sputtering parameters were: Pa, sputtering power 100 W, sputtering atmosphere 99.999% argon, gas flow rate 40 SCCM, substrate temperature 150℃, chamber pressure 1.3 Pa, and sputtering time 9 min. A CdSe window layer was then prepared, and a 60 nm thick CdSe thin film was sputtered using magnetron sputtering. The magnetron sputtering parameters were: vacuum degree 5 × 10⁻⁶ Pa. -4 The sputtering conditions were: Pa, sputtering power 80W, sputtering atmosphere 99.999% argon, gas flow rate 40 SCCM, substrate temperature 120℃, chamber pressure 1.3Pa, and sputtering time 5min. The resulting deposited FTO conductive glass was obtained.
[0055] (3) Deposition of CdTe thin film using CSS equipment The FTO conductive glass obtained in step (2) was placed in a CSS device for heating. The substrate was heated to 550°C, the source temperature was 680°C, the distance between the source and the substrate was 2cm, and the pressure was 10 torr for 400s to obtain a CdTe thin film with a thickness of 3μm.
[0056] (4) Post-treatment using a saturated cadmium chloride methanol solution. By spin coating, a saturated CdCl2 methanol solution was spin-coated on the surface of the CdTe thin film obtained in step (3) at room temperature at a spin coating speed of 2000 r / min for 60 s, so that a CdCl2 thin film was uniformly covered on the surface of the CdTe thin film. Then, it was annealed at 450℃ for 30 minutes, and then the surface of the film was rinsed with pure water to remove excess cadmium chloride, so as to obtain the post-treated FTO conductive glass.
[0057] (5) Select As(SCN)3 powder with a purity of 99.5% and a particle size of 80-150 mesh, or As(SCN)3 powder with a purity of 99.8% and a particle size of 100 mesh. Head-200 mesh NaSCN powder was added to a mixture of anhydrous ethanol and DMF (volume ratio 1:1) at a mass ratio of 7:3 and stirred for 35 min until completely dissolved. Then, 3% (w / w) of SbCl3 dopant was added, and stirring was continued for 25 min until completely dissolved, resulting in a mixed solution with a total concentration of 0.4 mol / L of As(SCN)3 and NaSCN. The mixed solution was ultrasonically dispersed in a 200W ultrasonic instrument for 10 min to remove bubbles and impurities. Then, the mixed solution was spin-coated onto the cadmium telluride film surface of post-treated FTO conductive glass using a spin coater at a spin speed of 2000 r / min for 60 minutes. The spin-coating environment was room temperature. The spin-coated substrate was placed in an annealing furnace and annealed using a segmented annealing process under the protection of an inert gas (nitrogen or argon) at a flow rate of 80 sccm: First, the temperature was increased to 120℃ at a heating rate of 10℃ / min and held for 20 min to remove the solvent from the film; then, the temperature was increased to 280℃ at a heating rate of 10℃ / min and held for 20 min to promote the crystallization and fusion of As(SCN)3 and NaSCN, and to optimize the film density and interfacial adhesion; finally, the film was naturally cooled to room temperature to obtain a dense and uniform As(SCN)3 and NaSCN composite back contact layer with a thickness of 30 nm. (6) An Au electrode layer was deposited on the surface of the As(SCN)3 and NaSCN composite back contact layer using magnetron sputtering. The magnetron sputtering parameters were: vacuum degree 5×10 -4 Using 99.999% argon gas, sputtering power of 150 W, sputtering pressure of 1.3 Pa, gas flow rate of 30 SCCM, and sputtering time of 20 min, an Au electrode layer with a thickness of 100 nm was obtained, thus completing the fabrication of cadmium telluride thin-film solar cells.
[0058] Comparative Example 1 The only difference from Example 1 is that step (5) uses a single CuSCN as the back contact layer, specifically including the following steps: Steps (1)-(4) are the same as in Example 1.
[0059] (5) Select CuSCN powder with a purity of 99.5% and a particle size of 80-150 mesh, and add it to ammonia water at a concentration of 5 mg / ml. Stir for 35 min until completely dissolved to obtain a mixed solution with a total concentration of 5 mg / ml of CuSCN and ammonia water. Place the mixed solution in a 200W ultrasonic instrument and ultrasonically disperse for 10 min to remove bubbles and impurities. Then, spin coat the mixed solution onto the cadmium telluride film surface of the post-treated FTO conductive glass using a spin coater at a spin coating speed of 2000 r / min. n, spin coating time 60s, spin coating environment at room temperature, the spin-coated substrate is placed in an annealing furnace, under the protection of an inert gas (nitrogen or argon) at a flow rate of 80sccm, and annealed using a segmented annealing process: first, the temperature is raised to 120℃ at a heating rate of 10℃ / min and held for 20min to remove the solvent in the film; then the temperature is raised to 280℃ at a heating rate of 10℃ / min and held for 20min; finally, it is naturally cooled to room temperature to obtain a CuSCN composite back contact layer with a thickness of 30nm; Step (6) is the same as in Example 1.
[0060] Comparative Example 2 The only difference from Example 1 is that step (5) uses NaSCN as the back contact layer, specifically including the following steps: Steps (1)-(4) are the same as in Example 1.
[0061] (5) Select NaSCN powder with a purity of 99.5% and a particle size of 80-150 mesh, and a purity of 99.8%. Add 5 mg / ml of NaSCN powder to anhydrous ethanol and stir for 35 min until completely dissolved. Then add 3% SbCl3 dopant and continue stirring for 25 min until completely dissolved to obtain a mixed solution with a NaSCN concentration of 5 mg / ml. Place the mixed solution in a 200W ultrasonic instrument and ultrasonically disperse for 10 min to remove bubbles and impurities. Then spin-coat the mixed solution onto the cadmium telluride film surface of the post-treated FTO conductive glass. On the surface, the spin coating speed was 2000 r / min, the spin coating time was 60 s, and the spin coating environment was room temperature. The substrate after spin coating was placed in an annealing furnace and annealed using a segmented annealing process under the protection of an inert gas (nitrogen or argon) at a flow rate of 80 sccm: first, the temperature was increased to 120℃ at a heating rate of 10℃ / min and held for 20 min to remove the solvent in the film; then the temperature was increased to 280℃ at a heating rate of 10℃ / min and held for 20 min; finally, the temperature was naturally cooled to room temperature to obtain a NaSCN composite back contact layer with a thickness of 30 nm. Step (6) is the same as in Example 1.
[0062] Comparative Example 3 The only difference from Example 1 is that step (5) uses ZnTe:Cu as the back contact layer (ZnTe:Cu=95:5), and specifically includes the following steps: Steps (1)-(4) are the same as in Example 1.
[0063] (5) Using a 6-inch (ZnTe:Cu=95:5) target from Jiangsu Pioneer Microelectronics Technology Co., Ltd., a 20nm thick back contact layer was magnetron sputtered onto the cadmium telluride thin film surface of the post-treated FTO conductive glass. The magnetron sputtering parameters were: vacuum degree 5×10 -4 The sputtering parameters were: Pa, sputtering power 150W, sputtering atmosphere 99.999% argon, gas flow rate 80 SCCM, substrate temperature 200℃, chamber pressure 1.3Pa, and sputtering time 1min30s.
[0064] Step (6) is the same as in Example 1.
[0065] Comparative Example 4 The only difference from Example 1 is that step (5) does not employ a segmented annealing process, and specifically includes the following steps: Steps (1)-(3) are the same as in Example 1.
[0066] (5) Select As(SCN)3 powder with a purity of 99.5% and a particle size of 50-100 mesh, and NaSCN powder with a purity of 99.8% and a particle size of 100-200 mesh, add them to DMF solvent at a mass ratio of 5:5, stir for 30 min until completely dissolved, and obtain a mixed solution with a total concentration of 0.2 mol / L of As(SCN)3 and NaSCN; put the mixed solution into a 150W ultrasonic instrument for ultrasonic dispersion for 20 min to remove bubbles and impurities, and then spin coat the mixed solution onto the cadmium telluride film surface of the post-treated FTO conductive glass using a spin coater. The spin coat speed is 2000 r / min, the spin coat time is 60 s, the spin coat environment is room temperature, the annealing furnace is heated to 250℃ at a heating rate of 10℃ / min, the substrate after spin coating is placed in the annealing furnace at 250℃ and kept at 20 min, and finally naturally cooled to room temperature to obtain an As(SCN)3 and NaSCN composite back contact layer with a thickness of 30 nm; Step (6) is the same as in Example 1.
[0067] Comparative Example 5 The only difference from Example 1 is that step (5) uses a single As(SCN)3 as the back contact layer, specifically including the following steps: Steps (1)-(4) are the same as in Example 1.
[0068] (5) Select As(SCN)3 powder with a purity of 99.5% and a particle size of 80-150 mesh, add it to anhydrous acetone at a concentration of 5 mg / ml, stir for 35 min until completely dissolved, then add 3% SbCl3 dopant and continue stirring for 25 min until completely dissolved to obtain a mixed solution of As(SCN)3 and anhydrous acetone at a concentration of 5 mg / ml; place the mixed solution in a 200W ultrasonic instrument for ultrasonic dispersion for 10 min to remove bubbles and impurities, and then use a spin coater to spin coat the mixed solution onto the cadmium telluride film surface of the post-treated FTO conductive glass. The spin coating speed was 2000 r / min, the spin coating time was 60 s, and the spin coating environment was room temperature. The substrate after spin coating was placed in an annealing furnace and annealed using a segmented annealing process under the protection of an inert gas (nitrogen or argon) at a flow rate of 80 sccm: first, the temperature was increased to 120℃ at a heating rate of 10℃ / min and held for 20 min to remove the solvent in the film; then the temperature was increased to 280℃ at a heating rate of 10℃ / min and held for 30 min; finally, the temperature was naturally cooled to room temperature to obtain a dense and uniform As(SCN)3 back contact layer with a thickness of 30 nm. Step (6) is the same as in Example 1.
[0069] Comparative Example 6 The only difference from Example 1 is that step (5) uses ZnTe:As as the back contact layer (ZnTe:As=95:5), specifically including the following steps: Steps (1)-(4) are the same as in Example 1.
[0070] (5) Using a 6-inch (ZnTe:As=95:5) target from Jiangsu Pioneer Microelectronics Technology Co., Ltd., a 20nm thick back contact layer was magnetron sputtered onto the cadmium telluride thin film surface of the post-treated FTO conductive glass. The magnetron sputtering parameters were: vacuum degree 5×10 -4 The sputtering parameters were: Pa, sputtering power 150W, sputtering atmosphere 99.999% argon, gas flow rate 80 SCCM, substrate temperature 200℃, chamber pressure 1.3Pa, and sputtering time 1min30s.
[0071] Step (6) is the same as in Example 1.
[0072] Technical effects: According to GB / T 6495.1-2025, at AM1.5G, 25℃, the steady-state light intensity is 1000 W / m². 2 The performance of the battery film was tested under the specified conditions.
[0073] Table 1 Performance parameters of cadmium telluride thin-film solar cells As shown in Table 1, the efficiencies of Examples 1-3 are superior to those of Comparative Examples 1-6, demonstrating that the As(SCN)3 / NaSCN composite film back contact layer is more effective than existing back contact layer films. This also confirms that the As(SCN)3 / NaSCN composite back contact layer can significantly improve the turn-on voltage and fill power of existing cadmium telluride thin-film battery devices. Simultaneously, it can reduce interfacial recombination, improve carrier collection efficiency, and avoid the problem of excessive copper diffusion affecting battery efficiency caused by traditional Cu-doped back contact layers.
[0074] The comparison between the examples and the comparative examples shows that the fill factor of the examples is significantly improved, the on-state voltage is also relatively improved, and the current density is related to the absorption layer, which is relatively difficult to improve.
[0075] Various materials have their own suitability (e.g., compared to Examples 1-3). A suitable doping ratio can improve the fill factor and open-circuit voltage, thereby improving the photoelectric conversion efficiency of the battery. Therefore, the doping ratio is not necessarily better the more it is. Under the same conditions, the higher the fill factor, the higher the efficiency. Under the same doping ratio, the photoelectric conversion efficiency of Comparative Examples 1-3 (optimal doping ratio) is inferior to that of the Examples.
[0076] The above are merely preferred embodiments of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.
Claims
1. A cadmium telluride thin-film solar cell, characterized in that, It includes a substrate layer, a window layer, a cadmium telluride absorber layer, a back contact layer, and a back electrode layer stacked in sequence; The back contact layer is an As(SCN)3 and NaSCN composite film with a thickness of 10-150 nm.
2. A cadmium telluride thin-film solar cell according to claim 1, characterized in that, The back contact layer also includes a dopant with a mass fraction of 0.5%-5%; The dopant is selected from one or more of CuCl2, SbCl3, and InCl3.
3. A cadmium telluride thin-film solar cell according to claim 1, characterized in that, The substrate is FTO conductive glass with a thickness of 1.1-3.2 mm.
4. A cadmium telluride thin-film solar cell according to claim 1, characterized in that, The window layer is a composite window layer of cadmium sulfide and cadmium selenide, with a thickness of 80-200 nm. The cadmium sulfide and cadmium selenide composite window layer includes a cadmium sulfide layer and a cadmium selenide layer sequentially stacked on the surface of the substrate layer. The thickness ratio of the cadmium sulfide layer to the cadmium selenide layer is 5:
3.
5. A cadmium telluride thin-film solar cell according to claim 1, characterized in that, The back electrode layer is a gold thin film with a thickness of 50-100 nm.
6. A method for preparing a cadmium telluride thin-film solar cell as described in any one of claims 1-5, characterized in that, Includes the following steps: A window layer was prepared on the substrate by magnetron sputtering, and a CdTe thin film was deposited on the surface of the window layer by near-space sublimation to obtain a cadmium telluride absorber layer. After post-treatment of the cadmium telluride absorber layer, a mixed solution of As(SCN)3 and NaSCN is spin-coated onto the surface of the cadmium telluride absorber layer, and then subjected to segmented annealing to obtain the back contact layer. The cadmium telluride thin-film solar cell is obtained by depositing a back electrode layer on the back contact layer using magnetron sputtering.
7. The preparation method according to claim 6, characterized in that, The total concentration of As(SCN)3 and NaSCN in the mixed solution is 0.05-0.5 mol / L, and the mass ratio of As(SCN)3 to NaSCN is 7:3-3:
7.
8. The preparation method according to claim 6, characterized in that, The segmented annealing process includes the following steps: Under an inert atmosphere, heat to 80℃-120℃ at a heating rate of 5-10℃ / min, hold for 10-20 minutes, then heat to 200℃-280℃ at a heating rate of 5-10℃ / min, and hold for 10-30 minutes.
9. The preparation method according to claim 6, characterized in that, The spin coating speed is 2000-5000 r / min, and the time is 30-60 s.
10. The preparation method according to claim 6, characterized in that, The step of depositing a CdTe thin film on the surface of the window layer using the near-space sublimation method includes: placing the FTO conductive glass with the deposited window layer as a substrate into a CSS device for heating, and depositing for 400s under the conditions of substrate temperature 550℃, source temperature 680℃, source-substrate distance of 2cm, and pressure of 10torr.