Back contact solar cells and photovoltaic modules

By setting multiple sub-regions with varying heights in the second region of the back-contact solar cell, the problem of discontinuous film deposition was solved, resulting in higher film quality and open-circuit voltage, and improved passivation performance of the back-contact solar cell.

CN123164880APending Publication Date: 2026-11-24LONGI GREEN ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611433203.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-15
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

In back-contact solar cells, discontinuous film deposition is prone to occur at the edge of the second semiconductor layer, resulting in poor film quality, deterioration of passivation performance, and reduction of open-circuit voltage.

Method used

Four sub-regions with height differences are set in the second region, including the first platform sub-region, the first slope sub-region, the second platform sub-region, and the second slope sub-region. The residence time and distribution of gaseous reactants are optimized to ensure that gaseous reactants are uniformly deposited in each sub-region and improve the film quality.

Benefits of technology

By optimizing the sub-region design of the second region, continuous deposition and dense coverage of the second semiconductor layer were achieved, improving the passivation performance and open-circuit voltage of the back-contact solar cell.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123164880A_ABST
    Figure CN123164880A_ABST
Patent Text Reader

Abstract

This application discloses a back-contact solar cell and a photovoltaic module. The cell includes a semiconductor substrate, which has a first surface. The first surface includes a second region, which further includes a first platform sub-region, a first slope sub-region, a second platform sub-region, and a second slope sub-region distributed along a first direction. The first platform sub-region is close to the first region, and the second slope sub-region is close to a third region. The first platform sub-region, the first slope sub-region, the second platform sub-region, and the second slope sub-region of the first surface are sequentially close to the second surface. By adding a first platform sub-region, this application facilitates the rapid spread of gaseous reactants, allowing for continuous deposition and growth of the portion of the second semiconductor layer located at the edge of the second region, resulting in a denser structure. This significantly improves the passivation performance of the back-contact solar cell, increases its open-circuit voltage, and reduces the impact of hot spots.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of photovoltaic technology, specifically relating to a back-contact solar cell and a photovoltaic module. Background Technology

[0002] The electrode structure of back-contact solar cells is located on the back side of the cell. Since there are no electrodes blocking the light-facing side, they have high conversion efficiency and are an important branch of high-efficiency cells.

[0003] In back-contact solar cells, N-regions and P-regions with opposite conductivity are set on the back surface of the semiconductor substrate, and the N-regions and P-regions are isolated from each other by an insulating structure.

[0004] However, in existing back-contact solar cells, the edges of the N-region or P-region are often prone to discontinuous film deposition and poor film quality, which leads to a sharp deterioration in the passivation performance of this area, directly reducing the open-circuit voltage of the cell and decreasing the conversion efficiency. Summary of the Invention

[0005] This application aims to provide a back-contact solar cell and photovoltaic module that at least solves the problem that the portion of the second semiconductor layer located at the edge is prone to quality issues.

[0006] In a first aspect, embodiments of this application provide a back-contact solar cell, comprising: A semiconductor substrate includes a first surface and a second surface opposite to each other; the first surface includes a first region, a second region and a third region arranged along a first direction, the second region being located between the first region and the third region; the surface of the third region is recessed toward the semiconductor substrate relative to the surface of the first region, and the surface of the second region is a transition sidewall of the semiconductor substrate from the first region to the third region; A first semiconductor layer is disposed in the first region; A second semiconductor layer is disposed in the third region and the second region, and extends to cover a portion of the first semiconductor layer in the first region; the first semiconductor layer and the second semiconductor layer have different electrical properties. And a second transparent conductive layer, disposed on the second semiconductor layer in the third region; The second region includes: a first platform sub-region, a first slope sub-region, a second platform sub-region, and a second slope sub-region distributed along the first direction; The first platform sub-region is close to the first region, and the second ramp sub-region is close to the third region; In the thickness direction of the back contact solar cell, the first platform sub-region, the first slope sub-region, the second platform sub-region, and the second slope sub-region of the first surface are sequentially close to the second surface; The second transparent conductive layer extends at least partially from the third region through the second region to cover the second semiconductor layer of the first region.

[0007] In this application, four sub-regions with different heights are set in the second region. This results in a large number of sub-regions of varying heights within the second region. Consequently, the gaseous reactants deposited in the film are intercepted or blocked by these sub-regions during their return journey, allowing them to remain in each sub-region for a longer period. This significantly increases the residence time of the gaseous reactants in the second region. In particular, the addition of a first platform sub-region to the back-contact solar cell, with its relatively flat surface, facilitates rapid spread of the gaseous reactants. Therefore, the gaseous reactants are more evenly distributed or more abundant in the second region, resulting in uniform distribution at the edges. Consequently, the portion of the second semiconductor layer located at the edges of the second region can continuously deposit and grow, achieving a denser and higher-quality film. This significantly improves the passivation performance and open-circuit voltage of the back-contact solar cell.

[0008] Meanwhile, in the thickness direction of the back-contact solar cell, the first platform sub-region, the first ramp sub-region, the second platform sub-region, and the second ramp sub-region of the first surface are sequentially close to the second surface of the semiconductor substrate. The surface of the third region is concave towards the semiconductor substrate relative to the surface of the first region. The surface of the second region is the transition sidewall of the semiconductor substrate from the first region to the third region. Thus, in the thickness direction of the back-contact solar cell, the first platform sub-region, the first ramp sub-region, the second platform sub-region, and the second ramp sub-region exist as a continuous transition from the first region to the third region, with good thickness transition continuity. From the side where the gas reactant enters, each sub-region of the second region does not block adjacent sub-regions, and each sub-region of the second region is fully exposed, ensuring that the gas reactant and each sub-region of the second region can fully contact each other. This also promotes the continuous deposition and growth of the part located at the edge of the second region in the second semiconductor layer, which is also relatively dense and has high film quality, further improving the passivation performance of the back-contact solar cell.

[0009] Furthermore, in the first platform sub-region near the first region, the second semiconductor layer has a high-quality, dense film that can cover the sidewalls of the first semiconductor layer, preventing any gaps between the second and first semiconductor layers and achieving a better hot spot protection design. However, if the second semiconductor layer is unevenly formed or of poor quality, defects such as voids may appear. In such cases, the subsequently applied second transparent conductive layer will directly cover the sidewalls of the first semiconductor layer, causing direct contact between the second transparent conductive layer and the first doped semiconductor layer, leading to severe leakage. This structure, where the transparent conductive layer directly contacts a semiconductor layer of a different polarity, differs from a normal hot spot protection structure. A normal hot spot protection structure involves contact between semiconductor layers of different conductivity types, with the second transparent conductive layer not directly contacting the first semiconductor layer. For example, charge carriers travel through the second transparent conductive layer → second semiconductor layer → first semiconductor layer → first transparent conductive layer, following the direction of the arrow, forming a hot spot protection channel.

[0010] In some embodiments, along the first direction, the width of the first platform sub-region is W1, and the width of the second platform sub-region is W2; W1 < W2.

[0011] In some embodiments, along the first direction, the width of the first platform sub-region is W1, the width of the second platform sub-region is W2, the width of the first ramp sub-region is W3, and the width of the second ramp sub-region is W4; W1 < W3 < W2 < W4.

[0012] In some embodiments, W2 / W1 is 10 to 300; and / or, W3 / W1 is 6 to 150; and / or, W4 / W3 is 1.2 to 500; and / or, W4 / W2 is 1.1 to 300.

[0013] In some embodiments, W1 is 2nm to 10nm, and / or W2 is 100nm to 600nm, and / or W3 is 60nm to 300nm, and / or W4 is 0.5μm to 3μm.

[0014] In some embodiments, in the thickness direction of the back-contact solar cell, the height of the first slope region is H1, the height of the second slope region is H2, H2 > H1, and H1 is 100 nm to 300 nm.

[0015] In some embodiments, H2 / H1 is 5 to 800; and / or, the difference between H2 and H1 is 6 μm to 8 μm; and / or, H2 is 2 μm to 8 μm.

[0016] In some embodiments, along the thickness direction of the semiconductor substrate, the included angle between the first platform sub-region and the first ramp sub-region is α; along the thickness direction of the semiconductor substrate, the included angle between the second platform sub-region and the second ramp sub-region is β, where α and β are different and both are obtuse angles; preferably, α ≥ β.

[0017] In some embodiments, in the semiconductor substrate thickness direction, the side surface of the first semiconductor layer is a first side surface; Relative to the first platform sub-region, at least a portion of the first side is inclined; and / or, Relative to the first platform sub-region, at least a portion of the first side is perpendicularly disposed; and / or, At least a portion of the first side has a recessed structure that is recessed into the first semiconductor layer.

[0018] In some embodiments, the degree of undulation of the portion of the second semiconductor layer located on the first platform sub-region is less than the degree of undulation of the portion of the first semiconductor layer located away from the first surface; and / or, The degree of undulation of the portion of the second semiconductor layer located on the second platform sub-region is less than the degree of undulation of the portion of the first semiconductor layer located away from the first surface.

[0019] In some embodiments, both the first platform sub-region and the second platform sub-region are planar.

[0020] In some embodiments, the third region includes a frustum-like structure; the second face includes a pyramid-like structure.

[0021] In some embodiments, both the frustum-like structure and the pyramid-like structure include at least two side edges; in the semiconductor substrate thickness direction, the side edges of the frustum-like structure and the pyramid-like structure are second side edges; the side edges have a top and a bottom, the bottom being closer to the semiconductor substrate than the top. The top of the second side has microstructures; The area with microstructures on the second side is the first sub-side, and the remaining area is the second sub-side; the position of the side edge corresponding to the first sub-side is the first segment; the remaining position is the second segment; In the same side edge of the same frustum-like structure: along the direction from the top to the bottom, the length of the first segment accounts for less than or equal to 90% of the length of the side edge; and / or, In the same side edge of the same pyramid-like structure: along the direction from the top to the bottom, the length of the first segment accounts for less than or equal to 90% of the length of the side edge.

[0022] In some embodiments, in the same side edge of the same frustum-like structure, the length of the first segment as a proportion of the length of the side edge along the direction from the top to the bottom is less than the length of the first segment as a proportion of the length of the side edge along the direction from the top to the bottom in the same side edge of the same pyramid-like structure.

[0023] In some embodiments, the truncated pyramid-like microstructure has the same or similar morphology to the pyramid-like microstructure; and / or, Both the frustum-like microstructure and the pyramid-like microstructure contain folded structures; and / or, Both the pyramid-like microstructure and the pyramid-like microstructure contain a cluster of nested ring structures.

[0024] In some embodiments, the height of the truncated pyramid structure is 0.5 μm to 5 μm along the thickness direction of the semiconductor substrate, and / or the height of the pyramid structure is 0.5 μm to 5 μm.

[0025] In some embodiments, the second slope sub-region has multiple vertical textures and multiple arc textures, the arc textures being superimposed on the vertical textures; the extension direction of the arc textures is a second direction, and the extension direction of the vertical textures is a first direction; the first direction and the second direction intersect.

[0026] In some embodiments, the first semiconductor layer is an N-type doped polycrystalline silicon layer; the back contact solar cell further includes a first passivation layer, which is located between the N-type doped polycrystalline silicon layer and the semiconductor substrate; The second semiconductor layer includes a P-type doped silicon layer, wherein the P-type doped silicon layer includes at least one of P-type doped amorphous silicon, P-type doped nanocrystalline silicon, and P-type doped microcrystalline silicon; The thickness of the P-type doped silicon layer is 20 nm to 80 nm.

[0027] In some embodiments, the doping concentration of the N-type doped polysilicon layer is 3E19cm. -3 up to 8E20cm -3 .

[0028] In some embodiments, the back-contact solar cell further includes: The first transparent conductive layer is located on the side of the first semiconductor layer away from the semiconductor substrate, and the first transparent conductive layer and the second transparent conductive layer are disconnected at least at the overlapping position of the first semiconductor layer and the second semiconductor layer; The first electrode structure is located on the side of the first transparent conductive layer away from the semiconductor substrate; The second electrode structure is located on the side of the second transparent conductive layer away from the semiconductor substrate.

[0029] In some embodiments, the back-contact solar cell further includes a front passivation antireflection layer located on the second surface.

[0030] Secondly, embodiments of this application propose a photovoltaic module, including: a plurality of battery strings connected in series and / or in parallel, the battery strings including: an electrical connector and any of the aforementioned back-contact solar cells, the electrical connector being electrically connected to the electrode structures of at least two of the back-contact solar cells; An encapsulation layer is used to cover the surface of the battery string; A cover plate is used to cover the surface of the encapsulation layer away from the battery string.

[0031] Additional aspects and advantages of this application will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of this application. Attached Figure Description

[0032] The above and / or additional aspects and advantages of this application will become apparent and readily understood from the description of the embodiments taken in conjunction with the following drawings, in which: Figure 1 This is a schematic diagram of the structure of a back-contact solar cell according to an embodiment of this application; Figures 2 to 4 This is a partial structural schematic diagram of several back-contact solar cells according to embodiments of this application; Figures 5 to 8 These are partial SEM images of several back-contact solar cells according to embodiments of this application; Figure 9 This is a structural schematic diagram of the fabrication steps of a back-contact solar cell according to an embodiment of this application.

[0033] Figure label: 1-Semiconductor substrate, 10-First surface, 11-Second surface, 12-First region, 13-Second region, 131-First platform sub-region, 132-First ramp sub-region, 133-Second platform sub-region, 134-Second ramp sub-region, 1341-Vertical texture, 1342-Arc texture, 14-Third region, 21-First side surface, 211-First edge, 22-Concave structure, 141-Fold-like structure, 142-Top, 143-Bottom, 144-Second side surface, 145-Side edge, 1451-First segment, 2-N-type doped polysilicon layer, 3-P-type doped silicon layer, 41-First transparent conductive layer, 42-Second transparent conductive layer, 5-First passivation layer, 6-Second passivation layer, 7-Front-side passivation layer, 8-Front-side anti-reflection layer, 91-First electrode structure, 92-Second electrode structure, 15-Silicon phosphide glass layer, 16-Mask layer. Detailed Implementation

[0034] The embodiments of this application will now be described in detail. Examples of these embodiments are illustrated in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain this application, and should not be construed as limiting this application. All other embodiments obtained by those skilled in the art based on the embodiments of this application without inventive effort are within the scope of protection of this application.

[0035] The inventors discovered that in existing back-contact solar cells, the edges of the second semiconductor layer often suffer from discontinuous film deposition and poor film quality. This is primarily because the second semiconductor layer is formed using gaseous reactants, such as through PECVD (plasma-enhanced chemical vapor deposition). However, existing back-contact solar cells typically have few flat sub-regions in the second region, and they are prone to forming steep sidewalls and sharp edges, easily leading to shading or obstruction. Consequently, the gaseous reactants have a shorter residence time in the second region, resulting in uneven or insufficient distribution. In particular, the narrow and complex spatial shapes at the edges of the second region make it difficult for the gaseous reactants to penetrate, causing discontinuous film deposition at the edges of the second semiconductor layer.

[0036] To address the aforementioned technical problems, this application incorporates four sub-regions with varying heights within the second region. This results in a larger number of sub-regions of different heights within the second region. Consequently, during their return journey, the gaseous reactants are intercepted or blocked by these sub-regions, allowing them to remain in each sub-region for an extended period. This significantly increases the residence time of the gaseous reactants in the second region. Furthermore, the addition of a first platform sub-region to the back-contact solar cell, with its relatively flat surface, facilitates rapid spread of the gaseous reactants. This leads to a more uniform or abundant distribution of the gaseous reactants in the second region, ensuring even distribution at the edges. Consequently, the portion of the second semiconductor layer located at the edges of the second region can be continuously deposited and is relatively dense, significantly improving the passivation performance and open-circuit voltage of the back-contact solar cell.

[0037] Meanwhile, in the thickness direction of the back-contact solar cell, the first platform sub-region, the first ramp sub-region, the second platform sub-region, and the second ramp sub-region of the first surface are sequentially close to the second surface of the semiconductor substrate. The surface of the third region is concave towards the semiconductor substrate relative to the surface of the first region. The surface of the second region is the transition sidewall of the semiconductor substrate from the first region to the third region. Thus, in the thickness direction of the back-contact solar cell, the first platform sub-region, the first ramp sub-region, the second platform sub-region, and the second ramp sub-region exist as a continuous transition from the first region to the third region, with good thickness transition continuity. From the side where the gas reactant enters, each sub-region of the second region does not block adjacent sub-regions, and each sub-region of the second region is fully exposed, ensuring that the gas reactant and each sub-region of the second region can fully contact each other. This also promotes the continuous deposition and growth of the part located at the edge of the second region in the second semiconductor layer, which is also relatively dense and has high film quality, further improving the passivation performance of the back-contact solar cell.

[0038] Furthermore, in the first platform sub-region near the first region, the second semiconductor layer has a high-quality, dense film that can cover the sidewalls of the first semiconductor layer, preventing any gaps between the second and first semiconductor layers and achieving a better hot spot protection design. However, if the second semiconductor layer is unevenly formed or of poor quality, defects such as voids may appear. In such cases, the subsequently applied second transparent conductive layer will directly cover the sidewalls of the first semiconductor layer, causing direct contact between the second transparent conductive layer and the first doped semiconductor layer, leading to severe leakage. This structure, where the transparent conductive layer directly contacts a semiconductor layer of a different polarity, differs from a normal hot spot protection structure. A normal hot spot protection structure involves contact between semiconductor layers of different conductivity types, with the second transparent conductive layer not directly contacting the first semiconductor layer. For example, charge carriers travel through the second transparent conductive layer → second semiconductor layer → first semiconductor layer → first transparent conductive layer, following the direction of the arrow, forming a hot spot protection channel.

[0039] The present application will be further explained below with reference to the specific accompanying drawings.

[0040] Reference Figures 1 to 6 The back-contact solar cell of this application may include: a semiconductor substrate 1, a first semiconductor layer, and a second semiconductor layer. The semiconductor substrate may be a silicon substrate, for example, semiconductor substrate 1 may be N-type monocrystalline silicon or P-type monocrystalline silicon, providing long-lived charge carriers. For ease of description, the following embodiments will first use N-type monocrystalline silicon as an example for semiconductor substrate 1. The first semiconductor layer and the second semiconductor layer have different electrical properties; one is a P-type semiconductor layer, and the other is an N-type semiconductor layer. Along the thickness direction Z of semiconductor substrate 1, semiconductor substrate 1 includes a first surface 10 and a second surface 11 facing each other. The first surface is the backlight surface, and the second surface is the light-facing surface. During normal operation of the solar cell, the side of the semiconductor substrate that mainly receives light is its light-facing surface, while the backlight surface and the light-facing side are opposite each other. For example, Figure 1 In the semiconductor substrate, the top surface is its backlight side, and the bottom surface is its light-facing side.

[0041] Reference Figures 1 to 6 The first surface 10 of the semiconductor substrate 1 includes a first region 12, a second region 13 and a third region 14 arranged along a first direction X, wherein the second region 13 is located between the first region 12 and the third region 14. Figures 1 to 6This illustration only shows a partial region of the back-contact solar cell along the first direction X. In the first direction X, the number of first regions 12 and the number of third regions 14 are typically greater than or equal to two. The surface of the third region 14 is concave relative to the surface of the first region 12 towards the semiconductor substrate. The surface of the second region 13 is a transition sidewall of the semiconductor substrate from the first region 12 to the third region 14. That is, among the three regions—first region 12, second region 13, and third region 14—the surface of the third region 14 is closest to the second surface, the first region 12 is furthest from the second surface, and the second region 13 is located between the third region and the first region 12. The second region 13 includes: a first platform sub-region 131, a first ramp sub-region 132, a second platform sub-region 133, and a second ramp sub-region 134 distributed along the first direction X. In this application, the distances of the first platform sub-region 131 from the second surface 11 at various positions along the first direction X are approximately equal, and the distances of the second platform sub-region 133 from the second surface 11 at different positions along the first direction X are also approximately equal. The distances between the first slope sub-region 132 and the second surface 11 vary at different positions along the first direction X, and the distances between the second slope sub-region 134 and the second surface 11 also vary at different positions along the first direction X. In this application, four sub-regions with height differences are set in the second region, resulting in a large number of sub-regions of different heights in the second region. Therefore, during the return journey, the gaseous reactants are intercepted or blocked by sub-regions of different heights in the second region, causing them to remain in each sub-region for a longer period of time. This significantly increases the residence time of the gaseous reactants in the second region. In particular, the addition of a first platform sub-region to the back contact solar cell, which is relatively flat, facilitates the rapid spread of the gaseous reactants. Therefore, the gaseous reactants are more evenly distributed or more abundant in the second region, resulting in a uniform distribution at the edges of the second region. Consequently, the portion of the second semiconductor layer located at the edges of the second region can be continuously deposited and grown, and is also relatively dense, significantly improving the passivation performance and open-circuit voltage of the back contact solar cell.

[0042] The first platform sub-region 131 is close to the first region 12, and the second slope sub-region 134 is close to the third region 14. In the first direction X, from the first region 12 to the adjacent third region 14, the first platform sub-region 131 is first, followed by the first slope sub-region 132, then the second platform sub-region 133, and finally the second slope sub-region 134.

[0043] Reference Figures 1 to 6In the thickness direction Z of the back-contact solar cell, the first platform sub-region 131, the first ramp sub-region 132, the second platform sub-region 133, and the second ramp sub-region 134 of the first surface 10 are successively close to the second surface 11. Each sub-region of the second region 13 forms a transition region from the first region to the third region in the thickness direction Z of the back-contact solar cell. The third region 14 of the first surface 10 is closer to the second surface 11 than the second region 13. It can be considered that the thickness of the semiconductor substrate in the first region is greater than the thickness of the semiconductor substrate in the third region 14. In adjacent first regions... Between the first platform sub-region, the first slope sub-region, the second platform sub-region, and the second slope sub-region, the thickness transition between the second and third regions is smooth. From the side where the gas reactant enters, none of the sub-regions in the second region block the adjacent sub-regions, and each sub-region in the second region is fully exposed, ensuring that the gas reactant and each sub-region in the second region can fully contact each other. This also promotes the continuous deposition and growth of the part of the second semiconductor layer located at the edge of the second region, which is relatively dense and has high film quality, further improving the passivation performance of the back contact solar cell.

[0044] A first semiconductor layer is disposed in a first region; a second semiconductor layer is disposed in the second region 13 and the third region 14 and extends to cover a portion of the first semiconductor layer in the first region; the first semiconductor layer and the second semiconductor layer have different electrical properties. The second region 13 serves as an isolation between the first and second semiconductor layers, preventing short circuits. A second transparent conductive layer 42 is disposed on the second semiconductor layer in the third region 14, extending at least partially from the third region 14 through the second region 13 to cover the second semiconductor layer in the first region 12. In this application, in the first platform sub-region 131 near the first region 12, the second semiconductor layer has good film quality and is relatively dense, covering the sidewalls of the first semiconductor layer without any gaps, thus achieving a better hot spot prevention design. If the second semiconductor layer is unevenly formed and of poor quality, defects such as holes may appear. The subsequently disposed second transparent conductive layer 42 will directly cover the sidewalls of the first semiconductor layer, causing direct contact between the second transparent conductive layer 42 and the first doped semiconductor layer, resulting in severe leakage.

[0045] Figures 2 to 4 Each of these forms a second region containing the aforementioned four sub-regions, but no structural schematic diagram of the second semiconductor layer is provided.

[0046] In some embodiments, refer to Figures 1 to 6The first semiconductor layer includes an N-type doped polycrystalline silicon layer 2. The back contact solar cell may also include a first passivation layer 5, which is located between the N-type doped polycrystalline silicon layer 2 and the semiconductor substrate 1. The first passivation layer 5 can provide good interface passivation and improve the passivation contact effect. For example, the first passivation layer 5 can be a tunneling silicon oxide layer, etc.

[0047] In some embodiments, the second semiconductor layer includes a P-type doped silicon layer 3, which includes at least one of P-type doped amorphous silicon, P-type doped nanocrystalline silicon, and P-type doped microcrystalline silicon.

[0048] In some embodiments, the second semiconductor layer includes a stacked P-type doped silicon layer 3 and a second passivation layer 6, with the second passivation layer 6 located between the semiconductor substrate 1 and the P-type doped silicon layer 3. The P-type doped silicon layer 3 includes at least one of P-type doped amorphous silicon, P-type doped nanocrystalline silicon, and P-type doped microcrystalline silicon. The second passivation layer 6 includes an intrinsic amorphous silicon layer, which has a good passivation effect. In this back-contact solar cell, a high-temperature first semiconductor layer is fabricated first, followed by a low-temperature second semiconductor layer, which prevents the second semiconductor layer from being damaged due to temperature and has high compatibility with existing back-contact solar cell processes.

[0049] The N-type doped polycrystalline silicon layer 2 may contain one or more elements from Group VA (e.g., phosphorus), and the P-type doped silicon layer 3 may contain one or more elements from Group IIIA (e.g., boron). Both the N-type doped polycrystalline silicon layer 2 and the P-type doped silicon layer 3 can be deposited on the surface of a semiconductor substrate using a CVD process.

[0050] In some embodiments, the thickness of the p-type doped silicon layer is between 20 nm and 80 nm. Too thin a layer can lead to insufficient doping concentration and poor passivation, while too thick a layer increases the probability of carrier recombination during transit and may also cause optical losses. Therefore, a p-type doped silicon layer within the aforementioned range provides suitable doping concentration, good passivation, low recombination probability, and minimal optical loss. For example, the thickness of the p-type doped silicon layer can be 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, or 80 nm.

[0051] In some embodiments, the doping concentration of the N-type doped polysilicon layer 2 is 3E19cm⁻¹. -3 up to 8E20cm -3The N-type doped polysilicon layer 2 has a higher doping concentration. Compared with the N-type single-crystal silicon semiconductor substrate, under the same wet etching process, the N-type doped polysilicon layer with a higher doping concentration has a faster etching rate. This is beneficial in two ways: firstly, it facilitates the rapid removal of the first semiconductor layer in the first plateau region during morphology modification; secondly, it facilitates the formation of a surface with greater undulation during the etching process. For example, the doping concentration of the N-type doped polysilicon layer 2 can be 3E19cm⁻¹. -3 5E19cm -3 9E19cm -3 E20cm -3 2E20cm -3 4E20cm -3 5E20cm -3 8E20cm -3 .

[0052] In some embodiments, refer to Figure 1 The back-contact solar cell also includes a first transparent conductive layer 41 located on the side of the first semiconductor layer away from the semiconductor substrate 1. The first transparent conductive layer 41 and the second transparent conductive layer 42 are disconnected at least at the point where they overlap to avoid short circuits. A first electrode structure 91 is located on the side of the first transparent conductive layer 41 away from the semiconductor substrate 1 and corresponds to the position of the first semiconductor layer. A second electrode structure 92 is located on the side of the second transparent conductive layer 42 away from the semiconductor substrate 1 and corresponds to the position of the second semiconductor layer. The first electrode structure 91 and the second electrode structure 92 are used to collect and conduct current. Both the first electrode structure 91 and the second electrode structure 92 may include a current collector electrode extending along a second direction. The second direction intersects the first direction X, and the two directions may be perpendicular or approximately perpendicular to each other, for example, the included angle between them is 80° to 100°.

[0053] It should be noted that the first transparent conductive layer 41 and the second transparent conductive layer 42 can be formed in the same process, and then formed after being broken at the overlapping position of the first semiconductor layer and the second semiconductor layer.

[0054] In some embodiments, refer to Figures 2 to 4Along the first direction X, the width of the first platform sub-region 131 is W1, and the width of the second platform sub-region 133 is W2; W1 < W2. Specifically, during the formation of the second semiconductor layer, the gaseous reactants typically approach the second region 13 and the third region 14 of the semiconductor substrate from the side of the first surface 10. After contacting the second region 13 and the third region 14, they then turn back towards the side of the first surface 10. During this turning back process, since the second ramp sub-region 134 and the second platform sub-region 133 are closer to the second surface 11, and the second ramp sub-region 134, the second platform sub-region 133, the first ramp sub-region 132, and the first platform sub-region 131 sequentially approach the entry position of the gaseous reactants, a portion of the gas turns back along the second ramp sub-region 134, the second platform sub-region 133, the first ramp sub-region 132, and the first platform sub-region 131 sequentially. Therefore, relative to the first... The first platform sub-region 131 and the second platform sub-region 133 are roughly the starting point of the return path, and the first platform sub-region 131 is roughly the ending point of the return path. Therefore, the width W2 of the second platform sub-region 133 is larger. Thus, in the initial stage of the return path, the gaseous reactants need to travel a longer path, and the contact time between the gaseous reactants and the semiconductor substrate is longer. This can promote a more uniform or greater distribution of the gaseous reactants in the second region. It can also promote a uniform distribution of the gaseous reactants at the edge of the second region. Therefore, the portion of the second semiconductor layer located at the edge of the second region can be continuously deposited and grown, and is also relatively dense, which significantly improves the passivation performance of the back contact solar cell and increases the open-circuit voltage of the back contact solar cell.

[0055] In some embodiments, refer to Figures 2 to 4Along the first direction X, the width of the first platform sub-region 131 is W1, the width of the second platform sub-region 133 is W2, the width of the first ramp sub-region 132 is W3, and the width of the second ramp sub-region 134 is W4, where W1 < W3 < W2 < W4. Specifically, as mentioned above, during the formation of the second semiconductor layer, the gaseous reactants typically approach the second region 13 and the third region 14 of the semiconductor substrate from the side of the first surface 10. After contacting the second region 13 and the third region 14, they then turn back towards the side of the first surface 10. During this turning back process, since the second ramp sub-region 134 and the second platform sub-region 133 are closer to the second surface 11, and the second ramp sub-region 134, the second platform sub-region 133, the first ramp sub-region 132, and the first platform sub-region 131 sequentially approach the entry position of the gaseous reactants, a portion of the gas turns back along the second ramp sub-region 134, the second platform sub-region 133, and the first ramp sub-region 131. If the domain 132 and the first platform sub-region 131 are successively folded back, then in this application, from the beginning to the end of the folding path of the gas reactant, the width of each sub-region decreases successively. That is, in the initial stage of the folding path, the gas reactant needs to travel a longer path, and the contact time between the gas reactant and the semiconductor substrate is longer. This can promote a more uniform or greater distribution of the gas reactant in the second region, and also promote a uniform distribution of the gas reactant at the edge of the second region. Therefore, the portion of the second semiconductor layer located at the edge of the second region can be continuously deposited and grown, and is also relatively dense, which significantly improves the passivation performance of the back contact solar cell and increases the open circuit voltage of the back contact solar cell.

[0056] It should be noted that, in this application, W1 < W3 < W2 < W4 specifically means that, between a first region and a third region adjacent to the first region, W1, W3, W2, and W4 have an increasing trend. The increasing method can be linear, exponential, etc., and is not limited thereto. The directions in which W1, W3, W2, and W4 are located are all parallel to the first direction X.

[0057] In some embodiments, refer to Figures 2 to 4Along the first direction X, the width of the first platform sub-region 131 is W1, the width of the second platform sub-region 133 is W2, the width of the first slope sub-region 132 is W3, and the width of the second slope sub-region 134 is W4. The ratio of W2 / W1 is between 10 and 300. If this ratio is too small, as mentioned above, the increase in the residence time of the gas reactant in the gas reactant return path or the contact time between the gas reactant and the second region is weak. If this ratio is too large, the process of forming the second region is difficult to achieve. Therefore, if W2 / W1 is within the above range, the increase in the residence time of the gas reactant in the gas reactant return path or the contact time between the gas reactant and the second region is large, which can further promote a more uniform or greater distribution of the gas reactant in the second region. It can also promote a uniform distribution of the gas reactant at the edge of the second region. Therefore, the portion of the second semiconductor layer located at the edge of the second region can be continuously deposited and grown, and is also relatively dense, which significantly improves the passivation performance of the back contact solar cell and increases the open-circuit voltage of the back contact solar cell.

[0058] For example, W2 / W1 can be 10, 12, 15, 18, 20, 50, 60, 80, 100, 120, 150, 180, 200, 250, or 300.

[0059] In some embodiments, refer to Figures 2 to 4 The ratio of W3 / W1 is 6 to 150. Similarly, within the above range, the increase in the residence time of gaseous reactants in the gaseous reactant return path or the contact time between gaseous reactants and the second region is relatively large. This can further promote a more uniform or greater distribution of gaseous reactants in the second region, and promote a uniform distribution of gaseous reactants at the edge of the second region. Therefore, the portion of the second semiconductor layer located at the edge of the second region can be continuously deposited and grown, and is also relatively dense, which significantly improves the passivation performance of the back contact solar cell and increases the open-circuit voltage of the back contact solar cell.

[0060] For example, W3 / W1 can be 6, 8, 10, 12, 15, 18, 20, 50, 60, 80, 100, 120, or 150.

[0061] In some embodiments, refer to Figures 2 to 4The W4 / W3 ratio is 1.2 to 500. Similarly, within the above range, the increase in the residence time of the gaseous reactants in the gaseous reactant return path or the contact time between the gaseous reactants and the second region is relatively large. This can further promote a more uniform or greater distribution of the gaseous reactants in the second region. It also promotes a uniform distribution of the gaseous reactants at the edge of the second region. Therefore, the portion of the second semiconductor layer located at the edge of the second region can be continuously deposited and grown, and is also relatively dense. This significantly improves the passivation performance of the back contact solar cell and increases the open-circuit voltage of the back contact solar cell.

[0062] For example, W4 / W3 can be 1.2, 2, 3, 4, 5, 6, 8, 10, 12, 15, 18, 20, 50, 60, 80, 100, 120, 150, 200, 250, 300, 350, or 400.

[0063] In some embodiments, refer to Figures 2 to 4 The W4 / W2 ratio is 1.1 to 300. Similarly, within the above range, the increase in the residence time of the gaseous reactants in the gaseous reactant return path or the contact time between the gaseous reactants and the second region is relatively large. This can further promote a more uniform or greater distribution of the gaseous reactants in the second region. It also promotes a uniform distribution of the gaseous reactants at the edge of the second region. Therefore, the portion of the second semiconductor layer located at the edge of the second region can be continuously deposited and grown, and is also relatively dense. This significantly improves the passivation performance of the back contact solar cell and increases the open-circuit voltage of the back contact solar cell.

[0064] For example, W4 / W2 can be 1.1, 2, 3, 4, 5, 6, 8, 10, 12, 15, 18, 20, 50, 60, 80, 100, 120, 150, 200, 250, 300.

[0065] In some embodiments, refer to Figures 2 to 4 W1 ranges from 2nm to 10nm. A larger W1 can increase the residence time of the gaseous reactants in the gaseous reactant return path or the contact time between the gaseous reactants and the second region. However, if W1 is too large, the process is difficult to implement and may lead to over-etching. Therefore, within the above range, W1 significantly increases the residence time of the gaseous reactants in the gaseous reactant return path or the contact time between the gaseous reactants and the second region. This can further promote a more uniform or greater distribution of the gaseous reactants in the second region, and also promote a uniform distribution of the gaseous reactants at the edges of the second region. Moreover, the process is easier to implement.

[0066] For example, W1 can be 2nm, 3nm, 4nm, 5nm, 6nm, 7nm, 8nm, 9nm, or 10nm.

[0067] In some embodiments, refer to Figures 2 to 4 W2 ranges from 100nm to 600nm. A larger W2 can increase the residence time of gaseous reactants in the gaseous reactant return path or the contact time between the gaseous reactants and the second region. However, if W2 is too large, the process is difficult to implement and may lead to over-etching. Therefore, within the above range, W2 significantly increases the residence time of gaseous reactants in the gaseous reactant return path or the contact time between the gaseous reactants and the second region. This can further promote a more uniform or greater distribution of gaseous reactants in the second region, and also promote a uniform distribution of gaseous reactants at the edges of the second region. Moreover, the process is easier to implement.

[0068] For example, W2 can be 100nm, 150nm, 200nm, 250nm, 300nm, 350nm, 400nm, 450nm, 500nm, 550nm, or 600nm.

[0069] In some embodiments, refer to Figures 2 to 4 The wavelength W3 ranges from 60nm to 300nm. A larger W3 can increase the residence time of the gaseous reactants in the gaseous reactant return path or the contact time between the gaseous reactants and the second region. However, an excessively large W3 makes the process difficult to implement and may lead to over-etching. Therefore, within the above-mentioned range, W3 significantly increases the residence time of the gaseous reactants in the gaseous reactant return path or the contact time between the gaseous reactants and the second region. This can further promote a more uniform or abundant distribution of the gaseous reactants in the second region, and also promote a uniform distribution of the gaseous reactants at the edges of the second region. Moreover, the process is easier to implement.

[0070] For example, W3 can be 60nm, 80nm, 90nm, 100nm, 150nm, 200nm, 250nm, or 300nm.

[0071] In some embodiments, refer to Figures 2 to 4 The wavelength W4 ranges from 500nm to 3000nm. A larger W4 can increase the residence time of the gaseous reactants in the gaseous reactant return path or the contact time between the gaseous reactants and the second region. However, an excessively large W4 makes the process difficult to implement and may lead to over-etching. Therefore, within the above range, W4 significantly increases the residence time of the gaseous reactants in the gaseous reactant return path or the contact time between the gaseous reactants and the second region. This can further promote a more uniform or abundant distribution of the gaseous reactants in the second region, and also promote uniform distribution of the gaseous reactants at the edges of the second region. Moreover, the process is easier to implement.

[0072] For example, W4 can be 500nm, 600nm, 900nm, 1000nm, 1500nm, 2000nm, 2500nm, or 3000nm.

[0073] In some embodiments, refer to Figures 2 to 4 In the thickness direction Z of the back-contact solar cell, the height of the first ramp region 132 is H1, and the height of the second ramp region 134 is H2, where H2 > H1, and H1 is between 100 nm and 300 nm. (Refer to...) Figures 2 to 4 The endpoint and starting point of H1 can be the first platform sub-region 131 and the second platform sub-region 133, respectively. The endpoint and starting point of H2 can be the second platform sub-region 133 and the bottom of the pyramid-like structure in the second region, respectively. Specifically, the thickness of the inner extension layer of the semiconductor layer in the first semiconductor layer, such as the N-type doped polysilicon layer 2, is typically tens of nanometers, and H1 is 100nm to 300nm. This indicates that during the formation of the first slope sub-region 132, the inner extension layer of the N-type doped polysilicon layer 2 in the first semiconductor layer has been basically etched clean, and H2 > H1. During the formation of the second slope sub-region 134, the inner extension layer of the N-type doped polysilicon layer 2 in the first semiconductor layer has also been basically etched clean. Most sub-regions of this second region do not have the inner extension layer of the N-type doped polysilicon layer 2 in the first semiconductor layer. Even if the doped layer in the second semiconductor layer is discontinuous in the second region, and even if the first transparent conductive layer 41 at the discontinuity position is in contact with the second region, since most sub-regions of the second region do not have the inner extension layer of the N-type doped polysilicon layer 2 in the first semiconductor layer, there is basically no risk of leakage, or the risk of leakage is very low, thus achieving the effect of precise control of the leakage channel. Furthermore, the heights H1 of the first slope sub-region and H2 of the second slope sub-region, in conjunction with the aforementioned W1, W2, W3, and W4, make the slope at the junction of the various sub-regions in the second region, as well as the slope of the slope itself, gentler. This makes it easier for the gaseous reactants to spread and distribute more evenly, thus improving the uniformity of the film layer. This further promotes the uniform distribution of gaseous reactants at the edge of the second region. Therefore, the portion of the second semiconductor layer located at the edge of the second region can be continuously deposited and grown, and is also relatively dense, significantly improving the passivation performance of the back contact solar cell and increasing the open-circuit voltage of the back contact solar cell.

[0074] For example, H1 can be 100nm, 120nm, 150nm, 180nm, 200nm, 220nm, 250nm, 290nm, or 300nm.

[0075] In some embodiments, the H2 / H1 ratio is between 5 and 800. If this ratio is too large, the process is difficult to implement and may cause the slope change at the junction of the sub-regions of the second region to be too abrupt. The distribution of gaseous reactants is easily blocked by the abrupt slope change, and the distribution of gaseous reactants at the junction of the sub-regions of the second region is likely to be discontinuous, resulting in discontinuity and non-uniformity of the second semiconductor layer. If this ratio is too small, the improvement on the spread of gaseous reactants is not good. Therefore, H2 / H1 within the above range further promotes the continuous deposition and growth of the portion of the second semiconductor layer located at the edge of the second region, and is also relatively dense, which significantly improves the passivation performance of the back contact solar cell and improves the open circuit voltage of the back contact solar cell.

[0076] For example, H2 / H1 can be 5, 6, 9, 10, 50, 80, 100, 200, 300, 400, 500, 600, 700, or 800.

[0077] It should be noted that in this application, H2 / H1 can be determined in the same second region, and the subsequent difference between H2 and H1 is also determined in the same second region.

[0078] In some embodiments, the difference between H2 and H1 is 6 μm to 8 μm. Similarly, the difference between H2 and H1 within the above range further promotes the continuous deposition and growth of the portion located at the edge of the second region in the second semiconductor layer, which is also relatively dense, significantly improving the passivation performance of the back contact solar cell and increasing the open circuit voltage of the back contact solar cell.

[0079] For example, the difference between H2 and H1 can be 6μm, 6.2μm, 6.5μm, 6.9μm, 7μm, 7.3μm, 7.5μm, 7.8μm, or 8μm.

[0080] In some embodiments, H2 is 2 μm to 8 μm. Similarly, H2 within the above range further promotes the continuous deposition and growth of the portion located at the edge of the second region in the second semiconductor layer, which is also relatively dense, significantly improving the passivation performance of the back contact solar cell and increasing the open circuit voltage of the back contact solar cell.

[0081] For example, H2 can be 2m, 3μm, 4μm, 5μm, 6μm, 7μm, or 8μm.

[0082] In some embodiments, refer to Figures 2 to 4Along the thickness direction Z of the semiconductor substrate, the angle between the first platform sub-region 131 and the first slope sub-region 132 is α, and the angle between the second platform sub-region 133 and the second slope sub-region 134 along the thickness direction Z of the semiconductor substrate is β. α and β are different and both are obtuse angles. On one hand, from the side where the gaseous reactant enters, each sub-region of the second region does not obstruct adjacent sub-regions, and each sub-region of the second region is fully exposed, ensuring that the gaseous reactant and each sub-region of the second region can fully contact each other. This promotes continuous deposition and growth of the portion located at the edge of the second region in the second semiconductor layer, resulting in a denser structure and further improving the passivation performance of the back contact solar cell. On the other hand, the difference between α and β makes the atmosphere of the gaseous reactant more chaotic and allows it to remain for a longer time, further promoting continuous deposition and growth of the portion located at the edge of the second region in the second semiconductor layer, resulting in a denser structure and significantly improving the passivation performance of the back contact solar cell, thus increasing the open-circuit voltage of the back contact solar cell.

[0083] In some embodiments, a≥b, during the return of gaseous reactants, b is relatively small and a is relatively large, which allows the gaseous reactants to remain for a longer time, further promoting the continuous deposition and growth of the portion located at the edge of the second region in the second semiconductor layer, which is also relatively dense, significantly improving the passivation performance of the back contact solar cell and increasing the open-circuit voltage of the back contact solar cell.

[0084] In some embodiments, refer to Figures 2 to 4 In the thickness direction Z of the semiconductor substrate, the side surface of the first semiconductor layer is designated as the first side surface 21, which intersects with the surface of the first semiconductor layer away from the semiconductor substrate. The edge of the same first side surface 21 away from the semiconductor substrate 1 is designated as the first edge 211 (the edge away from the second surface 11), and the edge closer to the semiconductor substrate 1 is designated as the second edge (the edge closer to the second surface 11). The first edge 211 refers to the boundary line or outline of the first side surface 21 away from the semiconductor substrate 1, and the second edge refers to the boundary line or outline of the first side surface 21 closer to the semiconductor substrate 1. Both edges extend perpendicularly to the plane of the paper. (Refer to...) Figure 3Relative to the first platform sub-region 131, at least a portion of the first side surface 21 of the first semiconductor layer is an inclined surface. That is, along the first direction X: at least a portion of the first side surface 211 is away from the second region 13, and the second side is close to the second region 13. From the first side to the second side, the first side surface is successively close to the second side. Since the first side surface 21 of the first semiconductor layer is an inclined surface and is successively close to the second side surface 11, along the thickness direction Z of the semiconductor substrate, or from the side where the gas reactant enters, the first side surface 21 of the first semiconductor layer is not blocked at any position. The first side surface 21 of the first semiconductor layer is fully exposed, ensuring that the gas reactant and the first side surface 21 of the first semiconductor layer can fully contact each other. This can promote the continuous deposition and growth of the portion of the second semiconductor layer located on the first side surface of the first semiconductor layer, which is also relatively dense, further improving the passivation performance of the back contact solar cell.

[0085] In some embodiments, refer to Figures 2 to 4 In the thickness direction Z of the semiconductor substrate, the side surface of the first semiconductor layer is designated as the first side surface 21, which intersects with the surface of the first semiconductor layer away from the semiconductor substrate. Within the same first side surface 21, the edge away from the semiconductor substrate 1 is designated as the first edge 211 (the edge away from the second surface 11), and the edge closer to the semiconductor substrate 1 is designated as the second edge (the edge closer to the second surface 11). (Refer to...) Figure 2 Relative to the first platform sub-region 131, at least a portion of the first side is vertically arranged. That is, from the first side 211 to the second side, at least a portion of the first side is perpendicular to the first platform sub-region 131. In other words, the first side 21 of the first semiconductor layer is a vertical surface. Then, along the thickness direction Z of the semiconductor substrate, or from the side where the gas reactant enters, the first side 21 of the first semiconductor layer is less obscured and more exposed. The gas reactant and the first side 21 of the first semiconductor layer can contact each other, which can promote the continuous deposition and growth of the portion of the second semiconductor layer located on the first side of the first semiconductor layer, and make it more dense.

[0086] In some embodiments, refer to Figures 2 to 4 In the thickness direction Z of the semiconductor substrate, the first semiconductor layer has a first side surface 21, which intersects with the surface of the first semiconductor layer away from the semiconductor substrate. (Refer to...) Figure 4 At least a portion of the first side 21 has a recessed structure 22 that is recessed into the first semiconductor layer, relative to Figure 3 and Figure 2 , Figure 4The concave structure 22 in the middle provides some shielding for the gaseous reactants, but it has the highest compatibility with existing processes and is easy to implement. At the same time, through the first platform sub-region added by the aforementioned second region 13, as well as other improvements, it is possible to achieve continuous deposition and growth at various positions of the second semiconductor layer, which is also relatively dense, further improving the passivation performance of the back contact solar cell.

[0087] It should be noted that the distribution position of the concave structure 22 in the first side surface 21 along the first direction X in the first side surface is not limited. For example, Figure 4 In this case, the concave structure 22 is located in the first side surface 21 near the first side. Alternatively, the concave structure 22 can also be located in the first side surface 21 near the second side. Or, the concave structure 22 can be located in the first side surface 21 between the second and first sides.

[0088] Figure 6 for Figure 5 An enlarged schematic diagram showing the position of the dashed ellipse. In some embodiments, refer to... Figure 5 and Figure 6 The undulation of the first platform sub-region 131 is less than the undulation of the surface of the first semiconductor layer away from the first surface (that is, the surface of the N-type doped polycrystalline silicon layer 2 away from the first surface). The undulation of the second platform sub-region 133 is less than the undulation of the surface of the first semiconductor layer away from the first surface (that is, the surface of the N-type doped polycrystalline silicon layer 2 away from the first surface). On the one hand, by setting the undulation of the first platform sub-region and the second platform sub-region to be relatively small, especially in the second region at the junction of the first semiconductor layer and the second semiconductor layer, since this region has undergone multiple processing such as laser processing and wet processing, there are more defects and exposures in the semiconductor substrate. Therefore, the film formation quality of the second semiconductor layer in the second region should be good to ensure the passivation performance of the back contact solar cell. On the other hand, in the first region, the first semiconductor layer has not undergone much process influence, so the passivation of the semiconductor substrate by the first semiconductor layer itself is relatively good. The surface undulation of the first semiconductor layer away from the first surface is larger, and the roughness is greater. When the first transparent conductive layer 41 is subsequently fabricated, the adhesion and contact area between the first transparent conductive layer 41 and the surface of the first semiconductor layer away from the first surface is larger. The first transparent conductive layer 41 and the first semiconductor layer form a three-dimensional interwoven heterogeneous interface, which greatly enhances the van der Waals forces and mechanical interlocking forces between the film layers, effectively releases the stress caused by the mismatch of thermal expansion coefficients, and significantly reduces the risk of peeling of the first transparent conductive layer 41 in subsequent processes or outdoor conditions, thereby improving the long-term reliability of the battery. The material of the first transparent conductive layer 41 can be TCO (transparent conductive oxide), etc. The material of the second transparent conductive layer is similar.

[0089] It should be noted that one way to achieve a larger degree of undulation on the surface of the first semiconductor layer that is far from the first surface is to have a higher doping concentration of the N-type doped polysilicon layer of the first semiconductor layer compared to the doping concentration of the semiconductor substrate. In the same etching process, the etching rate of the N-type doped polysilicon layer is faster, and there are significant differences in the etching rate at different locations, so a surface with a larger degree of undulation can be formed.

[0090] In some embodiments, the undulation of the portion of the second semiconductor layer located on the first platform sub-region 131 is less than the undulation of the portion of the first semiconductor layer located away from the first surface. That is, the portion of the second semiconductor layer located on the first platform sub-region 131 is smoother, while the portion located away from the first surface is rougher. By setting the undulation of the portion of the second semiconductor layer located on the first platform sub-region 131 to be relatively small, especially in the second region at the junction of the first and second semiconductor layers, where multiple processing steps such as laser processing and wet processing have resulted in more defects and exposure of the semiconductor substrate, the film quality of the second semiconductor layer in the second region must be good to ensure the passivation performance of the back contact solar cell. Similarly, in the first region, the covered first semiconductor layer has not undergone excessive processing influences, so the passivation of the semiconductor substrate by the first semiconductor layer itself is relatively good. Setting the undulation of the portion of the first semiconductor layer away from the first surface to be larger greatly enhances the van der Waals forces and mechanical interlocking forces between the film layers, effectively releasing the stress caused by the mismatch of thermal expansion coefficients, significantly reducing the risk of peeling of the first transparent conductive layer 41 in subsequent processes or outdoor conditions, thereby improving the long-term reliability of the battery. As mentioned earlier, the difference in the degree of undulation at different locations of the second semiconductor layer can be achieved by means of the difference in the degree of undulation between the first platform sub-region 131 and the surface of the first semiconductor layer away from the first surface (that is, the surface of the N-type doped polysilicon layer 2 away from the first surface), which can be formed by conformal shaping.

[0091] In some embodiments, the undulation of the portion of the second semiconductor layer located on the second platform sub-region is less than that of the portion of the first semiconductor layer located away from the first surface. That is, for the second semiconductor layer, the portion located on the second platform sub-region 133 is smoother, while the portion located on the first semiconductor layer away from the first surface is rougher. On the one hand, by setting the undulation of the portion of the second semiconductor layer located on the second platform sub-region 133 to be relatively small, especially in the second region at the junction of the first and second semiconductor layers, where multiple processing steps such as laser processing and wet processing have resulted in more defects and exposure of the semiconductor substrate, the film quality of the second semiconductor layer in the second region must be good to ensure the passivation performance of the back contact solar cell. Similarly, in the first region, the covered first semiconductor layer has not undergone excessive processing influences, so the passivation of the semiconductor substrate by the first semiconductor layer itself is relatively good. Setting the undulation of the portion of the first semiconductor layer away from the first surface to be larger greatly enhances the van der Waals forces and mechanical interlocking forces between the film layers, effectively releasing the stress caused by the mismatch of thermal expansion coefficients, significantly reducing the risk of peeling of the first transparent conductive layer 41 in subsequent processes or outdoor conditions, thereby improving the long-term reliability of the battery. As mentioned earlier, the difference in the degree of undulation at different locations of the second semiconductor layer can be achieved by means of the difference in the degree of undulation between the second platform sub-region 133 and the surface of the first semiconductor layer away from the first surface (that is, the surface of the N-type doped polysilicon layer 2 away from the first surface), which can be formed by conformal shaping.

[0092] In this application, the degree of undulation of the portion of the second semiconductor layer located on the second plateau sub-region can refer to the height difference between the high and low points of the portion of the second semiconductor layer located on the second plateau sub-region within a unit area or unit length along the thickness direction Z of the semiconductor substrate. The degree of undulation can be determined by measuring the roughness of the portion of the second semiconductor layer located on the second plateau sub-region within a unit area or unit length on the surface of the second semiconductor layer away from the semiconductor substrate, or by observing the undulation of the portion of the second semiconductor layer located on the second plateau sub-region within a unit area or unit length on the surface of the second semiconductor layer away from the semiconductor substrate using SEM (scanning electron microscopy), or by measuring the height difference distribution data of the portion of the second semiconductor layer located on the second plateau sub-region within a unit area or unit length on the surface of the second semiconductor layer away from the semiconductor substrate using a 3D microscope. The specific values ​​of the unit length and unit area are not limited here. For example, the unit length can be 1 nm, 10 nm, etc. The undulation at other locations in this application is similar, and will not be elaborated further to avoid repetition.

[0093] In some embodiments, refer to Figures 2 to 6Both the first platform sub-region 131 and the second platform sub-region 133 are planar. Here, "planar" means that, compared to the textured surface of the pyramid structure, the first and second platform sub-regions have relatively flat surfaces, or less undulation, or less roughness, and are relatively smooth and flat. By setting the first platform sub-region 131 and the second platform sub-region 133 to be relatively flat, especially in the second region at the junction of the first and second semiconductor layers, where there are many defects and exposed areas of the semiconductor substrate due to multiple processing steps such as laser processing and wet processing, it is crucial to ensure good film quality of the second semiconductor layer in the second region to guarantee the passivation performance of the back contact solar cell.

[0094] In some embodiments, refer to Figures 1 to 4 ,as well as Figure 7 The third region 14 includes a frustum-like structure 141; the second face 11 includes a pyramid-like structure. There can be multiple frustum-like structures; this application uses one frustum-like structure for illustration. There can also be multiple pyramid-like structures; this application uses one frustum-like structure for illustration. The projected area of ​​the top of the frustum-like structure 141 may be larger than the projected area of ​​the top of the pyramid-like structure. Figure 7The top 142 of the truncated pyramid structure 141 is octagonal in shape. It can be considered that the top of the truncated pyramid structure 141 has a larger projected area, making it flatter than the top of the pyramid structure. Alternatively, it can be considered that the truncated pyramid structure is sharpened, or that its top has a larger surface area, while the pyramid structure's top is sharp and essentially faceless. Therefore, compared to the sharp pyramid structure, the top of the truncated pyramid structure is a flatter surface, resulting in better film quality for the second semiconductor layer. Furthermore, on the second surface, i.e., the light-facing surface of the back-contact solar cell, the pyramid structure can increase the light-trapping effect of the front-incident light, improve light utilization, increase the short-circuit current of the back-contact solar cell, and improve power generation efficiency. Meanwhile, when the second semiconductor layer contains doped amorphous silicon, laser energy is applied to the second semiconductor layer on the truncated pyramid structure in the third region for laser crystallization. The truncated pyramid structure has a larger surface area at the top, allowing for more uniform absorption of laser energy in the top region of the second semiconductor layer. This increases the crystallization degree of the second semiconductor layer in the top region of the truncated pyramid structure, improves carrier transport efficiency, and reduces transport losses. Furthermore, the larger surface area at the top of the truncated pyramid structure increases the subsequent laser crystallization process window. A relatively flat top surface is easier to process than a sharp top surface, resulting in a larger process window. This is because the sharp apex of the pyramid structure receives less laser energy, leading to a concentrated electric field and easily causing localized breakdown of the second semiconductor layer, resulting in high-density defects such as pinholes. These micro- and nano-scale defects become fatal carrier recombination centers, causing a sharp deterioration in passivation performance and directly lowering the open-circuit voltage of the back-contact solar cell. Laser crystallization primarily involves the localized amorphous silicon being affected by laser energy, causing it to transform into nanocrystalline or microcrystalline silicon, increasing the crystallization degree of the material in the film and improving conductivity. Specifically, the lower the crystallinity of the second semiconductor layer, the smaller the grains within it, even exhibiting the disordered characteristics of amorphous silicon. Smaller grains result in more interfaces between the grains, leading to higher inter-grain resistance and increased contact resistance. Conversely, higher crystallinity results in larger grains, fewer inter-grain interfaces, and lower inter-grain resistance, reducing contact resistance and thus minimizing transport losses of charge carriers collected within the second semiconductor layer to the conductive material.

[0095] The second side 11 includes a pyramid-like structure. Although it has a relatively sharp top, the passivation layer 7 on the front side of the second side can usually be formed by atomic layer deposition and other methods. Its conformability is better, so good film quality can still be achieved on the second side, and good passivation and protection can be achieved on the second side.

[0096] In some embodiments, the back-contact solar cell further includes a front passivation and antireflection layer located on the second surface 11. This front passivation and antireflection layer may comprise a front passivation layer 7 and a front antireflection layer 8. The front passivation and antireflection layer can be a stacked structure of alumina and silicon nitride. Atomic layer deposition (ALD) of alumina has self-limiting surface chemical reaction characteristics, theoretically enabling atomically precise conformal deposition on any complex three-dimensional morphology. Whether at the pyramid tip or the microstructure mentioned in this application, the alumina film thickness and chemical composition remain highly uniform. As a protective and antireflection layer covering the alumina, plasma-enhanced chemical vapor deposition (PECVD) of silicon nitride, while not as conformal as ALD, has a relatively mature and controllable deposition process. Furthermore, the large number of hydrogen atoms released by silicon nitride at high temperatures can diffuse through the alumina to the entire interface, achieving "no dead angle" chemical passivation of the entire complex textured surface. On the other hand, the aforementioned front passivation and antireflection layer is easy to prepare and readily mass-produced.

[0097] It should be noted that the degree of crystallinity can be characterized by crystallinity rate. Increased crystallinity rate leads to increased carrier mobility, increased effective doping concentration, and improved conductivity of the second semiconductor layer. Crystallinity rate can be measured using Raman spectroscopy. Amorphous silicon, microcrystalline silicon, and crystalline silicon have different wavenumbers; for example, amorphous silicon is approximately 480 / cm², microcrystalline silicon is approximately 510 / cm², and crystalline silicon is 520.7 / cm². The amount of component affects the Raman spectral intensity of the corresponding peak, and the crystallinity rate can be obtained by integration. The degree of crystallinity can also be compared and explained by observing the grain distribution and size in different regions of the second semiconductor layer using TEM (transmission electron microscopy). For example, microcrystalline silicon has a short-range ordered atomic structure with larger grain sizes, while amorphous silicon is amorphous silicon with smaller grain sizes.

[0098] The orthographic projection area of ​​the top of a truncated pyramid structure refers to the area of ​​the projection of the top of the truncated pyramid structure onto the adjacent structures in the battery when illuminated by light rays parallel to the thickness direction Z of the semiconductor substrate. The determination of the orthographic projection area of ​​the top of a pyramid structure is similar, and will not be repeated here to avoid repetition.

[0099] In some embodiments, refer to Figure 2 and Figure 7Both the frustum-like structure 141 and the pyramid-like structure include at least two side edges 145. In the semiconductor substrate thickness direction, both the frustum-like structure 141 and the pyramid-like structure have a second side edge 144. The side edge 145 has a top 142 and a bottom 143, with the bottom 143 closer to the semiconductor substrate than the top 142. The top 142 may contain the highest point in both the frustum-like structure 141 and the pyramid-like structure. If the highest part of the frustum-like structure 141 is a plane formed by multiple points of equal height, the top may contain the geometric center of that plane. In both the frustum-like structure 141 and the pyramid-like structure, the second side edge 144 may contain a bottom edge 143 and a top edge 142. The bottom edge 143 may contain the lowest part of both the frustum-like structure 141 and the pyramid-like structure, such as a bottom outline. The top of the second side edge has a microstructure; the region of the second side edge with the microstructure is the first sub-side edge, and the remaining region is the second sub-side edge. The distinction between the first and second sub-side edges can be considered to be based on whether or not they have a microstructure. The side edge 145 of the second side surface includes: a first segment 1451 corresponding to the first sub-side surface, and a second segment corresponding to the second sub-side surface. Figure 7The portion of the side edge 145 excluding the first segment 1451 is the second segment. That is, the first sub-side face is the top 142 portion of the second side face of the frustum-like structure 141 and the pyramid-like structure, while the second sub-side face is the portion of the second side face of the frustum-like structure 141 and the pyramid-like structure excluding the first sub-side face. Both the first sub-side face of the frustum-like structure 141 and the first sub-side face of the pyramid-like structure have microstructures. Within the same side edge of the same frustum-like structure 141 and the same pyramid-like structure: along the direction from the top 142 to the bottom 143, if the length of the first segment 1451 is less than or equal to 90% of the length of the side edge 145, then the first sub-side face of the second side face of the frustum-like structure 141 includes the top, while the second sub-side face includes the bottom. The second sub-side face is the portion of the second side face of the frustum-like structure 141 and the pyramid-like structure including the bottom, and it is also the adjacent portion of an adjacent frustum-like structure 141 or an adjacent pyramid-like structure. These positions are relatively complex. The first sub-side, typically characterized by numerous voids or defects, requires greater passivation. Due to the obstruction of adjacent frustum-like structures 141 and pyramid-like structures, the probability of light reaching the second sub-side is relatively low, resulting in a lower demand for light trapping. Therefore, the second sub-side has a greater need for passivation and a smaller need for light trapping. Light usually preferentially reaches the first sub-side, leading to a greater demand for light trapping. Simultaneously, the top 142 typically has fewer voids or defects, further reducing the need for passivation. In other words, the first sub-side has a greater demand for light trapping and a weaker demand for passivation. Therefore, in this application, the microstructure of the first sub-side, which has a greater demand for light trapping and a weaker demand for passivation, can improve light utilization, increase the short-circuit current of the back-contact solar cell, and improve power generation efficiency. Furthermore, during the formation of the microstructure, the first sub-side is more easily exposed to etchants, making its microstructure easier to form and facilitating mass production. In this application, for the second sub-side with high passivation requirements but relatively low light trapping requirements, the second sub-side has a smooth and flat surface without microstructures, resulting in a high-quality passivation and antireflection layer that ensures excellent passivation effects at all locations. Furthermore, the second semiconductor layer typically contains amorphous silicon. The design described above eliminates the problem of amorphous silicon epitaxial nucleation to form monocrystalline silicon caused by deep and narrow geometric shielding. Monocrystalline silicon has a weaker passivation effect than amorphous silicon, thus completely breaking the existing technical contradiction of "stronger light trapping, weaker passivation." This provides a technical path for back-contact solar cells to eliminate the fundamental contradiction between optical gain and passivation quality.In summary, this application divides the second side of the truncated pyramid structure and the pyramid structure according to their different requirements for light trapping and passivation. Different textured morphologies are designed for different sub-regions, which takes into account both light absorption and light trapping effect, can further improve short-circuit current, further improve the photoelectric conversion efficiency of solar cells, and ensure excellent passivation effect at all points of the back contact solar cell.

[0100] It should be noted that, within the same side edge 145, the length of the first segment 1451 and the direction of the length of the side edge 145 are both parallel to the extension direction of the side edge 145. The length of the first segment 1451 can be the straight-line distance between the top endpoint of the side edge 145 and the endpoint of the first segment 1451 away from the top. The method for determining the length of the side edge 145 is similar. In this application, the methods for determining the length of the side edge 145 and the length of the first segment 1451 include, but are not limited to, the above-described examples. Figure 7 In the diagram, the black dotted rings represent the outline of the first sub-side away from the top, while the white solid rings represent the bottom outline. The aforementioned microstructures on the semiconductor substrate surface may exhibit some conformity in the corresponding portion of the second semiconductor layer. These microstructures can be observed by peeling away the outer structure, or by observing them on the outer structure itself. For example, regarding the third region, the microstructures can be observed in the portion of the second semiconductor layer corresponding to the third region, or in the portion of the outer structure of the second semiconductor layer away from the semiconductor substrate that corresponds to the third region. As long as the approximate outline of the microstructure is observed in the portion of the second semiconductor layer corresponding to the third region, or in the portion of the outer structure of the second semiconductor layer away from the semiconductor substrate that corresponds to the third region, it is equivalent to the third region of the semiconductor substrate possessing the aforementioned microstructures. The first sub-side corresponding to the first segment 1451 refers to the portion of the side edge 145 located on the first sub-side, which is the first segment 1451. The second sub-side corresponding to the second segment refers to the portion of the side edge 145 located on the second sub-side, which is the second segment.

[0101] For example, for frustum-like structures and pyramid-like structures, in the same side edge 145, the length of the first segment 1451 accounts for 90%, 80%, 70%, 60%, 50%, 40%, 30%, 20%, 10%, 8%, and 5% of the length of the side edge 145.

[0102] In some embodiments, in the same side edge of the same type of frustum structure, the length of the first segment relative to the length of the side edge along the direction from top to bottom is less than the length of the first segment relative to the length of the side edge in the same side edge of the same type of pyramid structure, that is, in the frustum structure, the length of the second segment accounts for a larger proportion of the length of the side edge, which further improves the film formation quality of the portion of the second semiconductor layer located in the third region, and can further improve the passivation effect of the bottom of the second side of the frustum structure 141.

[0103] In some embodiments, the height of the truncated pyramid structure in the third region is 0.5 μm to 5 μm. The height of the truncated pyramid structure is not too high, and the height difference is not too large, indicating that the height of the truncated pyramid structure in the third region is relatively suitable and relatively uniform. This is conducive to the rapid spread of gaseous reactants in the third region. Therefore, the gaseous reactants are more evenly distributed or more abundant in the third region. As a result, the portion of the second semiconductor layer located in the third region can be continuously deposited and grown, and is relatively dense. The quality of the passivation and antireflection layer formed is good, which can ensure that there is excellent passivation effect at each position. This significantly improves the passivation performance of the back contact solar cell, and improves the open-circuit voltage and fill factor of the back contact solar cell.

[0104] For example, the height of the frustum-like structure in the third region can be 0.5μm, 0.8μm, 1.0μm, 1.0μm, 1.05μm, 1.1μm, 1.15μm, 1.2μm, 1.25μm, 1.3μm, 1.35μm, 1.4μm, 1.45μm, 1.5μm, 1.6μm, 1.8μm, 2.0μm, 2.5μm, 3.0μm, 3.5μm, 4.0μm, 4.5μm, or 5.0μm.

[0105] In some embodiments, the height of the pyramid-like structure on the second surface is 0.5 μm to 1.5 μm. The height of the pyramid-like structure is not excessive. Here, the second surface is the light-facing surface of the semiconductor substrate. The smaller height of the pyramid-like structure on the light-facing surface of the semiconductor substrate allows for precise band-specific control of long-wavelength and short-wavelength light, while simultaneously considering both optical and electrical performance, ultimately improving the overall conversion efficiency of the battery. Specifically, firstly, the smaller height of the pyramid-like structure on the light-facing surface of the semiconductor substrate can efficiently couple short-wavelength light, reduce front reflection losses, enhance the capture of visible light, and improve the external quantum efficiency in the short-wavelength band; secondly, it is suitable for more refined front passivation and anti-reflection layer deposition, reducing the probability of front carrier recombination and increasing the open-circuit voltage, while not compromising the passivation effect of the light-facing surface.

[0106] For example, the height of the pyramid-like structure on the second surface can be 0.5μm, 0.8μm, 1.0μm, 1.0μm, 1.05μm, 1.1μm, 1.15μm, 1.2μm, 1.25μm, 1.3μm, 1.35μm, 1.4μm, 1.45μm, 1.5μm, 1.6μm, 1.8μm, 2.0μm, 2.5μm, 3.0μm, 3.5μm, 4.0μm, 4.5μm, or 5.0μm.

[0107] In some embodiments, the microstructures of the first sub-side of the frustum-like structure and the microstructures of the first sub-side of the pyramid-like structure have the same or similar morphology. Therefore, the microstructures of the first sub-side of the frustum-like structure and the microstructures of the first sub-side of the pyramid-like structure can be formed using the same process parameters, or even in the same process step. This results in good process compatibility and eliminates the need for multi-step texturing, thereby improving production efficiency.

[0108] In some embodiments, the microstructures of the first sub-side of the frustum-like structure and the microstructures of the first sub-side of the pyramid-like structure both contain pleated structures. Similarly, the microstructures of the first sub-side of the frustum-like structure and the microstructures of the first sub-side of the pyramid-like structure can be formed using the same process parameters, or even in the same process step, resulting in good process compatibility and eliminating the need for multi-step texturing, thus improving production efficiency.

[0109] In some embodiments, the microstructures of the first sub-side of the frustum-like structure and the microstructures of the first sub-side of the pyramid-like structure both include a cluster of nested ring structures. Similarly, the microstructures of the first sub-side of the frustum-like structure and the microstructures of the first sub-side of the pyramid-like structure can use the same process parameters, or even be formed in the same process step, which has good process compatibility and does not require multi-step texturing, thus improving production efficiency.

[0110] In some embodiments, the height of the pyramid-like structure on the second side is less than the height of the frustum-like structure in the third region. Here, the second side is the light-facing surface of the semiconductor substrate. The pyramid-like structure with a lower height on the light-facing surface of the semiconductor substrate enables precise band-specific control of long-wavelength and short-wavelength light, while simultaneously considering both optical and electrical performance, ultimately improving the overall conversion efficiency of the battery. Specifically, firstly, the pyramid-like structure with a smaller height on the light-facing surface of the semiconductor substrate can efficiently couple short-wavelength light, reduce front reflection losses, enhance the capture of visible light, and improve the external quantum efficiency in the short-wavelength band; secondly, it is suitable for more refined front passivation and anti-reflection layer deposition, reducing the probability of front carrier recombination and increasing the open-circuit voltage, while not compromising the passivation effect of the light-facing surface. Furthermore, the third region, with its slightly larger truncated pyramid structure, is where the second semiconductor layer on the backlight surface is primarily located. This region effectively scatters long-wavelength light, significantly extending the optical path of long-wavelength photons within the battery and enhancing absorption and utilization in the near-infrared band. Additionally, in conjunction with the second passivation layer in the second semiconductor layer, it further reflects unabsorbed long-wavelength photons back into the semiconductor substrate, reducing long-wavelength escape losses and increasing long-wavelength photocurrent. Moreover, the slightly larger truncated pyramid structure in the third region, compared to the slightly smaller pyramid structure on the light-facing surface of the semiconductor substrate, allows for full-spectrum light trapping optimization. Without increasing front-side recombination, it simultaneously improves the battery's short-circuit current and open-circuit voltage, ultimately achieving higher photoelectric conversion efficiency.

[0111] For example, the height of the frustum-like structure in the third region is 1.5 μm, and the height of the pyramid-like structure on the second face is 0.8 μm.

[0112] For example, the height of the frustum-like structure in the third region is 2.4 μm, and the height of the pyramid-like structure on the second face is 1.7 μm.

[0113] Figure 8 for Figure 5 A partially enlarged schematic diagram of the second slope sub-region, in some embodiments, refers to... Figure 5 and Figure 8The second slope region 134 has multiple vertical textures 1341 and multiple arc-shaped textures 1342, with the arc-shaped textures 1342 superimposed on the vertical textures 1341. The extension direction of the arc-shaped textures 1342 intersects the extension direction of the vertical textures 1341, either perpendicularly or approximately perpendicularly, such as at an angle of 80° to 110°. The extension direction of the vertical textures 1341 is the aforementioned first direction X, and the extension direction of the arc-shaped textures 1342 is the second direction Y. This textured surface morphology primarily increases surface roughness, improves light-trapping effects, and enhances the adhesion of subsequently deposited structural layers. During subsequent etching operations, the arc-shaped textures superimposed on the vertical textures form a barrier against the etching medium, such as etching paste, thereby preventing excessive expansion of the etching medium and its impact on other structures.

[0114] In some embodiments, the semiconductor substrate of the hybrid back-contact solar cell is an N-type monocrystalline silicon substrate. A first semiconductor layer forms the N-region, providing electron transport for the solar cell. The first semiconductor layer is an N-type doped polycrystalline silicon layer, and a tunneling silicon oxide layer is also present between the N-type doped polycrystalline silicon layer and the semiconductor substrate. A second semiconductor layer forms the P-region, providing hole transport for the solar cell. The second semiconductor layer includes an intrinsic amorphous silicon layer and a P-type doped amorphous silicon layer. The P-type doped amorphous silicon layer also contains a portion of P-type doped microcrystalline silicon and a portion of P-type doped nanocrystalline silicon. The tunneling silicon oxide layer and the intrinsic amorphous silicon layer can serve a passivation function. Additionally, in the second region, the intrinsic amorphous silicon layer can also serve an insulating function, isolating the doped polycrystalline silicon layer from the doped silicon layer. The first and second transparent conductive layers collect charge carriers. Metal electrodes are disposed on the transparent conductive layers, and the metal electrodes, together with the transparent conductive layers disposed below them, form a system for collecting and transporting charge carriers. The transparent conductive layer has an opening, which is used to isolate the N region from the P region and prevent the transparent conductive layers on the first region and the third region from connecting and causing a short circuit.

[0115] The combination of N-type doped polycrystalline silicon layers and P-type doped amorphous silicon layers, rather than using only amorphous silicon or only polycrystalline silicon layers, aims to achieve an optimal balance between carrier selective transport, passivation quality, and conductivity. If all layers are amorphous silicon, the N-type amorphous silicon layer has low doping efficiency and poor conductivity, resulting in high electron transport resistance and a low fill factor (FF). Furthermore, the strong parasitic absorption of the N-type amorphous silicon layer wastes some back-reflected light. If all layers are polycrystalline silicon, the dopant element in the P-type polycrystalline silicon layer is often boron. High-temperature annealing causes boron to tunnel through the silicon oxide layer and enter the semiconductor substrate, forming high-concentration recombination centers at the interface. This leads to a sharp increase in the surface recombination rate and a significant reduction in open-circuit voltage. To prevent boron from tunneling through the silicon oxide layer into the silicon substrate, the annealing temperature or time needs to be reduced, but this results in insufficient activation of the P-type polycrystalline silicon, increased resistivity, and a small process window. It is difficult to achieve a perfect balance between low contact resistance and low recombination current in P-type polycrystalline silicon layers.

[0116] Hybrid back-contact solar cells typically use N-type silicon wafers as the semiconductor substrate. On the back side, two electrode regions are fabricated: a P-type region (emitter) responsible for collecting photogenerated holes and blocking electrons, and an N-type region (back field) responsible for collecting photogenerated electrons and blocking holes. The heterojunction formed between the P-type amorphous silicon layer and the N-type monocrystalline silicon substrate has a naturally low barrier for holes and a high barrier for electrons due to its band bend, effectively filtering holes and blocking electrons, achieving perfect hole-selective contact. This structure is key to obtaining high open-circuit voltage. Furthermore, an intrinsic amorphous silicon layer exists between the P-type amorphous silicon layer and the N-type monocrystalline silicon substrate, providing extreme chemical passivation and further reducing interfacial recombination. The N-type polycrystalline silicon layer, combined with a tunneling silicon oxide layer, forms a majority carrier conductive structure. Electrons can tunnel through the tunneling silicon oxide layer without hindrance and rapidly transport within the highly conductive N-type polycrystalline silicon layer. This structure provides an extremely low-resistance channel for electrons and acts as an insulator for holes.

[0117] The process for hybrid back-contact solar cells typically involves first fabricating a high-temperature N-type polycrystalline silicon layer, followed by a low-temperature P-type amorphous silicon layer. This combination allows for seamless process integration. However, if an entirely amorphous silicon layer is used, the N-type region exhibits poor performance. If an entirely polycrystalline silicon layer is used, the P-type polycrystalline silicon faces the challenge of boron atoms easily diffusing and tunneling through the silicon oxide layer at high temperatures, damaging passivation. Furthermore, the hole selectivity of the P-type polycrystalline silicon layer is far inferior to that of the P-type amorphous silicon layer. If a fully high-temperature process is used, i.e., all polycrystalline silicon layers, the entire process involves multiple high-temperature cycles (thermal oxygen generation tunneling through the silicon oxide layer, boron diffusion, phosphorus diffusion, etc.), which can easily lead to an increase in internal defects in the monocrystalline silicon substrate, a decrease in bulk lifetime, higher requirements for substrate quality, and is not conducive to wafer thinning.

[0118] This application also provides a method for fabricating a back-contact solar cell, comprising the following steps.

[0119] Step S1: Provide a semiconductor substrate, including a first surface and a second surface opposite to each other; the first surface includes a first region, a second region and a third region arranged along a first direction, the second region being located between the first region and the third region.

[0120] Step S2: A first semiconductor layer is formed on the first surface of the semiconductor substrate.

[0121] Step S3: Remove the portions of the first semiconductor layer located on the first ramp sub-region, the second plateau sub-region, the second ramp sub-region, and the third region, exposing the first ramp sub-region, the second plateau sub-region, the second ramp sub-region, and the third region; in the thickness direction of the back contact solar cell, the first ramp sub-region, the second plateau sub-region, and the second ramp sub-region are sequentially close to the second surface; the surface of the third region is concave towards the semiconductor substrate relative to the surface of the first region, and the surface of the second region is the transition sidewall of the semiconductor substrate from the first region to the third region.

[0122] Step S4: Morphological modification is performed on the structure of one side of the first surface of the semiconductor substrate, removing the portion of the first semiconductor layer located in the first platform sub-region, thus exposing the first platform sub-region; the second region includes: a first platform sub-region, a first ramp sub-region, a second platform sub-region, and a second ramp sub-region distributed along the first direction; the first platform sub-region is close to the first region, and the second ramp sub-region is close to the third region. In the thickness direction of the back contact solar cell, the first platform sub-region, the first ramp sub-region, the second platform sub-region, and the second ramp sub-region are sequentially close to the second surface.

[0123] In this application, by modifying the morphology of the structure on one side of the first surface of the semiconductor substrate, damage such as microcracks and lattice defects left over from the previous process is completely removed, and all residual impurities such as mask residue are eliminated, effectively reducing recombination in the second region and improving the photoelectric conversion efficiency of the back contact solar cell.

[0124] Step S5: A second semiconductor layer is formed on the second region and the third region, the second semiconductor layer also extending to cover a portion of the first semiconductor layer in the first region; the first semiconductor layer and the second semiconductor layer have different electrical properties.

[0125] For example, the first step is polishing and cleaning: First, the semiconductor substrate is polished and cleaned. The semiconductor substrate can be an N-type silicon wafer with a resistivity of 0.5-30 Ω·cm, a thickness of 50-260 μm, and doped with P (phosphorus) or other group VA elements. The polishing process can use a mixture of 0.4-2.2 wt% KOH (potassium hydroxide) or NaOH (sodium hydroxide) and 0.7-2.0 wt% polishing additives, at a temperature of 60-85℃ for 4-10 minutes, using a standard or optimized standard cleaning process. Finally, the oxide layer is removed using 3-10 wt% HF (hydrofluoric acid) to obtain a polished semiconductor substrate.

[0126] Step 2: A tunneling silicon oxide layer (i.e., the first passivation layer) and an intrinsic polysilicon layer are deposited on the semiconductor substrate surface using low-pressure chemical vapor deposition (LPCVD). An N-type doped polysilicon layer is then formed using thermal diffusion. The thickness of the tunneling silicon oxide layer is 1-2 nm, and the thickness of the N-type doped polysilicon layer is 50-200 nm. (Refer to...) Figure 9 At the same time, a phosphosilicate glass layer 15 will form on the surface.

[0127] Step 3: Refer to Figure 9 A mask layer 16 is deposited on the back of the battery using one or a combination of PECVD, LPCVD, ALD, Cat-CVD, etc. The mask layer 16 is one or a combination of silicon nitride, silicon oxide, silicon oxynitride, etc., with a thickness of 10-150nm. Step 4: Refer to Figure 9 Using one of green nanosecond / picosecond or ultraviolet nanosecond / picosecond lasers, the mask layer 16 is ablated, roughly corresponding to the aforementioned first slope sub-region, first platform sub-region, second slope region, and third region, while removing the mask coating around the light-facing surface or the second surface.

[0128] Step 5: Texturing and cleaning the light-facing or second-facing surface of the semiconductor substrate and the laser-aperture area to form a textured surface structure.

[0129] To remove laser-induced damage, a polishing and cleaning process is first performed using soda ash, with a soda ash concentration of 0.1%-3% and a temperature of 50-80℃. Next, a soda ash / hydrogen peroxide system, such as a KOH-H2O2-H2O system, is used, employing a stock solution with a concentration of 45% KOH and 31% H2O2, in a volume ratio of 1:4:5. Cleaning is carried out at 65℃ for 180 seconds. Then, surface texturing is performed on the light-facing surface, the third region, and part of the second region of the semiconductor substrate using an additive 1:KOH:DIW system. The additive 1 concentration is 0.2-1.5%, the KOH concentration is 1-3%, and the temperature is 75-85℃. Preferably, the additive 1 concentration is 0.5-1%, and the KOH concentration is 1.5-2%. Additive 1 mainly comprises a nucleation promoter at a mass concentration of 3-8 wt%, a surfactant at a mass concentration of 2-10 wt%, an antifoamer at a mass concentration of 0.1-1 wt%, and a corrosion inhibitor at a mass concentration of 0.1-0.3 wt%. The nucleation promoter is a high molecular weight compound, such as one or more of polyvinylpyrrolidone (PVP, K value 30-90), polyethylene glycol (PEG, molecular weight 200-2000), hydroxyethyl cellulose (HEC), or polyacrylamide (PAM), providing numerous microscopic nucleation sites. The surfactant is a compound surfactant comprising non-ionic / anionic / amphoionic surfactants, such as nonionic isomeric tridecyl alcohol polyoxyethylene ether, fatty alcohol polyoxyethylene ether (AEO-7 / 9), and alkyl glycosides (AP). G), anionic sodium dodecyl sulfate (SDS), sodium dodecylbenzene sulfonate (LAS), and zwitterionic cocamidopropyl betaine (CAB) are used to balance wetting, defoaming, and easy cleaning properties; the defoamer is a polyether-modified silicone (such as polysiloxane-polyether copolymer) or a non-silicone polyether defoamer, which quickly breaks the gas foam generated by the reaction and prevents "bubble spot" defects; a trace amount of corrosion inhibitor such as benzotriazole (BTA) is used to regulate the corrosion rate of silicon and improve the crystal integrity of the pyramid. The key to forming the aforementioned microstructure is to perform détexturation on the light-facing surface, the third region, and part of the second region of the semiconductor substrate. This is mainly achieved by using additive 2: KOH: DIW system. According to the mass concentration, additive 2 mainly contains 0.1% to 0.5% main masking / dispersant, 0.01% to 0.1% textured catalyst, 0.005% to 0.02% defoamer, 0.01% to 0.5% microstructure modifier, and 0.05% to 0.2% reaction regulator.The primary masking / dispersant is sodium methylene bis(naphthalene) sulfonate (NNO), which can uniformly adsorb onto the semiconductor substrate surface, reducing the solid-liquid interfacial tension and allowing subsequent catalysts and modifiers to spread uniformly, inducing uniform etching initiation at the nanoscale. The texturing catalyst is a nitrogen-containing heterocyclic compound (such as pyridine, piperazine, imidazole derivatives, or quaternary ammonium bases). These organic bases can selectively adsorb onto high-energy sites (such as micro-protrusions and atomic steps) on the semiconductor substrate surface, catalyzing local etching rates. The defoaming agent is the same as additive 1. The microstructure modifier uses one or more of sodium silicate, polyvinylpyrrolidone (PVP), or low molecular weight polyethylene glycol (PEG-400 / 600), which is used to adsorb onto specific crystal faces, slowing down the etching rate of those crystal faces, thereby modifying the pyramid to ultimately form a two-textured morphology. The reaction regulator is disodium ethylenediaminetetraacetate (EDTA-2Na). Triethanolamine (TEA) is used to complex metallic impurities on the silicon wafer surface and in the solution, preventing their deposition on the semiconductor substrate surface and causing localized etching abnormalities (such as black spots or discoloration), while stabilizing the etching rate. In the additive 2:KOH:DIW system, the mass concentration of KOH is 0.5-3wt%, the temperature is 60-80℃, and the time is 30-200s. Preferably, the volume concentration of additive 2 is 0.5vol%-1.2vol%, the mass concentration of KOH is 1-2wt%, and the time is 60-120s. Diffusion modification of the light-facing surface, third region, and part of the second region of the semiconductor substrate mainly utilizes the natural crystal plane and energy difference existing in the "top-waist-bottom" of the original pyramid structure. The additive molecules, with their polar groups, preferentially adsorb on the active sites with higher surface energy, such as the bottom trenches and pyramid junctions, which correspond to the aforementioned second sub-sides. The adsorbed long chains or aggregates self-assemble into a dense, hydrophobic monolayer or micelle film at the bottom trenches. This dynamic molecular mask effectively isolates the etchant from contact with the underlying silicon atoms, protecting the second sub-side from etching during the subsequent secondary texturing process. However, the primary crystal plane of the first sub-side, due to its low surface energy and few active sites, has weak adsorption of additive molecules and cannot form an effective protective layer. This leaves the first sub-side exposed during the secondary texturing, allowing it to be selectively etched to form the aforementioned microstructure. Next, a cleaning process using KOH, H₂O₂, and H₂O is performed at 65°C for 180 seconds. The KOH-H₂O₂-H₂O mixture is prepared by first adding deionized water to a stock solution of approximately 45% KOH and 31% H₂O₂ at a volume ratio of 1:4:5. Then, a 5%-10% wt hydrofluoric acid solution is used for 200-600 seconds to remove the mask layer from the backlight surface. The waist mentioned in this application refers to the position located between the top and bottom of the pyramid structure in the thickness direction Z of the back contact solar cell.

[0130] Step 6: Fabricate a front passivation antireflection layer on the light-facing side using LPCVD / PECVD. The fabrication method includes one or a combination of PECVD, LPCVD, ALD, and Cat-CVD. The thickness of the stacked passivation antireflection film is 1-200 nm. The stacked passivation antireflection film can be a combination of intrinsic hydrogenated amorphous silicon, silicon oxide, aluminum oxide, silicon nitride, and hydrogenated silicon oxynitride.

[0131] Step 7: Remove the wrap-around plating. Use a chain wet process to remove the passivation and anti-reflection layer wrap-around plating on the front side while simultaneously modifying the edge morphology.

[0132] First, the material passes through a decoupling tank to remove the film layer deposited on the back of the solar cell during the front passivation and antireflection layer deposition. The decoupling solution used has a mass concentration of 5-20% and includes, but is not limited to, HF and NH4F solutions. After water washing and spraying, the material enters an edge modification tank. The solution used is additive 3, which mainly includes 0.05-1wt% of inhibitor / mask agent, 0.01-2wt% of wetting agent / activator, and 0.001-0.05wt% of defoamer. The inhibitors / masks are thiols with long alkyl chains, nitrogen-containing heterocyclic compounds (such as benzotriazole BTA derivatives), polyethylene glycol (PEG) or polyvinylpyrrolidone (PVP) with specific molecular weights. They utilize polar groups (-SH, -NH, C=O) to form strong adsorption with high-energy silicon atoms in the trenches, and the long chains or cyclic structures form steric hindrance and hydrophobic films. The wetting agents / activators are fluorocarbon or organosilicon superspreading surfactants and ethoxylated acetylsyl alcohols. Their main function is to reduce the surface tension of the solution, carry the masking agent molecules and spread them to the bottom of the deep and narrow trenches of the pyramid-like structure, and at the same time help to remove hydrogen bubbles generated by the reaction. The defoamers are cyclodextrin, hydroxyethyl cellulose, hydroxypropyl methyl cellulose or polyoxyethylene polyoxypropylene ether block copolymers. They quickly break up bubbles. If bubbles remain in the pyramid trenches, they will physically block the contact between the masking agent and the silicon surface, destroying the uniformity of the functional zones. The main function of additive 3 is to protect the bottom of the pyramid-like structure in the third region from etching, while sharpening the top of the pyramid-like structure in the third region to form a platform-like frustum structure. Simultaneously, the first sub-platform region is formed in this seventh step. Finally, a cleaner surface is obtained through cleaning in the SC1 tank. The SC1 tank has an effective length of 0.8-4m and contains cleaning solutions including alkali, oxidant, and additives. The mass ratio of alkali to oxidant in the alkaline solution is between 1:1 and 1:5. Additives can include surfactants, chelating agents, etc. Following the SC1 tank is a 2%-10% HF solution to remove the oxide layer on the back side and enhance the hydrophobic effect for rapid drying. Edge finishing and cleaning tanks can also be performed using tank-type equipment.

[0133] Step 8: Sequentially deposit the second passivation layer 6 and the P-type amorphous silicon layer using PECVD. The thickness of the intrinsic amorphous silicon layer is 1-50 nm; the thickness of the P-type amorphous silicon layer is 3-50 nm. The total thickness of the intrinsic amorphous silicon layer and the P-type amorphous silicon layer is 40 nm to 80 nm.

[0134] Step 9: Laser film opening. Using one of the following lasers, namely green nanosecond, green picosecond, ultraviolet nano, or ultraviolet picosecond, the second passivation layer 6 and the P-type amorphous silicon layer are vaporized and ablated to remove part of the second passivation layer 6 and the P-type amorphous silicon layer above the first region.

[0135] Step 10: Laser crystallization. Use one of the following lasers: green nanosecond, green picosecond, ultraviolet nano, or ultraviolet picosecond to laser crystallize the P-type amorphous silicon layer in the third region.

[0136] Step 11: Deposit a transparent conductive layer 4 on the backlight surface using PVD, with a film thickness of 10-500nm. Further, it can be 50nm-200nm. The transparent conductive layer 4 can be one of ITO (indium tin oxide), IWO (tungsten tin oxide), ITiO (titanium tin oxide), ICO (cerium tin oxide), or a stack thereof.

[0137] Step 12: Use laser to clean the transparent conductive layer 4 or use etching paste to form an opening, and insulate the transparent conductive layer 4 in the first and third regions to prevent leakage.

[0138] Step 13 Metallization: Print conductive paste on the first and third regions covering the transparent conductive layer 4, and cure to form the first electrode structure and the second electrode structure. There are no specific restrictions on the preparation method of the first electrode structure and the second electrode structure.

[0139] The structure of the back-contact solar cell formed in the above example can be referred to Figure 1 As shown, the system includes: a semiconductor substrate 1, which may be an N-type silicon substrate; a first region 12, a second region 13, and a third region 14 arranged along a first direction on the back surface of the silicon substrate; the second region 13 being disposed between the first region 12 and the third region 14; and the first region 12, the second region 13, and the third region 14 extending along a second direction. A first semiconductor layer is disposed in the first region, and the first semiconductor layer includes an N-type doped polycrystalline silicon layer. A tunneling silicon oxide layer (first passivation layer 5) is also present between the N-type doped polycrystalline silicon layer and the silicon substrate. A second semiconductor layer includes a P-type doped silicon layer 3. An intrinsic amorphous layer (second passivation layer 6) is also present between the P-type doped silicon layer 3 and the silicon substrate. The second semiconductor layer is disposed in the second and third regions and extends to cover a portion of the first semiconductor layer in the first region. (Refer to...) Figure 7The third region has a frustum-like structure, and the light-facing surface has a pyramid-like or pyramid-like structure. Both the frustum-like structure in the third region and the pyramid-like or pyramid-like structure on the light-facing surface include at least two lateral edges. The sides of the frustum-like and pyramid-like structures are called second lateral edges. Each lateral edge has a top and a bottom. The top of the second lateral edge has a microstructure. The area of ​​the second lateral edge with the microstructure is the first sub-lateral edge, and the remaining area is the second sub-lateral edge. Each lateral edge includes a first segment containing the top and a second segment facing away from the top; or, in other words, the position of the lateral edge corresponding to the first sub-lateral edge is the first segment; the remaining position is the second segment. A first transparent conductive layer 41 is located on the side of the first semiconductor layer away from the semiconductor substrate. A second transparent conductive layer 42 extends from the third region at least partially through the second region to cover the second semiconductor layer in the first region. The first transparent conductive layer 41 and the second transparent conductive layer are disconnected at least at the point where the first semiconductor layer and the second semiconductor layer overlap. A first electrode structure is located on the side of the first transparent conductive layer away from the semiconductor substrate and corresponds to the position of the first semiconductor layer. A second electrode structure is located on the side of the second transparent conductive layer away from the semiconductor substrate and corresponds to the position of the second semiconductor layer.

[0140] In some embodiments, the formation process of the first platform sub-region is mainly based on the characteristic that the etching rate of the first semiconductor layer is faster than that of the semiconductor substrate. The N-type doped polysilicon layer in the first semiconductor layer has a large doping concentration and a large thickness. The N-type doped polysilicon layer has a large doping concentration and is easy to be etched, thus etching away the first semiconductor layer on the first platform sub-region, and thus exposing the first sub-platform region.

[0141] In some embodiments, before removing the portion of the first semiconductor layer located in the first platform sub-region, the thickness of the entire first semiconductor layer is 40 nm to 250 nm. This relatively large thickness provides processing allowance for forming the frustum-like structure and the microstructure, resulting in a suitable thickness for the formed product. For example, the thickness of the entire first semiconductor layer can be 40 nm, 50 nm, 60 nm, 80 nm, 90 nm, 100 nm, 120 nm, 150 nm, 190 nm, 200 nm, 220 nm, or 250 nm.

[0142] This application also provides a photovoltaic module comprising multiple series-connected and / or parallel-connected cell strings, each cell string including: an electrical connector and any of the aforementioned back-contact solar cells. The electrical connector electrically connects at least two of the aforementioned back-contact solar cells. The electrical connector mentioned in this application may be a solder ribbon, a conductive electrical connector, etc. The photovoltaic module may further include: an encapsulation layer covering the surface of the cell strings, the encapsulation layer may include an encapsulating film, etc., and a cover plate covering the surface of the encapsulation layer away from the cell strings. The electrical connector here may refer to a solder ribbon, a conductive backplate, etc., without specific limitation. The cover plate may be glass, etc., without limitation on the specific material.

[0143] For example, in a battery string, an electrical connector electrically connects the first electrode structure of one of two adjacent back-contact solar cells to the second electrode structure of the other solar cell.

[0144] It should be noted that the back-contact solar cell, the preparation method of the back-contact solar cell, and the photovoltaic module provided in this application can be referred to each other. To avoid repetition, the relevant parts will not be described again.

[0145] It should be noted that the various embodiments provided in this application may exist independently or in combination without contradiction, and all are within the protection scope of this application.

[0146] The terms "first" and "second" in the specification and claims of this application may explicitly or implicitly include one or more of the features. In the description of this application, unless otherwise stated, "multiple" means two or more. Furthermore, "and / or" in the specification and claims indicates at least one of the connected objects, and the character " / " generally indicates that the preceding and following objects are in an "or" relationship.

[0147] In the description of this application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "upper", "lower", "front", "rear", "left", "right", "vertical", "horizontal", "top", "bottom", "inner", "outer", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc., indicating the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this application.

[0148] In the description of this application, it should be noted that, unless otherwise expressly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal connection between two components. Those skilled in the art can understand the specific meaning of the above terms in this application based on the specific circumstances.

[0149] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "illustrative embodiment," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of this application. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.

[0150] Although embodiments of this application have been shown and described, those skilled in the art will understand that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of this application, the scope of which is defined by the claims and their equivalents.

Claims

1. A back-contact solar cell, characterized in that, include: A semiconductor substrate includes a first surface and a second surface opposite to each other; the first surface includes a first region, a second region and a third region arranged along a first direction, the second region being located between the first region and the third region; the surface of the third region is recessed toward the semiconductor substrate relative to the surface of the first region, and the surface of the second region is a transition sidewall of the semiconductor substrate from the first region to the third region; A first semiconductor layer is disposed in the first region; A second semiconductor layer is disposed in the third region and the second region, and extends to cover a portion of the first semiconductor layer in the first region; the first semiconductor layer and the second semiconductor layer have different electrical properties. And a second transparent conductive layer, disposed on the second semiconductor layer in the third region; The second region includes: a first platform sub-region, a first slope sub-region, a second platform sub-region, and a second slope sub-region distributed along the first direction; The first platform sub-region is close to the first region, and the second ramp sub-region is close to the third region; In the thickness direction of the back contact solar cell, the first platform sub-region, the first slope sub-region, the second platform sub-region, and the second slope sub-region of the first surface are sequentially close to the second surface; The second transparent conductive layer extends at least partially from the third region through the second region to cover the second semiconductor layer of the first region.

2. The back-contact solar cell according to claim 1, characterized in that, Along the first direction, the width of the first platform sub-region is W1, the width of the second platform sub-region is W2, the width of the first ramp sub-region is W3, and the width of the second ramp sub-region is W4; W1 < W2; and / or, W1 < W3 < W2 < W4; and / or, W2 / W1 is 10 to 300; and / or, W3 / W1 is 6 to 150; and / or, W4 / W3 is 1.2 to 500; and / or, W4 / W2 is 1.1 to 300; and / or, W1 is 2nm to 10nm, and / or W2 is 100nm to 600nm, and / or W3 is 60nm to 300nm, and / or W4 is 0.5μm to 3μm.

3. The back-contact solar cell according to claim 1, characterized in that, In the thickness direction of the back-contact solar cell, the height of the first ramp sub-region is H1, the height of the second ramp sub-region is H2, H2 > H1, and H1 is 100 nm to 300 nm; and / or, H2 / H1 is 5 to 800; and / or, the difference between H2 and H1 is 6 μm to 8 μm; and / or, H2 is 2 μm to 8 μm.

4. The back-contact solar cell according to claim 1, characterized in that, Along the thickness direction of the semiconductor substrate, the angle between the first platform sub-region and the first ramp sub-region is α; along the thickness direction of the semiconductor substrate, the angle between the second platform sub-region and the second ramp sub-region is β, where α and β are different and both are obtuse angles; preferably, α ≥ β.

5. The back-contact solar cell according to claim 1, characterized in that, In the thickness direction of the semiconductor substrate, the side surface of the first semiconductor layer is the first side surface; Relative to the first platform sub-region, at least a portion of the first side is inclined; and / or, Relative to the first platform sub-region, at least a portion of the first side is perpendicularly disposed; and / or, At least a portion of the first side has a recessed structure that is recessed into the first semiconductor layer.

6. The back-contact solar cell according to claim 1, characterized in that, The degree of undulation of the portion of the second semiconductor layer located on the first platform sub-region is less than the degree of undulation of the portion of the first semiconductor layer located away from the first surface; And / or, The degree of undulation of the portion of the second semiconductor layer located on the second platform sub-region is less than the degree of undulation of the portion of the first semiconductor layer located away from the first surface.

7. The back-contact solar cell according to claim 1, characterized in that, Both the first platform sub-region and the second platform sub-region are planar.

8. The back-contact solar cell according to claim 1, characterized in that, The third region includes a frustum-like structure; the second face includes a pyramid-like structure.

9. The back-contact solar cell according to claim 8, characterized in that, Both the frustum-like structure and the pyramid-like structure include at least two side edges; in the semiconductor substrate thickness direction, the side edges of the frustum-like structure and the pyramid-like structure are second side edges; each side edge has a top and a bottom, with the bottom edge being closer to the semiconductor substrate than the top edge. The top of the second side has microstructures; The area with microstructures on the second side is the first sub-side surface, and the remaining area is the second sub-side surface; the position of the side edge corresponding to the first sub-side surface is the first segment. The remaining space is the second paragraph; In the same side edge of the same frustum-like structure: along the direction from the top to the bottom, the length of the first segment accounts for less than or equal to 90% of the length of the side edge; and / or, In the same side edge of the same pyramid-like structure: along the direction from the top to the bottom, the length of the first segment accounts for less than or equal to 90% of the length of the side edge.

10. The back-contact solar cell according to claim 9, characterized in that, In the same side edge of the same pyramidal structure: along the direction from the top to the bottom, the length of the first segment as a percentage of the length of the side edge is less than the length of the first segment as a percentage of the length of the side edge in the same side edge of the same pyramidal structure: along the direction from the top to the bottom.

11. The back-contact solar cell according to claim 9, characterized in that, The truncated pyramid-like microstructure has the same or similar morphology to the pyramid-like microstructure; and / or, Both the frustum-like microstructure and the pyramid-like microstructure contain folded structures; and / or, Both the pyramid-like microstructure and the pyramid-like microstructure contain a cluster of nested ring structures.

12. The back-contact solar cell according to claim 8, characterized in that, Along the thickness direction of the semiconductor substrate, the height of the truncated pyramid structure is 0.5 μm to 5 μm, and / or the height of the pyramid structure is 0.5 μm to 5 μm.

13. The back-contact solar cell according to claim 1, characterized in that, The second slope region has multiple vertical textures and multiple arc-shaped textures, with the arc-shaped textures superimposed on the vertical textures; the extension direction of the arc-shaped textures is a second direction, and the extension direction of the vertical textures is a first direction; the first direction and the second direction intersect.

14. The back-contact solar cell according to claim 1, characterized in that, The first semiconductor layer is an N-type doped polycrystalline silicon layer; the back contact solar cell further includes a first passivation layer, which is located between the N-type doped polycrystalline silicon layer and the semiconductor substrate; The second semiconductor layer includes a P-type doped silicon layer, wherein the P-type doped silicon layer includes at least one of P-type doped amorphous silicon, P-type doped nanocrystalline silicon, and P-type doped microcrystalline silicon; The thickness of the P-type doped silicon layer is 20 nm to 80 nm. The back-contact solar cell further includes: The first transparent conductive layer is located on the side of the first semiconductor layer away from the semiconductor substrate, and the first transparent conductive layer and the second transparent conductive layer are disconnected at least at the overlapping position of the first semiconductor layer and the second semiconductor layer; The first electrode structure is located on the side of the first transparent conductive layer away from the semiconductor substrate; The second electrode structure is located on the side of the second transparent conductive layer away from the semiconductor substrate.

15. A photovoltaic module, characterized in that, include: Multiple battery strings connected in series and / or in parallel, the battery strings comprising: electrical connectors and back-contact solar cells according to any one of claims 1 to 14, the electrical connectors being electrically connected to the electrode structures of at least two of the back-contact solar cells; An encapsulation layer is used to cover the surface of the battery string; A cover plate is used to cover the surface of the encapsulation layer away from the battery string.