Transfer method of light emitting device and semiconductor article

By designing a space for nitrogen release when the photoresist does not completely fill the channel gap, and by coating a sacrificial adhesive layer to fill the channel gap after laser stripping, the problems of chip skew and epitaxial damage caused by incomplete or complete filling of the photoresist are solved, thus improving the yield and accuracy of LED chip transfer.

CN123164906APending Publication Date: 2026-11-24BOE HUACAN OPTOELECTRONICS (GUANGDONG) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611097160.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-23
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

During mass transfer, issues with LED chip transfer position accuracy and yield can arise from photoresist not filling or completely filling the chip channels, including chip misalignment or epitaxial damage after laser stripping.

Method used

The design employs a partial filling of the channel gaps with photosensitive adhesive, reserving space for nitrogen release. After laser stripping, a sacrificial adhesive layer is coated to completely fill the channel gaps. The photosensitive adhesive and sacrificial adhesive layer are then etched away to avoid stress concentration and plasma side etching.

Benefits of technology

It effectively avoids stress accumulation and chip corner epitaxial damage caused by the lack of nitrogen release channels, solves the problem of plasma side etching caused by incomplete photoresist filling, and improves the accuracy and yield of transfer positions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123164906A_ABST
    Figure CN123164906A_ABST
Patent Text Reader

Abstract

This disclosure provides a method for transferring a light-emitting device and a semiconductor product, belonging to the field of optoelectronic manufacturing technology. The transfer method includes: bonding one side of a wafer having chips to a temporary substrate coated with a photosensitive adhesive layer to form a transfer substrate, wherein the photosensitive adhesive layer does not completely fill the channel gaps between the chips of the wafer; irradiating the transfer substrate with a laser to remove the substrate of the wafer; coating a sacrificial adhesive layer on the temporary substrate, such that the sacrificial adhesive layer completely fills the channel gaps; and etching the channel gaps to remove the photosensitive adhesive layer and the sacrificial adhesive layer within the channel gaps. This disclosure can avoid damage to the light-emitting device during the transfer process and improve the transfer yield of the light-emitting device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to the field of optoelectronic manufacturing technology, and in particular to a method for transferring light-emitting devices and a semiconductor article. Background Technology

[0002] In the mass transfer process, a chip-on-wafer (COW) with LED chips is bonded to a sapphire substrate coated with photosensitive adhesive to form a chip-on-carrier (COC) wafer. This is a preliminary step in the transfer of Micro LED chips from the growth substrate to the target substrate. The LED chips on the COW are mostly in the micrometer range. The bonding process uses hot pressing to align and bond the COW to a temporary sapphire carrier coated with photosensitive adhesive.

[0003] In related technologies, after forming the COC bonded wafer, the sapphire substrate is first removed using laser lift-off technology to achieve non-destructive separation between the sapphire substrate and the LED chip. Subsequently, the photosensitive adhesive layer between the chip channels is processed using ICP dry etching. Since the photosensitive adhesive filling state can be either incomplete or completely filled with the chip channels, the results after laser lift-off and etching will be slightly different.

[0004] If the photoresist does not completely fill the chip channel, the unfilled area will not be blocked by the photoresist after ICP etching. The plasma will directly interact with the photoresist on the bottom of the chip, causing side etching. This will lead to uneven stress on the LED chip during secondary bonding, causing it to tilt and affecting the accuracy of the transfer position. If the photoresist completely fills the chip channel, uneven side etching can be avoided. However, there is no space for the nitrogen gas generated by laser lift-off of GaN to be released, and the corners of the chip are stress concentration points. This will eventually lead to epitaxial damage at the corners of the chip after lift-off, affecting device performance and yield. Summary of the Invention

[0005] This disclosure provides a method for transferring a light-emitting device and a semiconductor product, which can prevent damage to the light-emitting device during the transfer process and improve the transfer yield of the light-emitting device. The technical solution is as follows: This disclosure provides a method for transferring a light-emitting device. The method includes: bonding one side of a wafer having chips to a temporary substrate coated with a photosensitive adhesive layer to form a transfer substrate, wherein the photosensitive adhesive layer does not completely fill the channel gaps between the chips of the wafer; irradiating the transfer substrate with a laser to remove the substrate of the wafer; coating a sacrificial adhesive layer on the temporary substrate to completely fill the channel gaps; and etching the channel gaps to remove the photosensitive adhesive layer and the sacrificial adhesive layer within the channel gaps.

[0006] In another implementation of the present disclosure, bonding one side of the wafer having a chip to a temporary substrate with a photosensitive adhesive layer coated on its surface includes: determining the amount of photosensitive adhesive layer to be applied evenly based on the area of ​​the channel gap of the wafer and the thickness of the chip; applying the photosensitive adhesive of the amount to be applied evenly to the temporary substrate; attaching the chip side of the wafer to the surface of the photosensitive adhesive; and curing the photosensitive adhesive to form the transfer substrate.

[0007] In another implementation of this disclosure, the amount of adhesive coating is less than or equal to the product of the area of ​​the channel gap of the wafer and the thickness of the chip.

[0008] In another implementation of the present disclosure, curing the photosensitive adhesive to form the transfer substrate includes: controlling the bonding heating temperature to be between 80°C and 250°C, and controlling the thermal curing time to be between 5 min and 60 min, so that the photosensitive adhesive is cured into the photosensitive adhesive layer.

[0009] In another implementation of the present disclosure, irradiating the transfer substrate with a laser to remove the substrate of the wafer includes: controlling the laser energy density to be between 300 mJ / cm² and 1200 mJ / cm², so that the laser irradiates the interface between the epitaxial material of the wafer and the substrate of the wafer, causing the epitaxial material of the wafer to decompose and generate nitrogen gas that enters the channel gap.

[0010] In another implementation of the present disclosure, coating the sacrificial adhesive layer on the temporary substrate includes: coating photosensitive adhesive between the chips of the temporary substrate and holding it at 80°C to 250°C for 5 to 60 minutes.

[0011] In another implementation of the present disclosure, coating the temporary substrate between the chips with photosensitive adhesive includes: using a photosensitive adhesive with a viscosity range of 10 cps to 3000 cps, controlling the spin coating speed to be 1000 rpm to 5000 rpm, and ensuring that the photosensitive adhesive completely fills the channel gap.

[0012] In another implementation of the present disclosure, etching the channel gap includes: controlling the reaction chamber pressure to 5 mTorr to 20 mTorr, the upper electrode power to 500 W to 1500 W, the lower electrode power to 100 W to 300 W, the etching gas being a mixture of O2 and CF4 with a flow ratio of 5:1 to 50:1, and the etching time to 200 s to 2500 s.

[0013] In another implementation of the present disclosure, after etching the channel gap, the method further includes cleaning the transfer substrate with TMAH for a cleaning time of 20s to 1200s and a TMAH concentration of 2% to 10%.

[0014] This disclosure provides a semiconductor article prepared by the transfer method described above. The semiconductor article includes: a temporary substrate, a plurality of chips, and photosensitive adhesive blocks disposed corresponding to the chips. The photosensitive adhesive blocks are located on the temporary substrate, and the chips are located on the corresponding photosensitive adhesive blocks.

[0015] The beneficial effects of the technical solutions provided in this disclosure include at least the following: The transfer method provided in this disclosure first employs a design where the photosensitive adhesive layer does not completely fill the channel gap between wafer chips. During the laser lift-off of the wafer substrate, the unfilled channel gap serves as a release space for nitrogen gas generated during the laser lift-off of the GaN material. This effectively avoids stress accumulation caused by the lack of a nitrogen release channel and also avoids epitaxial damage after lift-off caused by stress concentration at the chip corners, ensuring the structural integrity of the LED chip. After laser lift-off, a new step is added where a sacrificial adhesive layer is coated on a temporary substrate to completely fill the channel gap. Then, the channel gap is etched to remove the photosensitive adhesive layer and the sacrificial adhesive layer. At this point, the completely filled sacrificial adhesive layer can prevent plasma from directly interacting with the photosensitive adhesive at the bottom of the chip during ICP etching, fundamentally solving the plasma side etching problem caused by incomplete channel filling. This prevents the LED chip from tilting due to uneven stress during subsequent secondary bonding and transfer processes, ensuring transfer position accuracy.

[0016] This disclosed embodiment adopts a two-step design: first, the photoresist is not completely filled to reserve space for nitrogen release, and then a sacrificial adhesive layer is added to block side etching. This design solves two mutually exclusive problems in related technologies: epitaxial damage after peeling caused by complete filling of the photoresist and side etching and chip transfer misalignment caused by incomplete filling of the photoresist. This design can effectively improve the yield and reliability of mass transfer of light-emitting devices. Attached Figure Description

[0017] To more clearly illustrate the technical solutions in the embodiments of this disclosure, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of this disclosure. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0018] Figure 1 This is a schematic diagram of a COC (Chip of Criteria) sheet provided by related technologies; Figure 2 This is a schematic diagram of another COC chip provided by related technologies; Figure 3 This is a schematic diagram of a COC wafer after etching, provided by related technologies; Figure 4 This is a flowchart of a method for transferring light-emitting devices according to an embodiment of the present disclosure; Figure 5 This is a flowchart of another method for transferring light-emitting devices provided in this disclosure embodiment; Figure 6 This is a transition state diagram of a light-emitting device provided in an embodiment of this disclosure.

[0019] The markings in the diagram are explained as follows: 10. Chips; 20. Photosensitive adhesive layer; 30. Temporary substrate; 40. Channel clearance; 50. Sacrificial adhesive layer. Detailed Implementation

[0020] To make the objectives, technical solutions, and advantages of this disclosure clearer, the embodiments of this disclosure will be described in further detail below with reference to the accompanying drawings.

[0021] Unless otherwise defined, the technical or scientific terms used herein shall have the ordinary meaning understood by one of ordinary skill in the art to which this disclosure pertains. The terms “first,” “second,” “third,” and similar terms used in this patent application specification and claims do not indicate any order, quantity, or importance, but are merely used to distinguish different components. Similarly, the terms “an” or “a” and similar terms do not indicate a quantity limitation, but rather indicate the presence of at least one. The terms “comprising” or “including” and similar terms mean that the elements or objects preceding “comprising” or “including” encompass the elements or objects listed following “comprising” or “including” and their equivalents, and do not exclude other elements or objects. The terms “connected” or “linked” and similar terms are not limited to physical or mechanical connections, but can include electrical connections, whether direct or indirect. The terms “upper,” “lower,” “left,” “right,” “top,” and “bottom,” etc., are used only to indicate relative positional relationships, and these relative positional relationships may change accordingly when the absolute position of the described objects changes.

[0022] In mass transfer processes, after the wafer-level chip (COW) is bonded to the sapphire substrate coated with photoresist to form a COC wafer, the filling state of the chip channel by the photoresist can be divided into two types due to the combined influence of the LED chip channel morphology and the photoresist coating thickness.

[0023] Figure 1 This is a schematic diagram of a COC (Chip of Criteria) sheet provided by related technologies. For example... Figure 1 As shown, the first type is where the photosensitive adhesive layer 20 does not completely fill the channel gap 40 between the chips 10.

[0024] Figure 2 This is a schematic diagram of another COC (Chip of Criteria) chip provided by related technologies. For example... Figure 2 As shown, the second type is where the photosensitive adhesive layer 20 completely fills the channel gap 40 between the chips 10.

[0025] Figure 3 This is a schematic diagram of a COC wafer after etching, provided by related technologies. For example... Figure 3 As shown, in the first incomplete state, the areas filled with photoresist layer 20 can function as masks during etching. However, in the unfilled channel areas, without the protection of photoresist, the plasma will directly react with the photoresist at the bottom of the chip 10, causing uneven side etching. This defect will lead to uneven stress on the LED chip 10 in the subsequent secondary bonding process, resulting in transfer misalignment and directly reducing the accuracy of the transfer position.

[0026] While the second, fully filled state avoids the problem of uneven lateral etching during the etching stage, the nitrogen gas generated by the decomposition of GaN material during the laser lift-off process lacks a release channel. Furthermore, the corners of the LED chip are stress concentration areas, and the stress cannot be released through the reserved space, ultimately causing epitaxial damage to the corners of the chip after lift-off (see...). Figure 2 (See diagram X in the middle), which seriously affects device performance and yield.

[0027] Therefore, this disclosure provides a method for transferring light-emitting devices. Figure 4 This is a flowchart illustrating a method for transferring light-emitting devices according to an embodiment of this disclosure. Figure 4 As shown, the transfer method includes: Step S11: Bond one side of the wafer with chip 10 to a temporary substrate 30 with photosensitive adhesive layer 20 coated on its surface to form a transfer substrate.

[0028] The photosensitive adhesive layer 20 does not completely fill the channel gap 40 between the chips 10 of the wafer.

[0029] Step S12: Laser irradiation of the transfer substrate to remove the substrate from the wafer.

[0030] Step S13: Coat a sacrificial adhesive layer 50 on the temporary substrate 30 so that the sacrificial adhesive layer 50 completely fills the channel gap 40.

[0031] Step S14: Etch the channel gap 40 to remove the photosensitive adhesive layer 20 and the sacrificial adhesive layer 50 within the channel gap 40.

[0032] The transfer method provided in this embodiment first employs a design where the photosensitive adhesive layer 20 does not completely fill the channel gap 40 between the wafer chips 10. During the laser lift-off of the wafer substrate, the unfilled channel gap 40 serves as a release space for nitrogen gas generated during the laser lift-off of the GaN material, effectively preventing stress accumulation caused by the lack of a nitrogen release channel. Simultaneously, it avoids epitaxial damage after lift-off caused by stress concentration at the corners of the chip 10, ensuring the structural integrity of the LED chip 10. After laser lift-off, a new step is added: coating a sacrificial adhesive layer 50 on a temporary substrate 30 and completely filling the channel gap 40. Then, the channel gap 40 is etched to remove the photosensitive adhesive layer 20 and the sacrificial adhesive layer 50. At this point, the completely filled sacrificial adhesive layer 50 can prevent plasma from directly interacting with the photosensitive adhesive at the bottom of the chip 10 during ICP etching, fundamentally solving the problem of plasma side etching caused by incomplete channel filling. This prevents the LED chip 10 from tilting due to uneven stress during subsequent secondary bonding and transfer processes, ensuring transfer position accuracy.

[0033] This disclosed embodiment adopts a two-step design: first, the photoresist is not completely filled to reserve space for nitrogen release, and then a sacrificial adhesive layer 50 is added to block side etching. This design solves two mutually exclusive problems in related technologies: epitaxial damage after peeling caused by complete filling of the photoresist and side etching of ICP and skewed transfer of chip 10 caused by incomplete filling of the photoresist. This design can effectively improve the yield and reliability of mass transfer of light-emitting devices.

[0034] Figure 5 This is a flowchart of another light-emitting device transfer method provided in this embodiment of the disclosure. Figure 6 This is a transition state diagram of a light-emitting device provided in an embodiment of this disclosure. For example... Figure 5 , 6 As shown, the transfer method includes: Step S21: Determine the amount of photoresist layer 20 to be uniformly coated based on the area of ​​the channel gap 40 of the wafer and the thickness of the chip 10.

[0035] For example, the amount of adhesive coating is less than or equal to the product of the area of ​​the channel gap 40 of the wafer and the thickness of the chip 10.

[0036] For example, the thickness of the photosensitive adhesive layer 20 is 2 μm to 5 μm.

[0037] In step S21 above, the thickness parameters of chip 10 and the area parameters of the channel gap 40 between chips 10 are first obtained by wafer inspection. The basic amount of photoresist is calculated according to the formula: the amount of photoresist ≤ the area of ​​the channel gap 40 × the thickness of chip 10. Finally, the thickness of the photosensitive adhesive layer 20 is controlled in the range of 2μm to 5μm to ensure that the amount of adhesive can only fill part of the channel and leave space for nitrogen release.

[0038] If the amount of adhesive is too large and fills the channel, the nitrogen gas generated by the laser lift-off of GaN will have no release channel; if the amount of adhesive is too small, an effective bonding layer cannot be formed. The parameter design of this step directly reserves nitrogen buffer space for subsequent steps to avoid chip 10 epitaxial damage caused by stress concentration.

[0039] Step S22: Coat the temporary substrate 30 with a uniform amount of photosensitive adhesive.

[0040] Specifically, this may include: fixing the temporary substrate 30 on the stage of the spin coating equipment, and uniformly coating the surface of the temporary substrate 30 with photosensitive adhesive using a spin coating process according to the determined spin coating amount parameters.

[0041] During the coating process, the ambient temperature is controlled at 22±1℃ and the humidity is kept stable between 30% and 60% to avoid uneven evaporation of the adhesive and ensure that the thickness deviation of the adhesive on the entire surface is ≤±0.1μm.

[0042] Step S23: Attach the chip 10 side of the wafer to the surface of the photosensitive adhesive and cure the photosensitive adhesive to form a transfer substrate.

[0043] like Figure 6 As shown, the specific process may include: aligning the side of the wafer with the LED chip 10 with the photosensitive adhesive surface on the temporary substrate 30, using a vacuum pressing device to make the chip 10 fully contact the adhesive surface, and then sending it into a thermosetting oven for curing to form a photosensitive adhesive layer 20.

[0044] During the curing of the photosensitive adhesive, the bonding heating temperature is controlled to be between 80℃ and 250℃, and the heat curing time is controlled to be between 5 minutes and 60 minutes, so that the photosensitive adhesive is cured into a photosensitive adhesive layer 20.

[0045] The above-mentioned bonding heating temperature ensures that the photosensitive adhesive is fully cured to obtain sufficient bonding strength, while avoiding excessive temperature that could lead to performance degradation of the epitaxial layer of the LED chip 10. The cured photosensitive adhesive layer 20 can stably fix the position of the chip 10, providing structural support for subsequent laser lift-off, while the unfilled channel gap 40 has been reserved.

[0046] Step S24: Laser irradiation of the transfer substrate to remove the substrate from the wafer.

[0047] Specifically, this may include: controlling the laser energy density to be between 300 mJ / cm² and 1200 mJ / cm², so that the laser irradiates the interface between the epitaxial material of the wafer and the substrate of the wafer, causing the epitaxial material of the wafer to decompose and generate nitrogen gas that enters the channel gap 40.

[0048] For example, a 248nm KrF excimer laser is used to irradiate the wafer side of the transfer substrate, and the laser energy density is controlled to be 500mJ / cm². The laser acts on the interface between the GaN epitaxial material and the sapphire substrate, causing GaN to decompose and generate nitrogen gas. The nitrogen gas is directly released into the reserved unfilled channel gap 40, and finally the non-destructive separation of the sapphire substrate and the LED chip 10 is completed.

[0049] The reserved channel gap 40 serves as a buffer space for nitrogen release, avoiding the problem of stress concentration at the corner of the chip 10 caused by the lack of nitrogen release in related technologies. This solves the defect of epitaxial damage to the chip 10 after laser stripping and ensures the structural integrity of the chip 10.

[0050] Step S25: Coat a sacrificial adhesive layer 50 on the temporary substrate 30 so that the sacrificial adhesive layer 50 completely fills the channel gap 40.

[0051] like Figure 6 As shown, specifically, it may include: coating photosensitive adhesive between each chip 10 of the temporary substrate 30, and holding it at 80°C to 250°C for 5 min to 60 min to form a sacrificial adhesive layer 50.

[0052] Optionally, when applying the photosensitive adhesive, a photosensitive adhesive with a viscosity range of 10 cps to 3000 cps is used, and the spin coating speed is controlled at 1000 rpm to 5000 rpm to ensure that the photosensitive adhesive completely fills the channel gap 40.

[0053] In one implementation, on the surface of the temporary substrate 30 after laser ablation, a photosensitive adhesive with a viscosity of 2000 cps is applied, and the spin coating speed is controlled at 2000 rpm to coat the sacrificial adhesive layer 50 onto the channel area between each chip 10; then it is cured by holding at 80°C to 250°C for 5 min to 60 min.

[0054] The fully filled sacrificial adhesive layer 50 can serve as a protective layer in subsequent etching processes, preventing plasma from directly contacting the initial photosensitive adhesive layer 20 at the bottom of the chip 10. This avoids the side etching problem caused by ICP etching from the root cause and solves the subsequent transfer skew defect caused by uneven etching of the photosensitive adhesive at the bottom of the chip 10.

[0055] Optionally, during the preparation of the sacrificial adhesive layer 50, a barrier layer with higher hardness can be added between the photosensitive adhesive layer 20 and the sacrificial adhesive layer 50.

[0056] For example, the barrier layer includes SiOx, SiNx, or gallium nitride. The barrier layer has a higher hardness than the photosensitive adhesive layer 20 and can only be removed under preset selective etching conditions.

[0057] When preparing the sacrificial adhesive layer 50, a barrier layer is first prepared on the surface of the photosensitive adhesive layer 20 or the temporary substrate 30. The thickness of the barrier layer is controlled between 30nm and 200nm to achieve a dense barrier effect. Then, the sacrificial adhesive layer 50 is formed on the surface of the barrier layer.

[0058] The high-hardness barrier layer can withstand the pressure during the subsequent coating and curing of the sacrificial adhesive layer 50, preventing the soft sacrificial adhesive from embedding into the bottom initial photosensitive adhesive layer 20 and ensuring the flatness of the bonding interface of the chip 10. The barrier layer has selective removal characteristics, and the barrier layer can be selected to be a material that only reacts with specific solutions. For example, SiOx / SiNx can be selected as the barrier layer for acidic etching solutions. After the channel etching is completed, the barrier layer can be removed separately by the corresponding selective etching process to avoid adhesive residue remaining on the surface or sidewalls of the chip 10 and reduce the impact on the photoelectric performance of the chip 10.

[0059] Step S26: Etch the channel gap 40 to remove the photosensitive adhesive layer 20 and the sacrificial adhesive layer 50 within the channel gap 40.

[0060] like Figure 6 As shown, specifically, it may include: controlling the reaction chamber pressure to 5 mTorr to 20 mTorr, the upper electrode power to 500 W to 1500 W, the lower electrode power to 100 W to 300 W, the etching gas being a mixture of O2 and CF4 with a flow ratio of 5:1 to 50:1, and the etching time to 200 s to 2500 s, in order to etch and remove the photosensitive adhesive layer 20 and the sacrificial adhesive layer 50 within the channel gap 40.

[0061] For example, the transfer substrate is sent into the ICP reaction chamber, the reaction chamber pressure is controlled at 10 mTorr, the upper electrode power is 600 W, the lower electrode power is 200 W, a mixed gas of O2 and FC4 is used as the etching gas, the etching time is 400 s, and the initial photosensitive adhesive layer 20 and the sacrificial adhesive layer 50 in the channel gap 40 are removed simultaneously, exposing the sidewall and bottom bonding interface of the chip 10.

[0062] The presence of the sacrificial adhesive layer 50 ensures that the plasma acts only on the adhesive layer during the etching process, without damaging the chip 10 itself. At the same time, it avoids the uneven side etching that occurs without adhesive layer protection in related technologies, ensuring a flat bottom interface of the chip 10, providing a uniform force surface for subsequent secondary bonding, and improving the accuracy of the transfer position.

[0063] Step S27: Clean the transfer substrate.

[0064] Specifically, this may include cleaning the transfer substrate with TMAH for a cleaning time of 20s to 1200s, with a TMAH concentration of 2% to 10%.

[0065] For example, the surface of the transfer substrate was cleaned for 500 seconds with a 3% TMAH solution to remove residual adhesive residue, reaction byproducts and surface contaminants after etching. After cleaning, the substrate was placed in an inert gas environment for later use.

[0066] This disclosure provides a semiconductor article prepared by the transfer method described above. The semiconductor article includes: a temporary substrate, a plurality of chips, and photosensitive adhesive blocks disposed corresponding to the chips. The photosensitive adhesive blocks are located on the temporary substrate, and the chips are located on the corresponding photosensitive adhesive blocks.

[0067] Alternatively, the chip can be a red light-emitting pixel chip, a green light-emitting pixel chip, or a blue light-emitting pixel chip.

[0068] In this embodiment, each pixel chip includes an epitaxial layer, a passivation layer, and an electrode. The epitaxial layer is located on the surface of the substrate and includes a p-type layer, a light-emitting layer, and an n-type layer stacked sequentially. The n-type layer has a groove exposing the p-type layer. The passivation layer is located on the surface of the n-type layer and within the groove, and the passivation layer has a via exposing the n-type layer and the groove.

[0069] The passivation layer has a first electrode and a second electrode on its surface, and the first electrode and the second electrode are connected to the n-type layer and the p-type layer through two through holes, respectively.

[0070] For a pixel chip that emits red light, the epitaxial layer is a red light epitaxial layer. For a pixel chip that emits green light, the epitaxial layer is a green light epitaxial layer. For a pixel chip that emits blue light, the epitaxial layer is a blue light epitaxial layer.

[0071] The red epitaxial layer comprises a first p-type layer, a first luminescent layer, and a first n-type layer stacked sequentially.

[0072] In the red-light epitaxial layer, the first p-type layer includes a p-type AlInP layer.

[0073] The first luminescent layer comprises alternating layers of AlGaInP quantum wells and AlGaInP quantum barriers, wherein the Al content in the AlGaInP quantum well layers and AlGaInP quantum barrier layers differs. The first luminescent layer may comprise 3 to 8 alternating stacked cycles of AlGaInP quantum well layers and AlGaInP quantum barrier layers.

[0074] The first n-type layer includes an n-type AlGaInP current-spreading layer.

[0075] In this embodiment of the disclosure, the green epitaxial layer includes a second p-type layer, a second luminescent layer, and a second n-type layer stacked sequentially.

[0076] In the green epitaxial layer, the second p-type layer includes a p-type GaN layer.

[0077] The second light-emitting layer comprises alternating InGaN quantum well layers and GaN quantum barrier layers. The second light-emitting layer may include 3 to 8 alternating stacked InGaN quantum well layers and GaN quantum barrier layers.

[0078] The second n-type layer includes an n-type GaN layer.

[0079] In this embodiment of the disclosure, the blue light epitaxial layer includes a third p-type layer, a third light-emitting layer, and a third n-type layer stacked sequentially.

[0080] In the blue light epitaxial layer, the third p-type layer includes a p-type GaN layer.

[0081] The third light-emitting layer may include alternating InGaN quantum well layers and GaN quantum barrier layers. The third light-emitting layer may include 3 to 8 alternating stacked InGaN quantum well layers and GaN quantum barrier layers.

[0082] The third n-type layer includes an n-type GaN layer.

[0083] Optionally, the thickness of the pixel chip 10 is 2 μm to 10 μm.

[0084] For example, the thickness of the red epitaxial layer is 5 μm, the thickness of the green epitaxial layer is 8 μm, and the thickness of the blue epitaxial layer is 6 μm.

[0085] For example, temporary substrates may include sapphire substrates, silicon substrates, glass substrates, gallium oxide substrates, and diamond substrates. These substrates are characterized by high surface flatness, high temperature resistance, and corrosion resistance.

[0086] The temporary substrate and photosensitive adhesive block work together to fix the chip position, ensuring the structural stability of the chip in subsequent laser lift-off, etching, bonding and other processes.

[0087] For example, the materials used to prepare the photosensitive adhesive block include thermoplastic resins, thermosetting resins, and photoresist-based adhesives. Examples include photosensitive adhesives with viscosities ranging from 10 cps to 3000 cps.

[0088] After curing, the photosensitive adhesive forms a stable bonding interface, firmly fixing the chip to the temporary substrate and preventing chip displacement or detachment during the transfer process. As a buffer layer between the chip and the temporary substrate, the photosensitive adhesive matches the difference in their thermal expansion coefficients, reducing thermal stress during the process that could cause chip warping or cracking.

[0089] The above is not intended to limit this disclosure in any way. Although this disclosure has been disclosed above through embodiments, it is not intended to limit this disclosure. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the technical solution of this disclosure. Any simple modifications, equivalent changes and alterations made to the above embodiments based on the technical essence of this disclosure without departing from the content of the technical solution of this disclosure shall still fall within the scope of the technical solution of this disclosure.

Claims

1. A method for transferring light-emitting devices, characterized in that, The transfer method includes: One side of the wafer with chips (10) is bonded to a temporary substrate (30) with a photosensitive adhesive layer (20) coated on its surface to form a transfer substrate, wherein the photosensitive adhesive layer (20) does not completely fill the channel gap (40) between the chips (10) of the wafer. The transfer substrate is irradiated with a laser to remove the substrate from the wafer; A sacrificial adhesive layer (50) is coated on the temporary substrate (30) so that the sacrificial adhesive layer (50) completely fills the channel gap (40). The channel gap (40) is etched to remove the photosensitive adhesive layer (20) and the sacrificial adhesive layer (50) within the channel gap (40).

2. The transfer method according to claim 1, characterized in that, Bonding one side of the wafer containing the chip (10) to a temporary substrate (30) with a photosensitive adhesive layer (20) coated on its surface includes: The amount of photoresist layer (20) is determined based on the area of ​​the channel gap (40) of the wafer and the thickness of the chip (10). The photosensitive adhesive of the specified amount is coated onto the temporary substrate (30); The chip (10) side of the wafer is attached to the surface of the photosensitive adhesive, and the photosensitive adhesive is cured to form the transfer substrate.

3. The transfer method according to claim 2, characterized in that, The amount of adhesive coating is less than or equal to the product of the area of ​​the channel gap (40) of the wafer and the thickness of the chip (10).

4. The transfer method according to claim 2, characterized in that, Curing the photosensitive adhesive to form the transfer substrate includes: The bonding heating temperature is controlled to be 80℃ to 250℃, and the heat curing time is controlled to be 5min to 60min, so that the photosensitive adhesive is cured into the photosensitive adhesive layer (20).

5. The transfer method according to any one of claims 1 to 4, characterized in that, Laser irradiation of the transfer substrate to remove the substrate of the wafer includes: The laser energy density is controlled to be between 300 mJ / cm² and 1200 mJ / cm², so that the laser irradiates the interface between the epitaxial material of the wafer and the substrate of the wafer, causing the epitaxial material of the wafer to decompose and generate nitrogen gas that enters the channel gap (40).

6. The transfer method according to any one of claims 1 to 4, characterized in that, Coating a sacrificial adhesive layer (50) on the temporary substrate (30) includes: Photosensitive adhesive is coated between each chip (10) on the temporary substrate (30) and kept at 80°C to 250°C for 5 to 60 minutes.

7. The transfer method according to claim 6, characterized in that, Coating photosensitive adhesive between the chips (10) on the temporary substrate (30) includes: Use a photosensitive adhesive with a viscosity range of 10 cps to 3000 cps and control the spin coating speed to 1000 rpm to 5000 rpm to ensure that the photosensitive adhesive completely fills the channel gaps (40).

8. The transfer method according to any one of claims 1 to 4, characterized in that, Etching the channel gaps (40) includes: The reaction chamber pressure is controlled from 5 mTorr to 20 mTorr, the upper electrode power is from 500 W to 1500 W, the lower electrode power is from 100 W to 300 W, the etching gas is a mixture of O2 and CF4 with a flow ratio of 5:1 to 50:1, and the etching time is from 200 s to 2500 s.

9. The transfer method according to any one of claims 1 to 4, characterized in that, After etching the channel gap (40), the process further includes: The transfer substrate was cleaned using TMAH for 20 to 1200 seconds, with a TMAH concentration of 2% to 10%.

10. A semiconductor article, characterized in that, The semiconductor article is prepared by the transfer method as described in any one of claims 1 to 9, and the semiconductor article includes: a temporary substrate, a plurality of chips and photosensitive adhesive blocks disposed corresponding to the chips, the photosensitive adhesive blocks being located on the temporary substrate and the chips being located on the corresponding photosensitive adhesive blocks.