Back contact cell and method of making same, stacked cell, photovoltaic module

By setting a three-dimensional structured second transparent conductive layer on the substrate texture structure of the back contact battery, the contact performance and conductivity of the transparent conductive layer are enhanced, solving the problem of low photoelectric conversion efficiency of existing back contact batteries, and achieving higher photoelectric conversion efficiency and a simplified process flow.

CN123164883APending Publication Date: 2026-11-24SHANGRAO JINKO SOLAR NO 3 INTELLIGENT MANUFACTURING CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611281350.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-21
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing back-contact batteries have problems with the contact performance between the transparent conductive layer and the connecting passivation conductive layer, as well as the integrity of the passivation layer, resulting in poor photoelectric conversion efficiency.

Method used

A second transparent conductive layer is disposed on the first textured structure of the substrate. The surface of the second transparent conductive layer contains second spherical grains with a three-dimensional structure, which fill the depressions of the textured structure, increase the contact performance, and improve the conductivity and lateral transmission capability through the combination of the first transparent conductive layer and the second transparent conductive layer.

Benefits of technology

It improves the photoelectric conversion efficiency of the back contact battery, simplifies the etching process of the transparent conductive layer, and reduces the process difficulty.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123164883A_ABST
    Figure CN123164883A_ABST
Patent Text Reader

Abstract

This application relates to the photovoltaic field, providing a back contact cell and its preparation method and manufacturing apparatus, a tandem cell, and a photovoltaic module, which can at least improve the photoelectric conversion efficiency of the back contact cell. The back contact cell includes: a substrate, the substrate including alternating first and second regions; the surface of the second region includes a first textured structure; a first passivated conductive structure located in the first region; a second passivated conductive structure located in the second region, the second passivated conductive structure covering the first textured structure; a first transparent conductive layer located on the surface of the first passivated conductive structure, the surface of the first transparent conductive layer including a plurality of first spherical grains and first plate-like grains; and a second transparent conductive layer located on the surface of the second passivated conductive structure, the surface of the second transparent conductive layer including second spherical grains.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the photovoltaic field, and particularly to a back contact battery and its preparation method and manufacturing apparatus, a tandem battery, and a photovoltaic module. Background Technology

[0002] Currently, with the gradual depletion of fossil fuels, solar cells are becoming increasingly widely used as a new energy alternative. A solar cell is a device that converts sunlight into electrical energy. Solar cells utilize the photovoltaic principle to generate charge carriers, which are then extracted using electrodes, thus facilitating the efficient utilization of electrical energy.

[0003] Current solar cells mainly include IBC cells (Interdigitated Back Contact), TOPCON (Tunnel Oxide Passivated Contact) cells, PERC cells (Passivated Emitter and Rear Cell), and heterojunction cells. Different film layer configurations and functional limitations are used to reduce optical losses and decrease photogenerated carrier recombination on and within the silicon substrate, thereby improving the photoelectric conversion efficiency of solar cells.

[0004] However, current back-contact batteries have some problems that result in poor photoelectric conversion efficiency, such as the contact performance between the transparent conductive layer and the passivated conductive layer or the integrity of the passivation layer. Summary of the Invention

[0005] This application provides a back contact battery, its preparation method and manufacturing apparatus, a tandem battery, and a photovoltaic module, which at least helps to improve the photoelectric conversion efficiency of the back contact battery.

[0006] According to some embodiments of this application, a first aspect of this application provides a back contact battery, comprising: a substrate, the substrate including alternating first regions and second regions; the substrate surface of the second region including a first textured structure; a first passivated conductive structure located in the first region; a second passivated conductive structure located in the second region, the second passivated conductive structure covering the first textured structure; a first transparent conductive layer located on the surface of the first passivated conductive structure, the surface of the first transparent conductive layer including a plurality of first spherical grains and first plate-like grains; and a second transparent conductive layer located on the surface of the second passivated conductive structure, the surface of the second transparent conductive layer including second spherical grains.

[0007] Optionally, the first size of the first spherical grain is smaller than the second size of the second spherical grain.

[0008] Optionally, the first textured structure includes a top and a tower surface, wherein the size of the second spherical grains of the second transparent conductive layer located at the top is larger than that of the second spherical grains of the second transparent conductive layer located at the tower surface.

[0009] Optionally, the crystallinity of the first transparent conductive layer is greater than that of the second transparent conductive layer.

[0010] Optionally, the first transparent conductive layer includes a first sublayer and a second sublayer, the first sublayer being located between the first passivated conductive structure and the second sublayer, and the distribution density of the first lamellar grains in the first sublayer being less than the distribution density of the first lamellar grains in the second sublayer.

[0011] Optionally, the surface of the second transparent conductive layer further includes a second sheet-like grain, the fourth dimension of which is smaller than the third dimension of the first sheet-like grain.

[0012] Optionally, the first spherical grains and the first plate-shaped grains have a first distribution density, and the second spherical grains and the second plate-shaped grains have a second distribution density, wherein the first distribution density is less than the second distribution density.

[0013] Optionally, the base surface of the first region is a flat surface.

[0014] Optionally, the first thickness of the first transparent conductive layer is greater than the second thickness of the second transparent conductive layer.

[0015] Optionally, the ratio of the second thickness to the first thickness is 0.7 to 0.9.

[0016] Optionally, the distribution density of the first spherical grains and the first plate-shaped grains ranges from 1:1 to 1:3.

[0017] Optionally, the substrate surface of the second region includes a second textured structure, the second passivated conductive structure covers the second textured structure, and the second roughness of the second textured structure is less than the first roughness of the first textured structure.

[0018] Optionally, the substrate includes a first surface and a second surface, the first surface including a first region and a second region, and the distance between the first region and the second surface is greater than the distance between the second region and the second surface.

[0019] Optionally, the surface of the second transparent conductive layer further includes a third spherical grain, the size of which is smaller than the size of the second spherical grain.

[0020] According to some embodiments of this application, a second aspect of this application also provides a method for fabricating a back contact battery, comprising: providing a substrate, the substrate including alternating first regions and second regions; forming an initial passivation conductive layer, the initial passivation conductive layer being located in the first region and the second region; removing the initial passivation conductive layer located in the second region, and forming a first texture structure on the surface of the substrate in the second region, the remaining initial passivation conductive layer being the first passivation conductive structure; forming a second passivation conductive structure, the second passivation conductive structure being located in the second region, the second passivation conductive structure covering the first texture structure; forming a first transparent conductive layer, the first transparent conductive layer being located on the surface of the first passivation conductive structure, the surface of the first transparent conductive layer including a plurality of first spherical grains and first plate-like grains; forming a second transparent conductive layer, the second transparent conductive layer being located on the surface of the second passivation conductive structure, the surface of the second transparent conductive layer including second spherical grains.

[0021] Optionally, the process steps for forming the first transparent conductive layer and the second transparent conductive layer include: forming a first transparent conductive film using first process parameters, wherein the first transparent conductive film is located on the surface of the first passivated conductive structure and the surface of the second passivated conductive structure, the surface of the first transparent conductive film located on the first passivated conductive structure includes first spherical grains, and the surface of the first transparent conductive film located on the second passivated conductive structure includes second spherical grains; forming a second transparent conductive film using second process parameters, wherein the second transparent conductive film is located on a portion of the surface of the first transparent conductive film; the surface of the second transparent conductive film includes first sheet-like particles.

[0022] Optionally, the substrate further includes a third region located between the second region and the third region; the process steps for forming the first transparent conductive layer and the second transparent conductive layer include: forming a transparent conductive film located in the first region, the second region, and the third region; wherein the surface of the transparent conductive film deposited in the second region includes second spherical grains, and the surface of the transparent conductive film deposited in the first region and the third region includes a plurality of first spherical grains and first plate-like grains; removing the transparent conductive film in the third region, retaining the transparent conductive film located in the first region as the first transparent conductive layer, and the transparent conductive film located in the second region as the second transparent conductive layer.

[0023] According to some embodiments of this application, a third aspect of this application also provides a stacked battery, comprising: a crystalline silicon bottom battery, wherein the crystalline silicon bottom battery is a back contact battery as described in any one of the above embodiments or a back contact battery prepared by any one of the above embodiments; and a perovskite top battery, wherein the perovskite top battery is located on one side of the crystalline silicon bottom battery.

[0024] According to some embodiments of this application, a fourth aspect of this application also provides a photovoltaic module, comprising: a battery string, formed by connecting a plurality of back-contact batteries as described in any one of the above embodiments, back-contact batteries prepared by any one of the above embodiments, or stacked batteries as described in the above embodiments; an encapsulation layer for covering the surface of the battery string; and a cover plate for covering the surface of the encapsulation layer opposite to the battery string.

[0025] According to some embodiments of this application, a fifth aspect of this application also provides a manufacturing apparatus for a back contact battery, comprising: an acquisition module for acquiring a substrate, the substrate including alternating first regions and second regions; a first manufacturing module for forming a first textured structure on the surface of the substrate in the second region; a second manufacturing module for forming a first passivated conductive structure on the first region, forming a second passivated conductive structure on the second region, forming a first transparent conductive layer on the surface of the first passivated conductive structure, and forming a second transparent conductive layer on the surface of the second passivated conductive structure; the second passivated conductive structure covering the first textured structure; the surface of the first transparent conductive layer including a plurality of first spherical grains and first plate-like grains; and the surface of the second transparent conductive layer including second spherical grains.

[0026] The technical solution provided in this application has at least the following advantages: In the back contact battery provided in this application embodiment, a second transparent conductive layer containing second spherical grains is disposed on a first textured structure. First, the second spherical grains are three-dimensional structures with relatively small grain sizes, allowing them to fill the depressions in the first textured structure and increase contact performance. Second, the second spherical grains are three-dimensionally grown, resulting in a thicker second transparent conductive layer covering the first textured structure, allowing for more complete coverage of the textured film layer and thus improving lateral transport capability. Third, the second spherical grains have good conductivity, which improves the conductivity of the transparent conductive layer. The etching performance of the first transparent conductive layer containing the first sheet-like grains is greater than that of the second transparent conductive layer containing the second spherical grains. Therefore, the process of forming both the first and second transparent conductive layers by etching a portion of the transparent conductive layer is simpler and reduces process difficulty. Attached Figure Description

[0027] One or more embodiments are illustrated by way of example with reference to the accompanying drawings. These illustrations do not constitute a limitation on the embodiments. Unless otherwise stated, the drawings in the accompanying drawings do not constitute a limitation on scale. In order to more clearly illustrate the technical solutions in the embodiments of this application or in the conventional art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0028] Figure 1 A schematic diagram of a back contact battery provided in an embodiment of this application; Figure 2 A scanning electron microscope image of the first transparent conductive layer in a back contact battery provided in an embodiment of this application; Figure 3 Another scanning electron microscope image of the first transparent conductive layer in a back contact battery provided in an embodiment of this application; Figure 4 A scanning electron microscope image of the second transparent conductive layer in a back contact battery provided in an embodiment of this application; Figure 5 A schematic diagram of a structure of the first transparent conductive layer in a back contact battery provided in an embodiment of this application; Figure 6 This is a schematic diagram of another structure of a back contact battery provided in an embodiment of this application; Figures 7-15 This is a schematic diagram of the structure of a back contact battery corresponding to each step in the preparation method of a back contact battery provided in another embodiment of this application; Figure 16 A schematic diagram of a stacked battery provided in yet another embodiment of this application; Figure 17 This is a schematic diagram of a photovoltaic module provided in another embodiment of this application. Detailed Implementation

[0029] As can be seen from the background technology, there is potential to further improve the photoelectric conversion efficiency of current back-contact batteries.

[0030] This application provides a back contact battery. The surface of a second transparent conductive layer deposited on a first textured structure contains second spherical grains, and the surface of a first transparent conductive layer contains first spherical grains and first sheet-like grains. In this way, the first textured structure can be filled based on the three-dimensional structure of the second spherical grains, which increases the contact performance between the second transparent conductive layer and the second passivated conductive structure, thereby improving the photoelectric conversion efficiency of the back contact battery.

[0031] In the description of the embodiments of this application, technical terms such as "first" and "second" are used only to distinguish different objects and should not be construed as indicating or implying relative importance or implicitly specifying the number, specific order, or primary and secondary relationship of the indicated technical features. In the description of the embodiments of this application, "multiple" means two or more, unless otherwise explicitly defined.

[0032] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.

[0033] In the description of the embodiments in this application, the term "and / or" is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent three cases: A exists, A and B exist simultaneously, and B exists. In addition, the character " / " in this document generally indicates that the related objects before and after it have an "or" relationship.

[0034] In the description of the embodiments of this application, the term "multiple" refers to two or more (including two), similarly, "multiple sets" refers to two or more (including two sets), and "multiple pieces" refers to two or more (including two pieces).

[0035] In the description of the embodiments of this application, the technical terms "center," "longitudinal," "lateral," "length," "width," "thickness," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," "outer," "clockwise," "counterclockwise," "axial," "radial," and "circumferential" indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing the embodiments of this application and simplifying the description, and are not intended to indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on the embodiments of this application.

[0036] In the description of the embodiments of this application, unless otherwise expressly specified and limited, the technical terms such as "installation," "connection," "joining," and "fixing" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral part; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; they can refer to the internal communication of two components or the interaction between two components. For those skilled in the art, the specific meaning of the above terms in the embodiments of this application can be understood according to the specific circumstances.

[0037] In the description of the embodiments of this application, electrical connection between one component and another means that both components are made of conductive materials, and the two components are in direct contact and connected or indirectly connected via other conductive materials. Therefore, when the photovoltaic module or cell is generating electricity, current flows between the two components. Electrical contact between one component and another means that both components are made of conductive materials, and current flows between the two components when the photovoltaic module or cell is generating electricity.

[0038] In the accompanying drawings corresponding to the embodiments of this application, the thickness and / or area of ​​layers, films, panels, regions, etc., are enlarged for better understanding and ease of description. Throughout the specification, the same reference numerals denote the same elements. It should be understood that when describing a component (such as a layer, film, region, or substrate) on or on the surface of another component, the component may be "directly" located on the surface of the other component, or there may be an intermediate component between the two components. Conversely, when describing a component on the surface of another component, or a component "directly" on another component, or a component having another component formed or disposed on its surface, it indicates that there is no intermediate component between the two components. Furthermore, when describing a component as "generally" formed on another component, the component is not formed on the entire surface of the other component due to manufacturing tolerances or errors.

[0039] In the description of the embodiments of this application, when a component "includes" another component, other components are not excluded unless otherwise stated, and other components may be further included. Furthermore, when a component such as a layer, film, region, or plate is referred to as being "on / located" on another component, it can be "directly on" the other component (i.e., located on the surface of the other component with no other components between them), or another component may be present therein. Moreover, when a component such as a layer, film, region, or plate is "directly located" on another component, or when a component such as a layer, film, region, or plate is located on the surface of another component, it indicates that no other components are located therein.

[0040] The embodiments of this application will now be described in detail with reference to the accompanying drawings. However, those skilled in the art will understand that many technical details have been provided in the embodiments of this application to facilitate a better understanding of the application. However, the technical solutions claimed in this application can be implemented even without these technical details and various variations and modifications based on the following embodiments.

[0041] According to some embodiments of this application, one aspect of this application provides a back contact battery for improving the photoelectric conversion efficiency of the back contact battery.

[0042] Figure 1A schematic diagram of a back contact battery provided in an embodiment of this application; Figure 2 A scanning electron microscope image of the first transparent conductive layer in a back contact battery provided in an embodiment of this application; Figure 3 Another scanning electron microscope image of the first transparent conductive layer in a back contact battery provided in an embodiment of this application; Figure 4 A scanning electron microscope image of the second transparent conductive layer in a back contact battery provided in an embodiment of this application; Figure 5 A schematic diagram of a structure of the first transparent conductive layer in a back contact battery provided in an embodiment of this application; Figure 6 This is a schematic diagram of another structure of a back contact battery provided in an embodiment of this application.

[0043] It should be noted that, Figure 1 The back contact battery shown is a partial cross-sectional view. The actual back contact battery includes multiple first regions, second regions, and a first electrode located on the first region and a second electrode located on the second region. The arrangement of the first region and the second region can be the arrangement of the P region and N region in the current back contact battery. For example, the P region and the N region are arranged alternately along the first direction X, or the top view of the P region is comb-shaped, the top view of the N region is comb-shaped, and the teeth in the comb shape of the P region and the teeth in the comb shape of the N region are overlapped along the second direction, which is perpendicular to the first direction X and perpendicular to the vertical direction Z.

[0044] refer to Figures 1-4 The back contact battery includes: a substrate 100, which includes alternating first regions 11 and second regions 12. The back contact battery includes: a first textured structure 13 on the surface of the substrate 100 in the second region 12. The back contact battery includes: a first passivated conductive structure 110 located in the first region 11. The back contact battery includes: a second passivated conductive structure 120 located in the second region 12, which covers the first textured structure 13. The back contact battery includes: a first transparent conductive layer 113 located on the surface of the first passivated conductive structure 110, the surface of which includes a plurality of first spherical grains 1131 and first plate-like grains 1132. The back contact battery includes: a second transparent conductive layer 123 located on the surface of the second passivated conductive structure 120, the surface of which includes second spherical grains 1231.

[0045] In the back contact battery provided in this application embodiment, a second transparent conductive layer 123 containing second spherical grains 1231 is disposed on the first textured structure 13. First, the second spherical grains 1231 are three-dimensional structures with relatively small grain sizes, which can fill the depressions in the first textured structure 13, increasing contact performance. Second, the second spherical grains 1231 are three-dimensionally grown, resulting in a thicker second transparent conductive layer 123 covering the first textured structure 13, allowing for more complete coverage of the textured structure's film layer, thereby improving lateral transport capability. Third, the second spherical grains 1231 have good conductivity, which can improve the conductivity of the transparent conductive layer. The etching performance of the first transparent conductive layer 113 containing first sheet-like grains 1132 is greater than that of the second transparent conductive layer 123 containing second spherical grains 1231. Therefore, the process of forming the first transparent conductive layer 113 and the second transparent conductive layer 123 by etching a portion of the transparent conductive layer is simpler, reducing process difficulty.

[0046] The back contact battery provided in the above embodiments will be described in detail below with reference to the accompanying drawings.

[0047] In some embodiments, the first passivated conductive structure 110 includes a first interface passivation layer 111 and a first doped conductive layer 112. The first interface passivation layer 111 is located on the surface of the substrate 100, and the first transparent conductive layer 113 is located on the surface of the first doped conductive layer 112 away from the first interface passivation layer 111. The second passivated conductive structure 120 includes a second interface passivation layer 121 and a second doped conductive layer 122. The second interface passivation layer 121 is located on the surface of the substrate 100, and the second transparent conductive layer 123 is located on the surface of the second doped conductive layer 122 away from the second interface passivation layer 121.

[0048] In some examples, the back contact cell can be an HBC cell (Heterojunction Back Contact Cell), the first passivation conductive structure 110 is a heterojunction structure, and the second passivation conductive structure 120 is a heterojunction structure. The materials of the first interface passivation layer 111 and the second interface passivation layer 121 can include at least one of amorphous silicon, microcrystalline silicon, or nanocrystalline silicon.

[0049] In some examples, the back contact cell can be a TBC cell (TOPCon Back Contact Cell, tunneled oxide passivated back contact cell), with the first passivation conductive structure 110 being a passivation contact structure and the second passivation conductive structure 120 being a passivation contact structure. The materials of the first interface passivation layer 111 and the second interface passivation layer 121 can both include at least one of silicon oxide, aluminum oxide, silicon nitride, silicon oxynitride, titanium oxide, hafnium oxide, zirconium oxide, or silicon carbide.

[0050] In some examples, the back contact cell can be an HTBC cell (Heterojunction Tunnel Oxide Passivated Back Contact Cell), where one of the first passivation conductive structure 110 and the second passivation conductive structure 120 is a passivation contact structure, and the other of the first passivation conductive structure 110 and the second passivation conductive structure 120 is a heterojunction structure. The material of one of the first interface passivation layer 111 and the second interface passivation layer 121 can include at least one of amorphous silicon, microcrystalline silicon, or nanocrystalline silicon, and the material of the other of the first interface passivation layer 111 and the second interface passivation layer 121 can include at least one of silicon oxide, aluminum oxide, silicon nitride, silicon oxynitride, titanium oxide, hafnium oxide, zirconium oxide, or silicon carbide.

[0051] The substrate 100 is used to receive light and generate photogenerated carriers. In some embodiments, the substrate 100 may be a semiconductor substrate.

[0052] In some embodiments, the material of the substrate 100 may be an elemental semiconductor material. Specifically, the elemental semiconductor material is composed of a single element, such as silicon or germanium. The elemental semiconductor material may be monocrystalline, polycrystalline, amorphous, or microcrystalline (a state simultaneously possessing both monocrystalline and amorphous states is called microcrystalline). For example, silicon may be at least one of monocrystalline silicon, polycrystalline silicon, amorphous silicon, and microcrystalline silicon.

[0053] In some embodiments, the substrate 100 may also be a compound semiconductor material. Common compound semiconductor materials include, but are not limited to, silicon germanide, silicon carbide, gallium arsenide, indium gallium arsenide, perovskite, cadmium telluride, copper indium selenide, etc.

[0054] The substrate 100 can also be a sapphire substrate, a silicon substrate on an insulator, or a germanium substrate on an insulator.

[0055] The substrate 100 can be an N-type semiconductor substrate or a P-type semiconductor substrate. The N-type semiconductor substrate is doped with an N-type dopant element, which can be at least one of group V elements such as phosphorus (P), bismuth (Bi), antimony (Sb), or arsenic (As). The P-type semiconductor substrate is doped with a P-type dopant element, which can be at least one of group III elements such as boron (B), aluminum (Al), gallium (Ga), or indium (In).

[0056] The substrate 100 has a first surface 102 and a second surface 101 facing each other.

[0057] In some embodiments, the cells used in a single-glass photovoltaic module are considered single-sided cells, and the second side 101 can serve as a light-receiving surface for receiving sunlight, while the first side 102 serves as a backlighting surface. In some embodiments, the cells used in a double-glass module or a bifacial module are considered bifacial cells, and both the first side 102 and the second side 101 can serve as light-receiving surfaces and can be used to receive sunlight. It is understood that the backlighting surface referred to in the embodiments of this application can also receive sunlight, but the degree of sunlight reception is weaker than that of the light-receiving surface, and therefore it is defined as a backlighting surface.

[0058] In some embodiments, the back-contact solar cell is a high bifaciality cell, meaning that both the front and back sides of the substrate 100 can serve as light-receiving surfaces and can be used to receive incident light.

[0059] It should be noted that, Figure 1 And the following Figure 6 The side facing the top is the illuminated side, and the side facing the bottom is the shaded side. Taking the first side as the illuminated side and the second side as the shaded side as an example.

[0060] The second surface 101 of the substrate 100 has a textured surface (not shown). The textured surface can improve the internal reflectivity of incident light, thereby improving the photoelectric conversion efficiency. The textured surface may include multiple protrusions (similar to a pyramid structure). The protrusions may be arranged adjacently or spaced apart, or they may be adjacent or partially overlapping. This application does not limit the number, arrangement, or shape of the protrusions.

[0061] The substrate 100 includes a first region 11 and a second region 12 arranged alternately along a first direction X. The first direction X and the second direction are used to illustrate the arrangement direction of the first region 11 and the second region 12.

[0062] In some embodiments, the first region 11 refers to the region where the first electrode 114 is projected onto the reference plane, and the first region 11 serves as a functional region for forming a first type of metal electrode; similarly, the second region 12 refers to the region where the second electrode 124 is projected onto the reference plane, and the second region 12 serves as a functional region for forming a second type of metal electrode.

[0063] In some embodiments, a spacer region (also a non-metallic electrode region) is provided between the first region 11 and the second region 12. Figure 15The third region 16) refers to the area where the orthographic projections of the first electrode 114 and the second electrode 124 on the reference plane do not overlap, i.e., the spacer region serves as a functional area where no metal electrode is formed. In other embodiments, there is no spacer region between the first region 11 and the second region 12, and there is a height difference between the first region 11 and the second region 12, so that the film layer on the first region 11 and the film layer on the second region 12 do not contact each other.

[0064] It should be noted that, to ensure that the films contacted by the first electrode 114 and the second electrode 124 are both corresponding functional films, the range of the first region 11 is set to be greater than or equal to the orthographic projection range of the first electrode 114 on the reference plane. That is, any orthographic projection of the first electrode 114 on the reference plane is located within the first region 11, and the distance between the edge of the first region 11 and the edge of the orthographic projection pattern is greater than or equal to 0. Similarly, the range of the second region 12 is greater than or equal to the orthographic projection range of the second electrode 124 on the reference plane. The reference plane is a flat surface perpendicular to the thickness direction (vertical direction Z) of the substrate 100. The reference plane is parallel to the surface formed by the first direction X and the second direction.

[0065] In addition, the first region 11, the second region 12, and the spacer region are regions defined by the functional partitioning of the substrate 100 (or the first surface 102) to illustrate the distribution of the film structure of the back contact solar cell. All three actually belong to the substrate 100 (or the first surface 102), and there is no boundary between the different regions. Only the film layers on them may be different. For example, the first region 11 has a first passivation conductive structure 110, the second region 12 has a second passivation conductive structure 120, and most of the spacer regions have a passivation layer (not shown).

[0066] In some embodiments, the first region 11 is either the N region or the P region, and the second region 12 is either the N region or the P region.

[0067] In some embodiments, the substrate 100 includes a first surface 102 and a second surface 101. The first surface 102 includes a first region 11 and a second region 12. The second region 12 is closer to the second surface 101 than the first region 11, or the second region 12 is recessed relative to the first region 11 toward the second surface 101, forming a groove.

[0068] In some embodiments, the distance between the first region 11 and the second surface 101 is greater than the distance between the second region 12 and the second surface 101.

[0069] In some embodiments, the difference between the distance between the first region 11 and the second surface 101 and the distance between the second region 12 and the second surface 101 is less than or equal to 5 μm, that is, the depth of the groove is less than or equal to 5 μm. Thus, the first surface 102 of the substrate 100 is a rough surface with an uneven structure. The restriction of the groove can increase the refractive index of the incident light, thereby improving the photoelectric conversion efficiency of the back contact solar cell.

[0070] The depth of the groove can be 0.5μm, 0.8μm, 1.2μm, 1.5μm, 2.3μm, 2.6μm, 3.1μm, 3.8μm, 4.2μm, 4.5μm or 4.9μm.

[0071] In some embodiments, the depth of the groove ranges from 0.5 μm to 1.5 μm. This range allows for control over the etching depth of the substrate 100. While ensuring complete etching of the film layer on the second region 12, less etching of the substrate 100 is required, avoiding adverse effects caused by excessive etching of the substrate 100. Furthermore, it reduces the etching time and the amount of etching solution, lowering fabrication costs. For example, the groove depth can be any one of 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1 μm, 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm, or 1.5 μm, or a range between any two.

[0072] In some embodiments, the inner wall of the groove forms an obtuse angle with the side surface of the groove, the obtuse angle being in the range of 110° to 150°. Thus, an obtuse angle is formed between the bottom surface of the groove and the side surface of the groove, and the side surface of the groove is inclined relative to the bottom surface, thereby increasing the internal reflectivity of the incident light.

[0073] The obtuse angle between the bottom surface of the groove and the side surface of the groove can be 110°, 115°, 120°, 125°, 130°, 135°, 140°, 145° or 150°.

[0074] The first passivation conductive structure 110 and the second passivation conductive structure 120 can be heterojunction structures and / or tunneling oxide passivation contact structures. These two structures will be described in detail below.

[0075] The heterojunction structure includes an intrinsic passivation layer and a first doped semiconductor layer. The intrinsic passivation layer chemically passivates the substrate surface, reducing surface recombination losses. The intrinsic passivation layer and the first doped semiconductor layer have different band gaps and affinity energies, causing the interface between them to bend and form a built-in electric field. This built-in electric field lowers the potential energy of photogenerated electrons, allowing them to migrate from the substrate into the first doped semiconductor layer and ultimately be collected by the first or second electrode. For photogenerated holes, the electric field prevents their movement towards the first doped semiconductor layer, forcing them to move towards the passivated conductive structure on the other side, thus achieving carrier separation.

[0076] In some embodiments, the material of the intrinsic passivation layer may include at least one of amorphous silicon, microcrystalline silicon, or nanocrystalline silicon. In actual back-contact batteries, the intrinsic passivation layer may be free of doped elements or contain trace amounts of doped elements.

[0077] In some embodiments, the thickness of the intrinsic passivation layer is 5 nm to 18 nm, for example, any value or a range between any two values ​​of 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, 15 nm, 16 nm, 17 nm, or 18 nm. Thus, the thickness of the intrinsic passivation layer can cover the surface of the substrate and form a continuous film, thereby passivating the surface of the substrate; the thickness of the intrinsic passivation layer is also moderate, allowing photogenerated electrons to tunnel into the first doped semiconductor layer.

[0078] In some embodiments, the thickness of the intrinsic passivation layer is 10 nm to 15 nm, for example, any value or a range between any two values ​​of 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, or 15 nm. In this way, the intrinsic passivation layer can effectively cover the substrate surface while allowing for high mobility of photogenerated electrons tunneling into the first doped semiconductor layer.

[0079] In some embodiments, the material of the first doped semiconductor layer includes a single-crystal, polycrystalline, amorphous, or microcrystalline silicon material layer. Accordingly, the crystal state of the first doped semiconductor layer may include at least one of microcrystalline, nanocrystalline, or a mixture of nanocrystalline and microcrystalline states.

[0080] The tunneling oxide passivation contact structure includes a tunneling oxide layer and a second doped semiconductor layer. The second doped semiconductor layer can form band bending on the substrate surface, and the tunneling oxide layer causes an asymmetric shift in the energy band on the substrate surface. This makes the potential barrier for majority carriers (also known as majority carriers) lower than the potential barrier for minority carriers (also known as minority carriers). Therefore, majority carriers can more easily tunnel through the tunneling oxide layer, while minority carriers have difficulty passing through it, thus achieving selective transport of carriers.

[0081] The tunneling oxide layer acts as a chemical passivation layer. By reducing the defect state density of the substrate through dangling bonds in the saturated substrate, it reduces the number of recombination centers in the substrate, thereby lowering the carrier recombination rate.

[0082] The second doped semiconductor layer acts as a field passivation layer. It forms an electrostatic field on the surface of the substrate pointing inward, causing minority carriers to escape from the interface, thereby reducing the minority carrier concentration and decreasing the carrier recombination rate at the substrate interface. This increases the open-circuit voltage, short-circuit current, and fill factor of the back contact cell, thus improving the photoelectric conversion efficiency of the back contact cell.

[0083] In some embodiments, the material of the tunneling oxide layer may include at least one of silicon oxide, aluminum oxide, silicon oxynitride, titanium oxide, hafnium oxide, and zirconium oxide.

[0084] In some embodiments, the thickness of the tunneling oxide layer is 0.5 nm to 5 nm. The thickness range of the tunneling oxide layer is 0.5 nm to 1.3 nm, 1.3 nm to 2.6 nm, 2.6 nm to 4.1 nm, or 4.1 nm to 5 nm. When the tunneling oxide layer is within any of these ranges, its thickness is relatively thin, allowing majority carriers to easily tunnel through it, while minority carriers have difficulty passing through, thus achieving selective carrier transport.

[0085] In some embodiments, the material of the second doped semiconductor layer includes a single-crystal, polycrystalline, amorphous, or microcrystalline silicon material layer. Accordingly, the crystal state of the second doped semiconductor layer may include at least one of microcrystalline, nanocrystalline, polycrystalline, or a mixture of nanocrystalline and microcrystalline states.

[0086] The back contact battery provided in this application embodiment can be arbitrarily combined based on the requirements of the first passivation conductive structure 110 and the second passivation conductive structure 120. In one example, the first passivation conductive structure 110 is a heterojunction structure, the first interface passivation layer 111 in the first passivation conductive structure 110 is an intrinsic passivation layer, and the first doped conductive layer 112 in the first passivation conductive structure 110 is a first doped semiconductor layer; the second passivation conductive structure 120 is a heterojunction structure, the second interface passivation layer 121 in the second passivation conductive structure 120 is an intrinsic passivation layer, and the second doped conductive layer 122 in the second passivation conductive structure 120 is a first doped semiconductor layer. The first doped semiconductor layer in the first passivation conductive structure 110 and the first doped semiconductor layer in the second passivation conductive structure 120 have different conductivity types. The first doped semiconductor layer in the first passivation conductive structure 110 is doped with either an N-type dopant element or a P-type dopant element, while the first doped semiconductor layer in the second passivation conductive structure 120 is doped with either an N-type dopant element or a P-type dopant element.

[0087] In another example, the first passivation conductive structure 110 is a heterojunction structure, the first interface passivation layer 111 in the first passivation conductive structure 110 is an intrinsic passivation layer, and the first doped conductive layer 112 in the first passivation conductive structure 110 is a first doped semiconductor layer; the second passivation conductive structure 120 is a tunneling oxide passivation contact structure, the second interface passivation layer 121 in the second passivation conductive structure 120 is a tunneling oxide layer, and the second doped conductive layer 122 in the second passivation conductive structure 120 is a second doped semiconductor layer. The first doped semiconductor layer in the first passivation conductive structure 110 and the second doped semiconductor layer in the second passivation conductive structure 120 have different conductivity types; the first doped semiconductor layer in the first passivation conductive structure 110 is doped with either an N-type dopant or a P-type dopant, and the second doped semiconductor layer in the second passivation conductive structure 120 is doped with either an N-type dopant or a P-type dopant.

[0088] In another example, the first passivation conductive structure 110 is a tunneling oxide passivation contact structure, the first interface passivation layer 111 in the first passivation conductive structure 110 is a tunneling oxide layer, and the first doped conductive layer 112 in the first passivation conductive structure 110 is a second doped semiconductor layer; the second passivation conductive structure 120 is a tunneling oxide passivation contact structure, the second interface passivation layer 121 in the second passivation conductive structure 120 is a tunneling oxide layer, and the second doped conductive layer 122 in the second passivation conductive structure 120 is a second doped semiconductor layer. The second doped semiconductor layer in the first passivation conductive structure 110 and the second doped semiconductor layer in the second passivation conductive structure 120 have different conductivity types. The second doped semiconductor layer in the first passivation conductive structure 110 is doped with either an N-type dopant or a P-type dopant, while the second doped semiconductor layer in the second passivation conductive structure 120 is doped with either an N-type dopant or a P-type dopant.

[0089] In some embodiments, the surface of the substrate 100 of the first region 11 is a flat surface 14. The flat surface 14 can be a polished surface, for example, a polished surface refers to a surface formed by methods such as chemical polishing (e.g., acid / alkali solution etching). Here, the flat surface 14 does not refer to a completely smooth flat surface, but rather a surface with relatively low roughness that exhibits smoothness.

[0090] In some embodiments, the surface of the substrate 100 of the second region 12 includes a first texture structure 13. The first texture structure 13 can be a pyramid structure, which can improve the internal reflectivity of incident light, thereby improving the photoelectric conversion efficiency. The first texture structure 13 can include multiple small pyramid structures, which can be arranged adjacently or spaced apart, or stacked or partially overlapped. This application does not limit the number, arrangement, or shape of the small pyramid structures.

[0091] The material of the first transparent conductive layer 113 may include at least one of indium oxide, tin-doped indium oxide, tungsten-doped indium oxide, titanium-doped indium oxide, cerium-doped indium oxide, molybdenum-doped indium oxide, hydrogen-doped indium oxide, zinc-doped indium oxide, zinc oxide, aluminum-doped zinc oxide, gallium-doped zinc oxide, tin oxide, or fluorine-doped tin oxide.

[0092] The surface of the first transparent conductive layer 113 includes a plurality of first spherical grains 1131 and first plate-shaped grains 1132.

[0093] It should be noted that the first spherical grain 1131 refers to a three-dimensional, approximately hemispherical or spherical aggregate of grains observed on the surface of the first transparent conductive layer 113. For example Figure 2 and Figure 3The scanning electron microscope image shows spherical grain aggregates. The first lamellar grain 1132 refers to the grain morphology observed on the surface of the first transparent conductive layer 113 that extends significantly in the two-dimensional direction (length and width) but is very thin in the third dimension (thickness), i.e., exhibiting irregular, flat polygonal flakes, for example... Figure 3 The scanning electron microscope image shows a plate-like aggregate of crystals.

[0094] The first spherical grain 1131 and the first plate-like grain 1132 can be tested using images obtained from equipment such as scanning electron microscope (SEM), transmission electron microscope (TEM), or reflection high-energy electron diffraction (RHEED). Figure 2 , Figure 3 as well as Figure 4 This is a scanning electron microscope (SEM) image obtained using a scanning electron microscope.

[0095] In some embodiments, the grain size (D50) of the first spherical grain 1131 ranges from 10 nm to 50 nm. The grain size range of the first spherical grain 1131 can be any value or a range between any two of 10 nm, 13 nm, 15 nm, 18 nm, 20 nm, 23 nm, 25 nm, 30 nm, 35 nm, 40 nm, 45 nm, or 50 nm.

[0096] The grain size of the first spherical grain 1131 is within the above-mentioned range or value is within the above-mentioned range. Under the premise of ensuring the conductivity of the first transparent conductive layer 113, the etching difficulty of the first transparent conductive layer 113 itself can be reduced, and the preparation cost of the first transparent conductive layer 113 and the second transparent conductive layer 123 can be reduced.

[0097] In some embodiments, the grain size (D50) of the first plate-like grain 1132 ranges from 10 nm to 100 nm. The grain size (D50) range of the first plate-like grain 1132 can be any value or a range between any two of the following: 10 nm, 13 nm, 15 nm, 18 nm, 20 nm, 23 nm, 25 nm, 30 nm, 35 nm, 40 nm, 45 nm, 50 nm, 55 nm, 60 nm, 65 nm, 70 nm, 75 nm, 80 nm, 85 nm, 90 nm, 95 nm, or 100 nm.

[0098] The grain size (D50) of the first plate-shaped grain 1132 is within the above range or the value is within the above range. The size of the first plate-shaped grain 1132 is moderate and can be deposited on the surface of the substrate 100 of the second region 12, thereby forming a good film layer and improving the film density of the first transparent conductive layer 113.

[0099] The "grain size" in the grain size of the first spherical grain 1131 and the "grain size" in the grain size of the first plate-shaped grain 1132 refer to the average size of a single crystal particle. D50 refers to the grain size corresponding to the cumulative value of all grains in the thin film of the first transparent conductive layer 113 when the sizes are arranged from smallest to largest.

[0100] Because the size of the first spherical grains 1131 is very small and the number of first spherical grains 1131 is very large compared to the entire first transparent conductive layer 113 / back contact cell / photovoltaic module, it is impossible to exhaustively measure all the first spherical grains 1131 in the entire first transparent conductive layer 113. Instead, several sampling points are selected at different locations in the first transparent conductive layer 113, and the average value of the D50 of the first spherical grains 1131 at these sampling points is measured and calculated to obtain the grain size (D50) of the first spherical grains 1131. That is, the average value of the D50 of the grain size of the first spherical grains 1131 can be measured by sampling. For example, the average value of the D50 of the grain size of the first spherical grains 1131 at 5 sampling points in the first transparent conductive layer 113 can be measured and calculated as the grain size (D50) of the first spherical grains 1131.

[0101] Similarly, the average value of the D50 of the first plate-shaped grain 1132 can be measured by sampling. For example, the average value of the D50 of the first plate-shaped grain 1132 at 5 sampling points in the first transparent conductive layer 113 can be measured and calculated as the grain size (D50) of the first plate-shaped grain 1132.

[0102] Alternatively, the grain size of the first spherical grain 1131 or the first plate-like grain 1132 can be directly measured using images obtained from testing equipment such as scanning electron microscopes, transmission electron microscopes, or high-energy reflected electron diffraction. In this embodiment, the grain size of the first spherical grain 1131 or the first plate-like grain 1132 can also be obtained using X-ray diffraction (XRD).

[0103] In some embodiments, the distribution density of the first spherical grains 1131 and the first plate-like grains 1132 ranges from 1:1 to 1:3. The distribution density of the first spherical grains 1131 and the first plate-like grains 1132 can be any value or a range between any two values ​​of 1:1, 1:1.3, 1:1.5, 1:1.8, 1:2, 1:2.3, 1:2.6, 1:28, or 1:3.

[0104] The distribution density of the first spherical grains 1131 and the first plate-shaped grains 1132 is within any of the above values ​​or any range. The distribution density of the first spherical grains 1131 and the first plate-shaped grains 1132 makes the first transparent conductive layer 113 a film layer with the first plate-shaped grains 1132 as the main conductive path. The more plate-shaped grains there are, the smaller the gap between the grains, and the resistivity of the film layer can be reduced, thereby improving the conductivity of the first transparent conductive layer 113.

[0105] Distribution density (also known as number density) refers to the ratio of the number of first spherical grains 1131 to the number of first plate-like grains 1132 per unit area. The distribution density of the first spherical grains 1131 and the first plate-like grains 1132 can be measured by sampling. For example, the average number density of the first spherical grains 1131 and the first plate-like grains 1132 at five sampling points in the first transparent conductive layer 113 can be used as the distribution density of the first spherical grains 1131 and the first plate-like grains 1132.

[0106] By using a top view of a scanning electron microscope and image analysis software (such as ImageJ) to count the spherical and lamellar grains within the field of view, the result can be obtained by dividing by the image area.

[0107] The material of the second transparent conductive layer 123 may include at least one of indium oxide, tin-doped indium oxide, tungsten-doped indium oxide, titanium-doped indium oxide, cerium-doped indium oxide, molybdenum-doped indium oxide, hydrogen-doped indium oxide, zinc-doped indium oxide, zinc oxide, aluminum-doped zinc oxide, gallium-doped zinc oxide, tin oxide, or fluorine-doped tin oxide.

[0108] In some embodiments, the crystallinity of the first transparent conductive layer 113 is greater than that of the second transparent conductive layer 123. For the first transparent conductive layer 113, the relatively higher crystallinity can improve its conductivity, achieving high conductivity on a relatively smooth surface, thus ensuring the contact performance and electrical performance between the first transparent conductive layer 113 and the first electrode 114. For the second transparent conductive layer 123, the first textured structure 13 on the surface of the substrate 100 can enable good contact performance between the second transparent conductive layer 123 and the second electrode 124, and can also reduce resistance and improve electrical performance.

[0109] It should be noted that the crystallinity of the first transparent conductive layer 113 refers to the volume or weight percentage of the crystalline portion (i.e., grains) in the first transparent conductive layer 113. The crystalline portion includes first spherical grains 1131 and first plate-like grains 1132. The crystallinity of the second transparent conductive layer 123 refers to the volume or weight percentage of the crystalline portion (i.e., grains) in the second transparent conductive layer 123. The crystalline portion includes second spherical grains 1231.

[0110] In addition, the crystallinity of the first transparent conductive layer 113 and the crystallinity of the second transparent conductive layer 123 can be obtained by using testing equipment such as transmission electron microscopy, Raman spectroscopy, or X-ray diffraction.

[0111] In some embodiments, the first thickness of the first transparent conductive layer 113 is greater than the second thickness of the second transparent conductive layer 123. The larger thickness of the first transparent conductive layer 113 allows for better coverage of the surface of the second doped conductive layer 122 and collection of charge carriers. The smaller thickness of the second transparent conductive layer 123 allows for the retention or conformal conformal formation of the first texture structure 13, resulting in an uneven surface on the surface of the second transparent conductive layer 123 away from the substrate 100. This improves internal reflection of incident light and enhances the photoelectric conversion efficiency of the back-contact battery.

[0112] Conformal means that the side of the first transparent conductive layer 113 away from the substrate has a surface morphology similar to or the same as the first texture structure 13.

[0113] In some embodiments, the ratio of the second thickness to the first thickness is 0.5 to 0.95. The ratio can be any value of 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, or 0.95, or a range between any two values. When the ratio of the second thickness to the first thickness is within the above range, the thickness of the first transparent conductive layer 113 can improve the lateral transmission capability, while the second transparent conductive layer 123 can both cover the first textured structure 13 and allow the surface of the second transparent conductive layer 123 away from the substrate 100 to exhibit an uneven morphology to improve the internal reflection of incident light.

[0114] In some embodiments, the ratio of the second thickness to the first thickness is 0.7 to 0.9. The ratio can be any value of 0.7, 0.75, 0.8, 0.85, 0.88, or 0.9, or a range between any two values. When the ratio of the second thickness to the first thickness is within the above range, the thickness of the first transparent conductive layer 113 can improve the lateral transmission capability, while the second transparent conductive layer 123 can both cover the first textured structure 13 and allow the surface of the second transparent conductive layer 123 away from the substrate 100 to exhibit an uneven morphology to improve the internal reflection of incident light. When the ratio of the second thickness to the first thickness is within the above range, the lateral transmission capability of the second transparent conductive layer 123 can also be improved, enhancing the transmission performance between the second transparent conductive layer 123 and the second electrode.

[0115] The surface of the second transparent conductive layer 123 includes second spherical grains 1231.

[0116] It should be noted that the second spherical grain 1231 refers to a three-dimensional, approximately hemispherical or spherical aggregate of grains observed on the surface of the second transparent conductive layer 123. For example... Figure 4 The scanning electron microscope image shows spherical aggregates of crystals.

[0117] The second spherical grain 1231 can be tested using images obtained from testing equipment such as scanning electron microscope, transmission electron microscope, or high-energy reflection electron diffraction. Figure 4 This is a scanning electron microscope (SEM) image obtained using a scanning electron microscope.

[0118] In some embodiments, the grain size (D50) of the second spherical grain 1231 ranges from 10 nm to 50 nm. The grain size range of the second spherical grain 1231 can be any value or a range between any two of 10 nm, 13 nm, 15 nm, 18 nm, 20 nm, 23 nm, 25 nm, 30 nm, 35 nm, 40 nm, 45 nm, or 50 nm.

[0119] The grain size of the second spherical grain 1231 is within the above-mentioned range or value. Under the premise of ensuring the conductivity of the second transparent conductive layer 123, the second spherical grain 1231 can be located in or fill the recess of the first texture structure 13, thereby achieving better coverage performance and improving the electrical performance between the second doped conductive layer 122 and the second electrode 124.

[0120] It should be noted that the "grain size" in the grain size of the first spherical grain 1131 refers to the average size of a single crystal particle. D50 refers to the grain size corresponding to the cumulative value of all grains in the thin film of the second transparent conductive layer 123 when the sizes are arranged from smallest to largest.

[0121] It should also be noted that, compared to the entire second transparent conductive layer 123 / back contact cell / photovoltaic module, the grain size of the second spherical grains 1231 is very small and the number of second spherical grains 1231 is very large. Therefore, it is impossible to exhaustively measure all the second spherical grains 1231 in the entire second transparent conductive layer 123. Instead, several sampling points are selected at different locations in the second transparent conductive layer 123, and the average value of the D50 of the grain size of the second spherical grains 1231 at these sampling points is measured and calculated to obtain the grain size (D50) of the second spherical grains 1231. That is, the average value of the D50 of the grain size of the second spherical grains 1231 can be measured by sampling. For example, the average value of the D50 of the grain size of the second spherical grains 1231 at 5 sampling points in the second transparent conductive layer 123 can be measured and calculated as the grain size (D50) of the second spherical grains 1231.

[0122] Alternatively, the grain size of the second spherical grain 1231 or the grain size of the second plate-shaped grain can be directly measured using images obtained from testing equipment such as scanning electron microscopes, transmission electron microscopes, or high-energy reflection electron diffraction. In this embodiment, the grain size of the second spherical grain 1231 can also be obtained using an X-ray diffractometer.

[0123] In some embodiments, the first size of the first spherical grain 1131 is smaller than the second size of the second spherical grain 1231. Thus, the second spherical grains 1231 can fill the recesses of the first textured structure 13 and bond together to form an integral film layer.

[0124] It should be noted that the first dimension, the second dimension, and the subsequent third and fourth dimensions are all grain sizes. The testing methods and equipment can refer to the above-mentioned testing methods and equipment for grain sizes.

[0125] In some embodiments, the surface of the second transparent conductive layer 123 further includes second lamellar grains, the fourth dimension of which is smaller than the third dimension of the first lamellar grains 1132. Thus, the grain boundary density of the first transparent conductive layer 113 is low, improving carrier mobility; when the second transparent conductive layer 123 conformally covers the first textured structure 13, it can better adapt to the undulations of the substrate 100, reducing problems such as discontinuity in coverage or stress concentration caused by excessively large grains. Simultaneously, the fine grains help form a denser film, enhancing the protective effect on the underlying passivation layer.

[0126] It should be noted that the second sheet-like grain refers to the grain morphology observed on the surface of the second transparent conductive layer 123 that extends significantly in the two-dimensional direction (length and width) but is very thin in the third dimension (thickness), i.e., it presents an irregular, flat polygonal sheet.

[0127] The second type of plate-like grain can be tested using images obtained from testing equipment such as scanning electron microscopes, transmission electron microscopes, or high-energy reflected electron diffraction.

[0128] In some embodiments, the first spherical grains 1131 and the first sheet-like grains 1132 have a first distribution density, and the second spherical grains 1231 and the second sheet-like grains have a second distribution density, wherein the first distribution density is less than the second distribution density. Thus, the first transparent conductive layer 113 has good lateral conductivity and low resistivity, effectively reducing series resistance. The second transparent conductive layer 123 can adapt to the undulating substrate 100 of the first textured structure 13 based on the second spherical grains 1231, thereby better covering and conforming to the first textured structure 13. Furthermore, the relatively small grain size of the second spherical grains 1231 and the second sheet-like grains allows for greater flexibility and deformation, reducing interfacial stress caused by thermal expansion coefficient mismatch and preventing film cracking or delamination.

[0129] It should also be noted that the second distribution density (also known as the number density) refers to the ratio of the number of second spherical grains 1231 to the number of second plate-shaped grains per unit area. The distribution density of the second spherical grains 1231 and the second plate-shaped grains can be measured using a sampling method. For example, the average number density of the second spherical grains 1231 and the second plate-shaped grains at five sampling points in the second transparent conductive layer 123 can be used as the distribution density of the second spherical grains 1231 and the second plate-shaped grains.

[0130] In some embodiments, the surface of the second transparent conductive layer 123 further includes a third spherical grain, the size of which is smaller than the size of the second spherical grain 1231. The second transparent conductive layer 123 comprises two spherical grains of different sizes, wherein the third spherical grain is located closer to the surface of the second doped conductive layer 122, and the second spherical grain 1231 is located on the surface of the third spherical grain farther from the second doped semiconductor layer. Thus, the first texture structure 13 can be filled and conformally conformed to the small size of the third spherical grain, and the second spherical grain 1231 is used to improve conductivity and unevenness, increasing the internal reflection of incident light from the second transparent conductive layer 123.

[0131] It should be noted that the test method, size, and distribution density / proportion of the third spherical grain can be referred to the test method, size, and distribution density / proportion of the second spherical grain 1231, and will not be repeated here.

[0132] In some embodiments, on the side of the second transparent conductive layer 123 closer to the second doped conductive layer 122, the proportion of the third spherical grains is greater than the proportion of the second spherical grains 1231. On the side of the second transparent conductive layer 123 farther from the second doped conductive layer 122, the proportion of the third spherical grains is less than the proportion of the second spherical grains 1231.

[0133] In some embodiments, the first textured structure 13 includes a top and a tower surface. The size of the second spherical grains 1231 of the second transparent conductive layer 123 located at the top is larger than that of the second spherical grains 1231 of the second transparent conductive layer 123 located on the tower surface. Thus, the larger grains have better conductivity, which can improve the conductivity and contact performance between the second transparent conductive layer 123 and the second electrode 124. The smaller size of the second spherical grains 1231 on the tower surface makes it easier to achieve continuous coverage on steep slopes, preventing pinhole defects on the tower surface and thus avoiding reverse leakage current in the second transparent conductive layer 123.

[0134] It should be noted that the top of the first texture structure 13 can refer to the apex of a pyramid structure, and the surface of the first texture structure 13 can refer to the surface of a pyramid structure. In another example, the top of the first texture structure 13 can refer to the top of the concave-convex structure on the side away from the base 100, and the surface of the first texture structure 13 can refer to a curved surface / arc / plane that is distinct from the top.

[0135] In some embodiments, reference Figure 5 The first transparent conductive layer 113 includes a first sublayer 131 and a second sublayer 132. The first sublayer 131 is located between the first passivated conductive structure 110 and the second sublayer 132. The distribution density of the first lamellar grains 1132 in the first sublayer 131 is less than that in the second sublayer 132. Thus, the first sublayer 131 has fewer first lamellar grains 1132 and more first spherical grains 1131, possessing more grain boundaries, which can act as gettering centers to capture impurity ions introduced from the external environment or the TCO bulk phase, preventing them from diffusing to the underlying interface. The second sublayer 132 has more first lamellar grains 1132 and fewer first spherical grains 1131. The high-density fine lamellar grains form a dense, nanoscale unevenness on the surface, which can form a gradient refractive index layer, improving the short-wavelength response.

[0136] It should be noted that the distribution density of the first plate-like grains 1132 in the first sub-layer 131 and the distribution density of the first plate-like grains in the second sub-layer 132 can be referred to the description of the distribution density of the first plate-like grains 1132 in the first transparent conductive layer 113, and will not be described in detail here.

[0137] In some embodiments, reference Figure 6 The substrate 100 surface of the second region 12 includes a second textured structure 15, and a second passivated conductive structure 120 covers the second textured structure 15. The second roughness of the second textured structure 15 is less than the first roughness of the first textured structure 13. Thus, the first region 11 has a relatively flat surface, allowing for the deposition of a thinner first passivated conductive structure 110 to achieve atomically uniform coverage, significantly reducing the interface defect state density. The first textured structure 13 on the second region 12 provides a larger specific surface area, enhancing the scattering of incident light and reducing optical losses.

[0138] Roughness refers to the maximum height of the profile (Rz), which is the distance between the peak and valley lines of the profile within the sampling length of the sampling area. For example, the first roughness of the first texture structure 13 refers to the distance between the peak and valley lines of the profile within the sampling range on the first transparent conductive layer 113. The second roughness of the second texture structure refers to the distance between the peak and valley lines of the profile within the sampling range on the second transparent conductive layer 123.

[0139] Roughness can be measured using testing equipment including, but not limited to, contact probe profilometers (profilometers), optical profilometers (white light interferometry / confocal microscopy), atomic force microscopes (AFM), or scanning electron microscopes.

[0140] It should also be noted that the first roughness average value of the first texture structure 13 can be measured using a sampling method. For example, the first roughness average value of the first texture structure 13 at 5 sampling points in the first transparent conductive layer 113 can be measured and calculated as the first roughness of the first texture structure 13. The second roughness average value of the second texture structure can also be measured using a sampling method. For example, the second roughness average value of the second texture structure at 5 sampling points in the second transparent conductive layer 123 can be measured and calculated as the second roughness of the second texture structure.

[0141] Continue to refer to Figure 1 The back contact battery includes a first electrode 114, which is in electrical contact with a first transparent conductive layer 113.

[0142] Continue to refer to Figure 1 The back contact battery includes a second electrode 124, which is in electrical contact with a second transparent conductive layer 123.

[0143] In some embodiments, either the first electrode 114 or the second electrode 124 may be sintered from a sintering-type metal paste or from a LECO (Laser-enhanced contact optimization) paste. The metal paste and the LECO paste may include at least one of silver, aluminum, copper, tin, gold, lead, or nickel.

[0144] In some embodiments, the back contact battery further includes an antireflection layer, which is located on the surface of the first transparent conductive layer 113, the surface of the second transparent conductive layer 123, and the surface of the second doped conductive layer 122.

[0145] It should be noted that in a back contact battery containing an antireflective layer or a passivation layer, the connection between the first electrode 114 and the first transparent conductive layer 113 can be a contact connection or an indirect connection through conductive particles; the connection between the second electrode 124 and the second transparent conductive layer 123 can be a contact connection or an indirect connection through conductive particles. The conductive particles can be silver crystals, silver aggregates, silver particles, or other conductive metal particles.

[0146] In the back contact battery provided in this application embodiment, a second transparent conductive layer 123 containing second spherical grains 1231 is disposed on the first textured structure 13. First, the second spherical grains 1231 are three-dimensional structures with relatively small grain sizes, which can fill the depressions in the first textured structure 13, increasing contact performance. Second, the second spherical grains 1231 are three-dimensionally grown, resulting in a thicker second transparent conductive layer 123 covering the first textured structure 13, allowing for more complete coverage of the textured structure's film layer, thereby improving lateral transport capability. Third, the second spherical grains 1231 have good conductivity, which can improve the conductivity of the transparent conductive layer. The etching performance of the first transparent conductive layer 113 containing first sheet-like grains 1132 is greater than that of the second transparent conductive layer 123 containing second spherical grains 1231. Therefore, the process of forming the first transparent conductive layer 113 and the second transparent conductive layer 123 by etching a portion of the transparent conductive layer is simpler, reducing process difficulty.

[0147] Accordingly, another aspect of this application provides a method for preparing a back contact battery, which is used to prepare the back contact battery provided in the above embodiments. The same or corresponding technical features as those in the above embodiments will not be described in detail here.

[0148] Figures 7-15 This is a schematic diagram of the structure of a back contact battery corresponding to each step in the preparation method of a back contact battery provided in another embodiment of this application.

[0149] refer to Figure 7It includes: providing a substrate 100, the substrate 100 including alternating first regions 11 and second regions 12.

[0150] The first surface 102 and the second surface 101 of the substrate 100 are smoothed surfaces. The second surface 101 is texturized. The texturization process includes chemical etching, for example, cleaning the original substrate with a mixed solution of potassium hydroxide and hydrogen peroxide. Specifically, the desired textured surface structure can be formed by controlling the concentration ratio of potassium hydroxide and hydrogen peroxide solution.

[0151] In some embodiments, textured structures (not shown) can also be formed using methods such as laser etching, mechanical methods, or plasma etching. In laser etching, laser process parameters are controlled to obtain a textured structure with the desired morphology. The textured structure includes multiple pyramidal structures.

[0152] refer to Figure 8 The preparation method includes: forming an initial passivation conductive layer, wherein the initial passivation conductive layer is located in the first region 11 and the second region 12.

[0153] refer to Figure 8 A first film layer 103 is formed on the first region 11 and the second region 12 of the substrate 100 by chemical vapor deposition (CVD); a second film layer is formed on the first film layer 103 by PECVD (Plasma-Enhanced Chemical Vapor Deposition); a doped source layer is formed on the surface of the second film layer by PECVD; a doping process is performed to migrate some of the dopants in the doped source layer to the second film layer, and the second film layer is crystallized to form a first doped film 104, and the doped source layer is converted into an oxide film.

[0154] In some embodiments, a thinning process is also involved to reduce the thickness of the formed oxide film. In some embodiments, the oxide film is removed. The oxide film removal process can be laser etching or wet etching.

[0155] refer to Figure 9 The preparation method includes removing the initial passivation conductive layer located in the second region 12 and forming a first texture structure 13 on the surface of the substrate 100 in the second region 12, and the remaining initial passivation conductive layer is the first passivation conductive structure 110.

[0156] refer to Figure 9The process parameters for removing the first doped film 104 on the second region 12 include: the etching solution is an alkaline solution with a concentration ratio of 0.1 PPM (parts per million) to 0.6 PPM, the etching time is 20 s to 500 s, and the etching temperature is 50 ℃ to 90 ℃.

[0157] Continue to refer to Figure 9 While removing the first doped film 104 on the second region 12, the substrate 100 will continue to be etched to form grooves and the first texture structure 13, that is, the surface of the substrate 100 in the first region 11 and the surface of the substrate 100 in the second region 12 form a height difference.

[0158] The remaining first film layer 103 serves as the first interface passivation layer 111, and the remaining first doped film 104 serves as the first doped conductive layer 112.

[0159] refer to Figure 10 and Figure 11 The preparation method includes: forming a second passivated conductive structure 120, the second passivated conductive structure 120 being located in the second region 12, and the second passivated conductive structure 120 covering the first texture structure 13.

[0160] refer to Figure 10 A third film layer 105 is formed on the first region 11 and the second region 12 of the substrate 100 by chemical vapor deposition; a second doped film 106 is formed on the third film layer 105 by PECVD5 process.

[0161] refer to Figure 11 A mask layer is formed on the surface of the second doped film 106 corresponding to the second region 12 and on the surface of the second doped film 106 in part of the first region 11. The spacing between adjacent mask layers is smaller than the size of the first region 11 along the first direction X.

[0162] Continue to refer to Figure 11 Using the mask layer as a mask, the third film layer 105 and the second doped film 106 located on the first region 11 are removed. The remaining third film layer 105 serves as the second interface passivation layer 121, and the remaining second doped film 106 serves as the second doped conductive layer 122. The mask layer is then removed.

[0163] refer to Figure 12 and Figure 13The preparation method includes: forming a first transparent conductive layer 113, the first transparent conductive layer 113 being located on the surface of a first passivated conductive structure 110, the surface of the first transparent conductive layer 113 including a plurality of first spherical grains 1131 and first plate-shaped grains 1132; forming a second transparent conductive layer 123, the second transparent conductive layer 123 being located on the surface of a second passivated conductive structure 120, the surface of the second transparent conductive layer 123 including second spherical grains 1231.

[0164] refer to Figure 12 The fabrication method includes: forming a transparent conductive film 107, which is located in a first region 11 and a second region 12. The transparent conductive film 107 is located on the surface of the first doped semiconductor layer away from the substrate 100 and on the surface of the second doped semiconductor layer. The surface of the transparent conductive film 107 deposited in the second region 12 includes second spherical grains 1231, and the surface of the transparent conductive film 107 deposited in the first region 11 includes a plurality of first spherical grains 1131 and first plate-like grains 1132.

[0165] It should be noted that the process for forming the transparent conductive film 107 is magnetron sputtering deposition. When forming the transparent conductive film 107 on the surface of the second doped conductive layer 122, because the surface of the substrate 100 in the first region 11 has a first textured structure 13, the conductivity of the surface of the second doped conductive layer 122 is relatively poor, leading to charge accumulation and the formation of second spherical grains 1231, which continue to form. When forming the transparent conductive film 107 on the surface of the first doped conductive layer 112, because the surface of the substrate 100 in the second region 12 is a flat surface, the conductivity of the surface of the first doped conductive layer 112 is poor in the early stages, forming first spherical grains 1131. In the later stages, the conductivity of the flat surface is better, thus tending towards two-dimensional growth, forming first plate-like grains 1132.

[0166] It should also be noted that during the formation of the transparent conductive film 107, the process parameters of magnetron sputtering deposition can be kept unchanged, or the process parameters can be adjusted later, such as adjusting the sputtering power to control 1kw~10kw, temperature 100℃~230℃, oxygen content 3scccm~50scccm, and belt speed 5mm / s~40mm / s, etc.

[0167] refer to Figure 13 The preparation method includes: removing the transparent conductive film 107 at the junction of the first region 11 and the second region 12, retaining the transparent conductive film 107 located in the first region 11 as the first transparent conductive layer 113, and the transparent conductive film 107 located in the second region 12 as the second transparent conductive layer 123.

[0168] In some embodiments, the process steps for forming the first transparent conductive layer 113 and the second transparent conductive layer 123 include: forming a first transparent conductive film with first process parameters, the first transparent conductive film being located on the surface of the first passivated conductive structure 110 and the surface of the second passivated conductive structure 120, the surface of the first transparent conductive film located on the first passivated conductive structure 110 including first spherical grains 1131, and the surface of the first transparent conductive film located on the second passivated conductive structure 120 including second spherical grains 1231; forming a second transparent conductive film with second process parameters, the second transparent conductive film being located on a portion of the surface of the first transparent conductive film; the surface of the second transparent conductive film including first sheet-like particles.

[0169] In some embodiments, the first process parameters include: pressure 0.3 Pa to 0.5 Pa, power 1 kW to 1.5 kW, belt speed 5 mm / s to 10 mm / s, oxygen flow rate 3 sccm to 10 sccm, argon flow rate 200 sccm to 500 sccm, and temperature 100℃ to 150℃.

[0170] In some embodiments, the second process parameters include: pressure 0.5 Pa to 2 Pa, power 3 kW to 10 kW, belt speed 7 mm / s to 50 mm / s, oxygen flow rate 15 sccm to 50 sccm, argon flow rate 500 sccm to 1500 sccm, and temperature 150℃ to 230℃.

[0171] In some embodiments, reference Figure 14 and Figure 15 The substrate 100 further includes a third region 16, which is located between the second region 12 and the first region 11. The process steps for forming the first transparent conductive layer 113 and the second transparent conductive layer 123 include: forming a transparent conductive film 107, which is located in the first region 11, the second region 12 and the third region 16; wherein the surface of the transparent conductive film 107 deposited in the second region 12 includes second spherical grains 1231, and the surface of the transparent conductive film 107 deposited in the first region 11 and the third region 16 includes a plurality of first spherical grains 1131 and first sheet grains 1132; removing the transparent conductive film 107 in the third region 16, retaining the transparent conductive film 107 located in the first region 11 as the first transparent conductive layer 113, and the transparent conductive film 107 located in the second region 12 as the second transparent conductive layer 123.

[0172] Accordingly, another embodiment of this application provides a stacked battery, comprising the back contact battery provided in the above embodiments and the back contact battery prepared by the preparation method of the back contact battery provided in the above embodiments. The same or corresponding technical features as the above embodiments will not be described in detail here.

[0173] Figure 16This is a schematic diagram of a stacked battery provided in another embodiment of this application.

[0174] refer to Figure 16 The tandem solar cell (TSC) includes: a crystalline silicon bottom cell, which is a back contact cell as provided in the above embodiments or a back contact cell prepared by the preparation method provided in the above embodiments; and a perovskite top cell, which is located on one side of the crystalline silicon bottom cell.

[0175] In some embodiments, the perovskite top cell 140 may include: a first transport layer, a perovskite substrate 100, a second transport layer, and a transparent conductive layer stacked together. The first transport layer is disposed opposite to the crystalline silicon bottom cell 130.

[0176] In some examples, the first transport layer can be either an electron transport layer or a hole transport layer, and the second transport layer can be either an electron transport layer or a hole transport layer.

[0177] In some embodiments, the perovskite top cell 140 has a wider bandgap than the crystalline silicon bottom cell 130. Therefore, stacking the perovskite top cell 140 on top of the crystalline silicon bottom cell 130 can give the stacked cell a wider spectral response range, thereby maximizing the utilization of solar energy and improving the efficiency of the stacked cell.

[0178] In some embodiments, the tandem solar cell may further include an intermediate connecting layer (not shown in the figure), which connects the crystalline silicon bottom cell 130 and the perovskite top cell 140.

[0179] In some cases, an intermediate connecting layer is used to enable carrier transport between the crystalline silicon bottom cell 130 and the perovskite top cell 140. This layer is typically a tunnel junction or a very thin metal or transparent electrode composite layer. Optionally, the intermediate connecting layer can be a transparent conductive oxide, which possesses excellent optoelectronic properties, high photon transmittance, and high conductivity, thereby enabling the perovskite top cell 140 and the crystalline silicon bottom cell 130 to maintain good ohmic contact.

[0180] In some cases, the first and second bus electrodes in the back contact cell of the crystalline silicon bottom cell 130 can also serve as an intermediate connection layer to achieve electrical connection with the perovskite top cell 140. Electrical connection between the two actually means that both are made of conductive materials, and they are directly contacted or connected via other conductive materials. Therefore, when the tandem cell is in power generation mode, there is an electrical connection between them.

[0181] Accordingly, another embodiment of this application provides a photovoltaic module comprising the back contact cell provided in the above embodiments and the back contact cell prepared by the preparation method of the back contact cell provided in the above embodiments. The same or corresponding technical features as those in the above embodiments will not be described in detail here.

[0182] Figure 17 This is a schematic diagram of a photovoltaic module provided in another embodiment of this application.

[0183] refer to Figure 17 The photovoltaic module includes: a battery string, which is formed by connecting multiple back contact batteries 30 as provided in the above embodiments, back contact batteries 30 prepared by the preparation method provided in the above embodiments, or stacked batteries as provided in the above embodiments; an encapsulation layer 31 for covering the surface of the battery string; and a cover plate 32 for covering the surface of the encapsulation layer 31 away from the battery string.

[0184] The battery string includes a connecting member 318 for electrically connecting two adjacent back contact batteries 30. In some embodiments, multiple back contact batteries 30 can be electrically connected through the connecting member 318, which is welded to the main grid / sub-grid on the back contact battery 30.

[0185] In some embodiments, the connecting member 318 is welded to a sub-grid on the battery cell, the sub-grid including a first electrode and a second electrode. In some embodiments, the connecting member 318 is welded to a main grid on the battery cell, the main grid including a first main grid and a second main grid, the first main grid being welded to a first electrode and the second main grid being welded to a second electrode.

[0186] Figure 17 This illustration only shows one positional relationship between the back contact batteries 30, where electrodes of different polarities in each back contact battery 30 are located on the same surface, and the sides of each back contact battery 30 with the first electrode and the second electrode face the same direction. The connecting component 318 connects to the same side of two adjacent back contact batteries 30. In other embodiments, the back contact batteries may also be arranged such that the sides of two adjacent back contact batteries with the first electrode and the second electrode are located on different sides, in which case the connecting component 318 connects to the different sides of the two adjacent back contact batteries.

[0187] In some embodiments, the back contact battery 30 is electrically connected in the form of a single sheet or multiple segments to form multiple battery strings, and the multiple battery strings are electrically connected in series and / or parallel. The back contact battery 30 can be a single sheet of battery or a slice of battery, where a slice of battery refers to a battery formed by cutting a complete sheet of battery.

[0188] In some embodiments, the encapsulation layer 31 includes a first encapsulation layer and a second encapsulation layer. The first encapsulation layer covers one of the front or back sides of the back contact battery 30, and the second encapsulation layer covers the other of the front or back sides of the back contact battery 30. Specifically, at least one of the first encapsulation layer or the second encapsulation layer may be an organic encapsulation film such as polyvinyl butyral (PVB), ethylene-vinyl acetate copolymer (EVA), polyolefin thermoplastic elastomer (POE), or polyethylene terephthalate (PET). Alternatively, at least one of the first encapsulation layer or the second encapsulation layer may also be an EP film, an EPE film, or a PVP film. Among them, EP film refers to a co-extruded film composed of stacked EVA film and POE film; EPE film refers to a co-extruded film formed by sequentially stacking EVA film, POE film, and EVA film; and PVP film refers to a co-extruded film formed by stacking POE film, EVA film, and POE film. Co-extruded films can be prepared by sequentially extruding one or more raw materials onto another pre-made film during the film processing, or by bonding different types of pre-made films together.

[0189] It is worth noting that there is a dividing line between the first encapsulation layer and the second encapsulation layer before the lamination process. After the lamination process, the photovoltaic module will no longer have the concept of a first encapsulation layer and a second encapsulation layer. That is, the first encapsulation layer and the second encapsulation layer have formed an integral encapsulation layer 31.

[0190] In some embodiments, the cover plate 32 can be a glass cover plate, a plastic cover plate, or other cover plate with light-transmitting function. Specifically, the surface of the cover plate 32 facing the encapsulation layer 31 can be an uneven surface, thereby increasing the utilization rate of incident light. The cover plate 32 includes a first cover plate and a second cover plate, wherein the first cover plate is opposite to the first encapsulation layer, and the second cover plate is opposite to the second encapsulation layer; or the first cover plate is opposite to the side of the back contact solar cell, and the second cover plate is opposite to the other side of the back contact solar cell.

[0191] Accordingly, another embodiment of this application provides a manufacturing apparatus for a back contact battery, which prepares the back contact battery provided in the above embodiment based on the preparation method of the back contact battery provided in the above embodiment. The same or corresponding technical features as those in the above embodiment will not be described in detail here.

[0192] The manufacturing apparatus for a back contact battery includes: an acquisition module for acquiring a substrate 100, the substrate 100 including alternating first regions 11 and second regions 12; a first manufacturing module for forming a first textured structure 13 on the surface of the substrate 100 in the second region 12; and a second manufacturing module for forming a first passivated conductive structure 110 on the first region 11, forming a second passivated conductive structure 120 on the second region 12, forming a first transparent conductive layer 113 on the surface of the first passivated conductive structure 110, and forming a second transparent conductive layer 123 on the surface of the second passivated conductive structure 120; the second passivated conductive structure 120 covers the first textured structure 13; the surface of the first transparent conductive layer 113 includes a plurality of first spherical grains 1131 and first plate-like grains 1132; and the surface of the second transparent conductive layer 123 includes second spherical grains 1231.

[0193] Those skilled in the art will understand that the above embodiments are specific examples of implementing this application, and in practical applications, various changes can be made in form and detail without departing from the spirit and scope of this application. Any person skilled in the art can make their own modifications and alterations without departing from the spirit and scope of this application; therefore, the scope of protection of this application should be determined by the scope defined in the claims.

Claims

1. A back-contact battery, characterized in that, include: The substrate includes alternating first and second regions; the substrate surface of the second region includes a first texture structure. A first passivated conductive structure is located in the first region; A second passivated conductive structure is located in the second region and covers the first texture structure. A first transparent conductive layer is located on the surface of the first passivated conductive structure, and the surface of the first transparent conductive layer includes a plurality of first spherical grains and first plate-shaped grains. A second transparent conductive layer is located on the surface of the second passivated conductive structure, and the surface of the second transparent conductive layer includes second spherical grains.

2. The back contact battery according to claim 1, characterized in that, The first size of the first spherical grain is smaller than the second size of the second spherical grain.

3. The back contact battery according to claim 1, characterized in that, The first texture structure includes a top and a tower surface, wherein the size of the second spherical grains of the second transparent conductive layer located at the top is larger than that of the second spherical grains of the second transparent conductive layer located at the tower surface.

4. The back contact battery according to claim 1, characterized in that, The crystallinity of the first transparent conductive layer is greater than that of the second transparent conductive layer.

5. The back contact battery according to claim 1, characterized in that, The first transparent conductive layer includes a first sublayer and a second sublayer. The first sublayer is located between the first passivated conductive structure and the second sublayer. The distribution density of the first plate-like grains in the first sublayer is less than the distribution density of the first plate-like grains in the second sublayer.

6. The back contact battery according to any one of claims 1 to 5, characterized in that, The surface of the second transparent conductive layer also includes a second sheet-like grain, the fourth dimension of which is smaller than the third dimension of the first sheet-like grain.

7. The back contact battery according to claim 6, characterized in that, The first spherical grains and the first plate-shaped grains have a first distribution density, and the second spherical grains and the second plate-shaped grains have a second distribution density, wherein the first distribution density is less than the second distribution density.

8. The back contact battery according to any one of claims 1 to 5, characterized in that, The substrate surface of the first region is a flat surface.

9. The back contact battery according to claim 8, characterized in that, The first thickness of the first transparent conductive layer is greater than the second thickness of the second transparent conductive layer.

10. The back contact battery according to claim 9, characterized in that, The ratio of the second thickness to the first thickness is 0.7 to 0.

9.

11. The back contact battery according to claim 8, characterized in that, The distribution density of the first spherical grains and the first plate-shaped grains ranges from 1:1 to 1:

3.

12. The back contact battery according to any one of claims 1 to 5, characterized in that, The substrate surface of the second region includes a second textured structure, the second passivated conductive structure covers the second textured structure, and the second roughness of the second textured structure is less than the first roughness of the first textured structure.

13. The back contact battery according to any one of claims 1 to 5, characterized in that, The substrate includes a first surface and a second surface. The first surface includes a first region and a second region. The distance between the first region and the second surface is greater than the distance between the second region and the second surface.

14. The back contact battery according to any one of claims 1 to 5, characterized in that, The surface of the second transparent conductive layer also includes a third spherical grain, the size of which is smaller than the size of the second spherical grain.

15. A method for preparing a back-contact battery, characterized in that, include: A substrate is provided, the substrate comprising alternating first and second regions; An initial passivation conductive layer is formed, the initial passivation conductive layer being located in the first region and the second region; The initial passivation conductive layer located in the second region is removed, and a first texture structure is formed on the substrate surface in the second region. The remaining initial passivation conductive layer is the first passivation conductive structure. A second passivated conductive structure is formed, the second passivated conductive structure is located in the second region, and the second passivated conductive structure covers the first texture structure; A first transparent conductive layer is formed, the first transparent conductive layer is located on the surface of the first passivated conductive structure, and the surface of the first transparent conductive layer includes a plurality of first spherical grains and first plate-shaped grains; A second transparent conductive layer is formed, the second transparent conductive layer is located on the surface of the second passivated conductive structure, and the surface of the second transparent conductive layer includes second spherical grains.

16. The method for preparing a back contact battery according to claim 15, characterized in that, The process steps for forming the first transparent conductive layer and the second transparent conductive layer include: A first transparent conductive film is formed using first process parameters. The first transparent conductive film is located on the surface of the first passivated conductive structure and the surface of the second passivated conductive structure. The surface of the first transparent conductive film located on the first passivated conductive structure includes first spherical grains, and the surface of the first transparent conductive film located on the second passivated conductive structure includes second spherical grains. A second transparent conductive film is formed using second process parameters. The second transparent conductive film is located on the surface of a portion of the first transparent conductive film. The surface of the second transparent conductive film includes first sheet-like particles.

17. The method for preparing a back contact battery according to claim 15, characterized in that, The substrate further includes a third region, which is located between the second region and the third region; The process steps for forming the first transparent conductive layer and the second transparent conductive layer include: A transparent conductive film is formed, the transparent conductive film being located in the first region, the second region, and the third region; wherein, the surface of the transparent conductive film deposited in the second region includes second spherical grains, and the surface of the transparent conductive film deposited in the first region and the third region includes a plurality of first spherical grains and first plate-like grains; Remove the transparent conductive film in the third region, retain the transparent conductive film in the first region as the first transparent conductive layer, and retain the transparent conductive film in the second region as the second transparent conductive layer.

18. A stacked battery, characterized in that, include: A crystalline silicon bottom cell, wherein the crystalline silicon bottom cell is a back contact cell as described in any one of claims 1 to 14 or a back contact cell prepared by the preparation method as described in any one of claims 15 to 17; A perovskite top cell, wherein the perovskite top cell is located on one side of the crystalline silicon bottom cell.

19. A photovoltaic module, characterized in that, include: A battery string is formed by connecting multiple back contact batteries as described in any one of claims 1 to 14, back contact batteries prepared by the preparation method as described in any one of claims 15 to 17, or stacked batteries as described in claim 18. An encapsulation layer is used to cover the surface of the battery string; A cover plate is used to cover the surface of the encapsulation layer that faces away from the battery string.

20. An apparatus for manufacturing a back contact battery, characterized in that, include: An acquisition module is used to acquire a substrate, the substrate comprising alternating first and second regions; A first manufacturing module is used to form a first texture structure on the substrate surface in the second region; The second manufacturing module is used to form a first passivated conductive structure on the first region, a second passivated conductive structure on the second region, a first transparent conductive layer on the surface of the first passivated conductive structure, and a second transparent conductive layer on the surface of the second passivated conductive structure; the second passivated conductive structure covers the first textured structure; the surface of the first transparent conductive layer includes a plurality of first spherical grains and first plate-like grains; the surface of the second transparent conductive layer includes second spherical grains.