A light control film for photovoltaic modules, a method of making and use in photovoltaic modules
By setting a transparent microstructure layer on the light guide film and adjusting the refractive index, the reflected light path is changed, which solves the problems of excessive reflection angle and insufficient light deflection in the light guide film, improves the photoelectric conversion efficiency and power output of photovoltaic modules, enhances the ability to capture light at low incident angles, and reduces the risk of short circuits in the modules.
Patent Information
- Application Number
- CN202611314219.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-27
- Publication Date
- 2026-11-24
AI Technical Summary
In existing photovoltaic modules, the light guide film has problems such as excessive reflection angle, insufficient light deflection, limited light capture ability at low incident angles, easy wear of the metal reflective layer, and risk of short circuit in the module, resulting in insufficient power generation efficiency and output power of photovoltaic modules.
A transparent microstructure layer is set on the optical microstructure layer of the traditional light guide film. By adjusting the refractive index and microstructure arrangement of the transparent microstructure layer, the reflected light path and incident angle are changed to enhance the total internal reflection effect. An insulating protective layer is set on the surface of the transparent microstructure layer to prevent wear of the metal reflective layer.
It improves the photoelectric conversion efficiency and power output of photovoltaic modules, enhances the ability to capture light at low incident angles, reduces light loss, lowers the risk of module short circuit, and improves light utilization and module power.
Smart Images

Figure CN123164889A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of photovoltaic module technology, and in particular to a dimming film for photovoltaic modules, its preparation method, and its application in photovoltaic modules. Background Technology
[0002] Solar energy is a clean and renewable energy source, and photovoltaic (PV) modules can directly convert solar energy into electricity. However, the cost of PV power generation is still higher than that of traditional thermal power generation. Therefore, increasing the output power per unit area of PV modules is one of the most effective ways to reduce the cost of PV power generation.
[0003] During the manufacturing process of photovoltaic modules, to reduce the breakage rate during lamination and other module processes, and also for process simplicity and module aesthetics, photovoltaic modules have gaps of 3-5mm between cells and between strings. Calculated across the entire module, the area of these gaps accounts for 4-5% of the module's area. These areas are part of the module's area and can transmit sunlight. Although the inner surface of traditional photovoltaic glass has an irregular embossed structure, it cannot effectively guide the sunlight transmitted through these areas to the cell area for absorption and utilization; therefore, its contribution to the module's power generation is negligible.
[0004] Currently, the industry is improving the solar energy utilization efficiency of solar cells by introducing light guide films into photovoltaic modules. For example, Trina Solar Co., Ltd. has disclosed a reflective gap film (authorization announcement number CN220400607U), which adopts a segmented structure, including a first reflective segment of insulating reflective material and a second reflective segment of reflective material. This segmented design ensures maximum output power of the module. Another technical solution uses a double-sided reflective protective coating structure (authorization announcement number CN221327727U), with metal coatings on both the upper surface of the light guide layer and the lower surface of the substrate layer to improve reflectivity and substrate protection. In addition, conventional light guide films often use a single-layer aluminum-coated microprism structure, which reflects light onto the photovoltaic module glass through the prism surface reflective layer and guides it to the solar cell through total internal reflection.
[0005] However, the above-mentioned existing technologies still have the following problems: (1) The light guide film with a single-layer aluminum-plated microprism structure has insufficient light deflection and cannot effectively guide the high-efficiency area of the battery cell. The reflection angle is too large, and some reflected light leaks out of the module due to insufficient flatness of the photovoltaic patterned glass surface, making it difficult to completely enter the glass interior for propagation; (2) The directional reflected light is relatively concentrated. The light reflected to both sides at a specific position will be blocked by the cross section and edge of the battery cell, resulting in extremely low light efficiency in the local area. As the gap between the photovoltaic module cells continues to decrease, this phenomenon becomes increasingly serious; (3) The ability to capture low incident angle light is limited. Under low incident angle illumination conditions such as early morning or evening, some light escapes from the module after being reflected twice or more on the aluminum-plated inclined surface, resulting in a decrease in light guide efficiency; (4) In the production of the light guide film, each process will cause wear to the metal reflective layer on the surface of the light guide film during coating and subsequent processes, resulting in a reduction in reflection effect; (5) With the industry's EVA thinning and the rise of BC modules, the use of existing light guide films in photovoltaic modules poses a risk of short circuits in the modules.
[0006] Therefore, there is an urgent need for a new type of optical structure film that can effectively reduce the reflection angle and adjust and maintain the efficient light propagation direction to achieve efficient light collection and deflection, so as to further improve the power generation efficiency and overall power output of photovoltaic modules under different incident angles. Summary of the Invention
[0007] Based on the technical problems existing in the background art, this invention proposes a dimming film for photovoltaic modules, its preparation method, and its application in photovoltaic modules. By setting a transparent microstructure layer on the basis of the optical microstructure layer of a traditional light guide film, and adjusting the refractive index and microstructure arrangement of the transparent microstructure layer, the incident sunlight that originally directly hit the optical microstructure layer is refracted by the transparent microstructure layer, changing the incident angle and the exit angle. This achieves the effect of changing the reflected light path and reducing the reflection angle. Ultimately, the sunlight reflected by the optical microstructure layer to the front glass can be reflected to the high-efficiency power generation area of the solar cell at a higher incident angle and with the optimal light path. This avoids the loss of sunlight due to penetration of glass or reflection to the ineffective or inefficient areas of the photovoltaic cell (the cut section of the photovoltaic cell, the perimeter of the photovoltaic cell) in traditional light guide films. This increases the total amount of light illuminating the high-efficiency power generation area of the solar cell, thereby improving the photoelectric conversion efficiency and output power of the photovoltaic module and increasing the power generation.
[0008] The present invention proposes a dimming film for photovoltaic modules, including an optical microstructure layer, which is used to directionally reflect sunlight that shines on the optical microstructure layer to the front glass of the photovoltaic module, and then to be totally reflected to the surface of the solar cell by the interface between the front glass and the air. The dimming film also includes a transparent microstructure layer located on the surface of the optical microstructure layer; the refractive index of the transparent microstructure layer is greater than the refractive index of the encapsulation film layer of the photovoltaic module located on the surface of the transparent microstructure layer, and its surface is an inclined transmission structure. The transparent microstructure layer is used to refract sunlight that has been incident on the optical microstructure layer before it is directionally reflected onto the front glass, so that the incident angle of the sunlight after directional reflection by the optical microstructure layer onto the front glass is increased.
[0009] In this invention, a transparent microstructure layer is disposed on the optical microstructure layer. When incident sunlight passes through the transparent microstructure layer for the first time, the angle of incidence is changed by refraction (the light enters the high-refractive-index material from the low-refractive-index material). After being reflected by the reflective layer, the light passes through the transparent microstructure layer for the second time and is refracted again, changing the exit angle (the light enters the low-refractive-index material from the high-refractive-index material). This changes the reflected light path and reduces the reflection angle. At the same time, the refractive index of the transparent microstructure layer is greater than that of the encapsulating film layer located on the surface of the transparent microstructure layer. A refractive index difference interface is formed between the transparent microstructure layer and the encapsulating film layer, allowing the reflected light to hit the front glass at a larger angle of incidence, enhancing the total internal reflection effect, avoiding light loss due to light penetration through the glass, and ensuring that the reflected light is reflected to the high-efficiency area of the photovoltaic cell at the optimal angle and along the optimal light path.
[0010] Preferably, when the encapsulating film layer is an EVA film layer or a POE film layer, the refractive index of the transparent microstructure layer is 1.52-1.70, more preferably 1.55-1.65.
[0011] Preferably, the inclined transmission structure is at least one of a triangular prism, a semi-elliptic, a triangular pyramid, a cone, or a pyramid.
[0012] In this invention, the surface of the transparent microstructure layer is an inclined transmission structure. Compared with the planar transmission structure, the latter causes a large amount of sunlight that has been directionally reflected by the optical microstructure layer to undergo total internal reflection at the interface between the transparent microstructure layer and the encapsulating film. This results in repeated reflection and loss of a large amount of light between the planar transparent structure layer and the optical microstructure layer, preventing the light from reaching the front glass of the photovoltaic module and causing a significant loss of light.
[0013] Preferably, the surface of the optical microstructure layer is an oblique reflective structure, and the oblique reflective structure is preferably a multi-channel isosceles triangular prism structure arranged in parallel, and the geometric center line of the triangular prism structure forms an angle of 15°-175° with the length direction of the dimming film; Preferably, the apex angle of the triangular prism structure is 100°-140°; the length of the triangular base of the triangular prism structure is 15-50μm, and the thickness is 5-30μm.
[0014] In this invention, the arrangement of the triangular prism structure in the optical microstructure layer when viewed from above, with the angle between the geometric center line of the triangular prism and the cutting edge of the dimming film forming an inclination angle of 15°-175°.
[0015] Preferably, the inclined transmission structure on the surface of the transparent microstructure layer is also a continuous parallel arrangement of multiple isosceles triangular prisms. Preferably, the apex angle of the transparent microstructure layer triangular prism structure is greater than or equal to the apex angle of the optical microstructure layer triangular prism structure, and the difference between the two apex angles is preferably 0°-15°. Preferably, the length of the triangular base of the transparent microstructure layer triangular prism structure is 15-50 μm, and the thickness is 8-30 μm.
[0016] In this invention, when the apex angle of the transparent microstructure layer triangular prism structure is greater than or equal to the apex angle of the optical microstructure layer triangular prism structure, some of the sunlight directionally reflected by the optical microstructure layer is also reflected at the transparent microstructure layer. When the reflected light shines on the front glass, the incident angle is objectively increased.
[0017] Preferably, the geometric center line of the transparent microstructure layer triangular prism structure forms an angle of 0°-45° with the geometric center line of the optical microstructure layer triangular prism structure, and more preferably an angle of 15°-35°.
[0018] In this invention, the arrangement of the triangular prism structure in the transparent microstructure layer when viewed from above forms an angle of 0°-45° with the geometric center line of the triangular prism structure in the optical microstructure layer. The optical microstructure and the transparent microstructure are arranged in a rotating, intersecting, or parallel staggered configuration. The direction of light propagation can be controlled by adjusting the angle between them.
[0019] Preferably, the optical microstructure layer is composed of a microstructure layer and a metallic reflective layer deposited on the surface of the microstructure layer; Preferably, the metal reflective layer is a metal reflective layer or alloy reflective layer formed by one or a mixture of silver and aluminum; Preferably, the metal reflective layer is obtained by vapor deposition, vacuum electroplating or vacuum spraying, and the thickness of the metal reflective layer is preferably 50-100 nm, and the optical density OD value is 2.0-4.0.
[0020] Preferably, the transparent microstructure layer is an acrylic resin layer, which is formed by UV curing or thermal curing of the following raw materials in parts by weight: 20-80 parts of UV-curable resin, 20-80 parts of reactive diluent, 1-5 parts of photoinitiator, 5-25 parts of high refractive index nanofiller, and 0-10 parts of additives. The photocurable resin has a refractive index of 1.45-1.65 and is selected from at least one of polyurethane acrylate, epoxy acrylate, or polyester acrylate; the high refractive index nanofiller is selected from... , Or one or more of ZnS, with a particle size of 10-100 nm.
[0021] Preferably, the dimming film further includes a substrate layer located on the surface of the optical microstructure layer away from the transparent microstructure layer, so as to support the optical microstructure layer; Preferably, the substrate layer is a PET layer with a thickness of 15-50 μm; Preferably, the dimming film further includes an adhesive film layer located on the surface of the substrate layer away from the optical microstructure layer, so as to bond and fix the dimming film to the back sheet or back glass of the photovoltaic module. Preferably, the adhesive film layer is an EVA adhesive film layer or a POE adhesive film layer with a thickness of 50-150 μm.
[0022] The present invention also proposes a method for preparing the above-mentioned dimming film for photovoltaic modules, comprising the following steps: S1. After forming a microstructure layer on the substrate layer through a transfer process, a metallic reflective layer is deposited on the surface of the microstructure layer to obtain an optical microstructure layer. S2. A transparent microstructure layer adhesive is coated on the optical microstructure layer, and a transparent microstructure layer is formed by hot pressing or transfer printing using a mold. After curing, the dimming film for the photovoltaic module is obtained.
[0023] Preferably, in step S2, the adhesive solution for the transparent microstructure layer is prepared by the following method: mixing photocurable resin, reactive diluent, photoinitiator, high refractive index nanofiller and additives evenly, and then degassing under vacuum to obtain the adhesive solution; The adhesive is coated on the optical microstructure layer with a thickness of 10-40 μm, and the UV curing energy is 200-800 mJ / cm², or the thermal curing temperature is 80-150℃.
[0024] The present invention also proposes an application of the above-mentioned dimming film in a photovoltaic module, wherein the dimming film is located in the cell-free area of the photovoltaic module; Preferably, the cell-free area of the photovoltaic module is the cell gap area, and the cell-free area of the busbar is the perimeter or the surrounding edge.
[0025] Compared with the prior art, the beneficial effects of the present invention are as follows: In this invention, a light-regulating film with adjustable reflection angle and reflection path is formed by setting a transparent microstructure layer on the surface of the optical microstructure layer. When used in the cell-free area of a photovoltaic module, sunlight irradiated onto the light-regulating film is reflected to the high-efficiency power generation area of the photovoltaic cell at the optimal reflection angle and reflection path. Compared with traditional gap light guide films, which only include an optical microstructure layer, although the optical microstructure layer can directionally reflect transmitted light irradiated onto the optical microstructure layer through the gap area to the front glass of the photovoltaic module, and then utilize the principle of total internal reflection at the interface between the front glass and the air to make secondary use of sunlight at the edge of the cell, thereby improving the utilization rate of sunlight in the module, this type of light guide film has the following defects: (1) Because the front glass is patterned glass, the flatness of its surface makes it impossible to achieve a perfect total reflection effect. A large part of the light will inevitably pass through the photovoltaic glass and be scattered into the air, resulting in power loss of the module. (2) Due to the use of directional reflection, the light reflected to both sides at a specific position will be blocked by the cross section and edge of the cell, resulting in extremely low power generation of the cell cross section, leading to extremely low light efficiency in the local area. As the gap between the cells of the photovoltaic module continues to decrease, this phenomenon will cause increasingly serious losses. (3) The limited ability to capture light at low incident angles results in limited gain for photovoltaic modules in the early morning or evening; (4) In the production of light guide film, the metal reflective layer on the surface of the light guide film will inevitably be worn down in each process during coating and subsequent processes, resulting in reduced reflection effect and performance loss. (5) With the industry's trend of EVA thinning and the rise of BC modules, the use of light guide film in photovoltaic modules currently poses a great risk of causing module short circuits. To this end, the dimming film of the present invention further comprises a transparent microstructure layer on the surface of the optical microstructure layer. The transparent microstructure layer is used to refract the transmitted light that irradiates the optical microstructure layer before it is reflected to the front glass, thereby reducing the reflection angle of the light reflected to the front glass. In this way, the following can be achieved: (1) High light utilization rate: The double-layer refractive and reflective structure enables multi-angle light capture and redistribution, encapsulating more light within the glass for transmission. Tests show that the light-gathering film of this invention improves the gap light recovery rate by 15%-25% compared to traditional single-layer light guide films. (2) Adjustable structure: By adjusting the angle between the transparent microstructure layer and the optical microstructure layer, the light distribution can be controlled to adapt to different module structures. Through optical simulation, most of the incident light can be refracted and the reflection angle can be reduced to ≤30°, reducing the impact of the cell cross-section and the solder ribbon shadow area on the reflected light, and the module power can be increased by about 1.5%-3.5%; (3) Enhance the response of low-angle reflected light: Lowering the reflection angle lengthens the total internal reflection path of light. At the same time, it changes the incident angle of the incident light and the reflection angle of the reflected light, thus changing the propagation path of the light. The distance that the light can propagate in the glass increases by 2-4 times, and more light is reflected to the middle position of the solar cell. (4) Protection: A transparent microstructure layer is applied to the surface of the metal reflective layer to prevent wear of the metal reflective layer during the subsequent processing and application of the dimming film; (5) Insulation function: The transparent microstructure layer set on the metal reflective layer also has an insulation effect. The transparent microstructure layer with a thickness of 8-30μm can provide insulation performance with a withstand voltage of ≥1500V, avoiding short circuit of the module, and is especially suitable for new photovoltaic modules such as BC module and TOPCon module. Attached Figure Description
[0026] Figure 1 This is a schematic diagram of the structure of a photovoltaic module; Figure 2 A schematic diagram of the structure of a traditional light guide film for photovoltaic modules; Figure 3 This is a schematic diagram of the structure of the dimming film for photovoltaic modules of the present invention; Figure 4 A schematic diagram of the reflected light path of a conventional light guide film for photovoltaic modules and the dimming film of this invention; Figure 5 A diagram illustrating the reflected light path of a conventional light guide film for photovoltaic modules and the dimming film of this invention; Figure 6 The diagram shows the gain effect of the reflected light path between the traditional light guide film and the dimming film of this invention for photovoltaic modules. Figure 7 This is a diagram illustrating the reflected light path of the transparent microstructure layer of the present invention, which has a planar transmission structure on its surface. Figure 8 This is a diagram illustrating the reflected light path of the transparent microstructure layer of the present invention, which has a sloping transmissive structure on its surface. Figure 9 This is a top view of the dimming film for photovoltaic modules of the present invention; Figure 10 This is a top view of the reflected light path of the dimming film for photovoltaic modules according to the present invention; Figure 11 A schematic diagram of the total internal reflection light spot of a conventional light guide film for photovoltaic modules and the dimming film of this invention; Figure 12 This is a schematic diagram of the cell arrangement of the photovoltaic module of the present invention. Detailed Implementation
[0027] like Figure 1As shown, the photovoltaic module includes a front glass 110 and a back sheet or back glass 150 disposed opposite to each other, and a solar cell layer 130 sealed between the front glass 110 and the back sheet or back glass 150. The solar cell layer 130 is encapsulated inside an encapsulating film layer, which includes an upper encapsulating film layer 120 and a lower encapsulating film layer 140. The solar cell layer 130 includes multiple solar cells arranged in an array with gaps between them and capable of transmitting sunlight. The photovoltaic module also includes at least one light guide film 160, which is disposed on the back sheet or back glass 150 and located in the gap area between two adjacent solar cells.
[0028] like Figure 2 As shown, the conventional light guide film 160 for photovoltaic modules includes an adhesive film layer 164, a substrate layer 163, and an optical microstructure layer 162 stacked sequentially from bottom to top. The adhesive film layer 164 is used to bond and fix the light guide film 160 to the back sheet or back glass 150. The adhesive film layer 164 can be an EVA adhesive film layer or a POE adhesive film layer, for example, an EVA adhesive film layer, with a thickness of 50-100μm, for example, 100μm. The substrate layer 163 is used to support the optical microstructure layer 162. The substrate layer 163 can be a PET substrate layer with a thickness of 15-50μm, for example, 25μm. The optical microstructure layer 162 is used to directionally reflect sunlight passing through the gaps in the solar cells and illuminating the optical microstructure layer 162 to the front glass 110 of the photovoltaic module, and then to be totally reflected by the interface between the front glass 110 and the air to the surface of the solar cells.
[0029] like Figure 2 As shown, the optical microstructure layer 162 can be composed of a microstructure layer 1622 and a metal reflective layer 1621 deposited on the microstructure layer 1622; the metal reflective layer 1621 can be a metal reflective layer formed of silver or aluminum or an alloy reflective layer formed of both, for example, an aluminum layer; the thickness of the metal reflective layer is 50-100nm, for example, 80nm, and the optical density OD value is 2.0-4.0, for example, 3.0.
[0030] like Figures 1-2 As shown, the surface of the optical microstructure layer 162 is a sloping reflective structure, which can realize the directional reflection of sunlight. Specifically, it can directionally reflect the transmitted light that passes through the gap of the solar cell and shines on the optical microstructure layer 162 to the interface between the front glass and the air, and at the interface, total internal reflection occurs, thereby reflecting it to the surface of the solar cell and realizing the utilization of light.
[0031] like Figure 1As shown, ideally, all sunlight passing through the gaps in the solar cells can be totally reflected onto the surface of the solar cells along reflection path a, thus improving the efficiency of the module. However, in reality, because the front glass is patterned glass, the flatness of its surface makes it impossible to achieve a perfect total reflection effect. Some sunlight will pass through the front glass along reflection path b and be scattered into the air, while a large portion of sunlight will be blocked by the solar cells along path c, or reflected to the back of the solar cells. It is impossible to achieve total reflection to the front of the solar cells, so obviously the module cannot achieve efficient utilization of sunlight.
[0032] like Figure 3 As shown, the present invention provides a dimming film for photovoltaic modules, which, in addition to the aforementioned light guide film (i.e., the adhesive film layer 164, the substrate layer 163, and the optical microstructure layer 162 stacked sequentially from bottom to top), also includes a transparent microstructure layer 161 located on the surface of the optical microstructure layer 162; the transparent microstructure layer 161 is used to refract sunlight that has been irradiated onto the optical microstructure layer 162 before it is directionally reflected onto the front glass 110, so as to increase the incident angle of the reflected light reflected onto the front glass 110.
[0033] In the dimming film for photovoltaic modules of the present invention, a transparent microstructure layer 161 is further included on the surface of the optical microstructure layer 162, and the refractive index of the transparent microstructure layer 161 is greater than the refractive index of the encapsulating film on the surface of the transparent microstructure layer 161 of the photovoltaic module. For example, when the encapsulating film is an EVA film layer (refractive index ≈ 1.48), the transparent microstructure layer 161 can be an acrylic resin layer, specifically formed by UV curing the following raw materials in parts by weight: 50 parts of polyurethane acrylate (refractive index 1.50), 30 parts of IBOA (isobornyl acrylate), 10 parts of dipentaerythritol hexaacrylate, and 3 parts of photoinitiator 184. The mixture consists of 8 parts nanoparticles (20 nm in diameter, 2.5 in refractive index), 1 part leveling agent, and 0.5 parts defoamer; at this point, the refractive index of the transparent microstructure layer 161 is 1.58.
[0034] like Figure 4As shown, by controlling the refractive index of the aforementioned transparent microstructure layer, sunlight incident on the optical microstructure layer 162 is refracted before being directionally reflected onto the front glass 110. This causes the incident sunlight, originally directly hitting the optical microstructure layer 162, to be refracted and have its angle of incidence changed the first time it passes through the transparent microstructure layer 161. The sunlight reflected by the optical microstructure layer 162 is then refracted again the second time it passes through the transparent microstructure layer 161, changing its exit angle. This not only increases the incident angle of the reflected light from the optical microstructure layer 162 to the front glass 110 (i.e., makes the angle between the directionally reflected light and the front glass much lower than the angle required for total internal reflection at the interface between the front glass and air, thus allowing for more total internal reflection), but also... To the solar cell, this reduces light leakage at the total internal reflection interface, thus achieving a better total internal reflection effect (the lower the reflection angle, the better the total internal reflection effect of the front glass), improving the utilization rate of reflected light; it can also deflect the reflected light path, changing directional reflection into local scattering, reducing the impact of the solar cell cross-section on the shading of reflected light; at the same time, it lengthens the total internal reflection light path and changes the light path angle, increasing the contact time between the light and the solar cell surface and the light absorption area, thereby increasing the light absorption rate; subsequently, it can also control the reflection of more sunlight to the middle position of the cell, further improving the photoelectric conversion efficiency; in addition, it can also avoid wear on the metal reflective layer on the surface of the dimming film, providing an insulating effect and preventing short circuits in the module.
[0035] like Figure 5 As shown in a, in traditional light guide films, the reflected light path is that sunlight is directly and directionally reflected from the optical microstructure layer to the front glass of the photovoltaic module, and then totally reflected from the interface between the front glass and the air to the surface of the solar cell.
[0036] like Figure 5 As shown in b, in the dimming film of this invention, the reflected light path is as follows: sunlight is directionally reflected by the optical microstructure layer 162, then refracted by the transparent microstructure layer 161. The reflected light will illuminate the front glass of the photovoltaic module at a larger incident angle, and then be totally reflected by the interface between the front glass and the air to the surface of the solar cell. Generally, when sunlight is directionally reflected by the optical microstructure layer 162 to the front glass, the angle between the reflected light and the front glass is less than 40°. After refraction by the transparent microstructure layer 161, when sunlight is directionally reflected by the optical microstructure layer 162 to the front glass, the angle between the reflected light and the front glass is less than 30°, or even smaller.
[0037] like Figure 6As shown, although the traditional light guide film 160 can reflect sunlight in a directional manner, the directional reflected light is more concentrated, resulting in more light being blocked by the laminated solar cells within the very small gaps in the film strip. Furthermore, the light is concentrated more on the back of the solar cells, leading to a more severe loss of light gain. In other words, the higher quality and more concentrated directional reflected light is more severely blocked due to the gaps between the modules. In contrast, the dimming film described in this invention can deflect the reflected light path, transforming directional reflection into local scattering. Therefore, more light is reflected to the front of the solar cells. From the actual reflection results, the latter reflects more light to the surface of the solar cells, resulting in a more significant module gain effect.
[0038] like Figure 7 As shown, in the dimming film of the present invention, when the surface of the transparent microstructure layer 161 is a planar transmission structure, a large amount of sunlight directionally reflected by the optical microstructure layer 162 will undergo total internal reflection at the interface between the transparent microstructure layer 161 and the encapsulating film, failing to reach the front glass of the photovoltaic module, resulting in significant light loss. Therefore, preferably, the surface of the transparent microstructure layer 161 is a sloping transmission structure, specifically a triangular prism, a semi-elliptic, a triangular pyramid, a cone, or a pyramid shape, etc.
[0039] In this invention, in order to achieve directional reflection, the transmitted light that passes through the gaps in the solar cells and illuminates the optical microstructure layer 162 is directionally reflected at an angle greater than the total reflection angle to the interface between the front glass and the air. The surface of the optical microstructure layer 162 can be a continuous parallel arrangement of multiple isosceles triangular prism structures. The apex angle of the triangular prism structure is 100°-140°, the length of the base is 15-50μm, the thickness is 5-30μm, and the angle between the geometric center line of the triangular prism structure and the length direction of the dimming film is 15°-175°.
[0040] like Figure 8 As shown, regarding the structural configuration of the aforementioned optical microstructure layer 162, the surface of the transparent microstructure layer 161 is also a continuous, parallel arrangement of multiple isosceles triangular prism structures. When the apex angle of the triangular prism structure of the transparent microstructure layer 161 is greater than or equal to the apex angle of the triangular prism structure of the optical microstructure layer 162, some of the sunlight directionally reflected by the optical microstructure layer is also reflected at the transparent microstructure layer. This reflected light objectively increases the incident angle of sunlight directionally reflected by the optical microstructure layer to the front glass. Therefore, preferably, the apex angle of the triangular prism structure of the transparent microstructure layer is greater than or equal to the apex angle of the triangular prism structure of the optical microstructure layer, and the difference between the two apex angles is preferably 0°-15°.
[0041] like Figure 9As shown, to increase the total amount of light irradiating the high-efficiency area of the solar cell, preferably, the geometric center line of the triangular prism structure of the transparent microstructure layer 161 and the geometric center line of the triangular prism structure of the optical microstructure layer 162 are at an angle of 0°-45°, preferably 15°-35°, and the length of the base of the triangle is 15-50μm and the thickness is 8-30μm. In actual operation, by adjusting the arrangement of the triangular prisms of the transparent microstructure layer 161 and the arrangement of the triangular prisms of the optical microstructure layer 162 to form different ridge angles, thereby forming a rotating cross or parallel misaligned arrangement, the effect of adjusting the direction of light propagation can be achieved.
[0042] like Figure 10 As shown in the figure, when the green dot represents the incident light source, adjusting the angle between the ridge peaks of the transparent microstructure layer 161 and the optical microstructure layer 162 adjusts the propagation angle and divergence direction of the reflected light path. Preferably, when the geometric midlines of the triangular prisms in the transparent microstructure layer 161 and the optical microstructure layer 162 are controlled to form an angle of 0°-45°, sunlight illuminating the dimming film can be reflected to the front glass of the photovoltaic module with the optimal reflection angle and path. Then, it is totally reflected from the interface between the front glass and the air to the high-efficiency area of the photovoltaic cell. This avoids the reflection of light from the traditional light guide film to the ineffective or inefficient areas of the photovoltaic cell (the cut section of the photovoltaic cell, the edges of the photovoltaic cell), ultimately increasing the total amount of light illuminating the high-efficiency area of the solar cell, thereby improving the photoelectric conversion efficiency and output power of the photovoltaic module and increasing power generation.
[0043] like Figure 11 As shown, in the conventional light guide film 160, when the surface of the optical microstructure layer 162 is a continuous parallel arrangement of multiple isosceles triangular prism structures, the vertex angle of the triangular prism structure is 120°, the length of the base is 45μm, the thickness is 10μm, and the angle between the geometric center line of the triangular prism structure and the length direction of the light guide film is 45°; using a laser pointer to pass through a convex lens and reduce the light spot to a point, it is perpendicularly incident on the laminated component gap light guide film. The light path direction and occlusion are observed, and the results are as follows. Figure 11a; In the dimming film of this invention, when the surface of the optical microstructure layer 162 is controlled to be a continuous parallel arrangement of multiple isosceles triangular prism structures, with a vertex angle of 120°, a base length of 45μm, a thickness of 10μm, and an angle of 45° between the geometric midline of the triangular prism structure and the length direction of the dimming film, and the surface of the transparent microstructure layer 161 is also a continuous parallel arrangement of multiple isosceles triangular prism structures, with a vertex angle of 122°, a base length of 50μm, a thickness of 12μm, and angles of 0° and 15° between the geometric midline of the transparent microstructure layer 161 and the geometric midline of the optical microstructure layer 162, respectively; similarly, a laser pointer is used to pass through a convex lens to reduce the light spot to a point, and then it is perpendicularly incident on the dimming film between the laminated components. The light path direction and the occlusion situation are observed, and the results are as follows. Figure 11 b and 11c.
[0044] contrast Figure 11 The results from AC show that when the laser pointer spot falls in the middle of the gap light guide film or the dimming film, there are total reflection spots on both sides. However, the total reflection spot of the traditional light guide film with only the optical microstructure layer 162 is not obvious and the light intensity is weak. In contrast, the total reflection spot of the dimming film of the present invention, which has both the optical microstructure layer 162 and the transparent microstructure layer 161, is more obvious. More light is concentrated on the surface of the solar cell, resulting in a more significant gain effect on the module.
[0045] like Figure 12 As shown, the present invention also provides a schematic diagram of the cell arrangement of a photovoltaic module, which intuitively shows that the cell-free area of the photovoltaic module can specifically be the cell-free area 1 of the busbar, the cell gap area 2, and the surrounding edges 3.
[0046] This invention also provides a method for preparing a dimming film for photovoltaic modules, comprising: S1. Preparation of PET substrate layer: In this step, A / B / A co-extrusion, biaxial stretching, and heat setting are used to obtain the PET substrate layer; S2. Fabrication of optical microstructure layers: In this step, UV adhesive is coated on the PET substrate, and a sloping structure layer with a triangular prism structure is molded on the UV-molded surface. A metallic reflective layer is prepared on the surface of the sloping structure layer by deposition evaporation, vacuum electroplating, and vacuum spraying processes. S3. Preparation of the adhesive film layer: In this step, an EVA or POE adhesive layer is coated or laminated onto the other surface of the PET substrate. S4. Preparation of transparent microstructure layer: In this step, an adhesive is applied to the optical microstructure layer and the desired transparent microstructure is cured by hot pressing with a mold or UV molding; or a thermosetting adhesive or UV adhesive is applied to the reflective layer and the desired transparent structure is cured by roller pressing; or a thermosetting adhesive or UV adhesive is applied to the reflective layer to bond the microstructure film, roll-to-roll transfer is performed and cured, and then the microstructure film is peeled off to transfer the desired transparent microstructure onto the reflective layer.
[0047] Example 1
[0048] A dimming film for photovoltaic modules, in addition to the aforementioned structure of a conventional light guide film (i.e., the adhesive film layer 164, the substrate layer 163, and the optical microstructure layer 162 stacked sequentially from bottom to top), also includes a transparent microstructure layer 161 located on the surface of the optical microstructure layer 162. The transparent microstructure layer 161 has a refractive index of 1.58 and is specifically an acrylic resin layer, which is formed by UV curing of the following raw materials in parts by weight: 50 parts of polyurethane acrylate (refractive index 1.50), 30 parts of IBOA (isobornyl acrylate), 10 parts of dipentaerythritol hexaacrylate, 3 parts of photoinitiator 184, 8 parts of TiO2 nanoparticles (particle size 20nm, refractive index 2.5), 1 part of leveling agent, and 0.5 parts of defoamer; The surface of the transparent microstructure layer 161 is a continuous parallel arrangement of multiple isosceles triangular prism structures. The vertex angle of the triangular prism structure is 125°, the length of the base of the triangle is 40 μm, and the thickness is 15 μm. The surface of the optical microstructure layer 162 is also a continuous parallel arrangement of multiple isosceles triangular prism structures. The vertex angle of the triangular prism structure is 120°, the length of the base of the triangle is 26 μm, and the thickness is 12 μm. The geometric center line of the triangular prism structure makes an angle of 45° with the length direction of the dimming film. The geometric midline of the transparent microstructure layer 161 triangular prism structure forms a 25° angle with the geometric midline of the optical microstructure layer 162 triangular prism structure.
[0049] Example 2
[0050] The only difference between this embodiment and Embodiment 1 is the apex angle of the triangular prism structure of the transparent microstructure layer 161. Five sets of dimming film samples with apex angles of 120°, 125°, 130°, 135°, and 140° of the triangular prism of the transparent microstructure layer 161 were prepared, with other parameters the same as in Embodiment 1. Each set of dimming films was placed in a photovoltaic module, and the module power gain was tested. The results are shown in Table 1 below.
[0051] Table 1. Power gain of components with different apex angles of the triangular prism
[0052] As shown in Table 1, the power gain of the component is the largest, 3.5W, when the apex angle of the transparent microstructure layer is 130°; when the apex angle of the transparent microstructure layer is equal to that of the optical microstructure layer (120°), the gain is 2.8W; when the apex angle is too large (140°), the gain decreases; therefore, the apex angle of the transparent microstructure layer is preferably 125°-135°.
[0053] Example 3
[0054] The only difference between this embodiment and Embodiment 1 is the angle between the geometric center line of the triangular prism structure of the transparent microstructure layer 161 and the geometric center line of the triangular prism structure of the optical microstructure layer 162. Five sets of dimming film samples with angles of 0°, 15°, 25°, 35°, and 45° were prepared, with other parameters the same as in Embodiment 1. Each set of dimming films was placed in a photovoltaic module, and a monochromatic high-collimation beam (wavelength 650-670nm) was emitted by a laser generator in a dark room, penetrating the front glass to illuminate the surface of the dimming film. The current generated by the solar cell layer was detected, and the results are shown in Table 2.
[0055] Table 2 Current gain effect at different angles
[0056] As shown in Table 2, the current gain is optimal when the included angle is 25°. When the included angle is 0°, the two prisms are arranged in parallel, resulting in a decrease in gain. When the included angle is too large (45°), the optical path is excessively deflected, and some light rays deviate from the effective area of the solar cell, leading to a decrease in gain.
[0057] Example 4
[0058] The only difference between this embodiment and Example 1 is the type and amount of high-refractive-index nanofiller in the transparent microstructure layer. Five groups of dimming film samples were prepared, and the measured refractive indices of the transparent microstructure layers of each group were 1.58, 1.56, 1.59, 1.62, and 1.49, respectively. Each group of dimming films was placed in a photovoltaic module, and the power gain of the module was tested. The results are shown in Table 3.
[0059] Table 3 Power gain of components with different fillers
[0060] As shown in Table 3, adding high refractive index nanofillers can significantly improve the power gain of the components. The gain effect is best when the refractive index is 1.58-1.59. When the refractive index is too low (1.49), the difference between the refractive index and the refractive index of the encapsulating film is insufficient, and the gain is limited. When the refractive index is too high (1.62), it may lead to an increase in interface reflection loss, and the gain will decrease instead.
[0061] Example 5
[0062] The dimming film described in Example 1 and the traditional light guide film were subjected to long-term reliability comparison tests. The test conditions and results are shown in Table 4.
[0063] Table 4 Long-term reliability test results
[0064] As shown in Table 4, the dimming film of this invention, due to the transparent microstructure layer covering the surface of the metal reflective layer, provides excellent protection and significantly outperforms traditional light guide films in long-term reliability testing. Particularly in the insulation withstand voltage test, traditional light guide films, with their directly exposed aluminum metal layer, are at risk of insulation failure, while the dimming film of this invention passed all tests.
[0065] Example 6
[0066] This embodiment provides three methods for preparing transparent microstructure layers: Method 1 (Mold Hot Pressing Method): A thermosetting adhesive (60 parts epoxy acrylate resin, 30 parts reactive diluent, 2 parts thermosetting agent, and 10 parts TiO2 nanofiller) is coated on the optical microstructure layer to a thickness of 20 μm. The coating is then hot-pressed using a precision mold (temperature 120℃, pressure 0.5 MPa, time 5 min). After thermosetting, the mold is peeled off to obtain a transparent microstructure layer.
[0067] Method 2 (UV Transfer Method): Coat the optical microstructure layer with UV adhesive (50 parts polyurethane acrylate, 30 parts IBOA, 10 parts dipentaerythritol hexaacrylate, 3 parts photoinitiator 184). The coating consists of 8 parts nanofiller, 1 part leveling agent, and 0.5 parts defoamer, with a thickness of 15 μm. It is then imprinted using a UV transfer mold with a UV curing energy of 500 mJ / cm². After peeling off the mold, a transparent microstructure layer is obtained.
[0068] Method 3 (Thin Film Transfer Method): Apply UV adhesive (12μm thickness) to the optical microstructure layer, attach a PET film with microstructure, roll it with a roller (pressure 0.3MPa), UV curing energy 400mJ / cm², peel off the PET film, and transfer the microstructure onto the optical microstructure layer.
[0069] The power gains of the dimming film components prepared by the three methods are as follows: Method 1 3.0W, Method 2 3.2W, and Method 3 2.8W. Method 2 (UV transfer method) has the best results, while Method 3 has a slightly lower gain due to possible microstructure deformation during the transfer process.
[0070] Example 7
[0071] The only difference between this embodiment and Example 1 is the thickness of the transparent microstructure layer. Five groups of dimming film samples with thicknesses of 8μm, 12μm, 15μm, 20μm, and 30μm were prepared, with other parameters the same as in Example 1. The component power gain and insulation withstand voltage performance of each group of samples were tested, and the results are shown in Table 5.
[0072] Table 5 Performance of transparent microstructure layers with different thicknesses
[0073] As shown in Table 5, when the thickness of the transparent microstructure layer is 12-20 μm, the power gain and insulation performance of the module are well balanced; when the thickness is too thin (8 μm), the insulation performance is insufficient; when the thickness is too thick (30 μm), the absorption loss increases due to the increased optical path, and the power gain decreases.
[0074] Example 8 The dimming film described in Example 1 was applied to a BC (back contact) module. BC modules, lacking front-side grid lines, require higher insulation performance. Test results showed that the BC module using the dimming film of this invention achieved a power gain of 3.0W and passed the 1500V insulation withstand voltage test; while in BC modules using traditional light guide films, insulation failure occurred in 3 / 10 of the samples, with a power gain of only 2.5W. The dimming film of this invention exhibits significant advantages in insulation and power gain in BC modules.
[0075] Example 9
[0076] Under simulated low incident angle (solar altitude angle 15°-30°) conditions at dawn / dusk, the optical gain of the dimming film described in Example 1 and the traditional light guide film were tested. The results showed that the power gain of the dimming film described in Example 1 was 2.5W under low incident angle conditions, while the traditional light guide film was only 1.2W. The dimming film of this invention, through the refraction of the transparent microstructure layer, effectively changes the propagation path of light at low incident angles, allowing more light to enter the glass interior for total internal reflection, significantly improving light utilization under low incident angle conditions.
[0077] Example 10
[0078] The only difference between this embodiment and Embodiment 1 is the surface shape of the transparent microstructure layer. Transparent microstructure layers with five different surface shapes—triangular prism, semi-elliptic, triangular pyramid, conical, and pyramidal—were prepared, with other parameters identical to those in Embodiment 1. Each set of dimming films was placed in a photovoltaic module, and the module power gain was tested. The results are shown in Table 6.
[0079] Table 6 Power gain of components with different microstructure shapes
[0080] As shown in Table 6, the triangular prism and pyramidal transparent microstructure layers exhibit better power gain. The semi-elliptical and conical shapes have slightly lower gains due to the greater difficulty in controlling the refraction angle. The triangular prism shape is the preferred option due to its mature manufacturing process and controllable structure.
[0081] Example 11
[0082] The only difference between this embodiment and Embodiment 1 is the gap width between the photovoltaic module cells. Four sets of photovoltaic modules with gap widths of 1mm, 2mm, 3mm, and 5mm were prepared respectively. The dimming film of Embodiment 1 was cut to the corresponding width and placed in the gap area of each module. The power gain of the modules was tested, and the results are shown in Table 7.
[0083] Table 7 Power gain of components with different gap widths
[0084] As shown in Table 7, the absolute value of the component power gain increases with the increase of the gap width, but the gain efficiency per unit area decreases. Under the condition of a 1mm gap, the dimming film of the present invention can still achieve a power gain of 3.2W, proving that it is suitable for the current industry trend of small gap (zero pitch) components.
[0085] Example 12
[0086] The dimming film prepared in Example 1 was applied to a TOPCon (tunneling oxide passivated contact) module. The TOPCon module uses 182mm × 182mm solar cells, with 72 cells connected in series and a gap width of 2.0mm. Test results show that the TOPCon module using the dimming film described in Example 1 has a power gain of 3.6W and a module conversion efficiency improvement of 0.35%; while the TOPCon module using a traditional light guide film has a power gain of 2.1W. The dimming film of this invention exhibits excellent gain performance in TOPCon modules and passes the 2000V insulation withstand voltage test, meeting the high-voltage operation requirements of TOPCon modules.
[0087] Example 13
[0088] The dimming film described in Example 1 was applied to an HJT (heterojunction) module. The HJT module used 210mm × 210mm solar cells, with 60 cells connected in series and a gap width of 2.5mm. Test results showed that the HJT module using the dimming film of this invention had a power gain of 4.2W and a 0.42% improvement in module conversion efficiency; while the HJT module using a traditional light guide film had a power gain of 2.5W. HJT modules are more sensitive to light utilization; the dimming film of this invention, through double-layer microstructure refraction, significantly improves the light-harvesting capability of the HJT module.
[0089] Example 14 The only difference between this embodiment and Embodiment 1 is the material of the metal reflective layer 1621. Two types of metal reflective layers, aluminum and silver, were prepared, each with a thickness of 80 nm, while other parameters remained the same as in Embodiment 1. The reflectivity, component power gain, and cost of each dimming film were tested, and the results are shown in Table 8.
[0090] Table 8. Performance Comparison of Different Metal Reflective Layer Materials
[0091] As shown in Table 8, the silver layer has the highest reflectivity but a higher cost; the aluminum layer has the lowest cost but a slightly lower reflectivity. Considering both performance and cost, the aluminum layer is the preferred option.
[0092] Example 15
[0093] The only difference between this embodiment and Embodiment 1 is that... The nanofillers have different particle sizes. Five groups of dimming film samples with particle sizes of 10nm, 20nm, 50nm, 80nm, and 100nm were prepared respectively. The dosage was 8 parts for each sample, and other parameters were the same as in Example 1. The refractive index, haze, and power gain of the transparent microstructure layer of each group of samples were tested, and the results are shown in Table 9.
[0094] Table 9. Performance Comparison of Different Nanofiller Particle Sizes
[0095] As shown in Table 9, when the nanofiller particle size is 10-20 nm, the refractive index of the transparent microstructure layer is significantly improved and the haze is low, resulting in the best module power gain. When the particle size is too large (≥50 nm), the light scattering effect is enhanced, the haze increases significantly, leading to a white appearance of the module and a decrease in power gain. Therefore, the preferred nanofiller particle size is 10-30 nm.
[0096] Example 16
[0097] The dimming film described in Example 1 and the traditional light guide film were applied to 72 M10 (182mm) PERC modules and 78 G12 (210mm) TOPCon modules, respectively. The electrical performance parameters of the modules were tested under standard test conditions (STC: 1000W / m², AM1.5, 25℃), and the results are shown in Table 10.
[0098] Table 10 Actual Power Test of Large-Scale Components
[0099] As shown in Table 10, after using the dimming film of this invention, the maximum power Pmax of 72 M10 PERC modules increased from 555.2W to 562.1W, the gain was 6.9W, and the conversion efficiency increased from 21.35% to 21.62%. Compared with the traditional light guide film (gain 3.3W), the gain of the dimming film of this invention is increased by about 109%. After using the dimming film of this invention, the conversion efficiency of 78 G12 TOPCon modules reached 22.85%, demonstrating excellent large-scale application performance.
[0100] Example 17
[0101] The dimming film described in Example 1 was applied to a bifacial double-glass PERC module, with a transparent backsheet glass on the back of the bifacial module. The power gain on the front side, the power gain on the back side, and the bifaciality were tested, and the results are shown in Table 11.
[0102] Table 11 Application Testing of Bifacial Modules
[0103] As shown in Table 11, the traditional light guide film suffers from a 0.8W decrease in back-side power and a double-sided factor of 71.2% due to the obstruction of back-side incident light by the metal reflective layer. In contrast, the dimming film of this invention reduces the obstruction of back-side incident light due to the presence of the transparent microstructure layer, resulting in a back-side power decrease of only 0.3W and a double-sided factor maintained at 72.1%. The overall gain is 3.2W, which is superior to the 2.4W of the traditional light guide film.
[0104] Based on the above description, the dimming film of this invention has the following advantages compared with traditional single-layer light guide films: the module power gain is increased by 1.5-3.5W (PERC) and 3.0-4.2W (TOPCon / HJT); the gap light recovery utilization rate is increased by 15%-25%; the gain is increased by about 1 times under low incident angle conditions; the long-term reliability is significantly improved, and the power attenuation is reduced by more than 50%; the insulation performance is excellent, and it is suitable for new photovoltaic modules such as BC modules and TOPCon modules; the bifacial factor loss in bifacial modules is reduced by more than 60%.
[0105] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.
Claims
1. A dimming film for photovoltaic modules, comprising an optical microstructure layer for directionally reflecting sunlight irradiated by the optical microstructure layer onto the front glass of the photovoltaic module, and then totally reflecting it onto the surface of the solar cells through the interface between the front glass and the air. Its features are, The dimming film also includes a transparent microstructure layer located on the surface of the optical microstructure layer; the refractive index of the transparent microstructure layer is greater than the refractive index of the encapsulation film layer of the photovoltaic module located on the surface of the transparent microstructure layer, and its surface is an inclined transmission structure. The transparent microstructure layer is used to refract sunlight that has been incident on the optical microstructure layer before it is directionally reflected onto the front glass, so that the incident angle of the sunlight after directional reflection by the optical microstructure layer onto the front glass is increased.
2. The dimming film for photovoltaic modules according to claim 1, characterized in that, When the encapsulating film layer is an EVA film layer or a POE film layer, the refractive index of the transparent microstructure layer is 1.52-1.70, preferably 1.55-1.
65.
3. The dimming film for photovoltaic modules according to claim 1 or 2, characterized in that, The inclined transmission structure is at least one of the following: triangular prism, semi-elliptic, triangular pyramid, cone, or pyramid.
4. The dimming film for photovoltaic modules according to any one of claims 1-3, characterized in that, The surface of the optical microstructure layer is an oblique reflective structure. The oblique reflective structure is preferably a multi-channel isosceles triangular prism structure arranged in parallel, and the geometric center line of the triangular prism structure forms an angle of 15°-175° with the length direction of the dimming film. Preferably, the apex angle of the triangular prism structure is 100°-140°; the length of the triangular base of the triangular prism structure is 15-50μm, and the thickness is 5-30μm.
5. The dimming film for photovoltaic modules according to claim 4, characterized in that, The oblique transmission structure on the surface of the transparent microstructure layer is also a continuous parallel arrangement of multiple isosceles triangular prisms. Preferably, the apex angle of the transparent microstructure layer triangular prism structure is greater than or equal to the apex angle of the optical microstructure layer triangular prism structure, and the difference between the two apex angles is preferably 0°-15°. Preferably, the length of the triangular base of the transparent microstructure layer triangular prism structure is 15-50 μm, and the thickness is 8-30 μm.
6. The dimming film for photovoltaic modules according to claim 4 or 5, characterized in that, The geometric center line of the transparent microstructure layer triangular prism structure forms an angle of 0°-45° with the geometric center line of the optical microstructure layer triangular prism structure, preferably an angle of 15°-35°.
7. The dimming film for photovoltaic modules according to any one of claims 1-6, characterized in that, The optical microstructure layer consists of a microstructure layer and a metallic reflective layer deposited on the surface of the microstructure layer; Preferably, the metal reflective layer is a metal reflective layer or alloy reflective layer formed by one or a mixture of silver and aluminum; the thickness of the metal reflective layer is 50-100nm, and the optical density OD value is 2.0-4.
0.
8. The dimming film for photovoltaic modules according to any one of claims 1-7, characterized in that, The transparent microstructure layer is an acrylic resin layer, which is formed by UV curing or thermal curing of the following raw materials in parts by weight: 20-80 parts of UV-curable resin, 20-80 parts of reactive diluent, 1-5 parts of photoinitiator, 5-25 parts of high refractive index nanofiller, and 0-10 parts of additives. The photocurable resin has a refractive index of 1.45-1.65 and is selected from at least one of polyurethane acrylate, epoxy acrylate or polyester acrylate; the high refractive index nanofiller is selected from at least one of TiO2, ZrO2 or ZnS and has a particle size of 10-100 nm.
9. The dimming film for photovoltaic modules according to any one of claims 1-8, characterized in that, The dimming film also includes a substrate layer located on the surface of the optical microstructure layer away from the transparent microstructure layer; Preferably, the substrate layer is a PET layer with a thickness of 15-50 μm; The dimming film also includes an adhesive film layer located on the surface of the substrate layer away from the optical microstructure layer; Preferably, the adhesive film layer is an EVA adhesive film layer or a POE adhesive film layer with a thickness of 50-150 μm.
10. A method for preparing a dimming film for a photovoltaic module according to any one of claims 1-9, characterized in that, Includes the following steps: S1. After forming a microstructure layer on the substrate layer through a transfer process, a metallic reflective layer is deposited on the surface of the microstructure layer to obtain an optical microstructure layer. S2. A transparent microstructure layer adhesive is coated on the optical microstructure layer, and a transparent microstructure layer is formed by hot pressing or transfer printing using a mold. After curing, the dimming film for the photovoltaic module is obtained.
11. The method for preparing a dimming film for photovoltaic modules according to claim 10, characterized in that, In step S2, the adhesive solution for the transparent microstructure layer is prepared by the following method: the photocurable resin, reactive diluent, photoinitiator, high refractive index nanofiller and additives are mixed evenly, and the adhesive solution is obtained after vacuum degassing. Preferably, the coating thickness of the adhesive on the optical microstructure layer is 10-40 μm, the UV curing energy is 200-800 mJ / cm², or the thermal curing temperature is 80-150℃.
12. An application of the dimming film according to any one of claims 1-9 in a photovoltaic module, wherein the dimming film is located in the cell-free area of the photovoltaic module; the cell-free area of the photovoltaic module is preferably the cell gap area, the cell-free area of the busbar, or the perimeter.
Citation Information
Patent Citations
Reflective gap film and photovoltaic module
CN220400607U
Gap light guide film with double-sided reflective protective coating structure for photovoltaic module