Full-color light emitting diode chip and method of manufacturing the same

By setting sub-pixel regions with varying porosity gradients in a full-color LED chip, and utilizing lattice stress release capabilities, red, green, and blue light emission is achieved in the same epitaxial process. This solves the problems of cumbersome steps and thermal budget accumulation in existing technologies, ensuring the uniformity of the active layer and the light emission effect.

CN123164897APending Publication Date: 2026-11-24HC SEMITEK ZHEJIANG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611655292.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-26
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

In existing technologies, the selective epitaxial growth process of monolithic full-color integrated Micro-LED display technology is cumbersome, and multiple high-temperature epitaxial growths lead to thermal accumulation, affecting the performance of the active layer.

Method used

In a full-color light-emitting diode chip, by setting first, second, and third sub-pixel regions arranged at intervals on a first semiconductor layer, and setting pores with progressively increasing porosity in each region, a source layer is stacked in the same epitaxial process by utilizing the lattice stress release capability of gradient change, thereby achieving red, green, and blue light emission.

Benefits of technology

It achieves monolithic integration of three-color full-color light emission, avoiding the heat budget accumulation problem caused by multiple shading and staged epitaxial growth, and ensuring the uniformity of crystal quality and light emission effect of the active layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123164897A_ABST
    Figure CN123164897A_ABST
Patent Text Reader

Abstract

This disclosure provides a full-color light-emitting diode (LED) chip and its fabrication method, belonging to the field of semiconductor fabrication technology. The full-color LED chip includes a first semiconductor layer, an active layer, and a second semiconductor layer stacked sequentially. The first semiconductor layer has a first sub-pixel region, a second sub-pixel region, and a third sub-pixel region arranged at intervals on one side facing the active layer. Each of the first, second, and third sub-pixel regions has multiple pores, and the porosity of the first, second, and third sub-pixel regions increases sequentially. This disclosure avoids the need for multiple high-temperature epitaxial growth processes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure belongs to the field of semiconductor fabrication technology, and specifically relates to a full-color light-emitting diode chip and its fabrication method. Background Technology

[0002] Micro-LED (Micro Light Emitting Diode) display technology has garnered widespread attention in the fields of micro-displays and high-definition displays due to its characteristics such as high brightness, low power consumption, and high contrast. In Micro-LED display technology, achieving full-color integration of red, green, and blue LEDs on a single chip is a crucial direction for promoting its large-scale application.

[0003] In related technologies, the monolithic full-color integrated solution mainly adopts the selective epitaxial growth process. This process involves multiple masking operations and staged epitaxial growth to fabricate red, green, and blue light-emitting structures in different regions of the same wafer.

[0004] However, the selective epitaxial growth process is quite complicated, and the cumulative thermal budget caused by multiple high-temperature epitaxial growths can easily lead to performance degradation of the grown quantum wells. Summary of the Invention

[0005] This disclosure provides a full-color light-emitting diode chip and its fabrication method, which can avoid multiple high-temperature epitaxial growth processes. The technical solution is as follows: In a first aspect, embodiments of this disclosure provide a full-color light-emitting diode chip, comprising: a first semiconductor layer, an active layer, and a second semiconductor layer stacked sequentially; The first semiconductor layer has a first sub-pixel region, a second sub-pixel region, and a third sub-pixel region arranged at intervals on one side facing the active layer. Each of the first sub-pixel region, the second sub-pixel region, and the third sub-pixel region has multiple pores, and the porosity of the first sub-pixel region, the second sub-pixel region, and the third sub-pixel region increases sequentially.

[0006] In one implementation of this disclosure, the porosity of the first sub-pixel region is less than 10%; The porosity of the second sub-pixel region is 10%~20%; The porosity of the third sub-pixel region is greater than 20%.

[0007] In one implementation of this disclosure, the first sub-pixel region, the second sub-pixel region, and the third sub-pixel region are arranged in a triangular or linear pattern.

[0008] In one implementation of this disclosure, the full-color light-emitting diode chip includes an electron blocking layer; The electron blocking layer is located between the active layer and the second semiconductor layer.

[0009] Secondly, embodiments of this disclosure provide a method for fabricating a full-color light-emitting diode chip, comprising: Fabrication of the first semiconductor layer; One side of the first semiconductor layer is patterned to form a first sub-pixel region, a second sub-pixel region, and a third sub-pixel region arranged at intervals. Each of the first sub-pixel region, the second sub-pixel region, and the third sub-pixel region has multiple pores, and the porosity of the first sub-pixel region, the second sub-pixel region, and the third sub-pixel region increases sequentially. Preparation of active layer; Prepare the second semiconductor layer.

[0010] In one implementation of this disclosure, graphically representing one side of the first semiconductor layer includes: A photomask is provided, wherein the photomask has a first opening pattern, a second opening pattern and a third opening pattern arranged at intervals, the size of the first opening pattern, the second opening pattern and the third opening pattern decreasing sequentially; The first semiconductor layer is photolithographically ... The first semiconductor layer is etched based on the photoresist layer.

[0011] In one implementation of this disclosure, the size of the first opening pattern is 20~50μm; The size of the second opening pattern is 5~15μm; The size of the third opening pattern is 2~5μm.

[0012] In one implementation of this disclosure, the first opening pattern, the second opening pattern, and the third opening pattern are arranged in a triangular or linear pattern.

[0013] In one implementation of this disclosure, etching the first semiconductor layer based on the photoresist layer includes: Oxalic acid was selected as the etching solution, with a concentration of 0.2~0.3 mol / L and a temperature of 20~25℃. A constant current is applied with a current density of 1~3 mA / cm². 2 The corrosion time is 10~20 minutes.

[0014] In one implementation of this disclosure, the porosity of the first sub-pixel region is less than 10%; The porosity of the second sub-pixel region is 10%~20%; The porosity of the third sub-pixel region is greater than 20%.

[0015] The beneficial effects of the technical solutions provided in this disclosure include at least the following: The full-color light-emitting diode chip provided in this embodiment of the present disclosure has a first sub-pixel region, a second sub-pixel region, and a third sub-pixel region (hereinafter collectively referred to as the three sub-pixel regions) arranged at intervals on one side of the first semiconductor layer facing the active layer. Multiple pores with progressively increasing porosity are provided within the three sub-pixel regions, enabling different sub-pixel regions on the same first semiconductor layer to possess a gradient-varying lattice stress release capability. Thus, when the active layer is stacked on the first semiconductor layer, the first, second, and third sub-pixel regions with progressively increasing porosity can provide different degrees of stress relaxation to the active layer. During the epitaxial growth of the active layer, different degrees of stress release drive the active layer to incorporate different concentrations of In components, thereby causing the positions of the three sub-pixel regions of the active layer to naturally radiate three different wavelengths of light (such as blue light, green light, and red light).

[0016] Furthermore, since the three sub-pixel regions are located on the surface of the same first semiconductor layer, the active layer and the second semiconductor layer can be continuously stacked and formed in the same epitaxial process, avoiding the heat budget accumulation problem caused by multiple shielding and epitaxial growth in related technologies, and preventing the active layer from degrading in subsequent high-temperature processes.

[0017] In other words, the full-color light-emitting diode chip provided in this embodiment achieves three-color full-color light emission on a single chip while ensuring uniform active layer crystal quality corresponding to the three sub-pixel regions. Attached Figure Description

[0018] To more clearly illustrate the technical solutions in the embodiments of this disclosure, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of this disclosure. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0019] Figure 1 This is a schematic diagram of the structure of the full-color light-emitting diode chip provided in the embodiments of this disclosure; Figure 2 This is a partial top view of the first semiconductor layer provided in an embodiment of this disclosure; Figure 3 This is a flowchart illustrating a method for fabricating a full-color light-emitting diode chip according to an embodiment of this disclosure; Figure 4 This is a flowchart of another method for fabricating a full-color light-emitting diode chip provided in this embodiment.

[0020] The symbols in the diagram represent the following meanings: 10. First semiconductor layer; 110, First sub-pixel region; 120, Second sub-pixel region; 130, Third sub-pixel region; 140, Aperture; 20. Active layer; 30. Second semiconductor layer; 40. Electron blocking layer; 50. Substrate; 60. Buffer layer; 70. GaN layer.

[0021] The accompanying drawings have illustrated specific embodiments of this disclosure, which will be described in more detail below. These drawings and descriptions are not intended to limit the scope of the concept in any way, but rather to illustrate the concepts of this disclosure to those skilled in the art through reference to particular embodiments. Detailed Implementation

[0022] To make the objectives, technical solutions, and advantages of this disclosure clearer, the embodiments of this disclosure will be described in further detail below with reference to the accompanying drawings.

[0023] This disclosure provides a full-color light-emitting diode chip. Figure 1 See the schematic diagram of the full-color LED chip. Figure 1 In this embodiment, the full-color light-emitting diode chip includes a first semiconductor layer 10, an active layer 20, and a second semiconductor layer 30 stacked sequentially.

[0024] Figure 2 This is a partial top view of the first semiconductor layer 10, combined with... Figure 2 In this embodiment, the first semiconductor layer 10 has a first sub-pixel region 110, a second sub-pixel region 120 and a third sub-pixel region 130 arranged at intervals on one side facing the active layer 20. Each of the first sub-pixel region 110, the second sub-pixel region 120 and the third sub-pixel region 130 has a plurality of pores 140, and the porosity of the first sub-pixel region 110, the second sub-pixel region 120 and the third sub-pixel region 130 increases sequentially.

[0025] The full-color light-emitting diode chip provided in this embodiment of the present disclosure has a first sub-pixel region 110, a second sub-pixel region 120, and a third sub-pixel region 130 (hereinafter collectively referred to as sub-pixel regions) arranged at intervals on one side of the first semiconductor layer 10 facing the active layer 20. Multiple pores 140 with progressively increasing porosity are provided within the three sub-pixel regions, enabling different sub-pixel regions on the same first semiconductor layer 10 to possess a gradient-varying lattice stress release capability. Thus, when the active layer 20 is stacked on the first semiconductor layer 10, the first sub-pixel region 110, the second sub-pixel region 120, and the third sub-pixel region 130 with progressively increasing porosity can provide different degrees of stress relaxation to the active layer 20. During the epitaxial growth of the active layer 20, different degrees of stress release drive the active layer 20 to incorporate different concentrations of In components, thereby causing the active layer 20 to naturally radiate three different wavelengths of light (such as blue light, green light, and red light) corresponding to the three sub-pixel regions.

[0026] Furthermore, since the three sub-pixel regions are located on the surface of the same first semiconductor layer 10, the active layer 20 and the second semiconductor layer 30 can be continuously stacked and formed in the same epitaxial process, avoiding the heat budget accumulation problem caused by multiple shading and epitaxial growth in related technologies, and preventing the active layer 20 from degrading in subsequent high-temperature processes.

[0027] In other words, the full-color light-emitting diode chip provided in this embodiment achieves three-color full-color light emission on a single chip while ensuring uniform crystal quality of the active layer 20 corresponding to the three sub-pixel regions.

[0028] For example, the porosity of the first sub-pixel region 110 is less than 10%.

[0029] In the above implementation, the porosity of the first sub-pixel region 110 is controlled to be less than 10%, so that the first sub-pixel region 110 maintains a high lattice density and a small stress release, thereby limiting the In composition incorporation efficiency of the active layer 20 in this region and maintaining a shorter emission wavelength to stably form a blue light emission region (e.g., emission wavelength of about 450 nm).

[0030] If the porosity of the first sub-pixel region 110 is greater than or equal to 10%, the lattice stress in this region will be released too much, which will cause the active layer 20 to incorporate an excessive amount of In component, resulting in an unexpected redshift of the blue light wavelength and reducing the color purity of the blue light display.

[0031] For example, the porosity of the second sub-pixel region 120 is 10% to 20%.

[0032] In the above implementation, the porosity of the second sub-pixel region 120 is controlled within the range of 10% to 20%, so that the second sub-pixel region 120 can provide a moderate degree of lattice stress release, thereby guiding the active layer 20 to incorporate a moderate concentration of In component in this region, so that the emission wavelength is moderately red-shifted to stably form a green light emission region (e.g., emission wavelength of about 520nm).

[0033] If the porosity of the second sub-pixel region 120 is less than 10%, the stress relaxation effect in this region is weak, and the amount of In component incorporated is insufficient, causing the emission wavelength to shift towards the blue light band. Conversely, if the porosity of the second sub-pixel region 120 is greater than 20%, the stress release is too great, which can easily lead to excessive In atoms being incorporated into the active layer 20, causing the emission wavelength to shift towards the red light band and causing color crosstalk between green and red light.

[0034] For example, the porosity of the third sub-pixel region 130 is greater than 20%.

[0035] In the above implementation, the porosity of the third sub-pixel region 130 is controlled within a range greater than 20%, so that the third sub-pixel region 130 has a high micropore density and sufficient deformation space, which can release the lattice mismatch stress between the first semiconductor layer 10 and the active layer 20 more fully, thereby effectively improving the In composition incorporation efficiency of the active layer 20 in this region, causing a large red shift in the emission wavelength to stably form a red light emission region (e.g., emission wavelength of about 620nm).

[0036] If the porosity of the third sub-pixel region 130 is less than or equal to 20%, the lattice stress in this region is not sufficiently released, and the active layer 20 is difficult to incorporate a sufficiently high concentration of In component during growth, resulting in a shorter wavelength of emitted light that cannot meet the chromaticity requirements of the red light band.

[0037] See Figure 2 In this embodiment, the first sub-pixel region 110, the second sub-pixel region 120 and the third sub-pixel region 130 are arranged in a triangular or linear pattern.

[0038] In the above implementation, by setting the first sub-pixel region 110, the second sub-pixel region 120 and the third sub-pixel region 130 to be arranged in a triangular or linear pattern, the three-color light-emitting areas in a single full-color pixel unit form a regular and compact geometric layout in planar space.

[0039] For example, when the first sub-pixel region 110, the second sub-pixel region 120, and the third sub-pixel region 130 are arranged in a triangle, the three sub-pixel regions are adjacent to each other and have similar center-to-center spacing, which is beneficial for achieving uniform spatial mixing of the three colors of light within a shorter propagation distance. When the first sub-pixel region 110, the second sub-pixel region 120, and the third sub-pixel region 130 are arranged in a straight line, the sub-pixel regions are aligned sequentially along the same direction, resulting in a regular structure that simplifies the driving traces and layout design of high-density pixel arrays.

[0040] In other words, regardless of which arrangement method is adopted, it can be flexibly adapted to the specific light mixing requirements or wiring architecture of the display panel, thereby improving the display light mixing effect and layout rationality of the full-color LED chips.

[0041] Of course, in other embodiments, the first sub-pixel region 110, the second sub-pixel region 120 and the third sub-pixel region 130 may also be arranged in other shapes, such as L-shaped arrangement or arc-shaped arrangement, etc., and this disclosure does not limit them.

[0042] In this embodiment, the cross-sectional shape of the first sub-pixel region 110, the second sub-pixel region 120, and the third sub-pixel region 130 can be circular, square, or hexagonal.

[0043] In the above implementation, regular geometric shapes such as circles, squares or hexagons are used, which facilitates graphic design and array tiling on the photomask and ensures the regularity of the edge contours of each sub-pixel region.

[0044] In this embodiment, the first semiconductor layer 10 is an N-type GaN layer, the active layer 20 is a multiple quantum well (MQW) layer, and the second semiconductor layer 30 is a P-type GaN layer.

[0045] In this embodiment, the full-color light-emitting diode chip further includes a substrate 50, and a buffer layer 60 and a GaN layer 70 sequentially stacked between the substrate 50 and the first semiconductor layer 10. The substrate 50 can be a sapphire substrate.

[0046] In the above implementation, by setting a buffer layer 60 and a GaN layer 70 between the sapphire substrate and the first semiconductor layer 10, the lattice mismatch between the heterostructure and the epitaxial layer can be effectively alleviated, the through dislocation density can be reduced, and a flat epitaxial substrate with good crystal quality can be provided for the porous construction of the upper first semiconductor layer 10 and the growth of the active layer 20.

[0047] See also Figure 1In this embodiment, the full-color light-emitting diode chip includes an electron blocking layer 40. The electron blocking layer 40 is located between the active layer 20 and the second semiconductor layer 30.

[0048] In the above implementation, an electron blocking layer (EBL) 40 is placed between the active layer 20 and the second semiconductor layer 30. The high band barrier of the EBL 40 effectively blocks electron overflow. In this way, electrons are confined within the active layer 20 and undergo radiative recombination with holes, reducing non-radiative recombination losses and improving the internal quantum efficiency of the full-color LED chip.

[0049] Figure 3 This is a flowchart illustrating a method for fabricating a full-color light-emitting diode chip, as provided in this disclosure embodiment. Figure 3 In this embodiment, the preparation method includes: Step 301: Prepare the first semiconductor layer 10.

[0050] Step 302: Pattern one side of the first semiconductor layer 10 to form a first sub-pixel region 110, a second sub-pixel region 120, and a third sub-pixel region 130 arranged at intervals. Each of the first sub-pixel region 110, the second sub-pixel region 120, and the third sub-pixel region 130 has a plurality of pores 140, and the porosity of the first sub-pixel region 110, the second sub-pixel region 120, and the third sub-pixel region 130 increases sequentially.

[0051] Step 303: Prepare active layer 20.

[0052] Step 304: Prepare the second semiconductor layer 30.

[0053] The fabrication method provided in this disclosure involves fabricating a first semiconductor layer 10, followed by patterning one side to form a first sub-pixel region 110, a second sub-pixel region 120, and a third sub-pixel region 130 with progressively increasing porosity. Subsequently, an active layer 20 and a second semiconductor layer 30 are sequentially fabricated on the first semiconductor layer 10. The three sub-pixel regions with gradient porosity provide stress-relieving substrates of varying degrees for the subsequent growth of the active layer 20, allowing the active layer 20 to incorporate different concentrations of In components above different sub-pixel regions during the same epitaxial growth process, thereby achieving full-color tri-color emission. Furthermore, the active layer 20 is directly formed in the same epitaxial process, avoiding the thermal degradation risk caused by multiple selective epitaxial growth processes in related technologies and ensuring the uniformity of material quality in the three-color sub-pixel regions.

[0054] Figure 4A flowchart illustrating another method for fabricating a full-color light-emitting diode chip provided in this disclosure, in conjunction with... Figure 4 In this embodiment, the preparation method includes: Step 401: Provide a substrate 50, and sequentially fabricate a buffer layer 60, a GaN layer 70, and a first semiconductor layer 10 on the substrate 50.

[0055] The substrate 50 can be a sapphire substrate. A buffer layer 60, a GaN layer 70, and a first semiconductor layer 10 are sequentially grown on the sapphire substrate using a metal-organic chemical vapor deposition (MOCVD) process. The first semiconductor layer 10 is an N-type GaN layer.

[0056] Step 402: Pattern one side of the first semiconductor layer 10 to form a first sub-pixel region 110, a second sub-pixel region 120, and a third sub-pixel region 130 arranged at intervals. Each of the first sub-pixel region 110, the second sub-pixel region 120, and the third sub-pixel region 130 has multiple pores 140, and the porosity of the first sub-pixel region 110, the second sub-pixel region 120, and the third sub-pixel region 130 increases sequentially.

[0057] In this embodiment, step 402 includes: Step 4021: Provide a photomask with a first opening pattern, a second opening pattern and a third opening pattern (hereinafter collectively referred to as opening patterns) arranged at intervals on the photomask, the size of the first opening pattern, the second opening pattern and the third opening pattern decreasing sequentially.

[0058] For example, the size of the first opening pattern is 20~50μm, the size of the second opening pattern is 5~15μm, and the size of the third opening pattern is 2~5μm.

[0059] In the above implementation, the size of the first opening pattern is controlled within the range of 20~50μm, so that the formed first sub-pixel pattern has a small sidewall area ratio. During the etching process, the sidewall stress is released less, thereby spontaneously limiting the formation rate of the pore 140, which makes it easier to obtain a blue sub-pixel region with low porosity.

[0060] By controlling the size of the second opening pattern within the range of 5~15μm, the resulting second sub-pixel pattern has a moderate sidewall area ratio, which can provide a moderate sidewall stress release efficiency during the etching process, thereby spontaneously forming a green sub-pixel region with moderate porosity.

[0061] By controlling the size of the third opening pattern within the range of 2~5μm, the resulting third sub-pixel pattern has a large sidewall area ratio, allowing the sidewall stress to be fully released during the etching process, thereby accelerating the local corrosion reaction and spontaneously forming a red sub-pixel region with high porosity.

[0062] In this embodiment, the first opening pattern, the second opening pattern, and the third opening pattern are arranged in a triangular or linear pattern.

[0063] In the above implementation, by setting the first opening pattern, the second opening pattern, and the third opening pattern on the photomask to be arranged in a triangular or linear pattern, the sub-pixel array arranged in a triangular or linear pattern can be directly defined on the surface of the first semiconductor layer 10 after the photolithography pattern is transferred, thus taking into account both the spatial light mixing uniformity of the three-color sub-pixels and the convenience of laying out the driving connection lines.

[0064] Of course, in other embodiments, the first opening pattern, the second opening pattern, and the third opening pattern may also be arranged in other shapes, such as an L-shaped arrangement or an arc-shaped arrangement, and this disclosure does not limit this.

[0065] Step 4022: Photolithography is performed on the first semiconductor layer 10 using a photomask to form a photoresist layer having a first sub-pixel pattern (hereinafter collectively referred to as the sub-pixel pattern), a second sub-pixel pattern, and a third sub-pixel pattern, wherein the sidewall area ratios of the first sub-pixel pattern, the second sub-pixel pattern, and the third sub-pixel pattern increase sequentially.

[0066] It is worth noting that the sidewall area ratio of a subpixel graphic refers to the ratio between the area of ​​the inner sidewall and the total area of ​​all inner walls.

[0067] Step 4023: Based on the photoresist layer, etch the first semiconductor layer 10 to form a plurality of pores 140.

[0068] For example, in step 4023, etching the first semiconductor layer 10 based on the photoresist layer includes: selecting oxalic acid as the etching solution with a concentration of 0.2~0.3 mol / L, a temperature of 20~25°C, and applying a constant current with a current density of 1~3 mA / cm². 2 The corrosion time is 10~20 minutes.

[0069] In the above implementation method, oxalic acid is selected as the electrochemical etching solution, and the concentration of the oxalic acid solution is controlled within the range of 0.2~0.3 mol / L and the temperature is controlled within the range of 20~25℃, so that the electrolyte has mild and stable ionic conductivity and chemical corrosion activity.

[0070] Meanwhile, in the above implementation, a constant current is applied during the electrochemical etching process, and the current density is controlled at 1~3 mA / cm². 2 The corrosion time is controlled within the range of 10 to 20 minutes, so that sub-pixel patterns with different opening sizes can form a porosity gradient by relying on the difference in their own sidewall stress release within a unified electric field driving force and reaction time.

[0071] For example, after processing in step 4023, the porosity of the first sub-pixel region 110 is less than 10%, the porosity of the second sub-pixel region 120 is 10%~20%, and the porosity of the third sub-pixel region 130 is greater than 20%.

[0072] Step 4024: Remove the photoresist layer on the surface of the first semiconductor layer 10.

[0073] In step 402, by using a photomask with a first opening pattern, a second opening pattern, and a third opening pattern having successively smaller sizes, the first sub-pixel pattern, the second sub-pixel pattern, and the third sub-pixel pattern formed on the photoresist layer are homogenized, photolithographically ...

[0074] Furthermore, during the subsequent etching of the first semiconductor layer 10 based on the photoresist layer, the difference in sidewall stress release efficiency of sub-pixel patterns of different sizes is utilized to induce the first semiconductor layer 10 to spontaneously form a gradient porosity in the opening regions of different sizes, thereby forming the basis for subsequent wavelength modulation.

[0075] In this way, the control method for wavelength modulation is shifted from the complex regional etching parameter control in related technologies to the aperture size design of the photomask, avoiding the stringent requirements of the etching process window.

[0076] Step 403: Prepare active layer 20.

[0077] For example, the epitaxial wafer is reintroduced into the MOCVD reaction chamber, and an InGaN / GaN multiple quantum well layer is epitaxially grown on the surface of the first semiconductor layer 10 as the active layer 20. During the growth of the InGaN quantum well layer, an In source (such as trimethylindium), a Ga source (such as trimethylgallium), and an N source (such as ammonia) are introduced into the reaction chamber, and homogeneous or heterogeneous epitaxial growth is performed at a uniform growth temperature and gas precursor flow rate.

[0078] Because In atoms with larger atomic radii are repelled by the compressive stress of the underlying lattice when incorporated into the GaN lattice, the pre-formed porosity gradient on the surface of the first semiconductor layer 10 alters the lattice relaxation state of each sub-pixel region. Above the first sub-pixel region 110, due to the porosity being less than 10%, the surface lattice maintains high density, resulting in significant residual compressive stress and a strong repulsive effect on In atoms. This leads to a lower In-component incorporation efficiency, resulting in the growth of a low-In-component InGaN quantum well, corresponding to the formation of a blue emitting region. Above the second sub-pixel region 120, due to the porosity being between 10% and 20%, the moderate microporous structure releases some of the lattice compressive stress, weakening the repulsive barrier to In atoms. This results in a moderate In-component incorporation efficiency, leading to the growth of a medium-In-component InGaN quantum well, corresponding to the formation of a green emitting region. Above the third sub-pixel region 130, since the porosity is greater than 20%, the lattice mismatch stress between the first semiconductor layer 10 and the active layer 20 is fully released, which significantly reduces the barrier for In atoms to be incorporated into the lattice, resulting in a high incorporation efficiency of the In composition, thereby growing an InGaN quantum well with a high In composition, which corresponds to the formation of a red light-emitting region.

[0079] In this way, an active layer 20 with progressively increasing In composition can be spontaneously obtained above the three sub-pixel regions through a single epitaxial growth process, achieving monolithic integration of red, green, and blue light-emitting regions.

[0080] Step 404: Prepare electron blocking layer 40.

[0081] Step 405: Prepare the second semiconductor layer 30.

[0082] In the above implementation, steps 403 to 405 can be grown continuously in the same MOCVD epitaxial process, ensuring that the active layer 20, electron blocking layer 40 and second semiconductor layer 30 above each sub-pixel region have good consistency and crystal quality.

[0083] Unless otherwise defined, the technical or scientific terms used herein shall have the ordinary meaning understood by one of ordinary skill in the art to which this disclosure pertains. The terms “first,” “second,” “third,” and similar terms used in this patent application specification and claims do not indicate any order, quantity, or importance, but are merely used to distinguish different components. Similarly, the terms “an” or “a” and similar terms do not indicate a quantity limitation, but rather indicate the presence of at least one. The terms “comprising” or “including” and similar terms mean that the elements or objects preceding “comprising” or “including” encompass the elements or objects listed following “comprising” or “including” and their equivalents, and do not exclude other elements or objects. The terms “connected” or “linked” and similar terms are not limited to physical or mechanical connections, but can include electrical connections, whether direct or indirect. The terms “upper,” “lower,” “left,” “right,” etc., are used only to indicate relative positional relationships; when the absolute position of the described objects changes, the relative positional relationship may also change accordingly.

[0084] The above description is merely an optional embodiment of this disclosure and is not intended to limit this disclosure. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this disclosure should be included within the protection scope of this disclosure.

Claims

1. A full-color light-emitting diode chip, characterized in that, include: A first semiconductor layer (10), an active layer (20), and a second semiconductor layer (30) are stacked sequentially. The first semiconductor layer (10) has a first sub-pixel region (110), a second sub-pixel region (120) and a third sub-pixel region (130) arranged at intervals on one side facing the active layer (20). Each of the first sub-pixel region (110), the second sub-pixel region (120) and the third sub-pixel region (130) has a plurality of pores (140), and the porosity of the first sub-pixel region (110), the second sub-pixel region (120) and the third sub-pixel region (130) increases sequentially.

2. The full-color light emitting diode chip of claim 1, wherein, The porosity of the first sub-pixel region (110) is less than 10%; The porosity of the second sub-pixel region (120) is 10%~20%; The porosity of the third sub-pixel region (130) is greater than 20%.

3. The full-color light emitting diode chip of claim 1, wherein, The first sub-pixel region (110), the second sub-pixel region (120), and the third sub-pixel region (130) are arranged in a triangular or linear pattern.

4. The full-color light emitting diode chip of claim 1, wherein, Including an electron blocking layer (40); The electron blocking layer (40) is located between the active layer (20) and the second semiconductor layer (30).

5. A method of fabricating a full-color light emitting diode chip, characterized by, include: Prepare the first semiconductor layer (10); One side of the first semiconductor layer (10) is patterned to form a first sub-pixel region (110), a second sub-pixel region (120), and a third sub-pixel region (130) arranged at intervals. Each of the first sub-pixel region (110), the second sub-pixel region (120), and the third sub-pixel region (130) has a plurality of pores (140), and the porosity of the first sub-pixel region (110), the second sub-pixel region (120), and the third sub-pixel region (130) increases sequentially. Prepare the active layer (20); Prepare a second semiconductor layer (30).

6. The preparation method according to claim 5, characterized in that, Graphicalizing one side of the first semiconductor layer (10) includes: A photomask is provided, wherein the photomask has a first opening pattern, a second opening pattern and a third opening pattern arranged at intervals, the size of the first opening pattern, the second opening pattern and the third opening pattern decreasing sequentially; The first semiconductor layer (10) is photolithographically ... Based on the photoresist layer, the first semiconductor layer (10) is etched.

7. The preparation method according to claim 6, characterized in that, The size of the first opening pattern is 20~50μm; The size of the second opening pattern is 5~15μm; The size of the third opening pattern is 2~5μm.

8. The preparation method according to claim 6, characterized in that, The first opening pattern, the second opening pattern, and the third opening pattern are arranged in a triangular or linear pattern.

9. The preparation method according to claim 6, characterized in that, Based on the photoresist layer, etching the first semiconductor layer (10) includes: Oxalic acid was selected as the etching solution, with a concentration of 0.2~0.3 mol / L and a temperature of 20~25℃. A constant current was applied with a current density of 1-3 mA / cm 2 for 10-20 min.

10. The preparation method according to claim 5, characterized in that, The porosity of the first sub-pixel region (110) is less than 10%; The porosity of the second sub-pixel region (120) is 10%~20%; The porosity of the third sub-pixel region (130) is greater than 20%.